ANODE CATALYST LAYER FOR WATER ELECTROLYSIS CELL, MEMBRANE ELECTRODE JOINED BODY, SOLID POLYMER ELECTROLYTE WATER ELECTROLYSIS CELL, Ir / IrOx FIBER CATALYST AND ITS MANUFACTURING METHOD
The Ir/IrOx fiber catalyst addresses the high cost and durability issues of conventional PEM water electrolysis cells by promoting gas discharge and structural stability, enhancing the anode catalyst layer's performance and durability.
Patent Information
- Application Number
- JP2023077735
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-10
AI Technical Summary
Conventional PEM water electrolysis cells face issues with high costs due to the use of expensive iridium oxide powder, aggregation leading to dense electrode structures, and poor long-term durability due to gas retention and structural changes such as expansion and cracking.
Development of an Ir/IrOx fiber catalyst with a fiber structure for the anode catalyst layer, promoting gas discharge and enhancing durability by using a combination of metallic iridium and iridium oxide with controlled fiber diameter and length, and specific Ir(0) content.
The Ir/IrOx fiber catalyst improves gas discharge and suppresses structural changes, resulting in enhanced durability and performance of the anode catalyst layer, thereby extending the lifespan of the water electrolysis cell.
Smart Images

Figure 2024162336000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an anode catalyst layer for a water electrolysis cell used in a water electrolysis cell such as a solid polymer water electrolysis cell, a membrane electrode assembly including the same, and a solid polymer water electrolysis cell. [Background technology]
[0002] A well-known water electrolysis cell is the polymer electrolyte membrane (PEM) water electrolysis cell, which uses a solid polymer membrane as a separator, similar to a polymer electrolyte fuel cell (PEFC).The PEM water electrolysis cell has the advantages of being able to generate hydrogen using only water, the hydrogen gas does not contain any impurities other than water, and the operating temperature is low.
[0003] As shown in Figure 1, in a PEM water electrolysis cell, the electrolysis reaction of water (HO → 2H + +1 / 2O2+2e - ) generates oxygen on the anode side and hydrogen on the cathode side. Water electrolysis cells are used under conditions of high potential (approximately 1.5V to 2.0V) and rapid potential fluctuations. The anode atmosphere is highly acidic and has a high potential, so the materials that can be used as electrode catalysts are limited to precious metals. On the other hand, in PEFCs, which also use precious metal catalysts, electrode catalysts in which precious metal nanoparticles are supported on a carbon support are widely used. However, compared to PEFCs, the anodes of PEM water electrolysis cells are used at even higher potentials, which causes rapid carbon oxidation degradation, so carbon supports cannot be used for water electrolysis cell anodes as in PEFC anodes.
[0004] In conventional PEM water electrolysis cells, the anode catalyst layer contains 1-5 mg / cm of iridium oxide (IrO2). 2Iridium oxide is stable even at a high potential of 1.5 V to 2.0 V, and has high catalytic activity for the anode reaction (oxygen evolution reaction) in water electrolysis. Currently, many of the commonly used commercially available anode catalyst layers for water electrolysis use iridium oxide powder with a diameter of several microns as is (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-209379 A Summary of the Invention [Problem to be solved by the invention]
[0006] For practical use of PEM water electrolysis cells, it is necessary to minimize the amount of precious metal materials used in the anode catalyst layer. Conventional water electrolysis cell anodes that use iridium oxide powder as is are expensive, and because iridium oxide particles tend to aggregate, the electrode structure tends to become dense, making it difficult to properly discharge gas generated during water electrolysis, resulting in performance degradation due to gas retention and structural changes such as expansion and cracking of the anode catalyst layer, which poses issues regarding long-term durability. As such, with the conventional electrode design, it is not possible to reduce the amount of iridium oxide catalyst, and there are issues with long-term durability, so a new anode design was required.
[0007] Under these circumstances, an object of the present invention is to provide an anode catalyst layer for a water electrolysis cell that promotes discharge of evolved gas, suppresses structural change in the anode catalyst layer, and improves durability, and a membrane electrode assembly and a solid polymer water electrolysis cell including the anode catalyst layer. Another object of the present invention is to provide an Ir / IrOx fiber catalyst suitable for forming an anode catalyst layer for a water electrolysis cell, and a method for producing the same. [Means for solving the problem]
[0008] As a result of extensive research aimed at solving the above problems, the inventors focused on gas stagnation and gas discharge in the anode catalyst layer of a water electrolysis cell and discovered that the introduction of an Ir / IrOx fiber catalyst, which is an Ir-based catalyst with a fibrous structure, can promote the discharge of evolved gas, suppress structural changes in the anode catalyst layer, and improve durability, thereby completing the present invention.
[0009] That is, the present invention relates to the following inventions. <1> An anode catalyst layer for a water electrolysis cell, comprising an Ir / IrOx fiber catalyst made of metallic iridium (Ir) and iridium oxide (IrOx), and a proton-conductive electrolyte material. <2> The fiber diameter of the Ir / IrOx fiber catalyst is 20 to 300 nm, and the fiber length is 0.3 to 5 μm. <1> 2. An anode catalyst layer for a water electrolysis cell according to claim 1 . <3> The Ir(0) content in the analysis region near the surface of the Ir / IrOx fiber catalyst measured by X-ray photoelectron spectroscopy (XPS) is 3 atomic % or more and 30 atomic % or less. <1> or <2> 2. An anode catalyst layer for a water electrolysis cell according to claim 1 . <4> A membrane electrode assembly having a solid polymer electrolyte membrane, a cathode catalyst layer bonded to one surface of the solid polymer electrolyte membrane, and an anode catalyst layer bonded to the other surface of the solid polymer electrolyte membrane, wherein the anode catalyst layer is <1> from <3> 2. A membrane electrode assembly comprising the anode catalyst layer for a water electrolysis cell according to claim 1 . <5> <4> A solid polymer water electrolysis cell comprising the membrane electrode assembly according to claim 1.
[0010] <1a> An Ir / IrOx fiber catalyst made of metallic iridium (Ir) and iridium oxide (IrOx), having a fiber diameter of 20 to 300 nm and a fiber length of 0.3 to 5 μm. <2a> The Ir / IrOx fiber catalyst according to <1a>, wherein the content of Ir(0) in an analysis region near the surface as measured by X-ray photoelectron spectroscopy (XPS) is 3 atomic % or more and 30 atomic % or less. <3a> A method for producing the Ir / IrOx fiber catalyst according to <1a> or <2a>, comprising the following steps (1) to (3): Step (1) preparing a mixed solution containing an iridium precursor compound and a thickening polymer Step (2) Electrospinning the mixed solution to obtain a precursor fiber. Step (3) Heat-treating the precursor fiber obtained by electrospinning Effect of the Invention
[0011] The present invention provides an anode catalyst layer for a water electrolysis cell that promotes discharge of evolved gas, suppresses structural change in the anode catalyst layer, and improves durability, and a membrane electrode assembly and a solid polymer water electrolysis cell each including the anode catalyst layer. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a conceptual diagram showing a typical configuration of a solid polymer water electrolysis cell. [Diagram 2] FIG. 1 is a conceptual schematic diagram of an anode catalyst layer for water electrolysis according to the present invention. [Diagram 3] FIG. 1 is an explanatory diagram of an electrospinning process. [Figure 4] 1 is a schematic cross-sectional view of a membrane electrode assembly of the present invention. [Diagram 5] FE-SEM images of electrode catalysts, where (a) is Reference Example 1 (commercial IrO2 catalyst), (b) is Example 1 (fiber catalyst), and (c) is Example 2 (fiber catalyst). [Figure 6] 1 shows XRD profiles of Examples 1 and 2 and Reference Example 1. [Figure 7] 1 shows XPS analyses (Ir(4f) spectra) of Examples 1 and 2 and Reference Example 1, where (a) is Example 1, (b) is Example 2, and (c) is Reference Example 1. [Figure 8] 1 shows the conditions for conditioning voltage application to PEM water electrolysis cells using the fiber catalysts of Examples 1 and 2. [Figure 9] 1 shows IV characteristics (initial performance) of the PEM water electrolysis cells of Examples 1 and 2 and Reference Example 1. [Figure 10] 1 shows potential cycle conditions in the evaluation of potential cycle durability. [Figure 11] IV performance evaluation of each PEM water electrolysis cell before and after durability testing: (a) Example 1, (b) Example 2, and (c) Reference Example 1. [Figure 12] 1 shows overvoltage evaluation of the PEM water electrolysis cell of Example 1 before and after a durability test, (a) activation overvoltage, (b) concentration overvoltage, and (c) ohmic overvoltage. [Figure 13] 1 shows overvoltage evaluation of the PEM water electrolysis cell of Example 2 before and after a durability test, (a) activation overvoltage, (b) concentration overvoltage, and (c) ohmic overvoltage. [Figure 14] 1 shows overvoltage evaluation of the PEM water electrolysis cell of Reference Example 1 before and after a durability test, where (a) is activation overvoltage, (b) is concentration overvoltage, and (c) is ohmic overvoltage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples, and can be modified as desired without departing from the gist of the present invention. In this specification, the word "to" is used as an expression including the numerical values or physical quantities before and after it.
[0014] <1. Anode catalyst layer for water electrolysis cells> The present invention relates to an anode catalyst layer for a water electrolysis cell (hereinafter sometimes referred to as "the anode catalyst layer of the present invention") that contains an Ir / IrOx fiber catalyst made of metallic iridium (Ir) and iridium oxide (IrOx), and a proton-conductive electrolyte material.
[0015] Hereinafter, in this specification, "Ir / IrOx fiber catalyst consisting of metallic iridium (Ir) and iridium oxide (IrOx)" may be referred to as "Ir / IrOx fiber catalyst" or simply as "fiber catalyst".
[0016] Fig. 2 is a conceptual schematic diagram showing a typical structure of the anode catalyst layer of the present invention. As shown in Fig. 2, the anode catalyst layer 1 has a structure in which Ir / IrOx fiber catalysts 2 are in contact with each other and a proton-conductive electrolyte material 3 is held between them. With such a structure, the Ir / IrOx fiber catalysts 2 in contact with each other form a conductive path, and the anode catalyst layer as a whole has excellent electronic conductivity. Furthermore, the gaps between the long-diameter fiber catalysts can be made to be at least voids to the extent that they exhibit air permeability, so that they have excellent diffusibility for gases involved in the electrode reaction, such as hydrogen, oxygen, and water vapor, and can adequately retain the proton-conductive electrolyte material. Therefore, a water electrolysis cell having an anode catalyst layer of the present invention exhibits excellent electrode performance, is highly durable, and can perform water electrolysis for a long period of time.
[0017] The anode catalyst layer of the present invention is characterized by containing an Ir / IrOx fiber catalyst. Iridium oxide (IrOx) is an oxide that has excellent water electrolysis catalytic activity and electronic conductivity, but its electronic conductivity is inferior to that of metallic iridium (Ir). The Ir / IrOx fiber catalyst according to the present invention contains both metallic iridium (Ir) and iridium oxide (IrOx) and has excellent water electrolysis catalytic activity due to the iridium oxide (IrOx) and electronic conductivity due to the metallic iridium (Ir), and therefore can provide sufficient water electrolysis catalytic activity and electronic conductivity when used to form an anode catalyst layer for a water electrolysis cell.
[0018] The Ir / IrOx fiber catalyst according to the present invention is suitable for forming the anode catalyst layer of the present invention, but may also be used for other purposes.
[0019] The anode catalyst layer of the present invention will be described in more detail below.
[0020] (Ir / IrOx fiber catalyst) The Ir / IrOx fiber catalyst used in the anode catalyst layer of the present invention is a fiber-shaped electrode catalyst material containing iridium oxide (IrOx) and metallic iridium (Ir). Here, iridium oxide (IrOx) has electronic conductivity and is highly ion-conductive in the electrolysis of water (H2O→2H + +1 / 2O2+2e - ), and metallic iridium (Ir) has better electronic conductivity than iridium oxide (IrOx), so the Ir / IrOx fiber catalyst has both excellent water electrolysis catalytic activity and electronic conductivity.
[0021] The Ir / IrOx fiber catalyst according to the present invention contains metallic Ir and IrOx, and the ratio of metallic Ir to IrOx can be arbitrary as long as it has sufficient water electrolysis catalytic activity and electronic conductivity when formed into an anode catalyst layer of a water electrolysis cell. The Ir / IrOx fiber catalyst of the present invention includes fiber catalysts in which the entire fiber (surface and interior) is made of metallic Ir and IrOx, fiber catalysts in which the surface layer contains metallic Ir and IrOx and the interior of the fiber is metallic Ir and / or IrOx, and fibers in which the surface layer obtained by oxidizing the surface of a metallic Ir fiber is an iridium oxide layer.
[0022] As described later in the Examples, the metallic Ir and IrOx in the Ir / IrOx fiber catalyst can be evaluated by X-ray diffraction (XRD) and X-ray photoelectron spectroscopy (XPS).
[0023] The electrode catalyst material contained in the anode catalyst layer of the present invention may be only the Ir / IrOx fiber catalyst, but may also contain other substances within the range that does not impair the performance.
[0024] In the present invention, an Ir / IrOx fiber catalyst is used, so that when the anode catalyst layer is formed, adjacent fiber catalysts can be in continuous contact with each other, and a space large enough to smoothly diffuse gases such as hydrogen and oxygen and to smoothly discharge water (vapor) in the water electrolysis electrode can be formed.
[0025] The fiber diameter of the Ir / IrOx fiber catalyst may be within a range in which the fiber catalysts can contact each other and achieve both electrical conductivity and gas diffusion in the electrode when the anode catalyst layer is formed, and is preferably 20 to 300 nm, more preferably 50 to 250 nm. The fiber diameter of the Ir / IrOx fiber catalyst can be obtained by averaging the fiber diameters of any Ir / IrOx fiber catalyst (20 fibers) examined from an electron microscope image.
[0026] The fiber length of the Ir / IrOx fiber catalyst may be within a range in which the fiber catalysts can contact each other and can achieve both electrical conductivity and gas diffusion in the electrode when the anode catalyst layer is formed, and is, for example, within a range of 0.3 to 5 μm in total length (preferably within a range of 0.5 to 3 μm). The fiber length of the Ir / IrOx fiber catalyst can be obtained from an electron microscope image.
[0027] A preferred embodiment of the Ir / IrOx fiber catalyst according to the present invention contains both metallic Ir and IrOx on the surface. Here, the presence or absence of metallic Ir (Ir(0)) on the surface of an Ir / IrOx fiber can be verified by X-ray photoelectron spectroscopy (XPS). The Ir / IrOx fiber catalyst of the present invention has an Ir(0) content in the analysis region near the surface measured by XPS of preferably 3 atomic % or more and 30 atomic % or less, and more preferably 5 atomic % or more and 15 atomic % or less.
[0028] The Ir / IrOx fiber catalyst according to the present invention can be produced by any method as long as it has sufficient water electrolysis catalytic activity and electronic conductivity when used to form an anode catalyst layer of a water electrolysis cell. In particular, it can be suitably produced by a production method using electrospinning, which will be described later in <2. Production method of Ir / IrOx fiber catalyst>. An example of a suitable method for producing an Ir / IrOx fiber catalyst using an electrospinning method will be described in the examples below.
[0029] (Proton-conducting electrolyte materials) The anode catalyst layer of the present invention contains a proton-conductive electrolyte material used as an electrolyte material for a water electrolysis cell (hereinafter, may be referred to as "proton-conductive electrolyte material" or simply as "electrolyte material"). The electrolyte material contained in the anode catalyst layer together with the Ir / IrOx fiber catalyst may be the same as or different from the electrolyte material used in the electrolyte membrane for water electrolysis. From the viewpoint of improving the adhesion between the anode catalyst layer and the electrolyte membrane, it is preferable to use the same material.
[0030] Proton-conductive electrolyte materials are roughly divided into fluorine-based electrolyte materials that contain fluorine atoms in all or part of the polymer skeleton, and hydrocarbon-based electrolyte materials that do not contain fluorine atoms in the polymer skeleton, and both of these can be used as the electrolyte material.
[0031] Specific preferred examples of fluorine-based electrolyte materials include Nafion (registered trademark, manufactured by DuPont), Aciplex (registered trademark, manufactured by Asahi Kasei Corporation), and Flemion (registered trademark, manufactured by Asahi Glass Co., Ltd.).
[0032] Specific examples of suitable hydrocarbon electrolyte materials include polymers such as polysulfonic acid, polystyrene sulfonic acid, polyaryl ether ketone sulfonic acid, polyphenyl sulfonic acid, polybenzimidazole sulfonic acid, polybenzimidazole phosphonic acid, and polyimide sulfonic acid, as well as polymers having side chains such as alkyl groups.
[0033] The mass ratio of the Ir / IrOx fiber catalyst and the electrolyte material in the anode catalyst layer of the present invention may be appropriately determined so as to provide good proton conductivity in the anode catalyst layer formed using these materials and to facilitate gas diffusion and water vapor discharge in the anode catalyst layer. However, if the amount of electrolyte material is too large relative to the Ir / IrOx fiber catalyst, the proton conductivity improves but the gas diffusibility tends to decrease. Conversely, if the amount of electrolyte material is too small, the gas diffusibility improves but the proton conductivity tends to decrease. Therefore, the mass ratio of the electrolyte material to the Ir / IrOx fiber catalyst is preferably in the range of 10 to 50 mass%. If this mass ratio is less than 10 mass%, the continuity of the proton-conductive material is poor, and sufficient proton conductivity for the anode catalyst layer cannot be ensured. Conversely, if it is more than 50 mass%, the diffusibility of gases (oxygen, hydrogen, water vapor) and water inside the anode catalyst layer may decrease.
[0034] The water electrolysis electrode of the present invention may contain components other than the above-mentioned Ir / IrOx fiber catalyst and proton conductive material, provided such components do not impair the object of the present invention.
[0035] 2. Manufacturing method of Ir / IrOx fiber catalyst The above-mentioned Ir / IrOx fiber catalyst of the present invention can be suitably produced by the production method described below (hereinafter referred to as the "production method of the present invention"). That is, the method for producing an Ir / IrOx fiber catalyst according to the present invention includes the following steps. Step (1) preparing a mixed solution containing an iridium precursor compound and a thickening polymer Step (2) Electrospinning the mixed solution to obtain a precursor fiber. Step (3) Heat-treating the precursor fiber obtained by electrospinning
[0036] An example of a suitable method for producing an Ir / IrOx fiber catalyst according to the production method of the present invention will be described in the examples below.
[0037] Each step in the production method of the present invention will now be described in detail.
[0038] "Process (1)" Step (1) is a step of preparing a mixed solution containing an iridium precursor compound and a thickening polymer. In step (1), the types and amounts of the iridium precursor compound, the thickening polymer, and the solvent are selected so as to obtain a concentration and viscosity suitable for electrospinning in step (2).
[0039] The solvent of the mixed solution is appropriately selected from those capable of dissolving both the iridium precursor compound and the thickening polymer. Specific examples include water, methanol, ethanol, isopropanol, n-propanol, acetone, tetrahydrofuran (THF), N,N-dimethylformamide (DMF), etc. These may be used alone or in combination of two or more.
[0040] As the iridium precursor compound, inorganic compounds or organic compounds containing Ir can be selected, such as iridium chloride, chloroiridic acid, tris(acetylacetonato)iridium, hexaammineiridium chloride, and hydrates thereof. Among these, iridium chloride (IrCl3·xH2O) is a suitable example.
[0041] The thickening polymer is used to adjust the viscosity of the mixed solution so as to make it suitable for electrospinning in step (2) and may be any polymer that can be removed by heat treatment in step (3). There are no particular limitations on the type of polymer. Specific examples of the thickening polymer that can be used include polyvinyl alcohol, polyvinyl acetate, polyvinylpyrrolidone (PVP), polyacrylic acid, polyethylene oxide, etc. These may be used alone or in combination of two or more.
[0042] The mixed solution may contain additives other than the iridium precursor compound and the thickening polymer in order to ensure smooth spinning, provided that the object of the present invention is not impaired. Examples of additives include acetic acid, stearic acid, adipic acid, ethoxyacetic acid, benzoic acid, etc. Mixtures of two or more of these may be used.
[0043] The mixing order and mixing time when preparing the mixed solution are arbitrary as long as a homogeneous mixed solution is obtained. Any two or three or more of the iridium precursor compound, thickening polymer, and optional components may be blended in advance and then the remaining components may be mixed, or all of them may be mixed at once.
[0044] "Process (2)" Step (2) is a step of electrospinning the mixed solution obtained in step (1) to obtain a precursor fiber.
[0045] An explanatory diagram of the electrospinning method is shown in Figure 3. In the electrospinning method, the mixed solution obtained in step (1) is filled into a syringe, and the solution is discharged from the tip of a needle-shaped nozzle attached to the syringe while a high DC voltage (usually the nozzle is the positive electrode and the collector is the negative electrode) is applied between the needle-shaped nozzle attached to the syringe and a collector facing the nozzle. The mixed solution discharged from the nozzle is stretched by Coulomb force and the solvent is removed, resulting in the formation of a precursor fiber containing an iridium precursor compound and a thickening polymer.
[0046] The diameter of the precursor fiber can be controlled by the type and concentration of the iridium precursor compound and thickening polymer in the mixed solution, the liquid feed rate, the voltage applied between the nozzle and collector, the nozzle diameter, and other conditions, and the manufacturing conditions can be appropriately set to obtain the desired fiber diameter of the Ir / IrOx fiber catalyst. Although not particularly limited, in the case of the iridium precursor compound (iridium chloride (IrCl3·xH2O), thickening polymer (PVP), and ethanol / DMF mixed solvent disclosed in the examples, for example, by setting the voltage applied between the nozzle and collector to 10 to 30 kV and the solution rate to 0.1 to 1 mL / h, it is possible to obtain a precursor fiber having the desired fiber diameter of the Ir / IrOx fiber catalyst (20 to 300 nm) after the heat treatment in step (3).
[0047] "Process (3)" Step (3) is a step of heat treating the precursor fiber obtained by electrospinning in step (2). In step (2), the obtained precursor fiber contains an iridium precursor compound and a thickening polymer, and since it has low activity and electronic conductivity as it is, it is converted into fibrous Ir / IrOx by heat treatment.
[0048] The heat treatment conditions are appropriately selected taking into consideration the types of iridium precursor compound and thickening polymer, the desired Ir / IrOx ratio, etc., but conditions under which highly active Ir / IrOx can be obtained are preferably an oxidizing atmosphere at a temperature in the range of 300° C. or higher and 500° C. or lower (preferably 400° C. or higher and 450° C. or lower). The oxidizing atmosphere is usually an air atmosphere, but it may be oxygen only or a mixture of oxygen and an inert gas. Water vapor may be added to the atmosphere as necessary.
[0049] In step (3), since not only the attained temperature but also the heating rate affects the physical properties of the Ir / IrOx fiber catalyst, the heating rate is determined within a range in which the desired activity and electronic conductivity are obtained, and an example of this is a heating rate of 0.1 to 3°C / min.
[0050] The Ir / IrOx fiber obtained in step (3) can be pulverized as necessary to adjust the fiber length to the desired length.
[0051] The Ir / IrOx fiber catalyst of the present invention can be produced by the above-mentioned production method of the present invention, and has a fiber diameter of 20 to 300 nm (preferably 50 to 250 nm) and a fiber length of 0.3 to 5 μm (preferably 0.5 to 3 nm). In the Ir / IrOx fiber catalyst of the present invention, the Ir(0) content in the analysis region near the surface measured by X-ray photoelectron spectroscopy (XPS) is preferably 3 atomic % or more and 30 atomic % or less.
[0052] As described above, the Ir / IrOx fiber catalyst of the present invention is suitable for forming the anode catalyst layer of the present invention, but may also be used for other purposes.
[0053] <3. Membrane electrode assembly and solid polymer water electrolysis cell> The membrane electrode assembly (MEA) of the present invention is a membrane electrode assembly comprising a solid polymer electrolyte membrane, a cathode catalyst layer bonded to one side of the solid polymer electrolyte membrane, and an anode catalyst layer bonded to the other side of the solid polymer electrolyte membrane, wherein the anode catalyst layer comprises the above-mentioned anode catalyst layer for a water electrolysis cell.
[0054] Furthermore, the solid polymer water electrolysis cell of the present invention (hereinafter may be referred to as a PEM water electrolysis cell, or simply as a water electrolysis cell) comprises the above-mentioned membrane electrode assembly of the present invention, and generally has a structure in which the membrane electrode assembly is sandwiched between gas diffusion layers (cathode gas diffusion layer, anode gas diffusion layer) and separators in which gas flow paths are formed. In practice, a stack is formed in which the PEM water electrolysis cells (single cells) of the present invention are stacked in a number corresponding to the power generation performance, and used by assembling other associated devices such as a gas supply device, a cooling device, etc.
[0055] Hereinafter, components of the MEA of the present invention and the PEM water electrolysis cell (single cell) of the present invention other than the anode catalyst layer of the present invention will be described. However, since the components of the present invention other than the anode catalyst layer are similar to those of known water electrolysis cells (single cells), detailed description will be omitted and only a brief description will be given.
[0056] Fig. 4 is a schematic diagram showing a cross-sectional structure of a membrane electrode assembly 10 according to an embodiment of the present invention. As shown in Fig. 4, the membrane electrode assembly 10 has a structure in which a cathode catalyst layer 4a and an anode catalyst layer 5a are disposed facing a solid polymer electrolyte membrane 6, and the membrane electrode assembly 10 is sandwiched between a cathode gas diffusion layer 4b and an anode gas diffusion layer 5b.
[0057] The cathode 4 is composed of a cathode catalyst layer 4a and a cathode gas diffusion layer 4b. As long as the object of the present invention is not impaired, a conventionally known cathode catalyst layer and a cathode gas diffusion layer used in a conventional membrane electrode assembly or a PEM water electrolysis cell can be used, and can be appropriately selected depending on the type of solid electrolyte membrane. Typically, the cathode catalyst layer includes a carbon material (graphite, carbon black, activated carbon, etc.) carrying precious metal particles as a catalyst, and an electrolyte material. The cathode diffusion layer includes a conductive carbon-based sheet-like member, and preferably, a water-repellent carbon cloth, carbon paper, carbon nonwoven fabric, etc. can be used.
[0058] The anode 5 is composed of an anode catalyst layer 5a and an anode gas diffusion layer 5b. As described above, the electrode catalyst layer 5a uses the anode catalyst layer for a water electrolysis cell of the present invention, and therefore a detailed description thereof will be omitted.
[0059] As the anode gas diffusion layer 5b of the anode 5, any known anode gas diffusion layer used in a water electrolysis cell can be used as long as it does not impair the object of the present invention. A suitable specific example is a sheet-like porous titanium body.
[0060] The "sheet-shaped titanium porous body" is a sheet-shaped porous body made of titanium or a titanium alloy. In this specification, the term "titanium alloy" means "an alloy containing 40 mol % or more of Ti." There are no particular limitations on the metal to be alloyed with Ti, so long as it does not impair the object of the present invention. Titanium or titanium alloys are resistant to corrosion even in the harsh environment during water electrolysis and have excellent durability.
[0061] The sheet-like titanium porous body should have the properties required for an anode diffusion layer for a water electrolysis cell, such as mechanical strength and porosity. As long as the object of the present invention is not impaired, a sintered body of titanium (titanium alloy) particles, a sheet-like titanium (titanium alloy) mesh sheet, or a laminate thereof can be used, although a sheet-like titanium fiber aggregate is preferably used.
[0062] The titanium fiber aggregate in sheet form can be formed by sintering or pressing titanium fibers. The length and thickness of the titanium fibers in the titanium fiber aggregate are optional.
[0063] The titanium fibers may also be coated with Pt.
[0064] The thickness of the sheet-like titanium fiber assembly is appropriately selected in consideration of mechanical strength, handling, and the like, so long as it does not impair the purpose of the anode diffusion layer, but is typically 10 μm to 1 mm.
[0065] A known proton-conductive solid polymer electrolyte membrane can be used as the solid electrolyte membrane 6. Although the thickness is exaggerated in Fig. 4, the thickness of the solid polymer electrolyte membrane 6 is preferably thin enough to reduce electrical resistance without causing damage.
[0066] The electrolyte material constituting the solid polymer electrolyte membrane may be one that does not decompose under the operating conditions of the PEM water electrolysis cell, and conventionally known materials are used as electrolyte materials for PEM water electrolysis cells, such as fluorine-based electrolyte materials and hydrocarbon-based electrolyte materials. In particular, electrolyte membranes formed from fluorine-based electrolyte materials are preferred because they have excellent heat resistance and chemical stability. Specifically, Nafion (registered trademark, manufactured by DuPont), Aciplex (registered trademark, manufactured by Asahi Kasei Corporation), and Flemion (registered trademark, manufactured by Asahi Glass Co., Ltd.) are preferred examples. Examples of the hydrocarbon-based polymer electrolyte material include polymers such as polysulfonic acid, polystyrene sulfonic acid, polyaryl ether ketone sulfonic acid, polyphenyl sulfonic acid, polybenzimidazole sulfonic acid, polybenzimidazole phosphonic acid, and polyimide sulfonic acid, as well as polymers having side chains such as alkyl groups.
[0067] Embodiments of the water electrolysis cell of the present invention have been described above with reference to the drawings. However, these are merely examples of the water electrolysis cell of the present invention, and various configurations other than those described above may be adopted as long as the water electrolysis anode catalyst layer of the present invention is used as the anode catalyst layer.
[0068] The cathode separator and the anode separator (not shown) are not particularly limited, and any known separators can be used.
[0069] Furthermore, there is no limitation on the method of using the water electrolysis cell of the present invention. Typically, the water electrolysis cell of the present invention (single cells) is stacked in a number appropriate for performance to form a stack, and the cell is used by assembling other associated devices such as a gas supply device, a cooling device, etc. EXAMPLES
[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0071] 1. Manufacturing of Ir / IrOx Fiber <Example 1> "Process (1)" IrCl3·xH2O (Tokyo Chemical Industry Co., Ltd.) (0.748 g) was added as an iridium precursor compound to a mixed solvent of ethanol (9 mL) / DMF (N,N-dimethylformamide, Aldrich) (9 mL), and ultrasonicated for 30 minutes. The mixture was then stirred for approximately 24 hours to obtain an iridium precursor compound solution. Next, PVP (polyvinylpyrrolidone, Aldrich) (1.5636 g) was added as a thickening polymer, and the mixture was stirred at room temperature for approximately 24 hours to obtain a mixed solution containing the iridium precursor compound and the thickening polymer. "Process (2)" Using the apparatus shown in Figure 3, precursor fibers were produced by electrospinning using the mixed solution obtained in step (1). A syringe pump (LM S Co., Ltd.) was used to extrude the mixed solution containing the precursor compounds at 0.6 mL / h, and electrospinning was performed by applying 14 kV using a high-voltage power supply (HVU-30P100, MEC Co., Ltd.). After electrospinning, the precursor fibers were obtained by drying in a vacuum for at least 1 hour. "Process (3)" The obtained precursor fiber was collected on a hot plate using a brass mesh as a collector and heat-treated in air under heat treatment conditions (heating rate: 1°C / min, reached temperature: 500°C, holding time: 2 hours) to remove chlorine and other substances contained in the polymer compound (thickening polymer) and precursor, thereby obtaining the Ir / IrOx fiber catalyst (fiber_1) of Example 1.
[0072] <Example 2> The Ir / IrOx fiber catalyst (fiber_2) of Example 2 was obtained in the same manner as in Example 1, except that the heat treatment conditions in step (3) in Example 1 were a temperature rise rate of 3°C / min, a reached temperature of 500°C, and a holding time of 2 hours.
[0073] <Example 3> The Ir / IrOx fiber catalyst (fiber_3) of Example 3 was obtained in the same manner as in Example 1, except that the heat treatment conditions in step (3) in Example 1 were a temperature rise rate of 1.5°C / min, a reached temperature of 450°C, and a holding time of 2 hours.
[0074] <Example 4> The Ir / IrOx fiber catalyst (fiber_4) of Example 4 was obtained in the same manner as in Example 1, except that the heat treatment conditions in step (3) in Example 1 were a temperature rise rate of 3°C / min, a reached temperature of 400°C, and a holding time of 6 hours.
[0075] <Example 5> The Ir / IrOx fiber catalyst (fiber_5) of Example 5 was obtained in the same manner as in Example 1, except that the heat treatment conditions in step (3) in Example 1 were a temperature rise rate of 3°C / min, a reached temperature of 450°C, and a holding time of 6 hours.
[0076] Table 1 shows the heat treatment conditions for producing the Ir / IrOx fiber catalysts of Examples 1 to 5 (fiber_1 to fiber_5).
[0077] [Table 1]
[0078] 2. Physical property evaluation 2-1: Evaluation by electron microscope Using a scanning electron microscope (FE-SEM), the microstructures of the fiber catalysts (fiber_1 to fiber_5) of Examples 1 to 5 were observed. In addition, a commercially available IrO2 catalyst was observed as Reference Example 1. Table 2 shows the heat treatment conditions, and the fiber diameters (fiber diameters) and ratios of the fibers obtained by microstructure observation. The ratio of fibers was determined from the area occupied by Ir / IrOx fibers and other forms of Ir / IrOx in the FE-SEM image. As representative examples of microstructural observation, FIG. 5(a) shows an FE-SEM image of the commercially available IrO2 catalyst of the reference example, FIG. 5(b) shows the fiber catalyst of Example 1, and FIG. 5(c) shows the fiber catalyst of Example 2.
[0079] As shown in FIG. 5(a), the IrO2 catalyst of Reference Example 1 was composed of aggregates of IrO2 particles, and the maximum particle size of each particle was about 300 nm. On the other hand, the fiber catalysts of Examples 1 to 5 each had a fibrous shape. The fiber catalyst of Example 1 (FIG. 5(b)) had a fiber diameter of 150 to 200 nm, and the fiber catalyst of Example 2 (FIG. 5(c)) had a fiber diameter of 30 to 100 nm. The fiber catalyst of Example 3 (not shown) had a fiber diameter of 50 to 150 nm, the fiber catalyst of Example 4 (not shown) had a fiber diameter of 50 to 120 nm, and the fiber catalyst of Example 5 (not shown) had a fiber diameter of 30 to 100 nm. In addition to the fiber portions, agglomerated portions of 3 μm or more were also confirmed in the fiber catalysts of Examples 1 to 5. As shown in Table 2, the fiber catalyst of Example 1 had few agglomerated portions, and 70% of the total was present as fibers.
[0080] [Table 2]
[0081] 2-2: Evaluation by XRD FIG. 6 shows the results of evaluation of the fiber catalysts of Examples 1 and 2 and the commercially available catalyst of Reference Example 1 by X-ray diffraction. As shown in FIG. 6, it was confirmed that the commercially available IrO2 catalyst of Reference Example 1 was mainly composed of Ir oxide and was amorphous. On the other hand, it was confirmed that the fiber catalysts of Examples 1 and 2 were composed of metallic Ir and IrO2. In addition, it was confirmed that the crystallinity was higher than that of the commercially available IrO2 catalyst of Reference Example 1.
[0082] 2-3: Evaluation by XPS The composition and chemical bond state of elements present on the surface of the fiber catalysts (fiber_1, fiber_2) of Examples 1 and 2 and the commercially available IrO2 catalyst were evaluated by XPS. Figures 7(a) to (c) show the XPS analysis results in the 58 to 70 eV region of Ir(4f). Table 3 summarizes the results of the separation analysis of the peaks in Figures 7(a) to (c).
[0083] As shown in Figures 7(a) and 7(b), the fiber catalysts of Examples 1 and 2 had peaks attributable to IrO2 at 61.1 eV and 64.1 eV as Ir(III) and at 62.4 eV and 65.0 eV as Ir(IV), confirming that IrO2 was the main component. It was also confirmed that the peak of Ir(0) (metallic Ir) was included at 60.9 eV on the low energy side. As shown in Table 3, the ratio of Ir(0) (Ir4f 7 / 2 and Ir4f 5 / 2 % in Example 1 and 14 atomic % in Example 2. On the other hand, in the commercially available IrO2 catalyst of Reference Example 1, a peak derived from IrO2 appeared, but no peak attributable to Ir(0) was observed.
[0084] [Table 3]
[0085] 2-4. Nitrogen adsorption measurement evaluation Table 4 shows the results of nitrogen adsorption measurements carried out on the fiber catalysts of Examples 1 and 2 (fiber_1, fiber_2) and the commercially available IrO2 catalyst. As shown in Table 4, it was found that the fiber catalysts of Examples 1 and 2 had a significantly smaller specific surface area than the commercially available IrO2 catalyst.
[0086] [Table 4]
[0087] 3. Electrochemical Evaluation 3-1. Fabrication of membrane electrode assembly (MEA) and PEM water electrolysis cell A membrane electrode assembly (MEA) and a PEM water electrolysis cell having an anode catalyst layer containing the fiber catalysts (fiber_1, fiber_2) of Examples 1 and 2, or the commercially available IrO2 catalyst of Reference Example 1 were prepared as follows. In the following, the MEA and PEM water electrolysis cell equipped with an anode catalyst layer containing the fiber catalysts of Examples 1 and 2 and the commercially available IrO2 catalyst of Reference Example 1 will be referred to as the MEA and PEM water electrolysis cell of Examples 1 and 2, and the MEA and PEM water electrolysis cell of Reference Example 1, respectively.
[0088] The MEA preparation conditions are summarized in Table 5. The fiber catalysts (fiber_1, fiber_2) of Examples 1 and 2 or a commercially available IrO2 catalyst were used as the anode catalyst material, and 46.5 wt% Pt / KB (TEC10E50E) manufactured by TKK was used as the cathode catalyst material. 5% Nafion as proton conductor (ionomer) in the catalyst layer (R) (SIGMA ALDRICH) as electrolyte membrane, and Nafion117 (Dupont TM ) was used to fabricate the MEA. The catalyst dispersion was prepared by weighing the anode and cathode catalyst powders into vials, and adding a small amount of ultrapure water, 99.5% ethanol, and 5% Nafion. The solid content of the dispersion was 5 wt% for the anode and 3 wt% for the cathode. The Nafion ratio was 15 wt% for the anode and 28 wt% for the cathode.
[0089] A stirring bar was placed in the vial containing the dispersion, and the mixture was stirred for 1 hour using a stirrer. To further disperse the mixture, the mixture was stirred for 30 minutes using an ultrasonic homogenizer under ice water cooling. The anode catalyst dispersion after stirring was placed in the sample tube of a catalyst spray printer, and 1 cm 2 The cathode catalyst dispersion was then sprayed onto the back of the Nafion electrolyte membrane in the same manner, and printed on both sides. The catalyst loading was 0.5 mg / cm for the anode catalyst layer. 2 , 0.3 mg / cm in the cathode catalyst layer 2 It was decided. After printing the catalyst on both sides of the electrolyte membrane, the Nafion ionomer in the catalyst layer was bonded to the Nafion electrolyte membrane by hot pressing at 0.82 kN for 190 seconds on a press table set to 132°C, which is near the glass transition temperature at which the Nafion electrolyte membrane softens.
[0090] [Table 5]
[0091] The PEM water electrolysis cell (single cell) had water-repellent carbon paper (GDL25BA, SGL CARBON JAPA LTD.) as the cathode current collector and Pt-coated Ti sintered compact (Nikko Techno) as the anode current collector on both sides of the MEA. A bipolar plate with a flow path (anode: titanium, cathode: carbon), power supply plate, insulating sheet, and clamping plate were placed on both electrodes in that order and fixed with bolts at a tightening pressure of 4 Nm. The cell was placed in an incubator (DKS300, Yamato Scientific Co., Ltd.), and water was fed from the flow channel ends on both sides of the cell at a flow rate of 5 mL / min using a liquid delivery pump (EHN-B11VC1R, Iwaki Co., Ltd.), with the opposite end of the flow channel set as the outlet. The temperature inside the furnace, including the cell and the flowing water, was set to 80°C. To ensure that the electrolyte membrane of the MEA was sufficiently hydrated, water was allowed to flow for 100 hours, after which a current of 0.2 A / cm was applied. 2When the fiber catalysts of Examples 1 and 2 were used as the anode catalyst layer, the voltage application conditioning shown in FIG.
[0092] 3-2. Initial performance evaluation The single cell power generation evaluation jig incorporating the PEM water electrolysis cells of Examples 1 and 2 and Reference Example was placed in a thermostatic chamber set to a cell temperature of 80° C., and electrochemical evaluation was carried out under the following conditions. (Anode conditions) Electrode area: 1cm 2 Pure water supply rate: 5mL / min (Cathode conditions) Electrode area: 1cm 2 Pure water supply rate: 5mL / min
[0093] FIG. 9 shows the IV characteristics of the PEM water electrolysis cells of Examples 1 and 2 and the Reference Example. As shown in FIG. 9, in terms of the IV characteristics, the PEM water electrolysis cell of Example 1 exhibited a higher current density at a given voltage value than the PEM water electrolysis cell of Example 2, and thus exhibited superior water electrolysis performance.
[0094] 3-3. Evaluation of potential cycle durability The potential cycle durability of the PEM water electrolysis cells of Examples 1 and 2 and Reference Example 1 was evaluated under potential cycle conditions simulating renewable energy as shown in FIG.
[0095] FIG. 11 shows the IV performance evaluation of the PEM water electrolysis cells of Examples 1 and 2 and Reference Example 1 before and after the durability test. 11 shows that after the durability test, the PEM water electrolysis cells of Examples 1 and 2 using the Ir / IrO2 fiber catalyst showed less performance degradation than the PEM water electrolysis cell of Reference Example 1 using the commercially available IrO2 catalyst. Therefore, it was confirmed that the use of the Ir / IrO2 fiber catalyst in the anode catalyst layer provides higher potential cycle durability than the use of the commercially available IrO2 catalyst (IrO2 particle aggregate) in the anode catalyst layer.
[0096] For a more detailed investigation, impedance measurements were performed before and after a durability test on each of the PEM water electrolysis cells of Examples 1 and 2 and Reference Example 1. The impedance measurement results were separated into activation overpotential, concentration overpotential, and ohmic overpotential, and the results are shown in Figures 12 to 14.
[0097] As shown in Figures 12(c), 13(c), and 14(c), the ohmic overvoltages of the PEM water electrolysis cells of Examples 1 and 2 and Reference Example 1 were due to resistance derived from the electrolyte membrane, and showed little change before and after the durability test. In addition, as shown in Figures 12(a), 13(a), and 14(a), the activation overvoltage of each PEM water electrolysis cell also showed little change before and after the durability test. On the other hand, as shown in Figures 12(b), 13(b), and 14(b), the concentration overpotential of the PEM water electrolysis cell of Reference Example 1 which used the commercially available IrO2 catalyst (IrO2 particle agglomerates) increased significantly after the durability test, whereas the increase was small in the PEM water electrolysis cells of Examples 1 and 2 which used the Ir / IrO2 fiber catalyst. From the above results, it was found that an increase in concentration overpotential in particular has a large effect on the deterioration of IV performance. It is known that immediately after the durability test, the reaction product gas accumulates in the catalyst layer, and if the gas is not properly discharged, the concentration overpotential increases. The PEM water electrolysis cells of Examples 1 and 2, which used the Ir / IrO2 fiber catalyst in the anode catalyst layer, suppressed the increase in concentration overpotential, suggesting the possibility that they have a structure that makes it easy to discharge the generated gas. [Industrial Applicability]
[0098] INDUSTRIAL APPLICABILITY The present invention provides a water electrolysis cell having an anode catalyst layer with improved durability, and is therefore industrially promising. [Explanation of symbols]
[0099] 1. Anode catalyst layer for water splitting cells 2. Ir / IrOx fiber catalyst 3. Proton-conducting electrolyte materials 4 Cathode 4a Cathode catalyst layer 4b Gas diffusion layer 5 Anode 5a Anode catalyst layer 5b Gas diffusion layer 6 Solid polymer electrolyte membrane 10 Membrane electrode assembly (MEA)
Claims
1. An anode catalyst layer for a water electrolysis cell, comprising an Ir / IrOx fiber catalyst made of metallic iridium (Ir) and iridium oxide (IrOx), and a proton-conductive electrolyte material.
2. 2. The anode catalyst layer for a water electrolysis cell according to claim 1, wherein the Ir / IrOx fiber catalyst has a fiber diameter of 20 to 300 nm and a fiber length of 0.3 to 5 μm.
3. 2. The anode catalyst layer for a water electrolysis cell according to claim 1, wherein the Ir(0) content in an analysis region near the surface of the Ir / IrOx fiber catalyst is 3 atomic % or more and 30 atomic % or less, as measured by X-ray photoelectron spectroscopy (XPS).
4. 4. A membrane electrode assembly comprising: a solid polymer electrolyte membrane; a cathode catalyst layer bonded to one side of the solid polymer electrolyte membrane; and an anode catalyst layer bonded to the other side of the solid polymer electrolyte membrane, wherein the anode catalyst layer is the anode catalyst layer for a water electrolysis cell according to claim 1.
5. A polymer electrolyte water electrolysis cell comprising the membrane electrode assembly according to claim 4.
6. The Ir / IrOx fiber catalyst is made of metallic iridium (Ir) and iridium oxide (IrOx), and has a fiber diameter of 20 to 300 nm and a fiber length of 0.3 to 5 μm.
7. 7. The Ir / IrOx fiber catalyst according to claim 6, wherein the content of Ir(0) in an analysis region near the surface as measured by X-ray photoelectron spectroscopy (XPS) is 3 atomic % or more and 30 atomic % or less.
8. A method for producing the Ir / IrOx fiber catalyst according to claim 6 or 7, comprising the steps of: A manufacturing method comprising the following steps (1) to (3). Step (1) preparing a mixed solution containing an iridium precursor compound and a thickening polymer Step (2) Electrospinning the mixed solution to obtain a precursor fiber Step (3) Heat-treating the precursor fiber obtained by electrospinning
Citation Information
Patent Citations
Preparation method of supported catalyst for PEM electrolyzed water
CN114657577A
Fibrous metal oxide catalyst
JP2007319839A
Composite body and method for producing composite body
JP2021143442A
Iridium and / or iridium oxide microsphere-based porous material, preparation method therefor, and uses thereof
US20200087164A1
Inorganic structure, device, and method for manufacturing inorganic structure
WO2019049996A1
Cited By
Carbon-coated iridium dioxide water electrolysis hydrogen production catalyst as well as preparation method and application thereof