Polarizing plate, polarizing plate with retardation layer, and image display device

By controlling iodine adsorption and adhesive layer thickness in polarizing plates, the decrease in polarization is suppressed, maintaining optical properties in high-temperature, high-humidity environments, suitable for thinner polarizing plates and retardation layers.

JP2024163298APending Publication Date: 2024-11-21NITTO DENKO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024158350
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Thin polarizing plates and polarizing plates with retardation layers experience a significant decrease in the degree of polarization in high-temperature, high-humidity environments.

Method used

The polarizing plate is designed with specific constraints on the iodine adsorption amounts in the adhesive layers and thicknesses, ensuring that the sum of iodine adsorption per unit area in the first and second adhesive layers is less than 0.300 mg/cm², and the adhesive layers are 0.3 μm or less, combined with a polarizer thickness of 10 μm or less and a retardation layer with controlled optical properties.

Benefits of technology

This configuration maintains high polarization in high-temperature, high-humidity conditions, preventing iodine migration and ensuring optical properties are preserved, allowing for thinner polarizing plates with reduced display unevenness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163298000001_ABST
    Figure 2024163298000001_ABST
Patent Text Reader

Abstract

To provide a polarizing plate and polarizing plate with a retardation layer, which are thin and exhibit little reduction in the polarization degree in high-temperature high-humidity environments.SOLUTION: A polarizing plate of the present invention comprises a polarizer, a protective layer adhered to a viewing side of the polarizer via a first adhesive layer, and a second adhesive layer provided on a side of the polarizer opposite the first adhesive layer. An iodine adsorption A1 of the first adhesive layer per unit area and an iodine adsorption A2 of the second adhesive layer per unit area satisfy the following expression (1): (A1+A2)<0.300(mg / cm2) ...(1). A polarizing plate with a retardation layer of the present invention comprises the above polarizing plate, and a retardation layer with a circularly or elliptically polarizing function adhered to the polarizing plate via the second adhesive layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate, a polarizing plate with a retardation layer, and an image display device. [Background technology]

[0002] In recent years, image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices, inorganic EL display devices), have rapidly become widespread. A polarizing plate and a retardation plate are typically used in image display devices. In practice, a retardation layer-attached polarizing plate in which a polarizing plate, a retardation plate, and an adhesive layer are integrated is widely used (e.g., Patent Document 1). Recently, as the demand for thinner image display devices has increased, the demand for thinner polarizing plates and retardation layer-attached polarizing plates has also increased. However, a thin polarizing plate has a problem that the degree of polarization is significantly reduced in a high-temperature and high-humidity environment. Furthermore, a similar problem may occur in a thin retardation layer-attached polarizing plate using such a polarizing plate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 3325560 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and its main object is to provide a polarizing plate and a polarizing plate with a retardation layer that are thin and suppress the decrease in polarization degree in a high-temperature and high-humidity environment. [Means for solving the problem]

[0005] A polarizing plate according to an embodiment of the present invention includes a polarizer, a protective layer attached to the viewing side of the polarizer via a first adhesive layer, and a second adhesive layer disposed on the polarizer on the opposite side to the first adhesive layer, where the iodine adsorption amount A1 per unit area of ​​the first adhesive layer and the iodine adsorption amount A2 per unit area of ​​the second adhesive layer satisfy the following formula (1): (A1+A2)<0.300(mg / cm 2 ) ···(1). In one embodiment, A1 and A2 are each 0.200 mg / cm 2 The following is the result. In one embodiment, the first adhesive layer and / or the second adhesive layer has a thickness of 0.3 μm or less. In one embodiment, the polarizer has a thickness of 10 μm or less. In one embodiment, the polarizer has a single transmittance of 40.0% to 45.0%. According to another aspect of the present invention, there is provided a polarizing plate with a retardation layer, the polarizing plate having the above-mentioned polarizing plate and a retardation layer having a circular polarization function or an elliptically polarizing function, which is bonded to the polarizing plate via the above-mentioned second adhesive layer. In one embodiment, the retardation layer is a layer in which a liquid crystal compound is aligned and fixed. In one embodiment, the retardation layer is a single layer, the retardation layer has Re(550) of 100 nm to 190 nm, Re(450) / Re(550) of 0.8 to 0.95, and the angle between the slow axis and the absorption axis of the polarizer is 40° to 50°. In one embodiment, the retardation layer includes a first retardation layer and a second retardation layer; the first retardation layer has Re(550) of 200 nm to 300 nm, and the angle between the slow axis and the absorption axis of the polarizer is 10° to 20°; and the second retardation layer has Re(550) of 100 nm to 190 nm, and the angle between the slow axis and the absorption axis of the polarizer is 70° to 80°. According to yet another aspect of the present invention, there is provided an image display device, the image display device comprising the above polarizing plate or the above retardation layer-attached polarizing plate. Effect of the Invention

[0006] According to an embodiment of the present invention, in a polarizing plate, by setting the iodine adsorption amount per unit area of ​​the adhesive layer adjacent to the polarizer to a predetermined value or less, it is possible to obtain a thin polarizing plate in which the decrease in the degree of polarization in a high-temperature and high-humidity environment is suppressed. As a result, it is possible to obtain a polarizing plate with a retardation layer that can maintain optical properties in a high-temperature and high-humidity environment and realize an image display device with small display unevenness. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view of a retardation layer-attached polarizing plate according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a retardation layer-attached polarizing plate according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When angles are referred to herein, the angles include both clockwise and counterclockwise angles relative to a reference direction, so for example, "45°" means ±45°.

[0010] A. Polarizing plate A-1. Overall structure of polarizing plate FIG. 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100 in the illustrated example includes a polarizer 10, a protective layer (viewing-side protective layer) 20 attached to the viewing side of the polarizer 10 via a first adhesive layer 31, and a second adhesive layer 32 arranged on the opposite side of the polarizer 10 to the first adhesive layer 31. The adhesive layer is made of an adhesive or a pressure-sensitive adhesive. Typically, an optically functional layer can be attached via the second adhesive layer 32. Representative examples of the optically functional layer include another protective layer (inner protective layer) and a retardation layer. The inner protective layer can be preferably omitted. When the optically functional layer is a retardation layer, a retardation layer-attached polarizing plate is constructed. The retardation layer-attached polarizing plate will be described in detail in Section B below. When the second adhesive layer 32 is made of a pressure-sensitive adhesive, the polarizing plate 100 can be attached to an image display cell via the second adhesive layer 32.

[0011] In an embodiment of the present invention, the iodine adsorption amount A1 per unit area of ​​the first adhesive layer 31 and the iodine adsorption amount A2 per unit area of ​​the second adhesive layer 32 satisfy the following formula (1): (A1+A2)<0.300(mg / cm 2 ) ···(1). (A1+A2) is preferably 0.200 mg / cm 2 or less, more preferably 0.100 mg / cm 2 More preferably, it is 0.080 mg / cm or less. 2 or less, and particularly preferably 0.060 mg / cm 2 (A1+A2) is, for example, 0.020 mg / cm 2 or more. If (A1+A2) is in this range, it is possible to suppress the migration of iodine in the polarizer to the first adhesive layer and the second adhesive layer in a high-temperature, high-humidity environment. As a result, even in a high-temperature, high-humidity environment, the decrease in the iodine concentration in the polarizer is suppressed, and therefore a polarizing plate in which the decrease in the polarization degree is suppressed can be realized. The amount of iodine adsorption per unit area of ​​the adhesive layer can be adjusted by appropriately setting the type of adhesive or pressure-sensitive adhesive constituting the adhesive layer, the thickness of the adhesive layer, etc.

[0012] Preferably, A1 and A2 are both 0.200 mg / cm 2 (A1+A2) is 0.300mg / cm 2 and A1 and A2 are both less than 0.200 mg / cm 2 When the (A1+A2) is 0.300 mg / cm or less, it is possible to further suppress the migration of iodine in the polarizer to the adhesive layer under a high-temperature and high-humidity environment. 2 Even if the amount of A1 or A2 is less than 100 μm, if one of A1 and A2 is extremely large, a large amount of iodine in the polarizer may migrate to the first adhesive layer or the second adhesive layer (i.e., the adhesive layer having a larger amount of iodine adsorption per unit area) in a high-temperature and high-humidity environment. As a result, the iodine concentration in the polarizer may decrease significantly, and the polarization degree may decrease. In one embodiment, one of A1 and A2 is preferably 0.195 mg / cm or less. 2 or less, more preferably 0.190 mg / cm 2 More preferably, it is 0.180 mg / cm or less. 2 the other is preferably 0.035 mg / cm 2More preferably, it is 0.030 mg / cm or less. 2 More preferably, it is 0.025 mg / cm or less. 2 In this case, one of A1 and A2 is, for example, 0.150 mg / cm 2 or more; the other may be, for example, 0.015 mg / cm 2 In this configuration, a thicker adhesive can be used in one of the adhesive layers. In another embodiment, both A1 and A2 are preferably 0.045 mg / cm 2 More preferably, it is 0.040 mg / cm or less. 2 More preferably, it is 0.035 mg / cm or less. 2 or less, and particularly preferably 0.030 mg / cm 2 In this case, A1 and A2 are each, for example, 0.010 mg / cm 2 With this configuration, the decrease in the polarization degree in a high-temperature and high-humidity environment can be more significantly suppressed. Also, this configuration can contribute to further reducing the thickness of the polarizing plate.

[0013] The first adhesive layer 31 and the second adhesive layer 32 each have (A1+A2) of 0.300 mg / cm 2It may be made of any suitable adhesive or pressure-sensitive adhesive as long as the thickness is less than 1 μm. Specifically, the first adhesive layer 31 and the second adhesive layer 32 may both be made of an adhesive, one may be made of an adhesive and the other may be made of a pressure-sensitive adhesive, or both may be made of a pressure-sensitive adhesive. In one embodiment, the first adhesive layer may be made of an adhesive, and the second adhesive layer may be made of a pressure-sensitive adhesive. In another embodiment, both the first adhesive layer and the second adhesive layer may be made of a pressure-sensitive adhesive. When the adhesive layer is made of an adhesive, its thickness is preferably 2 μm or less, more preferably 1 μm or less, even more preferably 0.5 μm or less, and particularly preferably 0.3 μm or less. On the other hand, the thickness may be, for example, 0.05 μm or more. When the adhesive layer is made of a pressure-sensitive adhesive, its thickness is preferably 2 μm to 40 μm, more preferably 3 μm to 35 μm, and even more preferably 4 μm to 32 μm. By appropriately setting the thickness depending on the material constituting the pressure-sensitive adhesive, an adhesive layer having the desired iodine adsorption amount per unit area can be formed.

[0014] The polarizer, the protective layer, the first adhesive layer, and the second adhesive layer will be specifically described below.

[0015] A-2. Polarizer Any appropriate polarizer can be adopted as the polarizer 10. For example, the resin film forming the polarizer may be a single-layer resin film or a laminate of two or more layers.

[0016] Specific examples of polarizers made of a single-layer resin film include hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films that have been dyed with iodine or a dichroic substance such as a dichroic dye and stretched, and polyene-based oriented films such as dehydrated PVA films and dehydrochlorinated polyvinyl chloride films. A polarizer obtained by dyeing a PVA film with iodine and uniaxially stretching it is preferably used because of its excellent optical properties.

[0017] The dyeing with iodine is carried out, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment, or may be carried out while dyeing. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based film in water and washing it with water before dyeing, it is possible to wash off dirt and antiblocking agents on the surface of the PVA-based film, and also to swell the PVA-based film and prevent uneven dyeing.

[0018] Specific examples of polarizers obtained using laminates include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate can be produced by, for example, applying a PVA-based resin solution to the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to make the PVA-based resin layer a polarizer. In this embodiment, stretching typically includes immersing the laminate in an aqueous solution of boric acid to stretch it. Furthermore, stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95°C or higher) before stretching in the aqueous solution of boric acid. The obtained laminate of resin substrate / polarizer may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or the resin substrate may be peeled off from the laminate of resin substrate / polarizer, and any suitable protective layer may be laminated on the peeled surface depending on the purpose. Details of the method for producing such a polarizer are described in, for example, JP2012-73580A and JP6470455A. The entire disclosures of these publications are incorporated herein by reference.

[0019] The thickness of the polarizer is preferably 15 μm or less, more preferably 12 μm or less, further preferably 10 μm or less, and particularly preferably 8 μm or less. On the other hand, the thickness of the polarizer can be, for example, 1 μm or more, for example, 2 μm or more, or for example, 3 μm or more. If the thickness of the polarizer is in this range, curling during heating can be well suppressed, and good appearance durability during heating can be obtained.

[0020] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is preferably 40.0% to 45.0%, more preferably 41.0% to 44.0%, and even more preferably 42.0% to 44.0%. The degree of polarization of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.

[0021] A-3.Protective layer The viewing-side protective layer 20 and the inner protective layer (if present) are each formed of any suitable film that can be used as a protective layer for a polarizer. Specific examples of materials that are the main components of the film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. Other examples include thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxys, and silicones. Other examples include glassy polymers such as siloxane polymers. Polymer films described in JP 2001-343529 A (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition.

[0022] The viewer-side protective layer 20 may be subjected to a surface treatment such as a hard coat treatment, an anti-reflection treatment, an anti-sticking treatment, or an anti-glare treatment, if necessary. In addition, the viewer-side protective layer 20 may be subjected to a treatment for improving visibility when viewed through polarized sunglasses (typically, by imparting an (elliptical) polarization function or an ultra-high phase difference) if necessary. By performing such a treatment, excellent visibility can be achieved even when the display screen is viewed through polarized lenses such as polarized sunglasses. Therefore, the polarizing plate and the polarizing plate with a phase difference layer can be suitably applied to an image display device that can be used outdoors.

[0023] The thickness of the viewer-side protective layer 20 is preferably 10 μm to 50 μm, and more preferably 15 μm to 35 μm. When a surface treatment is applied, the thickness of the viewer-side protective layer 20 includes the thickness of the surface treatment layer.

[0024] In one embodiment, the inner protective layer (if present) is preferably optically isotropic. In this specification, "optically isotropic" means that the in-plane retardation Re(550) is 0 nm to 10 nm, and the retardation in the thickness direction Rth(550) is -10 nm to +10 nm. The thickness of the other protective layer is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and further preferably 10 μm to 30 μm. In an embodiment of the present invention, the inner protective layer may preferably be omitted.

[0025] A-4. First adhesive layer and second adhesive layer As described above, the first adhesive layer and the second adhesive layer each have (A1+A2) of 0.300 mg / cm 2 As long as the thickness of the first adhesive layer is less than 100 μm, the first adhesive layer and the second adhesive layer may be made of any suitable adhesive or pressure-sensitive adhesive. As also described above, the first adhesive layer and the second adhesive layer may both be made of an adhesive, one may be made of an adhesive and the other may be made of a pressure-sensitive adhesive, or both may be made of a pressure-sensitive adhesive. In one embodiment, the first adhesive layer may be made of an adhesive, and the second adhesive layer may be made of a pressure-sensitive adhesive. In another embodiment, both the first adhesive layer and the second adhesive layer may be made of a pressure-sensitive adhesive. In this section, the first adhesive layer and the second adhesive layer may be collectively referred to simply as adhesive layers.

[0026] A representative example of the adhesive is a water-based adhesive. By using a water-based adhesive, a very thin adhesive layer (for example, 0.3 μm or less) can be formed. The water-based adhesive preferably contains a PVA-based resin. From the viewpoint of adhesiveness, the average polymerization degree of the PVA-based resin contained in the water-based adhesive is preferably about 100 to 5000, more preferably 1000 to 4000. From the viewpoint of adhesiveness, the average saponification degree is preferably about 85 mol % to 100 mol %, more preferably 90 mol % to 100 mol %.

[0027] The PVA resin preferably contains an acetoacetyl group. This is because it can provide excellent adhesion between the polarizer and the protective layer and excellent durability. The acetoacetyl group-containing PVA resin can be obtained, for example, by reacting a PVA resin with diketene by any method. The degree of modification of the acetoacetyl group-containing PVA resin with an acetoacetyl group is typically 0.1 mol % or more, preferably about 0.1 mol % to 40 mol %, more preferably 1 mol % to 20 mol %, and particularly preferably 2 mol % to 7 mol %. The degree of modification of the acetoacetyl group is a value measured by NMR.

[0028] The aqueous adhesive (before curing) is preferably in the form of a liquid (typically an aqueous solution). The resin concentration in the liquid is preferably 0.1% by weight to 15% by weight, and more preferably 0.5% by weight to 10% by weight. The viscosity of the liquid is preferably 1 to 50 mPa·s. The pH of the liquid is preferably 2 to 6, more preferably 2.5 to 5, even more preferably 3 to 5, and particularly preferably 3.5 to 4.5.

[0029] The aqueous adhesive may preferably contain a metal compound colloid. The metal compound colloid is a metal compound fine particle dispersed in a dispersion medium, and is electrostatically stabilized due to mutual repulsion of the same type of charge of the fine particles, and can have permanent stability. By containing such a metal compound colloid, an adhesive layer with a very small amount of iodine adsorption per unit area can be formed. It has been known that knick defects (defects that cause light leakage) can be suppressed by using an aqueous adhesive containing a metal compound colloid. On the other hand, the present inventors have found that a remarkable effect can be obtained by using an aqueous adhesive containing a metal compound colloid as a result of trial and error to solve the problem of the decrease in polarization degree of a thin polarizing plate under a high temperature and high humidity environment, and have found that such a remarkable effect can be caused by the very small amount of iodine adsorption per unit area of ​​the adhesive layer. It is presumed that such a very small amount of iodine adsorption per unit area is due to the synergistic effect of the effect of being able to form a very thin adhesive layer, the effect of the binder resin being a PVA-based resin, and the effect of the metal compound colloid.

[0030] The average particle size of the fine particles forming the metal compound colloid is set to any appropriate value as long as it does not adversely affect optical properties such as transparency and polarization properties. It is preferably 1 nm to 100 nm, and more preferably 1 nm to 50 nm, because this allows the fine particles to be uniformly dispersed in the adhesive layer.

[0031] Any suitable compound can be used as the metal compound. For example, metal oxides such as alumina, silica, zirconia, titania, etc.; metal salts such as aluminum silicate, calcium carbonate, magnesium silicate, zinc carbonate, barium carbonate, calcium phosphate, etc.; minerals such as celite, talc, clay, kaolin, etc. are included. A colloidal metal compound having a positive charge is preferably used. Examples of the metal compound include alumina, titania, etc., and alumina is particularly preferred.

[0032] The amount of metal compound colloid (solid content) is preferably 200 parts by weight or less, more preferably 10 parts by weight to 200 parts by weight, even more preferably 20 parts by weight to 175 parts by weight, and particularly preferably 30 parts by weight to 150 parts by weight, per 100 parts by weight of the PVA-based resin.

[0033] The water-based adhesive may further contain additives. Representative additives include crosslinking agents (e.g., compounds having at least two functional groups reactive with PVA-based resins); coupling agents such as silane coupling agents and titanium coupling agents; various tackifiers; and stabilizers such as ultraviolet absorbers, antioxidants, heat stabilizers, and hydrolysis stabilizers. The types, numbers, and combinations of additives can be appropriately set according to the purpose.

[0034] Representative examples of the adhesive include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, number, combination, and compounding ratio of the monomers forming the base resin of the adhesive, as well as the compounding amount of the crosslinking agent, reaction temperature, reaction time, and the like, an adhesive having desired properties according to the purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more. From the viewpoints of transparency, processability, durability, and the like, an acrylic adhesive (acrylic adhesive composition) is preferred. The acrylic adhesive composition typically contains a (meth)acrylic polymer as a main component. The (meth)acrylic polymer may be contained in the adhesive composition at a ratio of, for example, 50% by weight or more, preferably 70% by weight or more, and more preferably 90% by weight or more of the solid content of the adhesive composition. The (meth)acrylic polymer contains an alkyl (meth)acrylate as a main component as a monomer unit. Incidentally, (meth)acrylate refers to acrylate and / or methacrylate. The alkyl (meth)acrylate may be contained in the monomer components forming the (meth)acrylic polymer at a ratio of preferably 80% by weight or more, more preferably 90% by weight or more. The alkyl group of the alkyl (meth)acrylate may be, for example, a linear or branched alkyl group having 1 to 18 carbon atoms. The average number of carbon atoms in the alkyl group is preferably 3 to 9, more preferably 3 to 6. A preferred alkyl (meth)acrylate is butyl acrylate. Examples of monomers (copolymerizable monomers) constituting the (meth)acrylic polymer include, in addition to alkyl (meth)acrylates, carboxyl group-containing monomers, hydroxyl group-containing monomers, amide group-containing monomers, aromatic ring-containing (meth)acrylates, and heterocycle-containing vinyl monomers. Representative examples of the copolymerization monomer include acrylic acid, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, acryloylmorpholine, phenoxyethyl acrylate, and N-vinyl-2-pyrrolidone. Preferred are acrylic acid, 4-hydroxybutyl acrylate, and acryloylmorpholine.By using such a monomer as a copolymerization monomer, an adhesive layer having a small iodine adsorption amount per unit area can be formed. The acrylic adhesive composition may preferably contain a silane coupling agent and / or a crosslinking agent. Examples of the silane coupling agent include an epoxy group-containing silane coupling agent. Examples of the crosslinking agent include an isocyanate-based crosslinking agent and a peroxide-based crosslinking agent. Furthermore, the acrylic adhesive composition may contain an antioxidant and / or a conductive agent. Details of the adhesive are described in, for example, JP 2006-183022 A, JP 2015-199942 A, JP 2018-053114 A, JP 2016-190996 A, and WO 2018 / 008712 A, and the descriptions in these publications are incorporated herein by reference.

[0035] The pressure-sensitive adhesive preferably has a storage modulus of 1.0×10 4 Pa~1.0×10 6 Pa, more preferably 1.0×10 4 Pa~1.0×10 5 When the storage modulus of the pressure-sensitive adhesive is within this range, it is possible to reduce internal stress caused by dimensional changes in the polarizer when it is heated and / or when it is folded or attached to a curved surface.

[0036] The creep amount ΔCr of the adhesive at 70°C is, for example, 65 μm or less, and may be 50 μm or less, 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, or even 15 μm or less. The lower limit of the creep amount ΔCr is, for example, 0.5 μm. If the creep amount is within such a range, as in the case of the storage elastic modulus, the internal stress due to the dimensional change of the polarizer can be alleviated when heated and / or when folded or attached to a curved surface. The creep value can be measured, for example, by the following procedure: A load of 500 gf is applied vertically downward to the adhesive attached to a stainless steel test plate at a joint surface of 20 mm long x 20 mm wide, with the test plate fixed. The creep amount (displacement amount) of the adhesive relative to the test plate is measured at each time point 100 seconds and 3600 seconds after the start of the load application, and the Cr 100 and Cr 3600 The measured Cr 100 and Cr 3600 From the formula ΔCr = Cr 3600 -Cr 100 The creep amount ΔCr can be calculated by the following equation.

[0037] B. Polarizing plate with retardation layer B-1. Overall structure of polarizing plate with retardation layer As described in the above item A-1, the polarizing plate according to the embodiment of the present invention may be configured as a polarizing plate with a retardation layer by bonding the retardation layer via the second adhesive layer 32. Therefore, the polarizing plate with a retardation layer may also be included in the embodiment of the present invention. The polarizing plate with a retardation layer according to the embodiment of the present invention can maintain optical properties even in a high-temperature and high-humidity environment, and can realize an image display device with little display unevenness.

[0038] FIG. 2 is a schematic cross-sectional view of a retardation layer-attached polarizing plate according to one embodiment of the present invention. The retardation layer-attached polarizing plate 200 of the illustrated example has a polarizing plate 100 and a retardation layer 120 attached to the polarizing plate 100 via a second adhesive layer 32. The retardation layer 120 typically has a circular polarization function or an elliptical polarization function. In the retardation layer-attached polarizing plate 200, a pressure-sensitive adhesive layer 140 is provided as the outermost layer on the opposite side of the retardation layer 120 from the polarizing plate 100, and the retardation layer-attached polarizing plate can be attached to an image display cell. The pressure-sensitive adhesive layer 140 can be made of any appropriate pressure-sensitive adhesive. For practical purposes, a separator (not shown) is temporarily attached to the surface of the pressure-sensitive adhesive layer 140 in a peelable manner. By temporarily attaching the separator, the pressure-sensitive adhesive layer is protected and the retardation layer-attached polarizing plate can be rolled.

[0039] The retardation layer is typically an alignment-solidified layer of a liquid crystal compound. By using a liquid crystal compound, the difference between nx and ny of the resulting retardation layer can be significantly increased compared to non-liquid crystal materials, so the thickness of the retardation layer for obtaining a desired in-plane retardation can be significantly reduced. As a result, a polarizing plate with a retardation layer can be significantly thinned. In this specification, the "alignment-solidified layer" refers to a layer in which the liquid crystal compound is aligned in a predetermined direction within the layer and the alignment state is fixed. The "alignment-solidified layer" is a concept that includes an alignment-solidified layer obtained by hardening a liquid crystal monomer as described later. In the retardation layer, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the retardation layer (homogeneous alignment).

[0040] In one embodiment, as shown in FIG. 2, the retardation layer is a single layer 120. In this case, the retardation layer typically exhibits inverse dispersion wavelength characteristics and can function as a λ / 4 plate. Specifically, Re(550) of the retardation layer is preferably 100 nm to 190 nm, Re(450) / Re(550) is preferably 0.8 to 0.95, and the angle between the slow axis of the retardation layer and the absorption axis of the polarizer is preferably 40° to 50°. Furthermore, in this case, preferably, another retardation layer (so-called positive C plate: not shown) whose refractive index characteristics show the relationship nz>nx=ny may be provided on the opposite side of the retardation layer from the polarizing plate.

[0041] In another embodiment, as shown in FIG. 3, the retardation layer has a first retardation layer 121 and a second retardation layer 122. In this case, typically, either the first retardation layer 121 or the second retardation layer 122 can function as a λ / 2 plate, and the other can function as a λ / 4 plate. For example, when the first retardation layer 121 can function as a λ / 2 plate and the second retardation layer 122 can function as a λ / 4 plate, the Re(550) of the first retardation layer 121 is preferably 200 nm to 300 nm, and the angle between its slow axis and the absorption axis of the polarizer 10 is preferably 10° to 20°; the Re(550) of the second retardation layer 122 is preferably 100 nm to 190 nm, and the angle between its slow axis and the absorption axis of the polarizer 10 is preferably 70° to 80°.

[0042] The total thickness of the retardation layer-attached polarizing plate (thickness from the viewing side protective layer to the pressure-sensitive adhesive layer) is preferably 80 μm or less, more preferably 70 μm or less, even more preferably 65 μm or less, and particularly preferably 60 μm or less. The lower limit of the total thickness may be, for example, 42 μm. According to the embodiment of the present invention, it is possible to realize a retardation layer-attached polarizing plate that is extremely thin and suppresses the decrease in the polarization degree of the polarizer in a high-temperature and high-humidity environment, and as a result, can maintain the overall optical characteristics in a high-temperature and high-humidity environment. Furthermore, a retardation layer-attached polarizing plate having such a total thickness can have extremely excellent flexibility and foldability. As a result, the retardation layer-attached polarizing plate can be particularly suitably applied to a curved image display device and / or a bendable or foldable image display device.

[0043] The retardation layer-attached polarizing plate may further include other optical functional layers. The type, characteristics, number, combination, arrangement position, etc. of the optical functional layers that can be provided in the retardation layer-attached polarizing plate may be appropriately set according to the purpose. For example, the retardation layer-attached polarizing plate may further have a conductive layer or a conductive layer-attached isotropic substrate (both are not shown). The conductive layer or the conductive layer-attached isotropic substrate is typically provided on the outside of the retardation layer 120 (the side opposite to the polarizing plate 100). The conductive layer or the conductive layer-attached isotropic substrate is typically an arbitrary layer that is provided as necessary, and may be omitted. In addition, when the conductive layer or the conductive layer-attached isotropic substrate is provided, the retardation layer-attached polarizing plate may be applied to a so-called inner touch panel type input display device in which a touch sensor is incorporated between an image display cell (for example, an organic EL cell) and a polarizing plate. In addition, for example, the retardation layer-attached polarizing plate may further include other retardation layers. Other optical characteristics (for example, refractive index characteristics, in-plane retardation, Nz coefficient, photoelastic coefficient), thickness, arrangement position, and the like of the retardation layer can be appropriately set depending on the purpose.

[0044] The above-described embodiments may be combined as appropriate, modifications that are obvious to those skilled in the art may be made to the components in the above-described embodiments, and the configurations in the above-described embodiments may be replaced with optically equivalent configurations.

[0045] The polarizing plate with a retardation layer may be in the form of a sheet or a long sheet. In this specification, the term "long sheet" means a long and narrow shape whose length is sufficiently longer than its width, and includes, for example, a long and narrow shape whose length is 10 times or more, preferably 20 times or more, than its width. The long polarizing plate with a retardation layer can be wound into a roll.

[0046] Hereinafter, the retardation layer will be described. When the retardation layer has a first retardation layer and a second retardation layer, the first retardation layer and the second retardation layer are collectively described simply as a retardation layer, and the first retardation layer and the second retardation layer are referred to as "first" and "second" only when it is necessary to distinguish between them.

[0047] B-2. Retardation layer As described above, the retardation layer is a layer of alignment and solidification of a liquid crystal compound (hereinafter, liquid crystal alignment and solidification layer). As the liquid crystal compound, for example, a liquid crystal compound having a nematic liquid crystal phase (nematic liquid crystal) can be mentioned. As such a liquid crystal compound, for example, a liquid crystal polymer or a liquid crystal monomer can be used. The mechanism of liquid crystallinity of the liquid crystal compound may be either lyotropic or thermotropic. The liquid crystal polymer and the liquid crystal monomer may be used alone or in combination.

[0048] When the liquid crystal compound is a liquid crystal monomer, the liquid crystal monomer is preferably a polymerizable monomer and a crosslinkable monomer. This is because the liquid crystal monomer can be polymerized or crosslinked (i.e., cured) to fix the alignment state of the liquid crystal monomer. After the liquid crystal monomer is aligned, for example, the liquid crystal monomers can be polymerized or crosslinked with each other to fix the alignment state. Here, a polymer is formed by polymerization, and a three-dimensional network structure is formed by crosslinking, but these are non-liquid crystals. Therefore, the formed retardation layer does not undergo transition to a liquid crystal phase, a glass phase, or a crystalline phase due to temperature changes specific to liquid crystal compounds, for example. As a result, the retardation layer becomes a retardation layer that is not affected by temperature changes and has extremely excellent stability.

[0049] The temperature range in which the liquid crystal monomer exhibits liquid crystallinity varies depending on the type of the liquid crystal monomer. Specifically, the temperature range is preferably 40°C to 120°C, more preferably 50°C to 100°C, and most preferably 60°C to 90°C.

[0050] Any suitable liquid crystal monomer can be used as the liquid crystal monomer. For example, the polymerizable mesogen compounds described in JP-A-2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, and GB2280445 can be used. Specific examples of such polymerizable mesogen compounds include BASF's product name LC242, Merck's product name E7, and Wacker-Chem's product name LC-Sillicon-CC3767. For example, nematic liquid crystal monomers are preferred as the liquid crystal monomer.

[0051] The liquid crystal alignment solidified layer can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. In one embodiment, the substrate is any appropriate resin film, and the liquid crystal alignment solidified layer (retardation layer 120 or first retardation layer 121) formed on the substrate can be transferred to the surface of the polarizing plate 100 via the second adhesive layer 32. When the retardation layer has the first retardation layer 121 and the second retardation layer 122, the second retardation layer 122 formed on the substrate can be transferred to the surface of the first retardation layer 121 via any appropriate adhesive.

[0052] As the above alignment treatment, any appropriate alignment treatment can be adopted. Specifically, mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment can be mentioned. Specific examples of the mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of the physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of the chemical alignment treatment include oblique evaporation method and photo-alignment treatment. The treatment conditions of various alignment treatments can be any appropriate conditions according to the purpose.

[0053] The alignment of the liquid crystal compound is performed by treating at the temperature at which the liquid crystal phase is exhibited according to the type of the liquid crystal compound. By performing such a temperature treatment, the liquid crystal compound takes a liquid crystal state and the liquid crystal compound aligns according to the alignment treatment direction on the substrate surface.

[0054] In one embodiment, the fixation of the alignment state is performed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is a polymerizable monomer or a crosslinkable monomer, the fixation of the alignment state is performed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or a crosslinking treatment.

[0055] Specific examples of the liquid crystal compound and details of the method for forming the alignment fixing layer are described in Japanese Patent Application Laid-Open No. 2006-163343. The description of the said publication is incorporated herein by reference.

[0056] Typically, the retardation layer shows a refractive index characteristic relationship of nx > ny = nz. Note that "ny = nz" includes not only the case where ny and nz are exactly equal but also the case where they are substantially equal. Therefore, within a range not impairing the effects of the present invention, ny > nz or ny < nz may occur.

[0057] The Nz coefficient of the retardation layer is preferably 0.9 to 1.5, more preferably 0.9 to 1.3. By satisfying such a relationship, when the polarizing plate with a retardation layer is used in an image display device, a very excellent reflected hue can be achieved.

[0058] When the retardation layer is a single layer, the in-plane retardation Re(550) of the retardation layer is preferably 100 nm to 190 nm, more preferably 110 nm to 170 nm, and even more preferably 130 nm to 160 nm, as described above; Re(450) / Re(550) is preferably 0.8 to 0.95, as described above. Furthermore, the angle between the slow axis of the retardation layer and the absorption axis of the polarizer is preferably 40° to 50°, more preferably 42° to 48°, and even more preferably about 45°, as described above. Furthermore, in this case, preferably, another retardation layer (so-called positive C plate) whose refractive index characteristics show the relationship nz>nx=ny may be provided on the opposite side of the retardation layer from the polarizing plate.

[0059] When the retardation layer has a first retardation layer 121 and a second retardation layer 122, either the first retardation layer 121 or the second retardation layer 122 can function as a λ / 2 plate, and the other can function as a λ / 4 plate. Here, a case where the first retardation layer 121 can function as a λ / 2 plate and the second retardation layer 122 can function as a λ / 4 plate will be described, but these may be reversed. The thickness of the first retardation layer 121 can be adjusted so as to obtain a desired in-plane retardation of the λ / 2 plate, and can be, for example, 1.5 μm to 2.5 μm. The thickness of the second retardation layer 122 can be adjusted so as to obtain a desired in-plane retardation of the λ / 4 plate, and can be, for example, 0.5 μm to 1.5 μm. As described above, the in-plane retardation Re(550) of the first retardation layer is preferably 200 nm to 300 nm, more preferably 230 nm to 290 nm, and even more preferably 250 nm to 280 nm. As described above, the in-plane retardation Re(550) of the second retardation layer is preferably 100 nm to 190 nm, more preferably 110 nm to 170 nm, and even more preferably 130 nm to 160 nm. As described above, the angle between the slow axis of the first retardation layer 121 and the absorption axis of the polarizer 10 is preferably 10° to 20°, more preferably 12° to 18°, and even more preferably about 15°. As described above, the angle between the slow axis of the second retardation layer 122 and the absorption axis of the polarizer 10 is preferably 70° to 80°, more preferably 72° to 78°, and even more preferably about 75°. With this configuration, it is possible to obtain characteristics close to ideal reverse wavelength dispersion characteristics, and as a result, it is possible to realize extremely excellent anti-reflection characteristics.

[0060] The first retardation layer and the second retardation layer may each exhibit an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or a flat wavelength dispersion characteristic in which the retardation value changes very little depending on the wavelength of the measurement light.

[0061] C. Image display device The polarizing plate described in the above item A and the retardation layer-attached polarizing plate described in the above item B can be applied to an image display device. Therefore, an image display device including a polarizing plate or a retardation layer-attached polarizing plate is also included in the embodiment of the present invention. The image display device typically includes an image display cell and a polarizing plate or a retardation layer-attached polarizing plate attached to the image display cell via an adhesive layer. The polarizing plate or the retardation layer-attached polarizing plate can typically be disposed on the viewing side of the image display cell. Representative examples of the image display device include a liquid crystal display device and an electroluminescence (EL) display device (e.g., an organic EL display device, an inorganic EL display device). In one embodiment, the image display device is an organic EL display device. In one embodiment, the image display device has a curved shape (substantially a curved display screen) and / or can be bent or folded. In such an image display device, the effect of the retardation layer-attached polarizing plate according to the embodiment of the present invention becomes remarkable. EXAMPLES

[0062] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified.

[0063] (1) Thickness The thickness of 10 μm or less was measured using an interference film thickness meter (manufactured by Otsuka Electronics, product name "MCPD-3000"), and the thickness of more than 10 μm was measured using a digital micrometer (manufactured by Anritsu, product name "KC-351C"). (2) Iodine adsorption amount 10 g of 0.127% iodine aqueous solution was placed in a 500 mL glass bottle. The adhesive or pressure sensitive adhesive used in the examples and comparative examples was cut to a predetermined size to be used as a measurement sample. This measurement sample was attached to the inside of the lid of the glass bottle, and the glass bottle was sealed with the lid. As a result, the measurement sample was suspended inside the sealed glass bottle. The distance between the bottom end of the measurement sample and the liquid surface of the iodine aqueous solution was about 40 mm. In this state, the glass bottle was heated at 65°C for 6 hours. After heating, the measurement sample was removed, and the iodine detection intensity (kcps) was measured using a scanning X-ray fluorescence analyzer (RIGAKU Corporation, "ZSX Primus IV"). The amount of iodine adsorption (mg) was calculated using the calibration curve of the measurement device, and the amount of iodine adsorption was proportional to the volume (cm) of the measurement sample. 3 ) to obtain the amount of iodine adsorption per unit volume (volumetric iodine adsorption: unit: mg / cm 3 The volumetric iodine adsorption is a value specific to the material. From the volumetric iodine adsorption and the thickness of the adhesive layer in the polarizing plate, the iodine adsorption per unit area (area iodine adsorption: unit: mg / cm 2 The calibration curve of the measuring device was, for example, as shown below. The calibration curve was prepared by measuring known samples. Iodine mass (μg) = iodine detection intensity (kcps) × 13.525

[0064] (3) Change in polarization degree ΔP The polarizing plates with retardation layers obtained in the examples and comparative examples were attached to non-alkali glass via an adhesive layer to prepare a measurement sample. The measurement sample was left standing for 500 hours in a chamber set to a 60°C and 95% RH environment. The polarization degree of the polarizing plate with retardation layers (effectively a polarizer) before heating and humidifying was P0, and the polarization degree after heating and humidifying was P 500 Then, ΔP was calculated from the following formula. ΔP=P 500 -P0 The degree of polarization was calculated as follows. The single transmittance Ts, parallel transmittance Tp, and crossed transmittance Tc of the retardation layer-attached polarizing plate (effectively a polarizer) were measured using an ultraviolet-visible spectrophotometer (Otsuka Electronics' "LPF-200"), and were taken as Ts, Tp, and Tc of the polarizer, respectively. These Ts, Tp, and Tc are Y values ​​measured using a 2-degree visual field (C light source) according to JIS Z8701 and corrected for visibility. The degree of polarization P was calculated from the obtained Tp and Tc using the following formula. Polarization degree P(%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0065] [Production Example 1: Preparation of Water-Based Adhesive] An aqueous adhesive (adhesive A) was obtained by mixing 6.02 parts of acetoacetyl-modified PVA (degree of polymerization 1200, degree of acetoacetyl modification 4.6%, degree of saponification 99.0 mol% or more, solids concentration 4%, manufactured by Mitsubishi Chemical Corporation, product name "Gosenex Z-200"), 25 parts of an aqueous solution containing positively charged alumina colloid (average particle diameter 15 nm) at a solids concentration of 3.2%, and 18.98 parts of pure water.

[0066] [Production Example 2: Preparation of Water-Based Adhesive] An aqueous adhesive (adhesive B) was obtained by mixing 7 parts of anionic PVA (degree of polymerization 1200, degree of saponification 99.0 mol% or more, solids concentration 10%, manufactured by Mitsubishi Chemical Corporation, product name "Gosenex N-300"), 25 parts of an aqueous solution containing positively charged alumina colloid (average particle diameter 15 nm) at a solids concentration of 3.5%, and 18 parts of pure water.

[0067] [Production Example 3: Preparation of acrylic adhesive] (Preparation of Acrylic Polymer) A monomer mixture containing 91 parts of butyl acrylate, 6 parts of acryloylmorpholine, 2.7 parts of acrylic acid, and 0.3 parts of 4-hydroxybutyl acrylate was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 100 parts of ethyl acetate for 100 parts of this monomer mixture, and nitrogen gas was introduced while gently stirring to replace the atmosphere with nitrogen. The liquid temperature in the flask was kept at about 55°C, and a polymerization reaction was carried out for 8 hours to prepare a solution of an acrylic polymer with a weight average molecular weight (Mw) of 2.7 million and Mw / Mn=3.8.

[0068] (Preparation of Adhesive) Adhesive C was obtained by blending 100 parts of the solid content of the acrylic polymer solution with 0.1 parts of trimethylolpropane / tolylene diisocyanate adduct (manufactured by Tosoh Corporation, product name "Coronate L"), 0.3 parts of a peroxide crosslinking agent (manufactured by Nippon Oil & Fats Corporation, product name "Niper BMT"), and 0.2 parts of an epoxy group-containing silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-403").

[0069] [Production Example 4: UV-curable adhesive] A commercially available ultraviolet-curing adhesive was used.

[0070] [Example 1] 1. Preparation of Polarizer As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of about 75° C. was used, and one side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a ratio of 9:1, and dissolving the mixture in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched 2.4 times in the machine direction (longitudinal direction) in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the final polarizer would be 43.0% (dyeing process). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4% by weight, potassium iodide concentration: 5% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, the film was dried in an oven maintained at about 90° C. while being brought into contact with a SUS heated roll whose surface temperature was maintained at about 75° C. (drying shrinkage treatment). In this manner, a polarizer having a thickness of 5 μm and a single transmittance of 43.0% was formed on the resin substrate, and a polarizing plate having a resin substrate / polarizer structure was obtained.

[0071] 2. Preparation of Polarizing Plates An HC-TAC film was attached to the polarizer surface of the resin substrate / polarizer laminate obtained above via the adhesive A (first adhesive layer) obtained in Production Example 1. Specifically, the adhesive A was applied so that the thickness after drying would be 0.1 μm, and the films were attached using a rolling machine, and then the adhesive A was dried. The HC-TAC film was a film in which a hard coat (HC) layer (thickness 7 μm) was formed on a triacetyl cellulose (TAC) film (thickness 25 μm), and the TAC film was attached to the polarizer side. Next, the resin substrate was peeled off, and the adhesive C (thickness 5 μm) obtained in Production Example 3 was placed on the peeled surface, to obtain a polarizing plate having a configuration of a viewing side protective layer (HC-TAC film) / first adhesive layer (adhesive A) / polarizer / second adhesive layer (adhesive C).

[0072] 3. Preparation of polarizing plate with retardation layer 3-1. Preparation of retardation layer 55 parts of the compound represented by formula (II), 25 parts of the compound represented by formula (III), and 20 parts of the compound represented by formula (IV) were added to 400 parts of cyclopentanone (CPN), and then the mixture was heated to 60°C and stirred to dissolve. After dissolution was confirmed, the mixture was returned to room temperature, and 3 parts of Irgacure 907 (manufactured by BASF Japan Ltd.), 0.2 parts of Megafac F-554 (manufactured by DIC Corporation), and 0.1 parts of p-methoxyphenol (MEHQ) were added and further stirred to obtain a solution. The solution was transparent and uniform. The obtained solution was filtered through a 0.20 μm membrane filter to obtain a polymerizable composition. On the other hand, the polyimide solution for the alignment film was applied to a glass substrate having a thickness of 0.7 mm by spin coating, dried at 100°C for 10 minutes, and then baked at 200°C for 60 minutes to obtain a coating film. The obtained coating film was subjected to rubbing treatment to form an alignment film. The rubbing treatment was performed using a commercially available rubbing device. The polymerizable composition obtained above was applied to a substrate (substantially an alignment film) by spin coating, and dried at 100° C. for 2 minutes. After the obtained coating film was cooled to room temperature, it was irradiated with 30 mW / cm 2 of a high-pressure mercury lamp. 2The liquid crystal alignment layer was irradiated with ultraviolet light at an intensity of 1000 nm for 30 seconds to obtain a liquid crystal alignment layer. The liquid crystal alignment layer had a thickness of 2.8 μm and an in-plane retardation Re(550) of 130 nm. The liquid crystal alignment layer had a Re(450) / Re(550) of 0.851 and showed reverse dispersion wavelength characteristics. This liquid crystal alignment layer was used as a retardation layer. [ka] [ka]

[0073] 3-2. Preparation of positive C plate A liquid crystal coating liquid was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (I) (the numbers 65 and 35 in the formula indicate the mol% of the monomer unit, and are conveniently represented as a block polymer: weight average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. Then, the coating liquid was applied to a substrate film (norbornene-based resin film: manufactured by Nippon Zeon Co., Ltd., trade name "Zeonex") using a bar coater, and then the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. This liquid crystal layer was irradiated with ultraviolet light to harden the liquid crystal layer, thereby forming a liquid crystal alignment solidified layer (positive C plate, thickness 3 μm) that becomes another retardation layer on the substrate. This layer had Re(590) of 0 nm and Rth(590) of -100 nm, and exhibited refractive index characteristics of nz>nx=ny. [ka]

[0074] 3-3. Preparation of polarizing plate with retardation layer The liquid crystal alignment solidified layer obtained in 3-1 above was transferred to the second adhesive layer surface of the polarizing plate obtained in 2 above, and further, the positive C plate obtained in 3-2 above was transferred to the liquid crystal alignment solidified layer surface via an ultraviolet curing adhesive to obtain a retardation layer-attached polarizing plate having a configuration of viewing side protective layer (HC-TAC film) / first adhesive layer (adhesive A) / polarizer / second adhesive layer (adhesive C) / retardation layer / adhesive / positive C plate. The obtained retardation layer-attached polarizing plate was subjected to the evaluation of (3) above. The results are shown in Table 1.

[0075] [Example 2] Except for changing the thickness of the second adhesive layer (adhesive C) from 5 μm to 30 μm, a polarizing plate with a retardation layer was obtained in the same manner as in Example 1. The obtained polarizing plate with a retardation layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0076] [Example 3] A polarizing plate with a retardation layer was obtained in the same manner as in Example 1, except that the adhesive B obtained in Production Example 2 was used as the first adhesive layer instead of the adhesive A obtained in Production Example 1. The obtained polarizing plate with a retardation layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0077] [Examples 4 to 12 and Comparative Examples 1 to 6] A polarizing plate with a retardation layer was obtained by combining the viewing-side protective layer, the first adhesive layer, and the second adhesive layer as shown in Table 1. The obtained polarizing plate with a retardation layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0078] In Table 1, HC-TAC refers to the above-mentioned HC-TAC film; HC-COP refers to a film in which an HC layer (thickness 2 μm) is formed on a cycloolefin resin (COP) film (thickness 25 μm); acrylic refers to an acrylic resin film; and commercial UV refers to a commercially available ultraviolet-curing adhesive.

[0079] [Table 1]

[0080] [evaluation] As is clear from Table 1, according to the embodiments of the present invention, by setting the sum of the iodine adsorption amount A1 per unit area of ​​the first adhesive layer and the iodine adsorption amount A2 per unit area of ​​the second adhesive layer to a predetermined value or less, it is possible to realize a polarizing plate and a polarizing plate with a retardation layer that are thin and have reduced deterioration in polarization degree in a high-temperature and high-humidity environment. [Industrial Applicability]

[0081] The polarizing plate and the retardation layer-attached polarizing plate of the present invention are suitably used as circular polarizing plates for liquid crystal displays, organic EL displays, and inorganic EL displays. [Explanation of symbols]

[0082] 10 Polarizer 20 protective layer 31 First adhesive layer 32 Second adhesive layer 100 Polarizing Plate 120 Retardation layer 121 First retardation layer 122 Second retardation layer 140 Adhesive layer 200 Polarizing plate with retardation layer

Claims

[Claim 1] a polarizer, a protective layer bonded to a viewing side of the polarizer via a first adhesive layer, and a second adhesive layer disposed on a side of the polarizer opposite to the first adhesive layer, The iodine adsorption amount A per unit area of ​​the first adhesive layer 1 and the iodine adsorption amount A per unit area of ​​the second adhesive layer 2 A polarizing plate that satisfies the following formula (1): (A 1 +A 2 )<0.300(mg / cm 2 ) ・・・(1)。

Citation Information

Patent Citations

  • Retardation film and optical device using the same

    JP3325560B2