Optical glass and optical element

By using specific glass components and an oxidizing gas contact method, the method addresses noble metal oxidation in optical glass manufacturing, achieving high refractive index and transparency while preventing coloration and tank deterioration.

JP2024163773APending Publication Date: 2024-11-22OHARA INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023079648
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing optical glass manufacturing methods using noble metal melting tanks face issues with noble metal oxidation and dissolution into the glass, leading to reduced glass quality and coloration, especially when high refractive index components are used.

Method used

Incorporating a predetermined amount of Ln2O3, TiO2, Nb2O5, WO3, and Bi2O3 components into the glass, and contacting the molten glass surface with an oxidizing gas to suppress reduction and coloration, while maintaining high refractive index and transparency.

Benefits of technology

The method produces high-quality optical glass with reduced coloration and improved transmittance, ensuring high refractive index and Abbe number without deteriorating the melting tank.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163773000001_ABST
    Figure 2024163773000001_ABST
Patent Text Reader

Abstract

To provide a high-refractive-index optical glass with high quality and superior transmittance.SOLUTION: An optical glass contains, in mass%, a total of 10.0% or more of Ln2O3 component (where Ln is at least one selected from the group consisting of La, Gd, Y, and Yb) and at least one selected from the group consisting of TiO2 component, Nb2O5 component, WO3 component and Bi2O3 component. Exposing an oxidation gas to the surface of the molten glass containing the above-mentioned components yields the optical glass.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical glass and an optical element. [Background technology]

[0002] As optical instruments and the like continue to improve in performance and functionality, the demands on the optical lenses used in these optical instruments are also increasing. Specifically, there is a demand for optical glass that has high internal homogeneity, extremely high transmittance, and satisfies optical properties such as refractive index and Abbe number.

[0003] High refractive index optical glass usually contains large amounts of high refractive index components such as TiO2, Nb2O5, WO3, and Bi2O3 as glass components. These components are easily reduced during the glass melting process, and there is a problem that the reduced components cause coloring of the glass. For this reason, various technologies have been proposed to reduce the reduction color in optical glass.

[0004] For example, Patent Document 1 proposes that oxidizing gas is bubbled through molten glass to suppress the reduction of high refractive index components and reduce coloring of the glass during the melting process. However, when optical glass is manufactured using such a technique, the problem of the precious metal material constituting the melting tank being dissolved in the molten glass becomes prominent. That is, when manufacturing glass with extremely high transparency and homogeneity such as optical glass, a melting tank whose container surface is made of a precious metal material such as platinum is used to melt the glass raw materials, and the precious metal may react with oxygen to produce a precious metal oxide such as PtO2. When such a precious metal oxide is dissolved in the molten glass, it leads to a deterioration in the quality of the glass, such as a decrease in transmittance and the generation of knots, and further accelerates the deterioration of the melting tank. In addition, when melting glass containing a large amount of high refractive index components, the precious metal material is oxidized by the bubbling of oxidizing gas to become Pt 4+ These precious metal ions also dissolve into the molten glass and cause coloring. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-12852 A Summary of the Invention [Problem to be solved by the invention]

[0006] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a high refractive index optical glass that is of high quality and has excellent transmittance. [Means for solving the problem]

[0007] The present inventors have discovered that an optical glass with reduced reduction color can be obtained by bringing an oxidizing gas into contact with the surface of a molten glass containing a predetermined amount of an Ln2O3 component (wherein Ln represents at least one selected from the group consisting of La, Gd, Y, and Yb) and at least one selected from the group consisting of a TiO2 component, a Nb2O5 component, a WO3 component, and a Bi2O3 component. That is, the gist of the present invention is as follows.

[0008] [1] In weight percent: Ln2O3 component (wherein Ln represents at least one selected from the group consisting of La, Gd, Y, and Yb) in a total content of 10.0% or more, At least one selected from the group consisting of a TiO2 component, a Nb2O5 component, a WO3 component, and a Bi2O3 component; Including, An optical glass obtained by bringing an oxidizing gas into contact with the surface of molten glass containing the above components. [2] An optical element made of the optical glass described in [1]. Effect of the Invention

[0009] According to the present invention, an optical glass with reduced reduction color can be obtained by bringing an oxidizing gas into contact with the surface of a molten glass containing a predetermined amount of an Ln2O3 component (wherein Ln represents at least one selected from the group consisting of La, Gd, Y, and Yb), and at least one selected from the group consisting of a TiO2 component, a Nb2O5 component, a WO3 component, and a Bi2O3 component. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view of one embodiment of an apparatus used in the manufacturing method of the present invention. [Diagram 2] 4 is a schematic cross-sectional view of another embodiment of an apparatus used in the manufacturing method of the present invention. FIG. [Diagram 3] 4 is a schematic cross-sectional view of another embodiment of an apparatus used in the manufacturing method of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Glass components] In this specification, the content of each component constituting the optical glass is expressed as mass% relative to the total mass of the composition converted into oxides, unless otherwise specified. Here, the "composition converted into oxides" refers to a composition that expresses each component contained in the glass, assuming that oxides, complex salts, metal fluorides, etc. used as raw materials for the glass components are all decomposed and converted into oxides during melting, with the total mass of the oxides produced being 100 mass%. The composition ranges of each component constituting the optical glass according to the present invention will be explained below.

[0012] The optical glass according to the present invention contains the Ln2O3 component in a total content of 10.0% or more, where Ln represents one or more elements selected from the group consisting of La, Gd, Y, and Yb. The optical glass according to the present invention contains the above components in a total content of 10.0% or more.

[0013] The Ln2O3 component (wherein Ln is one or more selected from the group consisting of La, Y, Gd, and Yb) can increase the refractive index of glass, but if contained in excess, it increases the devitrification tendency of glass. Therefore, the lower limit of the sum of the contents of the Ln2O3 components is preferably 35.0% or more, more preferably 40.0% or more, even more preferably 45.0% or more, and even more preferably 50.0% or more. On the other hand, the upper limit of the sum of the contents of the Ln2O3 components is preferably 70.0% or less, more preferably 65.0% or less, even more preferably 60.0% or less, and even more preferably 55.0% or less.

[0014] The La2O3 component, in which Ln is La, is a component that increases the refractive index of the glass and improves the chemical durability of the glass, and is an essential component in the optical glass of the present invention. In particular, by making the content of the La2O3 component 65.0% or less, the Abbe number can be increased while improving the devitrification resistance of the glass. Therefore, the content of the La2O3 component relative to the total mass of the glass in terms of oxides is preferably set to an upper limit of 65.0% or less, more preferably set to an upper limit of 62.0% or less, and most preferably set to an upper limit of 59.0% or less. On the other hand, the content of the La2O3 component relative to the total mass of the glass in terms of oxides is preferably set to an upper limit of 30.0% or more, more preferably set to an upper limit of 35.0% or more, and most preferably set to an upper limit of 40.0% or more.

[0015] The Gd2O3 component, in which Ln is Gd, is a component that increases the refractive index of the glass and increases the Abbe number when the content exceeds 0%. In particular, by making the content of the Gd2O3 component 20.0% or less, it is possible to obtain the desired optical number while improving the devitrification resistance of the glass. Therefore, the content of the Gd2O3 component relative to the total mass of the glass in terms of oxide composition is preferably 20.0% or less, more preferably 15.0% or less, more preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0016] The Y2O3 component, whose Ln is Y, is a component that increases the refractive index of the glass and increases the Abbe number when it is contained at more than 0%. In particular, by making the content of the Y2O3 component 15.0% or less, it is possible to obtain the desired optical number while increasing the devitrification resistance of the glass. Therefore, the upper limit of the content of the Y2O3 component relative to the total mass of the glass in terms of oxides is preferably 15.0% or less, more preferably 12.0% or less, and most preferably 11.0% or less. On the other hand, the lower limit of the content of the Y2O3 component relative to the total mass of the glass in terms of oxides is preferably more than 0%, more preferably 3.0% or more, and most preferably 5.0% or more.

[0017] The Yb2O3 component, in which Ln is Yb, is a component that increases the refractive index of the glass and increases the Abbe number when the content exceeds 0%. In particular, by making the content of the Yb2O3 component 5.0% or less, it is possible to obtain the desired optical number while improving the devitrification resistance of the glass. Therefore, the upper limit of the content of the Yb2O3 component relative to the total mass of the glass in terms of oxide composition is preferably 5.0% or less, more preferably 3.0% or less, and most preferably 1.0% or less.

[0018] The optical glass of the present invention can increase the refractive index and dispersion by including at least one component selected from the group consisting of TiO2, Nb2O5, WO3, and Bi2O3. In particular, by setting the mass sum of TiO2+Nb2O5+WO3+Bi2O3 to 5.0% or more and 35.0% or less, the refractive index (n d ) while reducing the reduction color derived from the high refractive index component. Therefore, the mass sum of TiO2+Nb2O5+WO3 is preferably 5.0% or more, more preferably 7.0% or more, more preferably 12.0% or more, more preferably 15.5% or more, and even more preferably 20.0% or more as the lower limit. On the other hand, the upper limit of the mass sum of TiO2+Nb2O5+WO3 is preferably 35.0% or less, more preferably 30.0% or less, and further preferably 27.0% or less.

[0019] The TiO2 component is a component that increases the refractive index of glass and enhances the chemical durability of glass when it is contained at more than 0%. In particular, by containing the TiO2 component, a high refractive index can be obtained. On the other hand, by making the content of the TiO2 component 25.0% or less, it is possible to suppress devitrification due to excessive content and to suppress deterioration of transmittance. The content of the TiO2 component relative to the total mass of the glass in terms of oxide composition is preferably more than 0%, more preferably 3.0% or more, and most preferably 6.0% or more as the lower limit. On the other hand, the content of the TiO2 component relative to the total mass of the glass in terms of oxide composition is preferably 25.0% or less, more preferably 20.0% or less, and most preferably 15.0% or less as the upper limit.

[0020] The Nb2O5 component is a component that increases the refractive index and Abbe number of the glass when it is contained at more than 0%, while the stability and devitrification resistance of the glass can be improved by making the content of the Nb2O5 component 15.0% or less. Therefore, the upper limit of the content of the Nb2O5 component relative to the total mass of the glass calculated as oxide is preferably 15.0% or less, more preferably 13.0% or less, and most preferably 11.0% or less.

[0021] The WO3 component is a component that increases the refractive index of glass when it is contained at more than 0%. In particular, by making the content of the WO3 component 15.0% or less, it is possible to increase the devitrification resistance of the glass and suppress a decrease in the transmittance of the glass for short-wavelength visible light. Therefore, the upper limit of the content of the WO3 component relative to the total mass of the glass in terms of oxide composition is preferably 15.0% or less, more preferably 10.0% or less, and most preferably 5.0% or less.

[0022] The B2O3 component is a component that promotes the formation of stable glass and thereby enhances resistance to devitrification. In particular, by making the content of the B2O3 component 25.0% or less, the decrease in refractive index caused by the B2O3 component is suppressed, making it easier to obtain a high refractive index. Therefore, the content of the B2O3 component relative to the total mass of the glass in terms of oxides is preferably set to an upper limit of 25.0%, more preferably set to an upper limit of 20.0%, and even more preferably set to an upper limit of 15.0%. On the other hand, the content of the B2O3 component relative to the total mass of the glass in terms of oxides is preferably set to an upper limit of 3.0% or more, more preferably set to an upper limit of 4.0% or more, and most preferably set to an upper limit of 5.0% or more.

[0023] When the SiO2 component is contained at more than 0%, it is an optional component in the optical glass of the present invention, which reduces the coloring of the glass, thereby increasing the transmittance of short-wavelength visible light, and promotes stable glass formation, thereby increasing the devitrification resistance of the glass. In particular, by making the content of the SiO2 component 20.0% or less, the decrease in refractive index caused by the SiO2 component is suppressed, making it easier to obtain a high refractive index. Therefore, the content of the SiO2 component relative to the total mass of the glass in terms of oxides is preferably 20.0% or less, more preferably 15.0% or less, more preferably 12.0% or less, and most preferably 9.0% or less as the upper limit. On the other hand, the content of the SiO2 component relative to the total mass of the glass in terms of oxides is preferably more than 0%, more preferably 1.0% or more, and most preferably 2.0% or more as the lower limit.

[0024] The Al2O3 component is an optional component in the optical glass of the present invention, which improves the chemical durability of the glass while increasing the viscosity of the glass when melted, when the content exceeds 0%. In particular, by making the content of the Al2O3 component 10.0% or less, the meltability of the glass can be improved while the tendency of the glass to devitrify can be reduced. Therefore, the upper limit of the content of the Al2O3 component relative to the total mass of the glass calculated as oxide is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0025] The ZrO2 component, when contained at more than 0%, reduces the coloring of the glass and increases the transmittance for short-wavelength visible light, while promoting stable glass formation and increasing the devitrification resistance of the glass, and is an optional component in the optical glass of the present invention. On the other hand, by making the content of the ZrO2 component 15.0% or less, devitrification due to excessive inclusion of the ZrO2 component can be reduced. Therefore, the content of the ZrO2 component relative to the total mass of the glass in terms of oxides is preferably set at an upper limit of 15.0% or less, more preferably at an upper limit of 12.0% or less, and most preferably at an upper limit of 9.0% or less. On the other hand, the content of the ZrO2 component relative to the total mass of the glass in terms of oxides is preferably set at a lower limit of more than 0%, more preferably at least 1.0%, and most preferably at least 3.0%.

[0026] The ZnO component is an optional component in the optical glass of the present invention, which lowers the liquidus temperature of the glass and increases the devitrification resistance of the glass when it is contained at more than 0%. In particular, by making the content of the ZnO component 15.0% or less, it is possible to easily obtain a high refractive index and low dispersion. Therefore, the upper limit of the content of the ZnO component relative to the total mass of the glass calculated as oxide is preferably 15.0% or less, more preferably 12.0% or less, and most preferably 9.0% or less.

[0027] The MgO component is an optional component that, when contained at more than 0%, lowers the liquidus temperature of the glass and increases the devitrification resistance of the glass, and also prevents the transmittance of visible light from decreasing, and is an optional component in the optical glass of the present invention. In particular, by making the content of the MgO component 10.0% or less, it is possible to easily obtain a high refractive index and low dispersion. Therefore, the content of the MgO component relative to the total mass of the glass calculated as oxide is preferably set to an upper limit of 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0028] The CaO component is an optional component in the optical glass of the present invention, which lowers the liquidus temperature of the glass and increases the devitrification resistance of the glass when it is contained at more than 0%. In particular, by making the CaO content 10.0% or less, it is possible to easily obtain a high refractive index and low dispersion, and to suppress the deterioration of the devitrification resistance and chemical durability of the glass. Therefore, the upper limit of the CaO content relative to the total mass of the glass calculated as oxide is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0029] The SrO component is an optional component in the optical glass of the present invention, which lowers the liquidus temperature of the glass and increases the devitrification resistance of the glass when it is contained at more than 0%. In particular, by making the content of the SrO component 10.0% or less, it is possible to easily obtain a high refractive index and low dispersion, and to suppress the deterioration of the devitrification resistance and chemical durability of the glass. Therefore, the content of the SrO component relative to the total mass of the glass calculated as oxide is preferably set to an upper limit of 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0030] The BaO component is an optional component in the optical glass of the present invention, which increases the refractive index of the glass and enhances the devitrification resistance of the glass when it is contained at more than 0%, and also prevents the transmittance of visible light from decreasing. In particular, by making the content of the BaO component 10.0% or less, it is possible to easily obtain a high refractive index and low dispersion, and to suppress the decrease in devitrification resistance and chemical durability. Therefore, the upper limit of the content of the BaO component relative to the total mass of the glass in terms of oxide composition is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0031] The Li2O component is an optional component in the optical glass of the present invention, which lowers the melting temperature of the glass when the content exceeds 0%. In particular, by making the content of the Li2O component 10.0% or less, a high refractive index can be easily obtained, and the stability of the glass can be improved to reduce the occurrence of devitrification. Therefore, the upper limit of the content of the Li2O component relative to the total mass of the glass calculated as oxide is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0032] The Na2O component is an optional component in the optical glass of the present invention, which lowers the melting temperature of the glass when the content exceeds 0%. In particular, by making the content of the Na2O component 10.0% or less, a high refractive index can be easily obtained, and the stability of the glass can be improved to reduce the occurrence of devitrification, etc. Therefore, the upper limit of the content of the Na2O component relative to the total mass of the glass calculated as oxide is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0033] The K2O component is an optional component in the optical glass of the present invention, which lowers the melting temperature of the glass when it is contained at more than 0%. In particular, by making the content of the K2O component 10.0% or less, it is possible to easily obtain a high refractive index, and to increase the stability of the glass and reduce the occurrence of devitrification, etc. Therefore, the content of the K2O component relative to the total mass of the glass calculated as oxide is preferably set to an upper limit of 10.0% or less, more preferably 5.0% or less, and even more preferably 3.0% or less.

[0034] The Ta2O5 component is a component that can increase the refractive index of the glass and improve the devitrification resistance when the Ta2O5 component is contained in an amount exceeding 0%. The upper limit of the Ta2O5 component content is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.

[0035] The P2O5 component is a component that can lower the liquidus temperature of glass and improve devitrification resistance when the content exceeds 0%. The upper limit of the P2O5 component content is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.

[0036] The GeO2 component is a component that can increase the refractive index of the glass and improve the devitrification resistance when the GeO2 component content exceeds 0%. The upper limit of the GeO2 component content is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.

[0037] The Ga2O3 component is a component that can improve the chemical durability of the glass and the devitrification resistance of the molten glass when the Ga2O3 component content exceeds 0%. The upper limit of the Ga2O3 component content is 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.

[0038] The Bi2O3 component is a component that can increase the refractive index and lower the glass transition point when contained at more than 0%. The upper limit of the content of the Bi2O3 component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.

[0039] The TeO2 component is a component that can increase the refractive index and lower the glass transition point when contained at more than 0%. The upper limit of the content of the TeO2 component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.

[0040] The SnO2 component is a component that, when contained at more than 0%, reduces oxidation of the molten glass to clarify it and increases the visible light transmittance of the glass. The upper limit of the content of the SnO2 component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.

[0041] The F component is a component that can improve the meltability of glass when it is contained at more than 0%, but on the other hand, a high content of the F component leads to devitrification due to volatilization of the F component. The upper limit of the F component content is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.

[0042] The Sb2O3 component is an optional component that promotes clarification and defoaming when melting glass. By making the content of the Sb2O3 component 0.1% or less, it is possible to suppress coloring, particularly in high refractive index glass. Furthermore, by making the content 0.1% or less, excessive foaming during glass melting is unlikely to occur, making it difficult for the Sb2O3 component to be alloyed with the melting equipment (particularly precious metals such as Pt). Therefore, the upper limit of the content of the Sb2O3 component is preferably 0.1% or less, more preferably 0.08% or less, and even more preferably 0.05% or less, but it may be 0%.

[0043] The component for clarifying and defoaming the glass is not limited to the above Sb2O3 component, and any fining agent, defoaming agent or combination thereof known in the field of glass manufacturing can be used.

[0044] The C component is a component that can maintain a reducing atmosphere in the platinum crucible, suppress the incorporation of platinum into the glass due to oxidation, and improve the transmittance, but if the content is high, the cationic components in the glass are reduced, causing coloring of the glass. Therefore, the content of the C component is preferably 8.0% or less, more preferably 5.0% or less, more preferably 3.0% or less, and most preferably 1.0% or less as the upper limit. On the other hand, the content of the C component is preferably more than 0%, more preferably 0.3% or more, even more preferably 0.5% or more, and most preferably 0.8% or more as the lower limit, but may be 0%.

[0045] The S component is a component that can maintain a reducing atmosphere in the platinum crucible, suppress the incorporation of platinum into the glass due to oxidation, and improve the transmittance, but if the content is high, the cationic components in the glass are reduced, causing coloring of the glass. Therefore, the content of the S component is preferably 8.0% or less, more preferably 5.0% or less, more preferably 3.0% or less, and most preferably 1.0% or less as the upper limit. On the other hand, the content of the S component is preferably more than 0%, more preferably 0.3% or more, even more preferably 0.5% or more, and most preferably 0.8% or more as the lower limit, but may be 0%.

[0046] Organic components such as sucrose are components that can maintain a reducing atmosphere in the platinum crucible, suppress the incorporation of platinum into the glass due to oxidation, and improve the transmittance, but if the content is high, the cationic components in the glass are reduced, causing coloring of the glass. Therefore, the content of organic components such as sucrose is preferably 10.0% or less, more preferably 8.0% or less, more preferably 6.0% or less, and most preferably 5.0% or less as the upper limit. On the other hand, the content of organic components such as sucrose is preferably more than 0%, more preferably 0.5% or more, even more preferably 1.0% or more, and most preferably 2.0% or more as the lower limit, but may be 0%.

[0047] The components that reduce glass are not limited to the above-mentioned C component, S component, and organic components such as sucrose, but any reducing agent known in the field of glass manufacturing or a combination thereof can be used.

[0048] <Ingredients that should not be included> Next, components that should not be contained in the optical glass of the present invention and components whose inclusion is undesirable will be described.

[0049] Other components not mentioned above may be added as necessary to the extent that they do not impair the properties of the glass of the present invention. However, transition metal components such as Ce, V, Cr, Mn, Fe, Co, Ni, Cu, Ag, and Mo, even when contained alone or in combination in small amounts, tend to color the glass and absorb specific wavelengths in the visible range, thereby reducing the effect of increasing the visible light transmittance of the present invention. Therefore, it is preferable that glass that transmits wavelengths in the visible range in particular does not substantially contain these components.

[0050] Furthermore, since lead compounds such as PbO and arsenic compounds such as As2O3 are components that have a high environmental impact, it is desirable that they are not contained substantially, that is, that they are not contained at all except for unavoidable contamination.

[0051] Furthermore, in recent years, there has been a trend to refrain from using the components Th, Cd, Tl, Os, Be, and Se as harmful chemical substances, and if they are used, environmental measures are required not only in the glass manufacturing process but also in the processing process and disposal after commercialization. Therefore, when environmental impact is important, it is preferable that these components are not substantially contained.

[0052] [Method of manufacturing optical glass] The optical glass according to the present invention can reduce the reduction color of the glass by contacting the surface of the molten glass with an oxidizing gas. The molten glass includes glass in the melting step, the fining step, the homogenizing step, and the forming step, and is characterized in that the surface of the molten glass is contacted with an oxidizing gas in an oxidizing gas atmosphere in at least one of the fining step, the homogenizing step, and the forming step. When oxygen gas is bubbled into the molten glass as in the conventional method, the precious metal elements (e.g., platinum) constituting the surface of the melting tank also react with oxygen, and the precious metal oxide is dissolved in the molten glass, resulting in a decrease in the transmittance and the generation of knots, which deteriorates the quality of the glass. In the present invention, the reduction color can be reduced by contacting the surface of the molten glass with an oxidizing gas in an oxidizing gas atmosphere in at least one of the fining step, the homogenizing step, and the forming step. Each step of the method for producing the optical glass of the present invention will be described in detail below.

[0053] [Melting process of glass raw materials] As the glass raw materials, a blended raw material (batch raw material) obtained by appropriately selecting the above-mentioned glass components and weighing and thoroughly mixing the raw materials corresponding to the glass components so as to obtain an optical glass with the desired characteristics, or a blended cullet can be used.

[0054] When cullet is used as the glass raw material, a cullet forming step (rough melting step) in which the batch raw material is roughly melted to form cullet is carried out before the melting step (remelting step). In addition, the refractive index of the cullet is preferably measured in advance, and each cullet may be mixed to obtain a desired refractive index value to form a blended cullet.

[0055] As a melting vat for heating and melting glass raw materials, a container or device made of a refractory material such as quartz may be used, or a melting vat whose inner wall (the surface that comes into contact with the molten glass) is made of a precious metal element may be used. The shape of the melting vat is not particularly limited, but for example, a container with an open top and whose inner wall is made of a platinum-containing alloy such as platinum-rhodium or platinum-gold, or a precious metal such as rhodium, gold, iridium, or palladium can be suitably used.

[0056] The melting tank is equipped with a heating means such as a heating element or high-frequency induction, and the glass raw materials are melted by the heating. The heating means preferably performs heating so as to keep the temperature of the molten glass almost constant. This makes it easier to proceed with melting and vitrification by dividing it into multiple steps, and reduces the rate at which bubbles are generated from the glass raw materials and molten glass, improving the thermal uniformity of the glass raw materials and molten glass, and allowing the production of optical glass with more uniform composition and characteristics.

[0057] The temperature at which the glass frit is melted in the melting step is appropriately selected from among temperatures at which the glass frit can be melted and vitrified after cooling. More specifically, the lower limit of the melting temperature is preferably 1100°C or higher, more preferably 1150°C or higher, and most preferably 1200°C or higher. The upper limit of the melting temperature is preferably less than 1500°C, more preferably less than 1450°C, and most preferably less than 1400°C. By setting the melting temperature in this range, it is possible to prevent the glass frit from remaining unmelted. In the present specification, the "melting temperature" refers to the average value of the temperature of the glass frit at the upper part of the melting tank and the temperature of the glass frit at the lower part of the melting tank.

[0058] The melting time is not particularly limited as long as it is a time sufficient for all unmelted glass to disappear, and can be appropriately adjusted depending on the amount of glass raw materials and the melting temperature.

[0059] The melting may be continuous, in which the glass raw materials are continuously charged into the melting tank, or batch melting, in which the glass raw materials are melted one at a time. When the continuous melting is performed, it is preferable to use a continuous melting tank. The continuous melting tank will be described later.

[0060] [Clarification process] Next, the molten glass is refined. The fining step is a step of degassing and defoaming the glass that has been through the melting step to remove dissolved gaseous components and bubbles, and also to further advance vitrification. By carrying out the fining step, it is possible to reduce devitrification of the glass.

[0061] The fining temperature is appropriately selected from temperatures at which vitrification can proceed, but is preferably higher than the melting temperature. More specifically, the lower limit of the fining temperature is preferably 1300°C or higher, more preferably 1350°C or higher, and most preferably 1400°C or higher. The upper limit is preferably less than 1450°C, more preferably less than 1500°C, and most preferably less than 1550°C. By setting the fining temperature within this range, the melt viscosity of the molten glass can be reduced, making it easier to remove dissolved gasified components and bubbles.

[0062] When the fining step is carried out using a continuous melting tank, a fining tank separate from the melting tank will be used. The shape of the fining tank is not particularly limited, and for example, a vessel with an open top and an inner wall made of platinum-containing alloys such as platinum-rhodium or platinum-gold, or precious metals such as rhodium, gold, iridium, or palladium can be suitably used.

[0063] It is preferable to shorten the fining time within a range that effectively removes dissolved gaseous components and bubbles and inhibits coloring of the glass.

[0064] [Homogenization process] The clarified molten glass is then stirred to homogenize it. The homogenization step is a step for homogenizing the molten glass to reduce striae and the like in the formed glass, and also for adjusting the viscosity of the molten glass so that it is suitable for forming.

[0065] Stirring may be performed by a stirrer equipped with a stirring blade at the tip of the rotating shaft. In this case, it is preferable to arrange the stirring device so that the stirring blade rotates along the bottom surface of the melting tank (or the homogenization tank when a continuous melting tank is used). This allows the molten glass to be stirred until just before the stirred tank becomes empty even when the molten glass is discharged from the stirred tank, and reduces the formation of bubbles from the start to the end of the outflow process. The material of the parts that come into contact with the molten glass, such as the stirring blades and rotating shaft, is appropriately selected from materials that have low reactivity with the molten glass and can withstand the temperature of the stirring process. More specifically, the above-mentioned noble metals can be suitably used.

[0066] The temperature at which the homogenization step is carried out (stirring temperature) is preferably equal to or lower than the fining temperature. More specifically, the upper limit of the stirring temperature is preferably less than 1350°C, more preferably less than 1300°C, and most preferably less than 1250°C. The lower limit of the stirring temperature is preferably equal to or higher than 1100°C, more preferably equal to or higher than 1150°C, and most preferably equal to or higher than 1200°C. Within this temperature range, air bubbles can be removed and the molten glass can be made uniform.

[0067] The time for which the homogenization step is carried out is not particularly limited as long as it is within a range in which the clarified molten glass can be homogenized and the viscosity can be adjusted to an appropriate level.

[0068] [Molding process] Next, the molten glass that has been subjected to the homogenization step is made to flow out of the melting tank and formed. For example, an outflow pipe extending from the bottom of the melting tank is provided, and the molten glass is made to flow out through the outflow pipe.

[0069] The outflow temperature is preferably lower than the fining temperature and the stirring temperature. More specifically, the outflow temperature in the outflow step is preferably less than 1300°C, more preferably less than 1250°C, and most preferably less than 1200°C. The lower limit of the outflow temperature is preferably 1000°C or higher, more preferably 1050°C or higher, and most preferably 1100°C or higher. By setting the outflow temperature within the above range, the fluidity of the molten glass can be kept constant. Note that the outflow temperature here does not mean the temperature of the melting tank, but the temperature of the molten glass flowing through the outflow pipe.

[0070] The molten glass flowing out of the melting tank is formed into a predetermined shape. In the forming step, any known forming method can be appropriately used as long as it can form the molten glass into a predetermined shape. For example, the molten glass may be poured into a mold to form a block, or the molten glass flow that flows down from an outlet pipe may be cut into pieces of a certain length (certain amount) to form glass blocks. Furthermore, if more precise shaping is performed in a subsequent step, the shapes of the individual pieces of glass obtained through the forming step do not need to be uniform.

[0071] [Contact with oxidizing gas] In the present invention, in at least one of the above-mentioned fining step, homogenizing step, and forming step, an oxidizing gas is brought into contact with the surface of the molten glass in an oxidizing gas atmosphere. By bringing an oxidizing gas into contact with the surface of the molten glass without bubbling the oxidizing gas, it is possible to reduce the reduction color of the glass and suppress deterioration of the melting tank.

[0072] The oxidizing gas is not particularly limited, but for example, oxygen, halogenated oxygen, etc. can be used.

[0073] In order to create an oxidizing gas atmosphere in the melting tank, in the fining and homogenizing steps, the oxidizing gas can be sprayed from the upper opening of the melting tank to bring the oxidizing gas into contact with the surface of the molten glass. In the forming step, when the molten glass is discharged through the outflow pipe and formed, the oxidizing gas is preferably sprayed onto the surface of the formed product. Although the surrounding atmosphere (air) can contribute to a certain degree of reduction in the reduction of the reduction color by contacting the molten glass, it cannot be said to be sufficient. In the present invention, the reduction color of the glass can be reduced by creating an oxidizing gas atmosphere on the surface of the molten glass by spraying the oxidizing gas, etc., and bringing the oxidizing gas into contact with the surface. In this case, the flow rate of the oxidizing gas can be appropriately changed depending on the volume of the melting tank. The reduction color reduction effect can be improved by keeping the melting tank in a substantially sealed state. Furthermore, when an oxidizing gas is blown onto the molten glass from an upper opening of the melting vat, the closer the blowing position is to the surface of the molten glass, the greater the effect of reducing reduction color in the glass.

[0074] The contact with the oxidizing gas may be carried out continuously or intermittently while the molten glass is stored in the melting tank.

[0075] As an embodiment of contacting the oxidizing gas with the surface of the molten glass, it is preferable to spray the oxidizing gas onto the surface of the molten glass. In this case, the position from which the oxidizing gas is sprayed is preferably close to the surface of the molten glass in order to create an oxidizing gas atmosphere on the glass surface, and for example, it is preferable to spray the oxidizing gas from a position 200 mm or less, 150 mm or less, 100 mm or less, 90 mm or less, 80 mm or less, 70 mm or less, 60 mm or less, 50 mm or less, or 40 mm or less above the surface of the molten glass. On the other hand, the position at which the oxidizing gas is blown is preferably separated from the surface of the molten glass to such an extent that no air bubbles are generated inside the molten glass; for example, the oxidizing gas is preferably blown from a position more than 0 mm, 5 mm or more, or 10 mm or more above the surface of the molten glass.

[0076] As an embodiment of the present invention, in the fining step and the homogenizing step, the interior of each melting vat is preferably made to be an oxidizing gas atmosphere so that oxygen is brought into contact with the surface of the molten glass.

[0077] In the present invention, the melting step may be performed by contacting the molten glass surface with an oxidizing gas. In particular, when the melting tank in which the melting step is performed is made of quartz, the reduction color of the glass can be further reduced by contacting the molten glass surface with an oxidizing gas in an oxidizing gas atmosphere. Furthermore, since a platinum crucible is not used, the incorporation of precious metal oxides such as PtO2 can be suppressed.

[0078] [Continuous melting tank] The melting, fining and homogenization steps described above may be carried out using one melting vat, but the melting, fining and homogenization steps can also be carried out in different continuous melting vats. Fig. 1 shows a cross-sectional configuration of an optical glass manufacturing apparatus 1 equipped with a continuous melting vat used in the optical glass manufacturing method according to this embodiment. The optical glass manufacturing apparatus 1 includes a melting vat 10, a fining vat 20 and a homogenization vat 30. The melting vat 10 and the fining vat 20 are connected at their bottoms by a connecting pipe 11, and the fining vat 20 and the homogenization vat 30 are connected at their bottoms by a connecting pipe 21.

[0079] In the melting vat 10, a melting step is carried out in which glass raw materials 12 are melted. Next, the glass molten in the melting vat 10 is discharged through the communicating pipe 11 into the fining vat 20, where a fining step is carried out. Next, the refined molten glass is discharged from the fining vat 20 through the communicating pipe 21 into the homogenization vat 30, where a stirring step is carried out. As a result, the molten glass flows through the melting vat 10, the fining vat 20, and the homogenization vat 30 in this order.

[0080] Subsequently, the molten glass that has been subjected to the homogenization step is discharged into a forming die 40 via an outflow pipe 31 extending from the bottom of the homogenization tank 30, where it solidifies into glass.

[0081] When the manufacturing method of the present invention is carried out using the optical glass manufacturing apparatus 1 equipped with the continuous melting tank described above, the contact step with the oxidizing gas can be performed by supplying the oxidizing gas to the melting tank 10, the fining tank 20, and the homogenization tank 30 through the gas sharing pipe 51 extending from the oxidizing gas supply device 50, as shown in FIG. 1, and supplying the oxidizing gas to the upper opening of each tank (between the opening of the tank and the molten glass surface), thereby creating an oxidizing gas atmosphere. In addition, the flow rate of the oxidizing gas can be adjusted or the supply can be stopped by the gas supply valve 52 provided in the middle of the gas sharing pipe 51. By closing some of the gas supply valves, the oxidizing gas can be supplied to each desired tank. Furthermore, the oxidizing gas atmosphere can be created more efficiently by appropriately adjusting the distance from the gas outlet of the gas sharing pipe 51 to the molten glass surface. The same effect can be obtained by making each tank approximately sealed and creating an oxidizing gas atmosphere inside the tank as shown in FIG. 2.

[0082] In the forming step, as the molten glass is poured into forming mold 40, an oxidizing gas can be blown onto the molten glass from the upper opening of forming mold 40 via shared gas pipe 51, thereby creating an oxidizing gas atmosphere around the forming mold and bringing oxygen into contact with the surface of the molten glass, as shown in Fig. 1. Alternatively, as shown in Fig. 3, an oxidizing gas can be blown onto the molten glass poured into forming mold 40 from the back side of forming mold 40, thereby bringing oxygen into contact with the surface of the molten glass.

[0083] [Physical Properties] The optical glass of the present invention has a refractive index (n d The refractive index (n dThe lower limit of this refractive index (n d The upper limit of the Abbe number (ν d The lower limit of this Abbe number (ν d ) is preferably 45.00 or less, more preferably 40.00 or less, and even more preferably 37.00 or less.

[0084] It is preferable that the optical glass of the present invention has a high visible light transmittance, particularly a high transmittance for light on the short wavelength side of visible light, and thus has little coloring. The shortest wavelength (λ ) at which a 10 mm thick sample of the optical glass of the present invention exhibits a spectral transmittance of 70% 70 ) is preferably 470 nm or less, more preferably 450 nm or less, even more preferably 430 nm or less, and even more preferably 420 nm or less.

[0085] In the optical glass of the present invention, (λ 70 ) and refractive index (n d ) is λ 70 ≦(n d It is preferable that the relationship of λ −2)×200+420 is satisfied. 70 ≦(n d It is more preferable that the relationship λ satisfies: 70 ≦(n d It is more preferable that the relationship of λ −2)×200+410 is satisfied, 70 ≦(n d It is more preferable that the relationship be satisfied. Glass with a high refractive index tends to have a poor transmittance, so by satisfying the above relational expression, the glass is recognized as an optical glass with a good transmittance even if it has a high refractive index.

[0086] The optical glass obtained by the manufacturing method according to the present invention can be precision press molded and typically used for lenses, prisms, and mirrors. In particular, it can be used as a preform material for press molding, or molten glass can be directly pressed. When used as a preform material, the manufacturing method and precision press molding method are not particularly limited, and known manufacturing methods and molding methods can be used.

[0087] Optical glass is useful for various optical elements and optical designs, and it is particularly preferable to press mold the optical glass obtained by the manufacturing method of the present invention to produce optical elements such as lenses, prisms, mirrors, etc. When the obtained optical elements are used in optical instruments that transmit visible light, such as cameras and projectors, high-definition and high-precision imaging characteristics can be achieved while miniaturizing the optical systems in these optical instruments. EXAMPLES

[0088] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.

[0089] [Preparation of glass raw materials] As the raw materials for each of the following components, high purity raw materials used in ordinary optical glass, such as oxides, carbonates, nitrates, fluorides, and metaphosphate compounds, were used. SiO24.8% B2O39.2% La2O3 53.1% Y2O34.8% ZrO25.8% TiO2 13.4% Nb2O58.0% WO30.8% Li2O 0.1% S 0.4%

[0090] [Example 1] The prepared glass raw materials were put into a melting tank with an inner wall made of a platinum alloy, and the glass raw materials were melted at a temperature of 1250°C for 7.0 hours, and the molten glass was refined (clarification process) for 0.5 to 1.5 hours to remove bubbles, etc., and then cooled to a temperature of 1250°C or lower, and finished stirring (homogenization process) was performed to remove striae. During this homogenization process, oxygen gas was supplied from the opening of the homogenization tank at a flow rate of 0.5 L / min, and the oxygen gas was blown from a position 60 mm above the surface of the molten glass, bringing the oxidizing gas into contact with the surface of the molten glass. Next, the molten glass was poured from the melting tank into a mold and slowly cooled (molding step) to obtain glass.

[0091] [Example 2] A glass was produced in the same manner as in Example 1, except that in the homogenization step, the flow rate of the oxygen gas supplied was changed to 1.0 L / min.

[0092] [Example 3] A glass was produced in the same manner as in Example 1, except that the flow rate of the oxygen gas supplied in the homogenization step was changed to 2.7 L / min.

[0093] [Example 4] Glass was produced in the same manner as in Example 1, except that in the homogenization step, the flow rate of the oxygen gas supplied was changed to 1.0 L / min, and in the molding step, the oxygen gas was supplied to the mold at a flow rate of 5.0 L / min.

[0094] [Comparative Example 1] A glass was prepared in the same manner as in Example 1, except that oxygen gas was not supplied.

[0095] [Measurement of refractive index and Abbe number] The refractive index (n d ), Abbe number (ν d ) was measured according to the V-block method specified in JIS B 7071-2:2018. Here, the refractive index (n d ) is shown as a measurement value for the d line (587.56 nm) of a helium lamp. d) is the refractive index for the d line of the helium lamp (n d ) and the refractive index (n F ), and the refractive index for the C line (656.27 nm) (n C ) value, the Abbe number (ν d )=[(n d -1) / (n F -n C The refractive indexes (n d ), Abbe number (ν d ) was determined by measuring the glass obtained by cooling at a rate of -25°C / hr. The measurement results are shown in Table 1 below.

[0096] [Evaluation of coloring degree] The degree of coloring of the glass was evaluated by the transmittance. The transmittance of each glass was measured. The transmittance of the glass was measured in accordance with the Japan Optical Glass Industry Association standard (JOGIS02-2019 Method for measuring the coloration of optical glass). Specifically, a plate-shaped glass sample with a thickness of 10 mm ± 0.1 mm, both sides of which are polished parallel to each other and flat, is prepared, and light is incident perpendicularly to the polished surface to measure the spectral transmittance, including surface reflection loss, in the wavelength range of 200 nm to 700 nm. The wavelength at which the spectral transmittance becomes 70% is defined as λ 70 It was decided. The evaluation results are shown in Table 1 below.

[0097] [Table 1]

[0098] As is clear from the evaluation results in Table 1, by contacting molten glass in an oxidizing gas atmosphere with an oxidizing gas in any of the steps subsequent to the melting step (clarification step, homogenization step, molding step), it is possible to obtain optical glass with a high refractive index and excellent transmittance (Examples 1 to 4). On the other hand, it is understood that in the conventional manufacturing method in which molten glass is not brought into contact with an oxidizing gas, the reduction color of the glass cannot be sufficiently reduced (Comparative Example 1).

Claims

1. In mass percent, Ln 2 O 3 component (wherein Ln represents at least one selected from the group consisting of La, Gd, Y, and Yb) in a total content of 10.0% or more, and TiO 2 Component: Nb 2 O 5 Ingredients: WO 3 Components and Bi 2 O 3 At least one selected from the group consisting of components; Including, An optical glass obtained by bringing an oxidizing gas into contact with the surface of molten glass containing the above components.

2. An optical element comprising the optical glass according to claim 1.

Citation Information

Patent Citations

  • Sealing material

    JP2002012852A