Composite electrolyte membrane and membrane electrode assembly
A composite electrolyte membrane with fine metal hexacyanoferrate particles addresses radical-induced deterioration in electrochemical devices, enhancing durability and efficiency by suppressing radical attack and maintaining hydrogen peroxide decomposition.
Patent Information
- Application Number
- JP2023079014
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
AI Technical Summary
Existing electrolyte membranes in electrochemical devices like fuel cells and water electrolyzers suffer from radical attack, leading to increased resistance, cross leakage, and reduced lifespan due to radical-induced deterioration and catalyst poisoning, with existing solutions like ferrocyanide complexes containing coarse particles reducing efficiency and potential leakage.
A composite electrolyte membrane containing fine metal hexacyanoferrate (M-HCF) particles with a particle size of 3.0 μm or less, dispersed in a solid polymer electrolyte, is used to enhance durability by suppressing radical-induced deterioration.
The composite electrolyte membrane exhibits high durability and reduced radical-induced deterioration, maintaining efficient hydrogen peroxide decomposition even with a lower content of M-HCF particles, preventing leakage and improving the overall performance of electrochemical devices.
Smart Images

Figure 2024163428000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite electrolyte membrane and a membrane electrode assembly, and more particularly to a composite electrolyte membrane containing fine metal hexacyanoferrate (M-HCF) particles, and a membrane electrode assembly including such a composite electrolyte membrane. [Background technology]
[0002] In various electrochemical devices using solid polymer electrolytes, such as soda electrolysis devices, water electrolysis devices, and fuel cells, membrane electrode assemblies (MEAs) are used in the area where electrochemical reactions occur. It is said that MEAs are deteriorated by radicals generated directly by the direct reaction of oxygen and hydrogen, or by radicals generated via electrochemical reactions, or by radicals generated via hydrogen peroxide, due to the attack of the electrolyte. For example, in fuel cells, radical attack is known to increase the resistance of the electrolyte membrane, increase cross leakage, and shorten the lifespan due to thinning. Furthermore, degradation products generated by radical attack may cause catalyst poisoning, which may result in a decrease in electrolytic performance and cell performance.
[0003] In order to solve this problem, various proposals have been made in the past. For example, Patent Document 1 states: (a) mixing an aqueous solution of potassium ferrocyanide with an aqueous solution of a nitrate to produce a ferrocyanide complex; (b) Immersing a fluorine-based electrolyte membrane in a dispersion liquid in which a ferrocyanide complex has been dispersed, thereby causing the fluorine-based electrolyte membrane to swell and become impregnated with the ferrocyanide complex. The electrolyte membrane obtained by the above process is disclosed. The document describes that the electrolyte membrane obtained in this manner has improved durability against hydrogen peroxide (lower F emission) compared to an untreated electrolyte membrane.
[0004] In Non-Patent Document 1, K n [Fe(CN) 6] (n=3, 4) is added to a membrane solution, which is then dried and washed with an acid to obtain an electrolyte membrane. The document states that the electrolyte membrane thus obtained is highly durable.
[0005] As described in Patent Document 1, when an aqueous solution of potassium ferrocyanide is mixed with an aqueous solution of a nitrate salt containing a metal element M, particles of a ferrocyanide complex are generated. Since the ferrocyanide complex particles have the ability to decompose hydrogen peroxide, adding the particles to an electrolyte membrane can suppress deterioration of the electrolyte membrane caused by radicals. However, the ferrocyanide complex particles thus obtained usually contain not only fine particles but also coarse particles. As the proportion of coarse particles contained in the ferrocyanide complex particles increases, the specific surface area of the particles decreases, which may result in a decrease in the efficiency of decomposing hydrogen peroxide.
[0006] In addition, Non-Patent Document 1 states that K n [Fe(CN) 6 It is described that the durability of the electrolyte membrane is improved by adding K n [Fe(CN) 6 ] is protonated H n [Fe(CN) 6 ] is a water-soluble compound. n [Fe(CN) 6 When a fuel cell was fabricated using an electrolyte membrane containing n [Fe(CN) 6 There is a concern that this will become protonated and leak out. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 6665714 [Non-patent literature]
[0008] [Non-Patent Document 1] Liu, X. et al., J. Memb. Sci., 2021, 629, 119282 Summary of the Invention [Problem to be solved by the invention]
[0009] The problem to be solved by the present invention is to provide a composite electrolyte membrane containing fine metal hexacyanoferrate (M-HCF) particles. Another object of the present invention is to provide a membrane electrode assembly including such a composite electrolyte membrane. [Means for solving the problem]
[0010] In order to solve the above problems, the composite electrolyte membrane according to the present invention comprises: A solid polymer electrolyte; M-HCF particles dispersed in the solid polymer electrolyte; Equipped with The M-HCF particles are A metal hexacyanoferrate containing at least one metal element M belonging to groups 3 to 15, D 90 (particle size when the cumulative distribution of particle size on a volume basis is 90%) is 3.0 μm or less.
[0011] The membrane electrode assembly according to the present invention comprises: An electrolyte membrane; an anode catalyst layer bonded to one surface of the electrolyte membrane; a cathode catalyst layer bonded to the other surface of the electrolyte membrane; Equipped with The electrolyte membrane is made of the composite electrolyte membrane according to the present invention. Effect of the Invention
[0012] When ions of metal element M are added to a solution in which a solid polymer electrolyte is dissolved or dispersed, and then ferrocyanide ions and / or ferricyanide ions are further added, fine M-HCF particles are generated in the solution. When this solution is coated on a substrate and dried, a composite electrolyte membrane containing fine M-HCF particles is obtained.
[0013] The composite electrolyte membrane thus obtained contains a smaller proportion of coarse M-HCF particles than composite electrolyte membranes produced by other methods, and therefore the composite electrolyte membrane of the present invention exhibits high durability even when the content of M-HCF particles is small. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a graph showing the total F discharge amount of the composite electrolyte membranes obtained in Examples 1 and 2 and Comparative Example 1. [Diagram 2] FIG. 2 is a graph showing the particle size distribution of the Ce-HCF particles obtained in Example 3 and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] [Configuration 1] A solid polymer electrolyte; M-HCF particles dispersed in the solid polymer electrolyte; Equipped with The M-HCF particles are A metal hexacyanoferrate containing at least one metal element M belonging to groups 3 to 15, D 90 (particle size when the cumulative distribution of particle size by volume is 90%) is 3.0 μm or less Composite electrolyte membrane.
[0016] [Configuration 2] 2. The composite electrolyte membrane according to claim 1, wherein the solid polymer electrolyte is a fluorine-based polymer electrolyte.
[0017] [Configuration 3] 3. The composite electrolyte membrane according to claim 1 or 2, wherein the content of the M-HCF particles is 0.01 mass % or more and 10.0 mass % or less.
[0018] [Configuration 4] The composite electrolyte membrane according to any one of configurations 1 to 3, wherein the metal element M includes at least one selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Ag, In, Sn, Bi, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Tb, and Lu.
[0019] [Configuration 5] An electrolyte membrane; an anode catalyst layer bonded to one surface of the electrolyte membrane; a cathode catalyst layer bonded to the other surface of the electrolyte membrane; Equipped with The electrolyte membrane is made of the composite electrolyte membrane according to any one of configurations 1 to 4. Membrane electrode assembly.
[0020] [Configuration 6] 6. The membrane electrode assembly of claim 5, wherein the M-HCF particles include Ce-HCF particles.
[0021] An embodiment of the present invention will be described in detail below. [1. Composite electrolytes] The composite electrolyte membrane according to the present invention is A solid polymer electrolyte; M-HCF particles dispersed in the solid polymer electrolyte; It is equipped with:
[0022] [1.1. Solid polymer electrolyte] In the present invention, the material of the solid polymer electrolyte is not particularly limited. The solid polymer electrolyte may be either a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte, and the composite electrolyte may contain either one of these solid polymer electrolytes, or may contain two or more of them. In order to obtain high durability, the solid polymer electrolyte is preferably a fluorine-based polymer electrolyte.
[0023] The type of acid group contained in the solid polymer electrolyte is not particularly limited. Examples of the acid group include a sulfonic acid group, a carboxylic acid group, a phosphonic acid group, and a sulfonimide group. The solid polymer electrolyte may contain only one of these acid groups, or may contain two or more of them.
[0024] Examples of fluorine-based polymer electrolytes include Nafion (registered trademark), Flemion (registered trademark), Aquivion (registered trademark), and Aciplex (registered trademark). The fluorine-based polymer electrolyte may be a fully fluorine-based electrolyte that does not contain a C—H bond in the polymer structure, or may be a partially fluorine-based electrolyte that contains a C—H bond and a C—F bond in the polymer structure.
[0025] Examples of the hydrocarbon-based polymer electrolyte include: (a) Polyetheretherketone, polysulfone, polyethersulfone, polyimide, polyphenylene, polyamide, polyamideimide, or a wholly aromatic hydrocarbon-based polymer electrolyte comprising a derivative thereof, into which an acid group such as a sulfonic acid group has been introduced; (b) partially aromatic hydrocarbon-based polymer electrolytes having an aromatic ring in a part of the polymer chain of an aliphatic hydrocarbon-based electrolyte; etc.
[0026] [1.2. M-HCF particles] [1.2.1. Definition] M-HCF particles are dispersed within the solid polymer electrolyte. In the present invention, the term "M-HCF particles" refers to particles containing metal hexacyanoferrate that contains at least one metal element M belonging to groups 3 to 15 of the elements.
[0027] "Metal hexacyanoferrate (M-HCF)" refers to a complex of a counter cation and a ferrocyanide ion or a ferricyanide ion, in which the counter cation is an ion of a metal element M. Specifically, "M-HCF" is a compound in which the valence of the counter cation (ion of metal element M) is n, (a) Ferrocyanide complex in which the oxidation state of the iron ion in the complex ion is II: M m [Fe(CN) 6 ] k rH 2 O (where n×m=4×k, r=0 to 14), or (b) Ferricyanide complex in which the oxidation state of the iron ion in the complex ion is III: M p [Fe(CN) 6 ] q rH 2 O (where n×p=3×q, r=0~14) This refers to.
[0028] [1.2.2. Counter cation] In the present invention, the counter cation is an ion of a metal element M (hereinafter, also referred to as "M ion"). The counter cation may be one type of M ion, or may be two or more types of M ions. However, when the counter cation is two or more types of M ions, the counter cation and an anion (ferrocyanide ion (Fe(II); [Fe(CN) 6 ] 4- ) or ferricyanide ion (Fe(III); [Fe(CN) 6 ] 3- )) must be electrically neutral. Furthermore, when two or more types of M ions are contained as counter cations, these ions do not necessarily form a salt with an integer ratio, and may form a solid solution of any composition as long as electrical neutrality is maintained between the ions and the anions.
[0029] In the present invention, the metal element M is at least one metal element belonging to groups 3 to 15 of the periodic table. The metal element M is preferably at least one metal element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Ag, In, Sn, Bi, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. Moreover, the metal element M is particularly preferably Ce. In other words, the M-HCF particles are particularly preferably Ce-HCF particles.
[0030] M-HCF, which contains metal ions (ions of groups 3 to 15 of the periodic table) as counter cations, is highly effective in suppressing electrolyte deterioration. This is because: (a) These M-HCFs themselves have a large radical inactivation effect, and (b) In the case where M in M-HCF is an element other than M' (e.g., Fe, Cu, etc.) having Fenton activity, when M' ions (e.g., Fe ions, Cu ions, etc.) are introduced from the outside, M in M-HCF and M' ions are exchanged, and M' is fixed as M'-HCF and inactivated. It is thought that.
[0031] [1.2.3. Specific examples of M-HCF] Examples of M-HCF include the following: (1) Ti-HCF: Ti[Fe(CN) 6 ]·2H 2 O., etc. (2) V-HCF: V 1.5 [Fe(CN) 6 ] etc. (3) Cr-HCF: Cr[Fe(CN) 6 ], K 2 Cr[Fe(CN) 6 ], Cr 2 [Fe(CN) 6 ] etc.
[0032] (4) Mn-HCF: KMn[Fe(CN) 6 ] 2 2H 2 O, Mn 2 [Fe(CN) 6 ], Mn2 [Fe(CN) 6 ]·0.5H 2 O、Mn 2 [Fe(CN) 6 ]·4H 2 O、Cs 2 Mn 2 [Fe(CN) 6 ]、Cs 2 Mn 2 [Fe(CN) 6 ]·4H 2 O、Cs 4 Mn 4 [Fe(CN) 6 ] 3 etc. (5)Fe-HCF: Fe 4 [Fe(CN) 6 ] 3 、Fe 2 [Fe(CN) 6 ] etc. (6)Co-HCF: Cs 2 Co[Fe(CN) 6 ] 2 、Cs 4 Co 4 [Fe(CN) 6 ] 6 、Co 2 [Fe(CN) 6 ]、Co 3 [Fe(CN) 6 ] 2 ·3H 2 O、Co 3 [Fe(CN) 6 ] 2 ·10H 2 O、Co 2 [Fe(CN) 6 ]·2H 2 O、Co 2 [Fe(CN) 6 ]·10H 2 O、(Co,Na) 2 [Fe(CN) 6 ]·3H 2 O、(Co,Na)Zn[Fe(CN) 6 ]·3H 2 O、Na 2 Co[Fe(CN) 6 ]、K 2 Co[Fe(CN)6 ]など。
[0033] (7)Ni-HCF: Ni 3 [Fe(CN) 6 ] 2 ·10H 2 O、KNi[Fe(CN) 6 ]、Na 2 Ni[Fe(CN) 6 ]、Na 2 Ni[Fe(CN) 6 ]·3H 2 Oなど。 (8)Cu-HCF: Cu 2 [Fe(CN) 6 ]、Cu 4 [Fe(CN) 6 ]、Cu 3 [Fe(CN) 6 ] 2 、Cu 3 [Fe(CN) 6 ]など。 (9)Zn-HCF: Zn 3 [Fe(CN) 6 ] 2 、Zn 2 [Fe(CN) 6 ]、Zn 3 [Fe(CN) 6 ] 2 ·xH 2 O、Cs 2 Zn 3 [Fe(CN) 6 ] 2 ·6H 2 Oなど。 (10)Zr-HCF:Zr[Fe(CN) 6 ]、Zr[Fe(CN) 6 ]·2H 2 Oなど。
[0034] (11)Ag-HCF: Ag 4 [Fe(CN) 6 ]、K 2 Ag 2 [Fe(CN) 6 ]·2H 2 O、Cu 3 Ag x Fe y[Fe(CN) 6 ] 2 (x+y=1)、(NH 4 ) 2 Ag 2 [Fe(CN) 6 ]·2.5H 2 O、Ag 3 Co[Fe(CN) 6 ] etc. (12)In-HCF: In 4 [Fe(CN) 6 ] 3 ·10H 2 O、CsIn[Fe(CN) 6 ] 3 ·2H 2 Oh (13)Sn-HCF: Sn 2 [Fe(CN) 6 ]·3.33H 2 Oh
[0035] (14)Bi-HCF: Bi 4 [Fe(CN) 6 ] 3 、BiK[Fe(CN) 6 ] etc. (15)La-HCF: La[Fe(CN) 6 ]·5H 2 O、CsLa[Fe(CN) 6 ]·H 2 Oh (16)Ce-HCF: Ce[Fe(CN) 6 ]、Ce 4 [Fe(CN) 6 ] 3 、CsCe[Fe(CN) 6 ]、CsCe[Fe(CN) 6 ]·H 2 Oh, Ce 4 [Fe(CN) 6 ] 3 ·14H 2 Oh
[0036] (17)Pr-HCF: Pr 4 [Fe(CN) 6 ] 3 、Pr[Fe(CN) 6]、Pr 4 [Fe(CN) 6 ] 3 ·10H 2 The CsPr[Fe(CN) 6 ]·5H 2 Oなど。 (18)Nd-HCF: Nd[Fe(CN) 6 ]、Nd[Fe(CN) 6 ]·4H 2 O、Nd 4 [Fe(CN) 6 ] 3 、CsNd[Fe(CN) 6 ]·5H 2 The KNd[Fe(CN) 6 ]など。 (19)Sm-HCF: Sm[Fe(CN) 6 ]·4H 2 O、CsSm[Fe(CN) 6 ]·5H 2 Oなど。
[0037] (20)Eu-HCF: Eu 4 [Fe(CN) 6 ] 3 、I[Fe(CN) 6 ]など。 (21)Gd-HCF: Gd 4 [Fe(CN) 6 ] 3 、Gd[Fe(CN) 6 ]、CsGd[Fe(CN) 6 ]·4H 2 The KGd[Fe(CN) 6 ]·4H 2 Oなど。 (22)Tb-HCF: Tb 4 [Fe(CN) 6 ] 3 、Tb[Fe(CN) 6 ]など。
[0038] (23)Dy-HCF: Dy 4 [Fe(CN) 6 ] 3 、Dy[Fe(CN) 6 ]など。 (24)Ho-HCF: Ho 4 [Fe(CN) 6 ] 3 , Ho[Fe(CN) 6 ] etc. (25)Er-HCF: Er 4 [Fe(CN) 6 ] 3 , Er[Fe(CN) 6 ], Er[Fe(CN) 6 ]·10H 2 O., etc.
[0039] (26)Tm-HCF: Tm 4 [Fe(CN) 6 ] 3 , Tm[Fe(CN) 6 ] etc. (27)Yb-HCF: Yb 4 [Fe(CN) 6 ] 3 , Yb[Fe(CN) 6 ] etc. (28)Lu-HCF: Lu 4 [Fe(CN) 6 ] 3 , Lu[Fe(CN) 6 ] etc.
[0040] [1.2.4.D 90 ] "D 90 " refers to the particle size of M-HCF particles when the cumulative distribution of volume-based particle size is 90% when particle size distribution is measured using a laser diffraction scattering method. The M-HCF particles according to the present invention are produced using the method described below, and therefore have a smaller D 90 By optimizing the manufacturing conditions, the D of M-HCF particles is 90 is 3.0 μm or less.
[0041] [1.2.5. Content of M-HCF particles] "M-HCF particle content" refers to the ratio of the mass of M-HCF particles to the total dry mass of the composite electrolyte membrane.
[0042] The greater the content of M-HCF particles, the more the radical degradation of the solid polymer electrolyte is suppressed. To obtain such an effect, the content of M-HCF particles is preferably 0.01 mass% or more. The content is more preferably 0.05 mass% or more, or 0.10 mass% or more. On the other hand, if the content of M-HCF particles is excessive, the mechanical strength of the composite electrolyte membrane may decrease, or the proton conductivity may decrease. Therefore, the content of M-HCF particles is preferably 10.0 mass% or less. The content is more preferably 5.0 mass% or less, or 3.0 mass% or less.
[0043] [1.3. Reinforcement materials] The composite electrolyte membrane according to the present invention may consist of only a solid polymer electrolyte and M-HCF particles, or may be a composite of these with a reinforcing material. In this case, the type of the reinforcing material is not particularly limited. Examples of the reinforcing material include: (a) Porous membranes and nonwoven fabrics of fluororesins such as polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), perfluoroethylenepropene copolymer (FEP), and ethylenetetrafluoroethylene copolymer (ETFE); (b) Porous membranes and nonwoven fabrics of hydrocarbon resins such as polyethylene (PE) and polypropylene (PP), etc.
[0044] [2. Membrane electrode assembly] The membrane electrode assembly according to the present invention comprises: An electrolyte membrane; an anode catalyst layer bonded to one surface of the electrolyte membrane; a cathode catalyst layer bonded to the other surface of the electrolyte membrane; It is equipped with:
[0045] [2.1. Electrolyte membrane] In the membrane electrode assembly according to the present invention, the electrolyte membrane is made of the composite electrolyte membrane according to the present invention. The M-HCF particles contained in the composite electrolyte membrane are preferably Ce-HCF particles. Other points regarding the composite electrolyte membrane are as described above, and therefore will not be described here.
[0046] [2.2. Anode catalyst layer, cathode catalyst layer] The anode catalyst layer and the cathode catalyst layer each comprise a composite of an electrode catalyst and a catalyst layer ionomer. In the present invention, the material and content of the electrode catalyst and the catalyst layer ionomer are not particularly limited, and an optimum material can be selected depending on the purpose.
[0047] [3. Manufacturing method of composite electrolyte membrane] The composite electrolyte according to the present invention comprises: (a) a first step of adding ions of a metal element M to a solution in which a solid polymer electrolyte is dissolved or dispersed to obtain a first solution; (b) a second step of further adding ferrocyanide ions and / or ferricyanide ions to the first solution to obtain a second solution; (c) a third step of coating the second solution on a substrate and drying the coating; It is equipped with:
[0048] [3.1. 1st step] First, ions of a metal element M are added to a solution in which a solid polymer electrolyte is dissolved or dispersed (first step), thereby obtaining a first solution containing the solid polymer electrolyte and M ions.
[0049] The concentration of the solid polymer electrolyte and the concentration of the M ions in the first solution are not particularly limited, and optimal concentrations can be selected depending on the purpose. The raw material of the M ion may be any material that is soluble in a solvent for dissolving or dispersing the solid polymer electrolyte. Examples of the raw material of the M ion include nitrates, chlorides, sulfates, perchlorates, and acetates.
[0050] [3.2. 2nd process] Next, ferrocyanide ions and / or ferricyanide ions are further added to the first solution (second step). When the ferrocyanide ions and / or ferricyanide ions are added to the first solution, the M ions react with the ferrocyanide ions and / or ferricyanide ions to generate fine M-HCF particles. As a result, a second solution is obtained in which the solid polymer electrolyte and the fine M-HCF particles are dispersed. The amount of ferrocyanide ions and / or ferricyanide ions added to the second solution is not particularly limited, and an optimal amount can be selected depending on the purpose.
[0051] The raw materials for the ferrocyanide ions and ferricyanide ions may be any materials that are soluble in a solvent for dissolving or dispersing the solid polymer electrolyte. Examples of raw materials for ferrocyanide ions and ferricyanide ions include: (a) The counter cation is an alkali metal ion (Li + , Na + , K + , Cs + ) soluble M-HCF, (b) The counter cation is an alkaline earth metal ion (Mg 2+ , Ca 2+ , Sr 2+ , B.A. 2+ ) soluble M-HCF, (c) The counter cation is an Al ion (Al 3+ ), or Ga ions (Ga 3+ ) soluble M-HCF etc.
[0052] [3.3. Third step] Next, the second solution is applied onto a substrate, and the coating is dried (third step). This results in the composite electrolyte according to the present invention. The conditions for applying the solution and the conditions for drying the coating are not particularly limited, and optimal conditions can be selected depending on the purpose.
[0053] [4. Effect] Examples of methods for obtaining a composite electrolyte membrane containing M-HCF particles include (a) a first method in which ferrocyanide ions and / or ferricyanide ions are added to a solution in which a solid polymer electrolyte is dissolved or dispersed, and then ions of a metal M are added to form a solution, which is then coated on a substrate and dried; or (b) A second method in which M-HCF particles and an electrolyte membrane are prepared first, and then the M-HCF particles are added to the electrolyte membrane using various methods. etc.
[0054] However, the composite electrolyte membrane produced using the above method contains a high proportion of coarse M-HCF particles. The reason why coarse M-HCF particles are likely to be formed by the first method is believed to be as follows: Ferrocyanide ions and / or ferricyanide ions are anions, and due to electronic repulsion with the sulfonic acid groups of the solid polymer electrolyte, they are not incorporated into the secondary particles of the electrolyte and remain in the solution. Even if ions of the metal element M are added to this, the solution becomes a reaction field, making it impossible to control the particle size. The reason why coarse M-HCF particles are easily formed by the second method is thought to be as follows: After synthesis of M-HCF, aggregation occurs between particles during the filtration and drying process. This is thought to be because these coarse M-HCF particles are difficult to disperse even in solution.
[0055] In contrast, when ions of metal element M are added to a solution in which a solid polymer electrolyte is dissolved or dispersed, and then ferrocyanide ions and / or ferricyanide ions are further added, fine M-HCF particles are generated in the solution. When this solution is applied to a substrate and dried, a composite electrolyte membrane containing fine M-HCF particles is obtained.
[0056] The composite electrolyte membrane thus obtained contains a smaller proportion of coarse M-HCF particles than composite electrolyte membranes produced by other methods, and therefore the composite electrolyte membrane of the present invention exhibits high durability even when the content of M-HCF particles is small. The reason why the formation of coarse M-HCF particles is suppressed by the method according to the present invention is believed to be as follows. When ions of a metal element M are added to a solid polymer electrolyte solution, H of the sulfonic acid group is + The secondary particles are ion-exchanged with M ions, and M ions are incorporated into the inside and outside of the secondary particles. At this time, there are almost no M ions in the solvent. When ferrocyanide ions and / or ferricyanide ions are then added, the secondary particles of the solid polymer electrolyte become the reaction field to form M-HCF particles, and it is considered that the M-HCF particles are unlikely to have a diameter larger than that of the secondary particles.
[0057] When Fe is mixed into the electrolyte membrane of a fuel cell from the outside, the hydrogen peroxide generated at the electrode reacts with the Fe, generating hydroxyl radicals. As a result, the electrolyte membrane is deteriorated by the radicals. To solve this problem, Ce ions are added to the electrolyte membrane, which makes it easier for hydrogen peroxide to decompose into harmless water and oxygen before it becomes hydroxyl radicals. As a result, deterioration of the electrolyte membrane is suppressed. However, with this method, Ce ions migrate and flow out of areas that require durability during operation, and there are cases where sufficient durability cannot be obtained.
[0058] In contrast, M-HCF has a strong radical inactivation effect by itself and is highly effective in suppressing the deterioration of the electrolyte membrane. Furthermore, when M is a metal element other than Fe (e.g., Ce), when M-HCF comes into contact with Fe ions, M is exchanged with Fe to form Fe-HCF. Therefore, when M-HCF, in which M is a metal element other than Fe, is added to the electrolyte membrane (particularly near the interface with the catalyst layer), Fe that has entered from the outside is exchanged with M in M-HCF, and Fe is immobilized. As a result, it is believed that the radical decomposition of hydrogen peroxide is suppressed and the durability of the electrolyte membrane is improved.
[0059] Furthermore, K, which is the raw material (precursor) for producing M-HCF, 4 [Fe(CN) 6 ] is water-soluble, whereas M-HCF is insoluble or poorly soluble in water, so there is little risk of M-HCF migrating or flowing out of the electrolyte membrane. EXAMPLES
[0060] (Examples 1 to 2, Comparative Example 1) [1. Sample preparation] [1.1. Electrolyte membrane A] Ce(NO 3 ) 3 6H 2 O was added and stirred. Ce(NO 3 ) 3 6H 2 The amount of O added is Ce 3+ The amount was adjusted so that the sulfonic acid group substitution rate with was 1 mol%. Then, 1 equivalent of K was added to the solution. 4 [Fe(CN) 6 ] was added to obtain solution A. Next, the solution A was applied onto the substrate using an applicator. The applied film was vacuum dried at 140° C. for 15 minutes to obtain an electrolyte membrane A containing Ce-HCF particles.
[0061] [1.2. Electrolyte membrane B] Ce(NO 3 ) 3 6H 2 O was added and stirred. Ce(NO 3 ) 3 6H 2 The amount of O added is Ce 3+ The amount was adjusted so that the sulfonic acid group substitution rate with was 2 mol%. Then, 1 equivalent of K was added to the solution. 4 [Fe(CN) 6 ] was added to obtain solution B. Next, an applicator was used to apply solution B onto the substrate. The coating was vacuum-dried at 140° C. for 15 minutes to obtain electrolyte membrane B containing Ce-HCF particles.
[0062] [1.3. Electrolyte membrane C] Nafion® solution (D2020, solid content: 21.5 mass%) containing FeSO 4 The solution was then stirred to obtain solution C. 4The amount of Fe added is 2+ The amount was set so that the sulfonic acid group substitution rate was 1 mol %. Next, an applicator was used to apply the solution C onto the substrate. The coating was dried in vacuum at 140° C. for 15 minutes to obtain an electrolyte membrane C containing Fe ions.
[0063] [1.4. Electrolyte membrane D] Nafion® solution (D2020, solid content: 21.5 mass%) containing FeSO 4 The solution was then stirred to obtain solution D. 4 The amount of Fe added is 2+ The amount was set so that the sulfonic acid group substitution rate was 2 mol%. Next, the solution D was applied onto the substrate using an applicator. The coating was vacuum-dried at 140° C. for 15 minutes to obtain an electrolyte membrane D containing Fe ions.
[0064] [1.5. MEA] The electrolyte membrane A cut into a 2.5 cm square was stacked with the electrolyte membrane C cut into a 2.5 cm square to obtain a laminated electrolyte membrane A. Next, catalyst layers were attached to both sides of the laminated electrolyte membrane A to obtain an MEA (Example 1). The electrolyte membrane B cut into a 2.5 cm square was stacked with the electrolyte membrane D cut into a 2.5 cm square to obtain a laminated electrolyte membrane B. Next, catalyst layers were attached to both sides of the laminated electrolyte membrane B to obtain an MEA (Example 2). Two sheets of the electrolyte membrane C cut into a 2.5 cm square were stacked together to obtain a laminated electrolyte membrane C. Next, catalyst layers were attached to both sides of the laminated electrolyte membrane C to obtain an MEA (Comparative Example 1).
[0065] [2. Test Method and Results] An open circuit test was carried out using the obtained MEA under conditions of 95° C. and 30% RH. After 90 hours, the total amount of F discharged from the MEA (total F discharge amount) was measured. Fig. 1 shows the total F discharge of the composite electrolyte membranes obtained in Examples 1 and 2 and Comparative Example 1. The total F discharge of Example 1 was 0.08 mg@90 hr. The total F discharge of Example 2 was 0.06 mg@90 hr. On the other hand, the total F discharge of Comparative Example 1 was 0.61 mg@90 hr. It can be seen from Fig. 1 that the total F discharge is significantly reduced by adding Ce-HCF particles to the electrolyte membrane.
[0066] (Example 3, Comparative Example 2) [1. Sample preparation] 1.1. Example 3 Solution A prepared in Example 1 was subjected to the test.
[0067] [1.2. Comparative Example 2] A potassium ferrocyanide aqueous solution and a cerium nitrate aqueous solution were mixed, filtered and washed to obtain Ce-HCF particles. This was added to a Nafion (registered trademark) solution (D2020, solid content: 21.5 mass%) to obtain solution G. The amount of Ce-HCF particles added was Ce 3+ The amount was set so that the sulfonic acid group substitution rate was 1 mol %.
[0068] [2. Test Method and Results] The particle sizes of the Ce-HCF particles contained in solutions A and G were measured using a laser diffraction / scattering particle size distribution analyzer (MT3300X, Microtrac (registered trademark)). Figure 2 shows the particle size distributions of the Ce-HCF particles obtained in Example 3 and Comparative Example 2. D of Ce-HCF particles in Example 3 90 On the other hand, the D of the Ce-HCF particles of Comparative Example 2 90 The particle size was 14.8 μm. Figure 2 shows that fine Ce-HCF particles can be obtained by adding Ce ions and ferrocyanide ions in this order to the electrolyte solution.
[0069] (Examples 4 to 5, Comparative Example 3) [1. Sample preparation] [1.1. Electrolyte membrane E] Nafion® solution (D2020, solid content: 21.5 mass%) containing FeSO 4 FeSO was added and stirred. 4 The amount of Fe added is 2+ The amount was adjusted so that the sulfonic acid group substitution rate with was 1 mol%. Then, 1 equivalent of K was added to the solution. 4 [Fe(CN) 6 ] was added to obtain solution E. Next, the solution E was applied onto the substrate using an applicator. The coating was dried in vacuum at 140° C. for 15 minutes to obtain an electrolyte membrane E containing Fe-HCF.
[0070] [1.2. Electrolyte membrane F] Nafion® solution (D2020, solid content: 21.5 mass%) containing FeSO 4 FeSO was added and stirred. 4 The amount of Fe added is 2+ The amount was adjusted so that the sulfonic acid group substitution rate with was 1 mol%. Then, 0.5 equivalents of K 4 [Fe(CN) 6 ] was added to obtain solution F. Next, an applicator was used to apply the solution F onto the substrate. The coating was vacuum-dried at 140° C. for 15 minutes to obtain an electrolyte membrane F containing Fe—HCF.
[0071] [1.3. MEA] A catalyst layer was attached to both sides of the electrolyte membrane E cut into a 2.5 cm square to obtain an MEA (Example 4). A catalyst layer was attached to both sides of the electrolyte membrane F cut into a 2.5 cm square to obtain an MEA (Example 5). Catalyst layers were attached to both sides of the electrolyte membrane C to obtain an MEA (Comparative Example 3).
[0072] [2. Test Method and Results] An open circuit test was carried out using the obtained MEA under conditions of 95° C. and 30% RH. After 90 hours, the total amount of F discharged from the MEA (total F discharge amount) was measured. The total F discharge amount was 0.05 mg@90 hr in Example 4. The total F discharge amount was 0.09 mg@90 hr in Example 5. Meanwhile, the total F discharge amount was 0.39 mg@90 hr in Comparative Example 3. It can be seen that the presence of Fe-HCF in the electrolyte membrane significantly reduces the total F discharge amount.
[0073] Comparative Example 4 [1. Sample preparation] A potassium ferrocyanide aqueous solution and an iron sulfate aqueous solution were mixed, filtered and washed to obtain Fe-HCF particles. The particles were added to a Nafion (registered trademark) solution (D2020, solid content: 21.5 mass%) to obtain solution H. The amount of Fe-HCF particles added was Fe 3+ The amount was set so that the sulfonic acid group substitution rate was 1 mol %.
[0074] [2. Test Method and Results] The particle sizes of the Fe-HCF particles contained in solutions E and H were measured using a laser diffraction / scattering type particle size distribution analyzer (MT3300X, Microtrac (registered trademark)). D of Fe-HCF particles of Example 4 90 On the other hand, the D of the Fe-HCF particles of Comparative Example 4 90 was 252 μm.
[0075] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]
[0076] The composite electrolyte membrane according to the present invention can be used as an electrolyte membrane for a polymer electrolyte fuel cell or a polymer electrolyte water electrolysis device.
Claims
1. A solid polymer electrolyte; M-HCF particles dispersed in the solid polymer electrolyte; Equipped with The M-HCF particles are A metal hexacyanoferrate containing at least one metal element M belonging to Groups 3 to 15, D 90 (particle size when the cumulative distribution of particle size on a volume basis is 90%) is 3.0 μm or less Composite electrolyte membrane.
2. 2. The composite electrolyte membrane according to claim 1, wherein the solid polymer electrolyte is a fluorine-based polymer electrolyte.
3. 2. The composite electrolyte membrane according to claim 1, wherein the content of the M-HCF particles is 0.01 mass % or more and 10.0 mass % or less.
4. 2. The composite electrolyte membrane according to claim 1, wherein the metal element M includes at least one selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Ag, In, Sn, Bi, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Tb, and Lu.
5. An electrolyte membrane; an anode catalyst layer bonded to one surface of the electrolyte membrane; a cathode catalyst layer bonded to the other surface of the electrolyte membrane; Equipped with The electrolyte membrane is made of a composite electrolyte membrane according to any one of claims 1 to 4. Membrane electrode assembly.
6. 6. The membrane electrode assembly according to claim 5, wherein the M-HCF particles include Ce-HCF particles.