Method for manufacturing circular polarization
The described method for manufacturing circularly polarizing plates addresses hole mark defects by precise laminate preparation, decolorization, and layering, resulting in improved quality and functionality for image display devices.
Patent Information
- Application Number
- JP2023078549
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Existing methods for manufacturing circularly polarizing plates result in appearance defects due to hole marks caused by tight winding of laminates with through holes, which are not effectively addressed in prior art.
A method involving the preparation of a polarizing film laminate roll with specific thicknesses and adhesive bonding, followed by decolorizing exposed polarizer portions, peeling protective films, and laminating a retardation layer to suppress hole marks, including optional steps for additional protective layers and adhesive application.
The method effectively suppresses appearance defects from hole marks, enhancing the quality and functionality of circularly polarizing plates for image display devices.
Smart Images

Figure 2024162719000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a circularly polarizing plate. [Background technology]
[0002] In image display devices such as organic electroluminescence (EL) display devices and liquid crystal display devices, members containing optically anisotropic films such as polarizing films and retardation films are used. In particular, in organic electroluminescence (EL) display devices, visibility is easily reduced due to external light reflection by metal electrodes, so circular polarizing plates that combine polarizing films and retardation films are used to prevent this external light reflection.
[0003] In addition, in order to meet the needs of diverse shapes and high performance of image display devices, polarizing plates having partial polarizing performance are required. As such polarizing plates, polarizing plates having a polarizer in which a non-polarizing portion is formed by a chemical treatment are known.
[0004] Patent Document 1 proposes a method for producing a polarizer having a non-polarizing portion, in which a surface protective layer having a plurality of through holes is laminated on a polarizer, the polarizing film laminate including the polarizer and the surface protective layer is wound into a roll, and then exposed areas of the polarizer (areas exposed through the through holes in the surface protective layer) are bleached to form non-polarizing portions. Hereinafter, the rolled polarizing film laminate may be referred to as a "polarizing film laminate roll." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-53645 A Summary of the Invention [Problem to be solved by the invention]
[0006] When a laminate including a surface protective layer having a plurality of through holes is wound into a roll, dents (hole marks caused by the through holes in the surface protective layer) may occur in the laminate due to tight winding. The technology described in Patent Document 1 leaves room for improvement in terms of suppressing the occurrence of poor appearance caused by hole marks in the polarizing film laminate roll.
[0007] In view of the above problems, an object of the present invention is to provide a method for producing a circularly polarizing plate capable of suppressing the occurrence of appearance defects caused by hole marks. [Means for solving the problem]
[0008] <Aspects of the present invention> The present invention includes the following aspects.
[0009] [1] A step Sa of preparing a roll of a polarizing film laminate including, in this order, a first protective film, a first polarizer protective layer, a polarizer, and a second protective film having a through hole; a step Sb of bringing a portion of the polarizer exposed through the through hole into contact with a treatment liquid while unwinding the polarizing film laminate from the roll to decolorize the portion, thereby forming a non-polarizing portion; a step Sc of peeling off the first protective film and the second protective film from the polarizing film laminate; a step Sd of laminating a retardation layer on the side of the first polarizer protection layer opposite to the polarizer side; The method for producing a circularly polarizing plate comprises the steps of:
[0010] [2] The method for producing a circularly polarizing plate described in [1] above, further comprising, after step Sc, step Se of laminating a second polarizer protective layer on the surface of the polarizer from which the second protective film has been peeled off.
[0011] [3] The method for producing a circularly polarizing plate according to [1] or [2] above, wherein the first protective film has a thickness of 50 μm or less.
[0012] [4] The method for producing a circularly polarizing plate described in any one of [1] to [3], wherein the thickness of the polarizing film laminate after the first protective film and the second protective film are peeled off in step Sc is 50 μm or less.
[0013] [5] The method for producing a circularly polarizing plate according to any one of [1] to [4] above, wherein the first polarizer protection layer and the polarizer are bonded with an adhesive.
[0014] [6] The method for producing a circularly polarizing plate according to any one of [1] to [5] above, wherein the first polarizer protective layer has a pencil hardness of 4B or more on a surface facing the first protective film.
[0015] [7] The method for producing a circularly polarizing plate according to any one of [1] to [6] above, wherein the second protective film has a thickness of 20 μm or more and 150 μm or less.
[0016] [8] The method for producing a circularly polarizing plate according to any one of [1] to [7] above, wherein the through hole has an opening diameter of 1 mm or more and 10 mm or less. Effect of the Invention
[0017] According to the present invention, it is possible to provide a method for producing a circularly polarizing plate capable of suppressing the occurrence of defective appearance caused by hole marks. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a perspective view illustrating an example of a roll of a polarizing film laminate. [Diagram 2] FIG. 2 is a partial cross-sectional view showing an example of a lamination state at a surface layer portion of a polarizing film laminate roll. [Diagram 3] 5A to 5C are process diagrams illustrating an example of a process for forming a non-polarizing portion. [Figure 4] FIG. 2 is a partial cross-sectional view showing an example of a polarizing film laminate after a non-polarizing portion has been formed. [Diagram 5]4 is a partial cross-sectional view showing an example of a polarizing film laminate after a first protective film and a second protective film have been peeled off. FIG. [Figure 6] 4 is a partial cross-sectional view showing an example of a polarizing film laminate after a second polarizer protective layer has been laminated thereon. FIG. [Figure 7] FIG. 2 is a partial cross-sectional view showing an example of a circularly polarizing plate obtained by the production method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Preferred embodiments of the present invention will now be described. All academic and patent documents described in this specification are incorporated herein by reference.
[0020] First, the terms used in this specification will be explained. The term "C plate" refers to a retardation film (retardation layer) having refractive index anisotropy in the thickness direction. Among C plates, a retardation film (retardation layer) having a negative retardation value in the thickness direction is called a "positive C plate", and a retardation film (retardation layer) having a positive retardation value in the thickness direction is called a "negative C plate".
[0021] The pencil hardness value is a value measured under a load of 500 g in accordance with the provisions of JIS K 5600-5-4. The "thickness" value of a layered material (more specifically, the first protective film, the first polarizer protective layer, the polarizer, the second protective film, the retardation layer, the second polarizer protective layer, etc.) is, unless otherwise specified, the arithmetic average value of 10 measured values obtained by observing a cross section of the layered material cut in the thickness direction with an electron microscope, randomly selecting 10 measurement points from the cross section image, and measuring the thickness of the selected 10 measurement points.
[0022] Hereinafter, the compound and its derivatives may be collectively referred to by adding "based" after the compound name. In addition, when the polymer name is represented by adding "based" after the compound name, it means that the repeating unit of the polymer is derived from the compound or its derivative, unless otherwise specified. In addition, acrylic and methacrylic may be collectively referred to as "(meth)acrylic". Unless otherwise specified, the components and functional groups exemplified in this specification may be used alone or in combination of two or more types.
[0023] The drawings referred to in the following description are intended to illustrate each component in a schematic manner for ease of understanding, and the size, number, shape, etc. of each component shown in the drawings may differ from the actual size, number, shape, etc., for convenience of drawing. Also, for convenience of explanation, in the drawings described later, the same components as those in the drawings described earlier may be given the same reference numerals, and explanations thereof may be omitted.
[0024] <Method of manufacturing circularly polarizing plate> The method for producing a circular polarizing plate according to this embodiment includes steps Sa, Sb, Sc, and Sd. In step Sa, a roll of a polarizing film laminate (polarizing film laminate roll) is prepared, which includes a first protective film, a first polarizer protective layer, a polarizer, and a second protective film having a through hole in this order. In step Sb, while the polarizing film laminate is unwound from the polarizing film laminate roll, the exposed portion of the polarizer from the through hole is brought into contact with a treatment liquid to decolorize and form a non-polarizing portion. In step Sc, the first protective film and the second protective film are peeled off from the polarizing film laminate. In step Sd, a retardation layer is laminated on the side opposite to the polarizer side of the first polarizer protective layer.
[0025] The method for producing a circularly polarizing plate according to this embodiment may further include a step (other step) other than step Sa, step Sb, step Sc, and step Sd. An example of the other step is step Se of laminating a second polarizer protective layer on the surface of the polarizer from which the second protective film has been peeled off after step Sc.
[0026] Hereinafter, step Sa may be referred to as a "roll preparation step." Step Sb may be referred to as a "non-polarizing portion formation step." Step Sc may be referred to as a "protective film peeling step." Step Sd may be referred to as a "retardation layer lamination step." Step Se may be referred to as a "second polarizer protective layer lamination step."
[0027] Hereinafter, each step of an example of a method for producing a circularly polarizing plate according to this embodiment will be described with reference to the drawings as appropriate.
[0028] [Roll preparation process] The roll preparation step will be described with reference to Fig. 1 and Fig. 2. Fig. 1 is a perspective view showing an example of a polarizing film laminate roll. Fig. 2 is a partial cross-sectional view showing an example of the lamination state of the surface layer portion of the polarizing film laminate roll.
[0029] The roll preparation step is a step of preparing a polarizing film laminate roll. First, the polarizing film laminate roll will be described. The polarizing film laminate roll 100 shown in FIG. 1 is a roll of a polarizing film laminate 10. As shown in FIG. 2, the polarizing film laminate 10 includes a first protective film 11, a first polarizer protective layer 12, a polarizer 13, and a second protective film 14 having a through hole 14a, in this order. An adhesive layer 15 is interposed between the first polarizer protective layer 12 and the polarizer 13. That is, the first polarizer protective layer 12 and the polarizer 13 are bonded with an adhesive. When the first polarizer protective layer 12 and the polarizer 13 are bonded with an adhesive, the adhesion between the first polarizer protective layer 12 and the polarizer 13 is increased, so that the polarizer 13 is more reliably protected. In this embodiment, the first polarizer protection layer 12 and the polarizer 13 are bonded together with an adhesive, but the present invention is not limited to this, and the first polarizer protection layer 12 and the polarizer 13 may be bonded together with a pressure-sensitive adhesive.
[0030] 2, the second protective film 14 is in contact with the polarizer 13, and a part of the polarizer 13 is exposed from a through-hole 14a of the second protective film 14. The first protective film 11 is also peelably attached to the first polarizer protective layer 12. Similarly, the second protective film 14 is also peelably attached to the polarizer 13.
[0031] The width of the polarizing film laminate 10 is, for example, from 500 mm to 2000 mm, and preferably from 1000 mm to 1500 mm. The length of the polarizing film laminate 10 is, for example, from 50 m to 6000 m, and preferably from 150 m to 4000 m.
[0032] In the example shown in FIG. 1, a plurality of through holes 14a are provided in a predetermined pattern. The arrangement pattern of the through holes 14a can be appropriately set depending on the purpose. The planar shape of the through holes 14a can be appropriately changed depending on the shape required for the non-polarizing portion 13a (see FIG. 4). Examples of the planar shape of the through holes 14a include a circle, an ellipse, a rectangle, and the like, and a circle is preferable. In the example shown in FIG. 1, the polarizing film laminate 10 is rolled so that the through holes 14a are arranged on the inside, but the present invention is not limited thereto, and the polarizing film laminate 10 may be rolled so that the through holes 14a are arranged on the outside.
[0033] The diameter of the opening of the through hole 14a can be changed as appropriate depending on the size of the non-polarizing portion 13a (see FIG. 4). The diameter of the opening of the through hole 14a is, for example, 0.5 mm or more and 20 mm or less, and preferably 1 mm or more and 10 mm or less.
[0034] In the example shown in Fig. 2, the opening edge of through hole 14a provided in second protective film 14 of polarizing film laminate 10 at the outermost periphery (first turn) is in contact with first protective film 11 of polarizing film laminate 10 located immediately below the outermost periphery (second turn). Hereinafter, the through hole provided in the second protective film of the polarizing film laminate at the first turn may be referred to as the "through hole at the first turn." Furthermore, the through hole provided in the second protective film of the polarizing film laminate at the nth turn (n is an integer of 2 or more) may be referred to as the "through hole at the nth turn."
[0035] In the state where the polarizing film laminate 10 is wound, excessive pressure tends to be applied below (inward) the opening edge of the through-hole 14a. In the example shown in FIG. 2, excessive pressure tends to be applied to the X portion of the first polarizer protective layer 12 of the polarizing film laminate 10 of the second turn through the first protective film 11 below the opening edge of the through-hole 14a of the first turn. As a result, the first polarizer protective layer 12 of the polarizing film laminate 10 of the second turn is likely to have a hole mark 12b (see FIG. 5) described later. Similarly, excessive pressure tends to be applied to the X portion of the first polarizer protective layer 12 of the polarizing film laminate 10 of the n+1th turn through the first protective film 11 below the opening edge of the through-hole 14a of the nth turn. As a result, the hole mark 12b is likely to be generated in the first polarizer protective layer 12 of the polarizing film laminate 10 of the n+1th turn. In particular, when the opening diameter of the through-hole 14a is 1 mm or more and 10 mm or less, the hole mark 12b tends to be easily generated in the first polarizer protection layer 12 of the polarizing film laminate 10 from the second turn onwards.
[0036] The roll preparation step may be a step of preparing a commercially available polarizing film laminate roll 100, or may include a step of forming the polarizing film laminate 10 and then winding the obtained polarizing film laminate 10. The method of forming the polarizing film laminate 10 is not particularly limited, and a known method described in, for example, JP 2016-53645 A or JP 2022-182000 A can be adopted. In the step of winding the polarizing film laminate 10, a winding device (not shown) is used to wind the polarizing film laminate 10 with a winding tension of, for example, 130 N / 1000 mm width or more to obtain the polarizing film laminate roll 100. By winding with a winding tension of 130 N / 1000 mm width or more, the occurrence of winding misalignment of the polarizing film laminate 10 can be suppressed. If the polarizing film laminate 10 is wound with a winding tension of 130 N / 1000 mm width or more, hole marks 12b (see FIG. 5) are likely to occur in the first polarizer protection layer 12 of the polarizing film laminate 10 from the second turn onward. In order to prevent damage to the polarizing film laminate 10 due to tight winding, it is preferable to wind the polarizing film laminate 10 with a winding tension of 250 N / 1000 mm width or less.
[0037] Next, each layer of the polarizing film laminate 10 will be described in detail.
[0038] (First protective film 11) The first protective film 11 is, for example, a laminate of a substrate (not shown) and an adhesive layer (not shown). When the first protective film 11 has a substrate and an adhesive layer, in the example shown in Fig. 2, the first protective film 11 and the first polarizer protective layer 12 are bonded together via the adhesive layer of the first protective film 11.
[0039] The substrate of the first protective film 11 is formed of any appropriate film. Examples of the constituent material of the film include non-transparent materials, specifically, polyester resins such as polyethylene terephthalate resins, polycycloolefin resins such as polynorbornene resins, polyolefin resins such as polypropylene, polyamide resins, polycarbonate resins, copolymer resins thereof, and the like. In this specification, the term "non-transparent material" means a material that is difficult to penetrate with a treatment liquid used in the non-polarizing portion forming step described later. In order to increase the hardness of the substrate of the first protective film 11, a polyester resin is preferable as the constituent material of the substrate. The thickness of the substrate of the first protective film 11 is, for example, 10 μm or more and 200 μm or less, and preferably 20 μm or more and 150 μm or less.
[0040] The adhesive layer of the first protective film 11 is formed of any appropriate adhesive (pressure-sensitive adhesive). Examples of the adhesive include (meth)acrylic adhesives, urethane adhesives, and silicone adhesives. The thickness of the adhesive layer of the first protective film 11 is, for example, 1 μm or more and 20 μm or less, and preferably 2 μm or more and 10 μm or less.
[0041] In order to increase the productivity of the circular polarizing plate by increasing the number of windings of the polarizing film laminate 10, the thickness of the first protective film 11 (for example, the total thickness of the substrate and the adhesive layer) is preferably 50 μm or less, and more preferably 40 μm or less. In order to suppress damage to the first polarizer protective layer 12, the thickness of the first protective film 11 (for example, the total thickness of the substrate and the adhesive layer) is preferably 10 μm or more, and more preferably 20 μm or more. If the thickness of the first protective film 11 is 50 μm or less, hole marks 12b (see FIG. 5) described below are likely to occur.
[0042] (Second protective film 14) The second protective film 14 is, for example, a laminate of a base material (not shown) and an adhesive layer (not shown). When the second protective film 14 has a base material and an adhesive layer, in the example shown in FIG. 2, the second protective film 14 and the polarizer 13 are attached to each other via the adhesive layer of the second protective film 14.
[0043] Examples of the constituent material of the substrate of the second protective film 14 include the materials listed as the constituent materials of the substrate of the first protective film 11 described above. The preferred range of the thickness of the substrate of the second protective film 14 is also the same as the preferred range of the thickness of the substrate of the first protective film 11 described above. The constituent material of the substrate of the first protective film 11 and the constituent material of the substrate of the second protective film 14 may be the same or different from each other. Furthermore, the thickness of the substrate of the first protective film 11 and the thickness of the substrate of the second protective film 14 may be the same or different from each other.
[0044] Examples of the adhesive constituting the adhesive layer of the second protective film 14 include those listed as the adhesive constituting the adhesive layer of the first protective film 11 described above. The preferred range of the thickness of the adhesive layer of the second protective film 14 is also the same as the preferred range of the thickness of the adhesive layer of the first protective film 11 described above. The adhesive constituting the adhesive layer of the first protective film 11 and the adhesive constituting the adhesive layer of the second protective film 14 may be the same or different from each other. Furthermore, the thickness of the adhesive layer of the first protective film 11 and the thickness of the adhesive layer of the second protective film 14 may be the same or different from each other.
[0045] Further, through holes 14a are formed in the second protective film 14. The method for forming the through holes 14a is not particularly limited, and examples thereof include mechanical processing, laser processing, and etching processing using a chemical reaction.
[0046] In order to increase the productivity of the circular polarizing plate by increasing the number of windings of the polarizing film laminate 10 while forming the non-polarizing portion 13a (see Figure 4) to an appropriate size in the non-polarizing portion forming process described below, the thickness of the second protective film 14 (e.g., the total thickness of the substrate and adhesive layer) is preferably 20 μm or more and 150 μm or less, more preferably 25 μm or more and 150 μm or less, and even more preferably 30 μm or more and 150 μm or less.
[0047] (Polarizer 13) The polarizer 13 includes, for example, a resin film, and preferably includes a polyvinyl alcohol-based resin film containing a dichroic material. Hereinafter, the polyvinyl alcohol-based resin may be referred to as a "PVA-based resin." The polarizer 13 may be a single-layer resin film or a laminate of two or more layers.
[0048] Examples of the dichroic substance include iodine and organic dyes. The dichroic substances can be used alone or in combination. A preferred dichroic substance is iodine. When iodine is used as the dichroic substance, the iodine complex contained in the polarizer 13 can be appropriately reduced by contacting the portion of the polarizer 13 exposed from the through hole 14a with a treatment liquid in the non-polarizing portion forming step described below. This allows appropriate characteristics (light transmittance, etc.) to be imparted to the formed non-polarizing portion 13a (see FIG. 4).
[0049] When the polarizer 13 is composed of a single-layer resin film, a specific example of the polarizer 13 is a PVA-based resin film that has been subjected to a dyeing treatment with iodine and a stretching treatment (typically, uniaxial stretching). The dyeing with iodine is performed, for example, by immersing the PVA-based resin film in an iodine aqueous solution. The stretching ratio of the uniaxial stretching is preferably 3 times or more and 7 times or less. The stretching may be performed after the dyeing treatment or while dyeing. Alternatively, the stretching may be performed after dyeing. If necessary, the PVA-based resin film is subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based resin film in water and washing it before dyeing, it is possible to remove dirt and antiblocking agents on the surface of the PVA-based resin film while swelling the PVA-based resin film and preventing uneven dyeing.
[0050] When the polarizer 13 is a laminate of two or more layers, a specific example of the polarizer 13 is a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate. When the polarizer 13 is a laminate of a resin substrate and a PVA-based resin layer laminated on the resin substrate, the PVA-based resin layer is disposed on the second protective film 14 side.
[0051] The polarizer 13 consisting of a laminate of two or more layers can be produced, for example, by applying a PVA-based resin solution to a resin substrate, drying the PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer, and stretching and dyeing the laminate. When stretching, for example, the laminate is immersed in an aqueous boric acid solution and stretched. The obtained laminate of the resin substrate / PVA-based resin layer may be used as it is, or the resin substrate may be peeled off from the laminate of the resin substrate / PVA-based resin layer, and any suitable protective layer may be laminated on the peeled surface according to the purpose. Details of the method for producing such a polarizer are described, for example, in JP-A-2012-73580 and JP-A-6470455.
[0052] The thickness of the polarizer 13 is preferably 15 μm or less, more preferably 12 μm or less, still more preferably 10 μm or less, and particularly preferably 8 μm or less. The thickness of the polarizer 13 is, for example, 1 μm or more, and preferably 3 μm or more.
[0053] The polarizer 13 preferably exhibits absorption dichroism at any wavelength of 380 nm or more and 780 nm or less. The single transmittance of the polarizer 13 is, for example, 41.5% or more and 46.0% or less, preferably 43.0% or more and 46.0% or less, and more preferably 44.5% or more and 46.0% or less. The polarization degree of the polarizer 13 is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.
[0054] (First polarizer protection layer 12) The first polarizer protective layer 12 is made of any appropriate film that can be used as a protective layer for the polarizer 13. The film may be a laminate of two or more layers. Specific examples of the constituent material of the film include cellulose-based resins such as triacetyl cellulose (TAC), polyester-based resins, polyvinyl alcohol-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyethersulfone-based resins, polysulfone-based resins, polystyrene-based resins, polycycloolefin-based resins, polyolefin-based resins, (meth)acrylic-based resins, acetate-based resins, urethane-based resins, (meth)acrylic urethane-based resins, epoxy-based resins, silicone-based resins, and the like.
[0055] In order to reliably protect the polarizer 13, the pencil hardness of the surface 12a (see FIG. 2) of the first polarizer protective layer 12 on the first protective film 11 side is preferably 4B or more, more preferably 3B or more, and even more preferably 2B or more. In order to improve the handleability of the polarizing film laminate 10, the pencil hardness of the surface 12a of the first polarizer protective layer 12 on the first protective film 11 side is preferably H or less. The pencil hardness of the surface 12a can be adjusted, for example, by changing the type of constituent material of the first polarizer protective layer 12. In order to adjust the pencil hardness of the surface 12a to 4B or more, the constituent material of the first polarizer protective layer 12 is preferably a polyolefin-based resin such as a polyethylene-based resin, a polycycloolefin-based resin such as a polynorbornene-based resin, a polyester-based resin such as a polyethylene terephthalate-based resin, a polyamide-based resin, or a polycarbonate-based resin, and more preferably a polycycloolefin-based resin such as a polynorbornene-based resin. When the pencil hardness of the surface 12a is 4B or more, hole marks 12b (see FIG. 5) described later are likely to occur.
[0056] The thickness of the first polarizer protective layer 12 is, for example, 300 μm or less, preferably 100 μm or less, more preferably 5 μm or more and 80 μm or less, and still more preferably 10 μm or more and 60 μm or less.
[0057] (Adhesive layer 15) The adhesive constituting the adhesive layer 15 is not particularly limited, and examples thereof include a thermosetting adhesive and an active energy ray curing adhesive, and an active energy ray curing adhesive is preferred from the viewpoint of improving productivity. Specific examples of the adhesive constituting the adhesive layer 15 include an epoxy resin adhesive, a silicone resin adhesive, an acrylic resin adhesive, a polyurethane adhesive, a polyamide adhesive, a polyether adhesive, and the like.
[0058] The thickness of the adhesive layer 15 is, for example, not less than 0.1 μm and not more than 3.0 μm, and preferably not less than 0.5 μm and not more than 2.8 μm.
[0059] [Non-polarized portion forming process] Next, the non-polarizing portion forming step will be described with reference to Fig. 3 and Fig. 4. Fig. 3 is a process diagram showing an example of the step of forming a non-polarizing portion. Fig. 4 is a partial cross-sectional view showing an example of a polarizing film laminate after the non-polarizing portion has been formed.
[0060] In the non-polarizing portion forming step, as shown in Fig. 3, while polarizing film laminate 10 is unwound from polarizing film laminate roll 100 in the direction of the arrow in the figure, the portions of polarizer 13 exposed from through holes 14a are brought into contact with treatment liquid 21 to be decolorized, thereby forming non-polarizing portions 13a (see Fig. 4). Hereinafter, the portions of polarizer 13 exposed from through holes 14a may be simply referred to as "exposed portions".
[0061] An example of the treatment liquid 21 is a basic solution. The method for bringing the treatment liquid 21 into contact with the exposed area is not particularly limited, and an example thereof is a method in which the polarizing film laminate 10 is immersed in the treatment liquid 21 while being transported, as shown in Fig. 3. After the polarizing film laminate 10 is immersed in the treatment liquid 21, the polarizing film laminate 10 may be washed by being immersed in a cleaning liquid 22 (e.g., water, alcohol, or a mixture thereof) while being transported, as shown in Fig. 3.
[0062] When the polarizer 13 contains iodine as a dichroic material, the iodine content of the exposed areas decreases when a basic solution is brought into contact with the exposed areas, whereby the exposed areas can be bleached and a plurality of non-polarizing portions 13a are formed in the polarizer 13.
[0063] The content of the dichroic material (specifically, iodine, etc.) in the non-polarized portion 13a is preferably 1.0% by weight or less, more preferably 0.5% by weight or less, and even more preferably 0.2% by weight or less. If the content of the dichroic material in the non-polarized portion 13a is within such a range, the non-polarized portion 13a can be sufficiently given the desired transparency. As a result, when the non-polarized portion 13a is associated with a camera portion of an image display device, excellent photographing performance can be achieved in terms of both brightness and color. On the other hand, the lower limit of the content of the dichroic material in the non-polarized portion 13a is usually below the detection limit. When iodine is used as the dichroic material, the iodine content can be determined, for example, from a calibration curve prepared in advance using a standard sample from X-ray intensity measured by fluorescent X-ray analysis.
[0064] The difference between the content of the dichroic material in the non-polarizing section 13a and the content of the dichroic material in the non-polarizing section 13a of the polarizer 13 is preferably 0.5% by weight or more, and more preferably 1% by weight or more. If the difference in content is within this range, the non-polarizing section 13a having high transparency can be formed.
[0065] The light transmittance of the non-polarized section 13a (for example, the light transmittance measured with light of a wavelength of 550 nm at 23° C.) is preferably 50% or more, more preferably 60% or more, even more preferably 75% or more, and particularly preferably 90% or more. Such a light transmittance increases the transparency of the non-polarized section 13a. As a result, when the non-polarized section 13a is associated with a camera section of an image display device, excellent photographing performance can be achieved in terms of both brightness and color.
[0066] The basic solution includes a basic compound and a solvent for dispersing and / or dissolving the basic compound. Any appropriate basic compound can be used as the basic compound. Examples of the basic compound include hydroxides of alkali metals such as sodium hydroxide, potassium hydroxide, and lithium hydroxide; hydroxides of alkaline earth metals such as calcium hydroxide; inorganic alkali metal salts such as sodium carbonate; organic alkali metal salts such as sodium acetate; and ammonia. These basic compounds can be used alone or in combination. Examples of preferred basic compounds include hydroxides of alkali metals and / or alkaline earth metals. Examples of more preferred basic compounds include sodium hydroxide, potassium hydroxide, and lithium hydroxide. When the basic compound includes hydroxides of alkali metals and / or alkaline earth metals, the iodine complex can be efficiently ionized, and the non-polarized portion 13a can be more easily formed.
[0067] Any appropriate solvent can be used as the solvent for the basic solution. Examples of the solvent include water; alcohols such as ethanol and methanol; ether; benzene; chloroform; and mixed solvents thereof. Examples of the preferred solvent include water and alcohol. When the solvent contains water and / or alcohol, iodine ions can be smoothly transferred from the polarizer 13 to the solvent, and the iodine ions can be easily removed when the basic solution is removed.
[0068] The concentration (normality) of the basic compound in the basic solution is, for example, from 0.01 N to 5 N, preferably from 0.05 N to 3 N, and more preferably from 0.1 N to 2.5 N. When the concentration of the basic compound is within such a range, the iodine concentration in the exposed portion can be efficiently reduced, and ionization of the iodine complex in the polarizer 13 other than the exposed portion can be suppressed.
[0069] In the non-polarized portion forming step, the polarized film laminate 10 may be immersed in a post-treatment liquid 23 (e.g., an acidic solution) after contacting the exposed areas with the treatment liquid 21. In the example shown in Fig. 3, after contacting the exposed areas with the treatment liquid 21, the polarized film laminate 10 is immersed in a cleaning liquid 22 while being transported, and then immersed in a post-treatment liquid 23. After immersing the polarized film laminate 10 in the post-treatment liquid 23, the polarized film laminate 10 may be washed by immersing it in a cleaning liquid 24 (e.g., water, alcohol, or a mixture thereof) while being transported, as shown in Fig. 3.
[0070] When the treatment liquid 21 is brought into contact with the exposed areas to form the non-polarized sections 13a, metal salts of alkali metals and / or alkaline earth metals may be generated in the non-polarized sections 13a. Hydroxide ions may be generated from these metal salts. The generated hydroxide ions may act (decompose or reduce) on dichroic substances (e.g., iodine complexes) present around the non-polarized sections 13a, expanding the non-polarized regions (low concentration regions). By performing a post-treatment process to reduce the metal salts of alkali metals and / or alkaline earth metals, the expansion of the non-polarized regions is suppressed, and therefore dimensional changes in the non-polarized sections 13a can be suppressed.
[0071] A representative metal salt capable of generating the hydroxide ions is borate, which can be generated, for example, by neutralizing the boric acid used in the stretching treatment with a basic solution (representatively, a solution of an alkali metal hydroxide and / or an alkaline earth metal hydroxide).
[0072] When the post-treatment liquid 23 (typically, an acidic solution) is brought into contact with the non-polarized section 13a, the metal salt of the alkali metal and / or alkaline earth metal can be transferred to the post-treatment liquid 23, and the content of the metal salt of the alkali metal and / or alkaline earth metal in the non-polarized section 13a can be reduced. In particular, when the post-treatment liquid 23 is an acidic solution, the hydroxide of the alkali metal and / or alkaline earth metal remaining in the non-polarized section 13a can be neutralized, and the alkali metal and / or alkaline earth metal can be chemically removed.
[0073] The content of alkali metal and / or alkaline earth metal salt in non-polarizing portion 13a after the post-treatment step is preferably 3.6% by weight or less, more preferably 2.5% by weight or less, even more preferably 1.0% by weight or less, and particularly preferably 0.5% by weight or less.
[0074] The acidic solution includes an acidic compound and a solvent for dispersing and / or dissolving the acidic compound. Any appropriate acidic compound can be used as the acidic compound. Examples of the acidic compound include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, hydrogen fluoride, and boric acid; and organic acids such as formic acid, oxalic acid, citric acid, acetic acid, and benzoic acid. The acidic compounds can be used alone or in combination. Preferred examples of the acidic compound include inorganic acids, and more preferred examples of the acidic compound include hydrochloric acid, sulfuric acid, and nitric acid.
[0075] As the solvent for the acidic solution, any suitable solvent can be used, including those listed above as the solvent for the basic solution.
[0076] The concentration (normality) of the acidic compound in the acidic solution is, for example, 0.01N or more and 5N or less, preferably 0.05N or more and 3N or less, and more preferably 0.1N or more and 2.5N or less.
[0077] In the example shown in Fig. 3, the polarizing film laminate 10 is immersed in a cleaning solution 24, and then, for example, a drying step (not shown) is performed, and then the polarizing film laminate 10 is wound up. The preferred range of the winding tension when winding the polarizing film laminate 10 is, for example, the same as the preferred range of the winding tension when winding the polarizing film laminate 10 in the above-mentioned roll preparation step. Note that, when winding the polarizing film laminate 10, the first protective film 11 and the second protective film 14 may be peeled off from the polarizing film laminate 10 while winding it up. In other words, the step of winding the polarizing film laminate 10 shown in Fig. 3 may also serve as the protective film peeling step described below.
[0078] [Protective film peeling process] Next, the protective film peeling step will be described. In the protective film peeling step, the first protective film 11 and the second protective film 14 are peeled off from the polarizing film laminate 10. In the following description, the polarizing film laminate after the first protective film and the second protective film are peeled off may be referred to as a "single-sided protective layer-attached polarizing plate."
[0079] The method of peeling the first protective film 11 and the second protective film 14 from the polarizing film laminate 10 is not particularly limited, and examples thereof include a method of peeling the first protective film 11 and the second protective film 14 from the polarizing film laminate 10 while transporting the polarizing film laminate 10 using a roll-to-roll type peeling device (not shown). By carrying out the protective film peeling step, a single-sided protective layer-attached polarizing plate 30 shown in FIG. 5 is obtained. In the single-sided protective layer-attached polarizing plate 30, a polarizer 13 having a non-polarizing portion 13a and a first polarizer protective layer 12 are laminated via an adhesive layer 15. In addition, in the single-sided protective layer-attached polarizing plate 30 obtained from the polarizing film laminate 10 of the second or subsequent round in FIG. 2, as shown in FIG. 5, a hole mark 12b is formed in a portion of the first polarizer protective layer 12 corresponding to the above-mentioned X portion (see FIG. 2).
[0080] In order to increase the productivity of the circular polarizer by increasing the number of windings of the polarizer 30 with a single-side protective layer, the thickness of the polarizer 30 with a single-side protective layer is preferably 50 μm or less, more preferably 40 μm or less. In addition, in order to improve the handleability of the polarizer 30 with a single-side protective layer, the thickness of the polarizer 30 with a single-side protective layer is preferably 10 μm or more, more preferably 15 μm or more. In addition, when the thickness of the polarizer 30 with a single-side protective layer is 50 μm or less, if the surface 12a on which the hole trace 12b of the first polarizer protective layer 12 is formed is arranged on the viewing side of the polarizer 13 when forming an image display device, the hole trace 12b tends to become apparent and a defective appearance tends to occur. As will be described later, in the circular polarizer obtained in this embodiment, the polarizer 13 is arranged on the viewing side of the hole trace 12b when forming an image display device. Therefore, in this embodiment, even if the thickness of the polarizer 30 with a single-side protective layer is 50 μm or less, the occurrence of a defective appearance can be suppressed.
[0081] [Second polarizer protective layer lamination process] Next, the second polarizer protective layer lamination step will be described with reference to Fig. 5 and Fig. 6. Fig. 6 is a partial cross-sectional view showing an example of a polarizing film laminate after the second polarizer protective layer is laminated. In the second polarizer protective layer lamination step, the second polarizer protective layer 42 is laminated on the surface 13b (see Fig. 5) of the polarizer 13 from which the second protective film 14 has been peeled off. In the example shown in Fig. 6, the second polarizer protective layer 42 is laminated on the surface 13b via an adhesive layer 41. Note that in the second polarizer protective layer lamination step, the second polarizer protective layer 42 may be laminated on the surface 13b via a pressure-sensitive adhesive layer (not shown).
[0082] The method for laminating the second polarizer protective layer 42 to surface 13b via the adhesive layer 41 is not particularly limited, and examples include a method in which a roll-to-roll laminating device (not shown) is used to transport the polarizing plate 30 with a single-sided protective layer while laminating (bonding) the second polarizer protective layer 42 to surface 13b via the adhesive layer 41.
[0083] Examples of the material of the second polarizer protective layer 42 include the materials listed as the materials of the first polarizer protective layer 12. The preferred range of the thickness of the second polarizer protective layer 42 is the same as the preferred range of the thickness of the first polarizer protective layer 12. The material of the first polarizer protective layer 12 and the material of the second polarizer protective layer 42 may be the same as or different from each other. The thickness of the first polarizer protective layer 12 and the thickness of the second polarizer protective layer 42 may be the same as or different from each other.
[0084] Examples of the adhesive constituting the adhesive layer 41 include the adhesives listed as the adhesives constituting the adhesive layer 15 described above. The preferred range of the thickness of the adhesive layer 41 is also the same as the preferred range of the thickness of the adhesive layer 15 described above. The adhesive constituting the adhesive layer 15 and the adhesive constituting the adhesive layer 41 may be the same as or different from each other. Furthermore, the thickness of the adhesive layer 15 and the thickness of the adhesive layer 41 may be the same as or different from each other.
[0085] The second polarizer protective layer lamination step may be performed before or after the retardation layer lamination step described below.
[0086] [Retardation layer lamination process] Next, the retardation layer lamination step will be described with reference to FIG. 7. FIG. 7 is a partial cross-sectional view showing an example of a circular polarizer obtained by the manufacturing method of this embodiment. In the retardation layer lamination step, a retardation layer is laminated on the opposite side of the polarizer 13 side of the first polarizer protective layer 12. In the example shown in FIG. 7, the first retardation layer 52 is bonded to the surface 12a of the first polarizer protective layer 12 opposite the polarizer 13 side via an adhesive layer 51, and then the second retardation layer 54 is bonded to the surface 52a of the first retardation layer 52 opposite the adhesive layer 51 side via an adhesive layer 53. This results in a circular polarizer 200. Note that after the first retardation layer 52 and the second retardation layer 54 are bonded to the surface 12a of the first polarizer protective layer 12 opposite the polarizer 13 side via the adhesive layer 53, the first retardation layer 52 may be bonded to the surface 12a of the first polarizer protective layer 12 opposite the polarizer 13 side via the adhesive layer 51.
[0087] The method of laminating the retardation layer in the retardation layer lamination step is not particularly limited as long as it is a method of laminating the retardation layer on the side opposite the polarizer 13 side of the first polarizer protective layer 12. Specific examples of the method of laminating the retardation layer include a method of laminating the retardation layer on the side opposite the polarizer 13 side of the first polarizer protective layer 12 by the lamination method described in JP-A-2021-18354.
[0088] On the other hand, as a lamination method different from the example shown in FIG. 7, a method of laminating a retardation layer on the surface 42a (see FIG. 6) opposite to the adhesive layer 41 side of the second polarizer protective layer 42 is also considered. However, when a retardation layer is laminated on the surface 42a opposite to the adhesive layer 41 side of the second polarizer protective layer 42, when the obtained circular polarizing plate is used in an image display device, the hole trace 12b is located on the viewing side of the polarizer 13, and the hole trace 12b becomes apparent. As a result, appearance defects are likely to occur. In contrast, in this embodiment, a retardation layer (the first retardation layer 52 and the second retardation layer 54 in the example of FIG. 7) is laminated on the side opposite to the polarizer 13 side of the first polarizer protective layer 12, so that when the obtained circular polarizing plate 200 is used in an image display device, the polarizer 13 is located on the viewing side of the hole trace 12b. As a result, the hole trace 12b becomes less noticeable in appearance, and therefore, according to this embodiment, it is possible to suppress the occurrence of appearance defects caused by the hole trace 12b.
[0089] The first retardation layer 52 may be, for example, a liquid crystal alignment solidified layer. The term "liquid crystal alignment solidified layer" refers to an alignment solidified layer of a liquid crystal compound. The term "alignment solidified layer" refers to a layer in which a compound is aligned in a predetermined direction within the layer and the alignment state is fixed. By using a liquid crystal compound for the alignment solidified layer, the difference between nx and ny of the resulting liquid crystal alignment solidified layer can be significantly increased compared to non-liquid crystal materials, so that the thickness of the liquid crystal alignment solidified layer for obtaining a desired in-plane retardation can be significantly reduced. As a result, a thin and lightweight circular polarizer can be achieved. When a thin circular polarizer is used for an image display device, if the surface 12a on which the hole trace 12b of the first polarizer protective layer 12 is formed is arranged on the viewing side of the polarizer 13, the hole trace 12b tends to become apparent and cause a defective appearance. In the circular polarizer obtained in this embodiment, the polarizer 13 is arranged on the viewing side of the hole trace 12b when forming the image display device. Therefore, according to this embodiment, even if a thin circular polarizing plate (a circular polarizing plate having a thin retardation layer) is used, the occurrence of defective appearance can be suppressed.
[0090] When the first retardation layer 52 is a liquid crystal alignment solidified layer, the liquid crystal alignment solidified layer is not particularly limited, and for example, the liquid crystal alignment solidified layer described in JP 2021-18354 A can be used. The liquid crystal alignment solidified layer is preferably a liquid crystal alignment solidified layer that functions as a quarter-wave plate. When the first retardation layer 52 is a liquid crystal alignment solidified layer that functions as a quarter-wave plate, the thickness of the first retardation layer 52 is, for example, 0.2 μm or more and 10 μm or less, preferably 0.5 μm or more and 7 μm or less.
[0091] When the first retardation layer 52 is a liquid crystal alignment solidified layer functioning as a quarter-wave plate, the second retardation layer 54 is preferably a positive C plate. In this configuration, a circular polarizing plate capable of blocking reflected light even from external light coming from an oblique direction can be formed. When the second retardation layer 54 is a positive C plate, the thickness of the second retardation layer 54 is, for example, 0.2 μm or more and 10 μm or less, and preferably 0.5 μm or more and 7 μm or less.
[0092] The first retardation layer 52 may be a liquid crystal alignment layer functioning as a half-wave plate. When the first retardation layer 52 is a liquid crystal alignment layer functioning as a half-wave plate, the thickness of the first retardation layer 52 is, for example, 0.2 μm to 10 μm, and preferably 0.5 μm to 7 μm.
[0093] When the first retardation layer 52 is a liquid crystal alignment solidified layer functioning as a 1 / 2 wavelength plate, the second retardation layer 54 is preferably a liquid crystal alignment solidified layer functioning as a 1 / 4 wavelength plate. In this case, it is preferable to arrange them so that the angle between the slow axis direction of the 1 / 2 wavelength plate and the absorption axis direction of the polarizer 13 is 75°±5°, and the angle between the slow axis direction of the 1 / 4 wavelength plate and the absorption axis direction of the polarizer 13 is 15°±5°. A circular polarizer having such a layer structure functions as a circular polarizer over a wide wavelength range of visible light, and therefore can reduce coloring of reflected light.
[0094] Examples of the adhesive constituting the adhesive layer 51 include the adhesives listed as the adhesives constituting the adhesive layer 15 described above. The preferred range of the thickness of the adhesive layer 51 is also the same as the preferred range of the thickness of the adhesive layer 15 described above. The adhesive constituting the adhesive layer 15 and the adhesive constituting the adhesive layer 51 may be the same as or different from each other. Furthermore, the thickness of the adhesive layer 15 and the thickness of the adhesive layer 51 may be the same as or different from each other.
[0095] Examples of the adhesive constituting the adhesive layer 53 include the adhesives listed as the adhesives constituting the adhesive layer 15 described above. The preferred range of the thickness of the adhesive layer 53 is also the same as the preferred range of the thickness of the adhesive layer 15 described above. The adhesive constituting the adhesive layer 15 and the adhesive constituting the adhesive layer 53 may be the same or different from each other. Furthermore, the thickness of the adhesive layer 15 and the thickness of the adhesive layer 53 may be the same or different from each other.
[0096] Although the retardation layer lamination step has been described above, in the present invention, only one retardation layer (e.g., a quarter wavelength plate) may be laminated on the opposite side of the first polarizer protective layer from the polarizer side. In addition, in the present invention, a retardation layer may be laminated on the opposite side of the first polarizer protective layer from the polarizer side via a pressure-sensitive adhesive layer.
[0097] [Conditions under which the effects of this embodiment are effectively exhibited] As described above, the manufacturing method of the circularly polarizing plate according to this embodiment can suppress the occurrence of defective appearance caused by hole marks. In this embodiment, by satisfying the following condition 1, the effect of this embodiment can be more effectively exhibited. Furthermore, in this embodiment, by satisfying the following condition 2, the effect of this embodiment can be more effectively exhibited. Furthermore, in this embodiment, by satisfying the following condition 3, the effect of this embodiment can be particularly effectively exhibited. Condition 1: The thickness of the first protective film is 50 μm or less, and the thickness of the polarizing plate with a single-sided protective layer is 50 μm or less. Condition 2: The above condition 1 is satisfied, and the surface of the first polarizer protective layer facing the first protective film has a pencil hardness of 4B or more. Condition 3: The above condition 2 is satisfied, and the diameter of the opening of the through hole in the second protective film is 1 mm or more and 10 mm or less.
[0098] Although the manufacturing method of the circular polarizer according to the present embodiment has been described above, the manufacturing method of the circular polarizer according to the present invention is not limited to the above embodiment. For example, the manufacturing method of the circular polarizer according to the present invention may further include a step of laminating an adhesive layer (hereinafter, referred to as "outer adhesive layer") on the opposite side of the first polarizer protective layer of the retardation layer after the retardation layer lamination step. The retardation layer is bonded to an image display cell (for example, a liquid crystal cell, an organic EL cell, etc.) via this outer adhesive layer to form an image display device. The adhesive constituting the outer adhesive layer is not particularly limited, and for example, a transparent adhesive having a base polymer such as an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyvinyl ether, a vinyl acetate-vinyl chloride copolymer, a modified polyolefin, an epoxy resin, a fluorine resin, a natural rubber, or a synthetic rubber can be appropriately selected and used. The thickness of the outer adhesive layer is not particularly limited, but is preferably 5 μm or more and 100 μm or less from the viewpoint of achieving both thinness and adhesiveness.
[0099] The method for producing a circularly polarizing plate according to the present invention may further include a step of temporarily attaching a release liner to the main surface of the outer pressure-sensitive adhesive layer opposite to the retardation layer side. The release liner protects the surface of the outer pressure-sensitive adhesive layer, for example, until the retardation layer is bonded to the image display cell. As a constituent material of the release liner, a plastic film formed from acrylic, polyolefin, cyclic polyolefin, polyester, etc. is preferably used. The thickness of the release liner is, for example, 5 μm or more and 200 μm or less. The surface of the release liner is preferably subjected to a release treatment. Examples of the material of the release agent used in the release treatment include silicone-based materials, fluorine-based materials, long-chain alkyl-based materials, and fatty acid amide-based materials.
[0100] In the method for producing a circularly polarizing plate according to the present invention, the step of laminating a second polarizer protective layer is not an essential step. For example, instead of the second polarizer protective layer, a pressure-sensitive adhesive layer and a release liner may be laminated in this order on the polarizer. [Explanation of symbols]
[0101] 10: Polarizing film laminate 11: First protective film 12: First polarizer protection layer 13: Polarizer 13a: Non-polarizing part 14: Second protective film 14a: Through hole 21: Processing liquid 42: Second polarizer protection layer 52: 1st retardation layer (retardation layer) 54:Second retardation layer (retardation layer) 200: Circular polarizing plate
Claims
1. a step Sa of preparing a roll of a polarizing film laminate including, in this order, a first protective film, a first polarizer protective layer, a polarizer, and a second protective film having a through hole; a step Sb of bringing a portion of the polarizer exposed through the through hole into contact with a treatment liquid while unwinding the polarizing film laminate from the roll to decolorize the portion, thereby forming a non-polarizing portion; a step Sc of peeling off the first protective film and the second protective film from the polarizing film laminate; a step Sd of laminating a retardation layer on the side of the first polarizer protection layer opposite to the polarizer side; The method for producing a circularly polarizing plate comprises the steps of:
2. The method for producing a circularly polarizing plate according to claim 1 , further comprising, after the step Sc, a step Se of laminating a second polarizer protective layer on the surface of the polarizer from which the second protective film has been peeled off.
3. The method for producing a circularly polarizing plate according to claim 1 , wherein the first protective film has a thickness of 50 μm or less.
4. The method for producing a circularly polarizing plate according to claim 1 , wherein the polarizing film laminate has a thickness of 50 μm or less after the first protective film and the second protective film are peeled off in the step Sc.
5. The method for producing a circularly polarizing plate according to claim 1 , wherein the first polarizer protection layer and the polarizer are bonded to each other with an adhesive.
6. The method for producing a circularly polarizing plate according to claim 1 , wherein a pencil hardness of a surface of the first polarizer protective layer facing the first protective film is 4B or more.
7. The method for producing a circularly polarizing plate according to claim 1 , wherein the second protective film has a thickness of 20 μm or more and 150 μm or less.
8. The method for producing a circularly polarizing plate according to claim 1 , wherein the through hole has an opening diameter of 1 mm or more and 10 mm or less.
Citation Information
Patent Citations
Polarizing film laminate, and method for manufacturing polarizer having non-polarizing part by using the polarizing film laminate
JP2016053645A
Cited By
Semiconductor device and semiconductor memory device
CN121711994A