Polyurethane elastic fiber, fabric containing the same, and sanitary material

By using non-metal pigments and ultraviolet absorbers, the polyurethane elastic fibers achieve enhanced resistance to discoloration and fading from light, sweat, and NOx gas, addressing the color fastness issues in existing technologies.

JP2024162504APending Publication Date: 2024-11-21ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023078061
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Polyurethane elastic fibers suffer from insufficient color fastness, leading to discoloration and fading due to light, temperature, humidity, and NOx gas exposure, which are not adequately addressed in existing technologies.

Method used

Incorporating pigments that do not contain metal components, specifically insoluble azo pigments, condensed azo pigments, and condensed polycyclic pigments, into the polyurethane elastic fibers, along with a benzotriazole ultraviolet absorber, to enhance resistance to discoloration and fading.

Benefits of technology

The solution provides polyurethane elastic fibers with improved resistance to discoloration and fading from environmental factors, ensuring stable color retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162504000001
    Figure 2024162504000001
  • Figure 2024162504000002
    Figure 2024162504000002
  • Figure 2024162504000003
    Figure 2024162504000003
Patent Text Reader

Abstract

To provide a polyurethane elastic fiber in a color other than black, which is hardly causing discoloration and fading due to exposure to light, sweat and NOx gas (i.e., which has an excellent discoloration resistant property).SOLUTION: There are provided a polyurethane elastic fiber containing a pigment (excluding black pigments) that does not contain a metal component, and a fabric and a sanitary material such as a diaper or a sanitary product, which contain the polyurethane elastic fibers.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyurethane elastic fiber, and a fabric and a sanitary material containing the same. [Background technology]

[0002] Polyurethane elastic fibers are highly stretchable and have excellent elastic properties, and taking advantage of these properties, they are widely used in hygiene materials such as innerwear, masks, sportswear, and diapers. In particular, in hygiene materials, colored fibers have been used in recent years to make it easier to distinguish the type and size.

[0003] Known methods for obtaining colored fibers include a post-dyeing method in which the fibers are dyed with a dye after they have been made into fibers, and a direct dyeing method in which a pigment is added to a spinning dope and then the fibers are made into fibers.

[0004] An example of the post-dyeing method is disclosed in Patent Document 1 below.

[0005] Moreover, an example of the original dyeing method is disclosed in the following Patent Document 2. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-95162 A [Patent Document 2] JP 2006-63461 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the polyurethane elastic fiber disclosed in Patent Document 1 has drawbacks in that it has insufficient color fastness, and the pigment is easily removed due to light, temperature, and humidity, causing discoloration and fading. Furthermore, Patent Document 2 does not mention discoloration or fading due to exposure to light, sweat, or NOx gas after fiberization, which are important when using polyurethane elastic fibers in practice, and does not disclose dope-dyed yarns in colors other than black.

[0008] In view of the problems of the prior art described above, the problem to be solved by the present invention is to provide a polyurethane elastic fiber in a color other than black that is resistant to discoloration and fading due to exposure to light, sweat, and NOx gas (i.e., has excellent discoloration resistance). [Means for solving the problem]

[0009] As a result of intensive research and repeated experiments in order to solve the above-mentioned problems, the inventors of the present application unexpectedly discovered that the above-mentioned problems can be solved by a polyurethane elastic fiber containing a pigment that does not contain a metal component (excluding black pigments), or containing at least one pigment (excluding black pigments) selected from the group consisting of insoluble azo pigments, condensed azo pigments, and condensed polycyclic pigments, and thus completed the present invention.

[0010] That is, the present invention is as follows. [1] A polyurethane elastic fiber characterized by containing a pigment that does not contain metal components (excluding black pigments). [2] The polyurethane elastic fiber according to [1] above, wherein the pigment not containing a metal component is at least one selected from the group consisting of an insoluble azo pigment, a condensed azo pigment, and a condensed polycyclic pigment. [3] A polyurethane elastic fiber comprising at least one pigment selected from the group consisting of insoluble azo pigments, condensed azo pigments, and condensed polycyclic pigments (excluding black pigments). [4] The pigment containing no metal component, or at least one pigment selected from the group consisting of an insoluble azo pigment, a condensed azo pigment, and a condensed polycyclic pigment, is represented by the following general formula (1): [ka] Or the following general formula (2): [ka] The polyurethane elastic fiber according to any one of the above [1] to [3], comprising a compound represented by the following formula: {In general formulas (1) and (2), Y1 to Y7 are a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, an alkoxy group, a hydroxyl group, a phenyl group, a phenoxy group, a phenoxycarbonyl group, an alkoxycarbonyl group, a carbamoyl group, an alkylamide group, a phenylamide group, or a halogenated alkyl group.} [5] The polyurethane elastic fiber according to any one of [1] to [4] above, wherein the pigment not containing a metal component, or the at least one pigment selected from the group consisting of an insoluble azo pigment, a condensed azo pigment, and a condensed polycyclic pigment, is at least one selected from the group consisting of CI Pigment Yellow 93, 94, 95, 128, and 166, and CI Pigment Red 139, 144, 166, 214, 220, 221, 242, 248, and 262. [6] The polyurethane elastic fiber according to any one of [1] to [5] above, wherein the pigment not containing a metal component, or at least one pigment selected from the group consisting of insoluble azo pigments, condensed azo pigments, and condensed polycyclic pigments, has a particle size (D50) at which the cumulative volume frequency is 50% in a particle size distribution measured in DMAc by a wet particle size distribution meter, of 10 μm or less. [7] The polyurethane elastic fiber according to any one of [1] to [6] above, wherein the content of the pigment not containing a metal component, or at least one pigment selected from the group consisting of an insoluble azo pigment, a condensed azo pigment, and a condensed polycyclic pigment, is 0.01 to 5 parts by mass per 100 parts by mass of the polyurethane elastic fiber. [8] The polyurethane elastic fiber according to any one of [1] to [7] above, further comprising 0.01 to 5 parts by mass of an ultraviolet absorbing agent per 100 parts by mass of the polyurethane elastic fiber. [9] The polyurethane elastic fiber according to [8], wherein the ultraviolet absorber is a benzotriazole-based ultraviolet absorber.

[10] A fabric comprising the polyurethane elastic fiber according to any one of [1] to [9] above.

[11] A sanitary material comprising the polyurethane elastic fiber according to any one of [1] to [9] above.

[12] The sanitary material according to

[11] above, which is a diaper or a sanitary product. Effect of the Invention

[0011] According to the present invention, it is possible to provide polyurethane elastic fibers in colors other than black that are resistant to discoloration and fading due to environmental factors such as exposure to light, sweat, and NOx gas. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and can be practiced in various modifications within the scope of the present invention.

[0013] One embodiment of the present invention is a polyurethane elastic fiber that contains a pigment that does not contain a metal component (excluding black pigments). By containing a pigment that does not contain a metal component, the metal component in the pigment does not undergo chemical reactions such as chelate formation, and discoloration or fading of the polyurethane elastic fiber due to exposure to light, sweat, and NOx gas can be suppressed.

[0014] A pigment that does not contain metal components is one that does not contain a metal element (metal element or metal ion) in its structural formula, or one that does not carry a metal.

[0015] The pigment that does not contain metal components is preferably at least one pigment selected from the group consisting of insoluble azo pigments, condensed azo pigments, and condensed polycyclic pigments (excluding black pigments), because such pigments have excellent chemical resistance and resistance to discoloration due to light.

[0016] The insoluble azo pigment refers to an azo compound that does not have a water-soluble substituent such as a sulfonic acid group, a carboxylic acid group, or a hydroxyl group. Specific examples of the insoluble azo pigment include CI Pigment Red 1, 3, 4, 5, 6, 7, 8, 9, 10, 12, 14, 15, 17, 18, 22, 23, 31, 112, 114, 146, 147, 150, 170, 171, 175, 176, 185, 208, and 238.

[0017] The condensed azo pigment is an insoluble disazo pigment, such as one containing a polar group or one with a large molecular weight due to a condensation reaction. Specific examples of the condensed azo pigment include CI Pigment Yellow 93, 94, and 95, and CI Pigment Red 144, 166, 214, 220, 221, 242, 248, and 262.

[0018] The condensed polycyclic pigment is a pigment having an aromatic ring structure consisting of a benzene ring or a heterocycle. Specific examples of the condensed polycyclic pigment include CI Pigment Orange 40, 43, and 51, CI Pigment Red 88, 122, 123, 149, 168, 177, 178, 179, 190, 194, 206, 207, and 209, and CI Pigment Violet 19, 36, and 38.

[0019] Another embodiment of the present invention is a polyurethane elastic fiber comprising at least one pigment selected from the group consisting of insoluble azo pigments, condensed azo pigments, and condensed polycyclic pigments, excluding black pigments.

[0020] The at least one pigment selected from the group consisting of insoluble azo pigments, condensed azo pigments, and condensed polycyclic pigments has particularly excellent solvent resistance and chemical resistance, and is therefore preferably represented by the following general formula (1) or (2): [ka] [ka] In the general formulas (1) and (2), Y1 to Y7 are a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, an alkoxy group, a hydroxyl group, a phenyl group, a phenoxy group, a phenoxycarbonyl group, an alkoxycarbonyl group, a carbamoyl group, an alkylamide group, a phenylamide group, or a halogenated alkyl group.

[0021] Specific examples of the pigment represented by general formula (1) include CI Pigment Brown 23, and CI Pigment Red 144, 166, 221, 242, 248, and 262.

[0022] Specific examples of the pigment represented by formula (2) include CI Pigment Orange 31 and CI Pigment Red 139.

[0023] In general formulas (1) and (2), the groups represented by Y1 to Y7 are preferably each independently a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, a hydroxy group, an alkoxycarbonyl group, or a halogenated alkyl group, and among these, from the viewpoint of compatibility with and dispersibility in a polyurethane polymer, a hydrogen atom, a fluorine atom, a chlorine atom, a hydroxy group, an alkoxycarbonyl group having 2 to 6 carbon atoms, or a fluorinated alkyl group having 1 to 3 carbon atoms is more preferable. Specific examples of pigments in which the groups represented by Y1 to Y7 in general formulas (1) and (2) are each independently a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, a hydroxy group, an alkoxycarbonyl group, or a halogenated alkyl group include CI Pigment Brown 23, CI Pigment Orange 31, and CI Pigment Red 139, 144, 166, 221, 242, 248, and 262. Specific examples of pigments in which the groups represented by Y1 to Y7 in general formulas (1) and (2) are each independently a hydrogen atom, a fluorine atom, a chlorine atom, a hydroxy group, an alkoxycarbonyl group having 2 to 6 carbon atoms, or a fluorinated alkyl group having 1 to 3 carbon atoms include CI Pigment Orange 31, and CI Pigment Red 139, 144, 166, 221, and 242.

[0024] From the viewpoint of exhibiting better discoloration resistance and fading resistance, the polyurethane elastic fiber of the present embodiment preferably contains at least one selected from the group consisting of CI Pigment Yellow 93, 94, 95, 128, and 166, and CI Pigment Red 139, 144, 166, 214, 220, 221, 242, 248, and 262, more preferably contains at least one selected from the group consisting of CI Pigment Red 139, 144, 166, 214, 220, 221, 242, 248, and 262, and particularly preferably contains CI Pigment Red 166.

[0025] The polyurethane elastic fiber of the present embodiment is a fiber obtained by spinning a polyurethane polymer. The polyurethane polymer is obtained by adopting a known urethanization reaction technique in which a prepolymer obtained by reacting a high molecular weight polyol with a diisocyanate is subjected to a chain extension reaction with a polyfunctional active hydrogen-containing compound as a chain extender.

[0026] Examples of the polymer polyol include various diols consisting of homopolymers or copolymers, such as polyether diols, polyester diols, polycarbonate diols, polyacryl diols, polythioester diols, polyester amide diols, mixtures thereof, and copolymers thereof, and polyether diols are preferred.

[0027] The number average molecular weight calculated from the hydroxyl value of the polymer polyol is preferably 1000 or more, and more preferably 1500 or more, in order to provide excellent stretchability of the polyurethane elastic fiber. On the other hand, from the viewpoint of the heat resistance and abrasion resistance of the finished yarn, it is preferably 3000 or less, and more preferably 2500 or less.

[0028] The diisocyanate may be an aliphatic, alicyclic, or aromatic diisocyanate having two isocyanate groups in the molecule, such as 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, a mixture thereof, or a copolymer thereof.

[0029] From the viewpoint of obtaining a uniform polyurethane polymer with little gel, the molar ratio of the diisocyanate to the polymer polyol (diisocyanate / polymer polyol) is preferably 1.80 or less, and more preferably 1.70 or less.

[0030] Examples of the polyfunctional active hydrogen-containing compound that is the chain extender include low molecular weight diamines and low molecular weight diols, which may be used alone or in combination.

[0031] Examples of the terminal terminator having a monofunctional active hydrogen atom include dialkylamines and monoalcohols, and these terminal terminators may be used alone or in combination.

[0032] Regarding the synthesis of polyurethane polymers, when synthesizing a urethane prepolymer consisting of a high molecular weight polyol and a diisocyanate, or when reacting the urethane prepolymer with an active hydrogen-containing compound, an organic solvent such as dimethylformamide, dimethylacetamide (DMAc), dimethylsulfoxide, etc. can be used, and dimethylacetamide (DMAc) is preferred.

[0033] The polyurethane polymer may contain various stabilizers, etc. For example, antioxidants such as hindered phenols and benzotriazoles, metal soaps such as magnesium stearate, various drugs, inorganic substances such as zinc oxide and titanium oxide, antibacterial agents and deodorants containing silver, zinc, or compounds thereof, antistatic agents, nitrogen oxide scavengers, thermal oxidation stabilizers, light stabilizers, etc. may be used in combination.

[0034] The polyurethane elastic fiber of the present embodiment can be produced by forming a polyurethane polymer into a fibrous form by known methods such as dry spinning, wet spinning, and melt spinning.

[0035] The polyurethane elastic fiber of the present embodiment may contain any lubricant and surface treatment agent in order to reduce the resistance during unwinding and the friction during use. The method for applying the lubricant and surface treatment agent is not particularly limited, and examples of the method include a method in which the lubricant and surface treatment agent are applied to the yarn by a chasing roller or the like before winding the yarn around a yarn tube during spinning.

[0036] Examples of lubricants and surface treatment agents include, but are not limited to, silicone-based oils such as dimethyl silicone, mineral oils, etc., which may be applied alone or in any combination.

[0037] From the viewpoints of suppressing filter clogging and aggregation, and suppressing uneven color development by improving dispersibility in the yarn, the pigment preferably has a particle size D50 measured by a particle size distribution meter of 10 μm or less, more preferably 8 μm or less, and even more preferably 5 μm or less.

[0038] The pigment content is preferably 0.01 parts by mass or more, more preferably 0.03 parts by mass or more, even more preferably 0.05 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 1 part by mass or less, relative to 100 parts by mass of the polyurethane elastic fiber. If the pigment content is 0.01 parts by mass or more, the color developability is sufficient, and the color is easily visible when used in fabrics, sanitary materials, etc. On the other hand, if the pigment content is 5 parts by mass or less, it is easy to obtain a yarn in which the pigment is uniformly dispersed.

[0039] The polyurethane elastic fiber of the present embodiment preferably further contains an ultraviolet absorbing agent in an amount of 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass, per 100 parts by mass of the polyurethane elastic fiber. If the content of the ultraviolet absorbing agent is 0.01 parts by mass or more, the yarn can exhibit sufficient resistance to embrittlement and yellowing caused by ultraviolet rays. On the other hand, if the content of the ultraviolet absorbing agent is 5 parts by mass or less, yarn breakage during spinning is less likely to occur.

[0040] The ultraviolet absorbing agent is a compound having the effect of absorbing light having a wavelength of about 200 to 400 nm, converting it into energy such as heat or infrared rays, and releasing it. Specifically, examples of inorganic ultraviolet absorbing agents include metal oxide fine particles such as titanium dioxide, cerium oxide, thallium oxide, lead oxide, and zirconium oxide. Examples of organic ultraviolet absorbing agents include ultraviolet absorbing agents based on benzotriazole, triazine, benzoxazine, salicylic acid ester, diphenylmethanone, anthranilate, cinnamic acid derivative, resorcinol, oxalinide, and coumarin derivative.

[0041] From the viewpoints of heat resistance of the yarn, compatibility with the spinning dope, and weather (light) stability, the ultraviolet absorbing agent is more preferably a benzotriazole-based ultraviolet absorbing agent.

[0042] The polyurethane elastic fiber of the present embodiment can be used as a bare yarn, or as a textured yarn covered with other fibers, entangled with other fibers, or twisted with other fibers, and can be interwoven or woven with other fibers to obtain a high-quality fabric without unevenness. Examples of the other fibers include natural fibers such as cotton, silk, and wool, polyamide fibers such as nylon 6 and nylon 66, polyester fibers such as polyethylene terephthalate, polytrimethylene terephthalate, and polytetramethylene terephthalate, cationic dyeable polyester fibers, cuprammonium regenerated rayon, viscose rayon, and acetate rayon.

[0043] The fabric of the present embodiment can be used for applications such as swimwear, girdles, brassieres, tights, pantyhose, waistbands, body suits, spats, sportswear, stretch outerwear, medical wear, and stretch linings.

[0044] The polyurethane elastic fiber of the present embodiment has good smoothness and little variation in frictional properties, and therefore, when used in sanitary materials such as diapers and sanitary napkins, high productivity and product stability can be obtained. EXAMPLES

[0045] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. The present invention also includes polyurethane elastic fibers isolated from products such as clothing and sanitary materials.

[0046] (1) Identification of pigments in polyurethane elastic fibers The polyurethane elastic fiber is dissolved in dimethylacetamide (DMAc), the resulting solution is centrifuged to separate the residue, and the residue is collected by filtration to isolate the pigment. The isolated pigment is subjected to pyrolysis GC / MS measurement, and the chemical composition of the pigment contained in the polyurethane elastic fiber is identified by comparing the obtained chromatogram with a database.

[0047] (2) Particle size at which the cumulative volume frequency is 50% (D50) in particle size distribution measured by a wet particle size distribution analyzer in DMAc Weigh out 0.1 g of pigment, add 49.9 g of dimethylacetamide (DMAc), and stir at room temperature for 24 hours to prepare a 0.2% by mass pigment dispersion. Using the prepared pigment dispersion, measure with a Beckman Coulter LS13320 (wet laser diffraction scattering particle size distribution analyzer, equipped with PIDS) by setting the dispersion solvent refractive index to 1.439. Inject the sample so that the relative intensity of the detector is in the range of 7 to 12%. In the particle size distribution chart obtained by this measurement, calculate the particle diameter (D50) at which the cumulative volume frequency is 50%.

[0048] (3) Evaluation method for color development As an index of color development, a spectrophotometer CM-5 (manufactured by Konica Minolta) was used with a D65 light source to measure the color difference ΔEab between the polyurethane elastic fiber (pigment-containing yarn) of each Example and Comparative Example and a polyurethane elastic fiber (pigment-free yarn) prepared in the same manner as each Example and Comparative Example except that no pigment was added, and the color difference ΔEab was calculated using the following formula: ΔEab={(L of pigmented yarn-L of non-pigmented yarn) 2 + (a for pigmented yarn - a for non-pigmented yarn) 2 + (b for pigmented yarn - b for non-pigmented yarn) 2} 1 / 2 {In the formula, the L value is a value that indicates brightness, and values ​​closer to 0 indicate black and values ​​closer to 100 indicate white. The a value indicates green to red, with negative values ​​indicating green and positive values ​​indicating red. The b value indicates blue to yellow, with negative values ​​indicating blue and positive values ​​indicating yellow.} The larger the ΔEab value, the greater the color change relative to the pigment-free yarn, meaning that the color development of the polyurethane elastic fiber is good. A ΔEab value of 10 or more is preferred.

[0049] (4) Evaluation method for color fastness against NOx gas, light exposure, and sweat As an index showing the degree of discoloration and fading, a spectrophotometer CM-5 (manufactured by Konica Minolta) and a D65 light source were used to measure the color difference ΔEab before and after each test described below using the following formula: ΔEab = {(L after test - L before test) 2 + (a after the test - a before the test) 2 + (b after test - b before test) 2} 1 / 2 {In the formula, the L value is a value that indicates brightness, and values ​​closer to 0 indicate black and values ​​closer to 100 indicate white. The a value indicates green to red, with negative values ​​indicating green and positive values ​​indicating red. The b value indicates blue to yellow, with negative values ​​indicating blue and positive values ​​indicating yellow.} The smaller the ΔEab value, the smaller the color change before and after the test and the better the resistance to discoloration and fading. A ΔEab value of 3 or less is preferred.

[0050] <NOx Exposure Test> For polyurethane elastic fibers, in accordance with JIS L 0855, the exposure test in a nitrogen oxide gas atmosphere was repeated 3 times until the standard dyed fabric reached the specified color change and fading grade.

[0051] <UV Irradiation Test> For polyurethane elastic fibers, ultraviolet rays were irradiated for 24 hours with a UV fade meter U48AU (manufactured by Suga Test Instruments Co., Ltd.).

[0052] <Sweat Immersion Test> After immersing 200 mg of polyurethane elastic fibers in 50 mL of artificial sweat S (acidic) (manufactured by Hayashi Pure Chemical Industries, Ltd., SDS code: Z8-15), they were taken out and stored at room temperature for 2 weeks.

[0053] (5) Spinning Stability Evaluation Using a spinning machine, spinning was carried out for 24 hours under the conditions described in the following examples and comparative examples. No thread breakage occurred, and the spinning pressure fluctuation per spinning die pack was 5 kg / cm 2 Those with the following conditions were judged to have good spinning stability.

[0054] [Example 1] 2000 g of polytetramethylene ether glycol with a number average molecular weight of 1800 and 445 g of 4,4'-diphenylmethane diisocyanate were reacted under stirring at 60°C for 3 hours in a dry nitrogen atmosphere to obtain a polyurethane prepolymer capped with isocyanate at the ends. After cooling this to room temperature, dimethylacetamide was added and dissolved to obtain a polyurethane prepolymer solution. On the other hand, a solution prepared by dissolving 38 g of ethylenediamine and 6 g of diethylamine in dry dimethylacetamide was added to the prepolymer solution at room temperature to obtain a polyurethane urea solution with a polyurethane solid content concentration of 30% by mass and a viscosity of 450 Pa·s (30°C).

[0055] The content in the polyurethane elastic fiber was 0.3 parts by mass of CI Pigment Red 168 as a pigment, 0.5 parts by mass of 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole as an ultraviolet absorber, and 1.0 parts by mass of 4,4'-butylidenebis(3-methyl-6-t-butylphenol) as an antioxidant, relative to 100 parts by mass of polyurethane elastic fiber, and dimethylacetamide was added thereto and dispersed with a homomixer to prepare a 15% by mass dispersion. This dispersion was mixed with the above-mentioned polyurethane urea solution to make a uniform solution, and then degassed at room temperature under reduced pressure to obtain a spinning stock solution. This spinning dope was dry spun using a spinning nozzle pack consisting of two circular holes at a winding speed of 800 m / min and a hot air temperature of 300°C, and the fibers were bundled using a false twisting device using compressed air. 3.0 parts by mass of a surface treatment agent was then applied to 100 parts by mass of polyurethane elastic fiber, and the fibers were wound around a paper tube to obtain a wound package of polyurethane elastic fiber of 22 dtex / 2 filaments. The surface treatment agent used was an oil solution consisting of 67% by mass of polydimethylsiloxane, 30% by mass of mineral oil, and 3.0% by mass of amino-modified silicone.

[0056] [Example 2] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Red 214.

[0057] [Example 3] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Red 166.

[0058] [Example 4] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Orange 5 so that the pigment content was 0.05 parts by mass per 100 parts by mass of the polyurethane elastic fiber.

[0059] [Example 5] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Yellow 93 and the pigment content was 3.0 parts by mass per 100 parts by mass of the polyurethane elastic fiber.

[0060] [Example 6] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the content of the ultraviolet absorbing agent was 0.1 part by mass per 100 parts by mass of the polyurethane elastic fiber.

[0061] [Example 7] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Brown 32 and the content of the ultraviolet absorbing agent was changed to 4.5 parts by mass per 100 parts by mass of the polyurethane elastic fiber.

[0062] [Example 8] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Red 144 so that the pigment content was 0.009 parts by mass per 100 parts by mass of the polyurethane elastic fiber.

[0063] [Example 9] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the content of the ultraviolet absorbing agent was 0.5 parts by mass per 100 parts by mass of the polyurethane elastic fiber.

[0064] [Comparative Example 1] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Red 48-2.

[0065] [Comparative Example 2] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Red 48-1.

[0066] [Comparative Example 3] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Red 48-4.

[0067] [Comparative Example 4] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Red 57-1 and the content of the ultraviolet absorbing agent was changed to 5.5 parts by mass per 100 parts by mass of the polyurethane elastic fiber.

[0068] [Comparative Example 5] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Red 48-2 and the pigment content was 0.006 parts by mass per 100 parts by mass of the polyurethane elastic fiber.

[0069] [Comparative Example 6] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Red 48-2 so that the pigment content was 0.01 parts by mass per 100 parts by mass of the polyurethane elastic fiber, and no ultraviolet absorber was added.

[0070] [Comparative Example 7] A polyurethane elastic fiber was obtained in the same manner as in Example 1, except that the pigment was changed to CI Pigment Orange 17.

[0071] The production conditions in the above-mentioned examples and comparative examples, and the various evaluation and analysis results of the obtained polyurethane elastic fibers are shown in Table 1 below.

[0072] [Table 1]

[0073] It can be seen from Table 1 that the polyurethane elastic fibers of Examples 1 to 9 have excellent resistance to discoloration and fading due to exposure to light, sweat, and NOx gas. [Industrial Applicability]

[0074] Use of the polyurethane elastic fiber according to the present invention can suppress discoloration and fading of the polyurethane elastic fiber, enabling the production of products with stable color tones. Therefore, the polyurethane elastic fiber according to the present invention can be suitably used for disposable diapers, swimwear, tights, pantyhose, sock fasteners, elastic cuffs, corsets, disposable diapers, bandages, innerwear, outerwear, legwear, sportswear, jeans, and other sanitary materials, etc.

Claims

1. A polyurethane elastic fiber containing a pigment that does not contain a metal component (excluding black pigments).

2. The polyurethane elastic fiber according to claim 1 , wherein the pigment not containing a metal component is at least one selected from the group consisting of an insoluble azo pigment, a condensed azo pigment, and a condensed polycyclic pigment.

3. A polyurethane elastic fiber comprising at least one pigment (excluding black pigments) selected from the group consisting of insoluble azo pigments, condensed azo pigments, and condensed polycyclic pigments.

4. The pigment containing no metal component, or at least one pigment selected from the group consisting of an insoluble azo pigment, a condensed azo pigment, and a condensed polycyclic pigment, is represented by the following general formula (1): [Formula 1] Or the following general formula (2): [Case 2] In the general formulas (1) and (2), Y 1 ~Y 7 is a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, an alkoxy group, a hydroxyl group, a phenyl group, a phenoxy group, a phenoxycarbonyl group, an alkoxycarbonyl group, a carbamoyl group, an alkylamide group, a phenylamide group, or a halogenated alkyl group.

5. The polyurethane elastic fiber according to any one of claims 1 to 3, wherein the pigment not containing a metal component, or the at least one pigment selected from the group consisting of an insoluble azo pigment, a condensed azo pigment, and a condensed polycyclic pigment, is at least one selected from the group consisting of C.I. Pigment Yellow 93, 94, 95, 128, and 166, and C.I. Pigment Red 139, 144, 166, 214, 220, 221, 242, 248, and 262.

6. 4. The polyurethane elastic fiber according to claim 1, wherein the pigment containing no metal component or at least one pigment selected from the group consisting of insoluble azo pigments, condensed azo pigments, and condensed polycyclic pigments has a particle size distribution in DMAc measured by a wet particle size distribution meter, the particle size distribution being 50% by cumulative volume (D50) of 10 μm or less.

7. 4. The polyurethane elastic fiber according to claim 1, wherein the content of the pigment not containing a metal component, or at least one pigment selected from the group consisting of an insoluble azo pigment, a condensed azo pigment, and a condensed polycyclic pigment, is 0.01 to 5 parts by mass per 100 parts by mass of the polyurethane elastic fiber.

8. The polyurethane elastic fiber according to any one of claims 1 to 3, further comprising 0.01 to 5 parts by mass of an ultraviolet absorbing agent per 100 parts by mass of the polyurethane elastic fiber.

9. The polyurethane elastic fiber according to claim 8 , wherein the ultraviolet absorbing agent is a benzotriazole-based ultraviolet absorbing agent.

10. A fabric comprising the polyurethane elastic fiber according to any one of claims 1 to 3.

11. A sanitary material comprising the polyurethane elastic fiber according to any one of claims 1 to 3.

12. The sanitary material according to claim 11, which is a diaper or a sanitary product.

Citation Information

Patent Citations

  • High-speed vapor deposition method

    JP1988000461A

  • JP95162A