Semiconductor device
The semiconductor device design addresses miniaturization and integration challenges by using In-Ga-Zn oxide and high-k gate insulators to improve electrical and frequency characteristics, reliability, and reduce power consumption, achieving high productivity and flexibility.
Patent Information
- Application Number
- JP2024148116
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-02-20
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2038-07-26
AI Technical Summary
Existing semiconductor devices face challenges in miniaturization, integration, electrical characteristics, frequency performance, reliability, data retention, writing speed, power consumption, and design flexibility, while maintaining high productivity and reliability.
A semiconductor device design featuring a specific configuration of oxide layers, conductors, and insulators with controlled film thicknesses and alignments, utilizing materials like In-Ga-Zn oxide and high-k gate insulators to enhance electrical properties and reduce parasitic capacitance.
The design enables miniaturization and high integration, improves electrical and frequency characteristics, enhances reliability, extends data retention, reduces power consumption, and increases writing speed, while maintaining stable electrical performance.
Smart Images

Figure 2024163154000001_ABST
Abstract
Description
[Technical field]
[0001] One embodiment of the present invention relates to a semiconductor device and a manufacturing method of the semiconductor device. One aspect of the invention relates to a semiconductor wafer, a module, and an electronic device.
[0002] In this specification and the like, a semiconductor device refers to a device that can function by utilizing semiconductor characteristics. This refers to semiconductor devices in general, including semiconductor elements such as transistors, semiconductor circuits, arithmetic units, and memory devices. The device is one aspect of a semiconductor device. device, lighting device, electro-optical device, power storage device, memory device, semiconductor circuit, imaging device, and There are cases where the child devices and the like can be said to have semiconductor devices.
[0003] Note that one embodiment of the present invention is not limited to the above technical fields. An aspect of the present invention relates to an article, a method, or a manufacturing method. is a process, machine, manufacture, or composition of matter. This concerns the issue of the [Background technology]
[0004] In recent years, the development of semiconductor devices has progressed, and LSIs, CPUs, and memories are mainly used. A CPU is a semiconductor integrated circuit (at least transistors and The semiconductor device is an assembly of semiconductor elements having a memory and electrodes that serve as connection terminals.
[0005] Semiconductor circuits (IC chips) such as LSI, CPU, and memory are mounted on circuit boards, e.g. They are mounted on printed wiring boards and used as components in a variety of electronic devices.
[0006] In addition, a transistor is formed using a semiconductor thin film formed on a substrate having an insulating surface. The transistor is used in integrated circuits (ICs) and image display devices (simply called displays). It is widely used in electronic devices such as transistors. Silicon-based semiconductor materials are widely known as semiconductor thin films that can be used, but other materials and Oxide semiconductors have been attracting attention as a new type of semiconductor.
[0007] In addition, a transistor including an oxide semiconductor has a very low leakage current in a non-conducting state. For example, the leakage current of a transistor using an oxide semiconductor is known to be small. A low-power CPU that utilizes this characteristic has been disclosed (see Patent Document 1). ).
[0008] In addition, a transistor using an oxide semiconductor is manufactured by embedding a gate electrode in an opening. A method for doing so has been disclosed (see Patent Document 2).
[0009] In recent years, as electronic devices have become smaller and lighter, transistors and other components have become more densely integrated. In addition, there is a demand for improved productivity of semiconductor devices including integrated circuits. It is being considered.
[0010] Examples of oxide semiconductors include oxides of single-element metals such as indium oxide and zinc oxide. In addition, oxides of multi-component metals are also known. Among the oxides of multi-component metals, in particular, Research on In-Ga-Zn oxide (hereinafter referred to as IGZO) is being actively conducted. do.
[0011] Research on IGZO has revealed that, among oxide semiconductors, IGZO is neither single crystal nor amorphous. AAC (c-axis aligned crystalline) structure and nc (n A crystalline structure was found (see Non-Patent Documents 1 to 3). In Non-Patent Documents 1 and 2, oxide semiconductors having a CAAC structure are used. Furthermore, a technology for fabricating a transistor using a CAAC structure and an nc structure has been disclosed. It has been reported in Non-Patent Documents 4 and 5 that even oxide semiconductors with lower crystallinity than and in Non-Patent Document 5.
[0012] Furthermore, transistors using IGZO as an active layer have extremely low off-state current (non- See Patent Document 6.) LSIs and displays that utilize these properties have been reported ( See non-patent literature 7 and non-patent literature 8. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] JP 2012-257187 A [Patent Document 2] JP 2017-050530 A [Non-patent literature]
[0014] [Non-Patent Document 1] S. Yamazaki et al., “SID Symposium Digest of Technical Papers”, 2012, volume 43, issue 1, p.183-186 [Non-Patent Document 2] S. Yamazaki et al., “Japanese Journal of Applied Physics”, 2014, volume 53, Number 4S, p.04ED18-1-04ED18-10 [Non-Patent Document 3] S. Ito et al., “The Proceedings of AM-FPD'13 Digest of Technical Papers”, 2013, p.151-154 [Non-Patent Document 4] S. Yamazaki et al., “ECS Journal of Solid State Science and Technology”, 2014, volume 3, issue 9, p.Q3012-Q3022 [Non-Patent Document 5] S. Yamazaki, “ECS Transactions”,2014, volume 64, issue 10, p.155-164 [Non-Patent Document 6] K. Kato et al., “Japanese Journal of Applied Physics”, 2012, volume 51, p.021201-1-021201-7 [Non-Patent Document 7] S. Matsuda et al., “2015 Symposium on VLSI Technology Digest of Technical Papers”, 2015, p.T216-T217 [Non-Patent Document 8] S. Amano et al., “SID Symposium Digest of Technical Papers”, 2010, volume 41, issue 1, p.626-629 Summary of the Invention [Problem to be solved by the invention]
[0015] An object of one embodiment of the present invention is to provide a semiconductor device that can be miniaturized or highly integrated. One embodiment of the present invention is to provide a semiconductor device having favorable electrical characteristics. One embodiment of the present invention is to provide a semiconductor device having favorable frequency characteristics. An object of one embodiment of the present invention is to provide a semiconductor device with high reliability. An object of one embodiment of the present invention is to provide a semiconductor device with high productivity. It shall be one.
[0016] One embodiment of the present invention is to provide a semiconductor device capable of retaining data for a long period of time. One object of one embodiment of the present invention is to provide a semiconductor device in which data can be written at a high speed. One object of one embodiment of the present invention is to provide a semiconductor device having high design freedom. One object of one embodiment of the present invention is to provide a semiconductor device capable of reducing power consumption. One object of the present invention is to provide a novel semiconductor device. is one of the challenges.
[0017] The description of these problems does not preclude the existence of other problems. It is not necessary for one embodiment to solve all of these problems. The subject matter will be self-evident from the description, drawings, claims, etc. Other issues can be extracted from the drawings, claims, etc. [Means for solving the problem]
[0018] One aspect of the present invention is a semiconductor device comprising: an oxide; first conductors disposed on the oxide and spaced apart from each other; and a second conductor, and a second conductor is disposed on the first conductor and the second conductor, and the first conductor and the second conductor are disposed on the first conductor and the second conductor. A first insulator having an opening formed therein overlapping the second conductor and a third insulator disposed in the opening. a conductor, an oxide, a first conductor, a second conductor, a first insulator, and a third conductor and a second insulator disposed between the first and second conductive layers, the second insulator being made of an oxide and a third conductive material. Between the first conductor or the second conductor and the third conductor, the first film thickness is formed. and a second thickness between the first and second layers, the first thickness being thinner than the second thickness. It is a semiconductor device.
[0019] In the above, the second insulator has a third insulator and a fourth insulator, The insulator is an oxide, a first conductor, a second conductor, and a first insulator and a third conductor. and a fourth insulator is disposed between the first conductor, the second conductor, and the first insulator. The insulating body may be disposed between the insulating body and a third insulating body.
[0020] In the above, the oxide, the first conductor, the second conductor, the first insulator, A fifth insulator is disposed between the first and second electrodes, the fifth insulator being made of at least one of aluminum and hafnium. It may be an oxide containing at least one of them.
[0021] In the above, the oxide is a material containing In and an element M (M is Al, Ga, Y, or Sn). and Zn.
[0022] In another embodiment of the present invention, a first oxide and a second oxide are disposed on the first oxide at a distance from each other. a first conductor and a second conductor disposed on the first conductor and the second conductor; a first insulator having an opening formed therein and overlapping the first conductor and the second conductor; a third conductor disposed in the mouth; and a first oxide, a first conductor, a second conductor, and a second insulator disposed between the first insulator and the third conductor; and a first oxide. A first conductor, a second conductor, and a first insulator and a second insulator are disposed between the first conductor and the second insulator. and a second oxide formed between the first oxide and the third conductor. , having a first thickness, and a third conductor between the first conductor or the second conductor and the third conductor, The semiconductor device has a first thickness and a second thickness, the first thickness being thinner than the second thickness. do.
[0023] In the above, the first oxide, the first conductor, the second conductor, and the first insulator A third insulator is disposed between the edge and the third insulator, the third insulator being made of aluminum and hafnium. The oxide may contain at least one of the above.
[0024] In the above, the fourth insulator is a first conductor, a second conductor, and a first insulator. A fourth insulator is disposed between the insulator and the second oxide and is made of aluminum and hafnium. The oxide may contain at least one of tungsten and tungsten.
[0025] In the above, the first oxide and the second oxide are each composed of In and an element M (M is Al). , Ga, Y, or Sn) and Zn.
[0026] In the above, the upper surface of the first insulator, the upper surface of the third conductor, and the upper surface of the second insulator The upper surfaces of the first insulator and the third conductor may be substantially aligned. A sixth insulator is disposed in contact with an upper surface of the first insulator and an upper surface of the second insulator, and the sixth insulator is It may be an oxide containing aluminum.
[0027] In the above, the first conductor and the second conductor are made of aluminum, chromium, Copper, silver, gold, platinum, tantalum, nickel, titanium, molybdenum, tungsten, hafnium Aluminum, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium At least one of tungsten, ruthenium, iridium, strontium, and lanthanum It is preferable that:
[0028] In the above, the first conductor and the second conductor are made of tantalum nitride, titanium nitride, or the like. titanium and aluminum nitrides, tantalum and aluminum nitrides, ruthenium oxides Ruthenium, ruthenium nitride, oxides containing strontium and ruthenium, and lanthanum and an oxide containing nickel. Effect of the Invention
[0029] According to one embodiment of the present invention, a semiconductor device that can be miniaturized or highly integrated can be provided. According to one embodiment of the present invention, a semiconductor device having favorable electrical characteristics can be provided. According to one embodiment of the present invention, a semiconductor device having favorable frequency characteristics can be provided. According to the present invention, a semiconductor device with high reliability can be provided. As a result, a semiconductor device with high productivity can be provided.
[0030] Alternatively, a semiconductor device capable of retaining data for a long period of time can be provided. Alternatively, a semiconductor device with a high data writing speed can be provided. It is possible to provide a semiconductor device having a high degree of freedom. It is possible to provide a semiconductor device. Alternatively, it is possible to provide a novel semiconductor device. .
[0031] The description of these effects does not preclude the existence of other effects. An embodiment does not necessarily have all of these effects. Effects other than these are described in the specification. The above will become apparent from the description, drawings, claims, etc. From the above description, it is possible to extract other effects. [Brief description of the drawings]
[0032] [Figure 1] 1A and 1B are a top view and a cross-sectional view of a semiconductor device according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view of a semiconductor device according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a cross-sectional view of a semiconductor device according to one embodiment of the present invention. [Figure 4] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Diagram 5] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 6] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 7] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 8] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 9] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 10] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 11] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 12] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 13] 1A and 1B are top views and cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 14] 1A and 1B are a top view and a cross-sectional view of a semiconductor device according to one embodiment of the present invention. [Figure 15] 1A and 1B are a top view and a cross-sectional view of a semiconductor device according to one embodiment of the present invention. [Figure 16] 1A and 1B are a top view and a cross-sectional view of a semiconductor device according to one embodiment of the present invention. [Figure 17] 1A and 1B are a top view and a cross-sectional view of a semiconductor device according to one embodiment of the present invention. [Figure 18] 1A and 1B are a top view and a cross-sectional view of a memory device according to one embodiment of the present invention. [Figure 19] FIG. 1 is a circuit diagram of a memory device according to one embodiment of the present invention. [Figure 20] FIG. 1 is a schematic diagram of a memory device according to one embodiment of the present invention. [Figure 21] FIG. 1 is a schematic diagram of a memory device according to one embodiment of the present invention. [Figure 22] FIG. 1 is a cross-sectional view illustrating a configuration of a memory device according to one embodiment of the present invention. [Figure 23] FIG. 1 is a cross-sectional view illustrating a configuration of a memory device according to one embodiment of the present invention. [Figure 24] FIG. 1 is a block diagram illustrating a configuration example of a storage device according to one embodiment of the present invention. [Diagram 25] FIG. 1 is a circuit diagram illustrating a configuration example of a memory device according to one embodiment of the present invention. [Figure 26] FIG. 1 is a circuit diagram illustrating a configuration example of a memory device according to one embodiment of the present invention. [Figure 27] FIG. 1 is a block diagram illustrating a configuration example of a storage device according to one embodiment of the present invention. [Figure 28] 1A and 1B are a block diagram and a circuit diagram illustrating a configuration example of a memory device of one embodiment of the present invention. [Figure 29] FIG. 1 is a block diagram showing an example of the configuration of an AI system according to one embodiment of the present invention. [Diagram 30] FIG. 1 is a block diagram illustrating an application example of an AI system according to one embodiment of the present invention. [Diagram 31] FIG. 1 is a schematic perspective view showing an example of the configuration of an IC incorporating an AI system according to one embodiment of the present invention. [Diagram 32] 1A to 1C are diagrams illustrating electronic devices according to one embodiment of the present invention. [Diagram 33]1A to 1C are diagrams illustrating electronic devices according to one embodiment of the present invention. [Diagram 34] 1A to 1C are diagrams illustrating electronic devices according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Hereinafter, the embodiments will be described with reference to the drawings. It is understood that the present invention can be practiced in many different ways without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that various changes in form and details may be made. Therefore, the present invention should not be construed as being limited to the description of the following embodiment modes.
[0034] Also, in the drawings, the size, layer thickness, or area are exaggerated for clarity. Therefore, the drawings are not necessarily limited to the scale. The examples are shown in schematic form, and are not limited to the shapes or values shown in the drawings. For example, In the actual manufacturing process, layers and resist masks are damaged by etching and other processes. However, in order to make it easier to understand, it may be omitted. In the drawings, the same parts or parts having similar functions are designated by the same reference numerals in different drawings. In addition, when referring to similar functions, In some cases, the hatch patterns are the same and no particular reference numbers are assigned.
[0035] In addition, the invention is easily understood, particularly in top views (also called "plan views") and perspective views. In order to simplify the description, some of the components may be omitted. The above information may be omitted.
[0036] In addition, in this specification, ordinal numbers such as 1st, 2nd, etc. are used for convenience. It does not indicate the order of processes or stacking. For example, "first" may be changed to "second "the" or "third" can be used as appropriate. The ordinal numbers described herein may not coincide with the ordinal numbers used to identify an aspect of the present invention. There are cases where this is the case.
[0037] In addition, in this specification, the terms "above" and "below" that indicate an arrangement are used to refer to the relationship between components. The positional relationship is used for convenience in describing the drawings. The relationship changes accordingly depending on the direction in which each configuration is depicted. The terms are not limited to those described above, and may be rephrased appropriately depending on the situation.
[0038] For example, in the present specification, it is explicitly stated that X and Y are connected. The cases are when X and Y are electrically connected and when X and Y are functionally connected. The case where X and Y are directly connected and the case where X and Y are directly connected are disclosed in the present specification, etc. Therefore, the connection relationship is limited to a specific one, for example, the connection relationship shown in the figure or text. Connections other than those shown in the drawings or text may not be included in the drawings or text. It shall be so.
[0039] Here, X and Y are objects (e.g., devices, elements, circuits, wiring, electrodes, terminals, conductive films, layer, etc.).
[0040] An example of a direct connection between X and Y is The elements that function as When a diode, display element, light-emitting element, load, etc. is not connected between X and Y, An element (e.g., a switch, transistor, or capacitor) that allows electrical connection between X and Y. (capacitor, inductor, resistor, diode, display element, light-emitting element, load, etc.) In this case, X and Y are connected.
[0041] An example of the case where X and Y are electrically connected is The elements that function as One or more diodes, display elements, light-emitting elements, loads, etc.) are connected between X and Y. The switch has a function of being controlled to be on and off. A switch can be in a conductive state (on) or a non-conductive state (off) to allow current to flow. The switch has the function of controlling whether or not current flows. When X and Y are electrically connected, X This also includes the case where and Y are directly connected.
[0042] An example of a case where X and Y are functionally connected is the case where the functional connection between X and Y is possible. Circuits that perform the functions of the following: logic circuits (inverters, NAND circuits, NOR circuits, etc.), signal Conversion circuits (DA conversion circuits, AD conversion circuits, gamma correction circuits, etc.), potential level conversion circuits ( Power supply circuits (boosting circuits, step-down circuits, etc.), level shifter circuits that change the potential level of signals, etc. ), voltage sources, current sources, switching circuits, amplifier circuits (which can increase the signal amplitude or current amount, etc.) (e.g., circuits that generate One or more devices (such as a synthesis circuit, memory circuit, or control circuit) can be connected between X and Y. For example, even if another circuit is inserted between X and Y, the signal output from X is If the signal is transmitted to Y, then X and Y are considered to be functionally connected. When X and Y are functionally connected, there are cases where X and Y are directly connected and cases where X and Y are functionally connected. This also includes the case where Y is electrically connected.
[0043] In this specification, a transistor includes a gate, a drain, and a source. The drain terminal is a diode that has at least three terminals. (source terminal, source region, or source electrode) and the source (source terminal, source region, or source electrode) A region in which a channel is formed is provided between the first and second electrodes. It is possible to pass a current between the source and the drain. The region where a channel is formed refers to a region through which current mainly flows.
[0044] In addition, the functions of the source and drain may differ depending on whether transistors of different polarities are used or the circuit In operation, when the direction of the current changes, the positions may be reversed. In the specification, the terms source and drain may be used interchangeably. do.
[0045] Note that the channel length is, for example, the length of a semiconductor (or transistor) in a top view of a transistor. When the transistor is in the on state, the gate electrode is connected to the semiconductor (the part of the semiconductor through which current flows) The source (source region or source This refers to the distance between the drain (drain region or drain electrode) and the source (source electrode). In a single transistor, the channel length does not necessarily have the same value in all regions. That is, the channel length of a transistor may not be fixed to a single value. In this specification, the channel length is any one of the values in the region where the channel is formed, This can be the maximum, minimum or average value.
[0046] The channel width is the width of the semiconductor (or transistor) when it is in the on state. The area where the gate electrode overlaps with the current-carrying part of the semiconductor, or the channel, is formed. The length of the part where the source and drain face each other in the region where the source and drain are connected. In a transistor, the channel width does not necessarily have the same value in all regions. That is, the channel width of a transistor may not be fixed to a single value. In this specification, the channel width is any one of the values, the maximum, in the region where the channel is formed. The maximum, minimum, or average value.
[0047] Depending on the structure of the transistor, the channel in the region where the channel is actually formed may be The effective channel width (hereinafter also referred to as the "effective channel width") of the transistor in a top view The channel width indicated by the For example, when the gate electrode covers the side of the semiconductor, the effective channel width becomes In some cases, the effect of the channel width becomes larger than that of the conventional method. In a transistor in which the gate electrode covers the side surface of the semiconductor, the channel formed on the side surface of the semiconductor In this case, the ratio of the channel formation region may be larger than the apparent channel width. , the effective channel width becomes larger.
[0048] In such cases, it may be difficult to estimate the effective channel width through actual measurements. For example, to estimate the effective channel width from the design value, the shape of the semiconductor must be known. Therefore, if the shape of the semiconductor is not known accurately, Channel width is difficult to measure accurately.
[0049] Therefore, in this specification, the apparent channel width is referred to as the "enclosed channel width (SCW: S In addition, in this specification, In this document, when simply referring to channel width, it means enclosed channel width or apparent channel width. In this specification, when the term "channel width" is used, It may refer to the effective channel width. Note that channel length, channel width, and effective channel The channel width, apparent channel width, and enclosed channel width are determined by analyzing cross-sectional TEM images. The value can be determined, for example, by
[0050] The impurities in a semiconductor are, for example, substances other than the main components that make up the semiconductor. Elements with a concentration of less than 0.1 atomic percent can be considered impurities. For example, The DOS (Density of States) of the semiconductor increases and the crystallinity decreases. When the semiconductor is an oxide semiconductor, the semiconductor characteristics may be deteriorated. The impurities to be changed include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, These include elements, Group 15 elements, and transition metals other than the main components of oxide semiconductors, for example: Hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, nitrogen, etc. Oxides In the case of a semiconductor, water may also function as an impurity. In some cases, oxygen vacancies may be formed due to the inclusion of impurities. In this case, impurities that change the properties of a semiconductor include, for example, oxygen and Group 1 elements excluding hydrogen. , Group 2 elements, Group 13 elements, Group 15 elements, etc.
[0051] In this specification and the like, a silicon oxynitride film is a film having a composition containing more oxygen than nitrogen. For example, the oxygen content is preferably 55 atomic % or more and 65 atomic % or less. , nitrogen is 1 atomic % or more and 20 atomic % or less, silicon is 25 atomic % or more and 35 atomic % or less, hydrogen The concentration range of 0.1 atomic % to 10 atomic % is also called oxynitride. A silicon film is a film whose composition contains more nitrogen than oxygen. Preferably, nitrogen is 55 atomic % or more and 65 atomic % or less, oxygen is 1 atomic % or more and 20 atomic % or less, Silicon concentration is 25 atomic % to 35 atomic % and hydrogen concentration is 0.1 atomic % to 10 atomic % It refers to what is included in the range.
[0052] In addition, in this specification and the like, the terms "film" and "layer" are interchangeable. For example, the term "conductive layer" can be changed to the term "conductive film." Alternatively, for example, the term "insulating film" may be changed to "insulating layer." It may be possible to change the term to:
[0053] In addition, in this specification, the term "insulator" may be replaced with "insulating film" or "insulating layer." In addition, the term "conductor" can be replaced with "conductive film" or "conductive layer." In addition, the term "semiconductor" can be replaced with "semiconductor film" or "semiconductor layer." can.
[0054] In addition, the transistors shown in this specification and the like are not field-effect transistors unless otherwise specified. In addition, unless otherwise specified, the transistors shown in this specification and the like are n Therefore, the threshold voltage (also called "Vth") is Unless otherwise specified, shall be greater than 0V.
[0055] In addition, in this specification, "parallel" means that two straight lines are at an angle of -10 degrees or more and 10 degrees or less. Therefore, it includes the case where the angle is between -5 degrees and 5 degrees. "Almost parallel" means that the two straight lines are arranged at an angle of -30 degrees or more and 30 degrees or less. "Perpendicular" means that two straight lines are arranged at an angle of 80 degrees or more and 100 degrees or less. Therefore, it includes the case where the angle is between 85 degrees and 95 degrees. " refers to a state in which two straight lines are arranged at an angle of 60 degrees or more and 120 degrees or less.
[0056] In this specification, the term "barrier film" refers to a film that prevents impurities such as hydrogen and oxygen from passing through. If the barrier film has conductivity, it is called a conductive barrier film. It is sometimes called.
[0057] In this specification, the term "metal oxide" refers to metals in a broad sense. Metal oxides are oxide insulators and oxide conductors (including transparent oxide conductors). ), oxide semiconductor (also called oxide semiconductor or simply OS) For example, when a metal oxide is used for the semiconductor layer of a transistor, Such a metal oxide may be called an oxide semiconductor. In the case of a transistor, a transistor having an oxide or an oxide semiconductor is used. This can be rephrased as ta.
[0058] In this specification and the like, normally off means that no potential is applied to the gate, or The current per 1 μm of channel width that flows through a transistor when a ground potential is applied to the gate At room temperature, -20 A or less, 1×10 at 85℃ -18 A or below, or 1×10 at 125℃ -16 This means that it is A or lower.
[0059] (Embodiment 1) An example of a semiconductor device including a transistor 200 according to one embodiment of the present invention will be described below. He explains.
[0060] <Example of semiconductor device configuration> 1A, 1B, and 1C show a transistor 2 according to one embodiment of the present invention. 00, and a top view and a cross-sectional view of the area around transistor 200.
[0061] FIG. 1A is a top view of a semiconductor device including a transistor 200. FIG. 1B) and FIG. 1C are cross-sectional views of the semiconductor device. FIG. 1(A) is a cross-sectional view of a portion indicated by a dashed line A1-A2 in FIG. FIG. 1(C) is a cross-sectional view taken along the dashed line A3-A4 in FIG. 1(A). 1 is a cross-sectional view of the portion indicated by the arrow A in FIG. In the top view of FIG. 1(A), some elements are omitted for clarity.
[0062] The semiconductor device of one embodiment of the present invention includes a transistor 200 and an insulator serving as an interlayer film. 210, an insulator 212, and an insulator 281. The conductor 203 functions as a wiring and the conductor 24 functions as a plug. 0 (conductor 240a and conductor 240b).
[0063] The conductor 203 is formed such that the conductor 203a is in contact with the inner wall of the opening of the insulator 212. The conductor 203b is formed further inside. The height of the upper surface of the insulator 212 can be made to be approximately the same. The reference numeral 203 indicates a laminated structure of a conductor 203a and a conductor 203b. However, the present invention is not limited to this. For example, the conductor 203 may be a single layer, or three or more layers. In the case where the structure has a laminated structure, the order of formation is Ordinal numbers may be assigned to distinguish them.
[0064] The conductor 240 is also made up of an insulator 244, an insulator 280, an insulator 274, and an insulator 276. A first conductor of the conductor 240 is formed in contact with the inner wall of the opening of 81, and a conductor The second conductor 240 is formed. Here, the height of the upper surface of the conductor 240 and the insulator The height of the upper surface of the conductor 240 in the transistor 200 can be made approximately the same. Although a configuration in which a first conductor and a second conductor of conductor 240 are stacked is shown, The present invention is not limited to this. For example, the conductor 240 may be a single layer, or three or more layers. When the structure has a laminated structure, the order of formation is determined by ordinal numbers. In some cases, a distinction may be made between the following:
[0065] [Transistor 200] As shown in FIG. 1, transistor 200 includes an oxide semiconductor layer disposed on a substrate (not shown). The oxide 230a is a layer of a silicide, the oxide 230b is a layer of a silicide, and the oxide 230b is a layer of a silicide. Conductor 242a and conductor 242b are arranged apart from each other, and conductor 242a and is disposed on the conductor 242b and overlaps and opens between the conductor 242a and the conductor 242b. An insulator 280 having an aperture formed therein, a conductor 260 disposed within the aperture, and an oxide 230b. , the conductor 242a, the conductor 242b, and the insulator 280 are disposed between the conductor 260 and the The insulator 250 disposed therebetween, the oxide 230b, the conductor 242a, the conductor 242b, and the insulator 250 are The insulating layer 250 includes an oxide 230c disposed between the insulating layer 280 and the insulator 250. As shown in FIG. 1, oxide 230a, oxide 230b, conductor 242a, and conductor 242b are formed on the oxide 230a. It is preferable that an insulator 244 is disposed between the insulator 42b and the insulator 280. As shown, the conductor 260 includes a conductor 260a provided inside the insulator 250 and a conductor and a conductor 260b provided so as to be embedded inside the body 260a. As shown in FIG. 1, the insulator 280, the conductor 260, and the insulator 250 Preferably, an insulator 274 is disposed thereon.
[0066] In the following, oxide 230a, oxide 230b, and oxide 230c are collectively referred to as oxide 230a, oxide 230b, and oxide 230c. The conductor 242a and the conductor 242b are sometimes referred to as oxide 230. In some cases, the conductor 242 is referred to as the conductor 242.
[0067] In the transistor 200, a region in which a channel is formed (hereinafter, a channel forming region ) and in the vicinity thereof, oxide 230a, oxide 230b, and oxide 2 30c are laminated, the present invention is not limited to this. For example, a single layer of oxide 230b, a two-layer structure of oxide 230b and oxide 230a, The structure may be a two-layer structure of the substrate 230b and the oxide 230c, or a laminate structure of four or more layers. In addition, in the transistor 200, the conductor 260 is shown as having a two-layer structure. However, the present invention is not limited to this. For example, the conductor 260 may have a single-layer structure. Alternatively, it may have a laminated structure of three or more layers.
[0068] Here, the conductor 260 functions as a gate electrode of the transistor, and the conductors 242a and and the conductor 242b function as a source electrode and a drain electrode, respectively. Thus, the conductor 260 is inserted through the opening in the insulator 280 and through the conductors 242a and 242b. The conductive material 260 and the conductive material 242 are formed so as to be embedded in the region between them. The arrangement of the conductors 242a and 242b is selected to be self-aligned with respect to the openings in the insulator 280. That is, in the transistor 200, the gate electrode is connected to the source electrode and the drain electrode. Therefore, the conductor 260 can be arranged between the conductors 260 and 260 in a self-aligning manner. Since the transistor 200 can be formed without providing a gate, the area occupied by the transistor 200 can be reduced. This allows miniaturization and high integration of semiconductor devices.
[0069] Furthermore, the conductor 260 is self-aligned in the region between the conductor 242a and the conductor 242b. Since the conductor 260 is formed, the area where the conductor 260 overlaps the conductor 242a or the conductor 242b is As a result, the conductor 260 does not have a gap between the conductor 242a and the conductor 242b. The parasitic capacitance formed can be reduced. This improves the switching speed and allows the transistor 200 to have high frequency characteristics.
[0070] The transistor 200 also includes an insulator 214 disposed on the insulator 212 and an insulator An insulator 216 is disposed on the insulator 214, and a conductive material is embedded in the insulator 214 and the insulator 216. A conductor 205 is arranged so as to be insulated from the insulator 216 and the conductor 205. A body 220, an insulator 222 disposed on the insulator 220, and a The insulating layer 224 is preferably provided with an oxide 230a. It is preferable that the
[0071] The transistor 200 also includes an oxide 230 (oxide 230a) including a channel formation region. , oxide 230b, and oxide 230c) are metal oxides that function as oxide semiconductors. It is preferable to use an oxide semiconductor (hereinafter also referred to as an oxide semiconductor).
[0072] The transistor 200 having an oxide semiconductor in a channel formation region is in a non-conducting state. Since the leakage current is extremely small, a semiconductor device with low power consumption can be provided. Conductors can be formed into films using methods such as sputtering, making them ideal for constructing highly integrated semiconductor devices. The transistor 200 may be used.
[0073] For example, the oxide 230 may be an In-M-Zn oxide (wherein the element M is aluminum or gallium). Al, yttrium, copper, vanadium, beryllium, boron, titanium, iron, nickel, Rumanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, Tantalum, tungsten, magnesium, etc.) The oxide 230 may be an In-Ga oxide or an In-Z An n-oxide may also be used.
[0074] Here, the oxide 230 becomes catalytic when impurities such as hydrogen, nitrogen, or metal elements are present. The carrier density may increase, resulting in a lower resistance. If the resistance decreases, the carrier density increases, which may result in a lower resistance.
[0075] A conductive layer is provided on the oxide 230 so as to contact the oxide 230 and functions as a source electrode and a drain electrode. The conductor 242 (the conductor 242a and the conductor 242b) absorbs the oxygen of the oxide 230. or when the oxide 230 has impurities such as hydrogen, nitrogen, or metal elements. When the oxide 230 has a function of supplying the electric field, a low resistance region may be partially formed in the oxide 230. be.
[0076] The insulator 244 is provided to suppress oxidation of the conductor 242. The body 242 is made of an oxidation-resistant material or a material that does not lose electrical conductivity significantly when it absorbs oxygen. In this case, the insulator 244 does not necessarily have to be provided.
[0077] FIG. 2 shows an enlarged view of a region 239 surrounded by a dashed line in FIG. 1(B). As shown in FIG. 1, the insulator 250 has a thickness T1 between the oxide 230b and the conductor 260. Between the conductor 242a or the conductor 242b and the conductor 260, a thickness T2 is In the insulator 250, the thickness T1 is preferably smaller than the thickness T2.
[0078] In order to make the thickness T1 of the insulator 250 thinner than the thickness T2, for example, the oxide 230b and The insulator 250 between the conductors 260 is a single layer, and the conductors 242 and 260 are It is preferable that the insulator 250 located between the oxide 230b and the conductor 230b has a laminated structure. When the insulator 250 between the conductor 242 and the conductor 260 is formed as a laminated structure, The number of layers of the insulator 250 located between 0 and the oxide 230b and the conductor 260 is It is only necessary to make the number of layers larger than the number of layers of the insulator 250 to be laminated.
[0079] In this way, by making the thickness T2 of the insulator 250 thicker than the thickness T1, the conductor 26 200 having high frequency characteristics by reducing the parasitic capacitance between the conductor 242 and the Furthermore, since the thickness T1 is small, the electric field from the gate electrode is weakened. Therefore, the transistor 200 can have favorable electrical characteristics.
[0080] As shown in FIG. 2, a conductor 242 is provided on the oxide 230 so as to be in contact with the oxide. The interface between the conductor 242 and the oxide 230 and the vicinity thereof are provided with a region 243 ( The oxide 230 is a transistor. The region 234 functions as a channel forming region of the semiconductor substrate 200, and a part of the region 243. A region 231 (region 231a and region 231b) that functions as a source region or a drain region b) and a region 232 (regions 232a, and region 232b).
[0081] In the region 231 that functions as a source region or a drain region, the region 243 in particular The carrier gas has a low oxygen concentration or contains impurities such as hydrogen, nitrogen, and metal elements. In other words, the region 231 is a region where the arsenic concentration has increased and the resistance has decreased compared to the region 234. This region has a high carrier density and low resistance. It also functions as a channel formation region. The region 234 has a higher or lower oxygen concentration than the region 231, particularly the region 243. Since the impurity concentration is low, the region 232 is a high resistance region with a low carrier density. The oxygen concentration in the region 231 is equal to or higher than the oxygen concentration in the region 234. The impurity concentration of the region 232 is preferably equal to or lower than that of the region 232. 31, and the impurity concentration of the region 234, or is preferably higher than that.
[0082] In addition, when the region 243, which is a low resistance region, contains a metal element, the region 243 is an oxide 23 In addition to the metal elements contained in 0, aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel Nickel, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese magnesium, zirconium, beryllium, indium, ruthenium, iridium, One or more of the metal elements selected from the group consisting of strontium, lanthanum, etc. It is preferred that the element has a group element.
[0083] In addition, in FIG. 2, the region 243 is a thickness direction of the oxide 230b. However, the present invention is not limited to this. For example, the region 24 3 may have a thickness approximately equal to that of oxide 230b, or may be the same thickness as oxide 230a. 2, the region 243 may be formed between the region 231 and the region 232. However, the present invention is not limited to this. For example, the insulating film 232 may be formed only in the region 231. However, it may be formed in the region 231 and a part of the region 232, or it may be formed in the region 231 and a part of the region 232. It may be formed in the region 232 and a part of the region 234 .
[0084] In addition, it may be difficult to clearly detect the boundaries between the regions of the oxide 230. The concentrations of metal elements, hydrogen, nitrogen, and other impurity elements detected in each region are The change is not limited to gradual changes in each area, but also continuous changes (also called gradation) within each area. In other words, the closer to the channel formation region, the more the metal elements, etc. It is sufficient that the concentrations of impurity elements such as hydrogen and nitrogen are reduced.
[0085] In order to selectively reduce the resistance of the oxide 230, for example, aluminum is used as the conductor 242. Aluminum, Chromium, Copper, Silver, Gold, Platinum, Tantalum, Nickel, Titanium, Molybdenum, Tungsten Tennium, hafnium, vanadium, niobium, manganese, magnesium, zirconium, Conductive ions such as lithium, indium, ruthenium, iridium, strontium, and lanthanum It is preferable to use a material containing at least one of a metal element and an impurity that enhances the resistance. Alternatively, in the formation of the conductive film 242A which becomes the conductor 242, oxygen deficiency is generated in the oxide 230. The material and deposition method in which impurities such as the elements to be formed or the elements to be captured by oxygen vacancies are implanted For example, the element may be hydrogen, boron, carbon, nitrogen, fluorine, Examples of rare gas elements include phosphorus, sulfur, chlorine, and rare gases. A typical example of a rare gas element is helium. Examples include fluorine, neon, argon, krypton, and xenon.
[0086] Here, in the transistor using an oxide semiconductor, a channel is formed in the oxide semiconductor. If impurities and oxygen vacancies exist in the region where the semiconductor device is to be mounted, the electrical characteristics are likely to fluctuate, resulting in poor reliability. In addition, oxygen vacancies may be present in a region in the oxide semiconductor where a channel is formed. Therefore, when the channel is formed, the transistor tends to have normally-on characteristics. It is preferable that oxygen vacancies in the region 234 be reduced as much as possible.
[0087] In order to suppress the normally-on state of the transistor, the oxide 230 and the adjacent insulator 25 0 contains more oxygen than is necessary for the stoichiometric composition (also called excess oxygen). It is preferable that the oxygen in the insulator 250 diffuses into the oxide 230 and the oxygen in the oxide 230 is removed. This reduces element deficiencies and suppresses the transistor from becoming normally on.
[0088] That is, the oxygen contained in the insulator 250 and the insulator 280 is converted into the oxide region 234 of the oxide 230. Diffusion into the oxide 230 can reduce oxygen vacancies in the region 234 of the oxide 230. do.
[0089] In addition, in order to provide an oxygen region in the insulator 250 and the insulator 280, The insulator 274 in contact with the upper surface of the insulator 280 is formed of oxide by a sputtering method. By using a sputtering method to form an oxide film, it is possible to obtain a film containing a large amount of oxygen. In addition, it is possible to form an insulating film containing less impurities such as water or hydrogen. Body 274 is preferably made of aluminum oxide.
[0090] When forming a film by sputtering, there are ions and sputtering gases between the target and the substrate. For example, the target is connected to a power source and has a potential E0. The substrate is also given a potential E1 such as a ground potential. In addition, there is a region between the target and the substrate that is at potential E2. The magnitude relationship between the potentials is E2>E1>E0.
[0091] Ions in the plasma are accelerated by the potential difference E2-E0 and collide with the target. This causes the sputtered particles to be ejected from the target. The ions adhere to the surface of the film and are deposited on it, forming a film. The ions bounce off the get, pass through the film formed as a recoil ion, and reach the insulating layer in contact with the surface to be coated. The ions in the plasma may be trapped in the insulator 250 and the insulator 280. The ions are accelerated by the potential difference E2-E1 and bombard the surface of the film. The ions reach the inside of the insulator 280. The ions are taken into the insulator 250 and the insulator 280. As a result, a region where ions are trapped is formed in the insulator 280. In the case of oxygen-containing ions, the insulators 250 and 280 have excess oxygen regions. A region is formed.
[0092] By introducing excess oxygen into the insulators 250 and 280, the insulators 250 and An excess oxygen region can be formed in the insulator 280. The excess oxygen of 0 is supplied to the oxide 230 by heat treatment or the like, and the region of the oxide 230 is It is possible to compensate for the oxygen deficiency in 234.
[0093] The insulator 280 may be silicon oxide, silicon oxynitride, silicon nitride oxide, or a void-containing It is preferable to use silicon oxide having an excess of oxygen. On the other hand, compared to materials such as silicon oxynitride mentioned above, The oxide 230 is formed by forming an oxide film on the oxide 230 using a sputtering method. Even if the oxygen concentration is increased, the excess oxygen region tends to be difficult to form. The insulator 280 having the insulating layer 280 is provided around the region 234 of the oxide 230. This effectively supplies excess oxygen from the insulator 280 to the region 234.
[0094] As described above, a semiconductor device including a transistor with large on-state current can be provided. Alternatively, a semiconductor device including a transistor with low off-state current can be provided. Alternatively, the fluctuation of the electrical characteristics is suppressed, the electrical characteristics are stable, and the reliability is improved. It is possible to provide a semiconductor device having such a structure.
[0095] The following describes in detail the configuration of a semiconductor device including a transistor 200 according to one embodiment of the present invention. This article explains:
[0096] As shown in FIG. 1(A) and FIG. 1(C), the conductor 203 extends in the channel width direction. The conductor 203 is connected to the conductor 204 and functions as a wiring for applying a potential to the conductor 205. It is preferable that the insulating material 212 is embedded therein.
[0097] The conductor 205 is disposed so as to overlap the oxide 230 and the conductor 260. The conductor 205 is preferably provided on and in contact with the conductor 203. It is preferable that the insulating material 216 is embedded in the edge material 214 .
[0098] Here, the conductor 260 functions as a first gate (also called a top gate) electrode. The conductor 205 may also serve as a second gate (also called a bottom gate) electrode. In this case, the potential applied to the conductor 205 may be the potential applied to the conductor 260. By changing the Vth of the transistor 200 independently of the potential applied to the transistor 200, In particular, by applying a negative potential to the conductor 205, the transistor By increasing the Vth of the transistor 200 above 0V, it is possible to reduce the off-current. Therefore, applying a negative potential to the conductor 205 increases the current flow rate of the conductor 260 compared to when no negative potential is applied. This can reduce the drain current when the potential applied to is 0V.
[0099] In addition, a conductor 205 is provided on the conductor 203, so that a first gate electrode and a wiring It is possible to appropriately design the distance between the conductor 260, which functions as a In other words, the insulator 214 and the insulator 216 are provided between the conductor 203 and the conductor 260. By providing the above, the parasitic capacitance between the conductor 203 and the conductor 260 is reduced, and the conductor 2 The dielectric strength between 03 and conductor 260 can be increased.
[0100] In addition, by reducing the parasitic capacitance between the conductor 203 and the conductor 260, the transistor 2 It is possible to improve the switching speed of the 00 and turn it into a transistor with high frequency characteristics. In addition, by increasing the dielectric strength between the conductor 203 and the conductor 260, Therefore, the reliability of the insulator 214 and the insulator 216 can be improved. It is preferable to make the film thickness of the conductor 203 thicker. Note that the direction in which the conductor 203 extends is not limited to this. For example, For example, it may be extended in the channel length direction of the transistor 200 .
[0101] As shown in FIG. 1A, the conductor 205 is made of an oxide 230 and a conductor 260. The conductor 205 is arranged so as to overlap the region 234 of the oxide 230. In particular, as shown in FIG. 1C, the conductor 205 is made of an oxide 23. The region 234 extends beyond the end portion intersecting with the channel width direction of the region 234. That is, on the outer side of the side surface of the oxide 230 in the channel width direction, It is preferable that the conductor 205 and the conductor 260 overlap with each other via an insulator.
[0102] With the above configuration, when a potential is applied to the conductor 260 and the conductor 205, The electric field generated from the conductor 260 and the electric field generated from the conductor 205 are connected, and the oxide 2 The channel forming region formed in 30 can be covered.
[0103] That is, the electric field of the conductor 260 functioning as the first gate electrode and the electric field of the conductor 260 functioning as the second gate electrode The electric field of the conductor 205, which functions as an electrode, causes the channel formation region 234 to In the present specification, the first gate electrode and the second gate electrode are The structure of a transistor in which the electric field of the gate electrode electrically surrounds the channel formation region This is called the surrounded channel (S-channel) structure.
[0104] The conductor 205 is in contact with the inner walls of the openings of the insulators 214 and 216. The conductive body 205a is formed on the inner side, and the conductive body 205b is formed on the inner side. The height of the upper surfaces of the conductors 205a and 205b and the height of the upper surface of the insulator 216 can be made approximately equal. Note that the transistor 200 has a structure in which the conductor 205a and the conductor 205b are stacked. However, the present invention is not limited to this structure. The structure may be a single layer or a laminated structure of three or more layers. In cases where the compounds have the above structure, they may be distinguished by assigning ordinal numbers in the order of their formation.
[0105] Here, the conductor 205a or the conductor 203a may be a hydrogen atom, a hydrogen molecule, a water molecule, a nitrogen atom, or the like. Diffusion of impurities such as atoms, nitrogen molecules, nitrogen oxide molecules (N2O, NO, NO2, etc.), and copper atoms It is preferable to use a conductive material that has a function of suppressing diffusion (i.e., the impurities are less likely to permeate). Alternatively, the diffusion of oxygen (for example, at least one of oxygen atoms, oxygen molecules, etc.) is suppressed. It is preferable to use a conductive material that has the function of preventing oxygen from permeating through the conductive material. In this specification, the function of suppressing the diffusion of impurities or oxygen refers to the above-mentioned impurities or or the function of suppressing the diffusion of any one or all of the above oxygen.
[0106] The conductor 205a or the conductor 203a has a function of suppressing the diffusion of oxygen, The electrical conductivity of the conductor 205b or the conductor 203b can be prevented from decreasing due to oxidation. Examples of conductive materials that have the function of suppressing oxygen diffusion include tantalum, nitride, and the like. It is preferable to use tantalum chloride, ruthenium, or ruthenium oxide. The conductor 205a or the conductor 203a may be a single layer or a multilayer of the above-mentioned conductive material. As a result, impurities such as hydrogen and water can penetrate the conductor 203 and the conductor 205. Through this, diffusion to the transistor 200 side can be suppressed.
[0107] The conductor 205b is a conductive material mainly composed of tungsten, copper, or aluminum. Although the conductor 205b is illustrated as a single layer, it may have a laminated structure. For example, a laminate of titanium, titanium nitride and the above conductive material may be used.
[0108] In addition, the conductor 203b functions as a wiring and therefore has higher conductivity than the conductor 205b. It is preferable to use a conductive material. For example, a conductive material mainly composed of copper or aluminum is used. The conductor 203b may have a laminated structure, for example, A laminate of titanium or titanium nitride and the above conductive material may also be used.
[0109] In particular, it is preferable to use copper for the conductor 203b. Copper has low resistance and is therefore suitable for wiring, etc. On the other hand, copper is easily diffused, so it diffuses into the oxide 230. In some cases, the electrical characteristics of the transistor 200 may be degraded. 4. Use materials such as aluminum oxide or hafnium oxide that have low copper permeability. This can suppress the diffusion of copper.
[0110] The conductor 205, the insulator 214, and the insulator 216 are not necessarily required. In that case, a part of the conductor 203 can function as the second gate electrode.
[0111] The insulators 210 and 214 are formed to prevent impurities such as water or hydrogen from traversing the insulators from the substrate side. It is preferable that the insulating film functions as a barrier insulating film to prevent the inclusion of the metal oxide in the transistor 200. Therefore, the insulator 210 and the insulator 214 are insulated from hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, and the like. Diffusion of impurities such as atoms, nitrogen molecules, nitrogen oxide molecules (N2O, NO, NO2, etc.), and copper atoms It is preferable to use an insulating material that has a function of suppressing the impurities from penetrating the insulating material. Alternatively, the diffusion of oxygen (for example, at least one of oxygen atoms, oxygen molecules, etc.) is suppressed. It is preferable to use an insulating material that has the function of preventing oxygen from permeating through the insulating material.
[0112] For example, aluminum oxide or the like is used as the insulator 210 and silicon nitride is used as the insulator 214. It is preferable to use silicon or the like. This allows impurities such as hydrogen and water to be absorbed into the insulator 210. and suppressing diffusion from the substrate side to the transistor 200 side beyond the insulator 214. Alternatively, oxygen contained in the insulator 224 etc. may be mixed with the insulators 210 and 21. 4, diffusion toward the substrate side can be suppressed.
[0113] In addition, by forming the conductor 205 on the conductor 203, the conductor An insulator 214 may be provided between the body 203 and the conductor 205. Even if a metal that easily diffuses, such as copper, is used for 3b, silicon nitride or the like is provided as the insulator 214. This can prevent the metal from diffusing into layers above the insulator 214. .
[0114] In addition, the insulators 212, 216, and 280, which function as interlayer films, and the insulators The dielectric 281 preferably has a lower dielectric constant than the insulator 210 or the insulator 214. By using a material with a low dielectric constant as the interlayer film, the parasitic capacitance between wiring lines can be reduced. .
[0115] For example, the insulators 212, 216, 280, and 281 may be made of an acid. silicon oxide, silicon oxynitride, silicon nitride oxide, aluminum oxide, hafnium oxide , Tantalum oxide, Zirconium oxide, Lead zirconate titanate (PZT), Strobo titanate A single layer of insulator such as Ba,SrTiO3 or Ba,Sr)TiO3 (BST) is Alternatively, these insulators may be made of, for example, aluminum oxide. , bismuth oxide, germanium oxide, niobium oxide, silicon oxide, titanium oxide, tungsten oxide Insulating materials such as tin oxide, yttrium oxide, and zirconium oxide may also be added. The insulator may be nitrided. The insulator may be silicon oxide, silicon oxynitride, or nitrided. Silicon may also be used in a laminated form.
[0116] The insulators 220, 222, 224, and 250 are gate insulators. It has the function of
[0117] Here, the insulator 224 in contact with the oxide 230 has more oxygen than the stoichiometric composition. It is preferable to use an insulator that contains a large amount of oxygen. It is preferable that the insulator containing such excess oxygen is formed in the oxide 230. By providing the oxide 230 in contact with the oxide 230, oxygen vacancies in the oxide 230 are reduced, and the signal quality of the transistor 200 is improved. The reliability can be improved.
[0118] As an insulator having an excess oxygen region, specifically, an oxide insulator in which a part of oxygen is released by heating is used. It is preferable to use oxide materials that release oxygen when heated. Thermal Desorption Spectroscopy (DSA) analysis revealed that oxygen atoms The converted amount of oxygen released is 1.0 x 10 18 atoms / cm 3 More than or equal to 1.0 ×10 19 atoms / cm 3 More preferably, 2.0×10 19 atoms / c m 3 or more than 3.0×10 20 atoms / cm 3 The oxide film is as described above. The surface temperature of the film during the TDS analysis is 100°C or higher and 700°C or lower, or The range of 00°C or more and 400°C or less is preferable.
[0119] Also, if the insulator 224 has an excess oxygen region, the insulator 222 may be oxygen-absorbed (e.g., It has a function of suppressing the diffusion of at least one of oxygen atoms, oxygen molecules, etc. (the oxygen is not permeable) It is preferable that the temperature is within the range of 100°C.
[0120] The insulator 222 has a function of suppressing the diffusion of oxygen and impurities, so that the oxide 230 The oxygen contained in the conductor 205 is preferably not diffused to the insulator 220 side. In this way, reaction with the oxygen contained in the insulator 224 and the oxide 230 can be suppressed.
[0121] The insulator 222 may be, for example, aluminum oxide, hafnium oxide, tantalum oxide, or zinc oxide. Lead zirconate titanate (PZT), strontium titanate (SrTiO3 ) or (Ba,Sr)TiO3 (BST), which are so-called high-k materials It is preferable to use the material in a single layer or a multilayer structure. As this progresses, problems such as leakage current may occur due to the thinning of the gate insulator. By using a high-k material as the insulator that functions as a thermal insulator, This makes it possible to reduce the gate potential during transistor operation.
[0122] In particular, it has the function of suppressing the diffusion of impurities and oxygen (the oxygen is less likely to permeate). ) Insulating materials containing oxides of one or both of aluminum and hafnium. It is advisable to use an insulator, which may contain oxides of either or both of aluminum and hafnium. The insulators include aluminum oxide, hafnium oxide, aluminum and hafnium. It is preferable to use oxides such as hafnium aluminate. When the insulator 222 is formed by using the above-mentioned method, the insulator 222 is resistant to oxygen release from the oxide 230 and A layer for suppressing the intrusion of impurities such as hydrogen from the periphery of the transistor 200 into the oxide 230. It functions as such.
[0123] Alternatively, for example, aluminum oxide, bismuth oxide, germanium oxide, etc. may be added to these insulators. tungsten oxide, yttrium oxide, Zirconium oxide may be added, or these insulators may be nitrided. Silicon oxide, silicon oxynitride or silicon nitride may be laminated on the insulator. .
[0124] In addition, the insulator 220 is preferably thermally stable. For example, silicon oxide and Silicon oxide nitride and silicon oxynitride are thermally stable and therefore suitable as high-k materials for insulator and insulator 2. By combining with 20, it is possible to obtain a laminated structure that is thermally stable and has a high relative dielectric constant. do.
[0125] The insulators 220, 222, and 224 each have a laminated structure of two or more layers. In this case, the laminated structure is not limited to the same material, and may be made of different materials. A laminated structure may also be used.
[0126] The oxide 230 is made up of an oxide 230a, an oxide 230b on the oxide 230a, and an oxide 230b on the oxide 230a. The oxide 230c is located on the oxide 230b. The oxide 230a is located under the oxide 230b. As a result, impurities from the structure formed below the oxide 230a are transferred to the oxide 230b. The diffusion can be suppressed. In addition, by having the oxide 230c on the oxide 230b, Diffusion of impurities from structures formed above oxide 230c into oxide 230b can be suppressed.
[0127] The oxide 230 has a layered structure made of oxides with different atomic ratios of metal atoms. Specifically, in the metal oxide used for the oxide 230a, the constituent elements The atomic ratio of element M in the oxide 230b is the atomic ratio of element M in the metal oxide in the constituent elements. It is preferable that the atomic ratio of the metal oxide 230a is larger than that of the element M. In the metal oxide used for the oxide 230b, the atomic ratio of element M to In is It is preferable that the atomic ratio of element M to In is larger than that of element In. In the metal oxide used, the atomic ratio of In to the element M is It is preferable that the atomic ratio of In is larger than that of the element M in the metal oxide. The oxide 230c is a metal oxide that can be used for the oxide 230a or the oxide 230b. The object can be used.
[0128] In addition, the energy of the conduction band minimum of the oxide 230a and the oxide 230c is It is preferable that the energy of the oxide is higher than the minimum energy of the conduction band of 0b. The electron affinity of the oxide 230a and the oxide 230c is smaller than the electron affinity of the oxide 230b. It is preferable that
[0129] Here, at the junctions of oxide 230a, oxide 230b, and oxide 230c, The energy level of the conduction band minimum changes gradually. The energy level of the conduction band minimum at the junction of the oxide 230c and the oxide 230b is In order to achieve this, the oxide At the interface between oxide 230a and oxide 230b, and at the interface between oxide 230b and oxide 230c In this case, the defect level density of the mixed layer formed in the step (b) is preferably reduced.
[0130] Specifically, oxide 230a and oxide 230b, and oxide 230b and oxide 230c, By having a common element other than oxygen (as the main component), a mixed layer with a low defect level density is formed. For example, when the oxide 230b is an In-Ga-Zn oxide, the oxide The material 230a and the oxide 230c are In-Ga-Zn oxide, Ga-Zn oxide, Gallium oxide or the like may be used.
[0131] At this time, the main path of the carriers may be the oxide 230b. By forming the oxide 230c in the above-described structure, the interface between the oxide 230a and the oxide 230b and reducing the defect state density at the interface between oxide 230b and oxide 230c. This reduces the effect of interface scattering on carrier conduction, and the transistor 200 provides a high on-current.
[0132] The oxide 230 has a region 231 and a region 234. At least a portion of the electrode 242 has an area in contact with the conductor 242 .
[0133] When the transistor 200 is turned on, the region 231a or the region 231b becomes a solenoid. On the other hand, at least a portion of the region 234 functions as a source region or a drain region. This region functions as a region in which a channel is formed. It may also have a region 232 that functions as a merging region.
[0134] In other words, by selecting the range of each area appropriately, you can create a circuit that meets your requirements. A transistor having the desired electrical characteristics can be easily provided.
[0135] The oxide 230 is a metal oxide that functions as an oxide semiconductor (hereinafter, also referred to as an oxide semiconductor). For example, the metal oxide that will become the region 234 is a band It is preferable to use a material with a gap of 2 eV or more, preferably 2.5 eV or more. By using metal oxides with a wide band gap, the off-state current of a transistor can be reduced. can be reduced.
[0136] A transistor including an oxide semiconductor has an extremely small leakage current in an off-state. Therefore, a semiconductor device with low power consumption can be provided. Since the film can be formed using the above, it can be used for transistors that constitute highly integrated semiconductor devices. This can be done.
[0137] On the oxide 230b, a conductor 242 is formed, which functions as a source electrode and a drain electrode. (Conductor 242a and conductor 242b) are provided. The conductor 242 is made of aluminum. Aluminum, Chromium, Copper, Silver, Gold, Platinum, Tantalum, Nickel, Titanium, Molybdenum, Tan Gusten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, Choose from beryllium, indium, ruthenium, iridium, strontium, and lanthanum. or an alloy containing the above-mentioned metal elements or a combination of the above-mentioned metal elements. For example, tantalum nitride, titanium nitride, tungsten nitride, etc. titanium and aluminum nitrides, tantalum and aluminum nitrides, ruthenium oxides Ruthenium, ruthenium nitride, oxides containing strontium and ruthenium, lanthanum and nickel It is preferable to use oxides containing titanium. Nitrides containing tantalum and aluminum, nitrides containing tantalum and aluminum, ruthenium oxide , ruthenium nitride, oxides containing strontium and ruthenium, oxides containing lanthanum and nickel Oxides are conductive materials that are resistant to oxidation or that maintain their conductivity even when they absorb oxygen. Therefore, it is preferable.
[0138] By providing the conductor 242 so as to be in contact with the oxide 230, the oxygen concentration in the region 243 In addition, the metal contained in the conductor 242 and the oxide 23 in the region 243 may be reduced. In such a case, a metal compound layer containing a component of 0 may be formed. The carrier density increases and region 243 becomes a low resistance region.
[0139] Here, the area between the conductor 242a and the conductor 242b overlaps the opening of the insulator 280. As a result, the conductor 260 is formed between the conductor 242a and the conductor 242b. It can be arranged in a consistent manner.
[0140] The insulator 244 is provided to cover the conductor 242 and suppresses oxidation of the conductor 242. At this time, the insulator 244 covers the side surface of the oxide 230 and is in contact with the insulator 224. It may be provided.
[0141] The insulator 244 may be selected from hafnium, aluminum, gallium, yttrium, zirconium, and the like. tungsten, titanium, tantalum, nickel, germanium, or magnesium For example, a metal oxide containing one or more metals selected from the group consisting of fluorine, fluorine, arsenic ...
[0142] In particular, the insulator contains oxides of either or both of aluminum and hafnium. , aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium oxide, ha ... It is preferable to use hafnium aluminate. In particular, hafnium aluminate is It has higher heat resistance than hafnium oxide film. Therefore, it is possible to prevent the formation of oxide film by heat in the subsequent process. It is preferable that the conductor 242 is made of a material having oxidation resistance or oxygen resistance. If the conductivity does not decrease significantly even if the insulator 244 absorbs the heat, the insulator 244 is not an essential component. The design may be appropriately adjusted depending on the transistor characteristics to be used.
[0143] The insulator 250 functions as a gate insulator. The insulator 250 is preferably disposed in contact with the upper and side surfaces of the substrate 210. It is preferable to form the insulating material from which oxygen is released. For example, thermal desorption spectroscopy Analysis (TDS analysis) showed that the amount of oxygen released was 1.0 x 10 18 ato ms / cm 3 More than 1.0×10 19 atoms / cm 3 More preferably 2.0×10 19 atoms / cm 3 or more than 3.0×10 20 atoms / c m 3 The oxide film is as above. The surface temperature of the film during the TDS analysis was The range of 100°C or higher and 700°C or lower is preferred.
[0144] Specifically, silicon oxide having excess oxygen, silicon oxynitride, silicon nitride oxide, Silicon nitride, silicon oxide doped with fluorine, silicon oxide doped with carbon, carbon and Silicon oxide doped with nitrogen and silicon oxide having vacancies can be used. Silicon oxide and silicon oxynitride are preferred because they are stable to heat.
[0145] The insulator 250 is an insulator that releases oxygen when heated, and is placed on the top surface of the oxide 230c. By providing the oxide 230b in contact with the insulator 250, the oxide 230b passes through the oxide 230c. In addition, oxygen can be effectively supplied to the region 234, similar to the insulator 224. It is preferable that the concentration of impurities such as water or hydrogen in the insulator 250 is reduced. The film thickness of 250 is preferably 1 nm or more and 20 nm or less.
[0146] In addition, the insulator 250 is provided not only between the oxide 230b and the conductor 260 but also between the conductor 242 and the The insulating layer 250 is also provided between the conductor 260 and the insulating layer 260. A parasitic capacitance is formed between 242 and the conductor 260, and the transistor 200 or the semiconductor If the characteristics of the device are adversely affected, the conductor 242 and the conductor 260 may be The thickness of the insulator 250 located between the oxide 230b and the conductor 260 is It is preferable to make it thicker than the film thickness. The insulator 250 between the oxide 230b and the conductor 260 has a two-layer structure. The insulator 250 may have a single-layer structure. An insulating film that will be the first insulator is formed on the inside of the insulating film 230C, and an anisotropic etchant is applied to the insulating film. Then, etching is performed to form a first insulator only on the inner wall of the oxide film 230C. By forming an insulating film that serves as an insulator, the insulating film located between the oxide 230b and the conductor 260 The insulator 250 has a single-layer structure, and the insulator 250 is disposed between the conductor 242 and the conductor 260. Therefore, the insulator 250 between the conductor 242 and the conductor 260 has a two-layer structure. The thickness of the film is made thicker than the thickness of the insulator 250 located between the oxide 230b and the conductor 260. It is possible.
[0147] In addition, in order to efficiently supply the excess oxygen contained in the insulator 250 to the oxide 230, A metal oxide may be provided between the insulator 250 and the conductor 260. The metal oxide serves as an insulating material. It is preferable to suppress the diffusion of oxygen from the body 250 to the conductor 260. By providing a metal oxide, the diffusion of excess oxygen from the insulator 250 to the conductor 260 is suppressed. In other words, the reduction in the amount of excess oxygen supplied to the oxide 230 can be suppressed. In addition, oxidation of the conductor 260 due to excess oxygen can be suppressed.
[0148] The metal oxide may also function as a part of the gate insulator. Therefore, when silicon oxide or silicon oxynitride is used for the insulator 250, the metal oxide It is preferable to use a metal oxide, which is a high-k material with a high relative dielectric constant, as the oxide. By making the base insulator have a laminated structure of the insulator 250 and the metal oxide, the base insulator is stable against heat. Therefore, the physical properties of the gate insulator can be improved. It is possible to reduce the gate potential applied during transistor operation while maintaining the film thickness. In addition, it is possible to reduce the equivalent oxide thickness (EOT) of the insulator that functions as the gate insulator. do.
[0149] Specifically, hafnium, aluminum, gallium, yttrium, zirconium, tantalum, tin, titanium, tantalum, nickel, germanium, magnesium, etc. A metal oxide containing one or more selected from the above can be used.
[0150] In particular, the insulator contains oxides of either or both of aluminum and hafnium. , aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium oxide, ha ... It is preferable to use hafnium aluminate. In particular, hafnium aluminate is It has higher heat resistance than hafnium oxide film. Therefore, it is possible to prevent the formation of oxide film by heat in the subsequent process. This is preferable because it is difficult to crystallize. However, the metal oxide is not an essential component. It is sufficient to design appropriately according to the transistor characteristics.
[0151] The conductor 260 that functions as the first gate electrode is shown in FIG. 1 as a two-layer structure. However, it may be a single-layer structure or a laminated structure of three or more layers.
[0152] The conductor 260a, like the conductor 205a, is a hydrogen atom, a hydrogen molecule, a water molecule, a nitrogen atom, Diffusion of impurities such as nitrogen molecules, nitrogen oxide molecules (N2O, NO, NO2, etc.), and copper atoms It is preferable to use a conductive material that has a function of suppressing oxygen (e.g., oxygen Use a conductive material that has the function of suppressing the diffusion of at least one of atoms, oxygen molecules, etc. It is preferable.
[0153] In addition, the conductor 260a has a function of suppressing the diffusion of oxygen, so that the insulator 250 The oxygen contained therein can suppress the conductor 260b from being oxidized and the conductivity from decreasing. Examples of conductive materials that have the function of suppressing oxygen diffusion include tantalum, nitride, and the like. It is preferable to use tantalum chloride, ruthenium, ruthenium oxide, or the like.
[0154] The conductor 260b is a conductive material mainly composed of tungsten, copper, or aluminum. In addition, since the conductor 260b also functions as wiring, It is preferable to use a conductor with high electrical conductivity, such as tungsten, copper, or aluminum. The conductive material 260b may be a laminated material. For example, it may be a laminated structure of titanium, titanium nitride and the above conductive material. stomach.
[0155] As shown in FIG. 1C, the conductor 205 intersects with the channel width direction of the oxide 230. When the conductor 260 extends in a region outside the end portion, the conductor 260 In this case, it is preferable that the conductor 205 overlaps with the insulator 250 interposed therebetween. On the outside of the side of the insulating material 230, the conductor 205, the insulator 250, and the conductor 260 are It is preferable to form a laminated structure.
[0156] With the above configuration, when a potential is applied to the conductor 260 and the conductor 205, The electric field generated from the conductor 260 and the electric field generated from the conductor 205 are connected, and the oxide 2 The channel forming region formed in 30 can be covered.
[0157] That is, the electric field of the conductor 260 functioning as the first gate electrode and the electric field of the conductor 260 functioning as the second gate electrode The electric field of the conductor 205, which functions as an electrode, causes the channel formation region 234 to can be electrically surrounded.
[0158] The insulator 280 is provided on the conductor 242 via the insulator 244. Preferably, the insulator 280 has an excess oxygen region. For example, silicon oxide is used as the insulator 280. , silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide doped with fluorine , silicon oxide doped with carbon, silicon oxide doped with carbon and nitrogen, silicon oxide with vacancies It is preferable that the insulating layer 100 has silicon oxide or resin. In particular, silicon oxide and oxide Silicon nitride is preferred because it is thermally stable. In particular, silicon oxide and oxide having vacancies are preferred. Silicon oxide is preferred because it allows for easy formation of excess oxygen regions in a later step.
[0159] As mentioned above, the insulator 280 preferably has an excess oxygen region. The insulator 280 from which the electrons are released is provided in contact with the oxide 230c. The oxygen is efficiently supplied to the region 234 of the oxide 230 through the oxide 230c. In addition, the concentration of impurities such as water or hydrogen in the insulator 280 is reduced. is preferred.
[0160] The upper surface of the insulator 280 is approximately the same as the upper surface of the conductor 260 and the upper surface of the insulator 250. A match is preferred.
[0161] The insulator 274 is disposed on the top surface of the insulator 280, the top surface of the conductor 260, and the top surface of the insulator 250. It is preferable that the insulator 274 is provided in contact with the surface. Thus, an excess oxygen region can be provided in the insulator 250 and the insulator 280. From this excess oxygen region, oxygen can be supplied into the oxide 230.
[0162] For example, the insulator 274 may be hafnium, aluminum, gallium, yttrium, Zirconium, tungsten, titanium, tantalum, nickel, germanium, or magnesium It is possible to use a metal oxide containing one or more metals selected from the group consisting of ruthenium, cadmium, and ruthenium. Cut.
[0163] In particular, aluminum oxide has high barrier properties and is a thin film with a thickness of 0.5 nm to 3.0 nm. Therefore, the diffusion of hydrogen and nitrogen can be suppressed even if the sputtering The aluminum oxide film formed by this method is a source of oxygen and also a barrier against impurities such as hydrogen. For example, an aluminum oxide film formed by sputtering can be used. By using minium for the insulator 274, the insulator 274 supplies oxygen to the insulator 280. At the same time, impurities such as hydrogen from above the insulator 274 are mixed into the insulator 280. It is possible to suppress the above.
[0164] In addition, it is preferable to provide an insulator 281 that functions as an interlayer film on the insulator 274. The insulator 281, like the insulator 224, has a low impurity concentration such as water or hydrogen in the film. is preferably reduced.
[0165] Also, the insulating material 281, the insulating material 274, the insulating material 280, and the insulating material 244 are formed The conductor 240a and the conductor 240b are disposed in the opening. The conductor 240a and the conductor 240b are disposed opposite each other with the conductor 260 in between. The height of the upper surface of 240b may be flush with the upper surface of the insulator 281.
[0166] In addition, the inner walls of the openings of the insulators 281, 274, 280, and 244 A first conductor of the conductor 240a is formed in contact with at least the bottom of the opening. A conductor 242a is located in the other portion, and the conductor 240a contacts the conductor 242a. Similarly, the inner walls of the openings of the insulators 281, 274, 280, and 244 A first conductor of the conductor 240b is formed in contact with at least the bottom of the opening. A conductor 242b is located in the other portion, and the conductor 240b contacts the conductor 242b.
[0167] Here, in FIG. 3(A), the area indicated by the dashed line A5-A6 in FIG. 1(A), i.e., the trajectory 3 shows a cross-sectional view of the source or drain region of a transistor 200. The conductive body 240a (the conductive body 240b) is at least on the conductive body 242a (the conductive body 242b). The oxide 230a is in contact with the side surface of the oxide 230b and the side surface of the oxide 230a. In particular, the conductor 240a (conductor 240b) is preferably a conductor of the oxide 230. On the sides that intersect with the width direction of the panel, the A5 side and / or the A6 side It is preferable that the conductor 240a (conductor 240b) is in contact with the oxide 230. The side surface intersecting the channel length direction may be configured to contact the side surface on the A1 side (A2 side). In this manner, the conductor 240a and the conductor 240b are connected to the conductor 242a (the conductor 242b). In addition to the top and side surfaces of oxide 230b and oxide 230a, the side surfaces of oxide 230b and oxide 230a are By making the conductor 240a (conductor 240b) and the conductor 242 contact the side surface, Without increasing the upper area of the contact part of a (conductor 242b), the contact surface of the contact part The product is increased, and the conductor 240a (conductor 240b) and the conductor 242a (conductor 242b) This reduces the contact resistance between the source electrode and the drain electrode of the transistor. It is possible to increase the on-current while miniaturizing the in-electrode.
[0168] FIG. 3B shows an example in which an opening is formed to expose a part of the conductor 242a (conductor 242b). When doing this, the mask alignment in the lithography method shifted in the A5 direction. In the channel width direction, the conductor 242a (the conductor 242b), By making the width of the opening larger than the width of the oxide 230b and the oxide 230a, Even if misalignment occurs, the conductor 240a (conductor 240b) can be connected to the conductor 242a ( The top and side surfaces of the conductor 242b, the side surfaces of the oxide 230b, and the top and side surfaces of the oxide 230a It can come into contact with the side, providing good contact.
[0169] The conductors 240a and 240b are mainly made of tungsten, copper, or aluminum. It is preferable to use a conductive material having the following components: 0b may have a laminated structure.
[0170] In addition, when the conductor 240 has a laminated structure, the oxide 230a, the oxide 230b, the conductor The conductors in contact with 242, insulator 244, insulator 280, insulator 274, and insulator 281 are Like the conductor 205a, the conductive material 205 has a function of suppressing the permeation of impurities such as water or hydrogen. It is preferable to use a conductive material having a high conductivity, such as tantalum, tantalum nitride, titanium, or nitride. It is preferable to use titanium, ruthenium, or ruthenium oxide. Conductive materials that have the function of suppressing the permeation of impurities such as hydrogen are used in single or multilayer configurations. By using the conductive material, impurities such as hydrogen and water can be removed from the upper layer of the insulator 281. Suppresses impurities from being mixed into the oxide 230 through the conductors 240a and 240b. It is possible.
[0171] Although not shown, a conductive material 240a and a conductive material 240b are disposed in contact with each other on the upper surface thereof. A conductor functioning as a line may be disposed. The conductor functioning as a wiring may be tungsten. It is preferable to use a conductive material containing copper or aluminum as a main component. The conductor may be a laminated structure, for example, a layer of titanium, titanium nitride, and the above-mentioned conductive material. The conductor may be a laminated conductor. The insulating film 14 may be formed so as to be embedded in the opening.
[0172] <Materials for semiconductor devices> The following describes constituent materials that can be used in the semiconductor device.
[0173] <<Substrate>> The substrate on which the transistor 200 is formed may be, for example, an insulating substrate, a semiconductor substrate, or A conductive substrate may be used. Examples of insulating substrates include glass substrates, quartz substrates, and silicon substrates. Fire substrate, stabilized zirconia substrate (yttria stabilized zirconia substrate, etc.), resin substrate The semiconductor substrate may be, for example, a semiconductor such as silicon or germanium. Solid substrate, or silicon carbide, silicon germanium, gallium arsenide, indium phosphide Compound semiconductor substrates made of zinc oxide, gallium oxide, etc. A semiconductor substrate having an insulating region inside the substrate, such as SOI (Silicon On Insulator) Conductive substrates include graphite substrates, metal substrates, and alloy substrates. Substrates with metal nitrides, conductive resin substrates, etc. Further, there are substrates in which a conductor or a semiconductor is provided on an insulating substrate, A substrate in which a conductor or an insulator is provided on a semiconductor substrate, a substrate in which a semiconductor or an insulator is provided on a conductor substrate Alternatively, a substrate having an element provided thereon may be used. The elements provided on the substrate include a capacitance element, a resistance element, a switch element, a light emitting element, a recording element, Memory elements, etc.
[0174] In addition, a flexible substrate may be used as the substrate. As a method of providing the insulating film, a transistor is formed on a non-flexible substrate, and then the transistor is peeled off. Another method is to separate the substrate from the non-flexible substrate and transfer it to a flexible substrate. A release layer may be provided between the substrate and the transistor. The substrate may be stretchable. The plate may have the property of returning to its original shape when bending or straining is stopped, or The substrate may have a property of not returning to its original shape. Preferably, the thickness is 10 μm or more and 500 μm or less, and more preferably, the thickness is 15 μm or more and 300 μm or less. By making the substrate thinner, it is possible to manufacture a semiconductor device having transistors more lightly. In addition, by making the substrate thin, it is possible to achieve stretchability even when glass or other materials are used. or have the property of returning to their original shape when bending or pulling is stopped. Therefore, it is necessary to reduce the shock applied to the semiconductor device on the board when it is dropped. That is, a robust semiconductor device can be provided.
[0175] The flexible substrate may be, for example, a metal, an alloy, a resin, or a glass, or the like. These fibers can be used as the substrate. A flexible substrate having a lower linear expansion coefficient is more environmentally friendly. The substrate that is flexible has a linear expansion coefficient of, for example, 1×10 -3 / K or less, 5×10 -5 / K or less, or 1×10 -5 / K or less Examples of resins that can be used include polyester, polyolefin, and polyamide ( Nylon, aramid, etc.), polyimide, polycarbonate, acrylic, etc. Aramid has a low linear expansion coefficient and is therefore suitable for use as a flexible substrate.
[0176] <<Insulators>> Insulators include oxides, nitrides, oxynitrides, nitride oxides, and metal oxides that have insulating properties. These include metal oxide nitrides, metal oxynitrides, and metal oxynitrides.
[0177] For example, as transistors become smaller and more highly integrated, the gate insulator becomes thinner. This can cause problems such as leakage current. By using high-k materials, the voltage required for transistor operation can be reduced while maintaining the physical thickness. On the other hand, it is possible to use a material with a low relative dielectric constant for the insulator that functions as the interlayer film. This reduces the parasitic capacitance between the wirings. The material should be selected accordingly.
[0178] Insulators with high relative dielectric constants include gallium oxide, hafnium oxide, and zirconium oxide. Oxides containing aluminum, aluminum and hafnium, and oxides containing aluminum and hafnium oxide nitride having silicon and hafnium, oxide having silicon and hafnium Examples of suitable materials include oxynitrides with hafnium, or nitrides with silicon and hafnium.
[0179] Insulators with low dielectric constants include silicon oxide, silicon oxynitride, and silicon nitride oxide. Silicon, silicon nitride, silicon oxide with fluorine, silicon oxide with carbon, Silicon oxide doped with carbon and nitrogen, silicon oxide with voids, or resin, etc. be.
[0180] In particular, silicon oxide and silicon oxynitride are thermally stable. For example, by combining it with resin, it is possible to create a laminated structure that is thermally stable and has a low dielectric constant. Examples of resins include polyester, polyolefin, polyamide (nylon), etc. Materials include acrylic, polyimide, polycarbonate, etc. For example, silicon oxide and silicon oxynitride can be combined with insulators with high dielectric constants. This makes it possible to obtain a laminated structure that is thermally stable and has a high relative dielectric constant.
[0181] In addition, a transistor using an oxide semiconductor can suppress the permeation of impurities such as hydrogen and oxygen. By surrounding the transistor with an insulator that has the function of suppressing the This can be done.
[0182] Examples of insulators that have a function of suppressing the permeation of impurities such as hydrogen and oxygen include: Boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, salt Argon, Gallium, Germanium, Yttrium, Zirconium, Lanthanum, Neo Insulators containing zinc, hafnium, or tantalum may be used in single or multilayer configurations. Specifically, it is used as an insulator that has the function of suppressing the permeation of impurities such as hydrogen and oxygen. , Aluminum oxide, Magnesium oxide, Gallium oxide, Germanium oxide, Yttrium oxide lithium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, or Metal oxides such as tantalum, silicon oxide nitride, silicon nitride, etc. can be used. Cut.
[0183] For example, the insulator 274 may be hafnium, aluminum, gallium, yttrium, Zirconium, tungsten, titanium, tantalum, nickel, germanium, or ma It is possible to use a metal oxide containing one or more metals selected from magnesium, etc. Silicon nitride and silicon nitride containing oxygen, i.e., silicon nitride, can also be used. For example, silicon oxide or silicon oxynitride can be used.
[0184] In particular, aluminum oxide has high barrier properties and is a thin film with a thickness of 0.5 nm to 3.0 nm. Even if the hafnium oxide is used, it is possible to suppress the diffusion of hydrogen and nitrogen. Although its barrier properties are lower than those of aluminum oxide, the barrier properties can be improved by increasing the film thickness. Therefore, by adjusting the thickness of the hafnium oxide, it is possible to control the amount of hydrogen and nitrogen The amount of addition can be adjusted appropriately.
[0185] For example, the insulator 250, which functions as a gate insulator, and the insulator 224 are For example, silicon oxide with excess oxygen regions or By forming a structure in which the silicon oxynitride is in contact with the oxide 230, the The oxygen deficiency can be compensated for.
[0186] Also, for example, in the insulator 222 which functions as part of the gate insulator, aluminum The insulator includes one or more oxides of tungsten, hafnium, and gallium. In particular, insulators containing oxides of aluminum and / or hafnium are As examples, aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium It is preferable to use hafnium aluminate or the like.
[0187] For example, the insulator 220 may be made of silicon oxide or silicon oxynitride, which is thermally stable. It is preferable to use a film having thermal stability and a high relative dielectric constant as the gate insulator. By forming a laminated structure with a thin film, the equivalent oxide thickness of the gate insulator can be increased while maintaining the physical thickness. It is possible to reduce the EOT.
[0188] By using the above-mentioned laminated structure, the on-current can be increased without weakening the effect of the electric field from the gate electrode. In addition, the physical thickness of the gate insulator can improve the gate insulating film. By keeping the distance between the gate electrode and the region where the channel is formed, It is possible to suppress the leakage current between the
[0189] The insulators 212, 216, 280, and 281 have a low dielectric constant. It is preferable to have an insulator. For example, the insulator 212, the insulator 216, the insulator 280, The insulator 281 may be silicon oxide, silicon oxynitride, silicon nitride oxide, or silicon nitride. Silicon oxide doped with fluorine, silicon oxide doped with carbon, and carbon and nitrogen It is preferred to have silicon oxide, silicon oxide having voids, or resin. Alternatively, the insulators 212, 216, 280, and 281 may be made of an acid. Silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, fluorine-added oxide silicon oxide doped with carbon, silicon oxide doped with carbon and nitrogen, It is preferable that the insulating layer has a laminated structure of silicon oxide having holes and a resin. Silicon and silicon oxynitride are thermally stable, so by combining them with resin, It is possible to obtain a laminated structure that is thermally stable and has a low relative dielectric constant. polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, Recarbonate or acrylic.
[0190] The insulators 210, 214, 244, and 274 may be hydrogen or the like. An insulator having a function of suppressing the permeation of impurities and oxygen may be used. The insulators 214, 244, and 274 may be, for example, aluminum oxide. , hafnium oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide oxide, zirconium oxide, lanthanum oxide, neodymium oxide, or tantalum oxide Metal oxide, silicon nitride oxide, silicon nitride, or the like may be used.
[0191] <<Conductors>> Conductive materials include aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, and titanium. Tantalum, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium Sium, zirconium, beryllium, indium, ruthenium, iridium, strontium Materials containing one or more metal elements selected from the group consisting of uranium, lanthanum, etc. can be used. In addition, semiconductors with high electrical conductivity, such as polycrystalline silicon containing impurity elements such as phosphorus, Conductors and silicides such as nickel silicide may also be used.
[0192] In addition, a plurality of conductive layers made of the above materials may be laminated. A laminated structure in which a material containing a metal element and a conductive material containing oxygen are combined may be used. In addition, a laminated material that combines the above-mentioned material containing a metal element and a conductive material containing nitrogen is In addition, the above-mentioned metal element-containing material, the conductive material containing oxygen, and the nitrogen A laminated structure in which the conductive material containing the element is combined with the conductive material containing the element may be used.
[0193] In the case where an oxide is used for the channel formation region of a transistor, The conductor that functions as a conductive material is a material containing the above-mentioned metal element and a conductive material containing oxygen. In this case, it is preferable to use a laminate structure in which an oxygen-containing conductive material is used as the It is preferable to provide the conductive material containing oxygen on the channel forming region side. This makes it easier for oxygen released from the conductive material to be supplied to the channel formation region.
[0194] In particular, the metal oxide in which the channel is formed is a conductor that functions as a gate electrode. It is preferable to use a conductive material containing oxygen and a metal element contained in the metal. Conductive materials containing metal elements and nitrogen may also be used, such as titanium nitride and tantalum nitride. In addition, a conductive material containing nitrogen such as indium tin oxide or tungsten oxide may be used. Indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, titanium oxide Indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide Indium tin oxide containing nitrogen may also be used. Mugallium zinc oxide may be used. By using such a material, the channel is formed In some cases, hydrogen can be captured from the metal oxide that is insulated from the outer In some cases, it may be possible to capture hydrogen that is mixed in from the surroundings, etc.
[0195] Conductor 260, conductor 203, conductor 205, conductor 242, and conductor 240 are The following metals are used: aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, titanium, molybdenum, etc. Density, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zinc Ruthenium, beryllium, indium, ruthenium, iridium, strontium, lanthanum or an alloy containing the above-mentioned metal elements or the above-mentioned metal elements. It is preferable to use an alloy of elements such as tantalum nitride, titanium nitride, Nitrides containing tungsten, titanium and aluminum, and nitrides containing tantalum and aluminum Ruthenium oxide, ruthenium nitride, oxides containing strontium and ruthenium, lanthanum It is preferable to use oxides containing tantalum and nickel. Tantalum, titanium and aluminum nitride, tantalum and aluminum nitride, oxide Ruthenium, ruthenium nitride, oxides containing strontium and ruthenium, lanthanum and niobium Nickel-containing oxides are conductive materials that are resistant to oxidation, or that retain their conductivity even after absorbing oxygen. In addition, polycrystalline silicon containing impurity elements such as phosphorus is preferred. The material uses semiconductors with high electrical conductivity, such as nickel silicide, This is also fine.
[0196] <<Metal oxides>> As the oxide 230, a metal oxide functioning as an oxide semiconductor (hereinafter, referred to as an oxide semiconductor) is used. (also referred to as "oxide 230") is preferably used. The metal oxide will now be described.
[0197] The metal oxide preferably contains at least indium or zinc. In addition to these, aluminum, gallium, and zinc are preferably included. , yttrium or tin. Also, boron, titanium, Iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium One selected from the group consisting of tungsten, hafnium, tantalum, and magnesium, Or, multiple types may be included.
[0198] Here, the metal oxide is an In-M-Zn oxide having indium, element M and zinc. The element M can be aluminum, gallium, yttrium, or Other elements that can be used for element M include boron, titanium, iron, Nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, Hafnium, tantalum, tungsten, magnesium, etc. However, as the element M, In some cases, a combination of two or more of the aforementioned elements may be used.
[0199] In this specification, metal oxides containing nitrogen are also referred to as metal oxides. Metal oxides containing nitrogen are also called metal oxynitrides (MEs). It may also be called tal oxynitride.
[0200] [Metal oxide composition] The following describes a CAC (C This paper explains the configuration of the Multicloud Aligned Composite Operating System (MSO).
[0201] In this specification, CAAC (c-axis aligned crystal l), and CAC (Cloud-Aligned Composite) CAAC represents an example of a crystal structure, and CAC represents a function or a material configuration. An example is shown below.
[0202] CAC-OS or CAC-metal oxide is a material that has a conductive function in some parts. The material has a function of insulating in part and a function of semiconductor in the whole material. Note that CAC-OS or CAC-metal oxide is used as the semiconductor of a transistor. When used in a dielectric layer, the conductive function is to allow the flow of electrons (or holes) that serve as carriers. The insulating function is to prevent the flow of electrons, which act as carriers. By making the function of the material and the function of the material complement each other, the material can be switched (On / Off). ff function) to CAC-OS or CAC-metal oxide. In CAC-OS or CAC-metal oxide, By separating the functions, the functionality of both can be maximized.
[0203] In addition, CAC-OS or CAC-metal oxide is a conductive area and an insulating area. The conductive region has the above-mentioned conductive function, and the insulating region has the above-mentioned insulating function. In addition, the conductive and insulating regions in the material are formed by nanoparticles. The conductive and insulating regions may be separated by different materials. In addition, the conductive area may be observed as a cloud-like connected area with a blurred periphery. This may be the case.
[0204] In addition, in the CAC-OS or CAC-metal oxide, a conductive region and The insulating regions are each 0.5 nm to 10 nm, preferably 0.5 nm to 3 nm. They may be dispersed in the material at sizes of less than one millimeter.
[0205] In addition, CAC-OS or CAC-metal oxide has different band gaps For example, CAC-OS or CAC-metal ox The ide consists of a wide gap component due to the insulating region and a conductive region. In this configuration, when the carrier flows, In addition, carriers mainly flow in the narrow gap component. The component with a gap acts complementary to the component with a wide gap to produce a narrow gap. Carriers also flow to the wide gap component in conjunction with the component with a large gap. CAC-OS or CAC-metal oxide is used as the channel formation region of the transistor. When used in a transistor, it has a high current driving force in the on-state, i.e., a large on-current. , and high field effect mobility can be obtained.
[0206] That is, CAC-OS or CAC-metal oxide is a matrix composite. matrix composite, or metal matrix composite It can also be called a composite matrix.
[0207] [Metal oxide structures] Oxide semiconductors (metal oxides) are classified into single-crystal oxide semiconductors and other non-single-crystal oxide semiconductors. As a non-single crystal oxide semiconductor, for example, CAAC-OS (c- axis aligned crystalline oxide semiconductor ctor), polycrystalline oxide semiconductor, nc-OS (nanocrystalline ox ide semiconductor), pseudo amorphous oxide semiconductor (a-like OS : amorphous-like oxide semiconductor), and Examples include amorphous oxide semiconductors.
[0208] CAAC-OS has a c-axis orientation and multiple nanocrystals are connected in the ab-plane direction. The nanocrystals are connected together to form a distorted crystal structure. In a region, a lattice arrangement is formed between a region having a uniform lattice arrangement and another region having a uniform lattice arrangement. This refers to the point where the direction of the
[0209] Nanocrystals are basically hexagonal, but are not limited to regular hexagons and may have non-regular hexagonal shapes. In addition, the distortion may have lattice arrangements such as pentagons and heptagons. In addition, in the CAAC-OS, clear grain boundaries (grain bows) were observed even in the vicinity of the strain. It is difficult to confirm the presence of the lattice distortion. This is because the CAAC-OS has ab-plane orientation. In the case of the SiO2, the arrangement of oxygen atoms is not dense, and the bond distance between atoms is reduced by the substitution of metal elements. This is because distortion can be tolerated due to changes in the distance, etc.
[0210] In addition, the CAAC-OS has a layer containing indium and oxygen (hereinafter, the In layer) and an elemental A layered crystal consisting of layers containing element M, zinc, and oxygen (hereinafter referred to as the (M,Zn) layer). Indium and element M tend to have a layered structure. When the element M in the (M,Zn) layer is replaced with indium, (In,M,Zn ) layer. Also, when the indium in the In layer is replaced with the element M, (In, M) layer.
[0211] CAAC-OS is a highly crystalline metal oxide. Since it is difficult to confirm the grain boundaries, the decrease in electron mobility caused by the grain boundaries is unlikely to occur. In addition, the crystallinity of metal oxides is reduced by the incorporation of impurities and the generation of defects. Therefore, CAAC-OS is designed to prevent impurities and defects (oxygen vacancies (V O :oxygen v It can also be said to be a metal oxide with low acancy. Metal oxides with CAAC-OS have stable physical properties. The metal oxides used are heat resistant and highly reliable.
[0212] nc-OS is a material that is used in microscopic regions (e.g., regions between 1 nm and 10 nm, especially regions between 1 nm and The atomic arrangement has periodicity in the region of 3 nm or less. There is no regularity in the crystal orientation between the crystals. Therefore, no orientation is observed throughout the film. Therefore, depending on the analysis method, nc-OS may be classified as a-like OS or amorphous oxide semiconductor. Sometimes it is indistinguishable from the body.
[0213] In addition, indium oxide, which is a type of metal oxide containing indium, gallium, and zinc, Insium-gallium-zinc oxide (IGZO) is composed of the above-mentioned nanocrystals. In particular, IGZO tends to have difficulty growing crystals in the air. Therefore, smaller crystals are more difficult to measure than larger crystals (here, crystals of several mm or cm). In some cases, crystals (eg, the above-mentioned nanocrystals) may be structurally more stable.
[0214] The a-like OS is a metal oxide semiconductor that has a structure between the nc-OS and the amorphous oxide semiconductor. The a-like OS has voids or low density regions. The ke-OS has a lower crystallinity than the nc-OS and CAAC-OS.
[0215] Oxide semiconductors (metal oxides) have a variety of structures, each with different properties. The oxide semiconductor of one embodiment of the present invention can be an amorphous oxide semiconductor, a polycrystalline oxide semiconductor, an a-li The ke-OS, nc-OS, and CAAC-OS may have two or more kinds.
[0216] [Transistors with metal oxide] Next, the case where the above metal oxide is used for a channel formation region of a transistor will be described. do.
[0217] By using the above metal oxide for the channel formation region of a transistor, a high field effect can be achieved. It is possible to realize a transistor with high mobility. It can be realized.
[0218] In addition, it is preferable to use a metal oxide having a low carrier density for the transistor. In the case of lowering the carrier density of the metal oxide film, the impurity concentration in the metal oxide film is lowered. In this specification, the impurity concentration is low and the defect level density is low. A material with a low level of density is called high-purity intrinsic or substantially high-purity intrinsic. For example, metal oxides are , the carrier density is 8×10 11 / cm 3 Less than 1 x 10 11 / cm 3 Less than More preferably, 1×10 10 / cm 3 Less than 1 x 10 -9 / cm 3 That's it. stomach.
[0219] In addition, a highly pure intrinsic or substantially highly pure intrinsic metal oxide film has a low density of defect states. Therefore, the trap level density may be low.
[0220] In addition, the charges trapped in the trap levels of metal oxides take a long time to disappear. Therefore, the trap level density is high. A transistor having a metal oxide in a channel formation region may have unstable electrical characteristics. be.
[0221] Therefore, in order to stabilize the electrical characteristics of the transistor, the impurity concentration in the metal oxide must be In order to reduce the impurity concentration in the metal oxide, It is preferable to reduce the impurity concentration in the adjacent film. These include alkali metals, alkaline earth metals, iron, nickel, silicon, etc.
[0222] In addition, a thin film with high crystallinity is used as the metal oxide semiconductor for the transistor. The use of the thin film improves the stability or reliability of the transistor. The thin film may be, for example, a thin film of a single crystal metal oxide or a thin film of a polycrystalline metal oxide. However, thin films of single crystal metal oxides or thin films of polycrystalline metal oxides are also used. To form a thin film on a substrate, a high temperature or laser heating process is required. This increases the cost of the manufacturing process and also reduces throughput.
[0223] In 2009, the In-Ga-Zn oxide with CAAC structure (CAAC-IGZO) was developed. The discovery of the compound 1001, which is called "the compound 1001", has been reported in Non-Patent Document 1 and Non-Patent Document 2. CAAC-IGZO has a c-axis orientation, the grain boundaries are not clearly observed, and the low It has been reported that it is possible to form a thin film on a substrate at low temperatures. The transistors made using this method have been reported to have excellent electrical properties and reliability.
[0224] In 2013, the company also developed an In-Ga-Zn oxide (nc-IGZO) with an nc structure. (See Non-Patent Document 3.) Here, nc-IGZO is a microscopic area The atomic arrangement has periodicity in the region (for example, the region of 1 nm to 3 nm), and different It has been reported that there is no regularity in the crystal orientation between the domains.
[0225] In Non-Patent Documents 4 and 5, the above CAAC-IGZO, nc-IGZO, The average crystal size of IGZO and low-crystalline IGZO thin films was measured by electron beam irradiation. The graph shows the change in the crystallinity of the thin film of IGZO before it was irradiated with an electron beam. Even in thin films, IGZO with a crystallinity of about 1 nm has been observed. In this study, completely amorphous structure In addition, the presence of IGZO, which has low crystallinity, was not confirmed. Compared with the thin films of CAAC-IGZO and nc-IGZO, the thin films of CAAC-IGZO and nc-IGZO were irradiated with electron beams. Therefore, CAA is a promising semiconductor for transistors. It is preferable to use a C-IGZO thin film or an nc-IGZO thin film.
[0226] Transistors using metal oxide have extremely low leakage current when off. Specifically, the off-state current per 1 μm of the transistor channel width is yA / μm (10 -2 4 For example, the non-patent document 6 shows that the order of the capacitance is 100 nm. The low leakage current of the transistors used in these chips is utilized to develop low-power CPUs. (See Non-Patent Document 7).
[0227] In addition, the leakage current of a transistor using a metal oxide is low. The application of transistors to display devices has been reported (see Non-Patent Document 8). In this case, the displayed image changes several dozen times per second. The number is called the refresh rate. The refresh rate is also called the drive frequency. Such high-speed screen switching, which is difficult for the human eye to perceive, can cause eye fatigue. This is thought to be the cause. Therefore, the refresh rate of the display device is lowered to improve image quality. It has been proposed to reduce the number of times the display is rewritten. By driving the display device, it is possible to reduce the power consumption of the display device. This is called idle stop (IDS) drive.
[0228] The discovery of the CAAC and nc structures led to the discovery of metal oxides with the CAAC or nc structures. The electrical characteristics and reliability of the transistor using the material are improved, and the manufacturing process is reduced in cost. This contributes to lowering the leakage current and improving throughput. Taking advantage of these characteristics, research is being conducted into the application of these transistors to display devices and LSIs. is.
[0229] [impurities] Here, the influence of each impurity in the metal oxide will be described.
[0230] When metal oxides contain silicon or carbon, which are group 14 elements, the metal oxide This leads to the formation of defect levels in the oxides. The concentration of silicon and carbon near the interface with the metal oxide was measured by secondary ion mass spectrometry (SIM S: Secondary Ion Mass Spectrometry The concentration of 18 atoms / cm 3 Less than or equal to 2×10 17 atoms / cm 3 The following applies.
[0231] In addition, when an alkali metal or alkaline earth metal is contained in a metal oxide, a defect level is formed. Therefore, alkali metals or alkaline earth metals may form a carrier. A transistor that uses a metal oxide containing metals in the channel formation region is a normally-on transistor. Therefore, the concentration of alkali metals or alkaline earth metals in the metal oxide Specifically, it is preferable to reduce the degree of Al in the metal oxide obtained by SIMS. The concentration of potassium metal or alkaline earth metal is 1×10 18 atoms / cm 3 The following are the preferred Or 2×10 16 atoms / cm 3 To the following:
[0232] In addition, when nitrogen is contained in a metal oxide, electrons that act as carriers are generated, and the carriers The density increases and it becomes easier to make the metal oxide containing nitrogen into a channel type. The transistors used in the metal-doped region tend to be normally-on. In the oxide, it is preferable that the nitrogen in the channel formation region is reduced as much as possible. For example, the nitrogen concentration in metal oxide is 5×10 19 atoms / cm 3 Less than 5 x 10 18 atoms / cm 3 Less than or equal to 1×10 18 atoms / cm 3 Less than 5×10, more preferably 17 atoms / cm 3 The following .
[0233] In addition, hydrogen contained in metal oxides reacts with oxygen that bonds with metal atoms to form water. When hydrogen enters the oxygen vacancy, the carrier In some cases, hydrogen atoms are formed by bonding with oxygen atoms that bond with metal atoms. Therefore, metal oxides containing hydrogen can generate electrons that are carriers. The transistor used tends to have normally-on characteristics.
[0234] In addition, hydrogen contained in metal oxides is generated at shallow defect levels (sDOS) in the metal oxides. In some cases, low level density states may be formed. Shallow defect levels refer to interface states located near the bottom of the conduction band. Shallow defect levels are found in metals. It is presumed that they exist near the boundary between high density and low density regions in the oxide. The high density and low density regions in the metal oxide are distinguished by the amount of hydrogen contained in the regions. That is, the high density region contains more hydrogen than the low density region. Microcracks are formed near the boundary between the high density and low density regions due to the stress and strain between the two regions. This tends to cause oxygen vacancies and indium dangling bonds near the cracks. When impurities such as hydrogen or water are localized here, shallow defect levels are formed. It is presumed that
[0235] Also, the high density regions in the metal oxide may be more crystalline than the low density regions. In addition, the high density region in the metal oxide may have a higher film density than the low density region. In addition, when the metal oxide has a composition containing indium, gallium, and zinc, The high density region includes indium, gallium, and zinc, and the low density region includes indium. In other words, the low density regions may have more gallium and zinc than the high density regions. The proportion of um may be low.
[0236] The shallow defect level is presumed to be caused by oxygen vacancies. As the loss increases, the shallow defect levels as well as the deep defect levels (dDOS) It is estimated that the density of states (DDS) will also increase. This is because it is believed to be due to oxygen deficiency. This refers to a defect level located near the center of the gap.
[0237] Therefore, by suppressing oxygen vacancies in metal oxides, shallow and deep defect levels can be reduced. It is possible to reduce both the levels of shallow defects and the levels of shallow defects. It may be possible to control this to some extent by adjusting the temperature during film formation of the oxide. The temperature during the deposition of the metal oxide is set to 170° C. or thereabouts, preferably 130° C. or thereabouts. By setting the temperature at about room temperature, or more preferably at room temperature, shallow defect levels can be reduced.
[0238] In addition, the shallow defect levels of metal oxides are important for the electrical properties of transistors that use metal oxides as semiconductor layers. That is, shallow defect levels affect the drain current of transistors. -In the gate voltage (Id-Vg) characteristic, the drain current Id is The change is gradual, and the quality of the rise characteristics of the transistor from the off state to the on state is poor. The S value (also called Subthreshold Swing, SS) is one of the indicators of the ) deteriorates. This is believed to be due to electrons being trapped in shallow defect levels.
[0239] For this reason, it is preferable that the amount of hydrogen in the metal oxide is reduced as much as possible. is the hydrogen concentration obtained by SIMS in metal oxides, expressed as 1×10 20 atoms / cm 3 Less than 1 x 10 19 atoms / cm 3 Less than 5×1 0 18 atoms / cm 3 less than 1×1018 atoms / cm 3 less than A metal oxide with sufficiently reduced impurities is used for the channel formation region of a transistor. By doing so, it is possible to impart stable electrical characteristics.
[0240] <Method for manufacturing semiconductor device> Next, a method for manufacturing a semiconductor device having a transistor 200 according to the present invention will be described with reference to FIG. 4 to 13. In addition, in each of FIG. 4 to 13, (A) is a top view. In addition, (B) in each figure corresponds to the region indicated by the dashed line A1-A2 in (A). 1 is a cross-sectional view of the transistor 200 taken along the channel length direction. C) is a cross-sectional view corresponding to the portion indicated by the dashed line A3-A4 in (A), The figures are also cross-sectional views of the channel width direction of the capacitor 200. For clarity, some elements are omitted from the illustration.
[0241] First, a substrate (not shown) is prepared, and an insulator 210 is formed on the substrate. The deposition of 210 was performed by sputtering, chemical vapor deposition (CVD), and or Deposition method, Molecular Beam Epitaxy (MBE) Beam Epitaxy method, Pulsed Laser Deposition (PLD) Deposition method or ALD (Atomic Layer Deposition) method This can be done using the tion method, etc.
[0242] The CVD method is a process that uses plasma (PECVD). Enhanced CVD method, Thermal CVD (TCVD) These methods are further classified into the VD method, which uses light, and the Photo CVD method, which uses light. Depending on the source gas, metal CVD (MCVD: Metal CVD) method, metal organic CVD method (MOCVD: Metal Organic CVD) method.
[0243] The plasma CVD method can produce high-quality films at relatively low temperatures. This is a film formation method that can reduce plasma damage to the workpiece because it does not use a plasma. For example, wiring, electrodes, elements (transistors, capacitors, etc.) included in a semiconductor device ) may become charged up by receiving an electric charge from the plasma. When accumulated electric charges destroy wiring, electrodes, elements, etc., contained in a semiconductor device. On the other hand, in the case of thermal CVD, which does not use plasma, such plasma damage occurs. Since the thermal CVD method does not require any heat treatment, the yield of the semiconductor device can be increased. Since no plasma damage occurs in the film, a film with few defects can be obtained.
[0244] In addition, the ALD method is also a film formation method that can reduce plasma damage to the workpiece. In addition, the ALD method produces films with fewer defects because no plasma damage occurs during film formation. It should be noted that some precursors used in the ALD method contain impurities such as carbon. For this reason, films deposited by the ALD method have a higher However, it may contain a large amount of impurities such as carbon. The amount of impurities is quantified using X-ray photoelectron spectroscopy ( Using XPS (X-ray Photoelectron Spectroscopy) This can be done.
[0245] The CVD and ALD methods are deposition methods in which particles emitted from a target are deposited. It is a film forming method in which a film is formed by a reaction on the surface of the object to be treated. Therefore, this is a film forming method that is not easily affected by the shape of the workpiece and has good step coverage. In addition, the ALD method has excellent step coverage and thickness uniformity, making it ideal for achieving high aspect ratios. However, the ALD method is relatively slow in forming a film. Because the deposition rate is slow, it should be used in combination with other deposition methods such as CVD, which has a faster deposition rate. may be preferred.
[0246] In the CVD and ALD methods, the composition of the resulting film is controlled by the flow rate ratio of the source gases. For example, in the CVD and ALD methods, the flow rate ratio of the source gases can be adjusted to any value. In addition, for example, in the CVD method and the ALD method, the film formation By changing the flow rate ratio of the source gas while heating, a film with a continuously changing composition can be formed. When forming a film while changing the flow rate ratio of the source gas, multiple film forming chambers can be used. Compared to forming a film using a vacuum, the time required for film formation is shorter because there is no time required for transportation or pressure adjustment. Therefore, the productivity of the semiconductor device can be improved. There is.
[0247] In this embodiment, the insulator 210 is formed by sputtering aluminum oxide. The insulator 210 may be formed as a multi-layer structure. For example, a sputtering method is used. Then, an aluminum oxide film is formed by the ALD method. Alternatively, a film of aluminum may be formed by the ALD method. A film of aluminum oxide is formed on the aluminum oxide by a sputtering method. A membrane structure may also be used.
[0248] Next, the insulator 212 is formed on the insulator 210. The insulator 212 is formed by sputtering. The deposition can be performed by using a deposition method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, the insulator 212 is formed of silicon oxide by a CVD method.
[0249] Next, an opening is formed in the insulator 212, reaching the insulator 210. The opening may be, for example, a groove. Also, the term "opening" may refer to the area where an opening is formed. The openings may be formed by wet etching, but it is more preferable to use dry etching. In addition, the insulator 210 is formed by etching the insulator 212. It is preferable to select an insulator that functions as an etching stopper film when forming an opening. For example, when a silicon oxide film is used for the insulator 212 that forms the opening, the insulator 21 0 is an insulating film that functions as an etching stopper film, and is made of silicon nitride film, aluminum oxide film, etc. For example, a hafnium oxide film or a hafnium oxide film may be used.
[0250] After the opening is formed, a conductive film that will become the conductor 203a is formed. The conductive film has oxygen permeability. It is preferable that the conductive material contains a conductive material having a function of suppressing the above-mentioned. For example, tantalum nitride ... etc. Alternatively, tantalum, tungsten, titanium, etc. may be used. It is a laminated film of tungsten, molybdenum, aluminum, copper, and molybdenum tungsten alloy. The conductive film that becomes the conductor 203a can be formed by a sputtering method, a CVD method, an MBE method, or the like. The deposition can be performed by using a deposition method, a PLD method, an ALD method, or the like.
[0251] In this embodiment, a conductive film that becomes the conductor 203a is formed by sputtering a nitride film. A film of titanium nitride laminated on tantalum oxide or tantalum nitride is formed. By using such a metal nitride as the conductor 203a, it is possible to form a conductor such as copper as the conductor 203b described later. Even if a metal that is easily diffused is used, the metal is prevented from diffusing out of the conductor 203a. It is possible.
[0252] Next, a conductive film that will become the conductor 203b is formed on the conductive film that will become the conductor 203a. The conductive film is formed by a sputtering method, a CVD method, an MBE method, a PLD method, or an ALD method. In this embodiment, the conductive film that becomes the conductor 203b is A film of a low resistance conductive material such as copper is deposited.
[0253] Next, a CMP process is performed to form a conductive film that will become the conductor 203a and the conductive film 203 A part of the conductive film to be b is removed to expose the insulator 212. As a result, the conductive film is left only in the opening. The conductive film that will become the conductor 203a and the conductive film that will become the conductor 203b remain. Thus, a conductor 203 having a flat upper surface and including a conductor 203a and a conductor 203b is formed. (See FIG. 4.) Note that the CMP process removes a part of the insulator 212. This may be the case.
[0254] Next, the insulator 214 is formed on the insulator 212 and the conductor 203. The deposition of the film is performed using the sputtering method, CVD method, MBE method, PLD method, or ALD method. In this embodiment, the insulator 214 is a nitride film formed by a CVD method. In this way, a silicon film is formed as the insulator 214, which is made of silicon nitride or the like through which copper is transmitted. By using an insulator that is difficult to disperse, even if a metal that easily diffuses, such as copper, is used for the conductor 203b, , the metal can be prevented from diffusing into layers above the insulator 214.
[0255] Next, the insulator 216 is deposited on the insulator 214. The deposition of the insulator 216 is carried out by sputtering. The deposition can be performed by using a deposition method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, the insulator 216 is formed as a silicon oxide film by a CVD method.
[0256] Next, an opening is formed in the insulator 214 and the insulator 216 so as to reach the conductor 203. The opening may be formed by wet etching, but it is more preferable to use dry etching. is preferable for microfabrication.
[0257] After the opening is formed, a conductive film that will become the conductor 205a is formed. The conductive film has a property that prevents oxygen from passing through. It is preferable that the conductive material contains a conductive material having a function of suppressing the heat generation. For example, tantalum nitride, tantalum nitride, etc. Alternatively, tantalum, tungsten, titanium nitride, etc. may be used. It is a laminated film of tungsten, molybdenum, aluminum, copper, and molybdenum-tungsten alloy. The conductive film that becomes the conductor 205a can be formed by a sputtering method, a CVD method, an MB method, or the like. The deposition can be performed by using the E method, the PLD method, the ALD method, or the like.
[0258] In this embodiment, a conductive film that becomes the conductor 205a is formed by sputtering a nitride film. A tantalum oxide film is formed.
[0259] Next, a conductive film that will become the conductor 205b is formed on the conductive film that will become the conductor 205a. The conductive film is formed by a sputtering method, a CVD method, an MBE method, a PLD method, or an ALD method. This can be done using, for example.
[0260] In this embodiment, the conductive film that becomes the conductor 205b is a titanium nitride film formed by a CVD method. A film of titanium nitride is then formed on the titanium nitride by a CVD method.
[0261] Next, a CMP process is performed to form a conductive film that will become the conductor 205a and the conductive film 205 A part of the conductive film to be b is removed to expose the insulator 216. As a result, the conductive film is left only in the opening. The conductive film that will become the conductor 205a and the conductor 205b remains. In this case, the conductor 205 can be formed by using the conductor 205a and the conductor 205b. (See FIG. 4.) Note that the CMP process may remove a portion of the insulator 216. do.
[0262] Next, the insulator 220 is formed on the insulator 216 and the conductor 205. The deposition of the film is performed using the sputtering method, CVD method, MBE method, PLD method, or ALD method. In this embodiment, the insulator 220 is made of an oxide film formed by a CVD method. A silicon film is formed.
[0263] Next, an insulator 222 is formed on the insulator 220. The insulator 222 is made of aluminum. It is preferable to form an insulator containing oxides of either or both of Al and hafnium. As an insulator containing oxides of one or both of aluminum and hafnium, aluminum oxide Hafnium, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminium It is preferable to use aluminum and / or hafnium. The insulator containing the oxide has a barrier property against oxygen, hydrogen, and water. 2 has a barrier property against hydrogen and water, and thus is provided around the transistor 200. Hydrogen and water contained in the resulting structure pass through the insulator 222 to the transistor 200. Inward diffusion is suppressed, and the generation of oxygen vacancies in the oxide 230 can be suppressed. do.
[0264] The insulator 222 is formed by sputtering, CVD, MBE, PLD, or A. This can be done using the LD method or the like.
[0265] Next, the insulator 224 is deposited on the insulator 222. The deposition of the insulator 224 is carried out by sputtering. The deposition can be performed by using a deposition method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, the insulator 224 is formed as a silicon oxide film by a CVD method.
[0266] Subsequently, it is preferable to carry out a heat treatment. The heat treatment is preferably carried out at a temperature of 250° C. or more and 650° C. or less. The temperature is preferably 300° C. or higher and 500° C. or lower, and more preferably 320° C. or higher and 450° C. or lower. Heat treatment should be performed in a nitrogen or inert gas atmosphere, or in an atmosphere containing oxidizing gas at less than 10 ppm. The heat treatment is carried out in an atmosphere containing 1% or more, or 10% or more. Alternatively, the heat treatment may be performed in a nitrogen or inert gas atmosphere, followed by desorption. To compensate for the lost oxygen, an atmosphere containing oxidizing gas at 10 ppm or more, 1% or more, or 10% or more Heat treatment may be carried out in air.
[0267] In this embodiment, the heat treatment is performed in a nitrogen atmosphere at 400° C. after the insulator 224 is formed. The heat treatment is performed for one hour at a temperature of 100° C. The hydrogen and water contained in the insulator 224 are removed by the heat treatment. It is possible to remove impurities such as
[0268] The heat treatment is performed after the formation of the insulator 220 and after the formation of the insulator 222. The heat treatment can be performed under the above-mentioned heat treatment conditions. However, the heat treatment after the formation of the insulator 220 is preferably performed in an atmosphere containing nitrogen.
[0269] Here, in order to form an excess oxygen region in the insulator 224, a plasma containing oxygen is used under reduced pressure. The oxygen-containing plasma treatment may be, for example, a high-density plasma treatment using microwaves. It is preferable to use a device having a power source for generating plasma. Alternatively, RF is provided on the substrate side. The high density plasma may be generated by applying a power source to the plasma source. By using this, high density oxygen radicals can be generated, and RF is applied to the substrate side. This allows oxygen radicals generated by high-density plasma to be efficiently introduced into the insulator 224. Alternatively, after performing a plasma treatment containing an inert gas using this apparatus, In order to compensate for the desorbed oxygen, a plasma treatment including oxygen may be performed. By appropriately selecting the conditions of the laser treatment, impurities such as hydrogen and water contained in the insulator 224 can be removed. In this case, the heat treatment is not necessary.
[0270] Here, the insulator 280, the insulator 244A, and the An insulator may be formed as a film to function as a stopper when etching the conductor 242B. As the insulator, any insulator that can be used for the insulator 222 may be used. The substrate is deposited by sputtering, CVD, MBE, PLD, or ALD. After the insulator film is formed, the above-mentioned heat treatment may be performed.
[0271] Next, on the insulator 224, an oxide film 230A which becomes the oxide 230a, and an oxide film 230b which becomes the oxide 230b are formed. The oxide film 230B is then formed in this order (see FIG. 4). It is preferable to form the oxide film 230 continuously without exposing the oxide film 230 to the atmosphere. A, and prevent impurities or moisture from the atmospheric environment from adhering onto the oxide film 230B. This makes it possible to keep the vicinity of the interface between the oxide film 230A and the oxide film 230B clean.
[0272] The oxide film 230A and the oxide film 230B are formed by sputtering, CVD, MBE, etc. The deposition can be performed by using a deposition method, a PLD method, an ALD method, or the like.
[0273] For example, the oxide film 230A and the oxide film 230B are formed by a sputtering method. In this case, oxygen or a mixture of oxygen and a rare gas is used as the sputtering gas. By increasing the ratio of oxygen contained in the sputtering gas, the excess oxygen in the oxide film to be formed is reduced. In addition, when the oxide film is formed by sputtering, For example, an In-M-Zn oxide target can be used.
[0274] In particular, when the oxide film 230A is formed, a part of the oxygen contained in the sputtering gas becomes an insulator. Therefore, the oxide film 230A may be sputtered with the oxide gas 224. The percentage of oxygen contained in the gas should be 70% or more, preferably 80% or more, and more preferably 100%. That's good.
[0275] In addition, when the oxide film 230B is formed by a sputtering method, the oxide film 230B is formed by sputtering. The ratio of oxygen to be added is set to 1% or more and 30% or less, preferably 5% or more and 20% or less. The oxygen-deficient oxide semiconductor is formed in the channel formation region. A transistor using this region can achieve a relatively high field effect mobility.
[0276] In this embodiment, the oxide film 230A is formed by sputtering In:Ga: The film is formed using a target of Zn=1:3:4 [atomic ratio]. In addition, the oxide film 230B and Then, the In:Ga:Zn atomic ratio was 4:2:4.1 by sputtering. Each oxide film is formed by appropriately selecting the film formation conditions and atomic ratio. In this way, it is possible to form the oxide 230 according to the desired characteristics.
[0277] Next, a heat treatment may be performed. The heat treatment may be performed under the above-mentioned heat treatment conditions. By the heat treatment, impurities such as hydrogen and water in the oxide film 230A and the oxide film 230B are removed. In this embodiment, the wafer is heated at 400° C. in a nitrogen atmosphere. After one hour of treatment, the sample was treated in an oxygen atmosphere at 400°C for one hour. cormorant.
[0278] Next, a conductive film 242A is formed on the oxide film 230B. Aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, titanium, molybdenum, tungsten Niobium, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium Gold selected from tungsten, indium, ruthenium, iridium, strontium, and lanthanum or an alloy containing the above metallic elements or a combination of the above metallic elements. It is preferable to use an alloy, etc. For example, tantalum nitride, titanium nitride, tungsten, titanium Nitrides containing tantalum and aluminum, nitrides containing tantalum and aluminum, ruthenium oxide Ruthenium, ruthenium nitride, oxides containing strontium and ruthenium, lanthanum and nickel It is preferable to use oxides containing tantalum nitride, titanium nitride, titanium and aluminium. Aluminum nitrides, tantalum and aluminum nitrides, ruthenium oxide, nitrides Ruthenium, oxides containing strontium and ruthenium, oxides containing lanthanum and nickel The material is a conductive material that does not easily oxidize or that maintains its conductivity even when it absorbs oxygen. The conductive film 242A can be formed by a sputtering method, a CVD method, an MBE method, or the like. The deposition can be performed by using a deposition method, a PLD method, an ALD method, or the like.
[0279] Next, the conductive film 242A is processed, and the oxide film 230A and the oxide film 230B are processed. A hard mask is formed for this purpose.
[0280] The conductive film 242A may be processed by lithography. Dry etching or wet etching can be used. The processing by this method is suitable for microfabrication.
[0281] In the lithography method, first, the resist is exposed through a mask. The regions are removed or left using a developer to form a resist mask. By etching through a resist mask, conductors, semiconductors, insulators, etc. can be obtained as desired. For example, KrF excimer laser light, ArF excimer laser light, The resist is removed using ultraviolet (EUV) light, X-rays, and other light sources. A resist mask can be formed by exposing the substrate to light. A liquid immersion technique may be used in which the substrate is exposed to light by filling the substrate with liquid (e.g., water). Alternatively, an electron beam or an ion beam may be used. In this case, since the pattern is drawn directly on the resist, the above-mentioned mask for resist exposure is not required. The resist mask is then subjected to a dry etching process such as ashing, or a wet etching process. Etching is performed, wet etching is performed after dry etching, or can be removed by wet etching followed by dry etching, etc. Cut.
[0282] Next, the conductive film 242A is etched using a resist mask to form a hard mask. After the conductor 242B is formed, The oxide film may be processed after removing the resist mask, or the resist mask may be left on. In the latter case, the resist mask may disappear during etching. After etching the oxide film, the hard mask may be removed by etching. In the embodiment, the conductor 242B is further processed to form a source electrode and a drain electrode. Therefore, conductor 242B is not removed.
[0283] The dry etching equipment is a capacitively coupled plasma (CCP) device with parallel plate electrodes. : Capacitively Coupled Plasma (CAP) etching equipment is used. The capacitively coupled plasma etching apparatus having parallel plate electrodes can Alternatively, a high frequency power source may be applied to one of the parallel plate type electrodes. A configuration in which a plurality of different high frequency power sources are applied to the electrodes may be used. Alternatively, a parallel plate electrode may be used. Alternatively, a high-density plasma source may be provided. A dry etching apparatus having a high density plasma source can be used. The plasma processing device is, for example, an inductively coupled plasma (ICP) type. A plasma etching apparatus or the like can be used.
[0284] Next, the conductor 242B is used as a hard mask to form the oxide film 230A and the oxide film 23 0B is processed into islands to form oxide 230a and oxide 230b (see FIG. 5). ) In addition, a part of the insulator 224 may be removed during this processing.
[0285] Here, the oxide 230a and the oxide 230b are at least partially connected to the conductor 205. The oxide 230a and the oxide 230b are formed so as to overlap each other. It is preferable that the oxide 230a and the oxide 232 are substantially perpendicular to the upper surface of the oxide 230. The side surface of the insulator 222 is substantially perpendicular to the upper surface of the insulator 222, so that the plurality of transistors 2 When forming the oxide 230a, it is possible to reduce the area and increase the density. Alternatively, the angle between the side surface of the insulating material 230b and the top surface of the insulating material 222 may be an acute angle. In this case, the angle between the side surface of the oxide 230a and the top surface of the insulator 222 is large. The higher the better.
[0286] In addition, the oxide 230a, the oxide 230b, and the side surfaces of the conductor 242B and the conductor 24 2B and the top surface of the casing 2B, the end of the side surface and the end of the top surface are curved. The curved surface is preferably a curved surface of the conductor 242B. At the end, the radius of curvature is 3 nm or more and 10 nm or less, preferably 5 nm or more and 6 nm or less. The absence of sharp edges improves film coverage in the subsequent film formation process.
[0287] The oxide film is processed by dry etching using the conductor 242B as a hard mask. Dry etching and wet etching can be used. Suitable for processing.
[0288] In addition, by carrying out the above-mentioned dry etching process, the etching gas, etc. Impurities caused by the oxidation may adhere to the side or inside of the oxide 230a and the oxide 230b. Impurities may include, for example, fluorine or chlorine.
[0289] In order to remove the above impurities, cleaning is performed. These include wet cleaning, plasma treatment using plasma, and cleaning by heat treatment. The above cleaning methods may be combined as appropriate.
[0290] Wet cleaning uses oxalic acid, phosphoric acid, hydrogen peroxide, or hydrofluoric acid. The cleaning process may be carried out using an aqueous solution diluted with carbonated water or pure water. Alternatively, ultrasonic cleaning using carbonated water may be performed. In this embodiment, pure water or carbonated water is used. Then, ultrasonic cleaning is performed.
[0291] Subsequently, a heat treatment may be performed. The heat treatment conditions are the same as those described above. However, if there is a concern that the conductor 242B may be oxidized by the heat treatment, The heat treatment is preferably performed in an atmosphere that does not contain oxygen. In the case where an oxidation-resistant material is included, the heat treatment may be carried out in an atmosphere containing oxygen.
[0292] Next, an insulating layer is formed on the insulator 224, the oxide 230a, the oxide 230b, and the conductor 242B. An insulator 244A is formed (see FIG. 6). The insulator 244A acts as an insulating barrier. Preferably, the oxides include one or both of aluminum and hafnium. It is preferable to form an insulating film containing an oxide of aluminum or hafnium or both. Examples of insulators containing oxides include aluminum oxide, hafnium oxide, aluminum and hafnium oxide. It is preferable to use oxides containing hafnium (e.g. hafnium aluminate). The insulator 244A having the above structure can suppress oxidation of the conductor 242B. If the conductor 242B includes an oxidation-resistant material, the insulator 244A does not necessarily have to be provided. The insulator 244A can be formed by sputtering, CVD, MBE, or PLD. The deposition can be performed by using a deposition method, an ALD method, or the like.
[0293] Next, the insulator 280 is formed on the insulator 244A. The insulator 280 has a relative dielectric constant of It is preferable to have a low insulator, for example, silicon oxide, silicon oxynitride, silicon oxide, or silicon nitride. Silicon oxide, silicon nitride, silicon oxide doped with fluorine, silicon oxide doped with carbon silicon oxide doped with carbon and nitrogen, silicon oxide with voids, or resin. In particular, silicon oxide, silicon oxynitride, silicon nitride oxide, etc. When silicon oxide having vacancies is used for the insulator 280, the insulator 280 may become vacant in a later process. This is preferable because an excess oxygen region can be easily formed. The insulator 280 is preferably formed by sputtering, CV The method can be performed by using a deposition method, an MBE method, a PLD method, an ALD method, or the like. Pin coat method, dip method, droplet ejection method (inkjet method, etc.), printing method (screen printing, offset printing, etc.), doctor knife method, roll coater method, or curtain coater method In this embodiment, the insulator 280 is a CV A silicon oxynitride film is formed by method D.
[0294] It is preferable that the insulator 280 is formed so that the upper surface is flat. For example, Alternatively, the insulator 280 may have a flat upper surface immediately after deposition. After deposition, the insulator 280 is formed by aligning the insulator from above so that it is parallel to a reference plane such as the back surface of the substrate. By removing the surface, the surface can be made flat. This process is called flattening. The polishing process includes CMP process, dry etching process, etc. As the flattening process, a CMP process is used. However, the top surface of the insulator 280 is not necessarily flat. It is not necessary to have one.
[0295] Next, the insulator 280 is heated so as to have at least an area overlapping the conductor 205. Then, a processing step is performed to form an opening 245 (see FIG. 7). However, the side of the insulator 280 can be machined approximately vertically, which is advantageous from the viewpoint of fine machining. It is preferable to use a dry etching method because the opening 245 can be formed by the following method. This is preferably done by forming a hard mask on the insulator 280. An electric conductor or an insulator may be used.
[0296] Next, the insulator 244A and the conductor 242B are processed, and the insulator 244 and the conductor 242 (conductor 242a and conductor 242b) are formed (see FIG. 8). In the above process, it is preferable to use dry etching capable of performing anisotropic etching. , the side of the oxide 230a, the surface of the oxide 230b, the side, and one of the surfaces of the insulator 224 In addition, a portion of the insulator 224 may be etched away by the processing. In addition, the cross section of the surface where the conductor 242a and the conductor 242b face each other is tapered. Alternatively, the cross section may have a generally vertical shape.
[0297] At this time, the insulator 280 and / or the hard mask are used as a mask to form a conductive Thus, the opening formed in the insulator 280 forms the conductive body 242a and the conductive body 242b. 245 overlaps the area between the conductor 242a and the conductor 242b. In a later step, the conductor 260 is self-aligned between the conductors 242a and 242b. can be positioned objectively.
[0298] Here, it is preferable to carry out a heat treatment. The heat treatment is preferably carried out at a temperature of 250° C. or higher and 650° C. or lower. The reaction temperature is preferably 300° C. or higher and 500° C. or lower, and more preferably 320° C. or higher and 450° C. or lower. The heat treatment is performed in a nitrogen or inert gas atmosphere. In the case of a conductor having oxidation resistance, the heat treatment may be performed in an atmosphere containing oxygen. The heat treatment may be performed under reduced pressure. For example, the heat treatment may be performed under a nitrogen atmosphere at 400 Treatment is carried out at a temperature of °C for 1 hour.
[0299] The heat treatment removes hydrogen, water, and the like contained in the oxide 230a and the oxide 230b. Impurities can be removed. In addition, the oxide 2 can be removed by dry etching in the above process. Damage to the oxide 230b or oxide 230a can be repaired. When the heat treatment is performed in an atmosphere containing oxygen, oxygen is added to the oxide 230a and the oxide 230b. It can be added.
[0300] In addition, the above-mentioned metal elements are diffused from the conductor 242 to the oxide 230 by the above-mentioned heat treatment. In addition, the oxide 230 can be doped with a metal element. Oxygen near the interface with conductor 242 may be absorbed by conductor 242. The vicinity of the interface between the object 230 and the conductor 242 becomes a metal compound, and the resistance becomes low. A part of the oxide 230 may be alloyed with the above-mentioned metal element. The metal element added to the oxide 230 becomes relatively stable by alloying with the metal element. Since the semiconductor device is in a highly reliable state, a highly reliable semiconductor device can be provided. As an example of the low resistance region of the oxide 230, a region 243a and a region Area 243b is shown.
[0301] The region 243a and the region 243b are adjacent to the conductor 242 of the oxide 230b. Although an example in which the dopant is provided so as to diffuse in the depth direction is shown, the present invention is not limited to this. The region 243a and the region 243b are formed throughout the oxide 230b in the depth direction. Alternatively, the region 243a may be formed in the oxide 230a. The region 243b is a region that is horizontally diffused from the conductor 242 (see FIG. 2). 231 and 232 shown in FIG. 23, the present invention is not limited thereto. The region 243a and the region 243b overlap with the conductor 242 (the region 231 ) or in a region (region) that overlaps with a portion of the conductor 260 formed in a later process. It may also be formed in the area 234 (part of the area 234).
[0302] Also, hydrogen in the oxide 230 diffuses to the region 231 shown in FIG. If the oxygen enters the oxygen vacancy in the region 234, the state becomes relatively stable. The hydrogen in the oxygen vacancies is released from the oxygen vacancies by heat treatment at 250°C or higher, and the hydrogen in the oxygen vacancies is released into the region 2. 31, enters the oxygen vacancies in the region 231, and becomes relatively stable. Therefore, the heat treatment makes the region 231 have a lower resistance, and the region 234 has a higher purity ( This reduces impurities such as water and hydrogen, resulting in higher resistance.
[0303] In addition, after heat treatment in a nitrogen or inert gas atmosphere, oxidizing gas is reduced to 10 ppm or more. The heat treatment may be performed in an atmosphere containing 1% or more, or 10% or more. 0°C or higher and 650°C or lower, preferably 300°C or higher and 500°C or lower, more preferably 320°C or higher The heating may be performed at a temperature of from 450°C to 500°C.
[0304] In addition, in the heat treatment after the formation of the conductive film 242A or the formation of the conductor 242, The conductive film 242A or the conductor 242 absorbs oxygen from the region 231 of the oxide 230. As a result, oxygen vacancies may occur in the region 231. By entering the loss, the carrier density in the region 231 increases. The region 231 becomes n-type and has a low resistance.
[0305] The oxygen concentration in region 231 may be lower than the oxygen concentration in region 234. The oxygen concentration in region 2 may be equal to or higher than the oxygen concentration in region 231 and equal to or lower than the oxygen concentration in region 234. In addition, the hydrogen concentration in the region 231 may be higher than the hydrogen concentration in the region 234. The hydrogen concentration in region 232 is equal to or greater than the hydrogen concentration in region 234 and equal to or less than the hydrogen concentration in region 231. There are cases.
[0306] Next, the side surface of the oxide 230a, the top surface and side surface of the oxide 230b, and the side surface of the conductor 242 2, an oxide 230c is formed on the insulator 280 so as to have a region in contact with the side surface of the insulator 280. Then, an oxide film 230C is formed (see FIG. 9).
[0307] The oxide film 230C is formed by a sputtering method, a CVD method, an MBE method, a PLD method, or the like. This can be done using the ALD method or the like. The oxide 230c can be selected according to the desired properties. The oxide film 230C is formed using the same film formation method as the oxide film 230A or the oxide film 230B. In the present embodiment, the oxide film 230C is formed by sputtering In. The film is formed using a target with an atomic ratio of Ga:Zn=1:3:4.
[0308] Next, an insulator 250A is formed on the oxide film 230C (see FIG. 9).
[0309] The insulator 250A is formed by sputtering, CVD, MBE, PLD, or ALD. The insulator 250A can be formed by depositing oxynitride by the CVD method. It is preferable to form a film of silicon carbide. The film forming temperature for forming the insulator 250A is It is preferable to set the temperature to 350°C or higher and lower than 450°C, and particularly to about 400°C. By forming the film at 400°C, an insulator with few impurities can be formed.
[0310] In addition, oxygen is excited by microwaves to generate high-density oxygen plasma, and the oxygen plasma is By exposing the insulator 250A to the argon, oxygen can be introduced into the insulator 250A.
[0311] Heat treatment may also be performed. The heat treatment may be performed under the above-mentioned heat treatment conditions. The heat treatment reduces the moisture concentration and hydrogen concentration of the insulator 250A. can be done.
[0312] Here, the conductor 242 and the conductor 260 formed in a later process may form a parasitic capacitance. That is, the insulating film provided on the side of the conductor 242 functions as a dielectric for the parasitic capacitance. On the other hand, the insulating film functions as a gate insulator for the transistor 200. It is preferable to form a thin film of 0 nm or less, preferably 10 nm or less, and more preferably 5 nm or less. It is preferable to form the insulating film on the side of the conductor 242 so that the parasitic capacitance can be neglected. In order to make it thicker, the insulating film is formed in a laminate structure of two or more layers at least on the side of the conductor 242. It is preferable to use this structure.
[0313] Therefore, anisotropic etching is performed on the insulator 250A to remove the side and It is preferable to form an insulator 250B on the side of the insulator 280 via an oxide film 230C. (See Figure 10.)
[0314] Next, an insulator 250C is formed to cover the oxide film 230C and the insulator 250B. (See FIG. 11.) Insulator 250C is made of the same material and using the same equipment as insulator 250A. By the above process, an insulator 250C is formed above the oxide 230b. On the side of the conductor 242, an insulator 250B and an insulator 250C are provided. That is, the side of the conductor 242 may have a thicker insulating layer than the insulating layer above the oxide 230b. Insulation may be provided.
[0315] Next, a conductive film 260A and a conductive film 260B are formed in this order (see FIG. 11). The conductive film 260A and the conductive film 260B are formed by a sputtering method, a CVD method, an MBE method, a PLD method, or the like. For example, the conductive film 260A may be formed by a method such as a SiO2 method or an ALD method. Alternatively, a titanium nitride film may be formed, and then a tungsten film may be formed as the conductive film 260B.
[0316] The conductive film 260A is formed of a metal nitride by a CVD method or a sputtering method. By using a metal nitride for the conductive film 260A, the insulator 250C has This can prevent the conductive film 260B from being oxidized by oxygen and causing a decrease in conductivity.
[0317] In addition, by laminating a low-resistance metal film as the conductive film 260B, a transistor with a low driving voltage can be obtained. A transistor can be provided.
[0318] Subsequently, a heat treatment can be performed. The heat treatment can be performed under the above-mentioned heat treatment conditions. In some cases, the heat treatment is not necessary. A low resistance region may be formed in 230b.
[0319] Next, the conductive film 260B, the conductive film 260A, the insulator 250B, the insulator 250C, and the acid The conductive film 230C is processed and planarized, and the conductive material 260 (the conductive material 260a and the conductive material 260b) is formed. 260b), insulator 250 (insulator 250a and insulator 250b), and oxide. 12. The planarization process is performed by using the CMP method to form the conductive film 26. 0B, the conductive film 260A, the insulator 250B, the insulator 250C, and the oxide film 230C are polished. The conductive film 260B and the conductive film 260C are preferably formed by etching. 60A, insulator 250B, insulator 250C, and oxide film 230C must be processed together. It is not necessary to change the processing conditions, but rather it is sufficient to change the processing conditions as appropriate.
[0320] In this manner, the conductor 260 is electrically connected to the opening in the insulator 280 and to the conductor 242a. The conductive body 260 is formed so as to be embedded in the region sandwiched between the conductive bodies 242b. Since this is done in a self-aligned manner without using lithography, the alignment of the conductor 260 is Therefore, the area occupied by the transistor 200 can be reduced. This allows for miniaturization and high integration of semiconductor devices. In addition, no lithography process is required. Therefore, it is expected that productivity will be improved by simplifying the process.
[0321] In addition, to miniaturize semiconductor devices, it is necessary to shorten the gate length. It is necessary to prevent the conductivity of the conductor 260 from decreasing. Increasing the aspect ratio of the conductor 260 can result in a shape with a high aspect ratio. In order to embed the conductor 260 in the opening of the insulator 280, the conductor 260 is provided with asphalt. Even if the shape has a high aspect ratio, the conductor 260 can be formed without collapsing during the process. This can be done.
[0322] At this time, the conductor 260 is at least partially composed of the conductor 205, the oxide 230a, and The insulating layer 230 is formed so as to overlap the oxide 230b.
[0323] In addition, the upper surface of the insulator 280, the upper surface of the conductor 260, and the upper surface of the insulator 250 are It is preferable that the upper surface and the upper surface of oxide 230c are roughly coincident.
[0324] Here, the insulator 250b is made of the oxide 230b, the conductor 242a (the conductor 242b), and The insulator 250a is disposed between the conductor 242 and the insulator 280. a (conductor 242b), and is disposed between the insulator 280 and the insulator 250b. That is, the insulator 250 is disposed between the oxide 230b and the conductor 260. Between the conductor 242 and the conductor 260, an insulator 250a and an insulator 250b are provided. Therefore, by manufacturing the transistor 200 by the above method, the insulator 25 The thickness T1 of the conductive material 260 can be made thinner than the thickness T2. 242 and provides a transistor 200 having high frequency characteristics. It is possible.
[0325] In this embodiment, the insulator 250 is made of the insulator 250a and the insulator 250b. However, the method for manufacturing the semiconductor device shown in this embodiment is not limited to this. For example, in the anisotropic etching process shown in FIG. The area corresponding to the bottom of the opening 245 is not completely removed, but the thickness of the film in that area is reduced. This allows the insulator 250A alone to have a thickness T1 smaller than the thickness T2. A border 250 may be formed.
[0326] In this embodiment, the insulator 250 is made of two layers, an insulator 250a and an insulator 250b. However, the configuration of the transistor 200 is not limited to this. The number of layers of the insulator 250 located between the conductor 260 is set to be the number of layers of the oxide 230b and the conductor 260. If the number of layers of the insulator 250 located between the 10 and 110 is to be more than that of the 100, the insulator 250 must be composed of three or more layers. It may be formed.
[0327] Next, the insulator 274 is formed on the insulator 280 and the conductor 260 (see FIG. 13). The insulator 274 is made of aluminum and / or hafnium, which have barrier properties. For example, it is preferable to use an oxide of aluminum oxide by sputtering. By using a sputtering method, it is possible to form a film containing a large amount of oxygen. Moreover, it is possible to form an aluminum oxide film containing less impurities such as water or hydrogen.
[0328] In addition, by forming the film in an atmosphere containing oxygen gas using a sputtering device, Oxygen can also be introduced into the insulators 250 and 280 while the insulator 274 is being formed. As a result, the insulator 274 can be used as an oxygen source to supply oxygen to the insulators 250 and 280. The oxygen in the insulator 274 is supplied to the insulator 250 and the insulator 280, forming an excess oxygen region. can be formed.
[0329] The insulators 250 and 280 in which the excess oxygen regions are formed as described above are Oxygen is introduced from the excess oxygen region through oxide 230c, etc., to region 234 of oxide 230. can be effectively delivered.
[0330] Subsequently, a heat treatment can be performed. The heat treatment can be performed under the above-mentioned heat treatment conditions. By performing the heat treatment, oxygen contained in the insulator such as the insulator 250 is converted into oxide 23. 0. Also, the oxygen vacancies formed in the region 231 of the oxide 230 can be captured. The captured hydrogen is absorbed into the insulator 274 through the insulator 244 and the insulator 280. In some cases, hydrogen in the oxide 230 can be reduced.
[0331] Next, the insulator 281 is formed on the insulator 274. The insulator 281 is formed by sputtering. This can be done using deposition, CVD, MBE, PLD, or ALD methods. Alternatively, it can be applied by spin coating, dipping, droplet ejection (inkjet method, etc.), printing, etc. Printing method (screen printing, offset printing, etc.), doctor knife method, roll coater method, Alternatively, it can be performed by using a curtain coater method or the like. The body 281 is made of silicon oxynitride.
[0332] Next, a part of the insulator 281 is removed. The insulator 281 is removed so that the upper surface is flat. For example, the insulator 281 has a flat upper surface immediately after deposition. Alternatively, for example, the insulator 281 may be formed so as to be parallel to a reference plane such as the back surface of the substrate. The insulating material may be removed from the top surface to provide flatness. The process is called planarization. Planarization processes include CMP and dry etching. In this embodiment, the CMP process is used as the planarization process. The upper surface of 281 does not necessarily have to be flat.
[0333] Next, the insulators 281, 274, 280, and 244 are coated with oxide 2. An opening reaching 30 is formed. The opening may be formed by using a lithography method. The conductor 240a and the conductor 240b are provided in contact with the side surface of the oxide 230. In order to expose the side of the oxide 230 in the opening that reaches the oxide 230, The opening is formed.
[0334] Next, a conductive film that will become the first conductor of the conductor 240 and the second conductor of the conductor 240 is The conductive film is formed by a method such as sputtering, CVD, MBE, PLD, etc. Alternatively, it can be performed using an ALD method or the like.
[0335] Next, a CMP process is performed to form a conductive film that will become the conductor 240a and the conductor 240b. A part of the conductive film is removed to expose the insulator 281. As a result, the conductive film remains only in the opening. By virtue of the presence of the insulating layer 242, it is possible to form the conductor 240a and the conductor 240b having flat upper surfaces. (See FIG. 13.) In addition, in some cases, the insulator 281 is removed by the CMP process. There is.
[0336] In this manner, a semiconductor device including the transistor 200 can be manufactured. As shown in FIG. 13, by using the manufacturing method of a semiconductor device described in this embodiment mode, It is possible to manufacture a transistor 200 having excellent electrical characteristics and capable of being miniaturized or highly integrated. can.
[0337] According to one embodiment of the present invention, a semiconductor device that can be miniaturized or highly integrated can be provided. According to one embodiment of the present invention, a semiconductor device having favorable electrical characteristics can be provided. According to one embodiment of the present invention, a semiconductor device having favorable frequency characteristics can be provided. According to one embodiment of the present invention, a highly reliable semiconductor device can be provided. According to one embodiment of the present invention, a semiconductor device with low off-state current can be provided. According to one embodiment of the present invention, a semiconductor device having a large on-state current can be provided. According to one embodiment of the present invention, a semiconductor device with reduced power consumption can be provided. According to one embodiment of the present invention, a semiconductor device with high productivity can be provided. It is possible.
[0338] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.
[0339] <Modifications of the semiconductor device> In the following, the above-mentioned <Configuration Example of Semiconductor Device> will be described with reference to FIGS. 14 to 17. An example of a semiconductor device including a transistor 200 according to another embodiment of the present invention will be described. Reveal.
[0340] 14 to 17, (A) of each figure shows a top view. FIG. 1(A) is a cross-sectional view corresponding to the portion indicated by the dashed line A1-A2 in FIG. Also, (C) of each figure is a cross-sectional view of the channel length direction of the capacitor 200. 4 is a cross-sectional view of the transistor 200 in the channel width direction. In each figure, (A) is a top view, and some elements are omitted for clarity. It is omitted in the illustration.
[0341] In the semiconductor device shown in FIG. 14 to FIG. 17, The structures constituting the semiconductor device (see FIG. 1) and having the same functions are denoted by the same reference numerals. In this section, the constituent materials of the transistor 200 are described in the section "Construction of a Semiconductor Device" below. The materials described in detail in the Examples can be used.
[0342] The transistor 200 shown in FIG. 14 includes an oxide 230, a conductor 242, and an insulator 28. 1 in that an insulator 252 is disposed between the oxide 230c and the Unlike transistor 200, insulator 252 can be used for insulator 244. It is sufficient to use an insulator that has a function of suppressing the permeation of impurities such as hydrogen and oxygen. By using such an insulator 252, the conductors 242a and 242b Oxidation of the surface in contact with the insulator 252 can be suppressed.
[0343] In addition, the transistor 200 shown in FIG. 14 has an insulator between the conductor 242 and the conductor 260. 252 is provided between the oxide 230b and the conductor 260, and no insulator 252 is provided between the oxide 230b and the conductor 260. Therefore, in the transistor 200 shown in FIG. It is possible to reduce the parasitic capacitance between the electric conductor 260 and the electric conductor 242. In the transistor 200 shown in FIG. 1, the thickness of the insulator 250 between the conductor 242 and the conductor 260 is The thickness of the insulator 250 between the oxide 230b and the conductor 260 is approximately the same. This is also fine.
[0344] In the transistor 200 shown in FIG. 1, the oxide 230 is In the example shown, three layers of oxide 230a, oxide 230b, and oxide 230c are laminated. The semiconductor device shown in the embodiment is not limited to this. For example, the transistor shown in FIG. As in the case of the converter 200, the oxide 230c may not be provided.
[0345] In addition, in the transistor 200 shown in FIG. In the embodiment, the insulator 244 is provided to cover the semiconductor device 224. The conductor device is not limited to this. For example, an oxidation-resistant material is used for the conductor 242. In this case, even if the insulator 244 is not provided as in the transistor 200 shown in FIG. good.
[0346] By adopting a configuration in which the insulator 244 is not provided, the insulator 274 is formed. The oxygen added to the oxide 80 can be supplied from the side of the oxide 230. In this case, oxygen added to the insulator 280 is supplied to the oxide 230 via the insulator 224. This allows oxygen to be more effectively supplied to the region 234 of the oxide 230. can be done.
[0347] The transistor 200 shown in FIG. 17 differs from the transistor 200 shown in FIG. 17. In the transistor 200 shown in FIG. For example, the oxide 230 may be doped with an element that can increase the carrier density and reduce the resistance. Region 243 may be formed by adding it as a punt.
[0348] The dopant is an element that forms an oxygen vacancy or an element that bonds with the oxygen vacancy. Representative examples of such elements include boron and phosphorus. In addition, hydrogen, carbon, nitrogen, fluorine, sulfur, chlorine, titanium, rare gases, etc. may also be used. Representative examples of rare gas elements include helium, neon, argon, krypton, and xenon. Non-metallic, etc. Also, aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, Titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium Nesium, zirconium, beryllium, indium, ruthenium, iridium, strontium One or more metal elements selected from the group consisting of thium, lanthanum, etc. Among the above, boron and phosphorus are preferable as dopants. When uran or phosphorus is used as a dopant, amorphous silicon or low-temperature polysilicon Since the equipment for the manufacturing line of confectionery can be used, capital investment can be reduced. The concentrations of the above elements may be measured using SIMS or the like.
[0349] In particular, it is preferable to use an element that easily forms an oxide as the element to be added to the region 243. Representative examples of such elements include boron, phosphorus, aluminum, magnesium, and the like. The element added to the region 243 takes away oxygen from the oxide 230 to form the oxide. As a result, many oxygen vacancies are formed in the region 243. When the hydrogen in the oxide 230 is bonded to the SiO 2 , carriers are generated, resulting in an extremely low resistance region. Furthermore, since the element added to the region 243 exists in the region 243 in the form of a stable oxide, Even if a subsequent process requiring high temperatures is performed, the metal is unlikely to be desorbed from the region 243. That is, the element to be added to the region 243 is an element that easily forms an oxide. This allows the formation of a region in the oxide 230 that is resistant to high resistance even when subjected to high-temperature processes.
[0350] Forming regions 243 in the oxide 230 to function as source or drain regions. Thus, the region 243 is provided without providing a source electrode and a drain electrode made of a metal. A conductor 240 can be connected which acts as a plug.
[0351] When a region 243 is formed by the addition of a dopant, for example, oxide 230c, an insulating A dummy gate is formed at a position where the conductive body 250 and the conductive body 260 are to be provided. The dopant can be added using the oxide 230 as a mask. In the above, a region 243 containing the above element is formed in a region where the dummy gate does not overlap. It is possible.
[0352] The dopant addition method is ionization, in which the ionized source gas is mass-separated and added. The ion doping method, which adds ionized source gas without mass separation, The mass separation method can be used. When this is done, the type of ions to be added and their concentrations can be strictly controlled. If separation is not performed, a high concentration of ions can be added in a short time. Alternatively, an ion doping method may be used in which molecular clusters are generated and ionized. A dopant may also be referred to as an ion, a donor, an acceptor, an impurity, or an element. stomach.
[0353] In addition, an element that forms oxygen vacancies is added to the region 243 and heat treatment is performed to form a channel. The hydrogen contained in the region 234, which functions as a hole formation region, is transferred to the oxygen vacancy contained in the region 243. This gives the transistor 200 stable electrical characteristics and This can improve reliability.
[0354] After the dopant is added, an insulator 280 is formed as shown in FIG. Then, the CMP process is performed until the dummy gate is exposed, and the exposed dummy gate is then removed. As a result, the opening 245 shown in FIG. 7 can be formed.
[0355] The configurations, structures, methods, etc. described in this embodiment may be the same as those described in other embodiments. , and the like can be used in appropriate combination.
[0356] (Embodiment 2) In this embodiment mode, a semiconductor device functioning as a memory device, which is different from the above embodiment modes, is described. One embodiment will be described with reference to FIGS.
[0357] <Storage device 1> 18(A) and (B) show a cell 600 constituting a memory device. The cell 600 is a transistor. The capacitor 100 includes a capacitor 200a, a transistor 200b, a capacitor 100a, and a capacitor 100b. FIG. 18(A) is a top view of the cell 600. FIG. 18(B) is a top view of the cell 600. 18(A) is a cross-sectional view of a portion indicated by a dashed line A1-A2 in FIG. In the drawings, some elements are omitted for clarity of the drawings.
[0358] The cell 600 includes a transistor 200a and a transistor 200b. The capacitor 100a is overlapped on the transistor 200a, and the capacitor 100b is overlapped on the transistor 200b. The cell 600 has a transistor 200a and a capacitor element 100b. 00b, and the capacitive elements 100a and 100b may be arranged in line symmetry. Therefore, it is preferable that the transistors 200a and 200b have the same configuration. It is preferable that the capacitive element 100a and the capacitive element 100b have the same configuration.
[0359] An insulator 13 is disposed on the insulator 281 on the transistor 200a and the transistor 200b. 0 and has an insulator 150 on the insulator 130. Here, the insulator 150 is Any insulator that can be used for 281 may be used.
[0360] Furthermore, the conductor 160 is disposed on the insulator 150. Also, the insulator 280 and the insulator 27 4, embedded in the openings formed in the insulator 281, the insulator 130, and the insulator 150. The lower surface of the conductor 240 is in contact with the conductor 242b. The top surface of 240 contacts the conductor 160 .
[0361] The transistor 200a and the transistor 200b are the same as those shown in the above embodiment. Therefore, the transistor 200a and the transistor 200b can be used. The configuration of transistor 00b can be referred to in the description of transistor 200. In FIG. 18(A) and (B), the elements of the transistor 200a and the transistor 200b are The reference numerals are omitted. Note that the transistor 200a and the transistor The transistor 200b is merely an example, and is not limited to this structure. An appropriate transistor may be used.
[0362] Both transistor 200a and transistor 200b are made of oxide 230. One of the source and drain of the transistor 200a and the transistor 200 Either the source or the drain of the transistor b is in contact with the conductor 242b. One of the source and drain of the transistor 200a and the source and drain of the transistor 200b and one of the drains is electrically connected to the conductor 240 via the conductor 242b. This allows the contact portion of the transistor 200a and the transistor 200b to be shared. This allows the number of plugs and contact holes to be reduced. By sharing the wiring electrically connected to one of the drains, the occupied area of the memory cell array is reduced. can be further reduced.
[0363] [Capacitive element 100a and capacitive element 100b] As shown in FIGS. 18A and 18B, the capacitor 100a overlaps with the transistor 200a. Similarly, the capacitor 100b is provided in a region overlapping with the transistor 200b. The capacitor element 100b has a structure corresponding to that of the capacitor element 100a. The detailed structure of the capacitance element 100a will be described below. Unless otherwise specified, the description of the capacitance element 100b is given in accordance with the description of the capacitance element 100a. It is possible.
[0364] The capacitance element 100a includes a conductor 110, an insulator 130, and a conductor 120 on the insulator 130. Here, the conductor 110 and the conductor 120 are conductors 203, 205, and Alternatively, a conductor that can be used for the conductor 260 or the like may be used.
[0365] The capacitive element 100a includes an insulator 244, an insulator 280, an insulator 274, and an insulator 28. The lower electrode is formed in an opening of the semiconductor device 1. The conductor 110 functions as a dielectric, and the conductor 120 functions as a top electrode. The conductors 130 of the capacitance element 100a are opposed to each other with an insulator 130 interposed therebetween. 10 is formed in contact with the conductor 242a of the transistor 200a.
[0366] In particular, the depth of the openings in the insulators 280, 274, and 281 is increased. By doing so, the capacitance of the capacitance element 100a can be increased without changing the projection area. Therefore, the capacitance element 100a is cylindrical (the side area is larger than the bottom area). It is preferable to do so.
[0367] With the above configuration, the capacitance per unit area of the capacitance element 100a can be increased, This allows the miniaturization or high integration of semiconductor devices to be promoted. The capacitance value of the capacitance element 100a is appropriately set by adjusting the film thickness of the insulator 274 and the insulator 281. Therefore, a semiconductor device with high design freedom can be provided. .
[0368] It is preferable that the insulator 130 is made of an insulator having a large dielectric constant. For example, aluminum An insulator including oxides of minium and / or hafnium may be used. As an insulator containing oxides of either or both of aluminum and hafnium, aluminum oxide Hafnium, hafnium oxide, aluminum and oxides containing hafnium (hafnium aluminium) It is preferable to use a laminate.
[0369] The insulator 130 may also be a laminated structure, for example, silicon oxide, silicon oxynitride, etc. Silicon, silicon oxide nitride, silicon nitride, aluminum oxide, hafnium oxide, aluminum Two or more layers of oxides containing nium and hafnium (hafnium aluminate) For example, hafnium oxide, aluminum oxide, etc. can be layered by the ALD method. It is preferable to form a laminate structure by depositing hafnium oxide and hafnium oxide in that order. The thickness of the aluminum oxide and the aluminum film is 0.5 nm or more and 5 nm or less, respectively. By using such a laminated structure, a capacitance element 10 having a large capacitance value and a small leakage current can be obtained. It can be set to 0a.
[0370] The conductor 110 or the conductor 120 may have a laminated structure. The body 110, or the conductor 120, may be titanium, titanium nitride, tantalum, or tantalum nitride. Conductive materials based on tungsten, copper, or aluminum The conductor 110 or the conductor 120 may have a laminated structure with a single conductive material. It may have a layered structure or a laminated structure of three or more layers.
[0371] In addition, in the opening in which the capacitance element 100a is formed, the insulator 140 is disposed inside the conductor 120. Here, the insulator 140 can be used for the insulator 281. In addition, the upper surface of the insulator 140 is approximately flush with the upper surface of the conductor 120. However, the present invention is not limited to this. For example, the thickness of the conductor 120 may be increased. Alternatively, the opening may be filled with the insulator 15 while the opening is formed inside the conductor 120. Alternatively, a film of 0 may be formed to fill the opening.
[0372] [Cell array structure] Next, an example of a cell array in which the above cells are arranged in a row or row, This will be explained with reference to FIG. 19 to FIG.
[0373] FIG. 19 is a circuit diagram showing one embodiment in which the cells shown in FIG. 18 are arranged in a matrix. FIG. 20 shows the neighborhood of a cell 600 and a cell 601 adjacent to the cell 600 in the circuit diagram shown in FIG. 21 is a schematic diagram showing a cross-sectional structure of the wiring WL, wiring BL, 19 to 21 are schematic diagrams showing the layout of the wiring B and the oxide 230. The extension direction of L is the x direction, the extension direction of the wiring WL is the y direction, and the direction perpendicular to the xy plane is The z direction is taken as the direction. Note that Fig. 19 and Fig. 21 show an example in which 3 × 3 cells are arranged. However, the present embodiment is not limited to this, and the memory cells or arrays included in the cell array may be The number and arrangement of lines, etc. may be set as appropriate. For this reason, some elements shown in FIG. 19 are omitted.
[0374] As shown in FIG. 19, the transistors 200a and 200b constituting the cell One of the source and drain is electrically connected to the common wiring BL (BL01, BL02, BL03). The wiring BL is connected to the transistors of the cells 600 arranged in the x direction. The source and drain of the transistor 200a are electrically connected to the source and drain of the transistor 200b. On the other hand, the first gate of the transistor 200a and the The first gate of the capacitor 200b is electrically connected to the different wirings WL (WL01 to WL06). In addition, these wirings WL are connected to the transistors of the cells 600 arranged in the y direction. A first gate of the transistor 200a and a first gate of the transistor 200b are connected to each other. and electrically connected.
[0375] In addition, one electrode of the capacitor 100a and one electrode of the capacitor 100b in the cell 600 One of the electrodes is electrically connected to the wiring PL. For example, the wiring PL extends in the y direction. It is enough to achieve this.
[0376] In addition, the transistor 200a and the transistor 200b in each cell 600 have a first A second gate BG may be provided. A potential applied to the BG turns on the The threshold voltage can be controlled. The BG is connected to the transistor 400. The potential applied to G can be controlled by transistor 400 .
[0377] For example, as shown in FIG. 20, the conductor 160 is extended in the x direction to function as the wiring BL. The conductor 260 is extended in the y direction to function as the wiring WL, and the conductor 120 is The conductor 203 can be extended in the y direction to function as a wiring PL. It can also be extended to function as wiring connecting to the BG.
[0378] As shown in FIG. 20, one electrode of the capacitor element 100b of the cell 600 is The functional conductor 120 also serves as one electrode of the capacitor element 100a of the cell 601. In addition, although not shown, the capacitance element 100a of the cell 600 The conductor 120 that functions as one electrode of the cell 600 is connected to the capacitive element of the cell adjacent to the left of the cell 600. The cell to the right of cell 601 has a similar configuration. Therefore, a cell array can be configured. By configuring the cell array, The spacing between adjacent cells can be reduced, reducing the projection area of the cell array. This allows for high integration.
[0379] In addition, as shown in FIG. 21, the oxide 230 and the wiring WL are arranged in a matrix. In this way, a semiconductor device having a circuit diagram shown in FIG. 19 can be formed. It is preferable to provide the wiring WL and the oxide 230 in a different layer. In addition, by providing the capacitance element 100a and the capacitance element 100b in the lower layer, the oxide 230 It is possible to realize a layout in which the long side direction and the wiring BL are approximately parallel to each other. This simplifies the cell layout, improves design freedom, and reduces process costs. It is possible.
[0380] In addition, in FIG. 21, the long side of the oxide 230 is approximately perpendicular to the extension direction of the wiring WL. Although the oxide 230 and the wiring WL are provided, the present invention is not limited to this. For example, The long side of the oxide 230 is not perpendicular to the extension direction of the wiring WL, and the long side of the oxide 230 is not perpendicular to the extension direction of the wiring WL. The layout may be such that the long side of the oxide 230 is inclined with respect to the direction of the substrate. and the wiring WL form an angle of 20° or more and 70° or less, preferably 30° or more and 60° or less. In this way, the oxide 230 and the wiring WL are provided.
[0381] Moreover, the cell array may be configured not only in a plane but also in a stacked configuration. By stacking the cells, the cells can be integrated and arranged without increasing the area occupied by the cell array. In other words, a 3D cell array can be constructed.
[0382] As described above, according to one embodiment of the present invention, a semiconductor device that can be miniaturized or highly integrated is provided. According to one embodiment of the present invention, a semiconductor device having good electrical characteristics can be provided. According to one embodiment of the present invention, a semiconductor device having a small off-state current can be provided. According to one embodiment of the present invention, a semiconductor device having a large on-state current can be provided. According to one embodiment of the present invention, a highly reliable semiconductor device can be provided. According to one embodiment of the present invention, a semiconductor device with reduced power consumption can be provided. According to one embodiment of the present invention, a semiconductor device with high productivity can be provided. can be provided.
[0383] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.
[0384] (Embodiment 3) In this embodiment mode, a semiconductor device functioning as a memory device, which is different from the above embodiment modes, is described. One embodiment will be described with reference to FIGS.
[0385] <Storage device 2> The memory device shown in FIG. 22 includes a transistor 300, a transistor 200, and a capacitor. FIG. 22 shows the transistors 200 and 300. 23 is a cross-sectional view of the transistor 300 in the longitudinal direction of the panel. 1 shows a cross-sectional view in the channel width direction.
[0386] The transistor 200 is a transistor in which a channel is formed in a semiconductor layer having an oxide semiconductor. The transistor 200 is used in a memory device because its off-state current is small. This makes it possible to retain the memory contents for a long period of time. Since no refresh operation is required or the frequency of refresh operations is extremely low, Power consumption can be reduced sufficiently.
[0387] In the memory device shown in FIG. 22, the wiring 1001 is electrically connected to the source of the transistor 300. , and the wiring 1002 is electrically connected to the drain of the transistor 300. The wiring 1003 is electrically connected to one of the source and drain of the transistor 200. The wiring 1004 is electrically connected to the top gate of the transistor 200, and the wiring 100 06 is electrically connected to the bottom gate of the transistor 200. The gate of the transistor 300 and the other of the source and drain of the transistor 200 are connected to a capacitance The wiring 1005 is electrically connected to one of the electrodes of the capacitor element 100. The power supply is electrically connected to the power supply.
[0388] The memory device shown in FIG. 22 has a characteristic that the potential of the gate of the transistor 300 can be held. By having this, it is possible to write, hold, and read information, as described below.
[0389] The writing and holding of data will be described. First, the potential of the wiring 1004 is changed to This brings the transistor 200 into a conducting state. Thus, the potential of the wiring 1003 is applied to the gate of the transistor 300 and the potential of the capacitor 100. The output of the transistor 300 is applied to a node SN electrically connected to one of the poles of the transistor 300. A certain charge is applied to the gate (write). Here, two different potential levels Either the charge that gives the low level charge or the charge that gives the high level charge is given. After that, the potential of the wiring 1004 is changed so that the transistor 200 is in a non-conducting state. By setting the transistor 200 to a potential such that the transistor 200 is in a non-conducting state, a voltage is applied to the node SN. The load is held (retained).
[0390] When the off-state current of the transistor 200 is small, the charge of the node SN is retained for a long period of time. It will be held.
[0391] Next, the reading of information will be described. A predetermined potential (constant potential) was applied to the wiring 1001. In this state, when an appropriate potential (read potential) is applied to the wiring 1005, the wiring 1002 becomes The potential depends on the amount of charge held in the n-channel transistor SN. In the case of a transistor of the type, when a high level charge is applied to the gate of the transistor 300, The apparent threshold voltage V th_H A low-level charge is applied to the gate of transistor 300. The apparent threshold voltage V for a given th_L This is because the temperature is lower than the The apparent threshold voltage is the voltage required to turn on the transistor 300. Therefore, the potential of the wiring 1005 is V th_H and V th_L By setting the potential V0 between these two, the charge applied to the node SN can be determined. For example, In a write operation, if a high-level charge is applied to node SN, The potential of 005 is V0 (>V th_H ), transistor 300 is conductive. On the other hand, when a low-level charge is applied to the node SN, the potential of the wiring 1005 becomes V0( <V th_L ), transistor 300 remains non-conductive. Therefore, by determining the potential of the wiring 1002, the data stored in the node SN can be read out. It is possible.
[0392] When memory cells are arranged in an array, the information of a desired memory cell is read out. For example, if the memory cell array is a NOR type, By making the transistor 300 of the memory cell from which information is not to be read non-conductive, the desired memory cell In this case, the charge applied to node SN is Regardless of the potential, the transistor 300 is in a non-conducting state, i.e., V th_H Lower A potential may be applied to the wiring 1005 connected to the memory cell from which data is not read. For example, when the memory cell array is a NAND type, the memory cells that do not read information By turning on the transistor 300 of the desired memory cell, information of only the desired memory cell can be read. In this case, the transistor 300 can be turned on regardless of the charge applied to the node SN. The potential at which the transistor is conductive, i.e., V th_L A higher voltage is applied to the memory that does not read information. This may be provided to the wiring 1005 connected to the memory cell.
[0393] <Structure of memory device 2> As shown in FIG. 22, a memory device according to one embodiment of the present invention includes a transistor 300, a transistor The transistor 200 is disposed above the transistor 300. The capacitance element 100 is provided above the transistor 300 and the transistor 200. It is being done.
[0394] The transistor 300 is disposed on a substrate 311, and includes a conductor 316, an insulator 315, and a substrate 316. A semiconductor region 313 consisting of a part of 311 and functioning as a source region or a drain region. The semiconductor device has a low resistance region 314a that is capable of performing a low resistance change and a low resistance region 314b that is capable of performing a low resistance change.
[0395] As shown in FIG. 23, the transistor 300 includes an upper surface of a semiconductor region 313 and a channel The side surfaces in the width direction are covered with the conductor 316 via the insulator 315. By making the resistor 300 a fin type, the effective channel width is increased, The on-characteristics of the transistor 300 can be improved. Since the temperature can be increased, the off-state characteristics of the transistor 300 can be improved. .
[0396] Transistor 300 can be either p-channel or n-channel.
[0397] A region in which a channel of the semiconductor region 313 is formed, a region in the vicinity thereof, a source region, or In the low resistance region 314a which becomes the drain region, and the low resistance region 314b, etc., It is preferable that the semiconductor material contains a silicon-based semiconductor, and it is preferable that the semiconductor material contains single crystal silicon. Or Ge (germanium), SiGe (silicon germanium), GaAs (gallium arsenide) It may be made of materials such as gallium aluminum arsenide (GaAlAs) or Silicon with effective mass controlled by applying stress to the crystal lattice and changing the lattice spacing. Alternatively, GaAs and GaAlAs may be used to form a transistor. The Sta 300 is a HEMT (High Electron Mobility Transistor) stor) may also be used.
[0398] The low resistance region 314a and the low resistance region 314b are formed by applying a semiconductor In addition to the conductive material, elements that impart n-type conductivity, such as arsenic or phosphorus, or p-type conductivity, such as boron, are added. The material contains an element that imparts electrical conductivity to the mold.
[0399] The conductor 316 that functions as the gate electrode is made of arsenic, phosphorus, or the like that imparts n-type conductivity. An element, or a semiconductor material such as silicon that contains an element that gives it p-type conductivity, such as boron Conductive materials such as aluminum, metal, alloy, or metal oxide materials can be used. .
[0400] Since the work function is determined by the conductor material, the conductor material can be changed to The Vth of the transistor can be adjusted. It is preferable to use a material such as tantalum. It is preferable to use a metal material such as tungsten or aluminum as a laminate for the conductor. In particular, tungsten is preferably used from the viewpoint of heat resistance.
[0401] Note that the transistor 300 shown in FIG. 22 is just an example, and the present invention is not limited to this structure. Appropriate transistors may be used depending on the configuration and driving method.
[0402] Covering the transistor 300 are an insulator 320, an insulator 322, an insulator 324, and an insulator 326. The edge members 326 are stacked in order.
[0403] The insulators 320, 322, 324, and 326 may be, for example, an acid. silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, aluminum oxide, Aluminum oxynitride, aluminum nitride oxide, aluminum nitride, or the like may be used.
[0404] The insulator 322 serves to eliminate a step caused by the transistor 300 and the like provided below. For example, the upper surface of the insulator 322 may have a function as a planarizing film. In order to improve flatness, the surface is flattened by a planarization process using a chemical mechanical polishing (CMP) method or the like. It may be possible.
[0405] The insulator 324 is also provided with a substrate 311 or a transistor 300, etc. A film having a barrier property to prevent diffusion of hydrogen and impurities is formed in the area where the sta 200 is provided. It is preferable to use
[0406] An example of a film having a barrier property against hydrogen is silicon nitride formed by a CVD method. Here, a semiconductor having an oxide semiconductor such as the transistor 200 can be used. When hydrogen diffuses into a semiconductor element, the characteristics of the semiconductor element may deteriorate. Therefore, a film for suppressing hydrogen diffusion is provided between the transistor 200 and the transistor 300. Specifically, the film that suppresses hydrogen diffusion is one that reduces the amount of hydrogen desorption. The membrane is thin.
[0407] The amount of desorption of hydrogen can be analyzed, for example, by using thermal desorption spectroscopy (TDS). For example, the amount of hydrogen desorbed from the insulator 324 can be calculated by TDS analysis. In the range of 50°C to 500°C, the amount of desorption converted to hydrogen atoms is Converted to a hit, it's 10 x 10 15 atoms / cm 2 Less than or equal to 5×10 15 a toms / cm 2 The following is acceptable.
[0408] It is preferable that the insulator 326 has a lower dielectric constant than the insulator 324. For example, The dielectric constant of the insulator 326 is preferably less than 4, more preferably less than 3. The relative dielectric constant of the insulator 326 is preferably 0.7 times or less than the relative dielectric constant of the insulator 324, and more preferably 0.6 times or less. It is more preferable to use a material with a low dielectric constant as the interlayer film to reduce the parasitic capacitance between wirings. It can be reduced.
[0409] In addition, the insulators 320, 322, 324, and 326 are provided with capacitive elements. 100, or a conductor 328 electrically connected to the transistor 200, and a conductor 33 0 and the like are embedded. Note that the conductor 328 and the conductor 330 are plugs or wiring. The conductor having the function of a plug or wiring is a In this specification and the like, the wiring and the In addition, the wiring and the plug electrically connecting thereto may be integral with each other. In some cases, the conductor functions as a wiring, and in other cases, part of the conductor functions as a plug.
[0410] The materials of the plugs and wiring (the conductors 328 and 330, etc.) are metal. Conductive materials such as metals, alloys, metal nitrides, or metal oxides are applied in a single layer or in a Materials such as tungsten and molybdenum, which have both heat resistance and electrical conductivity, can be used. It is preferable to use any high melting point material, and it is preferable to use tungsten. It is preferable to form the conductive member from a low resistance material such as aluminum or copper. By using this material, the wiring resistance can be reduced.
[0411] A wiring layer may be provided on the insulator 326 and the conductor 330. For example, in FIG. In the insulating layer 350, an insulator 352, and an insulator 354 are stacked in this order. In addition, a conductor 356 is formed on the insulators 350, 352, and 354. The conductor 356 functions as a plug or wiring. 6 can be provided using the same material as the conductor 328 and the conductor 330.
[0412] For example, the insulator 350 has a barrier property against hydrogen, similar to the insulator 324. It is preferable to use an insulator having a barrier property against hydrogen as the conductor 356. In particular, the insulator 350 having a barrier property against hydrogen is useful. A conductor having a barrier property against hydrogen is formed in the opening. The transistor 300 and the transistor 200 can be separated by a barrier layer. This makes it possible to suppress the diffusion of hydrogen from the transistor 300 to the transistor 200 .
[0413] As a conductor having a barrier property against hydrogen, for example, tantalum nitride or the like is used. In addition, by laminating tantalum nitride and highly conductive tungsten, The diffusion of hydrogen from the transistor 300 can be suppressed while maintaining the overall conductivity. In this case, the tantalum nitride layer having a barrier property against hydrogen is It is preferable that the insulating body 350 has a structure in which the insulating body 350 is in contact with the insulating body 350.
[0414] A wiring layer may be provided on the insulator 354 and the conductor 356. For example, in FIG. In the above, an insulator 360, an insulator 362, and an insulator 364 are stacked in this order. In addition, a conductor 366 is formed on the insulators 360, 362, and 364. The conductor 366 functions as a plug or a wiring. 66 may be formed using the same material as the conductor 328 and the conductor 330 .
[0415] For example, the insulator 360 has a barrier property against hydrogen, similar to the insulator 324. It is preferable to use an insulator having a barrier property against hydrogen as the conductor 366. In particular, the insulator 360 having a barrier property against hydrogen is useful. A conductor having a barrier property against hydrogen is formed in the opening. The transistor 300 and the transistor 200 can be separated by a barrier layer. This makes it possible to suppress the diffusion of hydrogen from the transistor 300 to the transistor 200 .
[0416] A wiring layer may be provided on the insulator 364 and the conductor 366. For example, in FIG. In the insulating layer 370, an insulator 372, and an insulator 374 are stacked in this order. In addition, a conductor 376 is formed on the insulators 370, 372, and 374. The conductor 376 functions as a plug or wiring. 76 may be formed using materials similar to those of the conductors 328 and 330 .
[0417] For example, the insulator 370 has a barrier property against hydrogen, similar to the insulator 324. It is preferable to use an insulator having a barrier property against hydrogen as the conductor 376. In particular, the insulator 370 having a barrier property against hydrogen is useful. A conductor having a barrier property against hydrogen is formed in the opening. The transistor 300 and the transistor 200 can be separated by a barrier layer. This makes it possible to suppress the diffusion of hydrogen from the transistor 300 to the transistor 200 .
[0418] A wiring layer may be provided on the insulator 374 and the conductor 376. For example, in FIG. In the above, an insulator 380, an insulator 382, and an insulator 384 are stacked in this order. In addition, a conductor 386 is formed on the insulators 380, 382, and 384. The conductor 386 functions as a plug or a wiring. 6 can be provided using the same material as the conductor 328 and the conductor 330.
[0419] For example, the insulator 380 has a barrier property against hydrogen, similar to the insulator 324. It is preferable to use an insulator having a barrier property against hydrogen. In particular, the insulator 380 having a barrier property against hydrogen is useful. A conductor having a barrier property against hydrogen is formed in the opening. The transistor 300 and the transistor 200 can be separated by a barrier layer. This makes it possible to suppress the diffusion of hydrogen from the transistor 300 to the transistor 200 .
[0420] In the above, the wiring layer including the conductor 356, the wiring layer including the conductor 366, the conductor 376 The wiring layer including the conductor 386 has been described. The memory device is not limited to this. Alternatively, the number of wiring layers may be three or less, or the number of wiring layers similar to the wiring layer including the conductor 356 may be five or more. Good too.
[0421] On the insulator 384, the insulator 210, the insulator 212, the insulator 214, and the insulator 216 are are stacked in order. It is preferable that any of the insulators 216 is made of a material that has a barrier property against oxygen and hydrogen. It is nice.
[0422] For example, the insulator 210 and the insulator 214 may include, for example, a substrate 311 or a transistor. Hydrogen and impurities are introduced from the region where the resistor 300 is provided to the region where the transistor 200 is provided. It is preferable to use a film having a barrier property that prevents the diffusion of the insulator 3. The same materials as those in 24 can be used.
[0423] As an example of a film that has a barrier property against hydrogen, silicon nitride formed by CVD method is used. Here, a semiconductor element having an oxide semiconductor, such as the transistor 200, However, the diffusion of hydrogen may deteriorate the characteristics of the semiconductor element. A film that suppresses hydrogen diffusion is used between the transistor 200 and the transistor 300. Specifically, the film that suppresses hydrogen diffusion is a film that reduces the amount of hydrogen desorption. do.
[0424] In addition, as a film having a barrier property against hydrogen, for example, the insulator 210 and the insulator 214 uses metal oxides such as aluminum oxide, hafnium oxide, and tantalum oxide. It is preferable that
[0425] In particular, aluminum oxide is highly resistant to oxygen and water, which can cause fluctuations in the electrical characteristics of transistors. It has a high blocking effect that does not allow impurities such as oxygen and moisture to pass through the membrane. Aluminum oxide is highly resistant to hydrogen, moisture, etc. during and after the transistor manufacturing process. This can prevent impurities from being mixed into the transistor 200. This can suppress the release of oxygen from the oxide that constitutes the 00. It is suitable for use as a protective film for the capacitor 200.
[0426] For example, the insulators 212 and 216 may be made of the same material as the insulator 320. In addition, by using a material with a relatively low dielectric constant as the interlayer film, the For example, the insulators 212 and 216 may be formed of insulators 212 and 216. For example, a silicon oxide film or a silicon oxynitride film can be used.
[0427] In addition, the insulators 210, 212, 214, and 216 each include a conductor. 218, and the conductor (conductor 205) constituting the transistor 200 are embedded. Note that the conductor 218 is electrically connected to the capacitor 100 or the transistor 300. The conductor 218 functions as a plug or wiring for connecting the conductor 328 and the The conductive material 330 may be used for the conductive material 330 .
[0428] In particular, the insulator 210 and the conductor 218 in the area in contact with the insulator 214 are resistant to oxygen, hydrogen, It is preferable that the conductive material has a barrier property against water. The transistor 300 and the transistor 200 have a barrier property against oxygen, hydrogen, and water. The hydrogen from transistor 300 to transistor 200 can be separated by a layer having The diffusion of the substance can be suppressed.
[0429] The transistor 200 is provided above the insulator 216. The structure of 200 can be realized by using the transistors included in the semiconductor device described in the previous embodiment. In addition, the transistor 200 shown in FIG. 22 is only an example, and the present invention is not limited to this structure. Appropriate transistors may be used depending on the circuit configuration and driving method.
[0430] An insulator 281 is provided above the transistor 200 .
[0431] An insulator 282 is provided on the insulator 281. The insulator 282 is resistant to oxygen and hydrogen. It is preferable to use a material that has a barrier property against the insulator 282. The insulator 282 may be made of the same material as the insulator 214. For example, the insulator 282 may be made of aluminum oxide. It is preferable to use metal oxides such as tungsten oxide, hafnium oxide, and tantalum oxide.
[0432] In particular, aluminum oxide is highly resistant to oxygen and water, which can cause fluctuations in the electrical characteristics of transistors. It has a high blocking effect that does not allow impurities such as oxygen and moisture to pass through the membrane. Aluminum oxide is highly resistant to hydrogen, moisture, etc. during and after the transistor manufacturing process. This can prevent impurities from being mixed into the transistor 200. This can suppress the release of oxygen from the oxide that constitutes the 00. It is suitable for use as a protective film for the capacitor 200.
[0433] Further, an insulator 286 is provided on the insulator 282. The insulator 286 is The same material as that of 320 can be used. In addition, a material with a relatively low dielectric constant is used as the interlayer film. By using the insulator 286, the parasitic capacitance between the wirings can be reduced. For example, a silicon oxide film or a silicon oxynitride film can be used.
[0434] In addition, the insulator 220, the insulator 222, the insulator 224, the insulator 280, the insulator 274, the insulator The edge 281, the insulator 282, and the insulator 286 are connected to the conductor 246 and the conductor 24 8th magnitude is embedded.
[0435] The conductor 246 and the conductor 248 are the capacitor element 100, the transistor 200, or The conductive layer functions as a plug or wiring that is electrically connected to the transistor 300. Conductor 246 and conductor 248 are made of the same material as conductor 328 and conductor 330. It can be established as follows.
[0436] Next, the capacitor 100 is provided above the transistor 200. The element 100 includes a conductor 110, a conductor 120, and an insulator .
[0437] The conductor 112 may be provided over the conductor 246 and the conductor 248. 112 is electrically connected to the capacitor element 100, the transistor 200, or the transistor 300. The conductor 110 functions as a plug or wiring for connection. The conductor 112 and the conductor 110 are formed at the same time. It is possible.
[0438] The conductor 112 and the conductor 110 may be made of molybdenum, titanium, tantalum, tungsten, or the like. Metal film containing elements selected from the group consisting of tin, aluminum, copper, chromium, neodymium, and scandium. or a metal nitride film containing the above-mentioned elements (tantalum nitride film, titanium nitride film, nitride Molybdenum film, tungsten nitride film, etc. can be used. Indium oxide with tungsten oxide, indium oxide with tungsten oxide Lead oxide, indium oxide with titanium oxide, indium tin oxide with titanium oxide, Conductive materials such as indium zinc oxide and indium tin oxide doped with silicon oxide are used. It can also be used.
[0439] In FIG. 22, the conductor 112 and the conductor 110 are shown to have a single-layer structure. However, the present invention is not limited to this, and may be a laminated structure of two or more layers. For example, Conductors that have barrier properties between weak conductors and those with high electrical conductivity have good adhesion to conductors with high electrical conductivity. may form a highly conductive material.
[0440] The conductor 120 is provided so as to overlap with the conductor 110 with the insulator 130 interposed therebetween. The conductor 120 is made of a conductive material such as a metal material, an alloy material, or a metal oxide material. High-melting-point materials such as tungsten and molybdenum that are both heat-resistant and conductive are used. It is preferable to use tungsten, and it is particularly preferable to use tungsten. When forming the ferrite core simultaneously with other structures, low resistance metal materials such as Cu (copper) and Al (aluminum) are used. It is best to use a stencil, such as
[0441] An insulator 150 is provided on the conductor 120 and the insulator 130. The insulator 50 can be provided using the same material as the insulator 320. The insulator 150 can also be provided using the same material as the insulator 320. It may also function as a planarizing film that covers the uneven shape underneath.
[0442] By using this structure, a semiconductor device using a transistor having an oxide semiconductor This makes it possible to suppress the fluctuation of electrical characteristics and improve reliability. It is possible to provide a semiconductor device including an oxide semiconductor having a large on-state current. It is possible to provide a semiconductor device including an oxide semiconductor that consumes a small amount of current. Alternatively, a semiconductor device having an oxide semiconductor can be provided. In a semiconductor device using a transistor, miniaturization or high integration can be achieved.
[0443] The configurations, structures, methods, etc. described in this embodiment may be the same as those described in other embodiments. , and the like can be used in appropriate combination.
[0444] (Embodiment 4) In this embodiment, a semiconductor device using an oxide according to one embodiment of the present invention will be described with reference to FIGS. A transistor used in the semiconductor device (hereinafter referred to as an OS transistor) and a capacitor element are applied. As an example of a memory device that is widely used, NOSRAM (registered trademark) will be described. The mark stands for "Nonvolatile Oxide Semiconductor RAM " and refers to RAM that has gain cell type (2T type, 3T type) memory cells. In the following, a memory device using OS transistors such as NOSRAM will be referred to as O This is sometimes called S memory.
[0445] NOSRAM is a memory device that uses OS transistors in memory cells (hereinafter referred to as The OS memory is composed of at least a capacitive element and a capacitive element. This is a memory that has an OS transistor that controls the charging and discharging of the element. Since the transistor has a small off-state current, the OS memory has excellent retention characteristics and is nonvolatile. It can function as a harpoon.
[0446] < <nosram1600>> FIG. 24 shows an example of the configuration of the NOSRAM. The NOSRAM 1600 shown in FIG. Cell array 1610, controller 1640, row driver 1650, column driver 1660 , and an output driver 1670. Note that the NOSRAM 1600 has multiple memory cells. It is a multi-valued NOSRAM that stores multi-value data.
[0447] The memory cell array 1610 includes a plurality of memory cells 1611, a plurality of word lines WWL, The word line RWL, the bit line BL, and the source line SL are The word line RWL is the read word line. One memory cell 1611 stores 3-bit (8-value) data.
[0448] The controller 1640 controls the entire NOSRAM 1600 and outputs the data WDA Write data to [31:0] and read data RDA[31:0]. Controller 1 640 is an external command signal (e.g., a chip enable signal, a write enable signal, 1630, the row driver 1650, the column driver 1660, and the output driver 1670. 1670 control signals are generated.
[0449] The row driver 1650 has the function of selecting a row to be accessed. has a row decoder 1651 and a word line driver 1652 .
[0450] The column driver 1660 drives the source lines SL and bit lines BL. 60 includes a column decoder 1661, a write driver 1662, and a DAC (digital-to-analog The 1663 includes a conversion circuit.
[0451] The DAC1663 converts 3-bit digital data into an analog voltage. 3 converts the 32-bit data WDA[31:0] into an analog voltage every 3 bits. .
[0452] The write driver 1662 has a function of precharging the source line SL, A function for electrically floating a source line SL, a function for selecting a source line SL, A function to input the write voltage generated by the DAC1663, and to precharge the bit line BL. and putting the bit line BL into an electrically floating state.
[0453] The output driver 1670 includes a selector 1671, an ADC (analog-to-digital conversion circuit), 1672 and an output buffer 1673. The selector 1671 selects the source line SL and transmits the potential of the selected source line SL to the ADC1672. The source line SL 72 has a function of converting an analog voltage into 3-bit digital data. The potential is converted to 3-bit data by the ADC 1672 and output to the output buffer 1673. Holds the data output from the ADC1672.
[0454] In this embodiment, the row driver 1650, the column driver 1660, and the output driver The configuration of the driver 1670 is not limited to the above. Depending on the configuration or driving method, these drivers and the wiring connected to the drivers are The layout of the lines may be changed, and the layout of the drivers and the wiring connected to the drivers may be changed. The functions of the source line SL may be changed or added. For example, one of the functions of the source line SL may be changed or added. The portion may be provided on the bit line BL.
[0455] In the above, the amount of information stored in each memory cell 1611 is set to 3 bits. However, the configuration of the memory device shown in this embodiment is not limited to this. The amount of information to be transmitted may be 2 bits or less, or 4 bits or more. When the amount of information stored in the memory cell 1611 is set to 1 bit, the DAC1663 and AD A configuration without C1672 is also possible.
[0456] <Memory cells 1611 to 1614> FIG. 25A is a circuit diagram showing a configuration example of the memory cell 1611. is a 2T type gain cell, and the memory cell 1611 has a word line WWL, a word line RWL, The memory cell 161 is electrically connected to the bit line BL, the source line SL, and the wiring BGL. 1 denotes a node SN, an OS transistor MO61, a transistor MP61, and a capacitance element C61 The OS transistor MO61 is a write transistor. Reference numeral 61 denotes a read transistor, which is, for example, a p-channel Si transistor. The capacitance element C61 is a storage capacitance for holding the potential of the node SN. This corresponds to the gate of transistor MP61 in this example.
[0457] The write transistor of the memory cell 1611 is composed of the OS transistor MO61. Therefore, the NOSRAM 1600 can retain data for a long time.
[0458] In the example of FIG. 25(A), the bit line is a common bit line for writing and reading. As shown in FIG. 25B, a bit line WBL functions as a write bit line, and a read A bit line RBL may be provided to function as an output bit line.
[0459] 25C to 25E show other configuration examples of the memory cell. 25(E) shows an example in which a write bit line WBL and a read bit line RBL are provided. However, as shown in FIG. 25(A), a bit line is provided that is shared between writing and reading. This is also fine.
[0460] The memory cell 1612 shown in FIG. 25C is a modification of the memory cell 1611. The output transistor has been changed to an n-channel transistor (MN61). The transistor MN61 may be an OS transistor or a Si transistor. stomach.
[0461] In the memory cell 1611 and the memory cell 1612, the OS transistor MO61 is a bottom The transistor may be an OS transistor without a gate.
[0462] The memory cell 1613 shown in FIG. 25(D) is a 3T type gain cell, and is connected to the word line WWL , RWL, bit line WBL, bit line RBL, source line SL, wiring BGL, wiring PCL The memory cell 1613 is electrically connected to the node SN, the OS transistor MO6 2, a transistor MP62, a transistor MP63, and a capacitance element C62. Transistor MO62 is a write transistor. Transistor MP62 is a read transistor. transistor, and transistor MP63 is a selection transistor.
[0463] The memory cell 1614 shown in FIG. 25(E) is a modification of the memory cell 1613. The output transistor and the selection transistor are n-channel transistors (transistor M N62, transistor MN63). The transistor MN63 may be an OS transistor or a Si transistor. .
[0464] The OS transistors provided in the memory cells 1611 to 1614 are bottom The transistor may be a transistor without a gate or a transistor with a bottom gate. .
[0465] In the above, memory cells 1611 and the like are connected in parallel, so-called NOR type memory. Although the storage device has been described above, the storage device shown in the present embodiment is not limited to this. For example, a so-called NAND type memory cell 1615 shown below is connected in series. The memory device may be of the type.
[0466] 26 is a circuit diagram showing a configuration example of a NAND type memory cell array 1610. The memory cell array 1610 shown in FIG. The memory cell 1615 includes a word line WWL, a word line RWL, a wiring BGL, and a memory cell 1615. The memory cell 1615 includes a node SN, an OS transistor MO63, a transistor MN64, The transistor MN64 is, for example, an n-channel Si transistor. The transistor MN64 is not limited to this, and may be a p-channel Si The transistor may be a silicon-doped transistor or an OS transistor.
[0467] In the following, the memory cell 1615a and the memory cell 1615b shown in FIG. 26 are taken as examples. Here, a connection to either memory cell 1615a or memory cell 1615b is The symbols for the wiring or circuit elements are indicated by adding the letters a or b.
[0468] In the memory cell 1615a, the gate of the transistor MN64a and the OS transistor One of the source and drain of the capacitor MO63a and one of the electrodes of the capacitance element C63a are connected to a potential The bit line WBL and the source and The other of the drains is electrically connected to the word line WWLa. The gate of the transistor MO63a is electrically connected to the wiring BGLa. The bottom gate of the OS transistor MO63a is electrically connected to the The gate line RWLa and the other electrode of the capacitive element C63a are electrically connected to each other.
[0469] The memory cell 1615b is symmetrical about the contact portion with the bit line WBL. The memory cell 1615b can be provided symmetrically to the cell 1615a. The circuit elements are connected to wiring in the same manner as the memory cell 1615a.
[0470] Furthermore, the source of the transistor MN64a in the memory cell 1615a is The drain of the transistor MN64b in the memory cell 1615b is electrically connected to the drain of the transistor MN64b in the memory cell 1615b. The drain of the transistor MN64a in the 615a is electrically connected to the bit line RBL. The source of the transistor MN64b in the memory cell 1615b is connected to a plurality of memory The resistor 1615 is electrically connected to the source line SL via a transistor MN64. In this way, in the NAND type memory cell array 1610, the bit line RBL and the source A plurality of transistors MN64 are connected in series between the lines SL.
[0471] In the memory device having the memory cell array 1610 shown in FIG. or word line RWL) (hereinafter referred to as a memory cell column). For example, a write operation is performed as follows: The OS transistor is connected to the word line WWL connected to the memory cell column to be written. Apply a voltage to turn on the OS transistor of the memory cell row to be written. This causes the transistor M063 in the specified memory cell column to be turned on. The potential of the bit line WBL is applied to the gate of N64 and one of the electrodes of the capacitance element C63. A predetermined charge is applied to the gate. Then, the OS transistor M When O63 is turned off, the gate can hold a certain amount of charge. In this way, data can be written to the memory cells 1615 in the specified memory cell column. can be done.
[0472] Also, for example, a read operation can be performed as follows. A word line RWL that is not connected to a memory cell column is applied to the gate of transistor MN64. A potential is applied so that the transistor MN64 is turned on regardless of the charge stored in the memory cell. The transistors MN64 in the memory cell columns other than the one in which data is to be read are turned on. The gate of the transistor MN64 is connected to the word line RWL connected to the memory cell column to be read. The charge held by the transistor MN64 is used to select the on or off state of the transistor MN64. A constant potential is applied to the source line SL, and a constant potential is applied to the bit line RB The read circuit connected to the source line SL and the bit line R is in an operating state. The multiple transistors MN64 between the BLs are in the on state except for the memory cell column to be read. Therefore, the conductance between the source line SL and the bit line RBL is This is determined by the state (on or off) of transistor MN64 in the memory cell column. The charge on the gate of the transistor MN64 in the memory cell column to be read Therefore, the conductance of the transistors is different, so the voltage of the bit line RBL is changed accordingly. The potential of the bit line RBL is read by the read circuit. This makes it possible to read information from the memory cells 1615 in the specified memory cell column.
[0473] Data is written by charging and discharging the capacitance element C61, the capacitance element C62, or the capacitance element C63. Therefore, in principle, there is no restriction on the number of times that NOSRAM1600 can be rewritten, and Data can be written and read with only a small amount of energy. Since it is possible to maintain the data, the frequency of refreshing can be reduced.
[0474] The semiconductor device shown in the above embodiment is a memory cell 1611, a memory cell 1612, and a memory When used in the cell 1613, the memory cell 1614, and the memory cell 1615, an OS transistor Transistors MO61, MO62, and MO63 200, and the capacitance elements C61, C62, and C63 are the capacitance elements 100 Using the transistor MP61, the transistor MP62, the transistor MP63, Transistor MN61, transistor MN62, transistor MN63, transistor MN64 The transistor 300 can be used as the capacitor. Since the area occupied by each set in top view can be reduced, the present embodiment The memory device can be further highly integrated. The storage capacity per unit area can be increased.
[0475] The structure described in this embodiment may be used in appropriate combination with structures described in other embodiments. can be done.
[0476] (Embodiment 5) In this embodiment, an OS transaction according to one embodiment of the present invention will be described with reference to FIGS. 27 and 28. As an example of a memory device to which resistors and capacitive elements are applied, let us consider DOSRAM. DOSRAM (registered trademark) is a registered trademark of Dynamic Oxide Semiconductor Corporation. RAM is an abbreviation for 1T (transistor) 1C (capacitor) type memory. DOSRAM, like NOSRAM, is a RAM that is used by the OS memory. It is used.
[0477] < <dosram1400>> An example of the configuration of the DOSRAM is shown in FIG. 27. As shown in FIG. 27, the DOSRAM 1400 , controller 1405, row circuit 1410, column circuit 1415, memory cells and sense amplifiers The MC-SA array 1420 includes a filter array 1420 (hereinafter referred to as the "MC-SA array 1420").
[0478] The row circuit 1410 includes a decoder 1411, a word line driver circuit 1412, and a column selector 14 13, the sense amplifier driver circuit 1414. The column circuit 1415 is a global sense The global sense amplifier array 1416 includes an input / output circuit 1417. 416 has a plurality of global sense amplifiers 1447. The MC-SA array 1420 Memory cell array 1422, sense amplifier array 1423, global bit line GBLL , with GBLR.
[0479] (MC-SA Array 1420) The MC-SA array 1420 connects the memory cell array 1422 to the sense amplifier array 142 Global bit line GBLL, global bit line GB The LR is stacked on the memory cell array 1422. In the DOSRAM 1400, The bit line structure is a hierarchical bit line structure with local bit lines and global bit lines. The structure is adopted.
[0480] The memory cell array 1422 is a local memory cell array having N pieces (N is an integer of 2 or more). 1425 <0> to local memory cell array 1425 <n-1>FIG. 28(A ) shows a configuration example of the local memory cell array 1425. 25 includes a plurality of memory cells 1445, a plurality of word lines WL, a plurality of bit lines BLL, In the example of FIG. 28A, the local memory cell array 1425 The structure is of an open bit line type, but may also be of a folded bit line type.
[0481] FIG. 28B shows a pair of bit lines connected to a common bit line BLL (bit line BLR). 1 shows an example of a circuit configuration of the memory cell 1445a and the memory cell 1445b. 445a includes a transistor MW1a, a capacitance element CS1a, a terminal B1a, and a terminal B2a. The word line WLa is connected to the bit line BLL (bit line BLR). 445b has a transistor MW1b, a capacitance element CS1b, a terminal B1b, and a terminal B2b, The word line WLb is connected to the bit line BLL (bit line BLR). When there is no particular restriction on either the memory cell 1445a or the memory cell 1445b, In some cases, the memory cells 1445 and their associated structures may not be labeled with an a or b. do.
[0482] The transistor MW1a has the function of controlling the charging and discharging of the capacitance element CS1a. The transistor MW1b has the function of controlling the charging and discharging of the capacitance element CS1b. The gate is electrically connected to the word line WLa, and the first terminal is connected to the bit line BLL (bit line BL R), and the second terminal is electrically connected to the first terminal of the capacitive element CS1a. The gate of the transistor MW1b is electrically connected to the word line WLb. The terminal is electrically connected to the bit line BLL (bit line BLR), and the second terminal is a capacitance element CS 1b. In this manner, the bit line BLL (bit line BL R) is used in common for the first terminal of transistor MW1a and the first terminal of transistor MW1b. can be done.
[0483] The transistor MW1 has a function of controlling the charging and discharging of the capacitance element CS1. The second terminal of the resistor is electrically connected to terminal B2. Terminal B2 is connected to a constant potential (e.g., a low voltage The source potential) is input.
[0484] The semiconductor device described in the above embodiment is used for the memory cell 1445a and the memory cell 1445b. In this case, the transistor MW1a is the transistor 200a, and the transistor MW1b is the transistor MW1b. The transistor 200b is used as the capacitor CS1a, the capacitor 100a is used as the capacitor CS2a, and The capacitance element 100b can be used as the capacitance element CS1b. Since the area occupied by each set of the capacitor and the capacitance element when viewed from above can be reduced, Therefore, the memory device according to the present embodiment can be highly integrated. The storage capacity per unit area of the device can be increased.
[0485] Transistor MW1 has a bottom gate that is electrically connected to terminal B1. Therefore, the Vth of the transistor MW1 is changed by the potential of the terminal B1. For example, the potential of terminal B1 is a fixed potential (e.g., a constant negative potential). Alternatively, the potential of the terminal B1 may be changed depending on the operation of the DOSRAM 1400. .
[0486] The bottom gate of transistor MW1 is connected to the gate, source, or drain of transistor MW1. Alternatively, the transistor MW1 may be provided with a bottom gate. It's not necessary.
[0487] The sense amplifier array 1423 includes N local sense amplifier arrays 1426 <0> No To local sense amplifier array 1426 <n-1>A local sense amplifier array The switch array 1426 includes a switch array 1444 and a plurality of sense amplifiers 1446. The bit line pair is electrically connected to the sense amplifier 1446. has a function of precharging the bit line pair, a function of amplifying the potential difference of the bit line pair, and a function of amplifying this potential The switch array 1444 selects a pair of bit lines and holds the difference. It has a function of bringing the bit line pair and the global bit line pair into a conductive state.
[0488] Here, a bit line pair is a pair of two bit lines that are compared simultaneously by a sense amplifier. Global bit line pairs are compared simultaneously by a global sense amplifier. A bit line pair is a pair of global bit lines. The global bit line pair can be called a pair of global bit lines. In the bit line pair, the bit line BLL and the bit line BLR form a bit line pair. The BLL and the global bit line GBLR form a global bit line pair. They are also referred to as a global bit line pair (BLL, BLR) and a global bit line pair (GBLL, GBLR).
[0489] (Controller 1405) The controller 1405 has a function of controlling the overall operation of the DOSRAM 1400 . The controller 1405 performs logical operations on command signals input from the outside and determines the operation mode. The row circuit 1410 and the column circuit 1420 are provided to determine the operation mode. A function for generating the control signal of 415, a function for holding the address signal input from the outside, The EEPROM has a function of generating an external address signal.
[0490] (row circuit 1410) The row circuit 1410 has the function of driving the MC-SA array 1420. The word line driver circuit 1412 has a function of decoding the address signal. A selection signal is generated to select the word line WL of the row to be accessed.
[0491] The column selector 1413 and the sense amplifier driver circuit 1414 are connected to the sense amplifier array 142. The column selector 1413 is a circuit for driving the bit line of the column to be accessed. The column selector 1413 has a function of generating a selection signal for selecting The switch array 1444 of each local sense amplifier array 1426 is controlled. A plurality of local sense amplifier arrays 1 The 426 is independently driven.
[0492] (column circuit 1415) The column circuit 1415 has a function of controlling the input of the data signal WDA[31:0], The data signal WDA[31:0] has the function of controlling the output of RDA[31:0]. data signal RDA[31:0] is a write data signal, and data signal RDA[31:0] is a read data signal.
[0493] The global sense amplifier 1447 supplies power to the global bit line pair (GBLL, GBLR). The global sense amplifier 1447 is electrically connected to the global bit line pair (GB It has the function of amplifying the potential difference between the G-channel LL and the G-channel LR, and the function of maintaining this potential difference. Data can be written to and read from the global bit line pair (GBLL, GBLR) by input This is performed by the output circuit 1417.
[0494] The write operation of the DOSRAM 1400 will be briefly described. Then, data is written to the global bit line pair. The address signal is held by the global sense amplifier array 1416. The switch array 1444 of the Calsense amplifier array 1426 switches the global bit The data on the line pair is written to the bit line pair of the target column. 26 amplifies and holds the written data. In 1425, the word line WL of the target row is selected by the row circuit 1410, and the selected row The data held in the local sense amplifier array 1426 is written to the memory cell 1445 of the do.
[0495] The following is an overview of the read operation of the DOSRAM1400. A row of the local memory cell array 1425 is specified. In the row 1425, the word line WL of the target row is selected, and the de-energization of the memory cell 1445 is performed. The local sense amplifier array 1426 writes data to the bit lines. The potential difference between the bit line pair is detected as data and stored. The address signal is specified among the data held in the local sense amplifier array 1426. The data of the corresponding column is written to the global bit line pair. The global sense amplifier 1416 detects and holds the data of the global bit line pair. The data held in the amplifier array 1416 is output to the input / output circuit 1417. The operation is completed.
[0496] In order to rewrite data by charging and discharging the capacitance element CS1, the DOSRAM1400 has In principle, there is no limit to the number of times it can be rewritten, and data can be written and rewritten with low energy. In addition, since the circuit configuration of the memory cell 1445 is simple, it is possible to read out a large capacity It is easy to
[0497] The transistor MW1 is an OS transistor. Since it is small, it is possible to suppress leakage of electric charge from the capacitance element CS1. Therefore, the retention time of DOSRAM1400 is much longer than that of DRAM. Since the frequency of refresh operations can be reduced, the power required for the refresh operations can be reduced. DOSRAM1400 is a memory device that frequently rewrites large amounts of data, such as image It is suitable for use as a frame memory for processing.
[0498] The MC-SA array 1420 has a stacked structure, so that the local sense amplifier array The bit line can be shortened to a length similar to that of the bit line 1426. This reduces the bit line capacitance, and the storage capacitance of the memory cell 1445 can be reduced. In addition, the local sense amplifier array 1426 is provided with a switch array 1444. This reduces the number of long bit lines. The load to be driven when accessing 00 is reduced, and power consumption can be reduced.
[0499] The structure described in this embodiment may be used in appropriate combination with structures described in other embodiments. can be done.
[0500] (Embodiment 6) In this embodiment mode, a semiconductor device according to the above embodiment mode is applied to the semiconductor device shown in FIG. Explain the I system.
[0501] FIG. 29 is a block diagram showing a configuration example of the AI system 4041. The device 41 includes a calculation unit 4010 , a control unit 4020 , and an input / output unit 4030 .
[0502] The arithmetic unit 4010 includes an analog arithmetic circuit 4011, a DOSRAM 4012, and a NOSR. AM4013 and FPGA (Field Programmable Gate Array) 4014 are included. The DOSRAM 4012 and the NOSRAM 4013 are the same as those shown in the above embodiment. , DOSRAM1400, and NOSRAM1600 can be used. Also, FPGA The 4014 uses configuration memory and OS memory in the registers. Here, we call this type of FPGA "OS-FPGA."
[0503] The control unit 4020 includes a CPU (Central Processing Unit) 40 21, GPU (Graphics Processing Unit) 4022, P LL (Phase Locked Loop) 4023 and SRAM (Static R andom Access Memory) 4024 and PROM (Programma ble Read Only Memory) 4025 and memory controller 4026 , a power supply circuit 4027, and a PMU (Power Management Unit) 40 28 and,
[0504] The input / output unit 4030 includes an external memory control circuit 4031, an audio codec 4032, and a video A codec 4033, a general-purpose input / output module 4034, and a communication module 4035, has.
[0505] The calculation unit 4010 can perform learning or inference using a neural network. Cut.
[0506] The analog arithmetic circuit 4011 is an A / D (analog / digital) conversion circuit, a D / A (digital The device has a digital / analog conversion circuit and a multiply-and-accumulate circuit.
[0507] The analog arithmetic circuit 4011 is preferably formed using an OS transistor. The analog arithmetic circuit 4011 using transistors has an analog memory and performs learning or It becomes possible to execute the multiply-and-accumulate operations required for inference with low power consumption.
[0508] The DOSRAM4012 is a DRAM formed using OS transistors. The SRAM 4012 temporarily stores digital data sent from the CPU 4021. The DOSRAM4012 is a memory that uses memory cells that include OS transistors and Si The memory cell and the read circuit section include a stacked transistor. Since the DOSRAM4012 can be implemented on different layers, the total circuit area can be reduced by It can be made smaller.
[0509] Calculations using neural networks can involve more than 1,000 pieces of input data. When storing the above input data in SRAM, the circuit area of SRAM is limited, and the memory capacity Since the RAM size is small, the input data must be divided into smaller chunks and stored. 2 enables memory cells to be highly integrated even in a limited circuit area, and SRA The memory capacity is larger than that of the M. Therefore, the DOSRAM4012 can efficiently read the above input data. It can be stored efficiently.
[0510] NOSRAM4013 is a non-volatile memory that uses OS transistors. The M4013 is a high-performance memory that can store data in a wide range of formats, including flash memory and ReRAM (Resistive Random Access Memory). Access Memory), MRAM (Magnetoresistive Ran Compared to other non-volatile memory such as DDR3, it is much faster to write data. It consumes little power when writing data. Also, unlike flash memory and ReRAM, The elements do not deteriorate when data is written, and there is no limit to the number of times data can be written.
[0511] In addition to 1-bit binary data, the NOSRAM4013 can also handle multi-value data of 2 or more bits. The NOSRAM4013 can store multi-value data. The memory cell area per bit can be reduced.
[0512] In addition to digital data, the NOSRAM4013 can also store analog data. Therefore, the analog arithmetic circuit 4011 converts the NOSRAM 4013 into an analog memory. The NOSRAM4013 can also be used as a memory. Therefore, no D / A or A / D conversion circuits are required. The RAM 4013 can reduce the area of the peripheral circuits. Analog data refers to data with a resolution of 3 bits (8 values) or more. Multi-valued data may also be included in the analog data.
[0513] The data and parameters used in the neural network calculations are stored in NOSRA. The above data and parameters can be stored in the M4013 via the CPU4021. The data may be stored in a memory provided outside the AI system 4041, but may also be stored in a memory provided inside the AI system 4041. The NOSRAM4013, which is equipped with the DDR32864, can store the above data and parameters at higher speeds and with lower power consumption. The NOSRAM4013 can store more data than the DOSRAM4012. Since the bit lines can be made longer, the memory capacity can be increased.
[0514] The FPGA 4014 is an FPGA that uses OS transistors. 1 uses FPGA4014 to realize the deep neural network simulation described later. Neural Networks (DNN), Convolutional Neural Networks (CNN), Recurrent Neural Networks (RNN) Neural Networks (RNN), Autoencoders, Deep Boltzmann Machines (DBM), Deep It is possible to configure the connections of neural networks, such as layered belief networks (DBNs). By configuring the above neural network connections in hardware, It can be executed quickly.
[0515] The FPGA 4014 is an FPGA having OS transistors. The memory area can be made smaller than that of an FPGA that is composed of SRAM. Even if the context switching function is added, the area increase is small. Staging allows data and parameters to be transmitted at high speed.
[0516] The AI system 4041 is composed of an analog arithmetic circuit 4011, a DOSRAM 4012, and a NOS The RAM4013 and FPGA4014 can be mounted on a single die (chip). Therefore, the AI system 4041 is designed to be fast and low power consumption, and to use neural networks. In addition, the analog arithmetic circuit 4011 and the DOSRAM4 012, NOSRAM4013, and FPGA4014 are manufactured using the same manufacturing process. Therefore, the AI system 4041 can be manufactured at low cost. .
[0517] The calculation unit 4010 includes a DOSRAM 4012, a NOSRAM 4013, and an FP It is not necessary to have all of GA4014. Depending on the problem that AI system 4041 wants to solve, DOSRAM4012, NOSRAM4013, and FPGA4014 A plurality of the electrodes may be selected and provided.
[0518] AI System 4041 uses deep neural networks to solve different problems. (DNN), Convolutional Neural Network (CNN), Recurrent Neural Network Recurrent neural networks (RNNs), autoencoders, deep Boltzmann machines (DBMs), and deep belief networks The PROM4025 can implement techniques such as dynamic random negation (DBN). A program for executing at least one program can be stored. Some or all of the program may be stored in NOSRAM 4013.
[0519] Existing programs available as libraries are based on the assumption that GPU processing will be used. Therefore, it is preferable that the AI system 4041 includes a GPU 4022. The system 4041 performs the multiply-and-accumulate operation, which is the rate-limiting operation among the multiply-and-accumulate operations used in learning and inference. The multiplication and accumulation operations can be executed by the calculation unit 4010, and other multiplication and accumulation operations can be executed by the GPU 4022. This allows for faster learning and inference.
[0520] The power supply circuit 4027 not only generates a low power supply potential for the logic circuits, but also The power supply circuit 4027 may also use an OS memory. 27 can reduce power consumption by storing the reference potential in the OS memory.
[0521] The PMU 4028 has the function of temporarily turning off the power supply to the AI System 4041. do.
[0522] The CPU 4021 and the GPU 4022 preferably have OS memory as a register. The CPU 4021 and the GPU 4022 have an OS memory, so that the power supply is Even when the power is turned off, data (logical values) can still be stored in the OS memory. As a result, the AI system 4041 can save power.
[0523] The PLL 4023 has a function of generating a clock. The clock generated by the PLL4023 is used as a reference. The PLL4023 has an OS memory. It is preferable that the PLL4023 has an OS memory, so that the clock oscillation period can be It is possible to hold a controlling analog potential.
[0524] The AI system 4041 may store data in an external memory such as a DRAM. Therefore, the AI System 4041 uses memory that acts as an interface with external DRAM. It is preferable that the memory controller 4026 is included. It is preferable to place the GPU 4021 or the GPU 4022 close to the CPU 4021. This allows for high-speed data exchange.
[0525] A part or all of the circuits shown in the control unit 4020 are formed on the same die as the operation unit 4010. By doing so, the AI system 4041 can achieve high speed and low power consumption. Neural network calculations can be performed.
[0526] The data used in the neural network calculations is stored in an external storage device (HDD). Disk Drive, SSD (Solid State Drive, etc.) Therefore, the AI system 4041 does not have an interface with an external storage device. It is preferable that the memory controller 4031 functions as an interface.
[0527] Learning and inference using neural networks often involves the use of audio and video. The I system 4041 has an audio codec 4032 and a video codec 4033 . The audio codec 4032 encodes and decodes audio data. The video codec 4033 encodes and decodes the video data.
[0528] The AI system 4041 performs learning or inference using data obtained from external sensors. Therefore, the AI system 4041 has a general-purpose input / output module 4034. The general-purpose input / output module 4034 is, for example, a USB (Universal Ser I2C (Inter-Integrated Circuit), etc. Includes.
[0529] The AI system 4041 can learn or make inferences using data obtained via the Internet. Therefore, the AI system 4041 preferably has a communication module 403 5.
[0530] The analog arithmetic circuit 4011 may use a multi-value flash memory as an analog memory. However, the flash memory has a limited number of rewritable times. Also, it is very difficult to form a multi-value flash memory embedded (formed on the same die as the arithmetic circuit and the memory). ).
[0531] Also, the analog arithmetic circuit 4011 may use ReRAM as an analog memory . However, ReRAM has a limited number of rewritable times and also has problems in terms of storage accuracy. Furthermore, since it is a two-terminal element, the circuit design for separating data writing and reading becomes complicated.
[0532] Also, the analog arithmetic circuit 4011 may use MRAM as an analog memory. However, MRAM has a low resistance change rate and has problems in terms of storage accuracy.
[0533] In view of the above, it is preferable for the analog arithmetic circuit 4011 to use an OS memory as an analog memory .
[0534] The configuration shown in this embodiment can be used in appropriate combination with the configuration shown in other embodiments .
[0535] (Embodiment 7) <Application Examples of AI System> In this embodiment, regarding the application examples of the AI system shown in the above embodiment, FIG. 30 is used The explanation will be given below.
[0536] FIG. 30(A) shows the AI system 4041 described in FIG. 29 arranged in parallel and connected via a bus line. This is AI system 4041A, which enables signals to be sent and received between systems.
[0537] The AI system 4041A shown in FIG. 30(A) includes a plurality of AI systems 4041_1 The AI systems 4041_1 to 4041_n (n is a natural number) are included. The AI systems 4041_n are connected to each other via a bus line 4098.
[0538] FIG. 30(B) shows the AI system 4041 described in FIG. 29 in the same manner as in FIG. 30(A). This AI system is placed in parallel and enables signals to be sent and received between systems via a network. System 4041B.
[0539] The AI system 4041B shown in FIG. 30B includes a plurality of AI systems 4041_1 The AI systems 4041_1 to 4041_n are 041_n are connected to each other via a network 4099.
[0540] The network 4099 includes the AI systems 4041_1 to 4041_n. Each of them may be provided with a communication module, and configured to perform wireless or wired communication. The communication module can communicate via an antenna. For example, World Wi The Internet, intranets, and extranets that form the foundation of the World Wide Web (WWW) PAN (Personal Area Network), LAN (Local A rea Network), CAN (Campus Area Network), MA N (Metropolitan Area Network), WAN (Wide Ar ea Network), GAN (Global Area Network), etc. It is possible to connect each electronic device to a computer network and perform communication. In this case, LTE (Long Term Evolution) is used as a communication protocol or technology. ), GSM (Global System for Mobile Comm) unication: registered trademark), EDGE (Enhanced Data Rates for GSM Evolution), CDMA2000 (Code Divisi on Multiple Access 2000), W-CDMA (registered trademark), etc. Communication standard: Wi-Fi (registered trademark), Bluetooth (registered trademark), ZigB Specifications standardized by IEEE such as ee (registered trademark) can be used.
[0541] By using the configurations shown in Fig. 30(A) and Fig. 30(B), the analytic signal obtained by an external sensor, etc. Log signals can be processed by separate AI systems, e.g., biometrics, brain The information such as brainwave, pulse, blood pressure, and body temperature is transmitted to the brainwave sensor, pulse wave sensor, blood pressure sensor, and temperature sensor. The analog signals can be acquired by various sensors such as sensors and processed by separate AI systems. By processing signals or learning in separate AI systems, a single AI The amount of information processed per system can be reduced. Therefore, signals can be processed with fewer calculations. As a result, the recognition accuracy can be improved. The AI system can instantly and comprehensively grasp complex changes in biological information from the information obtained. It is expected that you will be able to grasp it.
[0542] The structure described in this embodiment may be used in appropriate combination with structures described in other embodiments. can be done.
[0543] (Embodiment 8) In this embodiment, an example of an IC in which the AI system shown in the above embodiment is incorporated is shown. vinegar.
[0544] The AI system shown in the above embodiment is a digital processor including a CPU and other Si transistors. Analog arithmetic circuits using OS transistors, OS-FPGA and DOSR OS memory such as AM and NOSRAM can be integrated onto a single die.
[0545] Figure 31 shows an example of an IC incorporating an AI system. C7000 has leads 7001 and a circuit portion 7003. AI system IC700 0 is mounted on, for example, a printed circuit board 7002. These are then electrically connected to the printed circuit board 7002, whereby electronic components are mounted. The circuit portion 7003 has the same structure as that shown in the above embodiment mode. The various circuits described above are provided on one die. As shown in FIG. 1, the semiconductor device has a laminated structure including a Si transistor layer 7031, a wiring layer 7032, an OS transistor layer 7033, and a The OS transistor layer 7033 is divided into a Si transistor layer 703 1, it is easy to miniaturize the AI system IC7000. .
[0546] In Figure 31, the AI system IC7000 is packaged in a QFP (Quad Flat Package). However, the form of the package is not limited to this.
[0547] Digital processing circuits such as CPUs and analog arithmetic circuits using OS transistors, FPGAs and OS memories such as DOSRAM and NOSRAM are all made of Si transistors. A layer 7031, a wiring layer 7032, and an OS transistor layer 7033 can be formed. In other words, the elements constituting the AI system can be formed in the same manufacturing process. Therefore, the IC shown in this embodiment can be manufactured in a simple manner even if the number of constituent elements increases. This eliminates the need for additional memory, and the AI system can be incorporated at low cost.
[0548] The structure described in this embodiment may be used in appropriate combination with structures described in other embodiments. can be done.
[0549] (Embodiment 9) <Electronic equipment> The semiconductor device according to one embodiment of the present invention can be used in various electronic devices. 34A to 34C illustrate specific examples of electronic devices using a semiconductor device according to one embodiment of the present invention.
[0550] The robot 2100 shown in FIG. 32(A) includes a computing device 2110, an illuminance sensor 2101, Microphone 2102, upper camera 2103, speaker 2104, display 2105 , a lower camera 2106 , an obstacle sensor 2107 , and a movement mechanism 2108 .
[0551] The microphone 2102 has a function of detecting the user's voice and environmental sounds. The speaker 2104 has a function of emitting sound. The device communicates with the user using the phone 2102 and the speaker 2104. is possible.
[0552] The display 2105 has a function of displaying various information. The user's desired information can be displayed on the display 2105. The device 2105 may be equipped with a touch panel.
[0553] The upper camera 2103 and the lower camera 2106 capture images of the surroundings of the robot 2100. The obstacle sensor 2107 also detects the obstacles of the robot 21 using the moving mechanism 2108. Robot 2 can detect the presence or absence of obstacles in its path as it moves forward. 100 uses an upper camera 2103, a lower camera 2106, and an obstacle sensor 2107. It is possible for the robot to recognize the surrounding environment and move around safely.
[0554] The flying object 2120 shown in FIG. 32(B) includes a computing device 2121, a propeller 2123, and a camera. It has a drone 2122 and has the ability to fly autonomously.
[0555] In the flying object 2120, the above electronic components are used in the computing device 2121 and the camera 2122. There can be.
[0556] FIG. 32(C) is an external view showing an example of an automobile. The automobile 2980 is equipped with a camera 298. 1st place. In addition, the car 2980 is equipped with infrared radar, millimeter wave radar, laser radar, The car 2980 is equipped with various sensors such as a camera 2981. The system can analyze the surrounding traffic conditions, such as the presence or absence of pedestrians, and perform autonomous driving.
[0557] Figure 32(D) shows a case where multiple people who speak different languages communicate with each other. 2 shows a situation in which the portable electronic device 2130 is used for simultaneous interpretation.
[0558] The portable electronic device 2130 has a microphone and a speaker, and receives the user's voice. It has the ability to recognize and translate into the language spoken by the person you are speaking to.
[0559] In FIG. 32(D), the user has a portable microphone 2131. The microphone 2131 has a wireless communication function and transmits the detected sound to the portable electronic device 213. It has the ability to send to 0.
[0560] FIG. 33(A) is a schematic cross-sectional view showing an example of a pacemaker.
[0561] The pacemaker main body 5300 includes batteries 5301a and 5301b, a regulator, and , a control circuit, an antenna 5304, a wire 5302 to the right atrium, a wire 5303 to the right ventricle 03 and at least
[0562] The pacemaker body 5300 is placed in the body by surgery, and the two wires are connected to the clavicle of the human body. The wire is passed through the inferior vena cava 5305 and the superior vena cava 5306, and one end of the wire is inserted into the right ventricle and the other end into the right ventricle. The tip of the wire is placed in the right atrium.
[0563] In addition, the antenna 5304 can receive power, and the power is fed to multiple batteries 5301a, The 5301b is charged, and the frequency of pacemaker replacement can be reduced. The 5300 camera body has multiple batteries, making it highly safe and allowing it to continue functioning even if one of them fails. Since the other power source can still function even if one power source is turned off, it can also function as an auxiliary power source.
[0564] In addition to the antenna 5304 that can receive power, an antenna that can transmit physiological signals is provided. For example, physiological signals such as pulse, respiration rate, heart rate, and temperature may be monitored externally. A system may be configured to monitor cardiac activity as seen by the device.
[0565] The sensor 5900 shown in FIG. 33(B) is attached to the human body using an adhesive pad or the like. The sensor 5900 transmits a signal to electrodes 5931 attached to the human body via wiring 5932. The sensor receives the pulse rate, electrocardiogram, and other vital signs, and the acquired information is read as a wireless signal. The signal is transmitted to a terminal such as a reading device.
[0566] FIG. 34 is a schematic diagram showing an example of a cleaning robot.
[0567] The cleaning robot 5100 has a display 5101 arranged on the top surface and a It has a plurality of cameras 5102, a brush 5103, and an operation button 5104. Although not shown, the underside of the cleaning robot 5100 is provided with tires, a suction port, etc. The cleaning robot 5100 also has infrared sensors, ultrasonic sensors, acceleration sensors, and piezo sensors. It is equipped with various sensors such as sensors, light sensors, and gyro sensors. The 5100 is equipped with wireless communication means.
[0568] The cleaning robot 5100 moves by itself, detects dirt 5120, and sucks it out from a suction port provided on the bottom. It can suck up dirt from
[0569] In addition, the cleaning robot 5100 analyzes the images captured by the camera 5102 and detects walls, furniture, or The system can detect obstacles such as steps. Image analysis can also be used to detect wiring and other obstacles. If an object that may become entangled in the brush 5103 is detected, the rotation of the brush 5103 is stopped. can be done.
[0570] The display 5101 can display the remaining battery level, the amount of dirt sucked up, etc. The route traveled by the cleaning robot 5100 can be displayed on the display 5101. Also, the display 5101 may be a touch panel, and the operation buttons 5104 may be a display. It may be provided in the play 5101.
[0571] The cleaning robot 5100 can communicate with a portable electronic device 5140 such as a smartphone. The image captured by the camera 5102 can be displayed on the portable electronic device 5140. Therefore, the owner of the Cleaning Robot 5100 can check the state of the room even when he / she is away from home. In addition, the display on the display 5101 can be displayed on a portable electronic device such as a smartphone. You can also check it with a device.
[0572] For example, a memory device using the semiconductor device of one embodiment of the present invention can be used for the control information of the above-mentioned electronic devices. The semiconductor device according to one aspect of the present invention can store information, control programs, and the like for a long period of time. By using the device, highly reliable electronic equipment can be realized.
[0573] In addition, for example, the AI system shown in the above embodiment may be incorporated in the arithmetic device of the electronic device. In this embodiment, an IC in which the electronic device shown in FIG. The AI system enables the device to take appropriate action according to the situation while consuming little power. do.
[0574] This embodiment may be implemented in appropriate combination with the configurations described in other embodiments. is possible. [Explanation of symbols]
[0575] 200: transistor, 200a: transistor, 200b: transistor, 203: conductor conductor, 203a: conductor, 203b: conductor, 205: conductor, 205a: conductor, 20 5b: conductor, 210: insulator, 212: insulator, 214: insulator, 216: insulator, 2 18: conductor, 220: insulator, 222: insulator, 224: insulator, 230: oxide, 2 30a: Oxide, 230A: Oxide film, 230b: Oxide, 230B: Oxide film, 230c: Oxide, 230C: Oxide film, 231: Region, 231a: Region, 231b: Region, 232: Area, 232a: Area, 232b: Area, 234: Area, 239: Area, 240: Conductor , 240a: conductor, 240b: conductor, 242: conductor, 242a: conductor, 242A :Conductive film, 242b: Conductor, 242B: Conductor, 243: Region, 243a: Region, 24 3b: area, 244: insulator, 244A: insulator, 245: opening, 246: conductor, 24 8: conductor, 250: insulator, 250a: insulator, 250A: insulator, 250b: insulator , 250B: insulator, 250C: insulator, 252: insulator, 260: conductor, 260a: Conductor, 260A: Conductive film, 260b: Conductor, 260B: Conductive film, 274: Insulator, 2 80: insulator, 281: insulator, 282: insulator, 286: insulator,
Claims
1. a first insulator having an opening; a first conductor having a region disposed within the opening and functioning as a gate electrode; a second insulator having an area disposed within the opening and contacting a bottom surface and a side surface of the first conductor; an oxide semiconductor having a region overlapping with the first conductor; a second conductor having a region in contact with the oxide semiconductor, the oxide semiconductor includes indium oxide; the oxide semiconductor has a region facing a bottom surface of the first conductor via a first region of the second insulator; the second conductor has a region corresponding to a side surface of the first conductor via a second region of the second insulator; the first insulator has a region facing a side surface of the first conductor via a third region of the second insulator; A semiconductor device, wherein the second region and the third region are thicker than the first region.
2. In claim 1, A third conductor is provided. the third conductor has a region facing a bottom surface of the first conductor via the first region.
Citation Information
Patent Citations
Mis-type fet and manufacturing method of semiconductor device
JP2001345442A
Semiconductor device and manufacturing method thereof
JP2002094058A
Semiconductor device, module, and electronic apparatus
JP2017034051A
Semiconductor device, semiconductor device manufacturing method, module and electronic apparatus
JP2017034246A
Method for forming capacitive element, semiconductor device, module, and electronic device
JP2017085106A