Resist composition and patterning method

A tin cluster-based resist composition addresses sensitivity and resolution issues in EUV lithography by providing high sensitivity and improved LWR, suitable for precise microfabrication.

JP2024163579AInactive Publication Date: 2024-11-22SHIN ETSU CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023079324
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing resist compositions face challenges in achieving high sensitivity, resolution, and line width roughness (LWR) in photolithography, particularly in EUV lithography, due to issues like acid diffusion, shot noise, and insufficient solubility, which affect pattern formation and device performance.

Method used

A resist composition containing a tin cluster compound with a specific structure, combined with an organic solvent, forms the basis of a non-chemically amplified resist that exhibits high sensitivity and resolution, improving LWR through high EUV absorption and thermal stability.

Benefits of technology

The resist composition achieves fine pattern formation with high sensitivity and resolution, reducing shot noise effects and enhancing LWR, suitable for precise microfabrication in EUV lithography.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a resist composition with superior sensitivity, resolution and LWR in photolithography using high energy rays, and a patterning method using the resist composition.SOLUTION: A resist composition contains a tin compound represented by the formula (1) and an organic solvent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resist composition and a pattern forming method. [Background technology]

[0002] As the IoT market expands, there is a growing demand for higher integration, higher speeds, and lower power consumption in LSIs, and pattern rule miniaturization is progressing rapidly. In particular, logic devices are driving miniaturization. As cutting-edge miniaturization technologies, 10nm node devices are being mass-produced using double patterning, triple patterning, and quadruple patterning of ArF immersion lithography, and studies are underway to produce 7nm node devices using next-generation extreme ultraviolet (EUV) lithography with a wavelength of 13.5nm.

[0003] As miniaturization progresses, image blurring due to acid diffusion has become a problem (Non-Patent Document 1). In order to ensure resolution in fine patterns for the 45 nm generation and beyond, it has been proposed that control of acid diffusion is important in addition to improving dissolution contrast, as has been proposed in the past (Non-Patent Document 2). However, since chemically amplified resist compositions increase sensitivity and contrast through acid diffusion, if one tries to suppress acid diffusion to the maximum extent possible by lowering the post-exposure bake (PEB) temperature or shortening the time, the sensitivity and contrast will decrease significantly.

[0004] It is effective to suppress acid diffusion by adding an acid generator that generates a bulky acid. Therefore, it has been proposed to copolymerize an acid generator of an onium salt having a polymerizable olefin with a polymer. However, in the pattern formation of resist films for the 16 nm generation and beyond, it is thought that pattern formation cannot be achieved with chemically amplified resist materials from the viewpoint of acid diffusion, and the development of a non-chemically amplified resist composition is desired.

[0005] One example of a material for non-chemically amplified resist compositions is polymethyl methacrylate (PMMA). PMMA is a positive resist material in which the main chain is cut by electron beam (EB) or EUV irradiation, decreasing the molecular weight and improving the solubility in organic solvent developers. However, PMMA has the disadvantages of having low etching resistance and large outgassing during exposure because it does not have a ring structure.

[0006] Hydrogen silsesquioxane (HSQ) is a negative resist material that becomes insoluble in alkaline developer due to crosslinking caused by condensation reaction of silanols generated by EB or EUV irradiation. Chlorine-substituted calixarenes also function as negative resist materials. These negative resist materials have small molecular size before crosslinking and no blurring due to acid diffusion, so they have small edge roughness and very high resolution, and are used as pattern transfer materials to indicate the resolution limit of exposure equipment. However, these materials have insufficient sensitivity and further improvement is required.

[0007] One of the factors that makes it difficult to develop materials for EUV lithography is the small number of photons in EUV exposure. The energy of EUV is much higher than that of ArF excimer laser light, and the number of photons in EUV exposure is one-fourteenth of that in ArF exposure. Furthermore, the dimensions of the pattern formed by EUV exposure are less than half that of ArF exposure. For this reason, EUV exposure is easily affected by the variation in the number of photons. The variation in the number of photons in the extremely short wavelength radiation light region is a physical phenomenon called shot noise, and this effect cannot be eliminated. For this reason, so-called stochastics has attracted attention. Although the effect of shot noise cannot be eliminated, how to reduce this effect is being discussed. Not only does the shot noise increase the dimensional uniformity (CDU) and line width roughness (LWR), but the phenomenon of hole blockage has been observed with a probability of one in several million. When holes are blocked, electrical conduction is poor and the transistor does not work, which has a negative effect on the performance of the entire device.

[0008] As a method for reducing the effect of shot noise on the resist side, an inorganic resist composition that uses an element with high EUV absorption as a core has been proposed (Patent Document 1). However, although inorganic resist compositions have relatively high sensitivity, they are still not sufficient, and they have many problems such as insufficient solubility in resist solvents, storage stability, and defects.

[0009] Non-Patent Document 3 proposes a negative resist composition using a tin compound. This is a non-chemically amplified resist whose main component is tin, which has high EUV light absorption, and although the stochastics have been improved and a certain degree of improvement in sensitivity and resolution has been achieved, it is still insufficient, and there is a strong demand for the development of a further improved product. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2015-108781 A [Non-patent literature]

[0011] [Non-Patent Document 1] SPIE Vol. 5039, p1 (2003) [Non-Patent Document 2] SPIE Vol. 6520, p65203L-1 (2007) [Non-Patent Document 3] SPIE Vol. 9051, p90511B-1 (2014) Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a resist composition that exhibits excellent sensitivity, resolution, and LWR in photolithography using high-energy rays, particularly EUV lithography, and a pattern formation method using the resist composition. [Means for solving the problem]

[0013] As a result of intensive research into achieving the above-mentioned object, the inventors have discovered that a resist composition containing as a main component a tin cluster compound having a specific structure provides a resist film that has high sensitivity, and exhibits excellent resolution and LWR, and is extremely effective for precise microfabrication, which has led to the completion of the present invention.

[0014] That is, the present invention provides the following resist composition and pattern forming method. 1. A resist composition comprising a tin compound represented by the following formula (1) and an organic solvent: [ka] (In the formula, R 1A ~R 10A and R 1B ~R 10B are each independently a hydrocarbyl group having 1 to 20 carbon atoms. R 11 ~R 14 are each independently a hydrogen atom or a hydrocarbyl group having 1 to 20 carbon atoms. L a1 and L a2 are each independently a linking group. 2.L a1 and L a2 are each independently a group represented by any one of the following formulas (2a) to (2d): [ka] (In the formula, the dashed line represents a bond to Sn.) 3.R 1A ~R 10A and R 1B ~R 10B The resist composition of 1 or 2, wherein 4. The resist composition according to any one of 1 to 3, further comprising a surfactant. 5. A pattern forming method comprising the steps of forming a resist film on a substrate using the resist composition according to any one of 1 to 4, exposing the resist film to high-energy rays, and developing the exposed resist film using a developer. 6. The pattern formation method according to 5, wherein the high energy radiation is EB or EUV. Effect of the Invention

[0015] INDUSTRIAL APPLICABILITY The resist composition of the present invention is extremely useful in forming fine patterns in photolithography using high-energy rays, particularly EUV lithography, because it achieves both high sensitivity and high resolution and has excellent LWR. [Brief description of the drawings]

[0016] [Figure 1] 1 is a 1H-NMR spectrum of the tin compound M-1 obtained in Synthesis Example 1. [Diagram 2] 1 is a 119Sn-NMR spectrum of the tin compound M-1 obtained in Synthesis Example 2. [Diagram 3] 1 is a SEM image showing a line and space (LS) pattern with a space width of 20 nm and a pitch of 40 nm at Eop in Example 2-1. [Figure 4] 1 shows the results of plotting the relationship between film thickness and exposure dose for the resist film prepared in Example 3 (contrast curve and PEB shrink). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] [Resist composition] The resist composition of the present invention contains a predetermined tin compound and an organic solvent.

[0018] [Tin compounds] The tin compound is the main component of the resist composition of the present invention, and is represented by the following formula (1): In the present invention, the main component means the component other than the solvent that is contained in the largest amount. [ka]

[0019] In formula (1), R 1A ~R 10A and R 1B ~R 10B R is each independently a hydrocarbyl group having 1 to 20 carbon atoms. 11 ~R 14 are each independently a hydrogen atom or a hydrocarbyl group having 1 to 20 carbon atoms. a1 and L a2 are each independently a linking group.

[0020] R 1A ~R 10A , R 1B ~R 10B and R 11 ~R 14 The hydrocarbyl group having 1 to 20 carbon atoms and represented by the formula (I) may be saturated or unsaturated, and may be linear, branched or cyclic. Specific examples thereof include alkyl groups having 1 to 1,020 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, a tert-pentyl group, an n-pentyl group, an n-hexyl group, an n-octyl group, a 2-ethylhexyl group, an n-nonyl group, and an n-decyl group; a cyclopentyl group, a cyclohexyl group, a cyclopentylmethyl group, a cyclopentylethyl group, a cyclopentylbutyl group, a cyclohexylmethyl group, a cyclohexylethyl group, a cyclohexylbutyl group, a norbornyl group, a tricyclo[5.2.1.0 2,6 ]Cyclic saturated hydrocarbyl groups having 3 to 20 carbon atoms, such as a decyl group, an adamantyl group, an adamantylmethyl group, etc.; alkenyl groups having 2 to 20 carbon atoms, such as a vinyl group, an allyl group, etc.; aryl groups having 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, etc.; aralkyl groups having 7 to 20 carbon atoms, such as a benzyl group, a phenethyl group, etc.; and groups obtained by combining these.

[0021] In addition, some or all of the hydrogen atoms of the hydrocarbyl group may be substituted with a group containing a heteroatom such as an oxygen atom, a sulfur atom, a nitrogen atom or a halogen atom, and some of the -CH2- of the hydrocarbyl group may be substituted with a group containing a heteroatom such as an oxygen atom, a sulfur atom or a nitrogen atom, and as a result, the hydrocarbyl group may contain a hydroxy group, a cyano group, a halogen atom, a carbonyl group, an ether bond, a thioether bond, an ester bond, a sulfonate ester bond, a carbonate bond, a carbamate bond, a lactone ring, a sultone ring, a carboxylic acid anhydride (-C(=O)-OC(=O)-), etc.

[0022] R is popular because the raw materials are readily available and it is easy to manufacture. 1A ~R 10A are the same group, and R 1B ~R 10B are preferably the same group, and R 1A ~R 10A and R 1B ~R 10B It is preferred that all of the groups are the same.

[0023] R 1A ~R 10A and R 1B ~R 10B As R, an isopropyl group, an n-butyl group, a tert-butyl group, a benzyl group, etc. are preferable, and an n-butyl group, a t-butyl group, a benzyl group, etc. are more preferable. 11 ~R 14 is preferably a hydrogen atom or a methyl group.

[0024] L a1 and L a2 Examples of the linking group represented by the formula include groups represented by any of the following formulas (2a) to (2d). [ka] (In the formula, the dashed line represents a bond to Sn.)

[0025] Specific examples of the tin compound represented by formula (1) include, but are not limited to, those shown below, in which Bn is a benzyl group, nBu is an n-butyl group, tBu is a tert-butyl group, iPr is an isopropyl group, and Me is a methyl group. [ka]

[0026] [ka]

[0027] [ka]

[0028] [ka]

[0029] [ka]

[0030] [ka]

[0031] [ka]

[0032] [ka]

[0033] The tin compound represented by formula (1) may be used alone or in combination of two or more kinds. From the viewpoint of improving the uniformity of the components, it is preferable to use one kind alone or two kinds in combination.

[0034] The tin compound represented by formula (1) can be synthesized with reference to Z. Naturforsch. 2010, 65b, 1293-1300, Inorg. Chim. Acta 357, (9), 2791-2797, 2004, and the like.

[0035] [Organic solvents] The resist composition of the present invention contains an organic solvent. The solvent is not particularly limited as long as it can dissolve the tin compound represented by formula (1) and form a film. Examples of such organic solvents include ketones such as cyclohexanone and methyl-2-n-pentyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, and diacetone alcohol (DAA); ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; and propylene glycol monomethyl ether. Examples of the solvent include esters such as ether acetate (PGMEA), propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 2-hydroxyisobutyrate, tert-butyl acetate, cyclohexyl acetate, tert-butyl propionate, and propylene glycol mono tert-butyl ether acetate; lactones such as γ-butyrolactone; carboxylic acids such as acetic acid and propionic acid, aromatics such as toluene, xylene, cresol, anisole, and benzotrifluoride; and mixed solvents of these.

[0036] The content of the organic solvent is preferably from 200 to 20,000 parts by mass, and more preferably from 500 to 10,000 parts by mass, relative to 100 parts by mass of the tin compound represented by formula (1).

[0037] The resist composition of the present invention is a so-called molecular resist composition, which is a resist composition that is mainly composed of a low molecular weight compound and does not contain a base polymer used in a polymer-based resist composition. It is presumed that the resist composition of the present invention changes in solvent solubility and becomes insoluble in a developer due to photolysis of the tin compound, which is the main component, and the subsequent crosslinking reaction. Since this reaction is not a catalytic reaction, the resist composition of the present invention functions as a non-chemically amplified resist composition. Therefore, the limiting resolution is improved compared to conventional chemically amplified resist compositions mainly composed of multi-component polymers. In particular, in EUV lithography, tin atoms have high EUV absorption ability, so Stochastics is improved, and a resist material with excellent sensitivity and LWR can be provided.

[0038] The tin compound is a 10-nuclear tin complex, i.e., a cluster compound. The thermally stable cluster structure provides excellent storage stability. The aforementioned Non-Patent Document 3 exemplifies a tin cluster compound of a 12-nuclear complex, which also has the advantage of being thermally stable, but has low solubility in organic solvents. In this case, there is concern that precipitation and deterioration of film-forming properties may occur over time when the resist composition is stored for a long period of time. On the other hand, the tin compound has excellent solvent solubility. The reason for this is unclear, but it is believed that the L a1 and L a2 It is presumed that the presence of the linker moiety (i.e., the linker portion) reduces the rigidity of the cluster structure, which contributes to the solvent solubility. In addition, the tin compound has a characteristic that the film shrinks greatly during exposure. The pattern obtained by exposure can be made finer by shrinking, and it is also denser, so that defects such as pattern collapse and line breakage are no longer observed even in fine lines, and the limit resolution is improved. The film shrink is preferably 20% or more, more preferably 30% or more, and even more preferably 50% or more.

[0039] The resist composition of the present invention may contain a surfactant as another component. As the surfactant, a fluorine-based and / or silicone-based surfactant is preferable. As such a surfactant, the surfactants described in paragraph

[0276] of US Patent Application Publication No. 2008 / 0248425 can be used. These may be used alone or in combination of two or more. Furthermore, in the present invention, surfactants other than the fluorine-based and / or silicone-based surfactants described in paragraph

[0280] of US Patent Application Publication No. 2008 / 0248425 can also be used. When the resist composition of the present invention contains a surfactant, the content thereof is preferably 0.001 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the tin compound. The surfactants may be used alone or in combination of two or more.

[0040] [Pattern formation method] When the resist composition of the present invention is used for manufacturing various integrated circuits, known lithography techniques can be applied.For example, as a pattern forming method, the method includes the steps of forming a resist film on a substrate using the resist composition described above, exposing the resist film to high-energy radiation, and developing the exposed resist film using a developer.

[0041] First, the resist composition of the present invention is applied to a substrate for manufacturing integrated circuits (Si, SiO2, SiN, SiON, TiN, WSi, BPSG, SOG, organic anti-reflective film, etc.) or a substrate for manufacturing mask circuits (Cr, CrO, CrON, MoSi2, SiO2, etc.) by a suitable coating method such as spin coating, roll coating, flow coating, dip coating, spray coating, doctor coating, etc., so that the coating thickness is 0.01 to 2 μm. This is pre-baked on a hot plate, preferably at 60 to 150° C. for 10 seconds to 30 minutes, more preferably at 80 to 120° C. for 30 seconds to 20 minutes, to form a resist film.

[0042] Next, the resist film is exposed to high-energy radiation. Examples of the high-energy radiation include ultraviolet radiation, far-ultraviolet radiation, EB, EUV, X-rays, soft X-rays, excimer laser light, gamma rays, and synchrotron radiation. When ultraviolet radiation, far-ultraviolet radiation, EUV, X-rays, soft X-rays, excimer laser light, gamma rays, and synchrotron radiation are used as the high-energy radiation, the exposure dose is preferably 1 to 200 mJ / cm2, either directly or using a mask for forming a desired pattern. 2 Approximately, more preferably 10 to 100 mJ / cm 2 When EB is used as the high energy beam, the exposure dose is preferably 0.1 to 5000 μC / cm 2 either directly or using a mask for forming a desired pattern. 2 Approximately, more preferably 0.5 to 4000 μC / cm 2 The resist composition of the present invention is particularly suitable for fine patterning using high-energy rays such as KrF excimer laser light, ArF excimer laser light, EB, EUV, X-rays, soft X-rays, γ-rays, and synchrotron radiation, and is particularly suitable for fine patterning using EB or EUV.

[0043] The resist composition of the present invention may be subjected to post-exposure baking (PEB) in order to accelerate or complete the reaction after photodecomposition. When PEB is performed, it is preferable to perform it on a hot plate or in an oven after exposure under conditions of preferably 30 to 200° C., 10 seconds to 30 minutes, more preferably 60 to 180° C., 30 seconds to 20 minutes.

[0044] After exposure or PEB, development is performed using an organic solvent. Development is performed on the exposed resist film for 3 seconds to 3 minutes, preferably 5 seconds to 2 minutes, by a conventional method such as a dip method, a puddle method, or a spray method, to form a desired pattern. Since the resist composition of the present invention is a negative type, the portion irradiated with light becomes insoluble in the developer, and the portion not exposed to light dissolves.

[0045] The organic solvents used as developers include 2-octanone, 2-nonanone, 2-heptanone, 3-heptanone, 4-heptanone, 2-hexanone, 3-hexanone, diisobutyl ketone, methylcyclohexanone, acetophenone, methylacetophenone, propyl acetate, butyl acetate, isobutyl acetate, pentyl acetate, butenyl acetate, isopentyl acetate, propyl formate, cyclohexyl acetate, butyl formate, isobutyl formate, pentyl formate, isopentyl formate, methyl valerate, methyl pentenoate, methyl crotonate, methyl chloroform ... Examples of the organic solvent include ethyl lactate, methyl propionate, ethyl propionate, ethyl 3-ethoxypropionate, methyl lactate, ethyl lactate, propyl lactate, butyl lactate, isobutyl lactate, pentyl lactate, isopentyl lactate, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, methyl benzoate, ethyl benzoate, phenyl acetate, benzyl acetate, methyl phenylacetate, ethyl phenylacetate, benzyl formate, phenylethyl formate, methyl 3-phenylpropionate, benzyl propionate, 2-phenylethyl acetate, etc. These organic solvents may be used alone or in combination of two or more.

[0046] After development, rinsing is performed as necessary. As the rinsing liquid, a solvent that is miscible with the developer and does not dissolve the resist film is preferable. As such a solvent, alcohols having 3 to 10 carbon atoms, ether compounds having 8 to 12 carbon atoms, alkanes, alkenes, alkynes, and aromatic solvents having 6 to 12 carbon atoms are preferably used.

[0047] Examples of the alcohol having 3 to 10 carbon atoms include n-propyl alcohol, isopropyl alcohol, 1-butyl alcohol, 2-butyl alcohol, isobutyl alcohol, tert-butyl alcohol, 1-pentanol, 2-pentanol, 3-pentanol, tert-pentyl alcohol, neopentyl alcohol, 2-methyl-1-butanol, 3-methyl-1-butanol, 3-methyl-3-pentanol, cyclopentanol, 1-hexanol, 2-hexanol, 3-hexanol, Examples of such alcohols include 2,3-dimethyl-2-butanol, 3,3-dimethyl-1-butanol, 3,3-dimethyl-2-butanol, 2-ethyl-1-butanol, 2-methyl-1-pentanol, 2-methyl-2-pentanol, 2-methyl-3-pentanol, 3-methyl-1-pentanol, 3-methyl-2-pentanol, 3-methyl-3-pentanol, 4-methyl-1-pentanol, 4-methyl-2-pentanol, 4-methyl-3-pentanol, cyclohexanol, and 1-octanol.

[0048] Examples of the ether compound having 8 to 12 carbon atoms include di-n-butyl ether, diisobutyl ether, di-sec-butyl ether, di-n-pentyl ether, diisopentyl ether, di-sec-pentyl ether, di-tert-pentyl ether, and di-n-hexyl ether.

[0049] Examples of the alkanes having 6 to 12 carbon atoms include hexane, heptane, octane, nonane, decane, undecane, dodecane, methylcyclopentane, dimethylcyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, cycloheptane, cyclooctane, cyclononane, etc. Examples of the alkenes having 6 to 12 carbon atoms include hexene, heptene, octene, cyclohexene, methylcyclohexene, dimethylcyclohexene, cycloheptene, cyclooctene, etc. Examples of the alkynes having 6 to 12 carbon atoms include hexine, heptine, octyne, etc.

[0050] Examples of the aromatic solvent include toluene, xylene, ethylbenzene, isopropylbenzene, tert-butylbenzene, and mesitylene.

[0051] Rinsing can reduce the occurrence of resist pattern collapse and defects. Rinsing is not always necessary, and not performing rinsing can reduce the amount of solvent used. EXAMPLES

[0052] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The apparatus used is as follows. IR: Thermo Fisher Scientific NICOLET 6700 · 1 H-NMR: ECA-500 manufactured by JEOL Ltd.

[0053] [1] Synthesis of tin compounds [Synthesis Example 1] Synthesis of tin compound M-1 [ka] (In the formula, Bn is a benzyl group and Me is a methyl group.)

[0054] A mixture of 1.6 g of dibenzyl dichlorooxide, 1.5 g of dimethyl carbonate, 1.1 g of methanol, and 60 g of toluene was stirred at 110°C for 3 hours, then cooled to room temperature and filtered to remove insoluble matter, followed by vacuum concentration. Toluene was added to the concentrated residue obtained, which was then heated and dissolved, then cooled to room temperature and recrystallized to obtain 0.9 g of the target tin compound M-1 (yield 55%).

[0055] The IR spectrum data of the tin compound M-1 is shown below. The nuclear magnetic resonance spectrum ( 1 H-NMR / CDCl3 and 119 The results of Sn-NMR / CDCl3) are shown in Figures 1 and 2. 1Residual solvent (toluene) was observed in H-NMR. IR (D-ATR): 3635, 3079, 3057, 3023, 2929, 1599, 1538, 1492, 1451, 1405, 1366, 1210, 1115, 1052, 1029, 756, 731, 709, 698, 618, 518, 464, 455cm -1 .

[0056] [Synthesis Example 2] Synthesis of tin compound M-2 [ka] (In the formula, nBu is an n-butyl group, and Et is an ethyl group.)

[0057] A mixture of 1.0 g of di-n-butyldichlorotin, 0.3 g of sodium carbonate, and 100 g of 95% by mass ethanol aqueous solution was stirred at 60°C overnight, then returned to room temperature and filtered to obtain an insoluble matter. The insoluble matter was washed with a 30% by mass ethanol aqueous solution, and the washed powder was dried under reduced pressure to obtain 0.6 g of the target tin compound M-2 (yield 67%).

[0058] The IR spectrum data of the tin compound M-2 is shown below. IR (D-ATR): 2958, 2925, 2871, 2858, 1510, 1464, 1378, 1287, 1157, 1079, 1020, 965, 870, 826, 678, 640, 487cm -1 .

[0059] [Synthesis Example 3] Synthesis of tin compound M-3 [ka] (In the formula, nBu is an n-butyl group, and Me is a methyl group.)

[0060] A mixture of 2.5 g of di-n-butyltin oxide, 0.9 g of dimethyl carbonate, 20 g of toluene, and 0.2 g of methanol was stirred at 110° C. for 1 hour. After the reaction solution was returned to room temperature, it was concentrated under reduced pressure, and the concentrated residue was washed with methanol. The obtained powder was dried under reduced pressure by heating, to obtain 2.2 g of the target tin compound M-3 (yield 83%).

[0061] The IR spectrum data of the tin compound M-3 is shown below. IR (D-ATR): 2956, 2922, 2871, 2855, 2801, 1541, 1463, 1419, 1376, 1068, 669, 605, 577, 534cm -1 .

[0062] [2] Preparation of resist composition [Example 1-1, Comparative Examples 1-1 to 1-2] Resist materials were mixed and dissolved in the compositions shown in Table 1 below, and the resulting solutions were filtered through a 0.2 μm Teflon (registered trademark) filter to prepare resist composition R-1 of the present invention and comparative resist compositions CR-1 and CR-2.

[0063] [Table 1]

[0064] In Table 1, the materials P-1 (base polymer), PAG-1 (photoacid generator), Q-1 (sensitivity adjuster) and surfactant (SF-1) of the comparative chemically amplified resist composition CR-1 are as follows.

[0065] P-1: p-hydroxystyrene / 1-methylcyclopentyl methacrylate copolymer [ka]

[0066] PAG-1: Triphenylsulfonium 2-(adamantane-1-carbonyloxy)-1,1,3,3,3-pentafluoropropane-1-sulfonate [ka]

[0067] Q-1: 2-Morpholinoethyl laurate [ka]

[0068] SF-1: PF-636 (Omnova)

[0069] In Table 1, the tin compound CM-1, which is a material of the non-chemically amplified resist composition CR-2 as a comparative example, was synthesized according to the non-patent document: Angewandte Chemie, International Edition (2017), 56(34), 10140-10144. Its structure is as follows. [ka]

[0070] In Table 1, PGMEA is propylene glycol monomethyl ether acetate and DAA is diacetone alcohol.

[0071] [3] EB lithography evaluation (1) Evaluation of sensitivity, LWR and limiting resolution [Example 2-1, Comparative Examples 2-1 to 2-2] Each resist composition (R-1, CR-1 and CR-2) was spin-coated on a Si substrate on which a 60 nm-thick anti-reflective film DUV-42 manufactured by Nissan Chemical Industries, Ltd. was formed, and the substrate was pre-baked at 100° C. for 60 seconds using a hot plate to prepare a resist film with a thickness of 40 nm. The resist film was exposed using an EB lithography device manufactured by Elionix (ELS-F125, acceleration voltage 125 kV), and PEB was performed on a hot plate at a temperature listed in Table 2 for 60 seconds, and developed with a developer listed in Table 2 for 30 seconds to form a pattern. In Example 2-1 and Comparative Example 2-2, the resist film remained in the exposed area, and showed negative tone characteristics. In Comparative Example 2-1, the resist film remained in the unexposed area, and showed positive tone characteristics. As a result, a negative or positive type line and space (LS) pattern with a space width of 20 nm and a pitch of 40 nm was obtained. The obtained LS pattern was evaluated for sensitivity, LWR and limiting resolution according to the following method. The results are shown in Table 2. FIG. 3 shows an SEM image of a line and space (LS) pattern with a space width of 20 nm and a pitch of 40 nm at Eop in Example 2-1.

[0072] [Sensitivity evaluation] The LS pattern was observed under an electron microscope to determine the optimal exposure dose Eop (μC / cm) for obtaining an LS pattern with a space width of 20 nm and a pitch of 40 nm. 2 ) was calculated and used as the sensitivity.

[0073] [LWR rating] The LS pattern obtained by irradiating with the optimal exposure dose Eop was measured at 10 points in the longitudinal direction of the space width using a CD-SEM (CG-5000) manufactured by Hitachi High-Technologies Corporation, and the three times standard deviation (σ) (3σ) was calculated from the results and used as the LWR. The smaller this value, the less roughness and the more uniform the space width pattern that can be obtained.

[0074] [Limit resolution evaluation] The minimum line width (nm) of the LS pattern separated at the optimum exposure dose Eop was defined as the limiting resolution.

[0075] [Table 2]

[0076] From the results shown in Table 2, it was found that the resist composition of the present invention is excellent in LWR and limit resolution in negative pattern formation by organic solvent development using EB.

[0077] (2) Contrast curve and PEB shrink evaluation [Example 3] Resist composition R-1 was spin-coated on a Si substrate on which a 60 nm-thick anti-reflective film DUV-42 manufactured by Nissan Chemical Industries, Ltd. had been formed, and the substrate was pre-baked at 100° C. for 60 seconds using a hot plate to prepare a 40 nm-thick resist film. The resist film was then irradiated with an EB lithography system (ELS-F125) manufactured by Elionix at an acceleration voltage of 50 kV and an exposure dose of 3 to 3800 μC / cm. 2 The film was exposed to light in the range of 100 nm to 150 nm. After that, PEB was performed on a hot plate at 150°C for 60 seconds, the film thickness was measured, and the PEB shrink was calculated. Furthermore, development was performed using 2-heptanone for 30 seconds, and the film thickness after development was measured. The results of plotting the relationship between film thickness and exposure dose (contrast curve and PEB shrink) are shown in Figure 4.

[0078] The results shown in FIG. 4 indicate that the greater the exposure dose, the greater the PEB shrinkage and the greater the progress of insolubilization of the membrane.

[0079] Furthermore, although the sensitivity of the resist composition of the present invention was low in EB lithography, because it contains a high density of tin atoms which have high EUV light absorption ability, it is expected that the sensitivity will be considerably high in EUV lithography.

Claims

1. A resist composition comprising a tin compound represented by the following formula (1) and an organic solvent: 【Chemistry 1】 (In the formula, R 1A ~R 10A and R 1B ~R 10B are each independently a hydrocarbyl group having 1 to 20 carbon atoms. R 11 ~R 14 are each independently a hydrogen atom or a hydrocarbyl group having 1 to 20 carbon atoms. L a1 and L a2 are each independently a linking group.

2. L a1 and L a2 The resist composition according to claim 1, wherein each of the groups independently represents a group represented by any one of the following formulas (2a) to (2d): 【Chemistry 2】 (In the formula, the dashed line represents a bond to Sn.)

3. R 1A ~R 10A and R 1B ~R 10B 2. The resist composition according to claim 1, wherein is an isopropyl group, an n-butyl group, a tert-butyl group or a benzyl group.

4. The resist composition according to claim 1, further comprising a surfactant.

5. A pattern forming method comprising the steps of: forming a resist film on a substrate using the resist composition according to any one of claims 1 to 4; exposing the resist film to high-energy rays; and developing the exposed resist film using a developer.

6. 6. The pattern forming method according to claim 5, wherein the high energy beam is an electron beam or extreme ultraviolet ray.

Citation Information

Patent Citations

  • Photoresist materials and associated methods

    US20220365428A1

  • Negative resist composition, resist pattern forming method, and complex

    JP2015108781A