Solid electrolyte material for fluorine ion battery and method for manufacturing the same
A solid electrolyte material for fluoride ion batteries, comprising lanthanide and alkaline earth metal atoms, addresses low conductivity issues by enhancing ionic conductivity through specific production methods, allowing broader temperature operation.
Patent Information
- Application Number
- JP2023077989
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Fluoride ion batteries suffer from low ionic conductivity at low temperatures due to the properties of their solid electrolytes, limiting their operational range.
A solid electrolyte material composed of a metal composite fluoride containing lanthanide and alkaline earth metal atoms, with specific infrared absorption characteristics and minimal carbon content, is produced through heat-treatment in the presence of a fluorine-containing substance to enhance ionic conductivity.
The material exhibits high ionic conductivity for fluoride ions, enabling improved performance across a wider temperature range.
Smart Images

Figure 2024162463000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a solid electrolyte material for a fluoride ion battery and a method for producing the same. [Background technology]
[0002] Fluoride ion solid-state batteries that utilize the reaction of fluoride ions are known as batteries with high voltage and high energy density. Fluoride ion batteries operate at high temperatures, for example, at 150°C or higher, but have the problem that they do not operate at low temperatures due to the low ionic conductivity of the solid electrolyte. In this regard, for example, Patent Document 1 proposes a solid electrolyte material with a Tysonite structure. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-77992 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of one aspect of the present disclosure is to provide a solid electrolyte material for a fluoride ion battery having high ionic conductivity of fluoride ions. [Means for solving the problem]
[0005] A first aspect of the present disclosure is a solid electrolyte material for a fluoride ion battery, which includes a metal complex fluoride containing a lanthanoid metal atom, an alkaline earth metal atom, and a fluorine atom. The metal complex fluoride has an infrared absorption spectrum of 400 cm -1 More than 450cm -1 3150 cm for the absorption maximum in the wavenumber range below -1 More than 3250cm -1 The ratio of the absorption maxima in the following wavenumber range is 0.10 or less:
[0006] A second aspect is a method for producing a solid electrolyte material for a fluoride ion battery, the method including: preparing a first complex metal fluoride containing a lanthanoid metal atom, an alkaline earth metal atom, and a fluorine atom; and heat-treating the first complex metal fluoride in the presence of a fluorine-containing substance to obtain a second complex metal fluoride. Effect of the Invention
[0007] According to one aspect of the present disclosure, it is possible to provide a solid electrolyte material for a fluoride ion battery having high ionic conductivity of fluoride ions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In this specification, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. Furthermore, the content of each component in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified, when multiple substances corresponding to each component are present in the composition. Furthermore, the upper and lower limits of the numerical ranges described in this specification can be arbitrarily selected and combined from the numerical values exemplified as the numerical ranges. Hereinafter, the embodiments of the present invention will be described in detail. However, the embodiments shown below are examples of solid electrolyte materials for fluoride ion batteries and methods for producing the same for embodying the technical ideas of the present invention, and the present invention is not limited to the solid electrolyte materials for fluoride ion batteries and methods for producing the same shown below.
[0009] Solid electrolyte materials for fluoride-ion batteries The solid electrolyte material for a fluoride ion battery (hereinafter, simply referred to as "solid electrolyte material") contains a metal complex fluoride containing a lanthanoid metal atom, an alkaline earth metal atom, and a fluorine atom. The metal complex fluoride constituting the solid electrolyte material has an infrared absorption spectrum of 400 cm -1 More than 450cm -1 3150 cm for the absorption maximum in the wavenumber range below -1 More than 3250cm -1The ratio of maximum absorption values in the following wave number ranges (hereinafter also referred to as "specific ratio") is 0.10 or less.
[0010] A solid electrolyte material containing a metal complex fluoride containing a lanthanide metal atom, an alkaline earth metal atom, and a fluorine atom exhibits a 3200 cm -1 The small absorption peak around 3200 cm indicates high fluoride ion conductivity. This can be considered as follows, for example. -1 The absorption peak around is considered to be an absorption peak derived from the stretching vibration of a hydroxyl group, for example. The small intensity of the absorption peak derived from the stretching vibration of a hydroxyl group is considered to mean that there are few defects of fluorine atoms in the metal composite fluoride constituting the solid electrolyte material, and therefore it is considered that high ionic conductivity of fluoride ions can be exhibited.
[0011] Metal complex fluorides containing lanthanide metal atoms, alkaline earth metal atoms, and fluorine atoms have a 400 cm -1 More than 450cm -1 In solid electrolyte materials, the absorption maximum of this strong absorption peak is based on the wave number range of 3150 cm -1 More than 3250cm -1 The absorption maxima in the wavenumber range below are evaluated: 400 cm for solid electrolyte materials -1 More than 450cm -1 3150 cm for the absorption maximum in the wavenumber range below -1 More than 3250cm -1 The ratio of the maximum absorption values in the following wave number ranges (specific ratio) may be 0.1 or less, 0.05 or less, 0.03 or less, or 0.02 or less. The specific ratio may be, for example, 0.001 or more, or 0.01 or more. The infrared absorption spectrum of the solid electrolyte material is measured by the attenuated total reflection method (ATR method) using a Fourier transform infrared spectrometer.
[0012] A solid electrolyte material having a specific ratio in a specific range exhibits high whiteness. *a * b * L in color space * The value of L in solid electrolyte materials can be used to evaluate the lightness. * The value of L may be, for example, 70 or more, 80 or more, 85 or more, or 90 or more. * a * b * L in color space * The value is measured using a spectrophotometer for pellets obtained by compacting the solid electrolyte material at 30 kN.
[0013] The solid electrolyte material may contain carbon atoms derived from its manufacturing method. The carbon atoms may be derived from an organic solvent used in the manufacturing method, carbon dioxide in the air, or the like. When the solid electrolyte material contains carbon atoms, the carbon content (hereinafter also referred to as "TC") may be, for example, 200 ppm or less, 150 ppm or less, 100 ppm or less, or 80 ppm or less. When the TC is less than the above-mentioned range, the fluoride ion conductivity tends to be improved due to the small amount of impurities. In addition, the carbon atom content (TC) may be, for example, 10 ppm or more, 20 ppm or more, or 30 ppm or more. The carbon atom content in the solid electrolyte material is measured by quantifying the carbon dioxide generated by the heat treatment using, for example, a CHN elemental analyzer.
[0014] The solid electrolyte material exhibits high ionic conductivity of fluoride ions. For example, the ionic conductivity of fluoride ions in the solid electrolyte material is 10 -7 (S / cm) or more, preferably 10 -6 (S / cm) or more, or 10 -5 (S / cm) or more. The ionic conductivity of the solid electrolyte material is measured by an AC impedance method using a high-frequency impedance measuring device.
[0015] The metal complex fluoride constituting the solid electrolyte material may include a fluorite structure containing fluorine atoms, lanthanoid metal atoms, and alkaline earth metal atoms. In general, the fluorite structure is an ionic crystal structure composed of alkaline earth metal ions and fluoride ions in a ratio of 1:2. In the fluorite structure of the metal complex fluoride, in addition to alkaline earth metal ions and fluoride ions, lanthanoid metal ions are solid-dissolved. The lanthanoid metal ions are solid-dissolved in the fluorite structure, thereby improving the ionic conductivity. For example, this can be considered as follows. The lanthanoid metal ions are solid-dissolved, so that the content ratio of fluoride ions in the fluorite structure increases, and fluoride ions are present at interstitial positions. This can be considered to be because the fluoride ions are conducted between the lattices by a conduction mechanism of quasi-interstitial diffusion, in which the fluoride ions present at the interstitial positions and the fluoride ions present at the normal sites are pushed out and move in a domino effect.
[0016] The metal complex fluoride constituting the solid electrolyte material may contain, in addition to lanthanoid metal atoms and alkaline earth metal atoms, an additional component capable of forming an additional ion having an ionic radius larger than that of an alkaline earth metal ion. When the metal complex fluoride contains an additional component, the metal complex fluoride may have a crystal structure (hereinafter also referred to as a "specific crystal structure") containing an additional ion having an ionic radius larger than that of an alkaline earth metal ion as a main phase in a fluorite structure containing fluoride ions, lanthanoid metal ions, and alkaline earth metal ions. This allows the metal complex fluoride to exhibit high ionic conductivity. This can be considered to be because, for example, the lattice constant of the crystal of the metal complex fluoride becomes large when an additional ion having an ionic radius larger than that of an alkaline earth metal ion is contained in the crystal structure, and therefore the movement of the fluoride ion responsible for ionic conduction within the crystal becomes easy.
[0017] When the metal composite fluoride contains the specific crystal structure as the main phase, the content of the specific crystal structure in the crystal phase of the metal composite fluoride may be, for example, 60 mol% or more.The content of the specific crystal structure in the crystal phase of the metal composite fluoride may be preferably 80 mol% or more, or 100 mol%.
[0018] The fact that the metal complex fluoride contains lanthanoid metal atoms, alkaline earth metal atoms, and additional components in its composition can be confirmed, including their content ratio, by, for example, subjecting the metal complex fluoride to inductively coupled plasma (ICP) emission spectrometry. Since the fluorite structure is generally an ionic crystal, the detection of lanthanoid metal atoms, alkaline earth metal atoms, and additional components by ICP emission spectrometry can be considered to indicate that they are present as ions in the crystal structure of the metal complex fluoride.
[0019] In the composition of the metal complex fluoride, the ratio of the number of moles of fluorine atoms to the total number of moles of lanthanoid metal atoms, alkaline earth metal atoms, and additional components (hereinafter also referred to as "total cation moles") may be more than 1.87 and less than 3. The ratio of the number of moles of fluorine atoms to the total number of moles of cations in the composition of the metal complex fluoride may be preferably 1.9 or more, or 2 or more, and more preferably may be more than 2. It may also be preferably 2.8 or less, or 2.6 or less, and more preferably 2.3 or less. When the ratio of the number of moles of fluorine atoms is within the above range, the ion conductivity tends to be further improved. The number of moles of fluorine atoms contained in the composition of the metal complex fluoride is calculated based on the amount of metal ions quantified by ICP atomic emission spectroscopy, taking into account the valence of each of the total number of moles of lanthanoid metal ions, alkaline earth metal ions, and additional ions as 1.
[0020] For example, the lanthanide metal ion La 3+ , the alkaline earth metal ion Ba 2+ and the adduct ion Cs +are detected in a molar ratio of 1:1:1. In this case, if the total number of moles of lanthanum ions, barium ions, and cesium ions is 1, the detected amounts of lanthanum ions, barium ions, and cesium ions are each 1 / 3 on a molar basis. If the valence of lanthanum ions is 3, the valence of barium ions is 2, and the valence of cesium ions is 1, the number of moles of fluoride ions contained in the composition of the metal complex fluoride is calculated to be (1 / 3) x 3 + (1 / 3) x 2 + (1 / 3) x 1 = 2.
[0021] Examples of lanthanoid metal atoms contained in the metal composite fluoride constituting the solid electrolyte material include lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), and samarium (Sm). The lanthanoid metal atoms preferably include at least lanthanum, and may further include cerium, samarium, and the like, and more preferably may include at least lanthanum. The ratio of the number of moles of lanthanum to the total number of moles of lanthanum metal atoms contained in the metal composite fluoride may be, for example, 0.5 or more, preferably 0.7 or more, or 0.9 or more. The ratio of the number of moles of lanthanum may be, for example, 1 or less.
[0022] The molar ratio of the lanthanoid metal atoms in the composition of the metal complex fluoride may be, for example, more than 0 and less than 0.8 relative to the total molar number of the lanthanoid metal atoms, the alkaline earth metal atoms and the additional components. The molar ratio of the lanthanoid metal atoms may be preferably 0.05 or more, or 0.1 or more, and may be preferably 0.6 or less, or 0.4 or less. When the molar ratio of the lanthanoid metal atoms is within the above range, the main phase of the metal complex fluoride can have a fluorite structure.
[0023] Examples of alkaline earth metal atoms contained in the metal complex fluoride constituting the solid electrolyte material include calcium (Ca), strontium (Sr), barium (Ba), etc. The alkaline earth metal atoms preferably contain at least barium, and may further contain strontium, calcium, etc., and more preferably may contain at least barium. The ratio of the number of moles of barium to the total number of moles of alkaline earth metal atoms contained in the metal complex fluoride may be, for example, 0.5 or more, preferably 0.7 or more, or 0.9 or more. The ratio of the number of moles of barium may be, for example, 1 or less.
[0024] The molar ratio of alkaline earth metal atoms in the composition of the metal complex fluoride may be, for example, 0.2 or more and less than 1 with respect to the total molar ratio of lanthanoid metal atoms, alkaline earth metal atoms and additional components. The molar ratio of alkaline earth metal atoms may be preferably 0.4 or more and 0.8 or less. When the molar ratio of alkaline earth metal atoms is within the above range, the main phase of the metal complex fluoride can have a fluorite structure.
[0025] The ratio of the number of moles of lanthanoid metal atoms to the number of moles of alkaline earth metal atoms in the composition of the metal complex fluoride may be, for example, more than 0 and not more than 4. The ratio of the number of moles of lanthanoid metal atoms to the number of moles of alkaline earth metal atoms may be preferably 0.1 or more, or 0.3 or more, and may be preferably 1.5 or less, or 1.0 or less.
[0026] The additional ions formed from the additional components contained in the metal composite fluoride may be dissolved in the crystal structure contained in the metal composite fluoride as a main phase, or may be distributed approximately uniformly throughout the crystal structure contained in the metal composite fluoride as a main phase. Here, the additional ions being dissolved in the crystal structure contained in the metal composite fluoride as a main phase means that a part of the cations constituting the crystal structure contained in the metal composite fluoride as a main phase is replaced with the additional ions.
[0027] The additional component contained in the metal complex fluoride may be one that can form a cation having an ionic radius larger than that of the alkaline earth metal ion that constitutes the fluorite structure contained in the metal complex fluoride. The cation formed from the additional component may be an inorganic ion such as a metal ion, or an organic cation. Here, the ionic radius of the cation can be a value known in the literature in the case of a metal ion. The ionic radius of the organic cation is calculated by a simulation calculation such as density functional theory (DFT). For example, the ionic radius of the tetramethylammonium ion calculated by this method is about 0.18 nm to 0.27 nm. Specific examples of the additional ion include inorganic ions such as cesium (Cs) ion, rubidium (Rb), and ammonium ion, and organic cations such as methylammonium ion, dimethylammonium ion, trimethylammonium ion, tetramethylammonium ion, ethylammonium ion, diethylammonium ion, triethylammonium ion, and tetraethylammonium ion. The adduct ion may include at least one selected from the group consisting of a cesium (Cs) ion, a methylammonium ion, a dimethylammonium ion, a trimethylammonium ion, a tetramethylammonium ion, an ethylammonium ion, a diethylammonium ion, a triethylammonium ion, and a tetraethylammonium ion, and preferably includes at least a cesium ion.
[0028] The ratio of the number of moles of cesium to the total number of moles of the additional components contained in the metal complex fluoride may be, for example, 0.5 or more, preferably 0.6 or more, 0.8 or more, or 0.98 or more. The ratio of the number of moles of cesium may be, for example, 1 or less.
[0029] The adduct ion has a larger ionic radius than the alkaline earth metal ion. The ratio of the ionic radius of the adduct ion to the ionic radius of the alkaline earth metal ion may be, for example, greater than 1 and not greater than 3. The ratio of the ionic radius of the adduct ion to the alkaline earth metal ion may preferably be 1.05 or more, or 1.1 or more, and may preferably be 2 or less.
[0030] The ratio of the number of moles of the additional component in the composition of the metal complex fluoride to the total number of moles of the lanthanoid metal atom, the alkaline earth metal atom, and the additional component may be, for example, more than 0 and less than 0.38. The ratio of the number of moles of the additional component may be preferably 0.05 or more, or 0.2 or more, and may be preferably 0.35 or less, or 0.3 or less.
[0031] The ratio of the number of moles of the additional component in the composition of the metal complex fluoride to the number of moles of the alkaline earth metal atom may be, for example, more than 0 and less than 1. The ratio of the number of moles of the additional component to the number of moles of the alkaline earth metal atom may be preferably 0.1 or more, or 0.4 or more, and preferably 0.9 or less, or 0.7 or less. The ratio of the number of moles of the additional component in the composition of the metal complex fluoride to the number of moles of the lanthanoid metal atom may be, for example, more than 0 and 1.5 or less. The ratio of the number of moles of the additional component to the number of moles of the lanthanoid metal atom may be preferably 0.1 or more, or 0.3 or more, and preferably 1.2 or less, or 1.0 or less.
[0032] The metal complex fluoride may have a composition represented by the following formula (1). Ln (1-x―y) M x A y F z (1)
[0033] In formula (1), Ln represents a lanthanoid metal atom, M represents an alkaline earth metal atom, and A represents an additional component. x, y, and z may satisfy 0 < x < 1, 0 < y < 1, 0 < x + y < 1, and 1.87 < z < 3. x and y may preferably satisfy 0.4 ≦ x < 1, 0.4 < x + y < 1, and 0 < y < 0.38. z may preferably satisfy 2 ≦ z ≦ 2.6. x and y may more preferably satisfy 0.4 ≦ x < 0.8, 0.4 < x + y < 1, and 0.05 < y ≦ 0.35. z may preferably satisfy 2 < z ≦ 2.3.
[0034] Further, the metal composite fluoride may have a composition represented by the following formula (1a). Ln (1-x―y) M x Cs y F z (1a)
[0035] In formula (1), Ln represents a lanthanoid metal atom, M represents an alkaline earth metal atom. x, y, and z may satisfy 0 < x < 1, 0 < y < 1, 0 < x + y < 1, and 1.87 < z < 3. x and y may preferably satisfy 0.4 ≦ x < 1, 0.4 < x + y < 1, and 0 < y < 0.38. z may preferably satisfy 2 ≦ z ≦ 2.6. x and y may more preferably satisfy 0.4 ≦ x < 0.8, 0.4 < x + y < 1, and 0.05 < y ≦ 0.35. z may preferably satisfy 2 < z ≦ 2.3.
[0036] Details of the lanthanoid metal component, alkaline earth metal component, and additional component in formulas (1) and (1a) are as described.
[0037] The solid electrolyte material may have peaks at positions such as 2θ=25.3°±1°, 29.3°±1°, 41.9°±1°, and 49.6°±1° in X-ray diffraction (XRD) measurement using CuKα radiation. Preferably, at least two of these peaks may be simultaneously present, more preferably at least three of these peaks may be simultaneously present, and even more preferably four of these peaks may be simultaneously present. By having peaks at the above positions, the solid electrolyte material can be considered to include a fluorite structure.
[0038] The volume average particle size of the solid electrolyte material may be, for example, 1 nm or more and 100 μm or less, and preferably 20 nm or more and 10 μm or less. The volume average particle size of the solid electrolyte material is determined as a particle size corresponding to 50% of the volume cumulative from the small diameter side in the volume-based cumulative particle size distribution. The volume-based cumulative particle size distribution is measured, for example, using a laser diffraction type particle size distribution measuring device.
[0039] Method for producing solid electrolyte material for fluoride ion batteries A method for producing a solid electrolyte material for a fluoride ion battery includes a first step of preparing a first complex metal fluoride containing a lanthanoid metal atom, an alkaline earth metal atom, and a fluorine atom, and a second step of heat-treating the first complex metal fluoride in the presence of a fluorine-containing substance to obtain a second complex metal fluoride. The solid electrolyte material may contain the second complex metal fluoride obtained in the second step, or may consist of the second complex metal fluoride.
[0040] By heat-treating the first metal complex fluoride in the presence of a fluorine-containing substance, for example, defects of fluorine atoms contained in the first metal complex fluoride are reduced, which makes it possible to achieve high ionic conductivity of fluoride ions when forming a fluoride ion battery.
[0041] 1st step In the first step, a first metal complex fluoride containing a lanthanoid metal atom, an alkaline earth metal atom and a fluorine atom is prepared. The first metal complex fluoride may be prepared by receiving it from another source, or may be prepared by manufacturing a first metal complex fluoride having a desired composition. The composition of the first metal complex fluoride to be prepared may be the same as that of the metal complex fluoride contained in the solid electrolyte material described above.
[0042] The first metal complex fluoride may be produced by, for example, a first production method as follows. The first production method of the first metal complex fluoride may include a preparation step of preparing a mixture containing a lanthanoid metal source and an alkaline earth metal source, and optionally containing an additional component, and a heat treatment step of heat treating the mixture at a predetermined temperature to obtain the first metal complex fluoride. The obtained first metal complex fluoride may have a crystal structure containing additional ions in a fluorite structure containing lanthanoid metal ions and alkaline earth metal ions as a main phase. In addition, the additional ions may have a larger ionic radius than the alkaline earth metal ions and may contain at least cesium ions. At least one of the lanthanoid metal source, the alkaline earth metal source, and the additional component may contain fluoride ions.
[0043] In the preparation step, a mixture containing a lanthanide metal source and an alkaline earth metal source and, if necessary, an additional component is prepared. The details of the lanthanide metal contained in the lanthanide metal source, the alkaline earth metal contained in the alkaline earth metal source, and the additional component are as described above.
[0044] In one embodiment, the lanthanoid metal source may include a lanthanoid metal fluoride, the alkaline earth metal source may include an alkaline earth metal fluoride, and the additional component may include an additional ion fluoride. The content ratio of the lanthanoid metal fluoride, the alkaline earth metal fluoride, and the additional ion fluoride in the mixture may be such that, when the content of the lanthanoid metal ion contained in the lanthanoid metal fluoride is pmol, the content of the alkaline earth metal ion contained in the alkaline earth metal fluoride is qmol, the content of the additional ion contained in the additional ion fluoride is rmol, and the valence of the additional ion is n, 1.87<(3p+2q+nr) / (p+q+r)<3 is satisfied. By containing the lanthanoid metal fluoride, alkaline earth metal fluoride, and fluoride of the additional ion in such a content ratio, the ratio of the number of moles of fluoride ions in the composition of the first metal complex fluoride obtained is more than 1.87 and less than 3 with respect to the total number of moles of the lanthanoid metal ion, alkaline earth metal ion, and additional ion. The (3p+2q+nr) / (p+q+r) may be preferably 1.9 or more, or 2 or more, and more preferably more than 2. It may also be preferably 2.8 or less, or 2.6 or less, and more preferably 2.3 or less.
[0045] In one embodiment, the mixture may have a composition in which the ratio of the number of moles of fluoride ions contained in the mixture is greater than 1.87 and less than 3, where the sum of the number of moles of lanthanoid metal atoms contained in the lanthanoid metal source, the number of moles of alkaline earth metal atoms contained in the alkaline earth metal source, and the number of moles of an additional component capable of forming an additional ion is 1. The ratio of the number of moles of fluoride ions in the mixture may be preferably 1.9 or more, or 2 or more, and more preferably greater than 2. It may also be preferably 2.8 or less, or 2.6 or less, and more preferably 2.3 or less.
[0046] The lanthanoid metal source contained in the mixture may be a lanthanoid metal fluoride, a lanthanoid metal chloride, a lanthanoid metal hydroxide, a lanthanoid metal oxide, or the like. The lanthanoid metal ion source may be a hydrate. The lanthanoid metal ion source may preferably contain at least a lanthanoid metal fluoride. The ratio of the number of moles of the lanthanoid metal fluoride to the total number of moles of the lanthanoid metal source may be, for example, 0.2 or more, preferably 0.8 or more, based on the number of moles of the lanthanoid metal. The ratio of the number of moles of the lanthanoid metal fluoride may be, for example, 1 or less.
[0047] The purity of the lanthanide metal source may be, for example, 50% or more, preferably 80% or more, and the purity of the lanthanide metal source may be, for example, 100% or less.
[0048] The alkaline earth metal source contained in the mixture may include alkaline earth metal fluoride, alkaline earth metal chloride, alkaline earth metal hydroxide, alkaline earth metal oxide, etc. The alkaline earth metal source may be a hydrate. The alkaline earth metal source may preferably include at least an alkaline earth metal fluoride. The ratio of the number of moles of the alkaline earth metal fluoride to the total number of moles of the alkaline earth metal source may be, for example, 0.2 or more, preferably 0.8 or more, based on the number of moles of the alkaline earth metal. The ratio of the number of moles of the alkaline earth metal fluoride may be, for example, 1 or less.
[0049] The purity of the alkaline earth metal source may be, for example, 50% or more, preferably 80% or more, and the purity of the alkaline earth metal source may be, for example, 100% or less.
[0050] Examples of the additional component contained in the mixture include fluorides of the additional ions, chlorides of the additional ions, hydroxides of the additional ions, and oxides of the additional ions. The additional component may be a hydrate. The additional component may preferably include at least fluorides of the additional ions. The ratio of the number of moles of the fluorides of the additional ions to the total number of moles of the additional component may be, for example, 0.2 or more, preferably 0.8 or more, based on the number of moles of the additional ions. The ratio of the number of moles of the fluorides of the additional ions may be, for example, 1 or less. The additional component may include cesium atoms, and the additional ions may be cesium ions.
[0051] The purity of the additional component may be, for example, 50% or more, preferably 80% or more, and may be, for example, 100% or less.
[0052] The mixing ratio of the lanthanoid metal source, alkaline earth metal source and additional component in the mixture may be, for example, a ratio of the number of moles of the lanthanoid metal atoms contained in the lanthanoid metal source to the total number of moles (total number of moles of cations) of the lanthanoid metal atoms contained in the lanthanoid metal source and the additional ions contained in the additional component, which is more than 0 and less than 0.8 moles. The ratio of the number of moles of the lanthanoid metal atoms to the total number of moles of cations may be preferably 0.05 or more, or 0.1 or more, and may be preferably 0.6 or less, or 0.4 or less. The ratio of the number of moles of the alkaline earth metal atoms to the total number of moles of cations may be, for example, 0.2 or more and less than 1. The ratio of the number of moles of the alkaline earth metal atoms to the total number of moles of cations may be preferably 0.4 or more, and may be preferably 0.8 or less. The ratio of the number of moles of the additional ions to the total number of moles of cations may be, for example, more than 0 and less than 0.38. The ratio of moles of added ions to moles of total cations may preferably be 0.05 or more, or 0.2 or more, and may preferably be 0.35 or less, or 0.3 or less.
[0053] The molar ratio of the content of lanthanoid metal atoms to alkaline earth metal atoms in the mixture may be, for example, greater than 0 and less than 4, or greater than 0 and less than 1.5. The molar ratio of the content of lanthanoid metal atoms to alkaline earth metal atoms may be preferably 0.1 or more, or 0.3 or more, and may be preferably 1.4 or less, 1.2 or less, or 1.0 or less.
[0054] The mixture can be prepared by weighing out the lanthanoid metal source, the alkaline earth metal source, and the additional components contained as necessary to a desired mixing ratio, and then mixing them by a mixing method using a ball mill or the like, or a mixing method using a mixer such as a Henschel mixer or a V-type blender. The mixing may be performed by dry mixing, or by adding a solvent or the like and then performing wet mixing. The mixture may be one that has been dried. The drying process may be performed by, for example, heat drying, reduced pressure drying, freeze drying, or the like, or may be performed in combination. The heat drying conditions may be, for example, 30°C to 200°C and 0.5 hours to 24 hours.
[0055] The mixture may be preferably a product of mechanical milling of a lanthanoid metal source, an alkaline earth metal source, and an optional additional component. That is, the mixture may be obtained by mixing a lanthanoid metal source, an alkaline earth metal source, and an optional additional component by mechanical milling. The mechanical milling may be performed using, for example, a planetary ball mill, a bead mill, a ball mill, a jet mill, or the like. The conditions of the mechanical milling may be, for example, 0.5 hours to 48 hours, preferably 5 hours to 24 hours, when a planetary ball mill is used.
[0056] In the heat treatment step, the mixture is heat-treated at a predetermined first heat treatment temperature to obtain a first metal complex fluoride. The first heat treatment temperature in the heat treatment step is, for example, 200° C. or more and 1000° C. or less, preferably 300° C. or more or 400° C. or more, and preferably 700° C. or less or 600° C. or less.
[0057] The heat treatment may include increasing the temperature to a predetermined first heat treatment temperature, maintaining the first heat treatment temperature, and decreasing the temperature from the first heat treatment temperature. The rate of temperature increase to the first heat treatment temperature may be, for example, from room temperature, 1° C. / min to 20° C. / min, preferably 5° C. / min or more, and preferably 10° C. / min or less. The heat treatment time for maintaining the first heat treatment temperature may be, for example, 1 hour or more, preferably 5 hours or more. The heat treatment time may be, for example, 48 hours or less, preferably 20 hours or less, or 10 hours or less. The rate of temperature decrease from the first heat treatment temperature may be, for example, from room temperature, 1° C. / min to 20° C. / min.
[0058] The atmosphere in the heat treatment step may be, for example, an inert gas atmosphere. Examples of the inert gas include nitrogen gas and rare gases such as argon. The inert gas atmosphere may have an inert gas content of, for example, 90% by volume or more, preferably 95% by volume or more or 98% by volume or more, and may be substantially 100% by volume of inert gas. Here, "substantially" means that the presence of gases other than the inert gas that are inevitably mixed in is not excluded. The content of gases other than the inert gas may be, for example, 1% by volume or less.
[0059] The pressure in the atmosphere in the heat treatment step may be, for example, 0 MPa or more and 1 MPa or less as a gauge pressure. The heat treatment of the mixture can be carried out using, for example, a tubular furnace, a hearth lifting furnace, or the like.
[0060] The first metal complex fluoride obtained by the heat treatment step may have a composition in which the ratio of the number of moles of lanthanoid metal atoms to the total number of moles of lanthanoid metal atoms, alkaline earth metal atoms, and additional ions is greater than 0 and less than 0.6, the ratio of the number of moles of alkaline earth metal atoms is 0.4 or more and less than 1.0, and the ratio of the number of moles of additional ions is greater than 0 and less than 0.38.
[0061] The first metal complex fluoride may be produced by a second production method as follows. The second production method of the first metal complex fluoride may include a precursor preparation step of preparing a precursor, and a precursor heat treatment step of heat treating the precursor to obtain the first metal complex fluoride. The obtained first metal complex fluoride may have a crystal structure containing additional ions in a fluorite structure containing lanthanoid metal ions and alkaline earth metal ions as a main phase. The additional ions may have a larger ionic radius than the alkaline earth metal ions, and may contain at least cesium ions.
[0062] In the precursor preparation step, a precursor is prepared that contains a lanthanoid metal atom, an alkaline earth metal atom, and a fluorine atom, and optionally contains additional ions. The details of the lanthanoid metal atom, the alkaline earth metal atom, and the additional ions are as described above.
[0063] The precursor containing lanthanoid metal atoms, alkaline earth metal atoms, and fluorine atoms can be prepared, for example, as follows. A first aqueous solution containing lanthanoid metal ions, a second aqueous solution containing alkaline earth metal ions, and a third aqueous solution containing fluoride ions can be mixed to prepare the precursor as a fluoride containing lanthanoid metal atoms and alkaline earth metal atoms. The precursor produced by mixing the first aqueous solution, the second aqueous solution, and the third aqueous solution can be collected by solid-liquid separation (e.g., filtration).
[0064] The mixing can be carried out, for example, by mixing a mixture of the first aqueous solution and the second aqueous solution with the third aqueous solution. Alternatively, the first aqueous solution and the second aqueous solution may be added to the third aqueous solution and mixed. The temperature during mixing may be, for example, 0°C or higher and 100°C or lower, and preferably 10°C or higher and 80°C or lower. The atmosphere during mixing may be, for example, an air atmosphere. The mixing time may be, for example, 1 hour or higher and 72 hours or lower, and preferably 10 hours or higher and 24 hours or lower. Here, the mixing time is the time from the time when the mixing ratio of each aqueous solution reaches a desired range to the time when the next treatment (for example, filtration treatment) is started.
[0065] The first aqueous solution may be an aqueous solution of a lanthanoid metal source. Examples of the lanthanoid metal source constituting the first aqueous solution include inorganic acid salts, acetates, oxalates, etc. of lanthanoid metals. Inorganic acid salts include nitrates, sulfates, halogenates, etc. The purity of the lanthanoid metal source may be, for example, 50% or more, and preferably 80% or more. The purity of the lanthanoid metal source may be, for example, 100% or less. The concentration of the lanthanoid metal ion in the first aqueous solution may be, for example, 1 mmol / kg or more and 1000 mol / kg or less, preferably 10 mmol / kg or more or 100 mmol / kg or more, and preferably 100 mol / kg or less or 10 mol / kg or less.
[0066] The second aqueous solution may be an aqueous solution of an alkaline earth metal source. Examples of the alkaline earth metal source constituting the second aqueous solution include inorganic acid salts, acetates, and oxalates of alkaline earth metals. Inorganic acid salts include nitrates, sulfates, and halogen acid salts. The purity of the alkaline earth metal source may be, for example, 50% or more, and preferably 80% or more. The purity of the alkaline earth metal source may be, for example, 100% or less. The concentration of alkaline earth metal ions in the aqueous solution of the alkaline earth metal source may be, for example, 1 mmol / kg or more and 1000 mol / kg or less, preferably 10 mmol / kg or more or 100 mmol / kg or more, and preferably 100 mol / kg or less or 10 mol / kg or less.
[0067] The third aqueous solution may be an aqueous solution of a fluoride ion source. Examples of the fluoride ion source constituting the third aqueous solution include ammonium fluoride, hydrofluoric acid, and methylammonium fluoride. The purity of the fluoride ion source may be, for example, 50% or more, and preferably 80% or more. The purity of the fluoride ion source may be, for example, 100% or less. The concentration of the fluoride ion in the aqueous solution containing fluoride ions may be, for example, 1 mmol / kg or more and 1000 mol / kg or less, preferably 10 mmol / kg or more, 100 mmol / kg or more, or 1 mol / kg or more, and preferably 100 mol / kg or less, or 50 mol / kg or less.
[0068] The mixing ratio of the first aqueous solution and the second aqueous solution in the precursor preparation step may be, for example, more than 0 and less than 4, or more than 0 and less than 1.5, as a molar ratio of lanthanoid metal ions contained in the second aqueous solution to alkaline earth metal ions contained in the first aqueous solution. The molar ratio of lanthanoid metal ions to alkaline earth metal ions may be preferably 0.1 or more, 0.3 or more, or 0.5 or more, and may be preferably 1.4 or less, 1.2 or less, 1.0 or less, or 0.8 or less. The mixing ratio of the third aqueous solution may be, for example, more than 0.8 and less than 5, and may be preferably 1.2 or more, 1.5 or more, or 3 or more, and may be 4.5 or less, or 4 or less, as a molar ratio of fluoride ions contained in the third aqueous solution to the total number of moles of lanthanoid metal ions and alkaline earth metal ions.
[0069] The precursor obtained by mixing the first aqueous solution, the second aqueous solution, and the third aqueous solution may be contained in a precipitate formed by mixing the first aqueous solution, the second aqueous solution, and the third aqueous solution. The precipitate containing the precursor can be recovered from the reaction mother liquor by solid-liquid separation. The precipitate obtained by solid-liquid separation may be subjected to a washing treatment. The washing treatment may be performed using a liquid medium containing, for example, water. The washing treatment may be performed, for example, by holding the precipitate in a funnel or the like and passing a liquid medium through it, or by performing solid-liquid separation of a mixture of the precipitate and the liquid medium. The washing treatment may be performed until the electrical conductivity of the liquid medium separated from the precipitate is, for example, 1 mS / cm or less, preferably 0.5 mS / cm or less, or 0.1 mS / cm or less.
[0070] The precursor containing a lanthanoid metal, an alkaline earth metal, and a fluorine atom obtained as described above may be subjected to a drying treatment. The drying treatment may be performed, for example, by heat treating the precursor. The temperature in the drying treatment may be, for example, 50°C or higher and 300°C or lower, and preferably 100°C or higher or 200°C or lower. The drying treatment may be performed under reduced pressure. When the drying treatment is performed under reduced pressure, the atmospheric pressure may be, for example, 10 Pa or lower, and preferably 0.01 Pa or lower.
[0071] The precursor may further contain additional ions derived from the additional component in addition to the lanthanoid metal, alkaline earth metal and fluorine atoms. The additional ions may contain at least cesium ions, and may be substantially cesium ions. The precursor containing additional ions can be prepared by mixing a fluoride containing a lanthanoid metal and an alkaline earth metal with an additional component that generates additional ions. Specifically, a precursor containing additional ions can be obtained by mixing a solution or dispersion of the additional component containing the additional component and a liquid medium with a fluoride containing a lanthanoid metal and an alkaline earth metal. At least a part of the liquid medium may be removed from the obtained precursor containing additional ions.
[0072] Examples of the additional component contained in the solution or dispersion include fluorides of the additional ions, chlorides of the additional ions, hydroxides of the additional ions, oxides of the additional ions, carbonates of the additional ions, and hydrides of the additional ions. The details of the additional component are as described above. The liquid medium constituting the solution or dispersion of the additional component may contain at least water, and may be substantially water. The liquid medium may also contain a liquid other than water. When the liquid medium contains a liquid other than water, examples of the liquid other than water include organic solvents such as alcohols having 1 to 8 carbon atoms, methanol, and ethanol. The content of the additional component in the solution or dispersion of the additional component may be, for example, 50% by mass or more and 99.99% by mass or less, and preferably 90% by mass or more and 99% by mass or less.
[0073] The mixing ratio of the fluoride containing a lanthanoid metal and an alkaline earth metal to the additional component may be, for example, 0.1 or more and 0.5 or less, and preferably 0.2 or more or 0.3 or less, as a molar ratio of the additional ion contained in the additional component to the fluoride containing a lanthanoid metal and an alkaline earth metal.
[0074] In addition, the mixing ratio of the fluoride containing a lanthanoid metal and an alkaline earth metal to the additional component may be appropriately set according to the composition of the precursor containing the desired additional ion. For example, when the additional component is a fluoride of an additional ion, the mixing ratio of the fluoride containing a lanthanoid metal and an alkaline earth metal to the fluoride of the additional ion may be a mixing ratio that satisfies 1.87<(3p+2q+nr) / (p+q+r)<3, where the content of the lanthanoid metal contained in the fluoride is pmol, the content of the alkaline earth metal ion is qmol, the content of the additional ion contained in the fluoride of the additional ion is rmol, and the valence of the additional ion is n. (3p+2q+nr) / (p+q+r) may be preferably 1.9 or more, or 2 or more, and more preferably more than 2. It may also be preferably 2.8 or less, or 2.6 or less, and more preferably 2.3 or less.
[0075] The content of the lanthanoid metal atom, alkaline earth metal atom and additional ion in the precursor containing the additional ion may be, for example, a ratio of the number of moles of the lanthanoid metal atom to the total number of moles of the lanthanoid metal atom, the alkaline earth metal atom and the additional ion (total number of moles of cations) is more than 0 and less than 0.8 moles. The ratio of the number of moles of the lanthanoid metal atom to the total number of moles of cations may be preferably 0.05 or more, or 0.1 or more, and may be preferably 0.6 or less, or 0.4 or less. The ratio of the number of moles of the alkaline earth metal atom to the total number of moles of cations may be, for example, 0.2 or more and less than 1. The ratio of the number of moles of the alkaline earth metal atom to the total number of moles of cations may be preferably 0.4 or more, and may be preferably 0.8 or less. The ratio of the number of moles of the additional ion to the total number of moles of cations may be, for example, more than 0 and less than 0.38. The ratio of moles of added ions to moles of total cations may preferably be 0.05 or more, or 0.2 or more, and may preferably be 0.35 or less, or 0.3 or less.
[0076] The precursor obtained as above can be heat-treated to obtain the first metal complex fluoride. The temperature of the heat treatment of the precursor (hereinafter also referred to as the second heat treatment temperature) is, for example, 200°C or higher and 1000°C or lower, preferably 300°C or higher, 400°C or higher, or 500°C or higher, and preferably 800°C or lower, or 700°C or lower.
[0077] The heat treatment of the precursor may include increasing the temperature to a predetermined second heat treatment temperature, maintaining the second heat treatment temperature, and decreasing the temperature from the second heat treatment temperature. The rate of temperature increase to the second heat treatment temperature may be, for example, from room temperature, 1° C. / min to 20° C. / min, preferably 5° C. / min or more, and preferably 10° C. / min or less. The heat treatment time for maintaining the second heat treatment temperature may be, for example, 1 hour or more, preferably 5 hours or more. The heat treatment time may be, for example, 48 hours or less, preferably 20 hours or less, or 15 hours or less. The rate of temperature decrease from the second heat treatment temperature may be, for example, from room temperature, 1° C. / min to 20° C. / min.
[0078] The atmosphere in the heat treatment of the precursor may be, for example, an inert gas atmosphere. Examples of the inert gas include rare gases such as nitrogen gas and argon. The inert gas atmosphere may have an inert gas content of, for example, 90% by volume or more, preferably 95% by volume or more or 98% by volume or more, and may be substantially 100% by volume of inert gas. Here, "substantially" means that the presence of gases other than the inert gas that are inevitably mixed in is not excluded. The content of gases other than the inert gas may be, for example, 1% by volume or less.
[0079] The atmosphere in the heat treatment of the precursor may contain a fluorine-containing substance. In this case, effects such as reduction of fluorine atom deficiency in the crystal structure and reduction of impurities are expected. Examples of the fluorine-containing substance in the heat treatment atmosphere include F2, CHF3, CF4, PF3, PH5, BF3, NH4HF2, HF, SiF4, AsF3, KrF4, XeF2, XeF4, NF3, SF4, C2F6, C3F8, SiF4, SF6, CFC, HCFC, HFC, C2F4, C2F6, C3F8, and NOF. When the atmosphere in the heat treatment of the precursor contains a fluorine-containing substance, the concentration of the fluorine-containing substance in the atmosphere may be, for example, 3% by volume or more and 35% by volume or less, preferably 5% by volume or more or 10% by volume or more, and preferably 30% by volume or less or 25% by volume or less. Furthermore, when the atmosphere in the heat treatment of the precursor contains a fluorine-containing substance, the method for producing a solid electrolyte material for a fluoride ion battery may or may not include the second step described below.
[0080] The pressure in the atmosphere for the heat treatment of the precursor may be, for example, 0 MPa or more and 1 MPa or less as a gauge pressure. The heat treatment of the mixture can be carried out using, for example, a tubular furnace, a hearth lifting furnace, or the like.
[0081] The first metal complex fluoride obtained by heat treatment of the precursor may have a composition in which the ratio of the number of moles of lanthanoid metal atoms to the total number of moles of lanthanoid metal atoms, alkaline earth metal atoms, and additional ions is greater than 0 and less than 0.6, the ratio of the number of moles of alkaline earth metal atoms is 0.4 or more and less than 1.0, and the ratio of the number of moles of additional ions is greater than 0 and less than 0.38.
[0082] 2nd process In the second step, the first metal complex fluoride is heat-treated in the presence of a fluorine-containing substance to obtain a second metal complex fluoride. In the second step, the first metal complex fluoride may be heat-treated in contact with the fluorine-containing substance to obtain a second metal complex fluoride. The obtained second metal complex fluoride may be the desired solid electrolyte material.
[0083] It is believed that by heat-treating the first metal complex fluoride in contact with a fluorine-containing compound, fluorine atoms are supplied to the region in the crystal structure of the first metal complex fluoride where fluorine atoms are insufficient, and a second metal complex fluoride having fewer defects in the crystal structure can be obtained. This makes it possible to achieve high ionic conductivity of fluoride ions in the solid electrolyte material. It is also believed that the durability of the solid electrolyte material is improved.
[0084] The fluorine-containing substance used in the second step may be in a solid, liquid or gaseous state at room temperature. Examples of fluorine-containing substances in a solid or liquid state include NH4F. Examples of fluorine-containing substances in a gaseous state include F2, CHF3, CF4, PF3, PH5, BF3, NH4HF2, HF, SiF4, AsF3, KrF4, XeF2, XeF4, NF3, SF4, C2F6, C3F8, SiF4, SF6, CFC, HCFC, HFC, C2F4, C2F6, C3F8, NOF, etc. The fluorine-containing substance may include at least one selected from the group consisting of F2, CHF3, CF4, NH4HF2, HF, SiF4, KrF2, XeF2, XeF4 and NF3, and may preferably include at least one selected from the group consisting of F2 and HF.
[0085] When the fluorine-containing substance is in a solid or liquid state at room temperature, the first metal complex fluoride can be mixed with the fluorine-containing substance to bring them into contact with each other. The first metal complex fluoride may be mixed with the fluorine-containing substance in an amount of 1% by mass to 20% by mass, preferably 2% by mass to 10% by mass, calculated as the mass of fluorine atoms, relative to 100% by mass of the total amount of the first metal complex fluoride and the fluorine-containing substance.
[0086] The temperature at which the first metal complex fluoride and the fluorine-containing substance are mixed may be, for example, 20° C. or higher and lower than 400° C., and more preferably 150° C. or higher. When the temperature at which the first metal complex fluoride is contacted with the fluorine-containing substance in a solid or liquid state at room temperature is 20° C. or higher and lower than 200° C., the first metal complex fluoride may be contacted with the fluorine-containing substance and then heat-treated at a temperature of 200° C. or higher in the second step.
[0087] When the fluorine-containing substance is a gas, the first metal complex fluoride may be placed in an atmosphere containing the fluorine-containing substance and contacted with the fluorine-containing substance. The atmosphere containing the fluorine-containing substance may contain an inert gas such as a rare gas or nitrogen in addition to the fluorine-containing substance. In this case, the concentration of the fluorine-containing substance in the atmosphere may be, for example, 3% by volume or more and 35% by volume or less, preferably 5% by volume or more or 10% by volume or more, and preferably 30% by volume or less or 25% by volume or less.
[0088] The heat treatment in the second step may be performed by maintaining the third heat treatment temperature for a predetermined time while the first metal complex fluoride is in contact with the fluorine-containing substance. The third heat treatment temperature may be, for example, 100° C. or more and 650° C. or less, and may be preferably 400° C. or more, 425° C. or more, 450° C. or more, or 480° C. or more. The third heat treatment temperature may be preferably less than 600° C., 580° C. or less, 550° C. or less, or 520° C. or less.
[0089] When the third heat treatment temperature is equal to or higher than the lower limit, fluorine atoms are sufficiently supplied to the first metal complex fluoride, and the ionic conductivity of the fluoride ions in the obtained solid electrolyte material tends to be improved. When the third heat treatment temperature is equal to or lower than the upper limit, decomposition of the obtained first metal complex fluoride is more effectively suppressed, and the ionic conductivity of the fluoride ions in the obtained solid electrolyte material tends to be improved.
[0090] The heat treatment time in the heat treatment of the second step, i.e., the time for holding the third heat treatment temperature, may be, for example, 1 hour or more and 40 hours or less, preferably 2 hours or more or 3 hours or more, and preferably 30 hours or less, 10 hours or less, or 8 hours or less. If the heat treatment time at the third heat treatment temperature is within the above range, fluorine atoms can be sufficiently supplied to the first metal complex fluoride after contact with the liquid medium. This tends to make the crystal structure of the second metal complex fluoride more stable, and to obtain a solid electrolyte material with high ionic conductivity of fluoride ions.
[0091] The pressure in the heat treatment of the second step may be atmospheric pressure (0.101 MPa), or may be higher than atmospheric pressure but not higher than 5 MPa, or may be higher than atmospheric pressure but not higher than 1 MPa.
[0092] The method for producing a solid electrolyte material may include a sizing step in which the second metal composite fluoride obtained after the second step is subjected to a combination of crushing, grinding, classification, etc. The sizing step can provide a powder having a desired particle size.
[0093] The invention according to the present disclosure may include, for example, the following aspects. [1] A metal complex fluoride containing a lanthanoid metal atom, an alkaline earth metal atom and a fluorine atom, the metal complex fluoride having an infrared absorption spectrum of 400 cm -1 More than 450cm -1 3150 cm for the absorption maximum in the wavenumber range below -1 More than 3250cm -1 A solid electrolyte material for a fluoride ion battery, having a ratio of absorption maxima in the following wave number range of 0.10 or less:
[0094] [2] The solid electrolyte material according to [1], wherein the metal complex fluoride further contains cesium atoms.
[0095] [3] The metal complex fluoride has a molar ratio of the lanthanoid metal atom, the alkaline earth metal atom, and the cesium atom to the total molar number of the lanthanoid metal atom, the alkaline earth metal atom, and the cesium atom, The molar ratio of the lanthanoid metal atoms is more than 0 and less than 0.6, the molar ratio of the alkaline earth metal atoms is 0.4 or more and less than 1.0, and the molar ratio of the cesium atoms is more than 0 and less than 0.38. The solid electrolyte material according to [2] having such a composition.
[0096] [4] The metal composite fluoride is L * a * b * in the color space, and the value of L * is 70 or more. The solid electrolyte material according to any one of [1] to [3].
[0097] [5] The metal composite fluoride has a total carbon content of 200 ppm or less. The solid electrolyte material according to any one of [1] to [4].
[0098] [6] The metal composite fluoride has a composition represented by the following formula (1). The solid electrolyte material according to any one of [1] to [5]. Ln (1-x―y) M x Cs y F z (1) (In formula (1), Ln represents a lanthanoid metal atom, and M represents an alkaline earth metal atom. x, y, and z satisfy 0 < x < 1, 0 ≤ y < 1, 0 < x + y < 1, and 1.87 < z < 3)
[0099] [7] In the formula (1), x and y satisfy 0.4 ≤ x < 1, 0.4 < x + y < 1, and 0 < y < 0.38. The solid electrolyte material according to [6].
[0100] [8] Preparing a first metal composite fluoride containing a lanthanoid metal atom, an alkaline earth metal atom, and a fluorine atom, and heat-treating the first metal composite fluoride in the presence of a fluorine-containing substance to obtain a second metal composite fluoride. A method for producing a solid electrolyte material for a fluoride ion battery, including this.
[0101] [9] The method for producing the first metal complex fluoride according to [8], wherein the ratio of the content of the lanthanide metal atoms to the content of the alkaline earth metal atoms is greater than 0 and is not greater than 1.5.
[0102]
[10] The method according to [8] or [9], wherein the first metal complex fluoride further contains a cesium atom.
[0103]
[11] The first metal complex fluoride has a molar ratio of the lanthanoid metal atom, the alkaline earth metal atom, and the cesium atom to the total molar number of the lanthanoid metal atom, the alkaline earth metal atom, and the cesium atom, the ratio of the number of moles of the lanthanide metal atoms is greater than 0 and less than 0.6; The ratio of the mole numbers of the alkaline earth metal atoms is 0.4 or more and less than 1.0, The manufacturing method according to
[10] , wherein the ratio of the molar numbers of the cesium atoms is greater than 0 and less than 0.38.
[0104]
[12] The manufacturing method according to any one of [8] to
[11] , wherein the heat treatment in obtaining the second metal complex fluoride is carried out at a temperature in the range of 100°C or higher and 650°C or lower.
[0105]
[13] The method of any of [8] to
[12] , wherein the fluorine-containing substance comprises at least one selected from the group consisting of F2, CHF3, CF4, NH4HF2, HF, SiF4, KrF2, XeF2, XeF4 and NF3. EXAMPLES
[0106] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0107] Example 1 Composite fluoride manufacturing process The complex fluorides were prepared as follows: Barium nitrate (Ba(NO3)2), lanthanum nitrate (La(NO3)3·6H2O), and ammonium fluoride (NH4F) were added to 1 kg of pure water, respectively, and dissolved by stirring in an air atmosphere at room temperature to prepare a 0.2 mol / kg barium nitrate aqueous solution, a 1 mol / kg lanthanum nitrate aqueous solution, and a 10 mol / kg ammonium fluoride aqueous solution, respectively.
[0108] 600 g of a barium nitrate aqueous solution (0.2 mol / kg) and 80 g of a lanthanum nitrate aqueous solution (1 mol / kg) were added to a reaction vessel and mixed at room temperature under an air atmosphere. Then, 72 g of an ammonium fluoride aqueous solution (10 mol / kg) was added and stirred for 20 hours.
[0109] The reaction solution was filtered, and the filtered material was washed with pure water until the electrical conductivity of the filtrate was 0.1 mS / cm or less to obtain a precipitate. The precipitate was heat-treated at 120°C under vacuum for 12 hours to obtain a precursor of the first metal complex fluoride. The Ba:La composition ratio of the obtained precursor was confirmed to be Ba:La=0.6:0.4 by ICP analysis.
[0110] A dispersion of 1.92 g of cesium fluoride (CsF) dispersed in 0.1 g of water was added to 9.28 g of the precursor of the first metal complex fluoride obtained above, mixed, and then heat-treated at 200°C for 6 hours to dry it out, and further heat-treated at 600°C for 10 hours in an argon atmosphere to obtain the first metal complex fluoride. The composition of the first metal complex fluoride was Ba, CsF ... 0.48 La 0.32 Cs 0.2 F 2.12 It was.
[0111] The first metal complex fluoride obtained above was placed in a tubular furnace and heat-treated at 500°C for 8 hours in an atmosphere of 20% by volume of fluorine gas and 80% by volume of nitrogen gas to obtain a second metal complex fluoride, which is a solid electrolyte material according to Example 1.
[0112] Comparative Example 1 The first complex metal fluoride obtained in Example 1 was used as a solid electrolyte material according to Comparative Example 1.
[0113] Composition analysis The composition of the solid electrolyte material obtained above was determined by inductively coupled plasma (ICP) atomic emission spectrometry. Specifically, as a pretreatment method, the solid electrolyte material was melted in an alkali, then heated and dissolved in hydrochloric acid, and the composition amount of metal ions was measured using an inductively coupled plasma (ICP) atomic emission spectrometry analyzer (ICP-AES; Optima8300: manufactured by Perkin Elmer), and the molar ratio of fluoride ions in the composition was determined by setting the total composition amount of metal ions to 1. The results are shown in Table 1.
[0114] Ionic Conductivity Measurement A solid electrolyte layer sample was prepared from the solid electrolyte material obtained above as follows: 200 mg of the solid electrolyte material was weighed out and pressed at 380 MPa to obtain a solid electrolyte layer sample.
[0115] The solid electrolyte layer sample obtained above was measured by an AC impedance method (measurement temperature: 25°C, applied voltage: 500mV, measurement frequency range: 120MHz to 20Hz) using a high frequency impedance measurement system (Keysight impedance analyzer E4990A type), and the ionic conductivity of fluoride ions was calculated from the thickness of the solid electrolyte layer sample and the resistance value on the real axis of the Cole-Cole plot. The results are shown in Table 1.
[0116] Lightness measurement The solid electrolyte material obtained above was pressed at 30 kN to produce a green compact having a diameter of 10 mm and a thickness of 22 mm. The L * The value (brightness) was measured, and the results are shown in Table 1.
[0117] Infrared absorption spectrum The solid electrolyte material thus obtained was subjected to infrared absorption spectroscopy using a Fourier transform infrared spectrometer (product name: NicoletiS50, manufactured by Thermo Fisher Scientific) by the ATR method, and the infrared absorption spectrum was measured at 400 cm -1 More than 450cm -1 3150 cm for the absorption maximum in the wavenumber range below -1 More than 3250cm -1 The ratio of the maximum absorption values in the following wave number ranges (specific ratio) was calculated. The results are shown in Table 1. The infrared absorption spectrum using ATR-IR had a wave number resolution of 4.0 cm -1 The measurement was performed with the cumulative number of times set to 32.
[0118] 1 g of the solid electrolyte material was precisely weighed out and heat-treated at 900°C in an air atmosphere using a CHN elemental analyzer. The amount of carbon dioxide generated was quantified to determine the mass ratio of carbon contained in the sample as total carbon content (TC; ppm). The results are shown in Table 1.
[0119] [Table 1]
[0120] As shown in Table 1, the solid electrolyte material according to Example 1 exhibits high ionic conductivity.
Claims
1. A metal complex fluoride containing a lanthanide metal atom, an alkaline earth metal atom and a fluorine atom, The metal complex fluoride has an infrared absorption spectrum of 400 cm -1 More than 450cm -1 3150 cm for the absorption maximum in the wavenumber range -1 More than 3250cm -1 A solid electrolyte material for a fluoride ion battery, having a ratio of absorption maxima in the following wave number range of 0.10 or less:
2. The solid electrolyte material according to claim 1 , wherein the metal complex fluoride further contains cesium atoms.
3. The metal complex fluoride is L * a * b * L in color space * The solid electrolyte material according to claim 1 or 2, wherein the value of
4. The solid electrolyte material according to claim 1 or 2, wherein the metal composite fluoride has a total carbon content of 200 ppm or less.
5. The metal complex fluoride has a molar ratio of the lanthanoid metal atom, the alkaline earth metal atom, and the cesium atom to the total molar number of the lanthanoid metal atom, the alkaline earth metal atom, and the cesium atom, the ratio of the number of moles of the lanthanide metal atoms is greater than 0 and less than 0.6; the ratio of the number of moles of the alkaline earth metal atoms is 0.4 or more and less than 1.0; The solid electrolyte material according to claim 2 , having a composition in which the ratio of the number of moles of cesium atoms is greater than 0 and less than 0.
38.
6. The solid electrolyte material according to claim 1 , wherein the metal complex fluoride has a composition represented by the following formula (1): Ln (1-x―y) M x Cs y F z (1) (In formula (1), Ln represents a lanthanoid metal atom, M represents an alkaline earth metal atom, and x, y, and z satisfy 0<x<1, 0≦y<1, 0<x+y<1, and 1.87<z<3.)
7. The solid electrolyte material according to claim 6, wherein x and y in the formula (1) satisfy 0.4≦x<1, 0.4<x+y<1, and 0<y<0.
38.
8. Providing a first metal complex fluoride containing a lanthanide metal atom, an alkaline earth metal atom, and a fluorine atom; and heat-treating the first complex metal fluoride in the presence of a fluorine-containing substance to obtain a second complex metal fluoride.
9. The method according to claim 8 , wherein the first metal complex fluoride has a composition in which the ratio of the content of the lanthanoid metal atoms to the content of the alkaline earth metal atoms is greater than 0 and is not greater than 1.
5.
10. The method according to claim 8 , wherein the first metal complex fluoride further contains cesium atoms.
11. The first metal complex fluoride has a molar ratio of the lanthanoid metal atom, the alkaline earth metal atom, and the cesium atom to the total molar number of the lanthanoid metal atom, the alkaline earth metal atom, and the cesium atom, the ratio of the number of moles of the lanthanide metal atoms is greater than 0 and less than 0.6; the ratio of the number of moles of the alkaline earth metal atoms is 0.4 or more and less than 1.0; The method according to claim 10, wherein the composition has a ratio of the number of moles of cesium atoms that is greater than 0 and less than 0.
38.
12. The method according to claim 8 , wherein the heat treatment for obtaining the second complex metal fluoride is carried out at a temperature in the range of 100° C. or more and 650° C. or less.
13. The fluorine-containing material is F 2 , C.H.F. 3 , C.F. 4 , N.H. 4 H.F. 2 , HF, SiF 4 , KrF 2 , XeF 2 , XeF 4 and N.F. 3 The method according to any one of claims 8 to 11, further comprising at least one selected from the group consisting of:
Citation Information
Patent Citations
Solid electrolyte material, solid electrolyte layer, fluoride ion battery, and method for manufacturing the same
JP2018077992A