Semiconductor device and manufacturing method for the same
By employing a polycrystalline oxide semiconductor layer with controlled thickness variations, the semiconductor device addresses shape and electrical characteristic issues, achieving stable performance and improved yield.
Patent Information
- Application Number
- JP2023079566
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
AI Technical Summary
Conventional semiconductor devices using oxide semiconductor films face challenges with low etching resistance, leading to variations in shape and electrical characteristics, particularly on large-area substrates, which reduce yield.
The semiconductor device incorporates a polycrystalline oxide semiconductor layer with controlled film thickness variations of 1 nm or less, using a polycrystalline structure (Poly-OS) to enhance etching resistance, ensuring stable electrical characteristics and improved yield.
The solution stabilizes electrical characteristics and enhances yield by minimizing shape variations in the oxide semiconductor layer, achieving field effect mobility greater than 20 cm²/Vs and reducing recess formation during electrode formation.
Smart Images

Figure 2024163719000001_ABST
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to a semiconductor device. In particular, an embodiment of the present invention relates to a semiconductor device using an oxide semiconductor film as a channel. Also, an embodiment of the present invention relates to a method for manufacturing a semiconductor device. [Background technology]
[0002] In recent years, development of semiconductor devices using oxide semiconductor films as channels instead of silicon semiconductor films such as amorphous silicon, low-temperature polysilicon, and single crystal silicon has been progressing (see, for example, Patent Documents 1 to 6). A semiconductor device including such an oxide semiconductor film has a simple structure, similar to a semiconductor device including an amorphous silicon film, and can be manufactured on a glass substrate by a low-temperature process. In addition, it is known that a semiconductor device including an oxide semiconductor film has a higher field-effect mobility than a semiconductor device including an amorphous silicon film. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2021-141338 A [Patent Document 2] JP 2014-099601 A [Patent Document 3] Patent Publication No. 2021-153196 [Patent Document 4] JP 2018-006730 A [Patent Document 5] JP 2016-184771 A [Patent Document 6] Patent Publication No. 2021-108405 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in a conventional semiconductor device including an oxide semiconductor film, the oxide semiconductor film has low etching resistance, and it is difficult to control the shape of the oxide semiconductor film. In particular, in a semiconductor device manufactured using a large-area substrate such as a glass substrate, the variation in the shape of the oxide semiconductor film causes the variation in the electrical characteristics of the semiconductor device, which is a factor of reducing the yield.
[0005] An object of one embodiment of the present invention is to provide a semiconductor device having stable electrical characteristics and in which the variation in shape of an oxide semiconductor film is suppressed. Another object of one embodiment of the present invention is to provide a method for manufacturing a semiconductor device in which the variation in shape of an oxide semiconductor film is suppressed and the yield is improved. [Means for solving the problem]
[0006] A semiconductor device according to one embodiment of the present invention includes a gate electrode, a gate insulating layer on the gate electrode, an oxide semiconductor layer having a polycrystalline structure on the gate insulating layer, a source electrode and a drain electrode on the oxide semiconductor layer, and an interlayer insulating layer covering the source electrode and the drain electrode and in contact with the oxide semiconductor layer, wherein the oxide semiconductor layer includes a first region overlapping one of the source electrode and the drain electrode and a second region in contact with the interlayer insulating layer, and the difference between the film thickness of the first region and the film thickness of the second region is 1 nm or less.
[0007] A method for manufacturing a semiconductor device according to one embodiment of the present invention includes forming a gate electrode, forming a gate insulating layer on the gate electrode, forming an oxide semiconductor layer having a polycrystalline structure on the gate insulating layer, forming a source electrode and a drain electrode on the oxide semiconductor layer, and forming an interlayer insulating layer covering the source electrode and the drain electrode and in contact with the oxide semiconductor layer, wherein the oxide semiconductor layer includes a first region overlapping one of the source electrode and the drain electrode and a second region in contact with the interlayer insulating layer, and a difference between a film thickness of the first region and a film thickness of the second region is 1 nm or less. [Brief description of the drawings]
[0008] [Figure 1]1 is a schematic cross-sectional view showing a configuration of a semiconductor device according to an embodiment of the present invention. [Diagram 2] 1 is a schematic plan view showing a configuration of a semiconductor device according to an embodiment of the present invention; [Diagram 3] 1 is a flowchart illustrating a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 4] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Diagram 5] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 6] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 7] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 8] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 9] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 10] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 11] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 12] 1 is a schematic plan view showing an overview of a display device according to an embodiment of the present invention; [Figure 13] 1 is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention. [Figure 14] 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. [Figure 15] 1 is a schematic cross-sectional view showing a configuration of a display device according to one embodiment of the present invention. [Figure 16] 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. [Figure 17]1 is a schematic cross-sectional view showing a configuration of a display device according to one embodiment of the present invention. [Figure 18] 4 is a graph showing electrical characteristics of each sample in the examples. [Figure 19] 1 is a graph showing threshold values calculated from electrical characteristics of each sample in an example. [Figure 20] 1 is a graph showing the field effect mobility (field effect mobility in the saturation region) calculated from the electrical characteristics of each sample in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Each embodiment of the present invention will be described below with reference to the drawings. The following disclosure is merely an example. A configuration that a person skilled in the art can easily come up with by appropriately modifying the configuration of the embodiment while maintaining the gist of the invention is naturally included in the scope of the present invention. In order to make the explanation clearer, the drawings may be schematic in terms of the width, film thickness, shape, etc. of each part compared to the actual embodiment. However, the illustrated shapes are merely examples and do not limit the interpretation of the present invention. In this specification and each figure, elements similar to those described above with respect to the previous figures may be given the same reference numerals, and detailed explanations may be omitted as appropriate.
[0010] The term "semiconductor device" refers to any device that can function by utilizing semiconductor characteristics. Transistors and semiconductor circuits are included in the category of semiconductor devices. The semiconductor device of the following embodiment may be, for example, a display device, an integrated circuit (IC) such as a microprocessor (Micro-Processing Unit: MPU), or a transistor used in a memory circuit.
[0011] The term "display device" refers to a structure that displays an image using an electro-optical layer. For example, the term display device may refer to a display panel including an electro-optical layer, or may refer to a structure in which other optical members (e.g., a polarizing member, a backlight, a touch panel, etc.) are attached to a display cell. The "electro-optical layer" may include a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer, unless technically inconsistent. Therefore, in the embodiment, a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer are exemplified as the display device. However, the structure described in the embodiment may be applied to a display device including the other electro-optical layers described above.
[0012] In this specification and the like, the direction from the substrate toward the oxide semiconductor layer is referred to as "upper" or "upper". Conversely, the direction from the oxide semiconductor layer toward the substrate is referred to as "lower" or "lower". Thus, for convenience of explanation, the terms "upper" or "lower" are used in the explanation, but the substrate and the oxide semiconductor layer may be arranged so that their up-down relationship is reversed from that shown in the figure. In addition, the expression "oxide semiconductor layer on a substrate" merely describes the up-down relationship between the substrate and the oxide semiconductor layer, and other members may be arranged between the substrate and the oxide semiconductor layer. "Up" or "lower" means the order of stacking in a structure in which multiple layers are stacked, and when a pixel electrode is expressed as being above a semiconductor device, the semiconductor device and the pixel electrode may not overlap in a planar view. On the other hand, when a pixel electrode is expressed as being vertically above a semiconductor device, the semiconductor device and the pixel electrode may overlap in a planar view. Note that the planar view refers to a view from a direction perpendicular to the surface of the substrate.
[0013] In this specification and the like, the terms "film" and "layer" may be interchangeable in some cases.
[0014] In this specification, unless otherwise specified, the expressions "α includes A, B, or C," "α includes any of A, B, and C," or "α includes one selected from the group consisting of A, B, and C" do not exclude cases where α includes multiple combinations of A to C. Furthermore, these expressions do not exclude cases where α includes other elements.
[0015] The following embodiments can be combined with each other as long as no technical contradiction occurs.
[0016] First Embodiment A semiconductor device 10 according to one embodiment of the present invention will be described with reference to FIGS.
[0017] [Configuration of semiconductor device 10] The configuration of a semiconductor device 10 according to one embodiment of the present invention will be described with reference to Fig. 1 and Fig. 2. Fig. 1 is a cross-sectional view showing a schematic configuration of the semiconductor device 10 according to one embodiment of the present invention. Fig. 2 is a schematic plan view showing the configuration of the semiconductor device 10 according to one embodiment of the present invention. The cross-sectional view shown in Fig. 1 corresponds to a cross section taken along line A1-A2 shown in Fig. 2.
[0018] As shown in FIG. 1, the semiconductor device 10 is provided on a substrate 11. The semiconductor device 10 includes a gate electrode 12GE, gate insulating layers 14 and 16, an oxide semiconductor layer 26, a source electrode 32S, a drain electrode 32D, and interlayer insulating layers 34 and 38. When the source electrode 32S and the drain electrode 32D are not particularly distinguished from each other, they may be collectively referred to as the source electrode and the drain electrode 32. The gate electrode 12GE, the gate insulating layers 14 and 16, and the oxide semiconductor layer 26 may be collectively referred to as a transistor. The semiconductor device 10 is a so-called bottom-gate transistor in which the gate electrode 12GE is provided below the oxide semiconductor layer 26.
[0019] In this embodiment, the semiconductor device 10 will be described using a bottom-gate transistor as an example, but the semiconductor device 10 is not limited to the bottom-gate transistor. For example, the semiconductor device 10 may be a dual-gate transistor in which gate electrodes are provided above and below the oxide semiconductor layer 26.
[0020] The gate electrode 12GE is provided on the substrate 11. The gate insulating layers 14 and 16 are provided on the substrate 11 and the gate electrode 12GE. The gate insulating layers 14 and 16 have a laminated structure, and the gate insulating layer 16 is provided on the gate insulating layer 14. The oxide semiconductor layer 26 is provided on the gate insulating layers 14 and 16. The source electrode 32S and the drain electrode 32D are provided on the oxide semiconductor layer 26. The interlayer insulating layers 34 and 38 are provided on the oxide semiconductor layer 26 and the source electrode 32S and the drain electrode 32D. The interlayer insulating layers 34 and 38 have a laminated structure, and the interlayer insulating layer 38 is provided on the interlayer insulating layer 34. That is, the interlayer insulating layers 34 and 38 cover the source electrode 32S and the drain electrode 32D, and the interlayer insulating layer 34 is in contact with the oxide semiconductor layer 26.
[0021] Although not shown, a metal oxide layer may be provided between the gate insulating layer 16 and the oxide semiconductor layer 26. The metal oxide layer may have the same pattern as the oxide semiconductor layer 26. For example, an oxide containing aluminum (e.g., aluminum oxide, etc.) may be used as the metal oxide layer. The film thickness of the metal oxide layer is 1 nm or more and 10 nm or less, preferably 1 nm or more and 5 nm or less.
[0022] As shown in FIG. 2, in a plan view, the oxide semiconductor layer 26 overlaps with the gate electrode 12GE. The D1 direction is a direction connecting the source electrode 32S and the drain electrode 32D, and the D2 direction is a direction perpendicular to the D1 direction. In the semiconductor device 10, the channel length L corresponds to the length of a region (channel region) of the oxide semiconductor layer 26 between the source electrode 32S and the drain electrode 32D in the D1 direction, and the channel width W corresponds to the width of the channel region in the D2 direction. In a plan view, the region of the oxide semiconductor layer 26 overlapping with the source electrode 32S is the source region, and the region of the oxide semiconductor layer 26 overlapping with the drain electrode 32D is the drain region. That is, the channel region is located between the source region and the drain region.
[0023] The wiring 12W and the wiring 32W function as a gate wiring. The wiring 32W is electrically connected to the wiring 12W through a contact hole 15. Although the details will be described later, the wiring 12W is formed in the same layer as the gate electrode 12GE. Also, the wiring 32W is formed in the same layer as the source electrode 32S and the drain electrode 32D. Note that the wiring 32W may not be provided on the wiring 12W.
[0024] The oxide semiconductor layer 26 is transparent and has a polycrystalline structure including a plurality of crystal grains. Although details will be described later, the oxide semiconductor layer 26 having a polycrystalline structure can be formed by using a polycrystalline oxide semiconductor (Poly-OS) technique. Therefore, hereinafter, the oxide semiconductor included in the oxide semiconductor layer 26 may be described as Poly-OS.
[0025] The Poly-OS contains two or more metal elements including indium (i.e., indium and at least one or more metal elements other than indium), and the ratio of indium to the two or more metal elements is 50% or more. As the metal element other than indium, gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconium (Zr), or a lanthanoid element is used. The oxide semiconductor layer 26 may contain elements other than the above.
[0026] The crystal grains contained in the Poly-OS have a crystal grain size of 0.1 μm or more, preferably 0.3 μm or more, and more preferably 0.5 μm or more. The crystal grain size can be obtained by, for example, SEM observation, TEM observation, or Electron Back Scattered Diffraction (EBSD) method of the oxide semiconductor layer 26.
[0027] As described above, the crystal grains contained in the Poly-OS have a grain size of 0.1 μm or more, and therefore, in the oxide semiconductor layer 26 having a thickness of 10 nm or more and 30 nm or less, there is a region that contains only one crystal grain along the film thickness direction.
[0028] Poly-OS has excellent etching resistance. As will be described later in detail, Poly-OS has excellent etching resistance against the etching solution used in forming the source electrode 32S and the drain electrode 32D. Specifically, in forming the source electrode 32S and the drain electrode 32D, the oxide semiconductor layer 26 is hardly etched by the etching solution. Therefore, the film thickness of the first region (i.e., the source region or the drain region) of the oxide semiconductor layer 26 overlapping with one of the source electrode 32S and the drain electrode 32D is substantially the same as the film thickness of the second region (i.e., the channel region) of the oxide semiconductor layer 26 not overlapping with the source electrode 32S and the drain electrode 32D. In other words, the difference between the film thickness of the first region and the film thickness of the second region is 1.0 nm or less, preferably 0.5 nm or less, and more preferably 0.2 nm or less.
[0029] The variation in the shape of the oxide semiconductor layer is a factor that destabilizes the electrical characteristics of the semiconductor device. In particular, the variation in the thickness of the channel region of the oxide semiconductor layer is a significant factor in the variation in the electrical characteristics of the semiconductor device. For example, if the thickness of the channel region is smaller than a set value, the current flowing between the source electrode and the drain electrode decreases. Therefore, the on-current of the semiconductor device decreases, and the field effect mobility decreases. In addition, when the oxide semiconductor layer is etched in the formation of the source electrode and the drain electrode, not only the thickness of the channel region decreases, but also a recess is formed on the upper surface of the oxide semiconductor layer between the source electrode and the drain electrode. The interlayer insulating layer is formed so as to cover the recess formed on the upper surface of the oxide semiconductor layer, but if the interlayer insulating layer cannot sufficiently cover the recess, a gap is generated between the oxide semiconductor layer and the interlayer insulating layer, and between the source electrode and the drain electrode and the interlayer insulating layer. In such a state, the semiconductor device does not obtain stable electrical characteristics. That is, the variation in the shape of the oxide semiconductor layer reduces the yield of the semiconductor device.
[0030] In contrast, in the semiconductor device 10, the oxide semiconductor layer 26 contains Poly-OS and has high etching resistance. Therefore, in the formation of the source electrode 32S and the drain electrode 32D, the film thickness of the channel region is hardly reduced, and no recess is formed on the upper surface of the oxide semiconductor layer 26. Therefore, in the semiconductor device 10, the variation in the shape of the oxide semiconductor layer 26 is small, and stable electrical characteristics can be obtained. For example, in the semiconductor device 10, even when the gate insulating layers 14 and 16 having a film thickness of 400 nm or more are formed to improve the breakdown voltage, the variation in field effect mobility is small, and the field effect mobility is stable, even when the gate insulating layers 14 and 16 have a film thickness of 15 cm. 2 / Vs or more, even 20cm 2 A field effect mobility (field effect mobility in the linear region) of at least 1.0 V can be obtained.
[0031] [Method of Manufacturing Semiconductor Device 10] A method for manufacturing a semiconductor device 10 according to an embodiment of the present invention will be described with reference to Fig. 3 to Fig. 11. Fig. 3 is a flowchart for explaining a method for manufacturing a semiconductor device 10 according to an embodiment of the present invention. Figs. 4 to 11 are schematic cross-sectional views showing a method for manufacturing a semiconductor device 10 according to an embodiment of the present invention. Each step of the flowchart shown in Fig. 3 will be described in order below.
[0032] In step S1001 ("GE formation") of FIG. 3, a gate electrode 12GE is formed on a substrate 11 (see FIG. 4).
[0033] As the substrate 11, a rigid substrate having light transmission properties, such as a glass substrate, a quartz substrate, and a sapphire substrate, is used. When the substrate 11 needs to be flexible, a polyimide substrate, an acrylic substrate, a siloxane substrate, a fluororesin substrate, or a substrate containing a resin is used as the substrate 11. When a substrate containing a resin is used as the substrate 11, impurity elements may be introduced into the resin in order to improve the heat resistance of the substrate 11. Furthermore, when the semiconductor device 10 is used in an integrated circuit, a substrate not having light transmission properties, such as a semiconductor substrate such as a silicon substrate, a silicon carbide substrate, or a compound semiconductor substrate, or a conductive substrate such as a stainless steel substrate, may be used as the substrate 11.
[0034] The gate electrode 12GE is formed by processing a conductive film formed by a sputtering method. A metal material is used for the gate electrode 12GE. For example, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys or compounds thereof are used for the gate electrode 12GE. The above metal materials may be used as a single layer or as a laminated layer for the gate electrode 12GE.
[0035] In step S1002 ("GI formation") in FIG. 3, gate insulating layers 14 and 16 are formed on the gate electrode 12GE (see FIG. 4). The gate insulating layers 14 and 16 are formed by a CVD (Chemical Vapor Deposition) method or a sputtering method. An insulating material is used for the gate insulating layers 14 and 16. For example, silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), silicon nitride (SiN x ), silicon oxynitride (SiN x O y ) and other inorganic insulating materials are used. x N y is a silicon compound that contains a smaller ratio (x>y) of nitrogen (N) than oxygen (O). SiN x O y is a silicon compound that contains a smaller proportion of oxygen than nitrogen (x>y).
[0036] It is preferable that a gate insulating layer 14 using an insulating material containing nitrogen and a gate insulating layer 16 using an insulating material containing oxygen are formed in this order on the substrate 11. By using an insulating material containing nitrogen as the gate insulating layer 14, impurities diffusing from the substrate 11 toward the oxide semiconductor layer 26 can be blocked. In addition, by using an insulating material containing oxygen as the gate insulating layer 16, oxygen can be released by heat treatment. The temperature of the heat treatment at which the insulating material containing oxygen releases oxygen is, for example, 500° C. or less, 450° C. or less, or 400° C. or less. The insulating material containing oxygen may release oxygen when heated in any step of the manufacturing process of the semiconductor device 10.
[0037] The thickness of the gate insulating layer 14 is preferably larger than the thickness of the gate insulating layer 16. For example, the thickness of the gate insulating layer 14 is 200 nm or more, 300 nm or more, or 400 nm or more. For example, the thickness of the gate insulating layer 16 is 50 nm or more, 100 nm or more, or 150 nm or more. The thickness of the gate insulating layers 14 and 16 (i.e., the total thickness of the gate insulating layer 14 and the gate insulating layer 16) is preferably 300 nm or more, but is not limited to this.
[0038] In step S1004 ("OS film formation") in Fig. 3, an oxide semiconductor film 22 is formed on the gate insulating layers 14 and 16 (see Fig. 5). The oxide semiconductor film 22 is formed by sputtering or atomic layer deposition (ALD). The thickness of the oxide semiconductor film 22 is 10 nm to 50 nm, preferably 10 nm to 40 nm, and more preferably 10 nm to 30 nm.
[0039] A metal oxide having semiconductor properties can be used as the oxide semiconductor film 22. For example, an oxide semiconductor containing two or more metal elements including an indium (In) element (i.e., an indium element and at least one metal element other than the indium element) is used as the oxide semiconductor film 22. The ratio of the indium element to the two or more metal elements is 50% or more. As the metal element other than the indium element, a gallium (Ga) element, a zinc (Zn) element, an aluminum (Al) element, a hafnium (Hf) element, an yttrium (Y) element, a zirconium (Zr) element, or a lanthanoid element is used. It is preferable that the oxide semiconductor film 22 contains a Group 13 element. Note that an element other than the above may be used as the oxide semiconductor film 22.
[0040] When the oxide semiconductor film 22 is crystallized by OS annealing described later, the oxide semiconductor film 22 after deposition and before OS annealing preferably has an amorphous structure (for example, a structure with few crystalline components of the oxide semiconductor that is determined to be amorphous by XRD). That is, the oxide semiconductor film 22 is preferably formed under conditions that prevent the oxide semiconductor film 22 from crystallizing as soon as it is formed. For example, when the oxide semiconductor film 22 is formed by a sputtering method, the oxide semiconductor film 22 is formed while controlling the temperature of the object to be deposited (the substrate 11 and the structure formed thereon).
[0041] When a film is formed on a target object by sputtering, ions generated in the plasma and atoms recoiled from the sputtering target collide with the target object, and the temperature of the target object rises with the film formation process. When the temperature of the target object rises during the film formation process, the oxide semiconductor film 22 contains microcrystals immediately after the film formation. When the oxide semiconductor film 22 contains microcrystals, the crystal grain size cannot be increased by the subsequent OS annealing. In order to control the temperature of the target object, for example, the target object can be cooled while the film is formed. For example, the target object can be cooled from the surface opposite to the surface to be formed so that the temperature of the surface to be formed of the target object (hereinafter referred to as the "film formation temperature") is 100°C or less, 70°C or less, 50°C or less, or 30°C or less. In particular, the film formation temperature of the oxide semiconductor film 22 is preferably 50°C or less. By forming the oxide semiconductor film 22 while cooling the substrate 11, it is possible to obtain the oxide semiconductor film 22 having a small amount of crystalline components immediately after the film formation.
[0042] In the sputtering process, the oxide semiconductor film 22 having an amorphous structure is formed under conditions of an oxygen partial pressure of 10% or less. If the oxygen partial pressure is high, the oxide semiconductor film 22 contains excess oxygen, which causes microcrystals to be included in the oxide semiconductor film 22 immediately after the film formation. Therefore, it is preferable to form the oxide semiconductor film 22 under conditions of a low oxygen partial pressure. The oxygen partial pressure is, for example, 1% to 5%, and preferably 2% to 4%. Under conditions of an oxygen partial pressure of less than 1%, the distribution of oxygen in the film formation apparatus tends to be non-uniform. As a result, the composition of oxygen in the oxide semiconductor film also becomes non-uniform, and an oxide semiconductor film containing many microcrystals is formed, or an oxide semiconductor film that does not crystallize even when a subsequent OS annealing process is performed is formed.
[0043] In step S1005 ("OS pattern formation") in FIG. 3, a pattern of the oxide semiconductor layer 24 is formed (see FIG. 6). The pattern of the oxide semiconductor layer 24 is formed by photolithography. For example, a resist mask (not shown) is formed on the oxide semiconductor film 22, and the oxide semiconductor film 22 is etched using the resist mask. The oxide semiconductor film 22 may be etched by wet etching or dry etching. In the wet etching, an acidic etching solution may be used. As the etching solution, for example, oxalic acid, PAN, sulfuric acid, hydrogen peroxide solution, or hydrofluoric acid may be used. By the etching, the oxide semiconductor layer 24 having a predetermined pattern can be formed. Thereafter, the resist mask is removed.
[0044] It is preferable that the oxide semiconductor layer 24 having a predetermined pattern is formed (i.e., the patterning of the oxide semiconductor film 22) before the OS annealing. The Poly-OS after the OS annealing has high etching resistance, and the patterning by etching becomes difficult. In addition, by performing the OS annealing after the formation of the oxide semiconductor layer 24, damage (e.g., oxygen defects in the oxide semiconductor layer 24) caused during the formation of the oxide semiconductor layer 24 can be repaired.
[0045] In step S1006 ("OS anneal") in FIG. 3, after the oxide semiconductor layer 24 is formed, the oxide semiconductor layer 24 is subjected to a heat treatment (OS anneal) to form the oxide semiconductor layer 26 (see FIG. 7). In the OS anneal, the oxide semiconductor layer 24 is held at a predetermined temperature for a predetermined time. The predetermined temperature is 300° C. or more and 500° C. or less, and preferably 350° C. or more and 450° C. or less. The holding time at the temperature is 15 minutes or more and 120 minutes or less, and preferably 30 minutes or more and 60 minutes or less. By performing the OS anneal, the oxide semiconductor layer 24 having an amorphous structure is crystallized to form the oxide semiconductor layer 26 having a polycrystalline structure. That is, the oxide semiconductor layer 26 including the Poly-OS is formed by the OS anneal.
[0046] 3, contact holes are formed in the gate insulating layers 14 and 16 (see FIG. 8). This exposes the upper surface of the wiring 12W. If there is no need to connect the wiring 32W and the wiring 12W, the process of step S1008 does not need to be performed.
[0047] 3, the source electrode 32S, the drain electrode 32D, and the wiring 32W are formed (see FIG. 9). The source electrode 32S, the drain electrode 32D, and the wiring 32W are formed by performing patterning processing by wet etching on a conductive film formed by a sputtering method.
[0048] The source electrode 32S and the drain electrode 32D are made of the same metal material as the gate electrode 12GE. That is, as the metal material of the conductive film to be patterned, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys or compounds thereof are used. As the conductive film, the above-mentioned metal materials may be used in a single layer or in a multilayer structure. When the metal material is used in a single layer, the conductive film has, for example, a single layer structure of MoW alloy, Ti, or Cu. When the metal material is used in a multilayer structure, for example, the conductive film has a multilayer structure of Ti, Al, and Ti (Ti / Al / Ti structure), a multilayer structure of Cu and Ti (Cu / Ti structure), or a multilayer structure of Ti, Cu, and Ti (Ti / Cu / Ti structure). The source electrode 32S and the drain electrode 32D have the same configuration as the conductive film. In addition, the wiring 32W is formed at the same time as the formation of the source electrode 32S and the drain electrode 32D. In order to reduce the resistance of the wiring 32W, the conductive film preferably contains a low-resistance metal material such as Al or Cu. In addition, when the conductive film contains a metal material such as Cu, a barrier metal film containing Ti, Mo, or a MoW alloy is preferably provided between the oxide semiconductor layer 26 and the metal film containing Cu.
[0049] Here, the formation of the source electrode 32S and the drain electrode 32D having a stacked structure will be described using a Cu / Ti structure as an example. On the oxide semiconductor layer 26, a Ti film is formed as a first metal film in contact with the oxide semiconductor layer 26, and then a Cu film is formed as a second metal film on the first metal film. Next, a predetermined resist pattern is formed on the second metal film, and the second metal film and the first metal film are wet-etched using the resist pattern as a mask. As a result, a second metal layer containing Ti and a first metal layer containing Cu are formed from the second metal film and the first metal film, respectively.
[0050] In forming the source electrode 32S and the drain electrode 32D, a hydrogen peroxide-based etching solution is used as an etching solution for wet etching. The hydrogen peroxide-based etching solution contains a chelating agent such as ethylenediaminetetraacetic acid (EDTA) or phosphoric acid.
[0051] Poly-OS has excellent etching resistance. Specifically, the etching rate of the etchant used in forming the source electrode 32S and the drain electrode 32D is very small. This means that Poly-OS is hardly etched by the etchant. In other words, in the semiconductor device 10, even if a conductive film is directly formed on the oxide semiconductor layer 26 and the conductive film is patterned to form the source electrode 32S and the drain electrode 32D, the channel region of the oxide semiconductor layer 26 is hardly etched. Therefore, the film thickness of the first region (i.e., the source region or the drain region) of the oxide semiconductor layer 26 overlapping with one of the source electrode 32S and the drain electrode 32D is substantially the same as the film thickness of the second region (i.e., the channel region) of the oxide semiconductor layer 26 not overlapping with the source electrode 32S and the drain electrode 32D. In other words, the film thickness of the oxide semiconductor layer 26 can be controlled so that the difference between the film thickness of the first region and the film thickness of the second region is 1.0 nm or less, preferably 0.5 nm or less, and more preferably 0.2 nm or less.
[0052] For example, the etching rate of the oxide semiconductor layer 26 with respect to the etching solution (solution temperature: 30° C.) used in forming the source electrode 32S and the drain electrode 32D is less than 0.01 nm / sec or less than 0.20 nm / min. That is, even if the etching time is 60 seconds, the reduction in the film thickness of the oxide semiconductor layer 26 is less than 0.20 nm.
[0053] In a semiconductor device including an oxide semiconductor layer that does not have a polycrystalline structure such as IGZO, when a conductive film formed directly on the oxide semiconductor layer is patterned to form source and drain electrodes, the oxide semiconductor layer is also etched by wet etching in the patterning of the conductive film. Therefore, when manufacturing a semiconductor device in which the thickness of the channel region of the oxide semiconductor layer is 40 nm or less, it is necessary to form an oxide semiconductor film having a thickness of about 90 nm, and adjust the etching time in the formation of the source and drain electrodes so that the thickness of the channel region is 40 nm or less. However, when the etching rate is high, it is difficult to precisely control the thickness of the channel region by the etching time. In this case, the variation in the thickness of the channel region becomes large.
[0054] Furthermore, when the thickness of the channel region is significantly reduced, a recess is formed on the upper surface of the oxide semiconductor layer. The interlayer insulating layer is formed so as to cover the recess formed on the upper surface of the oxide semiconductor layer, but if the recess is deep, the interlayer insulating layer cannot cover the recess sufficiently. That is, a gap may be formed between the oxide semiconductor layer and the interlayer insulating layer, or between the source electrode and the drain electrode and the interlayer insulating layer. This not only causes instability in the electrical characteristics of the semiconductor device, but also may cause a decrease in reliability.
[0055] In contrast, the oxide semiconductor layer 26 contains Poly-OS and has high etching resistance. Therefore, the thickness of the channel region of the oxide semiconductor layer 26 can be controlled only by forming the oxide semiconductor film 22, without considering the reduction in the thickness of the oxide semiconductor layer 26 due to the etching solution used to form the source electrode 32S and the drain electrode 32D. Therefore, the oxide semiconductor film 22 can be formed to a thickness of 10 nm to 50 nm, preferably 10 nm to 40 nm, and more preferably 10 nm to 30 nm. In addition, since the oxide semiconductor layer 26 has high etching resistance, the selectivity of metal materials that can be used for the source electrode 32S, the drain electrode 32D, and the wiring 32W is improved.
[0056] Since the oxide semiconductor layer 26 has excellent etching resistance, it is possible to increase the etching rate of the conductive film in forming the source electrode 32S and the drain electrode 32D. For example, the etching rate of the first metal film in contact with the oxide semiconductor layer 26 is 0.1 nm / sec or more, preferably 0.5 nm / sec or more, and more preferably 0.9 nm / sec or more. In addition, when the second metal film formed on the first metal film contains Cu, the etching rate of the second metal film is 1.0 nm / sec or more, preferably 2.0 nm / sec or more, and more preferably 3.0 nm / sec or more.
[0057] In the formation of the source electrode 32S and the drain electrode 32D, the oxide semiconductor layer 26 is hardly etched, but the gate insulating layer 16 may be etched depending on the type of etching solution. For example, in order to prevent an unnecessary conductive film from remaining, over-etching is performed instead of just etching. In this case, the gate insulating layer 16 exposed from the conductive film is etched. In the gate insulating layer 16, the difference in thickness between the region overlapping with the oxide semiconductor layer 26 and the region not overlapping with the oxide semiconductor layer 26 is 5 nm or more, 10 nm or more, or 15 nm or more. In addition, the time of over-etching is controlled so that the thickness of the gate insulating layer 16 does not become too small, so that the difference in thickness between the region overlapping with the oxide semiconductor layer 26 and the region not overlapping with the oxide semiconductor layer 26 is 50 nm or less, preferably 30 nm or less, and more preferably 20 nm or less.
[0058] 3, an interlayer insulating layer 34 is formed on the oxide semiconductor layer 26, the source electrode 32S, and the drain electrode 32D. It is preferable to use an insulating material containing oxygen for the interlayer insulating layer 34. For example, silicon oxide (SiO x ) or silicon oxynitride (SiO x N y ), etc. are used. It is also preferable to use an insulating film with few defects as the interlayer insulating layer 34. For example, when the oxygen composition ratio in the interlayer insulating layer 34 is compared with the oxygen composition ratio in an insulating film having the same composition as the interlayer insulating layer 34 (hereinafter referred to as "another insulating film"), the oxygen composition ratio in the interlayer insulating layer 34 is closer to the stoichiometric ratio for the insulating film than the oxygen composition ratio in the other insulating film. For example, when silicon oxide (SiO x When SiO2 is used, the interlayer insulating layer 34 has a composition ratio closer to the stoichiometric ratio of silicon oxide (SiO2) than the gate insulating layer 14. The interlayer insulating layer 34 may be a layer in which no defects are observed when evaluated by electron spin resonance (ESR).
[0059] The interlayer insulating layer 34 can be formed by using the same film formation method as the gate insulating layers 14, 16. In order to increase the composition ratio of oxygen in the interlayer insulating layer 34, the film may be formed at a relatively low temperature (for example, a film formation temperature of less than 350° C.). In order to form an insulating film with few defects as the interlayer insulating layer 34, the interlayer insulating layer 34 may be formed at a film formation temperature of 350° C. or higher. Furthermore, after forming the interlayer insulating layer 34, a process of implanting oxygen into a part of the interlayer insulating layer 34 may be performed.
[0060] The thickness of the interlayer insulating layer 34 is 50 nm or more and 300 nm or less, 60 nm or more and 200 nm or less, or 70 nm or more and 150 nm or less.
[0061] 3, a metal oxide film 36 is formed on the interlayer insulating layer 34 (see FIG. 10). The metal oxide film 36 is formed by sputtering or atomic layer deposition (ALD).
[0062] A metal oxide containing aluminum as a main component is used as the metal oxide film 36. For example, aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y ), aluminum oxide nitride (AlN x O y ), Aluminum Nitride (AlN x ) is used. A metal oxide film containing aluminum as a main component means that the ratio of aluminum contained in the metal oxide film 36 is 1% or more of the entire metal oxide film 36. The ratio of aluminum contained in the metal oxide film 36 may be 5% or more and 70% or less, 10% or more and 60% or less, or 30% or more and 50% or less of the entire metal oxide film 36. The above ratio may be a mass ratio or a weight ratio.
[0063] The thickness of the metal oxide film 36 is 1 nm or more and 50 nm or less, preferably 1 nm or more and 30 nm or less. Aluminum oxide is preferably used as the metal oxide film 36. Aluminum oxide has high barrier properties against gases such as oxygen and hydrogen. Here, the barrier properties refer to a function of suppressing the permeation of gases such as oxygen and hydrogen through aluminum oxide. In other words, it means that gases such as oxygen and hydrogen in a layer provided under the aluminum oxide film are not transferred to a layer provided above the aluminum oxide film. Or, it means that gases such as oxygen and hydrogen in a layer provided above the aluminum oxide film are not transferred to a layer provided below the aluminum oxide film.
[0064] 3 ("oxidation anneal"), a heat treatment is performed (see FIG. 10) on the oxide semiconductor layer 26 with the interlayer insulating layer 34 and the metal oxide film 36 formed thereon. As a result, oxygen released from the interlayer insulating layer 34 is supplied to the oxide semiconductor layer 26. By providing the metal oxide film 36 so as to cover the substrate 11, it is possible to prevent the oxygen released from the interlayer insulating layer 34 from being released to the outside of the metal oxide film 36.
[0065] During the process from when the oxide semiconductor layer 26 is formed until when the interlayer insulating layer 34 is formed on the oxide semiconductor layer 26, many oxygen defects are generated in the oxide semiconductor layer 26. However, by the oxidation annealing in step S1012, oxygen released from the interlayer insulating layer 34 is supplied to the oxide semiconductor layer 26, and the oxygen defects are repaired.
[0066] 3, the metal oxide film 36 is removed (see FIG. 11). For example, the metal oxide film 36 may be removed using diluted hydrofluoric acid (DHF).
[0067] 3, an interlayer insulating layer 38 is formed on the interlayer insulating layer 34. It is preferable to use an insulating material containing nitrogen for the interlayer insulating layer 38. For example, silicon nitride (SiNx ) or silicon oxynitride (SiN x O y The interlayer insulating layer 38 can be formed by the same film formation method as that for the gate insulating layers 14 and 16.
[0068] Through the steps described above, the semiconductor device 10 shown in FIG. 1 can be manufactured.
[0069] As described above, in the manufacturing process of the semiconductor device 10, by forming the oxide semiconductor layer 26 containing Poly-OS having high etching resistance, the shape variation of the oxide semiconductor layer 26 is suppressed. In particular, the variation in the thickness of the channel region of the oxide semiconductor layer 26 can be reduced. As a result, the semiconductor device 10 has stable electrical characteristics and the yield is improved.
[0070] <Second embodiment> 12 to 15, a display device 20 using the semiconductor device 10 according to one embodiment of the present invention will be described. In the embodiment shown below, a configuration in which the semiconductor device 10 described in the first embodiment is applied to the circuitry of a liquid crystal display device will be described.
[0071] [Outline of the display device 20] Fig. 12 is a schematic plan view showing an overview of a display device 20 according to an embodiment of the present invention. As shown in Fig. 12, the display device 20 has an array substrate 300, a seal portion 310, a counter substrate 320, a flexible printed circuit board 330 (FPC 330), and an IC chip 340. The array substrate 300 and the counter substrate 320 are bonded together by the seal portion 310. In a liquid crystal region 220 surrounded by the seal portion 310, a plurality of pixel circuits 301 are arranged in a matrix. The liquid crystal region 220 is an area that overlaps with a liquid crystal element 311 described later in a plan view.
[0072] The seal area 240 in which the seal portion 310 is provided is the area surrounding the liquid crystal area 220. The FPC 330 is provided in the terminal area 260. The terminal area 260 is an area in which the array substrate 300 is exposed from the counter substrate 320, and is provided outside the seal area 240. The outside of the seal area 240 means the outside of the area in which the seal portion 310 is provided and the area surrounded by the seal portion 310. The IC chip 340 is provided on the FPC 330. The IC chip 340 supplies signals for driving each pixel circuit 301.
[0073] [Circuit configuration of display device 20] Fig. 13 is a block diagram showing a circuit configuration of a display device 20 according to an embodiment of the present invention. As shown in Fig. 13, a source driver circuit 302 is provided at a position adjacent to the liquid crystal region 220 in which the pixel circuits 301 are arranged in the second direction D2 (column direction), and a gate driver circuit 303 is provided at a position adjacent to the liquid crystal region 220 in the first direction D1 (row direction). The source driver circuit 302 and the gate driver circuit 303 are provided in the above-mentioned sealing region 240. However, the region in which the source driver circuit 302 and the gate driver circuit 303 are provided is not limited to the sealing region 240, and may be any region outside the region in which the pixel circuits 301 are provided.
[0074] A source line 304 extends from the source driver circuit 302 in the second direction D2 and is connected to the plurality of pixel circuits 301 arranged in the second direction D2. A gate electrode 12GE extends from the gate driver circuit 303 in the first direction D1 and is connected to the plurality of pixel circuits 301 arranged in the first direction D1.
[0075] A terminal section 306 is provided in the terminal region 260. The terminal section 306 and the source driver circuit 302 are connected by a connection wiring 307. Similarly, the terminal section 306 and the gate driver circuit 303 are connected by a connection wiring 307. By connecting the FPC 330 to the terminal section 306, an external device to which the FPC 330 is connected is connected to the display device 20, and each pixel circuit 301 provided in the display device 20 is driven by a signal from the external device.
[0076] The semiconductor device 10 according to the first embodiment is used as a transistor included in a pixel circuit 301, a source driver circuit 302, and a gate driver circuit 303.
[0077] [Pixel circuit 301 of display device 20] Fig. 14 is a circuit diagram showing a pixel circuit 301 of a display device 20 according to an embodiment of the present invention. As shown in Fig. 14, the pixel circuit 301 includes elements such as a semiconductor device 10, a storage capacitor 350, and a liquid crystal element 311. The semiconductor device 10 has a gate electrode 12GE, an oxide semiconductor layer 26, a source electrode 32S, and a drain electrode 32D. The gate electrode 12GE is connected to a gate wiring 305. The source electrode 32S is connected to a source wiring 304. The drain electrode 32D is connected to the storage capacitor 350 and the liquid crystal element 311.
[0078] [Configuration of display device 20] Fig. 15 is a schematic cross-sectional view of a display device 20 according to one embodiment of the present invention. The display device 20 shown in Fig. 15 uses the semiconductor device 10.
[0079] 15, a gate electrode 12GE is provided on a substrate 11. Gate insulating layers 14 and 16 are provided on the gate electrode 12GE. An oxide semiconductor layer 26 is provided on the gate insulating layers 14 and 16. A source electrode 32S and a drain electrode 32D are provided on the oxide semiconductor layer 26.
[0080] Interlayer insulating layers 34 and 38 are provided on the source electrode 32S and the drain electrode 32D. An insulating layer 39 is provided on the interlayer insulating layers 34 and 38. The insulating layer 39 is provided to reduce unevenness caused by the semiconductor device 10. A contact hole is formed in the interlayer insulating layers 34 and 38 and the insulating layer 39 so as to expose the upper surface of the source electrode 32S. A common electrode 42C that is provided in common to a plurality of pixels is provided on the insulating layer 39. An insulating layer 44 is provided on the common electrode 42C. The insulating layer 44 is provided inside the contact hole. By forming the insulating layer 44 from a silicon nitride film, it is possible to suppress the intrusion of moisture from the contact hole through the insulating layer 44. A pixel electrode 46P is provided on the insulating layer 44 and inside the contact hole. The pixel electrode 46P is connected to the drain electrode 32D.
[0081] Furthermore, a wiring 12C is provided on the substrate 11 and is connected to a wiring 32C through a contact hole provided in the gate insulating layers 14 and 16. The wiring 12C and the wiring 32C function as a capacitance wiring. Furthermore, an electrode 46C is provided on the insulating layer 39 and inside the opening. A storage capacitor 350 is formed by the common electrode 42C, the insulating layer 44, and the electrode 46C.
[0082] In this embodiment, a configuration in which the semiconductor device 10 is used in the pixel circuit 301 is illustrated as an example, but the semiconductor device 10 may also be used in a peripheral circuit including a source driver circuit 302 and a gate driver circuit 303.
[0083] <Third embodiment> A display device 20 using the semiconductor device 10 according to one embodiment of the present invention will be described with reference to Figures 16 and 17. In this embodiment, a configuration in which the semiconductor device 10 described in the first embodiment is applied to the circuit of an organic EL display device will be described. The outline and circuit configuration of the display device 20 are similar to those shown in Figures 12 and 13, and therefore description thereof will be omitted.
[0084] [Pixel circuit 301 of display device 20] FIG. 16 is a circuit diagram showing a pixel circuit of a display device 20 according to an embodiment of the present invention. As shown in FIG. 16, a pixel circuit 301 includes elements such as a driving transistor 110, a selection transistor 120, a storage capacitor 210, and a light-emitting element DO. The driving transistor 110 and the selection transistor 120 have the same configuration as the semiconductor device 10. The source electrode of the selection transistor 120 is connected to a signal line 211, and the gate electrode of the selection transistor 120 is connected to a gate line 212. The source electrode of the driving transistor 110 is connected to an anode power line 213, and the drain electrode of the driving transistor 110 is connected to one end of the light-emitting element DO. The other end of the light-emitting element DO is connected to a cathode power line 214. The gate electrode of the driving transistor 110 is connected to the drain electrode of the selection transistor 120. The storage capacitor 210 is connected to the gate electrode and drain electrode of the driving transistor 110. A grayscale signal that determines the light-emitting intensity of the light-emitting element DO is supplied to the signal line 211. A signal that selects a pixel row to which the above grayscale signal is written is supplied to the gate line 212.
[0085] [Cross-sectional structure of the display device 20] Fig. 17 is a schematic cross-sectional view showing the configuration of a display device 20 according to one embodiment of the present invention. The configuration of the display device 20 shown in Fig. 17 is similar to that of the display device 20 shown in Fig. 15, but the structure above the insulating layer 39 of the display device 20 shown in Fig. 17 is different from the structure above the insulating layer 39 of the display device 20 shown in Fig. 14. Hereinafter, a description of the configuration of the display device 20 shown in Fig. 17 that is similar to that of the display device 20 shown in Fig. 15 will be omitted, and only the differences between the two will be described.
[0086] As shown in FIG. 17, the display device 20 has a pixel electrode 390, a light-emitting layer 392, and a common electrode 394 (light-emitting element DO) above an insulating layer 39. The pixel electrode 390 is provided on the insulating layer 39 and inside a contact hole formed in the interlayer insulating layers 34, 38 and the insulating layer 39. An insulating layer 362 is provided on the pixel electrode 390. An opening 363 is provided in the insulating layer 362. The opening 363 corresponds to a light-emitting region. In other words, the insulating layer 362 defines a pixel. The light-emitting layer 392 and the common electrode 394 are provided on the pixel electrode 390 exposed by the opening 363. The pixel electrode 390 and the light-emitting layer 392 are provided individually for each pixel. On the other hand, the common electrode 394 is provided in common to a plurality of pixels. The light-emitting layer 392 is made of different materials depending on the display color of the pixel.
[0087] In the second and third embodiments, the semiconductor device 10 described in the first embodiment is applied to a liquid crystal display device and an organic EL display device. However, the semiconductor device 10 may be applied to a display device other than these display devices (for example, a self-luminous display device other than an organic EL display device or an electronic paper display device). The semiconductor device 10 can be applied to a variety of display devices, from small and medium-sized display devices to large display devices, without any particular limitations. Even when manufactured using a large-area substrate, the shape of the oxide semiconductor layer 26 in the semiconductor device 10 varies little. Therefore, when the semiconductor device 10 is applied to the display device 20, display unevenness can be reduced. Furthermore, the yield rate when manufacturing the display device 20 can be improved. EXAMPLES
[0088] Furthermore, the semiconductor device 10 according to an embodiment of the present invention will be described in detail based on examples, but the semiconductor device 10 is not limited to the examples described below.
[0089] [Etching rate] The etching solution used in the formation of the source and drain electrodes was used to remove the Poly-OS contained in the oxide semiconductor layer, the MoW, Ti, Al, and Cu used as the source and drain electrodes, and the silicon oxide (SiO x ) and silicon nitride (SiN x The etching rate of each material was calculated.
[0090] The samples for which the etching rate was measured will be described. A single film of each material was formed on a silicon wafer to obtain a sample of each material. Note that in the Poly-OS sample, an oxide semiconductor layer having a polycrystalline structure was formed by performing an OS annealing treatment after the formation of an oxide semiconductor film having an amorphous structure.
[0091] Wet etching (room temperature) of each material was performed using the etching solutions GHP-3 (manufactured by Kanto Chemical Co., Ltd.) containing a chelating agent and BTF-3 (manufactured by Kanto Chemical Co., Ltd.) containing phosphoric acid. After wet etching, the film thickness of each material was measured. Wet etching was performed under different etching time conditions for each material, and data on multiple film thicknesses with different etching times was obtained. A calibration curve was created based on the etching time and film thickness data, and the etching rate of each material was calculated. The calculated etching rates of each material are shown in Table 1. In Table 1, "less than 0.01 nm / sec" means that the film thickness before and after wet etching is roughly the same, and the film is hardly etched by wet etching.
[0092] [Table 1]
[0093] When GHP-3 is used as an etching solution, the etching rate of MoW is 0.14 nm / sec, whereas the etching rate of Poly-OS is less than 0.01 nm / sec. This means that, for example, when MoW is used as the conductive film (more specifically, the first metal film in contact with the oxide semiconductor layer 26) of the source electrode 32S and the drain electrode 32D of the semiconductor device 10, the oxide semiconductor layer 26 is hardly etched in the formation of the source electrode 32S and the drain electrode 32D by wet etching using GHP-3. Specifically, when the source electrode 32S and the drain electrode 32D have a MoW alloy single layer structure or a Cu / MoW structure, the oxide semiconductor layer 26 is hardly etched by GHP-3.
[0094] Furthermore, when BTF-3 is used as an etching solution, the etching rates of Ti and Al are 0.93 nm / sec and 0.92 nm / sec, respectively, whereas the etching rate of Poly-OS is less than 0.01 nm / sec. This means that, for example, when Ti is used as the conductive film (more specifically, the first metal film in contact with the oxide semiconductor layer 26) of the source electrode 32S and the drain electrode 32D of the semiconductor device 10, the oxide semiconductor layer 26 is hardly etched in the formation of the source electrode 32S and the drain electrode 32D by wet etching using BTF-3. Specifically, when the source electrode 32S and the drain electrode 32D have a Ti single layer structure, a Cu / Ti structure, or a Ti / Al / Ti structure, the oxide semiconductor layer 26 is hardly etched by BTF-3.
[0095] When BTF-3 was used as the etching solution, SiO x and SiN xis etched. This is because BTF-3 contains hydrofluoric acid. In contrast, Poly-OS has high etching resistance even to hydrofluoric acid, and is therefore hardly etched by BTF-3 containing hydrofluoric acid. Therefore, when the source electrode 32S and the drain electrode 32D are formed by wet etching using BTF-3, the gate insulating layer 16 may be etched more than the oxide semiconductor layer 26. In this case, the thickness of the gate insulating layer 16 in a region that does not overlap with the oxide semiconductor layer 26 is smaller than the thickness of the region that overlaps with the oxide semiconductor layer 26.
[0096] As shown in Table 1, Poly-OS is hardly etched by GHP-3 and BTF-3. Therefore, a resist pattern was formed on each material, and wet etching (at room temperature) was performed on each material using the resist pattern as a mask. After wet etching, the film thickness of each material was measured. The etching rate of each material was calculated based on the etching time and film thickness. The calculated etching rates of each material are shown in Table 2. Note that "less than 0.01 nm / min" in Table 2 means that the material is hardly etched by wet etching with an etching time of 5 minutes.
[0097] [Table 2]
[0098] As shown in Table 2, by increasing the etching time, the etching rate of Poly-OS for GHP-3 could be calculated. As a result, even when overetching for 1 minute was performed in the formation of the source electrode 32S and the drain electrode 32D by wet etching using BTF-3, the difference in film thickness between the source region or drain region and the channel region in the oxide semiconductor layer 26 was 1 nm or less. On the other hand, the etching rate of Poly-OS for BTF-3 could not be calculated. This means that Poly-OS has very high etching resistance against BTF-3. Therefore, when overetching for 1 minute was performed in the formation of the source electrode 32S and the drain electrode 32D by wet etching using BTF-3, the oxide semiconductor layer 26 including Poly-OS was hardly etched, and SiO x The gate insulating layer 16 including the oxide semiconductor layer 26 is etched by about 13 nm. In other words, in the oxide semiconductor layer 26, the difference in thickness between the source region or drain region and the channel region is 1 nm or less, and in the gate insulating layer 16, the difference in thickness between the region overlapping with the oxide semiconductor layer 26 and the region not overlapping with the oxide semiconductor layer 26 is 10 nm or more.
[0099] [Electrical characteristics] According to the flow chart shown in FIG. 3 of the first embodiment, the semiconductor device 10 was fabricated, and the electrical characteristics of the semiconductor device 10 were measured. In fabricating the semiconductor device 10, a Ti single-layer structure was used as the source electrode 32S and the drain electrode 32D. In fabricating the semiconductor device 10, the process of step S1008 in the flow chart shown in FIG. 3 was not performed. In addition, in order to investigate the influence of overetching in forming the source electrode 32S and the drain electrode 32D, the Ti single-layer structure was just etched with a mixture of ammonia water and hydrogen peroxide water (NH3 / H2O2 solution), and then multiple samples with different overetching conditions were fabricated. The conditions of each sample are shown in Table 3.
[0100] [Table 3]
[0101] FIG. 18 is a graph showing the electrical characteristics of each sample in the example. The horizontal axis of the graph in FIG. 18 is gate voltage (Vg), and the vertical axis is drain current (Id). FIG. 19 is a graph showing threshold values (Vth) calculated from the electrical characteristics of each sample in the example. FIG. 20 is a graph showing field effect mobility (field effect mobility in the linear region) calculated from the electrical characteristics of each sample in the example. The measurement conditions for the electrical characteristics are shown in Table 4.
[0102] [Table 4]
[0103] The graph of the electrical characteristics of each sample shown in Fig. 18 shows the measurement results of nine semiconductor devices 10 superimposed on each other. As can be seen from Fig. 18, the electrical characteristics of each sample are small. Also, as shown in Figs. 19 and 20, the threshold and field effect mobility of each sample are small. This is considered to be because the oxide semiconductor layer 26 is not etched when the source electrode 32S and the drain electrode 32D are formed, so that the shape of the oxide semiconductor layer 26 is not variably shaped, and the electrical characteristics are stable.
[0104] Fig. 19 also shows the average threshold value for each sample. As can be seen from Fig. 19, the average threshold value for each sample is a positive value, which indicates that the semiconductor device 10 is an enhancement type. Fig. 20 also shows the average field effect mobility for each sample. As can be seen from Fig. 20, the average field effect mobility for each sample is about 25.5 cm 2 / Vs, and the semiconductor device 10 is 20 cm 2 This indicates that the material has a field effect mobility of 100 / Vs or more.
[0105] Sample B-1 and Sample B-2 have different overetching times in wet etching using GHP-3, but no effect of the overetching time is observed. Sample C-1 and Sample C-2 have different overetching times in wet etching using BTF-3, but no effect of the overetching time is observed. Samples B-1 and B-2 and Samples C-1 and C-2 use different etchants in wet etching, but no effect of the difference in etchants is observed. The oxide semiconductor layer 26 containing Poly-OS has excellent etching resistance, and in the manufacture of the semiconductor device 10 using the oxide semiconductor layer 26, the process margin can be expanded. As a result, the yield in the manufacture of the semiconductor device 10 is improved.
[0106] The above-described embodiments and modifications of the present invention may be combined as appropriate as long as they are not mutually inconsistent. In addition, those in which a person skilled in the art appropriately adds or removes components or modifies designs, or adds or omits processes or modifies conditions, based on the semiconductor device and display device of each embodiment and modification are included in the scope of the present invention as long as they include the gist of the present invention.
[0107] Even if there are other effects and advantages different from those brought about by the aspects of each of the above-mentioned embodiments, those that are clear from the description in this specification or that can be easily predicted by a person skilled in the art are naturally understood to be brought about by the present invention. [Explanation of symbols]
[0108] 10: semiconductor device, 20: display device, 11: substrate, 12C: wiring, 12GE: gate electrode, 12W: wiring, 14: gate insulating layer, 15: contact hole, 16: gate insulating layer, 22: oxide semiconductor film, 24: oxide semiconductor layer, 26: oxide semiconductor layer, 32C: wiring, 32D: drain electrode, 32S: source electrode, 32W: wiring, 34: interlayer insulating layer, 36: metal oxide film, 38: interlayer insulating layer, 39: insulating layer, 42C: common electrode, 44: insulating layer, 46C: electrode, 46P: pixel electrode, 110: driving transistor, 120: selection transistor, 210: storage capacitor, 211: signal line, 212: gate line, 213: anode power line, 214: cathode power line, 220: liquid crystal region, 240: sealing region, 260: terminal region, 300: array substrate, 301: pixel circuit, 302: source driver circuit, 303: gate driver circuit, 304: source wiring, 305: gate wiring, 306: terminal section, 307: connection wiring, 310: sealing section, 311: liquid crystal element, 320: opposing substrate, 330: flexible printed circuit board, 340: chip, 350: storage capacitor, 362: insulating layer, 363: opening, 390: pixel electrode, 392: light-emitting layer, 394: common electrode
Claims
1. A gate electrode; a gate insulating layer on the gate electrode; an oxide semiconductor layer having a polycrystalline structure on the gate insulating layer; a source electrode and a drain electrode on the oxide semiconductor layer; an interlayer insulating layer covering the source electrode and the drain electrode and in contact with the oxide semiconductor layer; the oxide semiconductor layer includes a first region overlapping one of the source electrode and the drain electrode and a second region in contact with the interlayer insulating layer; A semiconductor device, wherein a difference between a film thickness of the first region and a film thickness of the second region is 1 nm or less.
2. the source electrode and the drain electrode include a first metal layer; an etching rate of the first metal layer with respect to an etching solution used in forming the first metal layer is 0.1 nm / sec or more; The semiconductor device according to claim 1 , wherein the etching rate of the oxide semiconductor layer with respect to the etching solution is less than 0.01 nm.
3. the source and drain electrodes further comprising a second metal layer comprising copper on the first metal layer; 3. The semiconductor device according to claim 2, wherein an etching rate of said second metal layer with respect to said etching solution is 0.5 nm / sec or more.
4. The semiconductor device according to claim 3 , wherein the first metal layer comprises molybdenum.
5. The semiconductor device according to claim 3 , wherein the etching solution contains a chelating agent.
6. The semiconductor device according to claim 2 , wherein the etching rate of the first metal layer is 0.5 nm / sec or more.
7. the source and drain electrodes further comprising a second metal layer comprising copper on the first metal layer; 7. The semiconductor device according to claim 6, wherein an etching rate of said second metal layer with respect to said etching solution is 1.0 nm / sec or more.
8. The semiconductor device according to claim 7 , wherein the first metal layer comprises titanium.
9. The semiconductor device according to claim 7 , wherein the etching solution contains phosphoric acid.
10. the oxide semiconductor layer contains indium and at least one metal element; 10. The semiconductor device according to claim 1, wherein a ratio of the indium element to the at least one metal element is 50% or more.
11. forming a gate electrode; forming a gate insulating layer on the gate electrode; forming an oxide semiconductor layer having a polycrystalline structure on the gate insulating layer; forming a source electrode and a drain electrode on the oxide semiconductor layer; forming an interlayer insulating layer covering the source electrode and the drain electrode and in contact with the oxide semiconductor layer; the oxide semiconductor layer includes a first region overlapping one of the source electrode and the drain electrode and a second region in contact with the interlayer insulating layer; A method for manufacturing a semiconductor device, wherein a difference between a film thickness of the first region and a film thickness of the second region is 1 nm or less.
12. The formation of the source electrode and the drain electrode includes: A first metal film is formed; forming a second metal film on the first metal film; using an etchant to etch the first metal film and the first metal film to form a first metal layer and a second metal layer on the first metal layer; an etching rate of the first metal film with respect to the etching solution is 0.1 nm / sec or more; The method for manufacturing a semiconductor device according to claim 11 , wherein an etching rate of the oxide semiconductor layer with respect to the etching solution is less than 0.
01.
13. the second metal film includes copper; 13. The method for manufacturing a semiconductor device according to claim 12, wherein an etching rate of the second metal film with respect to the etching solution is 0.5 nm / sec or more.
14. The method for manufacturing a semiconductor device according to claim 13 , wherein the first metal film contains molybdenum.
15. The method for manufacturing a semiconductor device according to claim 13 , wherein the etching solution contains a chelating agent.
16. The method for manufacturing a semiconductor device according to claim 12 , wherein the etching rate of the first metal film is 0.5 nm / sec or more.
17. the second metal film includes copper; 17. The method for manufacturing a semiconductor device according to claim 16, wherein an etching rate of the second metal film with respect to the etching solution is 1.0 nm / sec or more.
18. The method for manufacturing a semiconductor device according to claim 17 , wherein the first metal film contains titanium.
19. The method for manufacturing a semiconductor device according to claim 17 , wherein the etching solution contains phosphoric acid.
20. the oxide semiconductor layer contains indium and at least one metal element; 20. The method for manufacturing a semiconductor device according to claim 11, wherein a ratio of the indium element to the indium element and the at least one or more metal elements is 50% or more.
Citation Information
Patent Citations
Multilayer film including oxide semiconductor film and manufacturing method for semiconductor device
JP2014099601A
Semiconductor device
JP2016184771A
Semiconductor device and display device having semiconductor device
JP2018006730A
Semiconductor device manufacturing method
JP2021108405A
Manufacturing method for semiconductor device
JP2021141338A