Method of manufacturing rotor and rotor

The rotor manufacturing method addresses gap formation issues by using transfer molding with controlled conditions to insert a resin composition into the flux barrier, enhancing the fit and reducing manufacturing difficulties.

JP2024162713AInactive Publication Date: 2024-11-21SUMITOMO BAKELITE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023078537
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing rotor manufacturing methods face difficulties in inserting a molded body made of a resin composition into the flux barrier portion of the rotor core without leaving gaps.

Method used

A rotor manufacturing method involving transfer molding of a resin composition with specific temperature, pressure, and mold conditions to ensure the resin composition fits the shape of the flux barrier portion, using a thermosetting resin and soft magnetic particles to reduce gap formation.

Benefits of technology

The method effectively reduces the occurrence of gaps in the flux barrier portion, resulting in a rotor with improved fit and reduced manufacturing challenges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162713000001_ABST
    Figure 2024162713000001_ABST
Patent Text Reader

Abstract

To provide a method of manufacturing a rotor capable of reducing generation of a gap when a molded body made of a resin composition is inserted into a flux barrier portion of a rotor core, and to provide a rotor in which generation of a gap in the flux barrier portion of the rotor core is reduced.SOLUTION: A method for manufacturing a rotor 100 includes a step of inserting a cured product 30 made of a resin composition into a flux barrier portion 20 of a rotor core 80 by transfer molding the resin composition, where the rotor core 80 has a plate member 85, and the resin composition contains thermosetting resin (A).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a rotor and to a rotor. [Background technology]

[0002] As electrification continues to advance in automobiles, aircraft, and other fields, there is a demand for motors equipped in these vehicles to be more efficient and perform better.

[0003] In recent years, various studies have been conducted to improve the efficiency and performance of motors. Recent motor technologies include, for example, the technology described in Non-Patent Document 1.

[0004] Non-Patent Document 1 describes a motor in which a magnetic composite material is inserted into the flux barrier of the rotor. Non-Patent Document 1 describes that the high efficiency range of 94% can be expanded from 4,000 rpm to 8,000 rpm, and that a variable magnetic flux motor using a magnetic composite material has been realized. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Mitsuhide Sato and 6 others, "Proposal of a variable magnetic flux motor using magnetic composite material", Institute of Electrical Engineers of Japan Study Group (Rotary Machine Study Group), November 15-16, 2021, RM-21-106, p.23-28 Summary of the Invention [Problem to be solved by the invention]

[0006] There is known a rotor that includes a molded body made of a resin composition in the flux barrier section of the rotor core, as in the technology described in Non-Patent Document 1. However, according to the studies of the present inventors, it has been found that in the manufacturing method of such a rotor, it is sometimes difficult to insert the molded body into the hole in the flux barrier section without leaving any gaps.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and provides a method for manufacturing a rotor that can reduce the occurrence of gaps when a molded body made of a resin composition is inserted into the flux barrier section of the rotor core, and a rotor in which the occurrence of gaps in the flux barrier section of the rotor core is reduced. [Means for solving the problem]

[0008] According to the present invention, there are provided a rotor manufacturing method and a rotor as described below.

[0009] [1] The method includes a step of inserting a cured product of a resin composition into a flux barrier portion of a rotor core by transfer molding the resin composition; The rotor core has a plate member, The method for producing a rotor, wherein the resin composition contains a thermosetting resin (A). [2] The method for manufacturing a rotor according to the above [1], wherein in the above step, the injection pressure is 0.5 MPa or more and 5.0 MPa or less. [3] The method for manufacturing a rotor according to [1] or [2] above, wherein in the above process, the mold temperature is 100°C or higher and 200°C or lower. [4] The method for manufacturing a rotor according to any one of the above [1] to [3], wherein the rotor core has a laminate in which a plurality of the plate members are laminated. [5] The method for manufacturing a rotor according to any one of the above [1] to [4], wherein the plate member is an electromagnetic steel plate. [6] The method for producing a rotor according to any one of the above [1] to [5], wherein a saturation magnetic flux density at 25° C. of a cured product made of the resin composition is smaller than a saturation magnetic flux density at 25° C. of the plate member. [7] The rotor core further includes a magnet insertion portion for inserting a magnet, The method for manufacturing a rotor according to any one of the above [1] to [6], wherein the flux barrier portion is a hole independent of the magnet insertion portion. [8] The rotor core further includes a magnet insertion portion for inserting a magnet, The method for manufacturing a rotor according to any one of the above [1] to [6], wherein the flux barrier portion is a hole that is continuous with the magnet insertion portion. [9] The method for producing a rotor according to any one of the above [1] to [8], wherein the resin composition further contains soft magnetic particles (B).

[10] The method for producing a rotor according to [9], wherein the content of the soft magnetic particles (B) in the resin composition is 50% by volume or more and 90% by volume or less, when the entire resin composition is 100% by volume.

[11] The method for producing a rotor according to any one of the above [1] to

[10] , wherein the thermosetting resin (A) includes an epoxy resin.

[12] A rotor core having a flux barrier portion, The rotor core has a plate member, the flux barrier portion includes a transfer molding obtained by curing a resin composition, The resin composition comprises a thermosetting resin (A).

[13] The rotor according to

[12] , wherein the rotor core has a laminate in which a plurality of the plate members are stacked.

[14] The rotor according to

[12] or

[13] , wherein the saturation magnetic flux density of the transfer molded body at 25°C is smaller than the saturation magnetic flux density of the plate member at 25°C.

[15] The rotor according to any one of the above

[12] to

[14] , wherein the resin composition further contains soft magnetic particles (B). Effect of the Invention

[0010] According to the present invention, it is possible to provide a method for manufacturing a rotor that can reduce the occurrence of gaps when a molded body made of a resin composition is inserted into the flux barrier section of a rotor core, and a rotor in which the occurrence of gaps in the flux barrier section of the rotor core is reduced. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a plan view illustrating an example of a rotor according to the present embodiment. [Diagram 2] FIG. 2 is a plan view illustrating an example of a rotor according to the present embodiment. [Diagram 3] FIG. 2 is a cross-sectional view illustrating an example of a rotor according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Furthermore, a numerical range of "A to B" represents A or more and B or less unless otherwise specified.

[0013] As described above, there is known a rotor that includes a molded body made of a resin composition in the flux barrier section of the rotor core, as in the technology described in Non-Patent Document 1. Here, Non-Patent Document 1 describes a magnetic composite material obtained by mixing magnetic powder and resin and sintering the mixture as the molded body made of the resin composition.

[0014] As a method for inserting a compact that is a sintered body into the flux barrier portion of the rotor core, for example, a method in which a sintered body that has been machined to match the shape of the hole in the flux barrier portion is inserted into the flux barrier portion can be considered. According to the study of the present inventors, it was found that in the method of cutting the sintered body, it may be difficult to process the sintered body to match the shape of the hole in the flux barrier part when the shape of the hole in the flux barrier part is rounded, etc. If the sintered body cannot be processed to match the shape of the hole in the flux barrier, it becomes difficult to insert the sintered body into the hole in the flux barrier without leaving any gaps.

[0015] The present invention has been made in consideration of the above-mentioned circumstances, and provides a method for manufacturing a rotor that can reduce the occurrence of gaps when a molded body made of a resin composition is inserted into the flux barrier section of the rotor core, and a rotor in which the occurrence of gaps in the flux barrier section of the rotor core is reduced.

[0016] [Rotor manufacturing method] Fig. 1 and Fig. 2 are plan views each showing a typical example of a rotor according to the present embodiment. Fig. 3 is a cross-sectional view showing a typical example of a rotor according to the present embodiment. Note that the drawings are simplified and do not correspond to the actual dimensional ratio. The manufacturing method of the rotor 100 of this embodiment includes a step of inserting a cured product 30 made of a resin composition into the flux barrier portion 20 of the rotor core 80 by transfer molding the resin composition, the rotor core 80 having a plate member 85, and the resin composition containing a thermosetting resin (A).

[0017] The process of inserting the cured product 30 of the resin composition into the flux barrier portion 20 of the rotor core 80 by transfer molding the resin composition will be specifically described.

[0018] Examples of the method for transfer molding the resin composition include a method for transfer molding the resin composition using a known transfer molding device, specifically, a method in which a preheated resin composition is injected into a mold with a plunger and held in that state to harden the molten material.

[0019] The cured product 30 made of the resin composition of this embodiment is a transfer molded product obtained by curing a melt of the resin composition using the transfer molding device as described above. The cured product 30 made of the resin composition is also intended to include a molded product obtained by further post-curing the transfer molded product. The conditions for post-curing the transfer molded article are not particularly limited, but may be, for example, heating in air at 175° C. for 4 hours.

[0020] Examples of the method for inserting the cured product 30 of the resin composition into the flux barrier section 20 of the rotor core 80 include a method in which a transfer molding device is used, the rotor core 80 is arranged as a mold for the transfer molding device, and the molten resin composition is directly inserted into the flux barrier section 20 and held as such to harden the molten product; and a method in which a transfer molding device is used to prepare a cured product 30 of the resin composition that matches the shape of the hole in the flux barrier section 20, and the cured product 30 of the resin composition is inserted into the flux barrier section 20; among these, from the viewpoint of further simplifying the manufacturing process, a method in which a transfer molding device is used, the rotor core 80 is arranged as a mold for the transfer molding device, and the molten resin composition is directly inserted into the flux barrier section 20 and held as such to harden the molten product is.

[0021] The conditions for transfer molding the resin composition are not particularly limited, but the following conditions are preferred.

[0022] The temperature to which the resin composition is preheated is preferably 60° C. or higher, more preferably 70° C. or higher, and is preferably 100° C. or lower, and further preferably 90° C. or lower.

[0023] The mold temperature is preferably 100°C or higher, more preferably 120°C or higher, even more preferably 150°C or higher, even more preferably 160°C or higher, and even more preferably 170°C or higher, and from the viewpoint of further suppressing shrinkage of the resulting transfer molded body, it is preferably 200°C or lower, more preferably 190°C or lower, and even more preferably 180°C or lower. The temperature at which the resin composition is melted can be regarded as the same as the mold temperature.

[0024] The injection pressure is preferably 0.5 MPa or more, more preferably 0.8 MPa or more, more preferably 1.0 MPa or more, and is preferably 5.0 MPa or less, more preferably 4.5 MPa or less, and even more preferably 4.0 MPa or less. When the injection pressure is equal to or less than the above upper limit, when the rotor core 80 has a laminate in which multiple plate members 85 are stacked, the molten resin composition can be prevented from flowing into the gaps between the plate members 85. Here, the injection pressure means the pressure when the molten resin composition is injected into the mold.

[0025] The pressure retention time is preferably 30 seconds or more, more preferably 60 seconds or more, and even more preferably 90 seconds or more, and is preferably 500 seconds or less, more preferably 400 seconds or less, and even more preferably 350 seconds or less.

[0026] The molding device used for transfer molding the resin composition is not particularly limited, and examples thereof include known transfer molding devices, among which low-pressure transfer molding devices are preferred. A specific example of the low-pressure transfer molding device is KTS-30 (manufactured by Kotaki Seiki Co., Ltd.).

[0027] The rotor 100 obtained by the rotor manufacturing method of the present embodiment includes a rotor core 80 having a flux barrier section 20, and the flux barrier section 20 includes a cured product 30 made of a resin composition. The rotor 100 may further include a magnet (not shown) and the like.

[0028] [Rotor core] The rotor core 80 used in the rotor manufacturing method of this embodiment will be specifically described.

[0029] The rotor core 80 has a plate member 85 . The rotor core 80 preferably has a laminated body in which a plurality of plate members 85 are stacked. Here, the number of the plate members 85 is not particularly limited, but may be, for example, 2 to 500, or 10 to 300. Examples of the laminate in which plate members 85 are laminated include a laminate in which plate members 85 are laminated together by crimping, and a laminate in which plate members 85 are laminated together by bonding them with an adhesive.

[0030] The plate member 85 is not particularly limited, and for example, an electromagnetic steel plate, a permendur plate, an amorphous metal plate, etc. can be used, with the electromagnetic steel plate being preferred among these.

[0031] The rotor core 80 has a flux barrier portion 20 . Here, the flux barrier portion 20 means a hole for forming a magnetic gap. The flux barrier portion 20 is a hole formed in a direction perpendicular to the surface direction of the rotor core 80, and may or may not be a through hole. The rotor core 80 needs to have at least one flux barrier portion 20, and may have a plurality of flux barrier portions 20.

[0032] The shape of the flux barrier portion 20 in a plan view is not particularly limited and may be, for example, a rectangle, a circle, etc. The shape of the flux barrier portion 20 in a plan view is preferably a rounded shape such as a circle, from the viewpoint of suppressing stress concentration and further improving the strength of the rotor.

[0033] The rotor core 80 may further have a magnet insertion portion 50 for inserting a magnet (not shown). The magnet insertion portion 50 is a hole formed in a direction perpendicular to the surface direction of the rotor core 80, and may or may not be a through hole. The rotor core 80 may have multiple magnet inserts 50 .

[0034] When the rotor core 80 further includes the magnet insertion portion 50, the flux barrier portion 20 may be a hole independent of the magnet insertion portion 50. A hole independent of the magnet insertion portion 50 means a hole such as the flux barrier portion 20 illustrated in FIG.

[0035] When the rotor core 80 further includes the magnet insertion portion 50, the flux barrier portion 20 may be a hole continuous with the magnet insertion portion 50. The hole continuous with the magnet insertion portion 50 means a hole such as the flux barrier portion 20 illustrated in FIG. In FIG. 2, the center of the hole is magnet insertion portion 50 for inserting a magnet, and both ends of the hole are flux barrier portions 20.

[0036] [Resin composition] The resin composition used in the method for producing a rotor according to the present embodiment will be specifically described. The resin composition of the present embodiment contains a thermosetting resin (A).

[0037] The spiral flow of the resin composition of this embodiment at 175°C is preferably 10 cm or more, more preferably 20 cm or more, even more preferably 25 cm or more, even more preferably 30 cm or more, even more preferably 40 cm or more, and is preferably 200 cm or less, more preferably 180 cm or less, even more preferably 170 cm or less, even more preferably 160 cm or less. When the spiral flow of the resin composition at 175° C. is equal to or greater than the above lower limit, the flowability of the molten resin composition is good, and the resin composition can easily conform to the shape of the flux barrier portion. In this specification, the spiral flow of a resin composition at 175° C. means a spiral flow measured by the following measurement method. (Measurement method) Using a low pressure transfer molding machine, the resin composition is injected into a spiral flow measurement mold conforming to ANSI / ASTM D 3123-72, and the flow length (spiral flow) is measured under the following conditions: mold temperature 175°C, injection pressure 6.9 MPa, and pressure dwell time 120 seconds.

[0038] The gel time of the resin composition of this embodiment at 175°C is preferably 30 seconds or more, more preferably 40 seconds or more, even more preferably 45 seconds or more, even more preferably 60 seconds or more, even more preferably 70 seconds or more, and preferably 300 seconds or less, more preferably 250 seconds or less, even more preferably 200 seconds or less, even more preferably 150 seconds or less, even more preferably 120 seconds or less. When the gel time of the resin composition at 175°C is equal to or greater than the lower limit, the time required for the resin composition to harden can be secured, and therefore moldability can be improved, as well as handleability and fillability.When the gel time of the resin composition at 175°C is equal to or less than the upper limit, the time required for the resin composition to harden can be shortened, and therefore production time can be shortened, and productivity can be improved. In this specification, the gel time of a resin composition at 175° C. means the gel time measured by the following measurement method. (Measurement method) The resin composition is placed on a hot plate controlled at 175°C and kneaded with a spatula at one stroke per second. The time from when the resin composition is dissolved by heat to when it hardens is measured, and this is taken as the gel time.

[0039] The glass transition temperature of a cured product made from the resin composition of the present embodiment is preferably 100°C or higher, more preferably 110°C or higher, even more preferably 120°C or higher, and even more preferably 130°C or higher. There is no particular upper limit, but it may be, for example, 250°C or lower, or 200°C or lower. When the glass transition temperature of the cured product made of the resin composition is equal to or higher than the above lower limit, a rotor suitable for use in high-temperature environments can be provided. In this specification, the glass transition temperature of a cured product made of a resin composition means a glass transition temperature measured by the following measurement method. (Measurement method) The resin composition is injected and molded using a low-pressure transfer molding machine at a mold temperature of 175°C, injection pressure of 9.8MPa, and pressure retention time of 300 seconds to obtain a rectangular molded body with a width of 10 mm, a thickness of 1.5 mm, and a length of 55 mm. The molded body obtained is then post-cured under atmospheric conditions at 175°C for 4 hours to prepare a test piece for measuring the glass transition temperature. The glass transition temperature of the test piece for measuring the glass transition temperature is measured using a viscoelasticity measuring device under conditions of a measurement temperature range of 25°C to 300°C and a heating rate of 5°C / min.

[0040] The flexural strength at 25°C of the cured product made of the resin composition of this embodiment is, from the viewpoint of further improving the mechanical strength of the rotor, preferably 50 MPa or more, more preferably 70 MPa or more, and even more preferably 90 MPa or more, and the upper limit is not particularly limited, but may be, for example, 200 MPa or less, 170 MPa or less, or 150 MPa or less. The flexural modulus at 25°C of the cured product made of the resin composition of this embodiment is, from the viewpoint of further improving the mechanical strength of the rotor, preferably 20,000 MPa or more, more preferably 25,000 MPa or more, and even more preferably 27,000 MPa or more, and the upper limit is not particularly limited, but may be, for example, 50,000 MPa or less, or 48,000 MPa or less. In this specification, the flexural strength at 25° C. and the flexural modulus at 25° C. of a cured product made of a resin composition refer to values ​​measured by the following measurement method. (Measurement method) The resin composition is injected and molded using a low-pressure transfer molding machine at a mold temperature of 175°C, injection pressure of 9.8MPa, and pressure retention time of 300 seconds to obtain a rectangular molded body with a width of 10 mm, a thickness of 4 mm, and a length of 80 mm. The molded body obtained is then post-cured under atmospheric conditions at 175°C for 4 hours to prepare a test piece. The flexural strength and flexural modulus at 25°C of the test piece are measured in accordance with JIS K 6911 (2006) at a loading rate of 2 mm / min.

[0041] The saturation magnetic flux density at 25°C of the cured product made of the resin composition of this embodiment is preferably smaller than the saturation magnetic flux density at 25°C of the plate member 85. The saturation magnetic flux density at 25°C of a cured product made of the resin composition of this embodiment is preferably 1.50 T or less, more preferably 1.40 T or less, even more preferably 1.30 T or less, even more preferably 1.20 T or less, even more preferably 1.15 T or less, even more preferably 1.10 T or less, even more preferably 1.05 T or less, and even more preferably 1.00 T or less, and the lower limit is not particularly limited, and may be, for example, 0.20 T or more, or 0.30 T or more. In this specification, the saturation magnetic flux density at 25° C. of a cured product made of a resin composition means a saturation magnetic flux density measured by the following measurement method. (Measurement method) The resin composition is injected and molded using a low-pressure transfer molding machine at a mold temperature of 175°C, injection pressure of 9.8MPa, and pressure retention time of 300 seconds to obtain a cylindrical molded body with a diameter of 16 mmΦ and a height of 32 mm. The molded body is then post-cured under atmospheric conditions at 175°C for 4 hours to prepare a test piece for measuring saturation magnetic flux density. An external magnetic field of 100 kA / m is applied to the test piece for measuring saturation magnetic flux density at room temperature (25°C) using a DC / AC magnetization characteristic tester. The saturation magnetic flux density at 25°C is measured.

[0042] The resin composition of the present embodiment is preferably in a tablet form at 25° C. When the resin composition is in a tablet form, the storage property and handling property of the resin composition are further improved, and the resin composition is easily applicable to transfer molding.

[0043] Hereinafter, each of the components of the resin composition of the present embodiment will be described.

[0044] <Thermosetting resin (A)> The resin composition of the present embodiment contains a thermosetting resin (A). The thermosetting resin (A) is not particularly limited and may include, for example, at least one selected from the group consisting of epoxy resins, oxetane resins, (meth)acrylate resins, unsaturated polyester resins, diallyl phthalate resins, and maleimide resins, and preferably includes an epoxy resin.

[0045] Examples of the epoxy resin include at least one selected from the group consisting of bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, tetramethylbisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol E type epoxy resins, bisphenol M type epoxy resins, bisphenol P type epoxy resins, and bisphenol Z type epoxy resins; novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, aryl alkylene type epoxy resins, naphthalene type epoxy resins, anthracene type epoxy resins, phenoxy type epoxy resins, dicyclopentadiene type epoxy resins, norbornene type epoxy resins, adamantane type epoxy resins, fluorene type epoxy resins, trisphenylmethane type epoxy resins, and xyloc type epoxy resins.

[0046] The epoxy resin preferably includes at least one selected from the group consisting of bisphenol A type epoxy resin, trisphenylmethane type epoxy resin, biphenyl aralkyl type epoxy resin, cresol novolac type epoxy resin, Xylok type epoxy resin, and biphenyl type epoxy resin, more preferably includes at least one selected from the group consisting of triphenylmethane type epoxy resin, biphenyl aralkyl type epoxy resin, and cresol novolac type epoxy resin, and further preferably includes a biphenyl aralkyl type epoxy resin.

[0047] The epoxy resin is preferably a solid at 25° C. When the epoxy resin is a solid at 25° C., it becomes easy to prepare a resin composition that is in a tablet form at 25° C.

[0048] The content of the thermosetting resin (A) in the resin composition, when the entire resin composition is taken as 100 mass%, is preferably 0.50 mass% or more, more preferably 1.00 mass% or more, even more preferably 1.50 mass% or more, even more preferably 1.80 mass% or more, even more preferably 2.00 mass% or more, even more preferably 2.20 mass% or more, and is preferably 10.00 mass% or less, more preferably 8.00 mass% or less, even more preferably 6.00 mass% or less, and even more preferably 4.00 mass% or less.

[0049] The resin composition of the present embodiment may contain only one type of thermosetting resin (A), or may contain two or more types of thermosetting resins (A). In addition, even if the thermosetting resins (A) are the same type, those having different molecular weights may be used in combination.

[0050] <Soft magnetic particles (B)> The resin composition of the present embodiment preferably further contains soft magnetic particles (B). Soft magnetism refers to ferromagnetism with a small coercive force, and generally, ferromagnetism with a coercive force of 800 A / m or less is called soft magnetism. The soft magnetic particles (B) are iron-based particles whose main component is iron atoms (iron atoms have the largest mass content in the chemical composition), and more specifically, are iron alloys whose chemical composition has the largest mass content of iron atoms.

[0051] The soft magnetic particles (B) may contain elements other than iron as constituent elements. The soft magnetic particles (B) contain at least one element selected from the group consisting of B, C, N, O, Al, Si, P, S, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Cd, In, and Sn as an element other than iron, and preferably contain at least one element selected from the group consisting of Si, Ni, and Co, and more preferably contain Si element.

[0052] The soft magnetic particles (B) preferably contain at least one type selected from the group consisting of crystalline particles and amorphous particles. The soft magnetic particles (B) more preferably contain crystalline particles. Moreover, the soft magnetic particles (B) more preferably contain amorphous particles.

[0053] The soft magnetic particles (B) preferably include gas-water atomized powder. The gas-water atomized powder can be prepared by an atomization method using a mixture of water and gas as a pressure fluid. The gas-water atomized powder is a non-spherical atomized powder, which is different from the spherical atomized powder and the irregularly shaped water atomized powder. Gas-water atomized powder has the high sphericity characteristic of gas atomized powder and the high compact strength characteristic of water atomized powder, and a resin composition containing gas-water atomized powder as the soft magnetic particles (B) can give a cured product (transfer molded product) with improved fluidity and moldability as well as improved mechanical strength.

[0054] The particle size of the soft magnetic particles (B) is not particularly limited, but it is preferable to use a combination of large soft magnetic particles with a median size of 20 μm or more and 300 μm or less and small soft magnetic particles with a median size of less than 20 μm.

[0055] The median diameter can be obtained, for example, by a laser diffraction / scattering type particle size distribution measuring device. Specifically, the soft magnetic particles (B) are measured in a wet state by a SALD-7500nano manufactured by Shimadzu Corporation, a particle size distribution curve is obtained when the particles are measured on a volume basis, and the median diameter can be obtained by analyzing this distribution curve.

[0056] The content of the soft magnetic particles (B) in the resin composition is preferably 50% by volume or more, more preferably 60% by volume or more, even more preferably 65% ​​by volume or more, and preferably 90% by volume or less, more preferably 85% by volume or less, even more preferably 80% by volume or less, even more preferably 75% by volume or less, when the entire resin composition is taken as 100% by volume. By setting the content [volume %] of the soft magnetic particles (B) in the resin composition within the above range, the saturation magnetic flux density at 25° C. of the cured product made of the resin composition can be adjusted to a more appropriate range.

[0057] The content of the soft magnetic particles (B) in the resin composition, when the entire resin composition is taken as 100% by mass, is preferably 85.00% by mass or more, more preferably 88.00% by mass or more, even more preferably 90.00% by mass or more, and is preferably 98.00% by mass or less, more preferably 97.00% by mass or less, even more preferably 95.00% by mass or less, and even more preferably 94.00% by mass or less. By setting the content [mass %] of the soft magnetic particles (B) in the resin composition within the above range, the saturation magnetic flux density at 25° C. of the cured product made of the resin composition can be adjusted to a more appropriate range.

[0058] The resin composition of the present embodiment may contain only one type of soft magnetic particles (B), or may contain two or more types.

[0059] <Other ingredients> The resin composition of the present embodiment may further contain other components.

[0060] The resin composition of the present embodiment preferably further contains a silica filler (C) from the viewpoints of appropriately adjusting the melt viscosity of the resin composition and further improving the fluidity of the melt of the resin composition.

[0061] The resin composition of the present embodiment preferably further contains a phenol-based curing agent (D). The phenol-based curing agent (D) preferably contains any skeleton selected from the group consisting of a novolac skeleton and a biphenyl skeleton, from the viewpoint of further improving the durability of the cured product made of the resin composition.

[0062] The resin composition of the present embodiment preferably further contains a curing catalyst (E). The curing catalyst (E) refers to a component that accelerates the curing reaction of the thermosetting resin (A), and may also be called a curing accelerator. From the viewpoints of appropriately adjusting the gel time of the resin composition and further improving the mechanical strength of a cured product made of the resin composition, the curing catalyst (E) preferably contains a phosphorus atom-containing compound, and more preferably contains at least one selected from the group consisting of a tetra-substituted phosphonium compound, a phosphobetaine compound, an adduct of a phosphine compound and a quinone compound, and an adduct of a phosphonium compound and a silane compound. By using a latent curing catalyst, a resin composition having excellent moldability can be obtained.

[0063] The resin composition of the present embodiment may further contain components such as a coupling agent, a release agent, an adhesion aid, a stress reducing agent, a dispersant, an antioxidant, a colorant, an anti-corrosion agent, a dye, a pigment, and a flame retardant.

[0064] The contents of the silica filler (C), the phenol-based curing agent (D), the curing catalyst (E) and other components in the resin composition of this embodiment are each appropriate amounts.

[0065] The resin composition of the present embodiment can be industrially produced, for example, by first (1) mixing the components using a mixer, (2) then kneading using a roll at about 90° C. for 5 minutes or more, preferably about 10 minutes, to obtain a kneaded mixture, (3) cooling the kneaded mixture, and (4) pulverizing the mixture. In this manner, a powdered resin composition can be obtained.

[0066] The resin composition in tablet form at 25° C. can be obtained by tableting the powdered resin composition.

[0067] [rotor] The rotor 100 of this embodiment comprises a rotor core 80 having a flux barrier portion 20, the rotor core 80 having a plate member, the flux barrier portion 20 including a transfer molding 30 formed by curing a resin composition, and the resin composition including a thermosetting resin (A).

[0068] The transfer molded article 30 refers to a molded article obtained by curing a melt of a resin composition using a transfer molding device. The transfer molded article 30 is also intended to include a molded article obtained by further post-curing the above-mentioned molded article.

[0069] The saturation magnetic flux density of the transfer molded body 30 at 25°C is preferably smaller than the saturation magnetic flux density of the plate member at 25°C. The saturation magnetic flux density of the transfer molding 30 at 25°C is preferably 1.50 T or less, more preferably 1.40 T or less, even more preferably 1.30 T or less, even more preferably 1.20 T or less, even more preferably 1.15 T or less, even more preferably 1.10 T or less, even more preferably 1.05 T or less, and even more preferably 1.00 T or less, and the lower limit is not particularly limited, but may be, for example, 0.20 T or more, or 0.30 T or more. Here, in this specification, the saturation magnetic flux density of the transfer molded body 30 at 25°C means the saturation magnetic flux density measured at room temperature (25°C) by applying an external magnetic field of 100 kA / m using a DC / AC magnetization characteristic testing device.

[0070] The rotor core 80 and the resin composition constituting the rotor 100 of this embodiment are similar to the rotor core 80 and the resin composition used in the manufacturing method of the rotor of this embodiment described above. In addition, a preferred embodiment of the transfer molded body is similar to a preferred embodiment of the cured product made of the resin composition.

[0071] The rotor 100 of the present embodiment may further include a magnet (not shown) and the like.

[0072] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0073] The present embodiment will be described in detail below based on examples, but the present embodiment is not limited to the descriptions of these examples.

[0074] [Raw materials] First, the raw materials used in the examples will be described. Details of the raw materials listed in Table 1 are shown below.

[0075] <Soft magnetic particles (B)> Magnetic powder 1: amorphous magnetic powder (manufactured by Epson Atmix Corporation, product name: KUAMET6B2 150C01, median diameter: 40 μm, Fe content: 87.6 mass%, Si content: 6.7 mass%) Magnetic powder 2: crystalline magnetic powder (manufactured by Daido Steel Co., Ltd., product name: DAPMS7-100, gas water atomized powder, median diameter: 60 μm, Fe content: 93.4 mass%, Si content: 6.5 mass%) Magnetic powder 3: crystalline magnetic powder (manufactured by Daido Steel Co., Ltd., product name: DAPMS3-100, gas water atomized powder, median diameter: 70 μm, Fe content: 96.7 mass%, Si content: 3.0 mass%) Magnetic powder 4: crystalline magnetic powder (manufactured by Epson Atmix Corporation, product name: Fe-3.5Si-4.5Cr_PF-20F, median diameter: 10 μm, Fe content: 91.9 mass%, Si content: 3.5 mass%) Magnetic powder 5: amorphous magnetic powder (manufactured by Epson Atmix Corporation, product name: AW2-08_PF-3F, median diameter: 3 μm, Fe content: 87.4 mass%, Si content: 6.8 mass%) Magnetic powder 6: crystalline magnetic powder (manufactured by Shinto Kogyo Co., Ltd., product name: FSC-2, median diameter: 2 μm, Fe content: 91.1 mass%, Si content: 3.5 mass%)

[0076] <Coupling Agent> Coupling agent 1: Phenylaminopropyltrimethoxysilane (manufactured by Dow Corning Toray Co., Ltd., product name: CF-4083)

[0077] <Thermosetting resin (A)> Epoxy resin 1: biphenyl aralkyl type epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name: NC-3000L, solid at 25°C)

[0078] <Phenol-based hardener (D)> Phenolic resin 1: Phenol aralkyl resin containing biphenylene skeleton (manufactured by Meiwa Kasei Co., Ltd., product name: MEH-7851SS)

[0079] <Release agent> Wax 1: Synthetic wax (copolymer of 1-alkene and maleic anhydride) Wax 2: Stearic acid (NOF Corporation, product name: powdered stearic acid Sakura fine powder) Wax 3: Carnauba wax (manufactured by Toa Kasei Co., Ltd., product name: TOWAX-132)

[0080] <Adhesion aid> Adhesion aid 1: Compound containing benzotriazole-based compounds (manufactured by ADEKA Corporation, product name: Adeka STAB CDA-1M)

[0081] <Low stress agent> Silicone oil 1: Silicone oil (manufactured by Toray Dow Corning, product name: FZ-3730)

[0082] <Curing catalyst (E)> Curing catalyst 1: Tetraphenylphosphonium bis(naphthalene-2,3-dioxy)phenylsilicate (Sumitomo Bakelite Co., Ltd.) Curing catalyst 2: Tetraphenylphosphonium 4,4'-sulfonyldiphenolate (Sumitomo Bakelite Co., Ltd.)

[0083] <Silica filler (C)> Silica filler 1: Fused silica (median diameter 0.5 μm)

[0084] [Examples 1 to 4] <Preparation of resin composition> Each component shown in Table 1 was prepared in the ratio [parts by mass] shown in Table 1, and the soft magnetic particles were first mixed while the other components were added thereto and mixed uniformly to obtain the respective mixtures. The resulting mixture was then kneaded at 100° C. for 10 minutes. After kneading, the resulting kneaded product was cooled to room temperature to become solid, and then crushed and tableted. As a result, tablet-shaped resin compositions in Examples 1 to 4 were obtained, respectively.

[0085] <Preparation of transfer molded body 1 by curing resin composition> The tablet-like resin compositions obtained in Examples 1 to 4 were injection molded using a low-pressure transfer molding machine (manufactured by Kotaki Seiki Co., Ltd., product name: KTS-30) at a mold temperature of 175°C, injection pressure of 9.8 MPa, and pressure retention time of 300 seconds to obtain cylindrical transfer molded bodies with a diameter of 16 mmΦ and a height of 32 mm. The obtained molded bodies were then post-cured under atmospheric conditions at 175°C for 4 hours to obtain transfer molded bodies 1 each formed by curing the cylindrical resin composition.

[0086] <Preparation of transfer molded body 2 by curing resin composition> The tablet-like resin compositions obtained in Examples 1 to 4 were injection molded using a low-pressure transfer molding machine (manufactured by Kotaki Seiki Co., Ltd., product name: KTS-30) at a mold temperature of 175°C, injection pressure of 9.8 MPa, and pressure retention time of 300 seconds to obtain rectangular transfer molded bodies having a width of 10 mm, a thickness of 1.5 mm, and a length of 55 mm. The obtained molded bodies were then post-cured under atmospheric conditions at 175°C for 4 hours to obtain transfer molded bodies 2 each consisting of a cured rectangular resin composition.

[0087] <Preparation of transfer molded body 3 by curing resin composition> The tablet-like resin compositions obtained in Examples 1 to 4 were injection molded using a low-pressure transfer molding machine (manufactured by Kotaki Seiki Co., Ltd., product name: KTS-30) under conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a pressure retention time of 300 seconds, to obtain rectangular transfer molded bodies having a width of 10 mm, a thickness of 4 mm, and a length of 80 mm. The obtained molded bodies were then post-cured under atmospheric conditions at 175°C for 4 hours, to obtain transfer molded bodies 3 each formed by curing the rectangular resin composition.

[0088] [measurement] <Content of soft magnetic particles (B) relative to the entire resin composition [volume %]> The content [volume %] of the soft magnetic particles (B) relative to the entire resin composition was calculated using the volume of the obtained pellet-shaped resin composition and the volume of the soft magnetic particles (B) calculated from the density and content of the soft magnetic particles (B) in the resin composition.

[0089] <Spiral flow of resin composition at 175°C> Using a low pressure transfer molding machine (manufactured by Kotaki Seiki Co., Ltd., product name: KTS-30), the resin composition was injected into a metal mold for measuring spiral flow in accordance with ANSI / ASTM D 3123-72, and the flow length (spiral flow) was measured under the following conditions: mold temperature 175°C, injection pressure 6.9 MPa, and pressure dwell time 120 seconds. Spiral flow is a parameter of fluidity, and the larger the value, the better the fluidity. The unit is cm.

[0090] <Gel time of resin composition at 175°C> The resin composition was placed on a hot plate controlled at 175°C and kneaded with a spatula at one stroke per second. The time from when the resin composition was dissolved by heat to when it hardened was measured and this was taken as the gel time. The smaller the gel time value, the faster the hardening.

[0091] <Glass transition temperature of cured product made of resin composition> The glass transition temperature of transfer molding 2 (i.e., a transfer molding obtained by curing a rectangular resin composition having a width of 10 mm, a thickness of 1.5 mm, and a length of 55 mm) was measured using a viscoelasticity measuring device (manufactured by Hitachi High-Tech Corporation, product name: DMA7100) under conditions of a measurement temperature range of 25°C to 300°C and a heating rate of 5°C / min.

[0092] <Flexural strength at 25°C and flexural modulus at 25°C of cured product made of resin composition> The bending strength and bending modulus at 25°C of transfer molding 3 (i.e., a rectangular transfer molding obtained by curing a resin composition with a width of 10 mm, a thickness of 4 mm, and a length of 80 mm) were measured at a loading rate of 2 mm / min in accordance with JIS K 6911 (2006).

[0093] <Saturation magnetic flux density at 25°C of the cured product made of the resin composition> An external magnetic field of 100 kA / m was applied to the transfer molded body 1 (i.e., a cylindrical transfer molded body having a diameter of 16 mm and a height of 32 mm, obtained by curing a resin composition) at room temperature (25°C) using a DC / AC magnetization characteristic tester (manufactured by Metron Giken Co., Ltd., product name: MTR-3368). Thus, the saturation magnetic flux density at 25°C was measured.

[0094] The results of the above measurements for the resin compositions and transfer molded articles of Examples 1 to 4 are shown in Table 1.

[0095] [Table 1]

[0096] In Examples 1 to 4, transfer molded bodies 1 to 3 with different shapes were obtained, respectively. In particular, a rounded cylindrical molded body was obtained as transfer molded body 1. That is, by transfer molding the resin composition, it is possible to process it to match the shape of the hole in the flux barrier part. Therefore, it can be understood that according to the rotor manufacturing method and rotor of this embodiment, it is possible to reduce the occurrence of gaps when a molded body made of a resin composition is inserted into the flux barrier part of the rotor core. [Explanation of symbols]

[0097] 20 Flux Barrier Section 30 Cured product (transfer molded product) made of resin composition 50 Magnet insertion part 80 rotor core 85 Plate members 100 rotors

Claims

1. The method includes a step of inserting a cured product of a resin composition into a flux barrier portion of a rotor core by transfer molding the resin composition; The rotor core has a plate member, The method for producing a rotor, wherein the resin composition contains a thermosetting resin (A).

2. The method for manufacturing a rotor according to claim 1 , wherein in the step, the injection pressure is 0.5 MPa or more and 5.0 MPa or less.

3. The method for manufacturing a rotor according to claim 1 or 2, wherein in the step, the mold temperature is 100° C. or higher and 200° C. or lower.

4. The method for manufacturing a rotor according to claim 1 or 2, wherein the rotor core has a laminate in which a plurality of the plate members are stacked.

5. The method for manufacturing a rotor according to claim 1 or 2, wherein the plate member is an electromagnetic steel plate.

6. The method for manufacturing a rotor according to claim 1 or 2, wherein a saturation magnetic flux density at 25°C of the cured product made of the resin composition is smaller than a saturation magnetic flux density at 25°C of the plate member.

7. The rotor core further includes a magnet insertion portion for inserting a magnet, The method for manufacturing a rotor according to claim 1 , wherein the flux barrier portion is a hole independent of the magnet insertion portion.

8. The rotor core further includes a magnet insertion portion for inserting a magnet, The method for manufacturing a rotor according to claim 1 , wherein the flux barrier portion is a hole that is continuous with the magnet insertion portion.

9. The method for producing a rotor according to claim 1 or 2, wherein the resin composition further contains soft magnetic particles (B).

10. The method for manufacturing a rotor according to claim 9, wherein the content of the soft magnetic particles (B) in the resin composition is 50% by volume or more and 90% by volume or less, when the entire resin composition is taken as 100% by volume.

11. The method for manufacturing a rotor according to claim 1 or 2, wherein the thermosetting resin (A) includes an epoxy resin.

12. A rotor core having a flux barrier portion, The rotor core has a plate member, The flux barrier portion includes a transfer molding obtained by curing a resin composition, The resin composition comprises a thermosetting resin (A).

13. The rotor according to claim 12 , wherein the rotor core has a laminate in which a plurality of the plate members are stacked.

14. The rotor according to claim 12 or 13, wherein the saturation magnetic flux density of the transfer molded body at 25°C is lower than the saturation magnetic flux density of the plate member at 25°C.

15. The rotor according to claim 12 or 13, wherein the resin composition further comprises soft magnetic particles (B).