Bolometer-type infrared detector and method of manufacturing the same

A laminated structure with protective films shields carbon nanotubes in infrared detectors from environmental factors, ensuring stable operation by minimizing resistance fluctuations.

JP2024162607APending Publication Date: 2024-11-21NEC CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023078294
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Carbon nanotubes used as heat-sensitive elements in bolometer-type infrared detectors are susceptible to resistance changes due to external environmental factors like oxygen and moisture, leading to unstable operation.

Method used

A laminated structure comprising a first protective film, a light reflective film, and a second protective film is applied to the heat-sensitive element, with the first protective film made of metal oxide or nitride, polyimide, or acrylic resin, and the second protective film made of similar materials, to shield the element from environmental influences.

Benefits of technology

The laminated structure effectively stabilizes the resistance value of the heat-sensitive element, allowing the detector to operate reliably in both atmospheric and vacuum conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162607000001_ABST
    Figure 2024162607000001_ABST
Patent Text Reader

Abstract

To provide a bolometer-type infrared detector that has a resistance value hardly affected by an external environment, and also operates stably.SOLUTION: A bolometer type infrared detector has a lamination structure provided with a first protective film, a light reflective film, and a second protective film in this order on a photosensitive element, wherein: the first protective film is made of at least one or more selected from a group consisting of a metal oxide film, a metal nitride film, polyimide, acryl resin, and fluororesin; the light reflective film is a metal film; and the second protective film is made of at least one or more selected from the group consisting of a metal oxide film, a metal nitride film, polyimide, acryl resin, and fluororesin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a bolometer type infrared detector and a method for manufacturing the same. [Background technology]

[0002] In recent years, there has been an increasing demand for infrared detectors for the purpose of detecting heat, measuring the concentration of carbon dioxide and air pollutants, etc. A non-cooled infrared detector using the bolometer method changes the temperature of the light receiving part by absorbing incident infrared rays, and detects the radiation intensity of the infrared rays as an electrical signal from the change in resistance value caused by the temperature change of the material placed on the light receiving part, and has a variety of applications as an inexpensive infrared detector.

[0003] Currently, vanadium oxide, amorphous silicon, etc. are mainly used as the heat-sensing element of a bolometer (Patent Document 1). In addition, the use of carbon nanotubes (CNTs), which have a high absolute value of the temperature dependence of resistance change (temperature coefficient of resistance (TCR)), as the heat-sensing element of a bolometer is also being considered (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 09-257565 [Patent Document 2] JP 2015-49207 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above-mentioned thermal sensing elements, particularly CNTs, have the problem that their resistance value is easily affected by the external environment due to being electrically doped by oxygen and moisture in the air (resistance changes are likely to be caused by factors other than temperature changes), making their operation as a detector unstable.

[0006] In view of the above-mentioned problems, an object of the present invention is to provide a bolometer-type infrared detector whose resistance value is less susceptible to the external environment and which operates stably, and a method for manufacturing the same. [Means for solving the problem]

[0007] In order to achieve the above object, one embodiment of the present invention comprises: The present invention relates to a bolometer-type infrared detector having a laminated structure in which a first protective film, a light-reflecting film, and a second protective film are provided in that order on a thermal sensitive element, the first protective film being made of at least one selected from the group consisting of a metal oxide film, a metal nitride film, a polyimide, an acrylic resin, and a fluororesin, the light-reflecting film being a metal film, and the second protective film being made of at least one selected from the group consisting of a metal oxide film, a metal nitride film, a polyimide, an acrylic resin, and a fluororesin.

[0008] Also, another embodiment of the present invention is Providing a substrate having an insulating surface; forming a thermal element support layer on the substrate; forming a thermal element on the thermal element support layer; forming an electrode pair on the thermal sensitive element; forming a first protective film on the thermal element; forming a light reflecting film on the first protective film; forming a second protective film on the light reflecting film; The present invention relates to a method for manufacturing a bolometer type infrared detector, comprising the steps of: Effect of the Invention

[0009] According to the present invention, it is possible to provide a bolometer-type infrared detector whose resistance value is less susceptible to the external environment and which operates stably, and a method for manufacturing the same. [Brief description of the drawings]

[0010] [Figure 1]FIG. 1A is a cross-sectional view showing an outline of the structure of an infrared detector according to a first embodiment of the present invention, and FIG. 1B is a plan view showing an outline of the structure of an infrared detector according to the first embodiment of the present invention. [Diagram 2] FIG. 2A is a cross-sectional view showing the structure of the infrared detector of Example 1, and FIG. 2B is a cross-sectional view showing the structure of the infrared detector of Comparative Example 1. [Diagram 3] FIG. 3 is a graph showing the change in current value in air and in vacuum when 1 V is applied to the infrared detectors of Example 1 and Comparative Example 1. [Figure 4] FIG. 4 is a graph showing the current reduction rates of the infrared detectors of Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In the following embodiments, parts that are the same or equivalent to each other will be denoted by the same reference numerals.

[0012] <Bolometer type infrared detector> The present invention has discovered that the influence of the external environment on the thermal element can be reduced by optimizing the structure of the protective layer of the thermal element in an infrared detector. The bolometer-type infrared detector of the present invention has a laminated structure in which a first protective film, a light reflective film, and a second protective film are provided in this order on the thermal element.

[0013] An embodiment of the infrared detector of the present invention will be described with reference to FIG. 1. As shown in FIG. 1, in the infrared detector 10 of this embodiment, a heat-sensitive element support layer 16 is formed on a substrate having an insulating surface (a heat insulating layer 14, for example, an insulating film, is formed on the surface of a substrate 12), and a heat-sensitive element 22 is formed on the heat-sensitive element support layer 16. An electrode pair 24 is formed on the heat-sensitive element 22 at intervals, and each of the electrode pairs is electrically connected to the heat-sensitive element. This forms an electrical path between (one of the electrode pair)-(heat-sensitive element 22 (between the electrode pair))-(the other of the electrode pair). A first protective film 26 is formed on the heat-sensitive element 22, a light-reflecting film 28 is formed on the first protective film 26, and a second protective film 32 is formed on the light-reflecting film 28. Each component of the infrared detector of the present invention will be described below.

[0014] (Thermal element 22) Examples of the thermal element include, but are not limited to, carbon nanotubes, vanadium oxide, and amorphous silicon. The thermal element is preferably a carbon nanotube because of its high TCR value. The carbon nanotube film is a thin film made of a plurality of carbon nanotubes, preferably having a network structure, and functions as a bolometer film.

[0015] The thickness of the carbon nanotube film is not particularly limited, but is, for example, 1 nm or more, for example, several nm to 100 μm, preferably 10 nm to 10 μm, more preferably 50 nm to 1 μm. In one embodiment, it is preferably 20 nm to 500 nm, more preferably 50 nm to 200 nm. When the thickness of the carbon nanotube film is 1 nm or more, a good light absorption rate can be obtained. In addition, it is preferable that the thickness of the carbon nanotube film is 1 μm or less, preferably 500 nm or less, from the viewpoint of simplifying the manufacturing method. In addition, if the carbon nanotube film is too thick, the contact electrode deposited from above may not be in sufficient contact with the carbon nanotubes below the carbon nanotube film, and the effective resistance value may become high, but if it is within the above range, the increase in the resistance value can be suppressed. In addition, when the thickness of the carbon nanotube film is within the above-mentioned range of 10 nm to 1 μm, it is also preferable in that the printing technology can be suitably applied as a manufacturing method of the carbon nanotube film. The thickness of the carbon nanotube film can be obtained as the average value of the thicknesses measured at any 10 points of the carbon nanotube film.

[0016] The density of the carbon nanotube film is not particularly limited, but is, for example, 0.3 g / cm 3 ~1.4g / cm 3 , preferably 0.8 g / cm 3 ~1.3g / cm 3 , more preferably 1.1 g / cm 3 ~1.2g / cm 3 The density of the carbon nanotube film can be calculated from the weight, area, and thickness of the carbon nanotube film obtained above.

[0017] Since the bolometer-type infrared detector 10 of the present invention has the light reflecting film (metal film) 28, as described below, light is mainly absorbed by the second protective film (light absorbing film) 32, and little of it reaches the thermal element 22. Therefore, the thickness and density of the thermal element 22 are not restricted to the range required for light absorption, and can be set to a range in which the resistance value and TCR value are optimized, or a range in which it is easy to fabricate.

[0018] In addition to the above-mentioned components, the carbon nanotube film may contain, as appropriate, negative thermal expansion materials, ion conductive agents (surfactants, ammonium salts, inorganic salts), resins, organic binders, etc., which will be described later.

[0019] The carbon nanotube content in the carbon nanotube film can be selected as appropriate, but preferably, 0.1 mass% or more based on the total mass of the carbon nanotube film is effective, and more preferably, 1 mass% or more is effective. For example, 30 mass% or even 50 mass% or more is preferable, and in some cases 60 mass% or more may be preferable.

[0020] An example of a method for producing a carbon nanotube film will now be described in detail. A dispersion liquid in which carbon nanotubes are dispersed is applied onto a thermal element support layer, and then dried, and optionally heat-treated, to form a carbon nanotube film.

[0021] The carbon nanotube dispersion preferably contains a surfactant in addition to the carbon nanotubes. The surfactant contained in the carbon nanotube dispersion is preferably a nonionic surfactant. Unlike ionic surfactants, nonionic surfactants have a weak interaction with carbon nanotubes and can be easily removed after the dispersion is provided on a substrate. Therefore, a stable carbon nanotube conductive path can be formed and an excellent TCR value can be obtained. In addition, a nonionic surfactant with a long molecular length is preferable because the distance between the carbon nanotubes becomes large when the dispersion is provided on a substrate and the carbon nanotubes are less likely to re-aggregate after evaporation of water, and therefore the network state can be maintained.

[0022] The nonionic surfactant can be appropriately selected, but it is preferable to use one or more nonionic surfactants composed of a non-ionized hydrophilic portion and a hydrophobic portion such as an alkyl chain, such as a nonionic surfactant having a polyethylene glycol structure represented by polyoxyethylene alkyl ether, or an alkyl glucoside nonionic surfactant. As such a nonionic surfactant, polyoxyethylene alkyl ether is preferably used. The alkyl portion may contain one or more unsaturated bonds. In particular, polyoxyethylene (23) lauryl ether, polyoxyethylene (20) cetyl ether, polyoxyethylene (20) stearyl ether, polyoxyethylene (10) oleyl ether, polyoxyethylene (10) cetyl ether, polyoxyethylene (10) stearyl ether, polyoxyethylene (20) oleyl ether, polyoxyethylene (100) stearyl ether, etc. are more preferable. In addition, N,N-bis[3-(D-gluconamido)propyl]deoxycholamide, n-dodecyl β-D-maltoside, octyl β-D-glucopyranoside, and digitonin can also be used.

[0023] As a nonionic surfactant, polyoxyethylene sorbitan monostearate (molecular formula: C 64 H 126 O 26 , product name: Tween 60, manufactured by Sigma-Aldrich Co., Ltd., etc.), polyoxyethylene sorbitan trioleate (molecular formula: C 24 H 44 O6, product name: Tween 85, manufactured by Sigma-Aldrich Co., Ltd., etc.), octylphenol ethoxylate (molecular formula: C 14 H 22 O(C2H4O) n , n=1 to 10, product name: Triton X-100, manufactured by Sigma-Aldrich Co., Ltd., etc.), polyoxyethylene (40) isooctylphenyl ether (molecular formula: CH 17 C6H40(CH2CH20) 40 H, product name: Triton X-405, manufactured by Sigma-Aldrich Co., Ltd., etc.), poloxamer (molecular formula: CH 10O2, trade name: Pluronic, manufactured by Sigma-Aldrich Corporation, etc.), polyvinylpyrrolidone (molecular formula: (C6H9NO)n, n=5 to 100, manufactured by Sigma-Aldrich Corporation, etc.), etc. can also be used.

[0024] The concentration of the surfactant in the carbon nanotube dispersion can be appropriately controlled, and is preferably about the critical micelle concentration to 5% by mass, more preferably 0.001% to 3% by mass, and particularly preferably 0.01 to 1% by mass in order to suppress re-aggregation after application. If the concentration is less than the critical micelle concentration, dispersion is not possible, which is not preferable. In this specification, the critical micelle concentration (CMC) refers to the concentration at which the surface tension is measured by changing the concentration of the surfactant aqueous solution using a surface tensiometer such as a Wilhelmy surface tensiometer under atmospheric pressure at 25°C, and the surface tension is at an inflection point.

[0025] The dispersion medium for the carbon nanotube dispersion is not particularly limited as long as it can disperse and suspend the carbon nanotubes. Examples of the dispersion medium include water, heavy water, an organic solvent, and a mixture of these, and water is preferred.

[0026] The method for obtaining the carbon nanotube dispersion is not particularly limited, and a conventionally known method can be applied. For example, a carbon nanotube mixture, a dispersion medium, and a nonionic surfactant are mixed to prepare a solution containing carbon nanotubes, and the solution is ultrasonically treated to disperse the carbon nanotubes, thereby preparing a carbon nanotube dispersion (micelle dispersion). In addition to or instead of the ultrasonic treatment, a carbon nanotube dispersion method using mechanical shearing force may be used. Mechanical shearing may be performed in the gas phase. It is preferable that the carbon nanotubes are isolated in the micellar dispersion solution of the carbon nanotubes and the nonionic surfactant. Therefore, if necessary, ultracentrifugation may be used to remove bundles, amorphous carbon, impurity catalysts, and the like. During the dispersion treatment, the carbon nanotubes can be cut, and the length can be controlled by changing the crushing conditions, ultrasonic output, ultrasonic treatment time, and the like of the carbon nanotubes. For example, the aggregate size can be controlled by crushing untreated carbon nanotubes with tweezers, a ball mill, or the like. After these treatments, the length can be controlled to 100 nm to 5 μm by using an ultrasonic homogenizer at an output of 40 to 600 W, or in some cases 100 to 550 W, 20 to 100 KHz, and a treatment time of 1 to 5 hours, preferably 1 to 3 hours. If the treatment time is shorter than 1 hour, the particles may not be dispersed at all depending on the conditions, and may remain almost the same as their original length. From the viewpoint of shortening the dispersion treatment time and reducing costs, a treatment time of 3 hours or less is preferable.

[0027] By dispersing and cutting the carbon nanotubes, surface functional groups are generated on the surface or ends of the carbon nanotubes. The functional groups generated include carboxyl groups, carbonyl groups, hydroxyl groups, etc. In the case of treatment in a liquid phase, carboxyl groups and hydroxyl groups are generated, and in the case of treatment in a gas phase, carbonyl groups are generated.

[0028] Carbon nanotubes can be separated, for example, by an electric field induced layer formation method (ELF method: see, for example, K.Ihara et al. J.Phys.Chem.C.2011,115,22827-22832, Japanese Patent No. 5717233, which are incorporated herein by reference). An example of a separation method using the ELF method will be described. Carbon nanotubes, preferably single-walled carbon nanotubes, are dispersed in a nonionic surfactant, and the dispersion is placed in a vertical separation device, and a voltage is applied to electrodes arranged above and below, to separate the nanotubes by carrier-free electrophoresis. The mechanism of separation can be estimated, for example, as follows. When carbon nanotubes are dispersed in a nonionic surfactant, the micelles of semiconducting carbon nanotubes have a negative zeta potential, while the micelles of metallic carbon nanotubes have a zeta potential of the opposite sign (positive) (in recent years, it has been considered that they have a slightly negative zeta potential or are almost uncharged). Therefore, when an electric field is applied to the carbon nanotube dispersion, the semiconducting carbon nanotube micelles electrophores toward the anode (+) and the metallic carbon nanotube micelles electrophores toward the cathode (-) due to the difference in zeta potential. Finally, a layer in which the semiconducting carbon nanotubes are concentrated near the anode and a layer in which the metallic carbon nanotubes are concentrated near the cathode are formed in the separation tank. The voltage for separation can be appropriately set in consideration of the composition of the dispersion medium and the charge amount of the carbon nanotubes, and is preferably 1V or more and 200V or less, and more preferably 10V or more and 200V or less. From the viewpoint of shortening the time of the separation process, 100V or more is preferable. Also, from the viewpoint of suppressing the generation of bubbles during separation and maintaining separation efficiency, 200V or less is preferable. The purity of the separation is improved by repeating the separation. The dispersion after separation may be reset to the initial concentration and the same separation operation may be performed. This can further increase the purity.

[0029] The above-mentioned carbon nanotube dispersion / cutting step and separation step can provide a dispersion in which semiconducting carbon nanotubes having a desired diameter and length are concentrated. In this specification, the carbon nanotube dispersion in which semiconducting carbon nanotubes are concentrated may be referred to as a "semiconducting carbon nanotube dispersion". The semiconducting carbon nanotube dispersion obtained by the separation step means a dispersion containing semiconducting carbon nanotubes in an amount of generally 67% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, particularly preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more (the upper limit may be 100% by mass) of the total amount of carbon nanotubes. The tendency of separation of metallic and semiconducting carbon nanotubes can be analyzed by microscopic Raman spectroscopy and ultraviolet-visible-near infrared absorptiometry.

[0030] After the above-mentioned carbon nanotube dispersion / cutting step and before the separation step, a centrifugation treatment may be performed to remove bundles, amorphous carbon, metal impurities, etc. from the carbon nanotube dispersion liquid. The centrifugal acceleration can be appropriately adjusted, but is preferably 10,000×g to 500,000×g, more preferably 50,000×g to 300,000×g, and may be 100,000×g to 300,000×g in some cases. The centrifugation time is preferably 0.5 hours to 12 hours, more preferably 1 to 3 hours. The centrifugation temperature can be appropriately adjusted, but is preferably 4°C to room temperature, more preferably 10°C to room temperature.

[0031] The method for applying the carbon nanotube dispersion to the insulating film 18 is not particularly limited, and examples thereof include a dropping method, spin coating, printing, inkjet, spray coating, dip coating, etc. From the viewpoint of reducing manufacturing costs, a printing method is preferable. Examples of the printing method include coating (dispenser, inkjet, etc.), transfer (microcontact printing, gravure printing, etc.), etc.

[0032] The carbon nanotube dispersion applied onto the insulating film is dried and heat-treated to remove the surfactant and the solvent, thereby forming the carbon nanotube film 22. The temperature of the heat treatment can be appropriately set to a temperature equal to or higher than the decomposition temperature of the surfactant, but is preferably 150 to 500°C, more preferably 200 to 500°C, for example 200 to 400°C. A temperature of 200°C or higher is more preferable because it is easier to suppress the residue of the decomposed product of the surfactant. A temperature of 500°C or lower, for example 400°C or lower, is preferable because it is possible to suppress the deterioration of the substrate and other components. Also, decomposition and size change of the carbon nanotubes, and release of functional groups, etc. can be suppressed.

[0033] Carbon nanotubes can form, for example, parallel wire, fiber, network, or other structures, but preferably form a three-dimensional network structure which is less prone to aggregation and provides uniform conductive paths.

[0034] The carbon nanotubes may be single-walled, double-walled or multi-walled carbon nanotubes, but single-walled or several-walled (e.g., two-walled or three-walled) carbon nanotubes are preferred, and single-walled carbon nanotubes are more preferred. The carbon nanotubes preferably contain 80% by mass or more of single-walled carbon nanotubes, and more preferably contain 90% by mass or more (including 100% by mass).

[0035] The carbon nanotube film is preferably made of semiconducting carbon nanotubes having a large band gap and carrier mobility. The content of semiconducting carbon nanotubes, preferably semiconducting single-walled carbon nanotubes, in the carbon nanotubes is generally 67% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, particularly preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more (including 100% by mass).

[0036] The diameter of the carbon nanotube is not particularly limited, but from the viewpoint of increasing the band gap and improving the TCR, it is preferably between 0.6 and 1.5 nm, more preferably between 0.6 and 1.2 nm, and even more preferably between 0.7 and 1.1 nm. In one embodiment, it may be particularly preferable for the diameter to be 1 nm or less. If the diameter is 0.6 nm or more, it is easier to manufacture the carbon nanotube. If the diameter is 1.5 nm or less, it is easier to maintain the band gap in an appropriate range, and a high TCR can be obtained.

[0037] In this specification, the diameter of the carbon nanotubes means that the diameters of about 100 points of the carbon nanotubes on the heat insulating layer or in the formed thin film are measured using an atomic force microscope (AFM), and 60% or more, preferably 70% or more, in some cases more preferably 80% or more, and more preferably 100% are within the range of 0.6 to 1.5 nm. Preferably, 60% or more, preferably 70% or more, in some cases more preferably 80% or more, and more preferably 100% are within the range of 0.6 to 1.2 nm, and even more preferably 0.7 to 1.1 nm. In one embodiment, 60% or more, preferably 70% or more, in some cases more preferably 80% or more, and more preferably 100% are within the range of 0.6 to 1 nm.

[0038] The length of the carbon nanotubes is not particularly limited, but is preferably between 100 nm and 5 μm because they are easily dispersed and have excellent coating properties. From the viewpoint of the electrical conductivity of the carbon nanotubes, the length is preferably 100 nm or more. If the length is 5 μm or less, aggregation on the heat insulating layer and / or during film formation is easily suppressed. The length of the carbon nanotubes is more preferably 500 nm to 3 μm, and even more preferably 700 nm to 1.5 μm.

[0039] In this specification, the length of carbon nanotubes means that at least 60%, preferably at least 70%, in some cases more preferably at least 80%, and more preferably 100% of the length distribution of carbon nanotubes is within the range of 100 nm to 5 μm, as determined by observing and counting at least 100 tubes using an atomic force microscope (AFM). Preferably, at least 60%, preferably at least 70%, in some cases more preferably at least 80%, and more preferably 100% of the length is within the range of 500 nm to 3 μm. More preferably, at least 60%, preferably at least 70%, in some cases more preferably at least 80%, and more preferably 100% of the length is within the range of 700 nm to 1.5 μm.

[0040] When the diameter and length of the carbon nanotube are within the above ranges, the influence of the semiconducting properties becomes large and a large current value can be obtained, so that when used as a bolometer film, a high TCR value is likely to be obtained.

[0041] The carbon nanotubes may be heat-treated in an inert atmosphere or in a vacuum to remove surface functional groups, impurities such as amorphous carbon, catalysts, etc. The heat treatment temperature can be appropriately selected, but is preferably 800 to 2000°C, more preferably 800 to 1200°C.

[0042] (First protective film 26) The first protective layer is a film that exists directly on the thermal element. The first protective film is made of at least one selected from the group consisting of a metal oxide film, a metal nitride film, a polyimide, an acrylic resin, and a fluorine-based resin. The first protective film is preferably made of an oxide of at least one metal selected from the group consisting of Si, Hf, Y, La, and Ta, and / or a nitride of at least one metal selected from the group consisting of Si, Hf, Y, La, and Ta. The first protective film is particularly preferably made of a silicon oxide film and / or a silicon nitride film. The thickness of the first protective film can be appropriately set depending on the material, but is preferably 1 to 1000 nm, more preferably 1 to 500 nm, and particularly preferably 1 to 100 nm. When the thickness of the first protective film is in the above range, a sufficient protective effect for the thermal element can be obtained.

[0043] (Light-reflecting film (metal film) 28) The light reflecting film is a film that exists directly on the first protective film. The light reflecting film is a metal film, and is preferably a film of at least one metal having high reflectance selected from the group consisting of Au, Ag, Al, Cr, Ni, and Pt. The thickness of the light reflecting film can be appropriately set depending on the material, but is preferably 1 to 1000 nm, more preferably 5 to 500 nm, and particularly preferably 10 to 300 nm. When the thickness of the light reflecting film is within the above range, a sufficient effect of protecting the thermal element can be obtained, and a sufficient light reflecting effect can be obtained.

[0044] (Second protective film (light absorbing film) 32) The second protective layer is a film that exists directly above the light reflecting film. The second protective film has an effect of suppressing doping of the thermal element due to adsorption of oxygen and moisture in the air. As the second protective film, it is preferable to use a material that functions as a protective film and a light absorbing film. The second protective film is made of at least one selected from the group consisting of a metal oxide film, a metal nitride film, a polyimide, an acrylic resin, and a fluorine-based resin. The second protective film is preferably made of an oxide film of at least one metal selected from the group consisting of Si, Hf, Y, La, and Ta, and / or a nitride film of at least one metal selected from the group consisting of Si, Hf, Y, La, and Ta. It is particularly preferable that the second protective film is made of a silicon oxide film and / or a silicon nitride film. The thickness of the second protective film can be appropriately set depending on the material, but is preferably 1 to 1000 nm, more preferably 100 to 1000 nm, and particularly preferably 500 to 1000 nm. When the thickness of the second protective film is within the above range, it is possible to obtain a sufficient effect of protecting the thermal element and to obtain a sufficient effect of absorbing infrared rays. If necessary, an absorber such as black gold may be provided on the second protective film. When a black gold film is provided, the thickness of the second protective film may be 10 to 100 nm.

[0045] The bolometer type infrared detector of the present invention can have three functions, a function of protecting the heat-sensitive element, a function of absorbing infrared light, and a function of reflecting light, by laminating a three-layer structure of a first protective film / light reflecting film / second protective film on the heat-sensitive element. A part of the light incident from the upper surface is absorbed by the second protective film 32, and the light that is not absorbed is reflected by the light reflecting film 28 and returns to the second protective film 32 to be absorbed again. That is, most of the incident light is absorbed by the second protective film (light absorbing film) 32. At that time, the second protective film 32 generates heat due to the absorbed light, and the heat also warms the heat-sensitive element 22, causing a change in its resistance value.

[0046] The bolometer-type infrared detector of the present invention may have a structure in which the laminated structure of the above three layers (first protective film / light reflective film / second protective film) is repeated multiple times.

[0047] (24 electrode pairs) The material of the electrode pair may be appropriately selected in consideration of the bonding property with the thermal element, and may be, for example, a single metal such as titanium, gold, platinum, aluminum, copper, silver, tungsten, or cobalt, or an alloy containing at least one of these metals, either alone or in combination. The method of producing the electrode pair is not particularly limited, and may be, for example, formed by vapor deposition, sputtering, or printing. If necessary, masking of areas where the electrode pair should not be formed may be performed in advance. The thickness of the electrode pair may be appropriately adjusted, but is preferably 30 to 300 nm, and more preferably 50 nm to 200 nm. The distance between the two electrodes is preferably 2 to 100 μm, and more preferably 2 to 10 μm for miniaturization of the infrared detector.

[0048] (Thermal element support layer 16) The material of the thermal element support layer is not particularly limited, but examples thereof include silicon oxide (SiO2), silicon nitride film (SiN), etc. The method of forming the thermal element support layer is not particularly limited, and can be appropriately selected according to the material used.

[0049] (Substrate 12) The material constituting the substrate 12 may be an inorganic material or an organic material, and any material used in the art may be used without any particular limitation. Inorganic materials include, but are not limited to, glass, Si, SiO2, SiN, etc. Organic materials include, but are not limited to, plastics, rubber, etc., such as polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyethylene terephthalate, acrylonitrile styrene resin, acrylonitrile butadiene styrene resin, fluororesin, methacrylic resin, polycarbonate, etc.

[0050] (Thermal insulation layer 14) The heat insulating layer 14 is made of a resin with high heat insulating properties (low thermal conductivity). By covering the substrate surface with a resin with high heat insulating properties, it is possible to suppress the dissipation of heat from the carbon nanotube film. The thermal conductivity of the resin constituting the heat insulating layer is generally 0.3 W / mK or less, preferably 0.15 W / mK or less, and more preferably 0.1 W / mK or less in some cases. Since a lower thermal conductivity is preferable, the lower limit is not particularly limited, but is, for example, 0.02 W / mK or more, and in some cases 0.05 W / mK or more. In particular, it is preferable that the thermal conductivity of the heat insulating layer at least in the vertical direction (stacking direction) is within the above range. In this specification, the thermal conductivity can be a value obtained at 25°C according to a standard method (ASTM C177, ASTM E1461, etc.).

[0051] The thickness of the heat insulating layer may be appropriately set in consideration of the resin component used, but is preferably 10 to 1000 μm, more preferably 20 to 700 μm, and even more preferably 50 to 200 μm. If the thickness of the heat insulating layer is within the above range, sufficient heat insulation can be obtained.

[0052] Resins used for the heat insulating layer are not particularly limited, but include parylene. Parylene is a general term for paraxylylene-based polymers, and has a structure in which benzene rings are linked via CH2. Examples of parylene include those formed from a dimer represented by the following formula:

[0053] [ka]

[0054] In the above formula, at least one hydrogen atom of at least one benzene ring may be substituted with a halogen atom. Examples of halogen include fluorine (F), chlorine (Cl), bromine (Br), and iodine (I), and chlorine is preferred. The number of substitutions by halogen is 8 or less, preferably 6 or less, and more preferably 4 or less.

[0055] Parylene includes Parylene N, Parylene C, Parylene D, Parylene HT, and ParyFree, among which Parylene C (thermal conductivity: 0.084 (W / mK)) is the most suitable because it has the lowest thermal conductivity. Parylene is chemically stable and has excellent moisture, chemical, and insulation barrier properties. Parylene coating also has excellent temperature stability, mechanical properties, and tensile strength.

[0056] The method of forming the heat insulating layer is not particularly limited and can be appropriately selected according to the resin used. For example, when parylene is used, a parylene film can be formed by coating parylene on a substrate using a vacuum deposition apparatus. Specifically, when a solid dimer is heated under vacuum, it vaporizes and becomes a dimer gas. This gas is thermally decomposed to cleave the dimer and become a monomer form. In a deposition chamber at room temperature, this monomer gas polymerizes on all surfaces to form a thin and transparent polymer film. If necessary, the substrate may be pretreated, cleaned, and areas that should not be deposited may be masked before the deposition process.

[0057] The bolometer-type infrared detector of the present invention can be particularly suitably used for detecting electromagnetic waves having a wavelength of, for example, 0.7 μm to 1 mm, in addition to infrared light. Examples of electromagnetic waves falling within this wavelength range include infrared light and terahertz waves. EXAMPLES

[0058] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0059] [Example 1] A substrate with an insulating surface was prepared by forming a heat insulating layer 14, which is an insulating film, on the surface of the substrate 12. Wiring 34 was formed on the substrate. A heat-sensitive element support layer 16 was formed thereon, and a heat-sensitive element 22 was formed on the heat-sensitive element support layer 16. An electrode pair 24 was formed at a distance so as to be electrically connected to the heat-sensitive element 22. In addition, a first protective film 26, a light reflecting film 28, and a second protective film 32 were formed in this order on the heat-sensitive element 22. This resulted in the formation of a bolometer-type infrared detector having the structure shown in FIG. 2A (heat-sensitive element: carbon nanotubes with a thickness of 5 nm, first protective film: silicon oxide film with a thickness of 45 nm, light reflecting film: titanium film with a thickness of 5 nm, second protective film: silicon oxide film with a thickness of 45 nm). The electrode pair 24 was structured so that a current could be supplied from the outside, and an electric path was formed between one of the electrode pair, the heat-sensitive element, and the other of the electrode pair.

[0060] [Comparative Example 1] A substrate with an insulating surface was prepared by forming a heat insulating layer 14, which is an insulating film, on the surface of the substrate 12. Wiring 34 was formed on the substrate. A heat sensitive element support layer 16 was formed thereon, and a heat sensitive element 22 was formed on the heat sensitive element support layer 16. An electrode pair 24 was formed at a distance so as to be electrically connected to the heat sensitive element 22. In addition, a protective film 26 was formed on the heat sensitive element 22. In this way, a bolometer type infrared detector having the structure shown in FIG. 2B was formed (heat sensitive element: carbon nanotubes with a thickness of 5 nm, protective film: silicon oxide film with a thickness of 100 nm). The structure allows a current to be supplied to the electrode pair 24 from the outside, and an electric path is formed between one of the electrode pair, the heat sensitive element, and the other of the electrode pair.

[0061] In general, when a thermal element (carbon nanotube) is exposed to the atmosphere, oxygen and moisture are adsorbed on the surface, causing the resistance value to decrease, and when the element is evacuated, the adsorbed oxygen and moisture are released, causing the resistance value to increase. However, in order to make a bolometer-type infrared detector that operates stably, it is important that the resistance value is not easily affected by the external environment. Since the relationship between the resistance value (R), voltage (V), and current (I) is V=R·I, the effect of the external environment on the resistance value can be investigated by measuring the current in the atmosphere and in a vacuum. 1V was applied to the infrared detectors of Example 1 and Comparative Example 1, and the current in the atmosphere and in a vacuum was measured. Three elements were measured for each structure.

[0062] FIG. 3 shows the measurement results of the current, and FIG. 4 shows the ratio of the current amount in a vacuum to the current amount in the atmosphere. The open symbols are Example 1, and the filled symbols are Comparative Example 1. In the structure shown in Comparative Example 1 (a simple oxide film on the thermal element), the thermal element was not sufficiently protected, and the current increased significantly in the atmosphere compared to the vacuum (the resistance value decreased significantly). By using the structure shown in Example 1 (a laminated structure of a first protective film, a light reflecting film, and a second protective film on the thermal element), the thermal element could be sufficiently protected, and the change in current (i.e., the change in resistance value) between the vacuum and the atmosphere was small. In this way, it was confirmed that the protective film has a three-layer structure of the first protective film (nitride film or oxide film) / light reflecting film (metal film) / second protective film (nitride film or oxide film), which has the effect of suppressing the fluctuation of the resistance value due to the influence of the atmosphere.

[0063] Although the present invention has been described above with reference to the embodiments and examples, the present invention is not limited to the above-mentioned embodiments and examples. Various modifications that can be understood by those skilled in the art can be made to the configuration and details of the present invention within the scope of the present invention.

[0064] (Appendix 1) A bolometer-type infrared detector having a laminated structure in which a first protective film, a light-reflecting film, and a second protective film are provided in that order on a thermal sensitive element, the first protective film being made of at least one selected from the group consisting of a metal oxide film, a metal nitride film, a polyimide, an acrylic resin, and a fluororesin, the light-reflecting film being a metal film, and the second protective film being made of at least one selected from the group consisting of a metal oxide film, a metal nitride film, a polyimide, an acrylic resin, and a fluororesin. (Appendix 2) 2. The bolometer-type infrared detector according to claim 1, wherein the metal oxide film is a silicon oxide film. (Appendix 3) 3. The bolometer-type infrared detector according to claim 1 or 2, wherein the metal nitride film is a silicon nitride film. (Appendix 4) 4. The bolometer-type infrared detector of any of the preceding claims, wherein the metal film is a titanium film. (Appendix 5) 4. The bolometer-type infrared detector of any of the preceding claims, wherein the heat-sensitive element is a carbon nanotube film. (Appendix 6) The bolometer-type infrared detector according to any one of the preceding appendices, wherein the first protective film has a thickness of 1 to 1000 nm. (Appendix 7) The bolometer-type infrared detector according to any one of the preceding appendices, wherein the second protective film has a thickness of 1 to 1000 nm. (Appendix 8) The bolometer-type infrared detector according to any one of the preceding appendices, wherein the light reflecting film has a thickness of 1 to 1000 nm. (Appendix 9) 4. The bolometer-type infrared detector according to any one of the preceding claims, further comprising a black gold film on the second protective film. (Appendix 10) 4. The bolometer-type infrared detector according to any one of the preceding appendices, having a structure in which the laminated structure is repeated a plurality of times. (Appendix 11) 2. A bolometer-type infrared detector according to any preceding claim, comprising a heat-sensitive element on a heat-sensitive element support layer. (Appendix 12) 13. A bolometer-type infrared detector according to any preceding claim, having an electrode pair on the thermal sensitive element. (Appendix 13) 2. A bolometer-type infrared detector according to any one of the preceding claims, comprising a heat-sensitive element support layer on a substrate having an insulating surface. (Appendix 14) Providing a substrate having an insulating surface; forming a thermal element support layer on the substrate; forming a thermal element on the thermal element support layer; forming an electrode pair on the thermal sensitive element; forming a first protective film on the thermal element; forming a light reflecting film on the first protective film; forming a second protective film on the light reflecting film; A method for manufacturing a bolometer type infrared detector, comprising the steps of: [Explanation of symbols]

[0065] 10 Bolometer type infrared detector 12 Substrate 14 Thermal insulation layer 16 Heat-sensitive element support layer 22 Thermal element 24 electrode pairs 26 First protective film 28 Light reflective film 32 Second protective film 34 Wiring

Claims

1. A bolometer-type infrared detector having a laminated structure in which a first protective film, a light-reflecting film, and a second protective film are provided in that order on a thermal sensitive element, the first protective film being made of at least one selected from the group consisting of a metal oxide film, a metal nitride film, a polyimide, an acrylic resin, and a fluorine-based resin, the light-reflecting film being a metal film, and the second protective film being made of at least one selected from the group consisting of a metal oxide film, a metal nitride film, a polyimide, an acrylic resin, and a fluorine-based resin.

2. 2. The bolometer type infrared detector according to claim 1, wherein the metal oxide film is a silicon oxide film.

3. 2. The bolometer type infrared detector according to claim 1, wherein said metal nitride film is a silicon nitride film.

4. 2. The bolometer type infrared detector according to claim 1, wherein said metal film is a titanium film.

5. 2. The bolometer type infrared detector according to claim 1, wherein the heat sensitive element is a carbon nanotube film.

6. 2. The bolometer type infrared detector according to claim 1, wherein the first protective film has a thickness of 1 to 1000 nm.

7. 2. The bolometer type infrared detector according to claim 1, wherein the second protective film has a thickness of 1 to 1000 nm.

8. 2. The bolometer type infrared detector according to claim 1, wherein the light reflecting film has a thickness of 1 to 1000 nm.

9. 2. The bolometer type infrared detector according to claim 1, further comprising a black gold film on said second protective film.

10. 2. The bolometer type infrared detector according to claim 1, wherein the laminated structure is repeated a plurality of times.

11. Providing a substrate having an insulating surface; forming a thermal element support layer on the substrate; forming a thermal element on the thermal element support layer; forming an electrode pair on the thermal sensitive element; forming a first protective film on the thermal element; forming a light reflecting film on the first protective film; forming a second protective film on the light reflecting film; A method for manufacturing a bolometer type infrared detector, comprising the steps of:

Citation Information

Patent Citations

  • Vanadium oxide thin film and bolometer type infrared ray sensor using this film

    JP1997257565A

  • Infrared light-receiving element

    JP2015049207A