Method for forming web from fibrous material
The method of forming fibrous material packs without binders through lamination or mechanical entanglement addresses the complexity and cost issues of wet binder systems, improving strength and efficiency in the manufacturing process.
Patent Information
- Application Number
- JP2024135632
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2013-03-15
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2034-03-14
AI Technical Summary
Existing methods for forming fibrous material packs often rely on wet binders, which require complex systems for binder recovery and wash water, increasing costs and operational complexity.
A method for forming fibrous material packs without binders, using a continuous process that includes melting glass, forming fibers, and either laminating or mechanically entangling them to create binderless or dry binder-containing webs, which are then optionally treated with a dry binder.
This approach reduces manufacturing complexity and costs by eliminating the need for wet binder systems, while enhancing mechanical properties such as tensile and adhesive strength, and allows for high throughput and energy-efficient curing of dry binders.
Smart Images

Figure 2024164082000001_ABST
Abstract
Description
[Technical Field]
[0001] Related Applications This application is a continuation-in-part of U.S. patent application Ser. No. 13 / 632,895, filed October 1, 2012, entitled "Method of Forming a Pack from Fibrous Materials," which claims priority to U.S. provisional patent application Ser. No. 61 / 541,162, filed September 30, 2011, entitled "Method of Forming a Pack from Fibrous Materials." U.S. patent application Ser. No. 13 / 632,895 and U.S. provisional patent application Ser. No. 61 / 541,162 are incorporated herein by reference in their entireties. [Background technology]
[0002] Fibrous materials can be formed into a variety of products, including webs, packs, batts, and blankets. Packs of fibrous material can be used in many applications, including, but not limited to, insulation and soundproofing for buildings, building components, appliances, and aircraft. Packs of fibrous material are typically formed by a process involving fiberizers, forming hoods, furnaces, trimming, and packaging machines. Typical processes also include the use of wet binders, binder recovery water, and wash water systems. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] US Patent Application Publication No. 2010 / 0151223 [Patent Document 2] U.S. Patent No. 6,527,014 [Patent Document 3] U.S. Patent No. 5,932,499 [Patent Document 4] U.S. Patent No. 5,523,264 [Patent Document 5] U.S. Patent No. 5,055,428 [Patent Document 6] U.S. Patent No. 4,266,960 [Patent Document 7] U.S. Patent No. 5,603,743 [Patent Document 8] U.S. Patent No. 4,263,033 [Patent Document 9] International Publication No. 95 / 30036 [Patent Document 10] US Patent Application Publication No. 2008 / 0246379 [Patent Document 11] U.S. Patent No. 3,092,529 [Patent Document 12] International Publication No. 2010 / 002958 [Patent Document 13] U.S. Patent No. 7,329,456 [Patent Document 14] U.S. Patent No. 7,294,218 Summary of the Invention
[0004] This application discloses numerous exemplary embodiments of fibrous material webs and methods for making fibrous material webs. Binderless webs or webs with dry binders can be formed in a continuous process in which fibrous material, such as glass, is melted and formed into fibers. The fibers are formed into webs of binderless glass fibers or webs with dry binders. The binderless webs or webs with dry binders can be laminated and / or the fibers comprising the webs can be mechanically entangled, for example, by needling.
[0005] Other advantages of the web, batt, and methods of making the web and batt will become apparent to those skilled in the art from the following detailed description taken in conjunction with the accompanying drawings. [Brief explanation of the drawings]
[0006] [Figure 1A]1 is a flow chart of an exemplary embodiment of a method for forming a binderless laminate web or pack of glass fibers. [Figure 1B] 1 is a flow chart of an exemplary embodiment of a method for forming a binderless entangled web of glass fibers. [Figure 1C] 1 is a flow chart of an exemplary embodiment of a method for forming a binderless laminated and entangled web or pack of glass fibers. [Figure 2A] 1 is a flow chart of an exemplary embodiment of a method for forming a laminated web or pack of glass fibers with a dry binder. [Figure 2B] 1 is a flow chart of an exemplary embodiment of a method for forming a binderless entangled web of glass fibers with a dry-laid binder. [Figure 2C] 1 is a flow chart of an exemplary embodiment of a method for forming a binderless laminated and entangled web or pack of glass fibers with a dry binder. [Figure 2D] 1 is a flow chart of an exemplary embodiment of a method for forming a binderless laminated and entangled web or pack of glass fibers with a dry binder. [Figure 3A] 1 is a schematic diagram of an exemplary apparatus for forming a binderless laminate web or pack of glass fibers. [Figure 3B] 1 is a schematic diagram of an exemplary apparatus for forming a binderless entangled web of glass fibers. [Figure 3C] 1 is a schematic diagram of an exemplary apparatus for forming a binderless laminated and entangled web or pack of glass fibers. [Figure 3D] 1 is a schematic diagram of an exemplary apparatus for forming a binderless laminated and entangled web or pack of glass fibers. [Figure 3E] 1 is a schematic diagram of an exemplary storage configuration. [Figure 3F] 1 is a schematic diagram of an exemplary split flow configuration. [Figure 4] 1 is a schematic diagram of a forming apparatus for forming a web of glass fibers. [Figure 5]1 is a schematic diagram of an exemplary apparatus for forming a web or pack of glass fibers containing a dry binder. [Figure 5A] 1 is a schematic diagram of an exemplary apparatus for forming a web or pack of glass fibers containing a dry binder. [Figure 5B] 1 is a schematic diagram of an exemplary apparatus for forming a web or pack of glass fibers containing a dry binder. [Figure 6] 1 is a schematic elevation view of a process for forming a pack of fibrous material. [Figure 7] 1 is a schematic plan view of a process for forming a puck from fibrous material. [Figure 8] 1 is a schematic diagram of an exemplary apparatus for forming a web or pack of glass fibers containing a dry binder. [Figure 9A] 9A is a cross-sectional view taken along line 9A-9A of FIG. 8. [Figure 9B] 9A is a cross-sectional view taken along line 9A-9A of FIG. 8. [Figure 10A] 1 is a schematic diagram of an exemplary embodiment of an insulation product. [Figure 10B] 1 is a schematic diagram of an exemplary embodiment of an insulation product. [Figure 10C] 1 is a schematic diagram of an exemplary embodiment of an insulation product. [Figure 10D] 1 is a schematic diagram of an exemplary embodiment of an insulation product. [Figure 10E] 1 is a schematic diagram of an exemplary embodiment of an insulation product. [Figure 10F] 1 is a schematic diagram of an exemplary embodiment of an insulation product. [Figure 10G] 1 is a schematic diagram of an exemplary embodiment of an insulating batt or pack. [Figure 10H] 1 is a schematic diagram of an exemplary embodiment of an insulating batt or pack. [Figure 10I] 1 is a schematic diagram of an exemplary embodiment of an insulating batt or pack. [Figure 11] 1 is a schematic diagram of a setup for producing staple fibers. [Figure 12] FIG. 1 is a perspective view of a cooking range. [Figure 12A] FIG. 1 is a perspective view of a cooking range. [Figure 13] FIG. 1 is a front cross-sectional view of an exemplary embodiment of fiberglass insulation in a range. [Figure 13A] FIG. 1 is a front cross-sectional view of an exemplary embodiment of fiberglass insulation in a range. [Figure 14] 1 is a side cross-sectional view of an exemplary embodiment of fiberglass insulation in a range. FIG. [Figure 14A] 1 is a side cross-sectional view of an exemplary embodiment of fiberglass insulation in a range. FIG. [Figure 15A] 1 illustrates an exemplary embodiment of a method for producing a compression molded fiberglass product from a binderless or dry-binder type fiberglass batt. [Figure 15B] 1 illustrates an exemplary embodiment of a method for producing a compression molded fiberglass product from a binderless or dry-binder type fiberglass batt. [Figure 15C] 1 illustrates an exemplary embodiment of a method for producing a compression molded fiberglass product from a binderless or dry-binder type fiberglass batt. [Figure 16A] 1 illustrates an exemplary embodiment of a method for producing vacuum formed fiberglass products from binderless or dry-binder fiberglass batts. [Figure 16B] 1 illustrates an exemplary embodiment of a method for producing vacuum formed fiberglass products from binderless or dry-binder fiberglass batts. [Figure 16C] 1 illustrates an exemplary embodiment of a method for producing vacuum formed fiberglass products from binderless or dry-binder fiberglass batts. DETAILED DESCRIPTION OF THE INVENTION
[0007] The present invention will now be described with occasional reference to specific exemplary embodiments thereof. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0008] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. The terms used in describing the invention herein are for the purpose of describing particular embodiments only and are not intended to be limiting of the invention. When used in the description of the invention and the appended claims, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context clearly dictates otherwise.
[0009] Unless otherwise indicated, all numbers expressing dimensional quantities, such as length, width, height, etc., used in the specification and claims are to be understood as being modified in all instances by the term "about." Accordingly, unless otherwise indicated, the numerical properties set forth in the specification and claims are approximations that may vary depending upon the desired properties sought to be obtained in embodiments of the invention. Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the invention are approximations, the numerical values set forth in the specific examples are reported as precisely as possible. However, any numerical values inherently contain certain errors necessarily resulting from deviations found in their respective measurements.
[0010] The description and drawings disclose an improved method of forming a pack from fibrous material. Generally, the improved continuous process replaces the traditional method of applying a wet binder to the spun material with a novel method of making a batt or pack of fibers without any binder (i.e., a material that binds the fibers together) and / or a novel method of making a batt or pack of fibers with a dry binder.
[0011] The term "fibrous material," as used herein, is defined to mean any material formed by drawing or attenuating a molten material. The term "puck," as used herein, is defined to mean any product formed by fibrous material bonded together by adhesive and / or mechanical entanglement.
[0012] 1A and 3A illustrate a first exemplary embodiment of a continuous process or method 100 for forming a pack 300 (see FIG. 3A) from a fibrous material. The dashed line 101 surrounding the steps of method 100 indicates that the method is a continuous method, as described in more detail below. While the method and pack are described with respect to glass fibers, the method and pack are equally applicable to the production of fibrous products formed from other mineral materials, such as rock, slag, and basalt, as non-limiting examples.
[0013] Referring to Figure 1A, glass is melted 102. For example, Figure 3A schematically illustrates a melter 314. The melter 314 can deliver molten glass 312 to a forehearth 316. Melters and forehearths are known in the art and will not be described here. The molten glass 312 can be formed from various raw materials combined in proportions to provide a desired chemical composition.
[0014] Referring again to FIG. 1A , molten glass 312 is processed to form glass fibers 322 (104). The molten glass 312 can be processed in a variety of different ways to form the fibers 322. For example, in the example shown in FIG. 3A , the molten glass 312 flows from a forehearth 316 to one or more rotary spinners 318. The rotary spinners 318 receive the molten glass 312 and then form a veil 320 of glass fibers 322. As described in more detail below, the glass fibers 322 formed by the rotary spinners 318 are long and thin. Therefore, any desired spinners, rotary or otherwise, sufficient to form long, thin glass fibers 322 can be used. While the embodiment shown in FIG. 3A shows one rotary spinner 318, it should be appreciated that any desired number of rotary spinners 318 can be used.
[0015] The long, thin fibers can take a variety of different forms. In an exemplary embodiment, the long, thin fibers have a length ranging from about 0.25 inches to about 10.0 inches and a diameter ranging from about 9HT to about 35HT. HT stands for hundred thousandths of an inch. In an exemplary embodiment, the fibers 322 have a length ranging from about 1.0 inch to about 5.0 inches and a diameter ranging from about 14HT to about 25HT. In an exemplary embodiment, the fibers 322 have a length of about 3 inches and an average diameter of about 16-17HT. Without being bound by theory, it is believed that the use of relatively long, thin fibers advantageously provides superior heat and sound insulation performance, as well as superior strength properties, such as higher tensile strength and / or higher adhesive strength, over similarly sized packs having shorter, thicker fibers.
[0016] In exemplary embodiments in which the fibers are glass fibers, the term binderless means that the fibrous material, web, and / or pack comprises 99% or 100% glass alone, or 99% or 100% glass plus inert ingredients. Inert ingredients are any material that does not bond the glass fibers to one another. For example, in the exemplary binderless embodiments described herein, the glass fibers 322 can be optionally coated or partially coated with a lubricant after the glass fibers are formed. For example, the glass fibers 322 can be coated with any lubricant material that does not bond the glass fibers to one another. In exemplary embodiments, the lubricant can be a silicone compound, such as a siloxane, dimethylsiloxane, and / or a silane. The lubricant can also be another material or combination of materials, such as an oil or oil emulsion. The oil or oil emulsion can be a mineral oil or mineral oil emulsion and / or a vegetable oil or vegetable oil emulsion.
[0017] The glass fibers can be coated or partially coated with a lubricant in a variety of different ways. For example, the lubricant can be sprayed onto the glass fibers 322. In an exemplary embodiment, the lubricant is configured to prevent damage to the glass fibers 322 as they move through the manufacturing process and come into contact with various equipment as well as other glass fibers. The lubricant can also be useful in reducing dust in the manufacturing process. The application of the optional lubricant can be precisely controlled by any desired structure, mechanism, or device.
[0018] Referring to FIG. 1A, a web 321 of fibers that does not contain a binder or other material that binds the fibers together is formed (106). The web 321 can be formed in a variety of different ways. In the example shown in FIG. 3A, the glass fibers 322 are collected by an optional collection member 324. The collection member 324 is shaped and sized to receive the glass fibers 322. The collection member 324 is configured to divert the glass fibers 322 into a duct 330 for transport to a downstream processing station, such as a forming device 332, that forms the web 321. In other embodiments, the glass fibers 322 can be collected on a conveying mechanism (not shown) to form the web.
[0019] The forming apparatus 332 can be configured to form a continuous dry-laid web 321 of fibrous material having a desired thickness. In one exemplary embodiment, the dry-laid web 321 disclosed in this application has a thickness ranging from about 0.25 inches to about 4 inches and a viscosity of about 0.2 lb / ft 3 to approximately 0.6 lb / ft 3 In one exemplary embodiment, the drylaid web 321 disclosed in this application can have a thickness ranging from about 1 inch to about 3 inches and a density ranging from about 0.3 lb / ft 3 to approximately 0.5 lb / ft 3 In one exemplary embodiment, the drylaid web 321 disclosed in this application can have a thickness of about 1.5 inches and a density of about 0.4 b / ft 3The forming device 332 can take a variety of different forms. Any configuration for forming the dry-laid web 321 of glass fibers can be used.
[0020] In one exemplary embodiment, the forming apparatus 332 includes a rotating drum having a forming surface and zones of higher and lower pressure. Referring to FIG. 4 , the pressure P1 on the side 460 of the forming surface 462 where the fibers 322 are collected is higher than the pressure P2 on the opposite side 464. This pressure drop ΔP causes the fibers 322 to gather on the forming surface 462 and form the dry-laid web 321. In one exemplary embodiment, the pressure drop ΔP across the forming surface 462 is controlled to be low, producing a web with a low weight per area. For example, the pressure drop ΔP can be from about 0.5 inches to 30 inches of water. The velocity V of the air moving through the forming web, which results in this low pressure drop ΔP, can be up to 1,000 feet per minute.
[0021] The low areal weight web 321 has an areal weight of about 5 to about 50 grams per square foot. The low areal weight web can have the density and thickness ranges described above. The low areal weight web can have a thickness ranging from about 2.5 inches to about 4 inches, a thickness ranging from about 1 inch to about 3 inches, or a thickness of about 1.5 inches. The low areal weight web can have a density of about 0.2 lb / ft 3 to approximately 0.6 lb / ft 3 Densities ranging from approximately 0.3 lb / ft 3 to approximately 0.5 lb / ft 3 Densities ranging from 0.4 lb / ft 33A , the dry web 321 emerges from the forming apparatus 332. In one exemplary embodiment, the low areal weight web 321 has a measured areal weight distribution coefficient of variation = Sigma (1 standard deviation) / Mean (average) x 100% = between 0% and 40%. In exemplary embodiments, the weight distribution coefficient of variation is less than 30%, less than 20%, or less than 10%. In one exemplary embodiment, the weight distribution coefficient of variation is between 25% and 30%, e.g., about 28%. In one exemplary embodiment, the weight distribution coefficient of variation is about 28%. The weight distribution coefficient of variation is obtained by measuring multiple smaller, e.g., 2 inch x 2 inch, sample area sizes from a larger, e.g., 6 ft x 10 ft, sample using a light table.
[0022] In the example shown in FIG. 1A , the web 321 or multiple webs are laminated (108). For example, a single web 321 can be folded in the machine direction or cross-lapped at 90 degrees to the machine direction to form a laminate web 350. In another embodiment, the webs can be cut into sections and the sections stacked on top of each other to form a laminate web. In yet another exemplary embodiment, one or more dual spinners 318 and forming apparatus 332 can be implemented to continuously produce two or more webs in parallel. The parallel webs are then stacked on top of each other to form a laminate web.
[0023] In one exemplary embodiment, the lamination mechanism 332 is a folding or cross-folding mechanism that works in conjunction with a conveyor 336. The conveyor 336 is configured to move in a machine direction indicated by arrow D1. The folding or cross-folding mechanism is configured to receive the continuous web 321 and deposit alternating layers of the continuous web onto the first conveyor 336 as the first conveyor moves in direction D1. In the deposition process, the folding mechanism 334 will form alternating layers in the machine direction indicated by arrow D1, or the cross-folding mechanism 334 will form alternating layers in the cross-machine direction. Additional webs 321 can be formed and folded or cross-folded by additional folding or cross-folding mechanisms to increase the number of layers and throughput.
[0024] In one exemplary embodiment, the cross-folding mechanism is configured to precisely control the movement of the continuous web 321 to deposit the continuous web onto the conveyor 336 so as not to damage the continuous web. The cross-folding mechanism can include any desired structure and can be configured to operate in any desired manner. In one exemplary embodiment, the cross-folding mechanism includes a head (not shown) configured to move back and forth at 90 degrees relative to the machine direction D1. In this embodiment, the speed of the movable head is adjusted so that the movement of the head in both cross-machine directions is substantially the same, thereby providing uniformity in the resulting fibrous body layer. In an exemplary embodiment, the cross-folding mechanism includes a vertical conveyor (not shown) configured and centered on the centerline of the conveyor 336. The vertical conveyor is further configured to swing above the conveyor 336 by a pivot mechanism to deposit the continuous web onto the conveyor 336. While several examples of cross-folding mechanisms are described above, it should be appreciated that the cross-folding mechanism can be other structures, mechanisms, or devices, or combinations thereof.
[0025] The laminate web 350 can have any desired thickness. The thickness of the laminate web is a function of several variables. First, the thickness of the laminate web 350 is a function of the thickness of the continuous web 321 formed by the forming apparatus 332. Second, the thickness of the laminate web 350 is a function of the speed at which the lamination mechanism 334 deposits the continuous web 321 onto the conveyor 336. Third, the thickness of the laminate web 334 is a function of the speed of the conveyor 336. In the illustrated embodiment, the laminate web 350 has a thickness ranging from about 0.1 inches to about 20.0 inches. In an exemplary embodiment, the cross-folding mechanism 334 can form a laminate web 350 having from 1 to 60 layers. Optionally, the cross-folding mechanism can be adjustable, thereby enabling the cross-folding mechanism 334 to form a pack having any desired width. In certain embodiments, the pack can have an overall width ranging from about 98.0 inches to about 236.0 inches.
[0026] In one exemplary embodiment, the laminate web 350 is produced in a continuous process, as shown by the dashed box 101 in FIG. 1A. The fibers produced by the spinner 318 are fed directly to the forming apparatus 332 (i.e., the fibers are not collected, baled, and then unbaled for use in a remote forming apparatus). The web 321 is fed directly to the laminating apparatus 352 (i.e., the web is not formed, wound up, and then unwound for use in a remote laminating apparatus 352). In an exemplary embodiment of a continuous process, each process (forming and laminating in FIG. 1A) is connected to the spinning process, so that fibers from the spinner are used by the other process rather than being stored for later use. In another exemplary embodiment of a continuous process, one or more spinners 318 may have a greater throughput than required by the forming apparatus 332 and the laminating apparatus 352. Therefore, fibers do not necessarily need to be continuously fed by the spinner 318 to the forming apparatus 332 for the process to be continuous. For example, spinner 318 can produce batches of fiber that are accumulated within the same plant and fed to molding apparatus 332 in a continuous process, without the fiber being compressed, shipped, and re-baled in a continuous process. As another example of a continuous process, the fiber produced by spinner 318 can be alternately diverted to molding apparatus 332 and to another molding apparatus or for some other use or product. In another example of a continuous process, a portion of the fiber produced by spinner 318 is continuously diverted to molding apparatus 332, and the remaining portion of the fiber is diverted to another molding apparatus or for some other use or product.
[0027] Figure 3E shows that in any of the examples shown in Figures 3A - 3D, the fibers 322 can be collected by the accumulator 390. Arrow 392 indicates that the fibers 322 are supplied to the forming device 332 by the accumulator 390 in a controlled manner. The fibers 322 can remain in the accumulator 390 for a predetermined time to cool the fibers before being supplied to the forming device 332. In one exemplary embodiment, the fibers 322 are supplied to the forming device 332 by the accumulator 390 at the same rate at which the fibers 322 are supplied to the accumulator 390. Therefore, in this exemplary embodiment, the time that the fibers stay and cool in the accumulator is determined by the amount of fibers 322 in the accumulator. In this example, the residence time is the value obtained by dividing the amount of fibers in the accumulator by the rate at which the fibers are supplied to the forming device 332 by the accumulator. In another exemplary embodiment, the accumulator 390 can selectively start and stop the supply of fibers and / or adjust the rate at which the fibers are supplied.
[0028] Figure 3F shows that in any of the examples shown in Figures 3A - 3D, the fibers 322 can be selectively diverted between the forming station 332 and the second forming station 332' by a diverting mechanism 398. In one exemplary embodiment, the embodiments shown in Figures 3A - 3D can have both an accumulator 390 and a diverting mechanism 398.
[0029] In one exemplary embodiment, the web 321 is relatively thick and has a low basis weight, yet the continuous process still has a high throughput and all the fibers produced by the spinning machine are used to make the web. For example, a single layer of the web 321 can have a basis weight of about 5 to about 50 grams per square foot. The web with a low basis weight can have the density and thickness ranges described above. The high - throughput continuous process can be produced at between about 750 lbs / hr and 1500 lbs / hr, for example, at least 900 lbs / hr or at least 1250 lbs / hr. The laminated web 350 can be used for a variety of different applications.
[0030] 1B and 3B illustrate a second exemplary embodiment of a method 150 for forming a pack 300 (see FIG. 3B) from a fibrous material without the use of a binder. The dashed line 151 surrounding the steps of the method 150 indicates that the method is a continuous method. Referring to FIG. 1B, glass is melted (102). The glass may be melted as described above with respect to FIG. 3A. The molten glass 312 is processed (104) to form glass fibers 322. The molten glass 312 may be processed to form fibers 322 as described above with respect to FIG. 3A. A web 321 of fibers is formed (106), without a binder or other material that binds the fibers together. The web 321 may be formed as described above with respect to FIG. 3A.
[0031] Referring to FIG. 1B, fibers 322 of web 321 are mechanically entangled (202) to form entangled web 352 (see FIG. 3B). Referring to FIG. 3B, fibers of web 321 can be mechanically entangled by an entanglement mechanism 345, such as a needling device. The entanglement mechanism 345 is configured to entangle individual fibers 322 of web 321. Entangling the glass fibers binds the fibers of the web together. The entanglement improves the mechanical properties of the web, such as the tensile strength and shear strength. In the illustrated embodiment, the entanglement mechanism 345 is a needling mechanism. In other embodiments, the entanglement mechanism 345 can include other structures, mechanisms, or devices, or combinations thereof, including, by way of non-limiting example, a stitching mechanism.
[0032] The entangled web 352 can have any desired thickness. The thickness of the entangled web is a function of the thickness of the continuous web 321 formed by the forming apparatus 332 and the amount of compression of the continuous web 321 by the entanglement mechanism 345. In an exemplary embodiment, the entangled web 352 has a thickness ranging from about 0.1 inches to about 2.0 inches. In an exemplary embodiment, the entangled web 352 has a thickness ranging from about 0.5 inches to about 1.75 inches. For example, in one exemplary embodiment, the entangled web has a thickness of about ½”.
[0033] In one exemplary embodiment, the entangled web 352 is produced in a continuous process 151. The fibers produced by the spinner 318 are fed directly to the forming apparatus 332 (i.e., the fibers are not collected, baled, and then unbaled for use in a remote forming apparatus). The web 321 is fed directly to the entanglement apparatus 345 (i.e., the web is not formed, wound up, and then unwound for use in a remote entanglement apparatus 345). The entangled web 352 can be used in a variety of different applications. In an exemplary embodiment of a continuous process, each process (forming and entanglement in FIG. 1B) is connected to the spinning process, so that the fibers from the spinners are used by other processes rather than being stored for later use. In another exemplary embodiment of a continuous process, one or more spinners 318 may have a greater throughput than required by the forming apparatus 332 and / or the entanglement apparatus 345. Therefore, fibers do not necessarily need to be continuously supplied by spinner 318 to molding apparatus 332 for the process to be continuous. For example, spinner 318 can produce batches of fibers that are accumulated in the same factory and supplied to molding apparatus 332 in a continuous process, but the fibers are not compressed, shipped, and re-baled in a continuous process. As another example of a continuous process, fibers produced by spinner 318 can be alternately diverted to molding apparatus 332 and to another molding apparatus or for some other use or product. In another example of a continuous process, a portion of the fibers produced by spinner 318 are continuously diverted to molding apparatus 332, and the remaining portion of the fibers are diverted to another molding apparatus or for some other use or product.
[0034] FIG. 3D illustrates an exemplary embodiment of an apparatus similar to the embodiment illustrated in FIG. 3B for forming a single-layer, high-density pack. For example, the embodiment illustrated in FIG. 3D can produce a pack 300 that is denser than the highest density pack produced by the embodiment illustrated in FIG. 3B. The apparatus of FIG. 3D corresponds to the embodiment of FIG. 3B, except that a compression mechanism 375 is provided between the forming station 332 and the entanglement mechanism 345 and / or the entanglement mechanism 345 includes a compression mechanism. The compression mechanism 375 compresses the web 321, as indicated by arrow 377, before the web 321 is fed to the entanglement mechanism 345 and / or the web 321 is compressed at the entrance to the compression mechanism. The resulting entangled web 352 has a high density. The compression mechanism can take a variety of different forms. Examples of compaction mechanism 345 include, but are not limited to, rollers, belts, rotary tackers, additional needling mechanisms, perforated belts applying negative pressure to the side of the belt opposite the entangled web 352 (see similar example shown in FIG. 4 ), any mechanism including any combination of the listed compaction mechanisms, any mechanism including any combination of features of any of the listed compaction mechanisms, etc. Any configuration for compacting the web can be used. When entanglement mechanism 345 includes a compaction mechanism, compaction mechanism 375 can be omitted in the embodiment of single-layer high-density pack 300 shown in FIG. 3D . The compaction performed by compaction mechanism 375 and / or entanglement mechanism 345 can be any combination of compaction and / or needling, which compacts the pack in addition to entangling the fibers. Examples of compression and needling sequences for producing high density packs include, but are not limited to, roller compression followed by needling, double needling, roller compression followed by double needling, triple needling, pre-needling-top needling-bottom needling, pre-needling-bottom needling-top needling, roller compression-top needling-bottom needling, and roller compression-bottom needling-top needling.
[0035] The densely entangled web 352 of Figure 3D can have any desired thickness. The thickness of the entangled web is a function of the thickness of the continuous web 321 formed by the forming apparatus 332 and the amount of compression of the continuous web 321 by the compression mechanism 375 and the entanglement mechanism 345. In an exemplary embodiment, the densely entangled web 352 of Figure 3D has a thickness ranging from about 0.1 inches to about 5 inches. In an exemplary embodiment, the densely entangled web 352 has a thickness ranging from about 0.250 inches to about 3.0 inches. In an exemplary embodiment, the densely entangled web has a thickness of 0.4 lb / ft 3 to approximately 12 lb / ft 3 In one exemplary embodiment, the densely entangled web 352 of Figure 3D is produced in a continuous process in the same manner as described with respect to Figure 3B.
[0036] 1C and 3C illustrate another exemplary embodiment of a method 170 for forming a pack 370 (see FIG. 3C) from a fibrous material without the use of a binder. Referring to FIG. 1C, glass is melted (102). The dashed line 171 surrounding the steps of method 170 indicates that the method is a continuous process. The glass may be melted as described above with respect to FIG. 3A. Referring again to FIG. 1C, the molten glass 312 is processed (104) to form glass fibers 322. The molten glass 312 may be processed as described above with respect to FIG. 3A to form fibers 322. Referring to FIG. 1C, a web 321 of fibers without a binder or other material that binds the fibers together is formed (106). The web 321 may be formed as described above with respect to FIG. 3A. Referring to FIG. 1C, the web 321 or multiple webs are stacked (108). The web 321 or multiple webs may be stacked as described above with respect to FIG. 3A. Referring to FIG. 1C, the fibers 322 of the laminate web 350 are mechanically entangled (302) to form an entangled pack 370 of the laminate web.
[0037] 3C, the fibers of the laminate web 350 can be mechanically entangled by an entanglement mechanism 345, such as a needling device. The entanglement mechanism 345 is configured to entangle the individual fibers 322 that form the layers of the laminate web. Entangling the glass fibers 322 binds the fibers of the laminate web 350 together to form a pack. Mechanical entanglement improves mechanical properties such as tensile strength and shear strength. In the illustrated embodiment, the entanglement mechanism 345 is a needling mechanism. In other embodiments, the entanglement mechanism 345 can include other structures, mechanisms, or devices, or combinations thereof, including, by way of non-limiting example, a stitching mechanism.
[0038] The entangled pack 370 of the laminated web 350 can have any desired thickness. The thickness of the entangled pack is a function of several variables. First, the thickness of the entangled pack is a function of the thickness of the continuous web 321 formed by the forming apparatus 332. Second, the thickness of the entangled pack 370 is a function of the speed at which the folding or cross-folding mechanism 334 deposits layers of the continuous web 321 onto the conveyor 336. Third, the thickness of the entangled pack 370 is a function of the speed of the conveyor 336. Fourth, the thickness of the entangled pack 370 is a function of the amount of compression of the laminated web 350 by the entanglement mechanism 345. The entangled pack 370 can have a thickness ranging from about 0.1 inches to about 20.0 inches. In an exemplary embodiment, the entangled pack 370 can have from 1 to 60 layers. Each entangled web layer 352 can be 0.1 to 2 inches thick. For example, each entangled web layer can be about 0.5 inches thick.
[0039] In one exemplary embodiment, entangled pack 370 is produced in a continuous process. Fibers produced by spinner 318 are fed directly to forming apparatus 332 (i.e., the fibers are not collected, baled, and then unbaled for use in a remote forming apparatus). Web 321 is fed directly to laminating apparatus 352 (i.e., the web is not formed, wound up, and then unwound for use in a remote laminating apparatus 352). Laminated web 350 is fed directly to entangling apparatus 345 (i.e., the laminated web is not formed, wound up, and then unwound for use in a remote entangling apparatus 345). In an exemplary embodiment of a continuous process, each process (forming, laminating, and entangling in FIG. 1C ) is connected to the spinning process, so that fibers from the spinners are used by other processes rather than being stored for later use. In another exemplary embodiment of a continuous process, one or more spinners 318 may have a greater throughput than required by the forming device 332, the laminating device 352, and / or the entangling device. As such, fibers do not necessarily need to be continuously supplied by the spinners 318 to the forming device 332 for the process to be continuous. For example, the spinners 318 may produce batches of fibers that are accumulated within the same plant and supplied to the forming device 332 in a continuous process, but the fibers are not compressed, shipped, and re-baled in a continuous process. As another example of a continuous process, fibers produced by the spinners 318 may be alternately diverted to the forming device 332 and to another forming device or for some other use or product. In another example of a continuous process, a portion of the fibers produced by the spinners 318 are continuously diverted to the forming device 332, and the remaining portion of the fibers are diverted to another forming device or for some other use or product.
[0040] In an exemplary embodiment, the entangled pack 370 of laminated webs is made from a web 321 or multiple webs that are relatively thick and have a low weight per area, yet the continuous process still has a high throughput, and all of the fibers produced by the spinner are used to make the entangled pack. For example, a single layer of web 321 can have the above-mentioned weight per area, thickness, and density. A high-throughput continuous process can produce between about 750 lbs / hr and 1500 lbs / hr, e.g., at least 900 lbs / hr or at least 1250 lbs / hr. In an exemplary embodiment, the combination of high web throughput of the continuous process with mechanical entanglement, such as needling, is facilitated by laminating the web 321, such as by folding or cross-folding the web. By laminating the web 321, the linear speed of the material moving through the lamination device is slower than the speed at which the web is formed. For example, in a continuous process, a two-layer web would move through the entanglement device 345 at half the speed at which the web is formed (one-third the speed for a three-layer web, etc.). This reduction in speed allows for a continuous process in which a high throughput, low weight per areal web 321 is formed and converted into a multi-layer mechanically entangled pack 370. The entangled pack 370 of layered webs can be used in a variety of different applications.
[0041] In an exemplary embodiment, the lamination and entanglement of long, thin fibers results in a strong web 370. For example, the entanglement of long, thin glass fibers described in this application results in a laminated, entangled web with high tensile strength and high adhesive strength. Tensile strength is the strength of web 370 when web 370 is pulled in the direction of the length or width of the web. Adhesive strength is the strength of web 370 when web 370 is pulled apart across the thickness of the web.
[0042] Tensile strength and adhesive strength can be tested in a variety of different ways. In one exemplary embodiment, a machine such as an Instron machine pulls the web 370 at a constant speed (12 inches per second in the example below) and measures the amount of force required to pull the web apart. The force required to pull the web apart is recorded, including the peak force applied to the web before it tears or breaks.
[0043] In one method of testing tensile strength, the longitudinal tensile strength is measured by clamping the edges of the web along the width of the web and mechanically pulling the web 370 along the length of the web at a constant rate (12 inches per second in the example below) and recording the peak force applied along the length of the web. The cross-machine tensile strength is measured by clamping the sides of the web along the width of the web and pulling the web 370 along the width of the web at a constant rate (12 inches per second in the example below) and recording the peak force applied. The longitudinal tensile strength and the cross-machine tensile strength are averaged to determine the tensile strength of the sample.
[0044] In one method of testing adhesive strength, a sample of a given size (6" x 6" in the example below) is prepared. Each side of the sample is attached to a substrate, for example by gluing. The substrates on either side of the sample are mechanically pulled apart at a constant speed (12 inches per second in the example below) and the peak force applied is recorded. Dividing the peak force applied by the area of the sample (6" x 6" in the example below) gives the adhesive strength in units of force / area.
[0045] The following examples are presented to demonstrate the increased strength of the layered entangled web 370. In these examples, no binder is included, i.e., no aqueous or dry binder is included. These examples are not intended to limit the scope of the present invention unless expressly stated in the claims. Examples of layered entangled webs having four, six, and eight layers are presented. However, the layered entangled web 370 can have any number of layers. The length, width, thickness, number of folds, and weight of the layered entangled web 370 sample can vary depending on the application of the web 370. In the dense single-layer embodiment shown in FIG. 3D, the single-layer dense pack 300 can have a weight per square foot that is higher, e.g., two or more times higher, than the examples of the same thickness in the following six paragraphs.
[0046] In one exemplary embodiment, a 6 inch by 12 inch sample of web 370 has multiple layers, e.g., two folds (i.e., four layers), is between 0.5 inches and 2.0 inches thick, has a weight per square foot between 0.1 lbs / sqft and 0.3 lbs / sqft, has a tensile strength greater than 3 lbf, and has a tensile strength-to-weight ratio greater than 40 lbf / lbm, e.g., from about 40 to about 120 lbf / lbm. In an exemplary embodiment, the adhesive strength of this sample is greater than 0.1 lbs / sqft. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 5 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 7.5 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 10 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 12.5 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 13.75 lbf. In exemplary embodiments, the samples described in this paragraph have a tensile strength between 3 lbf and 15 lbf. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 2 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 10 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 15 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 20 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 5 lbf and the adhesive strength is greater than 2 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 7.5 lbf and the adhesive strength is greater than 7.5 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 10 lbf and the adhesive strength is greater than 10 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have a tensile strength greater than 12.5 lbf and an adhesive strength greater than 15 lbs / sqft.In exemplary embodiments, the samples described in this paragraph have a tensile strength greater than 13.75 lbf and an adhesive strength greater than 20 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have a tensile strength between 3 lbf and 15 lbf and an adhesive strength between 0.3 lbs / sqft and 30 lbs / sqft.
[0047] In one exemplary embodiment, a 6 inch by 12 inch sample of web 370 has multiple layers, e.g., two folds (i.e., four layers), is between 0.5 inches and 1.75 inches thick, has a weight per square foot between 0.12 lbs / sqft and 0.27 lbs / sqft, has a tensile strength greater than 3 lbf, a tensile strength-to-weight ratio greater than 40 lbf / lbm, e.g., from about 40 to about 120 lbf / lbm, and an adhesive strength greater than 1 lb / sqft. In an exemplary embodiment, the sample described in this paragraph has a tensile strength greater than 5 lbf. In an exemplary embodiment, the sample described in this paragraph has a tensile strength greater than 7.5 lbf. In an exemplary embodiment, the sample described in this paragraph has a tensile strength greater than 10 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 12.5 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 13.75 lbf. In exemplary embodiments, the samples described in this paragraph have a tensile strength between 3 lbf and 15 lbf. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 2 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 10 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 15 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 20 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 5 lbf and the adhesive strength is greater than 2 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 7.5 lbf and the adhesive strength is greater than 7.5 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 10 lbf and the adhesive strength is greater than 10 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have a tensile strength greater than 12.5 lbf and an adhesive strength greater than 15 lbs / sqft.In exemplary embodiments, the samples described in this paragraph have a tensile strength greater than 13.75 lbf and an adhesive strength greater than 20 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have a tensile strength between 3 lbf and 15 lbf and an adhesive strength between 0.3 lbs / sqft and 30 lbs / sqft.
[0048] In one exemplary embodiment, a 6 inch by 12 inch sample of web 370 has multiple layers, e.g., two folds (i.e., four layers), is between 0.5 inches and 1.25 inches thick, has a weight per square foot between 0.2 lbs / sqft and 0.3 lbs / sqft, has a tensile strength greater than 10 lbf, and has a tensile strength-to-weight ratio greater than 75 lbf / lbm, e.g., from about 75 to about 120 lbf / lbm. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 12.5 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 13.75 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is between 3 lbf and 15 lbf. In an exemplary embodiment, the adhesive strength of the sample described in this paragraph is greater than 3 lbs / sqft. In an exemplary embodiment, the adhesive strength of the sample described in this paragraph is greater than 10 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have an adhesive strength greater than 15 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have a tensile strength greater than 10 lbf and an adhesive strength greater than 3 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have a tensile strength greater than 12.5 lbf and an adhesive strength greater than 10 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have a tensile strength greater than 13.75 lbf and an adhesive strength greater than 15 lbs / sqft.
[0049] In an exemplary embodiment, a 6 inch by 12 inch sample of web 370 has multiple layers, e.g., three folds (i.e., six layers), is between 1.0 inch and 2.25 inches thick, has a weight per square foot between 0.15 lbs / sqft and 0.4 lbs / sqft, has a tensile strength greater than 5 lbf, and has a tensile strength-to-weight ratio greater than 40 lbf / lbm, e.g., from about 40 to about 140 lbf / lbm. In an exemplary embodiment, the adhesive strength of this sample is greater than 0.1 lbs / sqft. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 7.5 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 10 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 12.5 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 13.75 lbf. In exemplary embodiments, the samples described in this paragraph have a tensile strength between 5 lbf and 20 lbf. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 0.5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 1.0 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 1.5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 2.0 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 2.5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 3.0 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 7.5 lbf and the adhesive strength is greater than 0.40 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 10 lbf and the adhesive strength is greater than 0.6 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have a tensile strength greater than 12.5 lbf and an adhesive strength greater than 0.9 lbs / sqft. In exemplary embodiments, the samples described in this paragraph have a tensile strength between 5 lbf and 20 lbf and an adhesive strength between 0.1 lbs / sqft and 4 lbs / sqft.
[0050] In one exemplary embodiment, a 6 inch by 12 inch sample of web 370 has multiple layers, e.g., three folds (i.e., six layers), is between 1.0 and 1.50 inches thick, has a weight per square foot between 0.25 and 0.4 lbs / sqft, has a tensile strength greater than 9 lbf, and has a tensile strength-to-weight ratio greater than 50 lbf / lbm, e.g., from about 50 to about 140 lbf / lbm. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 12.5 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 13.75 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is between 9 and 15 lbf. In an exemplary embodiment, the adhesive strength of the sample described in this paragraph is greater than 0.5 lbs / sqft. In an exemplary embodiment, the adhesive strength of the sample described in this paragraph is greater than 1.0 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 1.5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 2.0 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 2.5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 3.0 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 9 lbf and the adhesive strength is greater than 0.5 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 12.5 lbf and the adhesive strength is greater than 1.0 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 13.75 lbf and the adhesive strength is greater than 2 lbs / sqft.
[0051] In one exemplary embodiment, a 6 inch by 12 inch sample of web 370 has multiple layers, e.g., four folds (i.e., eight layers), is between 0.875 inches and 2.0 inches thick, has a weight per square foot between 0.15 lbs / sqft and 0.4 lbs / sqft, has a tensile strength greater than 3 lbf, and has a tensile strength to weight ratio greater than 40 lbf / lbm, e.g., from about 40 to about 130 lbf / lbm. In an exemplary embodiment, the web has an adhesive strength greater than 0.3 lbs / sqft. In an exemplary embodiment, the adhesive strength of this sample is greater than 0.1 lbs / sqft. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 7.5 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is greater than 10 lbf. In an exemplary embodiment, the tensile strength of the sample described in this paragraph is between 3 lbf and 15 lbf. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 0.5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 1.0 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 2 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 3 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 4 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 10 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 7.5 lbf and the adhesive strength is greater than 0.5 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 10 lbf and the adhesive strength is greater than 1.0 lbs / sqft. In one exemplary embodiment, the samples described in this paragraph have a tensile strength between 3 lbf and 15 lbf and an adhesive strength between 0.3 lbs / sqft and 15 lbs / sqft.
[0052] In exemplary embodiments, a 6 inch by 12 inch sample of web 370 has multiple layers, e.g., four folds (i.e., eight layers), is between 1.0 and 2.0 inches thick, has a weight per square foot between 0.1 and 0.3 lbs / sqft, has a tensile strength greater than 9 lbf, and has a tensile strength-to-weight ratio greater than 70 lbf / lbm. In exemplary embodiments, the tensile strength of the sample described in this paragraph is greater than 10 lbf. In exemplary embodiments, the adhesive strength of the sample described in this paragraph is greater than 0.5 lbs / sqft. In exemplary embodiments, the adhesive strength of the sample described in this paragraph is greater than 1.0 lbs / sqft. In exemplary embodiments, the adhesive strength of the sample described in this paragraph is greater than 2 lbs / sqft. In exemplary embodiments, the adhesive strength of the sample described in this paragraph is greater than 3 lbs / sqft. In exemplary embodiments, the adhesive strength of the sample described in this paragraph is greater than 4 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 5 lbs / sqft. In exemplary embodiments, the adhesive strength of the samples described in this paragraph is greater than 10 lbs / sqft. In exemplary embodiments, the tensile strength of the samples described in this paragraph is greater than 10 lbf and the adhesive strength is greater than 5 lbs / sqft.
[0053] In an exemplary embodiment, the entangled web produced according to Figures 1A-1C and 3A-3C has combined physical properties in the ranges shown in Table 1 below.
[0054] [Table 1]
[0055] No. 6,239,999, and / or U.S. Patent No. 6,239,999, ...
[0056] 2A-2C illustrate an exemplary embodiment of a method similar to the embodiment of FIGS. 1A-1C, except that the web 521 (see FIG. 5) is formed (260) using a dry or non-aqueous binder. Method 200 of FIG. 2A generally corresponds to method 100 of FIG. 1A. Method 250 of FIG. 2B generally corresponds to method 150 of FIG. 1B. Method 270 of FIG. 2C generally corresponds to method 170 of FIG. 1C.
[0057] FIG. 2D illustrates a method 290 similar to method 270 of FIG. 2C. In FIG. 2D, steps within dashed boxes are optional. In the exemplary embodiment illustrated in FIG. 2D, a dry binder can optionally be added to the web in step 292 instead of (or in addition to) before the web is formed and / or to the laminated web in step 294. For example, if step 292 is included, the web can be formed without a dry binder, and then a dry binder is added to the web before and / or during lamination. If step 294 is included, the web can be formed and laminated without a dry binder, and then a dry binder is added to the laminated web.
[0058] Referring to FIG. 5 , dry binder (indicated by the large arrow) can be added to the fibers 322 and / or web 521 at various different points during the process. Arrow 525 indicates that the dry binder can be added to the fibers 322 at or above the collecting member. Arrow 527 indicates that the dry binder can be added to the fibers 322 in duct 330. Arrow 529 indicates that the dry binder can be added to the fibers 322 in the former 332. Arrow 531 indicates that the dry binder can be added to the web 321 after it exits the former 332. Arrow 533 indicates that the dry binder can be added to the web 321 as it is laminated by lamination device 334. Arrow 535 indicates that the dry binder can be added to the web 321 after it is laminated. Arrow 537 indicates that the dry binder can be added to the web 321 or laminated web in oven 550. 8, arrow 827 indicates that the dry binder can be added to the fibers 322 in duct 330 near the spinner. Arrow 829 indicates that the dry binder can be added to the fibers 322 in duct 330 at the duct elbow. Arrow 831 indicates that the dry binder can be added to the fibers in duct 330 at the exit end of the duct. Arrow 833 indicates that the dry binder can be added to the fibers 322 in forming device 332 having a drum-shaped forming surface. The dry binder can be added to the fibers 322 or web 321 in any manner to form the web 521 with a dry binder.
[0059] FIG. 5A is an embodiment similar to that of FIG. 5, except that the fibers 322 are collected by an accumulator 590. Arrow 592 indicates that the fibers 322 are fed in a controlled manner by the accumulator 590 to the former 332. The fibers 322 may reside in the accumulator 590 for a predetermined period of time to cool the fibers before being fed to the former 332. In one exemplary embodiment, the fibers 322 are fed by the accumulator 590 to the former 322 at the same rate at which the fibers 322 are fed to the accumulator 590. Therefore, in this exemplary embodiment, the time the fibers reside and cool in the accumulator is determined by the amount of fibers 322 in the accumulator. In this example, the residence time is the amount of fibers in the accumulator divided by the rate at which the fibers are fed to the former 332 by the accumulator. In another exemplary embodiment, the accumulator 390 can selectively start and stop feeding fibers and / or adjust the rate at which it feeds fibers. The dry binder can be applied to the fibers 322 at any of the locations shown in Figure 5. Additionally, the dry binder can be applied to the fibers 322 in the accumulator, as indicated by arrow 594, and / or as the fibers are transported from the accumulator 590 to the forming device 332, as indicated by arrow 596.
[0060] Figure 5B is an embodiment similar to that of Figure 5, except that fibers 322 can be selectively diverted between former 332 and a second former and / or for some other use by diverting mechanism 598. In one exemplary embodiment, the embodiment shown in Figure 5 can have both an accumulator 590 and diverting mechanism 598. The dry binder can be applied to fibers 322 at any location shown in Figure 5. Additionally, the dry binder can be applied to fibers 322 within the diverting mechanism, as indicated by arrow 595, and / or as the fibers are transferred from diverting mechanism 598 to former 332, as indicated by arrow 597.
[0061] In an exemplary embodiment, the dry binder is applied to the fibers 322 at a location significantly downstream from the spinner 318. For example, the dry binder can be applied to the fibers at a location where the temperature of the fibers and / or the air surrounding the fibers is significantly lower than the temperature of the fibers and the ambient air at the spinner. In one exemplary embodiment, the dry binder is applied at a location where the temperature of the fibers and / or the air surrounding the fibers is lower than the temperature at which the dry binder melts or fully cures or reacts. For example, a thermoplastic binder can be applied at a point in the production line where the temperature of the fibers 322 and / or the air surrounding the fibers is lower than the melting point of the thermoplastic binder. A thermosetting binder can be applied at a point in the production line where the temperature of the fibers 322 and / or the air surrounding the fibers is lower than the cure temperature of the thermosetting binder. That is, the thermosetting binder can be applied at a point in the manufacturing line where the temperature of the fibers 322 and / or the air surrounding the fibers is below the temperature at which the thermosetting binder fully reacts or fully crosslinks. In one exemplary embodiment, the dry binder can be applied at a point in the manufacturing line where the temperature of the fibers 322 and / or the air surrounding the fibers is below 300°F. In one exemplary embodiment, the dry binder can be applied at a point in the manufacturing line where the temperature of the fibers 322 and / or the air surrounding the fibers is below 250°F. In one exemplary embodiment, the temperature of the fibers and / or the air surrounding the fibers at the locations indicated by arrows 527, 529, 531, 533, and 535 in FIG. 5 is below the temperature at which the dry binder melts or fully cures.
[0062] In one exemplary embodiment, the binder applicator is a sprayer configured for dry powder. The sprayer is configured to have an adjustable spray force, thereby allowing for greater or lesser penetration of the dry powder into the continuous web of fibrous material. Alternatively, the binder applicator can be another structure, mechanism, or device, or combination thereof, such as, for example, a vacuum device sufficient to draw the dry binder into the continuous web of glass fibers 321. For example, the dry binder can include binder fibers supplied in bale form. The binder applicator includes a bale opener and a blower, which open the bale, separate the binder fibers from one another, and blow the binder fibers into a duct where the binder is mixed with the fiberglass fibers. The dry binder can include a powder. The binder applicator can include a screw dispenser that delivers binder powder to an air nozzle, which delivers the binder powder into a duct where the binder powder is mixed with the fibers. The dry binder can include a non-aqueous liquid. The binder applicator can include a nozzle that delivers a liquid binder into a duct where the binder is mixed with the fibers.
[0063] 9, 9A, and 9B illustrate an exemplary embodiment in which a binder 900, such as a fiber or powder form, a fiber form, or a non-aqueous liquid form, is applied by a modified air wrapper 902. Air wrappers are well known in the art. Examples of air wrappers are disclosed in U.S. Patent Nos. 6,275,929; 6,275,933; 6,275,949; and 6,275,959, which are incorporated herein by reference in their entireties. Any of the features of the air wrappers disclosed in U.S. Patent Nos. 6,275,929; 6,275,949; 6,275,949; and 6,275,949 can be used in the air wrapper 902 shown generally in this patent application. One existing type of air wrapper is the Air Full Veil Wrapper (AFVL). The air wrapper 902 shown in FIGS. 9, 9A, and 9B differs from conventional air wrappers in that the air wrapper is configured to apply the binder 900.
[0064] Figure 8 shows a rotary spinner 318, optional collection member 324, duct 330, and forming device 332. The device shown in Figure 8 typically also includes melting device 314 and forehearth 316 shown in Figure 5. The melting device 314, forehearth, and other components shown in Figure 5 have been omitted from Figure 8 to simplify the drawing.
[0065] Referring to Figure 8, a forming apparatus 332 can be configured to form a continuous web 321 of fibrous material having a desired thickness. The forming apparatus 332 can take a variety of different forms. Any configuration for forming a web 321 of glass fibers can be used. In the exemplary embodiment shown in Figure 8, the forming apparatus 332 includes a rotating drum 910 having a forming surface 462 and areas of higher and lower pressure. Collection of the fibers using a pressure drop ΔP across the surface 462 is as described with respect to Figure 4.
[0066] 9A and 9B, the air wrapper 902 includes a first blower 920 and a second blower 922. The air wrapper operates by blowing air, for example, by alternating blowing by the first and second blowers 920, 922. The blower 920 provides an airflow against the fibers moving in the duct toward the forming surface 462, while the blower 922 provides no airflow (see FIGS. 9A and 9B). After a controlled time, the blower 922 provides an airflow against the fibers moving in the duct toward the forming surface 462, while the blower 920 provides no airflow. This alternating action of the first and second blowers 920, 922 results in a uniform distribution of the fibers 322 collected on the forming surface 462.
[0067] The air wrapper 902 shown in Figures 9, 9A, and 9B differs from conventional air wrappers in that each of the blowers 920, 922 includes one or more binder introducers 904. The binder introducers 904 can take a variety of different forms. For example, the binder introducers 904 can deliver the binder 900 to the interior 930 of the housing 932 of the blowers 920, 922 as shown, or the binder introducers can be positioned to deliver the binder 900 into the airflow of the blowers 920, 922. For example, a nozzle of the binder introducer can deliver the binder into the airflow of the blowers 920, 922. Examples of binder introducers include, but are not limited to, nozzles and blowers that provide a smaller airflow than the blowers 920, 922. In one exemplary embodiment, the binder introduction device 904 injects the binder 900 into the interior 930 of the housing 932 when the blowers 920, 922 are not blowing. Then, when the blowers 920, 922 are turned on, the interior 930 is pressurized and the binder 900 is carried from the interior 930 into the fiber airflow. Within the airflow, the air from the air wrappers moves the fibers, providing a shaping effect to the distribution of the fibers on the forming surface 462, and the air also injects the binder to mix with the fibers in the airflow.
[0068] 9A and 9B, air wrapper 902 mixes binder 900 into fibers 332, which collect on forming surface 462 to form web 321. In one exemplary embodiment, binder introduction device 904 introduces binder 900 into blower 920 as blower 920 provides air flow 921 against the fibers moving in a duct toward forming surface 462, and air flow 921 provided by blower 920 mixes the binder with fibers 322 (shown in FIGS. 9A and 9B). Similarly, in this embodiment, when blower 922 provides airflow 921 against the fibers moving in the duct toward forming surface 462, binder introduction device 904 introduces binder 900 into blower 922, and the airflow 921 provided by blower 922 mixes the binder with fibers 322 (the airflow provided by blower 922 is not shown, but is the same as the airflow provided by blower 920). As a result, binder 900 is uniformly mixed with fibers 322.
[0069] The dry binder can take a variety of different forms. Any non-aqueous medium that holds the fibers 322 together to form the web 521 can be used. In one exemplary embodiment, the dry binder is composed of substantially 100% solids when initially applied to the fibers. The term "substantially 100% solids," as used herein, refers to any binder material that contains a diluent, such as water, equal to or less than about 2%, preferably equal to or less than 1%, of the binder's weight (at the time the binder is applied, not after the binder has dried or cured). However, it should be recognized that in certain embodiments, the binder can contain any desired amount of diluent, such as water, depending on the specific application and design requirements. In one exemplary embodiment, the dry binder is a thermoplastic resin-based material that is not applied in liquid form and is not water-based. In other embodiments, the dry binder can be other materials or mixtures of other materials, including, but not limited to, polymeric thermosetting resins. The dry binder can have any form or combination of forms, including, but not limited to, powder, particles, fibers, and / or hot melt. Examples of hot melt polymers include, but are not limited to, ethylene-vinyl acetate copolymer, ethylene-acrylate copolymer, low-density polyethylene, high-density polyethylene, atactic polypropylene, polybutene-1, styrene block copolymer, polyamide, thermoplastic polyurethane, styrene block copolymer, polyester, and the like. In one exemplary embodiment, the dry binder is a formaldehyde-free dry binder, meaning that the dry binder does not contain formaldehyde. However, formaldehyde can be formed when a formaldehyde-free dry binder is combusted. In one exemplary embodiment, sufficient dry binder is applied so that the cured fiber pack can be compressed for packaging, storage, and shipping, yet still regain its thickness when installed (a process known as "loft recovery").
[0070] 2A-2D and 5, the glass fibers 322 can be optionally coated or partially coated with a lubricant before or after the dry binder is applied to the glass fibers. In an exemplary embodiment, the lubricant is applied after the dry binder to enhance adhesion of the dry binder to the glass fibers 322. The lubricant can be any of the lubricants described above.
[0071] 5, the continuous web 521 containing the unreacted dry binder is transferred from the forming apparatus 332 to an optional lamination mechanism 334. The lamination mechanism can take a variety of different forms. For example, the lamination mechanism can be a folding mechanism that laminates the web 321 in the machine direction D1, or a cross-folding mechanism that folds the web in a direction substantially perpendicular to the machine direction. The cross-folding mechanism described above for laminating the binderless web 321 can also be used to laminate the web 521 containing the unreacted dry binder.
[0072] In an exemplary embodiment, the dry binder of the continuous web 521 is configured to be heat cured in a curing oven 550. In an exemplary embodiment, the dry binder holds the fibers 322 together, and the curing oven 550 replaces the entanglement mechanism 345. In another exemplary embodiment, both the curing oven 550 and the entanglement mechanism 345 are included.
[0073] 6 and 7 schematically illustrate another exemplary embodiment of a method for forming a puck from fibrous material, generally indicated at 610. Referring to FIG. 6, molten glass 612 is fed from a melter 614 to a forehearth 616. The molten glass 612 may be formed from various raw materials combined in proportions to provide a desired chemical composition. From the forehearth 616, the molten glass 612 flows to a plurality of rotary spinners 618.
[0074] 6, a rotary spinner 618 receives molten glass 612 and then forms a veil 620 of glass fibers 622 entrained in a stream of hot gas. As will be described in more detail below, the glass fibers 622 formed by the rotary spinner 618 are long and thin. Therefore, any desired spinner, rotary or otherwise, sufficient to form long and thin glass fibers 22 can be used. While the embodiment shown in FIGS. 6 and 7 shows two rotary spinners 618, it should be recognized that any desired number of rotary spinners 18 can be used.
[0075] The flow of hot gas can be generated by an optional blowing mechanism, such as, but not limited to, an annular blower (not shown) or an annular burner (not shown). Generally, the blowing mechanism is configured to direct the veil 620 of glass fibers 622 in a given direction, typically downward. It should be understood that the flow of hot gas can be generated by any desired structure, mechanism, or device, or any combination thereof.
[0076] As shown in Figure 6, an optional spray mechanism 626 can be positioned below the rotary spinner 618 and can be configured to spray fine droplets of water or other fluid onto the hot gas within the veil 620 to help cool the hot gas stream, protect the fibers 622 from contact damage, and / or enhance the bonding ability of the fibers 622. The spray mechanism 626 can be any desired structure, mechanism, or device sufficient to spray fine droplets of water onto the hot gas within the veil 620 to help cool the hot gas stream, protect the fibers 622 from contact damage, and / or enhance the bonding ability of the fibers 622. While the embodiment shown in Figure 6 illustrates the use of the spray mechanism 626, it should be appreciated that the use of the spray mechanism 626 is optional, and the method 610 of forming a puck from fibrous material can be performed without the use of the spray mechanism 626.
[0077] Optionally, the glass fibers 622 can be coated with a lubricant after the glass fibers are formed. In the illustrated embodiment, a plurality of nozzles 628 can be positioned around the veil 620 at a location below the rotary spinner 618. The nozzles 628 can be configured to supply a lubricant (not shown) to the glass fibers 622 from a lubricant supply (not shown).
[0078] The application of the lubricant can be precisely controlled by any desired structure, mechanism, or device, such as, but not limited to, a valve (not shown). In certain embodiments, the lubricant can be a silicone compound, such as siloxane, dimethylsiloxane, and / or silane. The lubricant can also be other materials or mixtures of materials, such as, for example, an oil or oil emulsion. The oil or oil emulsion can be a mineral oil or mineral oil emulsion and / or a vegetable oil or vegetable oil emulsion. In an exemplary embodiment, the lubricant is applied in an amount of about 1.0 percent oil and / or silicone compound by weight of the resulting pack of fibrous material. However, in other embodiments, the amount of lubricant can be more or less than about 1.0 percent oil and / or silicone compound by weight.
[0079] While the embodiment shown in FIG. 6 illustrates the use of a nozzle 628 to deliver a lubricant (not shown) to the glass fibers 622, it should be appreciated that the use of the nozzle 628 is optional and the method 610 of forming a puck from a fibrous material can be performed without the use of the nozzle 628.
[0080] In the illustrated embodiment, the glass fibers 622 entrained within the hot gas stream can be collected by an optional collection member 624. The collection member 624 is shaped and sized to readily receive the glass fibers 622 and the hot gas stream. The collection member 624 is configured to direct the glass fibers 622 and the hot gas stream into a duct 630 for transport to downstream processing stations, such as forming devices 632a and 632b. In other embodiments, the glass fibers 622 can be collected on a conveying mechanism (not shown), for example, to form a blanket or batt (not shown). The batt can be transported by the conveying mechanism to further processing stations (not shown). The collection member 624 and duct 630 can be any structure having a generally hollow configuration suitable for receiving and transporting the glass fibers 622 and the hot gas stream. While the embodiment shown in FIG. 6 illustrates the use of a collection member 624, it should be appreciated that the use of the collection member 624 to direct the glass fibers 622 and hot gas flow into the duct 630 is optional, and the method 610 of forming a puck from fibrous material can be performed without the use of the collection member 624.
[0081] 6 and 7, a single spinner 618 is associated with each duct 630, with the glass fibers 622 and hot gas stream from the single spinner 618 being the only source of glass fibers 622 and hot gas stream entering the duct 630. Alternatively, each duct 630 can be adapted to receive glass fibers 622 and hot gas streams from multiple spinners 618 (not shown).
[0082] Referring again to FIG. 6 , optionally, a header system (not shown) can be disposed between the forming apparatuses 632a and 632b and the spinners 618. The header system can be configured as a chamber within which the glass fibers 622 and gas flowing from the multiple spinners 618 can be combined while controlling the characteristics of the resulting combined flow. In certain embodiments, the header system can include a control system (not shown) configured to combine the glass fibers 622 and gas flow from the spinners 618 and further configured to direct the resulting combined flow to the forming apparatuses 632a and 632b. Such a header system can allow for maintenance and cleaning of a particular spinner 618 without having to shut down the remaining spinners 618. Optionally, the header system can incorporate any desired means for controlling and directing the glass fibers 622 and gas flow.
[0083] Referring now to FIG. 7 , the momentum of the gas stream with entrained glass fibers 622 will cause the glass fibers 622 to continue flowing through duct 630 to formers 632a and 632b. Formers 632a and 632b can be configured for several functions. First, formers 632a and 632b can be configured to separate the entrained glass fibers 622 from the gas stream. Second, formers 632a and 632b can be configured to form a continuous, thin, dry-laid web of fibrous material having a desired thickness. Third, formers 632a and 632b can be configured to allow the glass fibers 622 to separate from the gas stream in a manner that allows the fibers to be oriented within the web with any desired degree of “randomness.” The term “randomness,” as used herein, is defined to mean that the fibers 622 or portions of the fibers 622 can be non-preferentially oriented in any of the X, Y, or Z dimensions. In certain cases, having a high degree of randomness may be desirable. In other cases, it may be desirable to control the randomness of the fibers so that the fibers are non-randomly oriented, in other words, the fibers are substantially coplanar or substantially parallel to one another. Fourth, forming devices 632a and 632b can be configured to transport the continuous web of fibrous material to other downstream operations.
[0084] In the embodiment shown in FIG. 7, each of forming apparatuses 632a and 632b includes a drum (not shown) configured to rotate. The drum can include any desired number of foraminous surfaces and zones of higher or lower pressure. Alternatively, each of forming apparatuses 632a and 632b can be formed from other structures, mechanisms, and devices sufficient to separate entrained glass fibers 622 from the gas stream, form a continuous web of fibrous material having a desired thickness, and transport the continuous web of fibrous material to other downstream operations. In the illustrative embodiment shown in FIG. 7, each of forming apparatuses 632a and 632b is the same. However, in other embodiments, each of forming apparatuses 632a and 632b can be different from one another.
[0085] Referring again to FIG. 7 , the continuous web of fibrous material is transferred from forming devices 632 a and 632 b to optional binder applicator 646. Binder applicator 646 is configured to apply a “dry binder” to the continuous web of fibrous material. The term “dry binder,” as used herein, is defined to mean that the binder is composed of substantially 100% solids at the time the binder is applied. The term “substantially 100% solids,” as used herein, is defined to mean any binder material having a diluent, e.g., water, equal to or less than about 2% of the binder’s weight (at the time the binder is applied, not after the binder has dried and / or cured), preferably equal to or less than about 1%. However, it should be appreciated that in certain embodiments, the binder can include any desired amount of diluent, e.g., water, depending on specific application and design requirements. The binder can be configured to be heat cured in curing oven 650. In this application, the terms "cure" and "thermally set" refer to a chemical reaction and / or one or more phase changes that cause a dry binder to bond the fibers of a web to one another. For example, a thermosetting dry binder (or a thermosetting component of a dry binder) cures or thermally sets as a result of a chemical reaction that occurs as a result of the application of heat. A thermoplastic dry binder (or a thermoplastic component of a dry binder) cures or thermally sets as a result of being heated to a softened or molten phase and then cooled to a solid phase.
[0086] In an exemplary embodiment, the dry binder is a thermoplastic resin-based material that is not applied in liquid form and is not water-based. In other embodiments, the dry binder can be other materials or mixtures of materials, including, but not limited to, polymeric thermosetting resins. The dry binder can have any form or combination of forms, including, but not limited to, powders, particles, fibers, and / or hot melts. Examples of hot melt polymers include, but are not limited to, ethylene-vinyl acetate copolymers, ethylene-acrylate copolymers, low-density polyethylene, high-density polyethylene, atactic polypropylene, polybutene-1, styrene block copolymers, polyamides, thermoplastic polyurethanes, styrene block copolymers, polyesters, and the like. Sufficient dry binder is applied so that the cured fiber pack can be compressed for packaging, storage, and shipping, yet still regain its thickness when placed (a process known as "bulk recovery"). Applying the dry binder to a continuous web of fibers forms a continuous web, optionally with unreacted binder.
[0087] 6 and 7, binder applicator 646 is a sprayer configured for dry powder. The sprayer is configured with an adjustable spray force, thereby allowing for more or less penetration of the dry powder into the continuous web of fibrous material. Alternatively, binder applicator 646 can be another structure, mechanism, or device, or combination thereof, such as, for example, a vacuum device sufficient to draw a "dry binder" into the continuous web of fibrous material.
[0088] Although the embodiment shown in FIG. 7 depicts a binder applicator 646 configured to apply a dry binder to a continuous web of fibrous material, it is within the contemplation of the present invention that in certain embodiments, a dry binder is not applied to the continuous web of fibrous material.
[0089] Referring again to FIG. 7, a continuous web, optionally including an unreacted binder, is transferred from binder applicator 646 to corresponding cross-folding mechanisms 634a and 634b. As shown in FIG. 7, former 632a is associated with cross-folding mechanism 634a, and former 632b is associated with cross-folding mechanism 634b. Cross-folding mechanisms 634a and 634b function in conjunction with a first conveyor 636. First conveyor 636 is configured to move in a machine direction indicated by arrow D1. Cross-folding mechanism 634a is configured to receive the continuous web, optionally including an unreacted binder, from optional binder applicator 646 and to deposit alternating layers of the continuous web, optionally including an unreacted binder, onto first conveyor 636 as first conveyor 636 moves in machine direction D1, thereby forming an initial layer of a fibrous body. In this deposition process, cross-folder 634a forms alternating layers in the cross-machine direction indicated by arrow D2. Thus, as the deposited continuous web, optionally containing unreacted binder, moves in machine direction D1 from cross-folder 634a, additional layers are deposited onto the fibrous body by downstream cross-folder 634b. The resulting layers of fibrous body deposited by cross-folders 634a and 634b form a pack.
[0090] In the illustrated embodiment, the cross-folding mechanisms 634a and 634b are devices configured to precisely control the movement of the continuous web containing the unreacted binder and deposit the continuous web containing the unreacted binder onto the first conveyor 636, optionally without damaging the continuous web containing the unreacted binder. The cross-folding mechanisms 634a and 634b can include any desired structure and can be configured to operate in any desired manner. In one example, the cross-folding mechanisms 634a and 634b can include a head (not shown) configured to move back and forth in the cross-machine direction D2. In this embodiment, the speed of the movable head is adjusted so that the movement of the head in both cross-machine directions is substantially the same, thereby providing uniformity in the resulting layer of fibrous body. In another example, a vertical conveyor (not shown) configured and centered on the centerline of the first conveyor 636 can be used. The vertical conveyor is further configured to pivot above the first conveyor 636 to deposit the continuous web, optionally including the unreacted binder, onto the first conveyor 636. Although several examples of cross-folding mechanisms are described above, it should be recognized that the cross-folding mechanisms 634a and 634b can be other structures, mechanisms, or devices, or combinations thereof.
[0091] 7, a controller (not shown) optionally controls the positioning of the continuous web, optionally including unreacted binder, on the first conveyor 636 to provide improved pack uniformity. The controller can be any desired structure, mechanism, or device, or combination thereof.
[0092] The laminated web or pack can have any desired thickness. The thickness of the pack is a function of several variables. First, the thickness of the pack is a function of the thickness of the continuous web, optionally containing unreacted binder, formed by each of forming apparatuses 632a and 632b. Second, the thickness of the pack is a function of the speed at which cross-folding mechanisms 634a and 634b alternately deposit layers of the continuous web, optionally containing unreacted binder, onto first conveyor 636. Third, the thickness of the pack is a function of the speed of first conveyor 636. In the illustrated embodiment, the pack has a thickness ranging from about 0.1 inches to about 20.0 inches. In other embodiments, the pack can have a thickness less than about 0.1 inches or greater than about 20.0 inches.
[0093] As described above, the cross-folding mechanisms 634a and 634b are configured to deposit alternating layers of the continuous web, optionally including unreacted binder, onto the first conveyor 636 as it moves in the machine direction D1, thereby forming layers of the fibrous body. In the illustrated embodiment, the cross-folding mechanisms 634a and 634b and the first conveyor 636 are adjusted to form a fibrous body having a number of layers ranging from about 1 to about 60. In other embodiments, the cross-folding mechanisms 634a and 634b and the first conveyor 636 can be adjusted to form a fibrous body having any number of layers, including a fibrous body having more than 60 layers.
[0094] Optionally, the cross-folding features 634a and 634b can be adjustable, thereby allowing the cross-folding features 634a and 634b to form packs having any desired width. In certain embodiments, the packs can have an overall width ranging from about 98.0 inches to about 236.0 inches. Alternatively, the packs can have an overall width less than about 98.0 inches or greater than about 236.0 inches.
[0095] Although cross-folding mechanisms 634a and 634b are described above as jointly participating in forming the fibrous body, it should be appreciated that in other embodiments, cross-folding mechanisms 634a and 634b can operate independently of one another to form separate lanes of the fibrous body.
[0096] 6 and 7, the packs having layers formed by cross-folding mechanisms 634a and 634b are conveyed by a first conveyor 636 to an optional trimming mechanism 640. The optional trimming mechanism 640 is configured to trim the edges of the packs to form a desired pack width. In an exemplary embodiment, the packs can have a trimmed width ranging from about 980 inches to about 236.0 inches. Alternatively, the packs can have a trimmed width less than about 98.0 inches or greater than about 236.0 inches.
[0097] In the illustrated embodiment, optional trimming mechanism 640 includes a saw system having multiple rotary saws (not shown) positioned on either side of the puck. Alternatively, trimming mechanism 640 can be other structures, mechanisms, or devices, or combinations thereof, including, but not limited to, water jets, compression knives, etc.
[0098] In the illustrated embodiment, trimming mechanism 640 is advantageously located upstream from curing oven 650. Locating trimming mechanism 640 upstream from curing oven 650 allows the puck to be trimmed before it is thermally cured in curing oven 650. Optionally, material trimmed from the puck by trimming mechanism 640 can be returned to the flow of gas and glass fibers in duct 630 for reuse in forming apparatuses 632a and 632b. Recycling the trimmed material advantageously prevents potential environmental issues associated with disposal of the trimmed material. As shown in FIG. 6 , conduit 642 connects trimming mechanism 640 to duct 630 and is configured to facilitate the return of the trimmed material to forming apparatuses 632a and 632b. While the embodiments shown in FIGS. 6 and 7 illustrate recycling of the trimmed material, it should be appreciated that recycling of the trimmed material is optional, and method 610 of forming a puck from fibrous material can be performed without recycling the trimmed material. In another exemplary embodiment, the trimming mechanism 640 is located downstream from the curing oven 650. This location is particularly useful when the trimmed material is not being recycled. Trimming the puck forms a trimmed puck.
[0099] The trimmed pucks are transported by the first conveyor 636 to the second conveyor 644. As shown in Figure 6, the second conveyor 644 can be positioned so that it is "stepped down" from the first conveyor 636. The term "stepped down," as used herein, is defined to mean that the upper surface of the second conveyor 644 is positioned vertically below the upper surface of the first conveyor 636. Conveyor stepping down is described in more detail below.
[0100] Referring again to FIGS. 1 and 2 , the trimmed puck is conveyed by a second conveyor 644 to an optional entanglement mechanism 645. The entanglement mechanism 645 is configured to entangle the individual fibers 622 that form the layers of the trimmed puck. The entanglement of the glass fibers 622 within the puck binds the puck together. In embodiments including a dry binder, the entanglement of the glass fibers 622 can advantageously improve mechanical properties such as tensile strength and shear strength. In the illustrated embodiment, the entanglement mechanism 645 is a needling mechanism. In other embodiments, the entanglement mechanism 645 can include other structures, mechanisms, or devices, or combinations thereof, including, by way of non-limiting example, a stitching mechanism. While the embodiment shown in FIGS. 6 and 7 illustrates the use of the entanglement mechanism 645, it should be appreciated that the use of the entanglement mechanism 645 is optional, and the method 610 of forming a puck from a fibrous material can be performed without the use of the entanglement mechanism 645. The entanglement of the fibers within the pack forms an entangled puck.
[0101] The second conveyor 644 transports the optionally trimmed and / or optionally entangled pucks, optionally including a dry binder (hereinafter, both trimmed pucks and entangled pucks will be referred to simply as "pucks") to a third conveyor 648. If the puck includes a dry binder, the third conveyor 648 is configured to transport the puck to an optional curing oven 650. The curing oven 650 is configured to blow a fluid, such as heated air, through the puck, thereby curing the dry binder and rigidly bonding the glass fibers 622 to one another in a generally random three-dimensional structure. Curing the puck in the curing oven 650 forms a cured puck.
[0102] As mentioned above, the pack optionally includes a dry binder. The use of a dry binder rather than a traditional wet binder advantageously allows the curing oven 650 to use less energy to cure the dry binder in the pack. In the illustrated embodiment, the use of a dry binder in the curing oven 650 results in energy savings ranging from about 30.0% to about 80.0% compared to the energy used by conventional curing ovens to cure wet or water-based binders. In still other embodiments, energy savings may exceed 80.0%. The curing oven 650 can be any desired curing structure, mechanism, or device, or combination thereof.
[0103] The third conveyor 648 transports the cured pucks to a fourth conveyor 652. The fourth conveyor 652 is configured to transport the cured pucks to a cutting mechanism 654. Optionally, the cutting mechanism 654 can be configured in several cutting modes. In a first optional cutting mode, the cutting mechanism is configured to cut the cured puck vertically along the machine direction D1 to form lanes. The formed lanes can have any desired width. In a second optional cutting mode, the cutting mechanism is configured to horizontally bisect the cured puck to form a continuous puck having a thickness. The resulting bisect pucks can have any desired thickness. Cutting the cured puck forms the cut pucks.
[0104] In the illustrated embodiment, cutting mechanism 654 includes a saw and knife system. Alternatively, cutting mechanism 654 can be other structures, mechanisms, or devices, or combinations thereof. Referring again to FIGS. 6 and 7, cutting mechanism 654 is advantageously positioned to capture dust and other waste materials formed during the cutting operation. Optionally, dust and other waste materials from the cutting mechanism can be returned to the flow of gas and glass fibers in duct 630 for reuse within molding apparatuses 632a and 632b. Recycling of dust and waste materials advantageously prevents potential environmental problems associated with the disposal of dust and waste materials. As shown in FIGS. 6 and 7, conduit 655 connects cutting mechanism 654 to duct 630 and is configured to facilitate the return of dust and waste materials to molding apparatuses 632a and 632b. While the embodiments shown in Figures 6 and 7 illustrate recycling of dust and waste material, it should be appreciated that recycling of dust and waste material is optional and method 10 of forming pucks from fibrous material can be performed without recycling dust and waste material.
[0105] Optionally, prior to conveying the cured pack to the cutting mechanism 654, the major surfaces of the cured pack can be overlaid with one or more overlays by overlaying mechanisms 662a, 662b, as shown in FIG. 6 . In the illustrated embodiment, the top major surface of the cured pack is overlaid with overlay 663a provided by overlaying mechanism 662a, and the bottom major surface of the cured pack is overlaid with overlay 663b provided by overlaying mechanism 662b. The overlays can be any desired material, including paper, polymeric material, or nonwoven web. Overlaying mechanisms 662a and 662b can be any desired structure, mechanism, or device, or combination thereof. In the illustrated embodiment, overlays 663a and 663b are affixed to the cured pack (if the pack includes a binder) by adhesive. In other embodiments, overlays 663a and 663b are affixed to the cured pack by other methods, including ultrasonic welding, as a non-limiting example. While the embodiment shown in FIG. 6 shows the application of outer linings 663a and 663b to the major surfaces of the hardening pack, it should be appreciated that the application of outer linings 663a and 663b to the major surfaces of the hardening pack is optional and method 610 of forming a pack from fibrous material can be performed without applying outer linings 663a and 663b to the major surfaces of the hardening pack.
[0106] 6 and 7, the fourth conveyor 652 conveys the cut packs to an optional chopping mechanism 656. The chopping mechanism 656 is configured to cut the cut packs to a desired length across the machine direction D1. In the illustrated embodiment, the chopping mechanism 656 is configured to cut the cut packs as they move continuously in the machine direction D1. Alternatively, the chopping mechanism 656 can be configured for a batch chopping operation. Cutting the cut packs to a predetermined length forms dimensioned packs. The length of the chopped packs can have any desired dimension.
[0107] Chopping mechanisms are known in the art and will not be described herein. Chopping mechanism 656 can be any desired structure, mechanism, or device, or combination thereof.
[0108] Optionally, prior to conveying the cutting pack to the chopping mechanism 656, the minor surfaces of the cutting pack can be overlaid with one or more edging materials by edging mechanisms 666a, 666b, as shown in FIG. 7 . The edging materials can be any desired material, including paper, polymeric materials, or nonwoven webs. The edging mechanisms 666a and 666b can be any desired structure, mechanism, or device, or combinations thereof. In the illustrated embodiment, the edging materials 667a, 667b are affixed to the cutting pack by adhesive. In other embodiments, the edging materials 667a, 667b can be affixed to the cutting pack by other methods, including, but not limited to, ultrasonic welding. While the embodiment shown in FIG. 7 illustrates application of edging material 667a and 667b to the minor surfaces of the cutting pack, it should be appreciated that application of edging material 667a and 667b to the minor surfaces of the cutting pack is optional and method 610 of forming a pack from fibrous material can be performed without applying edging material 667a and 667b to the minor surfaces of the cutting pack.
[0109] 6, the fourth conveyor 652 conveys the sized packs to a fifth conveyor 658. The fifth conveyor 658 is configured to convey the sized packs to a packaging mechanism 660. The packaging mechanism 660 is configured to package the sized packs for a future operation. The term "future operation," as used herein, is defined to include any activity subsequent to the formation of the sized packs, including, but not limited to, storage, shipping, and installation.
[0110] In the illustrated embodiment, the packaging mechanism 660 is configured to form the dimensional packs into a package in the form of a roll. In other embodiments, the packaging mechanism 660 can form packages having other desired shapes, such as, but not limited to, slabs, batts, and irregularly shaped or die-cut pieces. The packaging mechanism 660 can be any desired structure, mechanism, or device, or combination thereof.
[0111] Referring again to FIG. 6 , conveyors 636, 644, 648, 652, and 658 are in a “step-down” relationship in the machine direction D1. A “step-down” relationship means that the top surface of the next conveyor is positioned vertically below the top surface of the previous conveyor. The “step-down” relationship of the conveyors advantageously provides a self-threading feature for puck transport. In the illustrated embodiment, the vertical offset between adjacent conveyors ranges from about 3.0 inches to about 10.0 inches. In other embodiments, the vertical offset between adjacent conveyors can be less than about 3.0 inches or greater than about 10.0 inches.
[0112] 6 and 7, the method 610 of forming a puck from fibrous material eliminates the use of wet binders, thereby eliminating the conventional need for wash water and wash water-related structures, such as forming hoods, return pumps and piping, etc. Eliminating the use of water other than cooling water and the application of lubricants, colorants and other optional chemicals advantageously allows for a significant reduction in the overall size (or "footprint") of the production line, as well as reduced implementation costs, operating costs, and maintenance and repair costs.
[0113] 6 and 7, the method 610 for forming a puck from a fibrous material advantageously allows for uniform and even deposition of long, thin fibers on forming apparatuses 632a and 632b. In the illustrated embodiment, the fibers 622 have lengths ranging from about 0.25 inches to about 10.0 inches and diameters ranging from about 9HT to about 35HT. In other embodiments, the fibers 22 have lengths ranging from about 1.0 inches to about 5.0 inches and diameters ranging from about 14HT to about 25HT. In still other embodiments, the fibers 22 can have lengths less than about 0.25 inches or greater than about 10.0 inches and diameters less than about 9HT or greater than about 35HT. Without being bound by theory, it is believed that the use of relatively long, thin fibers advantageously provides a puck with superior thermal and acoustic insulation performance over a similarly sized puck having shorter, thicker fibers.
[0114] 6 and 7 have been generally described above as forming packs of fibrous material, it should be understood that the same apparatus can be configured to form "unbonded loose-pack insulation," which term, as used herein, is defined to mean any conditioned insulation material configured for application in an air stream.
[0115] Although exemplary embodiments of a pack and a method 610 for forming a pack from a fibrous material are generally described above, it should be appreciated that other embodiments and variations of the method 610 are available and are generally described below.
[0116] Referring to FIG. 7, in another embodiment of method 610, cross-folding mechanisms 634a and 634b are configured to provide precise deposition of alternating layers of the continuous web onto first conveyor 36, thereby enabling elimination of downstream trimming mechanism 40.
[0117] Referring again to FIG. 7 , in another embodiment of method 610, the various layers of the pack can be “stratified.” The term “stratified,” as used herein, is defined to mean that each of the layers and / or layer portions can be configured to have different properties, including, by non-limiting example, fiber diameter, fiber length, fiber orientation, density, thickness, and glass composition. It is contemplated that the associated mechanisms that form the layers, i.e., the associated spinners, forming devices, and cross-folding mechanisms, can be configured to provide layers and / or layer portions with specific desired properties. Thus, a pack can be formed from layers and / or layer portions having different properties.
[0118] 10A-10C illustrate an exemplary embodiment of an insulation product 1000 including one or more thick low-density cores 1002 and one or more thin high-density tensile layers 1004. The thick low-density core 1002 can take a variety of different forms. For example, the low-density core 1002 can be made from any of the low-weight-per-area packs described above. In one exemplary embodiment, the low-density core 1002 is made from needled and / or laminated glass fibers. In one exemplary embodiment, the low-density core 1002 is binderless. In another exemplary embodiment, the fibers 322 of the low-density core are bonded to one another by a binder.
[0119] The thin, dense tensile layer 1004 can take a variety of different forms. In one exemplary embodiment, the thin, dense tensile layer 1004 is made from fiberglass fibers that are needled together. However, the fibers of the dense tensile 1000 can be processed using other processes and / or products that achieve suitable tensile strength. In one exemplary embodiment, the dense tensile layer 1004 is made from the dense pack 300 of the embodiment of FIG. 3D.
[0120] In the exemplary embodiment, the high density tensile layer 1004 is attached to the low density core 1002. The high density tensile layer 1004 can be attached to the low density core 1002 in a variety of different ways. For example, the layers 1002, 1004 can be attached to one another with an adhesive, an additional needling step, thermal bonding (when one or both of the layers 1002, 1004 include a binder), etc. Any method of attaching the layers to one another can be used. In the exemplary embodiment, the layers 1002, 1004 impart distinct properties to the insulation product 1000.
[0121] In the exemplary embodiment, the thick low density layer 1002 provides a high thermal resistance value R but has low tensile strength, and the thin high density tensile layer 1004 provides a low thermal resistance value R but has high tensile strength. The combination of the two layers gives the insulation product 1000 both high tensile strength and a high R-value.
[0122] 10D-10F illustrate an exemplary embodiment of an insulation product 1000 including one or more thick, low-density cores 1002 and one or more thin outer lining layers 1004. The thick, low-density core 1002 can take a variety of different forms, as described with respect to the embodiment shown in FIGS. 10A-10C. The outer lining layer 1004 can take a variety of different forms. The material of the outer lining layer 1004 can be selected to impart a variety of different properties to the insulation product. For example, the outer lining material can be selected to impart a desired amount of strength, reflectivity, acoustic performance, water impermeability, and / or vapor impermeability to the insulation product. The outer lining layer can be made from a variety of different materials, including, but not limited to, plastic, metal foil, scrim, paper, combinations of these materials, and the like. Any known outer lining layer can be used.
[0123] In the exemplary embodiment, the outer layer 1004 is attached to the low density core 1002. The outer layer 1004 can be attached to the low density core 1002 in a variety of different ways. For example, the layers 1002, 1004 can be attached to one another with an adhesive, thermal bonding, etc. Any method of attaching the layers to one another can be used. In the exemplary embodiment, the layers 1002, 1004 provide distinct properties to the insulation product 1000. In the exemplary embodiment, the thick, low density layer 1002 provides a high thermal resistance value R but has low tensile strength, and the outer layer 1004 provides tensile strength and other properties.
[0124] The examples shown in Figures 10G-10I are described with respect to strata having different densities. However, the strata can have different properties, which may or may not include different densities. These varying properties can be achieved by varying fiber density, fiber length, fiber diameter, and / or fiber type throughout the thickness of the pack. Figures 10G-10I show an exemplary embodiment of a layered batt or pack 1050 that includes one or more low-density strata 1052 and one or more high-density strata 1054. However, the transition between the low-density strata 1052 and the high-density strata 1054 can be gradual. In the examples shown in Figures 10A-10F, the insulation product 1000 is formed from separate layers. In the exemplary embodiment shown in Figures 10G-10I, the layered batt or pack 1050 is formed to have varying properties throughout the thickness of the batt or pack. The low-density strata 1052 can take a variety of different forms. For example, the low-density layer 1052 can be made in the same manner as any of the low-weight-per-area packs described above. In one exemplary embodiment, the low-density layer 1052 is made from fiberglass fibers. In one exemplary embodiment, the low-density layer 1052 is binderless. In another exemplary embodiment, the fibers 322 of the low-density layer 1052 are bonded to one another by a binder.
[0125] The thin densified tier 1054 can take a variety of different forms. In one exemplary embodiment, the densified tier 1054 is made from fiberglass fibers that are needled together. However, the fibers of the densified tier 1054 can be processed using other processes and / or products that achieve suitable tensile strength. In one exemplary embodiment, the densified tier 1054 is made in the same manner as the densified pack 300 of the embodiment of FIG. 3D is made.
[0126] In an exemplary embodiment, the fibers of the high-density layer 1054 are attached and / or entangled with the fibers of the low-density layer 1052. The fibers of the high-density layer 1054 can be attached to the fibers of the low-density layer 1052 in a variety of different ways. For example, the fibers of layers 1002, 1004 can be attached to one another by an adhesive, such as a binder applied to the pack, and / or by needling, or the like, performed when making the pack 1050. Any method of attaching or entangling the fibers of layers 1052, 1054 can be used. In an exemplary embodiment, layers 1052, 1054 impart different properties to the insulation product 1000.
[0127] The insulation batts, packs, and products of the embodiments of Figures 10A-10I can be combined with one another. For example, any of the layers of the insulation products shown in Figures 10A-10F can be layered, and the layered batts or packs of Figures 10G-10I can be provided with one or more outer layers, separate densification layers, etc. A variety of different insulation structures can be constructed from the embodiments shown in Figures 10A-10I.
[0128] In an exemplary embodiment, the thick, low-density layer 1052 provides a high thermal resistance value R but has low tensile strength, and the thin, high-density tensile layer 1004 provides a low thermal resistance value R but has high tensile strength. The combination of the two layers provides the bat or puck 1050 with both high tensile strength and a high R-value. The layers can be configured to provide a variety of different properties to the bat or puck. For example, alternating thin, high-density layers and thick, low-density layers provides a bat or puck with excellent acoustic properties.
[0129] In one exemplary embodiment, the dry binder can include or be coated with additives to impart desired properties to the pack. One non-limiting example of an additive is a flame retardant, such as baking soda. Another non-limiting example of an additive is a material that blocks the transmission of ultraviolet light through the pack. Yet another non-limiting example of an additive is a material that blocks the transmission of infrared light through the pack.
[0130] Referring to FIG. 6 , in another embodiment of method 610, as previously described, the hot gas flow can be generated by an optional blower mechanism, such as, but not limited to, an annular blower (not shown) or an annular burner (not shown). It is known in the art that the heat generated by the annular blower or annular burner is referred to as “heat of fiberization.” In this embodiment, it is contemplated that the heat of fiberization can be captured and recycled for use in other mechanisms or devices. The heat of fiberization can be captured at several locations in method 610. As shown in FIGS. 6 and 7 , ductwork 670 is configured to capture heat emanating from the spinner 618 and convey the heat for use in other mechanisms, such as optional curing oven 650. Similarly, piping 672 is configured to capture heat emanating from the hot gas flow in duct 30, and piping 674 is further configured to capture heat emanating from forming devices 632a and 632b. Recycled heat can also be used for purposes other than forming a fibrous pack, such as office heating.
[0131] In certain embodiments, the duct 630 can include a heat acquisition device, such as a heat extraction fixture, configured to acquire heat without significantly affecting the momentum of the flow of hot gas and entrained glass fibers 622. In other embodiments, any desired structure, device, or mechanism sufficient to acquire the heat of spinning can be used.
[0132] 6, in another embodiment of method 610, fibers or other materials having other desired properties may be mixed with the glass fibers 622 entrained in the gas stream. In this embodiment, a source 676 of other materials, such as, for example, synthetic or ceramic fibers, colorants and / or particles, may be provided such that such materials are introduced into duct 678.
[0133] Duct 678 can be connected to duct 630 to allow mixing with the glass fibers 622 entrained in the gas flow. In this manner, the properties of the resulting pack can be designed or tailored to desired properties, including, but not limited to, acoustic, thermal enhancement, or UV retardation properties.
[0134] In still other embodiments, it is contemplated that other materials may be placed between the layers deposited on the first conveyor 636 by the cross-folding mechanisms 634a and 634b. The other materials may include sheet materials such as, for example, liner, moisture barriers, or netting, or other non-sheet materials, including, but not limited to, powders, particles, or adhesives. The other materials may be placed between the layers in any desired manner. In this manner, the properties of the resulting pack may be further engineered or adjusted as desired.
[0135] 6 illustrates the application of a dry binder by a binder applicator 646, it should be appreciated that in other embodiments, the dry binder can be applied to the glass fibers 622 entrained in the gas stream. In this embodiment, a source of dry binder 680 can be introduced into a duct 682. The duct 682 is connected to the duct 630 to allow mixing of the dry binder with the glass fibers 622 entrained in the gas stream. The dry binder can be configured to adhere to the glass fibers in any desired manner, including an electrostatic process.
[0136] While the embodiment shown in FIG. 6 illustrates the use of a continuous web with cross-folding mechanisms 634a and 634b, it should be appreciated that in other embodiments, the web can be removed from forming devices 632a and 632b and stored for later use.
[0137] As previously mentioned, the trimmed material can optionally be returned to the gas and fiberglass flow in duct 630 and reused in formers 632a and 632b. In an exemplary embodiment, when an optional binder is included in the pack, the operating temperature of formers 332a and 332b is kept below the softening temperature of the dry binder, thereby preventing the binder from hardening prior to operation of downstream curing oven 550. In this embodiment, the maximum operating temperature of curing oven 650 ranges from about 165°F to about 180°F. In other embodiments, the maximum operating temperature of curing oven 650 can be lower than about 165°F or higher than about 180°F.
[0138] In exemplary embodiments, the long, thin fibers 322 described herein are used in other applications than those described above. For example, Figure 11 shows that the long, thin fibers 322 described above are not formed into a web and / or pack, but are provided as staple fibers that are air-laid, carded, or otherwise processed for use in a variety of different applications. In one application, the unbonded staple fibers are blended with aramid fibers such as Kevlar and Konex, and / or thermal bond fibers such as Celbond. These blended fibers can be used to form staple yarns and / or dry-laid nonwoven materials.
[0139] In the embodiment of Figure 11, melter 314 delivers molten glass 312 to forehearth 316. Molten glass 312 is processed to form glass fibers 322. Molten glass 312 can be processed in a variety of different ways to form fibers 322. For example, rotary spinner 318 receives molten glass 312 and then forms a veil 320 of glass fibers 322. Any desired spinner, rotary or otherwise, sufficient to form long, thin glass fibers 322 can be used.
[0140] Referring to FIG. 11 , an applicator 1100 applies a lubricant, also called a size, to the unbonded glass fibers. In the illustrated embodiment, the size is applied to the glass fibers below the spinner. However, in other embodiments, the size is applied to the glass fibers at other locations, such as in duct 330. The size strengthens the fibers and / or provides lubricity to the fibers, which aids in fiber processing, such as fiber needling or carding. Unbonded staple fibers 322 are provided at the exit of duct 330, as indicated by arrow 1102, where the fibers are collected in a container 1103 for use in a variety of different applications, either by themselves or in combination with other fibers, such as aramid fibers.
[0141] The sizing agent can take a variety of different forms. For example, the sizing agent can include silicone and / or silane. However, any sizing agent can be used depending on the application. The sizing agent can be adjusted based on the application in which the glass fiber is to be used.
[0142] The small fiber diameter and long fiber length allow the sized fibers to be used in applications where fibers previously could not be used because the fibers would break too easily. In one exemplary embodiment, the thinner the fiber, the easier it is to bend without breaking, so fibers 322 having a diameter of approximately 4 microns have a flexural modulus and resulting strength that is superior to conventional fibers. This improved flexural modulus and strength of the fiber helps the fiber withstand processes such as carding and air-laminating, which are typically destructive to conventional fibers. Additionally, the fine diameter of glass fibers improves both thermal and acoustic performance.
[0143] Glass webs, packs, and staple fibers can be used in a variety of different applications. Example applications include, but are not limited to, heating appliances such as ovens, ranges, and water heaters; heating, ventilation, and air conditioning (HVAC) components such as HVAC ducts; acoustical panels and materials such as building and / or vehicle acoustical panels; and molded fiberglass components such as compression-molded or vacuum-formed fiberglass components. In one exemplary embodiment, heating appliances such as ovens, ranges, and water heaters; heating HVAC components such as HVAC ducts; acoustical panels and materials such as building and / or vehicle acoustical panels; and / or molded fiberglass components such as compression-molded or vacuum-formed fiberglass components use or are manufactured from binderless fiberglass packs made according to one or more embodiments disclosed by this patent application. In an exemplary embodiment, because the fiberglass pack is binderless, there is no formaldehyde present in the fiberglass pack. In one exemplary embodiment, heating appliances such as ovens, ranges, and water heaters, heating HVAC components such as HVAC ducts, acoustic panels and materials such as building and / or vehicle acoustic panels, and / or molded fiberglass components such as compression molded or vacuum formed fiberglass components use or are manufactured from dry-laid fiberglass packs made according to one or more embodiments disclosed herein. In this exemplary embodiment, the dry-laid binder can be formaldehyde-free or a formaldehyde-free dry-laid binder. In the case of a formaldehyde-free binder, the binder itself does not contain formaldehyde, but formaldehyde may be a by-product when the binder is burned.
[0144] The fiberglass insulation packs described in this patent application can be used in a variety of different cooking ranges and in a variety of different configurations within any given cooking range. U.S. Patent No. 6,299,495 discloses an example of an insulation system for use within a range. U.S. Patent No. 6,299,495 is incorporated herein by reference in its entirety. The fiberglass packs described herein can be used in any of the heating appliance insulation structures described in U.S. Patent No. 6,299,495, including configurations that may be classified as prior art. Figures 12-14 correspond to Figures 1-3 of U.S. Patent No. 6,299,495.
[0145] Referring to FIG. 12 , a thermal oven 1210 includes a substantially flat upper cooking surface 1212. As shown in FIGS. 12-14 , the thermal oven 1210 includes a pair of opposing side panels 1252 and 1254, a rear panel 1224, a bottom panel 1225, and a front panel 1232. The opposing side panels 1252 and 1254, the rear panel 1224, the bottom panel 1225, the front panel 1232, and the cooking surface 1212 are configured to form an outer oven cabinet 1233. The front panel 1232 includes an insulated oven door 1218 pivotally connected to the front panel 1232. The oven door 1218 is hinged to the lower end of the front panel 1232, allowing the oven door to pivot away from the front panel 1232 and the oven cavity 1216. In the example shown in FIG. 12 , the oven door 1218 includes a window. In the example shown in Figure 12A, the oven door 1218 does not include a window, and the entire interior of the door is insulated.
[0146] 13 and 14, the outer oven cabinet 1233 supports an inner oven liner 1215. The inner oven liner 1215 includes opposing liner sides 1215a and 1215b, a liner top 1215c, a liner bottom 1215d, and a liner back 1215e. The opposing liner sides 1215a and 1215b, the liner top 1215c, the liner bottom 1215d, the liner back 1215e, and the oven door 1218 are configured to define an oven cavity 1216.
[0147] 13 and 14, the outside of the oven liner 1215 is covered with insulating material 1238, which may be made according to any of the embodiments disclosed herein. The oven door 1238 may also be filled with insulating material 1238, which may be made according to any of the embodiments disclosed herein. The insulating material 1238 is positioned in contact with the exterior surface of the oven liner 1215. The insulating material 1238 serves many purposes, including retaining heat within the oven cavity 1216 and limiting the amount of heat transferred to the outer oven cabinet 1233 by conduction, convection, and radiation.
[0148] As shown in the example illustrated in FIGS. 13 and 14 , an air gap 1236 is formed between the insulating material 1238 and the outer oven cabinet 1233. The air gap 1236 is used as additional insulation to limit conductive heat transfer between the oven liner 1215 and the outer oven cabinet 1233. The use of the air gap 1236 complements the insulating material 1238 to minimize the surface temperature of the exterior surface of the outer oven cabinet 1233. As shown in the example illustrated in FIGS. 13A and 14A , the insulating material 1238 can be sized such that no air gap is formed between the insulating material 1238 and the outer oven cabinet 1233. That is, in the embodiment of FIGS. 13A and 14A , the insulating layer 1238 completely fills the space between the oven liner 1215 and the outer oven cabinet 1233. In one exemplary embodiment, the insulation material used in the configurations shown in Figures 13, 13A, 14, and 14A, and any other configurations disclosed by the '066 patent application, is made from a binderless fiberglass pack made according to one or more embodiments disclosed by this patent application. In an exemplary embodiment, because the fiberglass pack is binderless, there is no formaldehyde present in the insulation layer 1238 of the embodiments of Figures 13, 13A, 14, and 14A.
[0149] The fiberglass packs described in this patent application can be used in a variety of different heating, ventilation, and air conditioning (HVAC) systems, such as the ductwork of HVAC systems. Furthermore, the insulation packs described in this patent application can be provided in a variety of different configurations within any given HVAC duct. U.S. Patent Nos. 5,629,992 (Patent Document 1), 5,629,992 (Patent Document 2), and pending U.S. patent application Ser. No. 13 / 764,920, filed February 12, 2013, all of which are assigned to the assignee of the present application, disclose examples of fiberglass insulation systems used within HVAC ducts. U.S. Patent No. 5,629,992 (Patent Document 1), 5,629,992 (Patent Document 2), and pending U.S. patent application Ser. No. 13 / 764,920, are incorporated herein by reference in their entireties. The fiberglass packs described herein can be used in any of the HVAC duct configurations described in U.S. Patent Nos. 5,629,992 (Patent Document 1), 5,629,992 (Patent Document 2), and pending U.S. patent application Ser. No. 13 / 764,920.
[0150] In one exemplary embodiment, the insulation materials used in HVAC ducts disclosed in U.S. Patent Nos. 6,279,999, 6,289,920, 6,313,926, and pending U.S. patent application Ser. No. 13 / 764,920 can be constructed from dry-laid fiberglass packs made according to one or more embodiments disclosed in this patent application. In this exemplary embodiment, the dry-laid binder can be a formaldehyde-free dry-laid binder or a formaldehyde-free dry-laid binder. In a formaldehyde-free binder, the binder itself does not contain formaldehyde, but formaldehyde may be a by-product when the binder is combusted.
[0151] In exemplary embodiments, the insulation materials used in HVAC ducts disclosed in U.S. Patent Nos. 5,629,999, 5,729,949, 5,729,959, and pending U.S. patent application Ser. No. 13 / 764,920 can be constructed from binderless fiberglass packs made according to one or more embodiments disclosed in this patent application. In exemplary embodiments, because the fiberglass packs are binderless, there is no formaldehyde present in the insulation material.
[0152] The fiberglass insulation packs described in this patent application can be used in a variety of different acoustic applications and can take a variety of different configurations within each application. Examples of sound attenuation batts include Owens Corning Sound Attenuation Batt and Owens Corning Sonobatts insulation, which can be placed behind various building panels, such as ceiling tiles or walls. U.S. Patent Nos. 5,629,997 and 5,629,997 describe example sound attenuation applications and are incorporated herein by reference in their entireties. The fiberglass packs described herein can be used in place of Owens Corning Sound Attenuation Batt and Owens Corning Sonobatts sound attenuation materials and can be used in any of the applications disclosed in U.S. Patent Nos. 5,629,997 and 5,629,997. Additional acoustic applications for the fiberglass insulation packs described in this patent application include, but are not limited to, duct liners, duct wraps, ceiling panels, wall panels, and the like.
[0153] In one exemplary embodiment, an acoustical pack made with one or more embodiments of the binderless or dry-binder packs disclosed herein and tested according to ASTM C522 at up to 1,500 feet above sea level has an average airflow resistivity of 3,000-150,000 (mks Rayls / m). In one exemplary embodiment, an acoustical pack made with one or more embodiments of the binderless or dry-binder packs disclosed herein and tested according to ASTM C423 at up to 1,500 feet above sea level has a Sound Absorption Average (SAA) ranging from 0.25 to 1.25. In one exemplary embodiment, an acoustical pack made with one or more embodiments of the binderless or dry-binder packs disclosed herein and tested according to ISO 354 at up to 1,500 feet above sea level has a sound absorption coefficient αw ranging from 0.25 to 1.25.
[0154] [Table 2]
[0155] In one exemplary embodiment, sound-proofing materials used in place of Owens Corning Sound Attenuation Batts and Owens Corning Sonobatts sound-proofing materials, and / or for any of the applications disclosed in U.S. Patent Nos. 5,999,499 and 5,999,499, are constructed from dry-laid fiberglass packs made according to one or more embodiments disclosed in this patent application. In this exemplary embodiment, the dry-laid binder can be a formaldehyde-free dry-laid binder or a formaldehyde-free dry-laid binder. In a formaldehyde-free dry-laid binder, the binder itself does not contain formaldehyde, but formaldehyde may be a by-product when the binder is burned.
[0156] In an exemplary embodiment, sound-proofing materials used in place of Owens Corning Sound Attenuation Batts and Owens Corning Sonobatts sound-proofing materials, and / or for any of the applications disclosed in U.S. Patent Nos. 5,999,499 and 5,999,499 are constructed from binderless fiberglass packs made according to one or more embodiments disclosed in this patent application. In this exemplary embodiment, because the fiberglass packs are binderless, there is no formaldehyde present in the sound-proofing material.
[0157] The fiberglass insulation packs described herein can be used in a variety of molded fiberglass products. For example, with reference to Figures 15A-15C, in one embodiment, a compression-molded fiberglass product can be made using the binderless and / or dry-binder fiberglass packs described herein. With reference to Figure 15A, a binderless and / or dry-binder fiberglass pack 1522 made according to any of the exemplary embodiments described herein is placed between first and second mold halves 1502. In the exemplary embodiment, only the binderless or dry-binder fiberglass pack 1522 is placed between the mold halves. That is, no additional material, such as, for example, a plastic sheet or plastic resin, is molded with the fiberglass pack.
[0158] 15B, the mold halves compress fiberglass pack 1522, as indicated by arrow 1504. Optionally, heat is applied to the mold halves and / or fiberglass pack, as indicated by arrow 1506. For example, if pack 1522 is a binderless fiberglass pack, the mold halves and / or fiberglass pack can be heated to an elevated temperature, such as above 700°F, for example, between 700°F and 1100°F, and in one exemplary embodiment, up to about 900°F. If pack 1522 is a dry-binder fiberglass pack, the mold halves and / or fiberglass pack can be heated to a lower temperature, such as the melting point of the dry binder in the pack.
[0159] 15C, the mold halves are then moved apart as shown by arrows 1508, ejecting the compression molded fiberglass part 1510. In one exemplary embodiment, the compression molded fiberglass part 1510 consists solely of, or consists essentially of, the material of the puck 1522.
[0160] 15A-15C, the compression molded fiberglass component is shaped. However, in other exemplary embodiments, the compression molded fiberglass component can be substantially flat. In one exemplary embodiment, the binderless or dry-binder compression molded fiberglass component 1610 has a density that is substantially higher than the density of the originally prepared fiberglass pack 1522, for example, four or more times the density of the originally prepared fiberglass pack 1522.
[0161] 16A-16C, in one exemplary embodiment, a vacuum formed fiberglass product can be made using the binderless or dry-binder fiberglass packs described herein. Referring to FIG. 16A, a binderless and / or dry-binder fiberglass pack 1522 made according to any of the exemplary embodiments described herein is placed on a vacuum mold component 1602. In one exemplary embodiment, only the binderless or dry-binder fiberglass pack 1522 is placed on the mold component 1602. That is, no additional material, such as, for example, a plastic sheet or plastic resin, is molded with the fiberglass pack.
[0162] 16B, the mold components apply a vacuum to the fiberglass pack 1522, as indicated by arrow 1604. Optionally, heat is applied to the mold components 1602 and / or the fiberglass pack, as indicated by arrow 1606. For example, if the pack 1522 is a binderless fiberglass pack, the vacuum mold components 1602 and / or the fiberglass pack 1522 can be heated to an elevated temperature, such as above 700°F, for example, between 700°F and 1100°F, and in one exemplary embodiment, up to about 900°F. If the pack 1522 is a dry-binder fiberglass pack, the mold halves and / or the fiberglass pack can be heated to a lower temperature, such as the melting point of the dry binder in the pack.
[0163] 15C, the vacuum mold component 1602 stops applying vacuum and the vacuum-formed fiberglass part 1610 is removed. In one exemplary embodiment, the compression-molded fiberglass part 1610 consists solely of, or consists essentially of, the material of the puck 1522.
[0164] 16A-16C, the vacuum-formed fiberglass component is shaped. However, in other exemplary embodiments, the vacuum-formed fiberglass component can be substantially flat. In one exemplary embodiment, the binderless or dry-binder vacuum-formed fiberglass component 1610 has a density that is substantially higher than the density of the originally prepared fiberglass pack 1522, for example, four or more times the density of the originally prepared fiberglass pack 1522.
[0165] In one exemplary embodiment, the insulating material molded according to the embodiment shown in Figures 15A-15C or the embodiment shown in Figures 16A-16C is made from a binderless fiberglass pack made according to one or more embodiments disclosed in this patent application. In the exemplary embodiment, because the fiberglass pack is binderless, no formaldehyde is present in the compression molded part 1510 or vacuum formed part of the embodiments shown in Figures 15A-15C and 16A-16C.
[0166] In an exemplary embodiment, insulation formed according to the embodiment shown in Figures 15A-15C or the embodiment shown in Figures 16A-16C is made from a dry-lay fiberglass pack made according to one or more embodiments disclosed in this patent application. In this exemplary embodiment, the dry-lay binder can be a formaldehyde-free dry-lay binder or a formaldehyde-free dry-lay binder. In a formaldehyde-free binder, the binder itself does not have formaldehyde, but formaldehyde may be a by-product when the binder is burned.
[0167] Several exemplary embodiments of mineral fiber webs, packs, and staple fibers, and methods of making mineral fiber webs, packs, and staple fibers are disclosed by the present application. The mineral fiber webs and packs and methods of making mineral fiber webs and packs according to the present invention can include any combination or subcombination of the features disclosed by the present application.
[0168] In accordance with the provisions of the patent statutes, the principles and aspects of the improved method for forming a puck from fibrous material have been described and illustrated in its preferred embodiment. However, it will be understood that the improved method for forming a puck from fibrous material may be practiced otherwise than as specifically described and illustrated without departing from its spirit or scope. [Explanation of symbols]
[0169] 300: Pack 312, 612: Molten glass 314, 614: Melting equipment 316, 616: Forehearth 318, 618: Rotary spinning machine 320, 620: Glass fiber veil 321, 521: Web 322, 622: Glass fiber 324, 624: Collection materials 330, 630, 678, 680, 682: Duct 332, 332', 632a, 632b: Molding equipment 334, 634a, 634b: stacking mechanism (folding mechanism) 345, 645: Entanglement mechanism 336, 636, 644, 648, 652, 658: Conveyor 350:Laminated web 352: Entangled Web 370: Entanglement pack 375: Compression mechanism 390, 590: Accumulator 525, 527, 529, 531, 533, 535, 537, 594, 595, 596, 597, 827, 829, 831, 833: Dry binder added 398, 598: Diversion mechanism 550, 650: Hardening furnace 610: Method for forming a pack from a fibrous material 640: Trimming mechanism 646: Binder applicator 654: Cutting mechanism 656: Chopping mechanism 660: Packaging mechanism 900: Binder 902: Air Trumpet 910: Rotating drum 1000: Insulation products 1002: Thick low density core (low density layer) 1004: Thin high-density tensile layer (outer layer) 1050: Layered vat or pack 1052: Low density hierarchy 1054: Dense hierarchy 1210: Heat oven 1215: Inner oven liner 1216: Oven cavity 1233: Outer oven cabinet 1236: Air gap 1238:Insulating materials 1502:Mold half part 1510: Compression molded fiberglass parts 1522: Binderless or dry binder fiberglass pack 1602: Vacuum mold components 1610: Vacuum formed fiberglass parts
Claims
1. 1. A continuous process for forming a pack of glass fibers, comprising: Melting the glass; treating the molten glass to form glass fibers; stacking the glass fibers and allowing the glass fibers to cool; forming a binderless web from the cooled glass fibers; and b. mechanically entangling said fibers of said web to form said glass fiber pack.
2. 2. The continuous process of claim 1, wherein the fibers are entangled by needling.
3. 2. The continuous process of claim 1, wherein said fiberglass binderless web has an area weight of 0.10 to 0.38 pounds per square foot and a thickness of 0.45 to 1.375 inches.
4. 2. The continuous process of claim 1, wherein the glass fibers have a diameter range ranging from 15HT to 19HT.
5. 6. The continuous process of claim 5, wherein said glass fibers have a length ranging from about 0.25 inches to about 10.0 inches.
6. 2. The continuous process of claim 1, wherein the glass fiber pack comprises from 99% to 100% glass, or from 99% to 100% glass and an inert ingredient that does not bond the glass fibers to one another.
7. 1. A continuous process for forming a pack of glass fibers, comprising: Melting the glass; treating the molten glass to form glass fibers; forming a binderless web from a first portion of the glass fibers; mechanically entangling the fibers of the web to form a pack of glass fibers; and redirecting a second portion of the glass fibers for another use.
8. 8. A continuous process according to claim 7, characterized in that the fibers are entangled by needling.
9. 8. The continuous process of claim 7, wherein said fiberglass binderless web has an area weight of 0.10 to 0.38 pounds per square foot and a thickness of 0.45 to 1.375 inches.
10. 8. The continuous process of claim 7, wherein the glass fibers have a diameter range ranging from 15HT to 19HT.
11. 11. The continuous process of claim 10, wherein the glass fibers have a length ranging from about 0.25 inches to about 10.0 inches.
12. 8. The continuous process of claim 7, wherein the glass fiber pack comprises from 99% to 100% glass, or from 99% to 100% glass and an inert component that does not bond the glass fibers to one another.
13. A binderless web of glass fibers, comprising: glass fibers that are mechanically entangled to form said web; the web having a weight per square foot of 0.10 to 0.38 pounds per square foot; the glass fibers have a diameter range of 15HT to 19HT; A binderless web of fiberglass, wherein the glass fibers have a length ranging from about 0.25 inches to about 10.0 inches.
14. 14. The binderless web of fiberglass of claim 13, comprising 99% to 100% glass, or 99% to 100% glass and an inert ingredient that does not bond the glass fibers to one another.
15. 14. The binderless fiberglass web of claim 13, wherein the glass fibers used to form it are not compressed in any way for packaging or shipping.
16. 14. The binderless fiberglass web of claim 13, wherein the glass fibers are mechanically entangled by needling.
17. 1. A continuous process for forming a pack of glass fibers, comprising: Melting the glass; treating the molten glass to form glass fibers; stacking the glass fibers and allowing the glass fibers to cool; forming a binderless web of said glass fibers; and b. laying up said binderless webs of glass fibers to form said pack.
18. 18. A continuous process according to claim 17, characterized in that the fibers are entangled by needling.
19. 20. The continuous process of claim 17, wherein said fiberglass binderless web has an area weight of 0.10 to 0.38 pounds per square foot and a thickness of 0.45 to 1.375 inches.
20. 20. The continuous process of claim 17, wherein the glass fibers have a diameter range ranging from 15HT to 19HT.
21. 21. The continuous process of claim 20, wherein the glass fibers have a length range of from about 0.25 inches to about 10.0 inches.
22. 20. The continuous process of claim 17, wherein the glass fiber pack comprises from 99% to 100% glass, or from 99% to 100% glass and an inert ingredient that does not bond the glass fibers to one another.
23. 1. A laminated binderless web of glass fibers, comprising: a first web of glass fibers; at least one additional web of glass fibers deposited on said first web of glass fibers; the first web having a weight per square foot of 0.05 to 0.2 pounds per square foot; the glass fibers have a diameter range ranging from 15HT to 19HT; 1. A laminated binderless web of fiberglass, wherein said glass fibers have a length range of from about 0.25 inches to about 10.0 inches.
24. 24. The binderless fiberglass web of claim 23, wherein the pack of glass fibers comprises from 99% to 100% glass, or from 99% to 100% glass and an inert ingredient that does not bond the glass fibers to one another.
25. 24. The binderless fiberglass web of claim 23, wherein the glass fibers used to form it are not compressed in any way for packaging or shipping.
26. 24. The binderless fiberglass web of claim 23, wherein the glass fibers are mechanically entangled by needling.
27. A binderless web of glass fibers, comprising: glass fibers that are mechanically entangled to form said web; the web having an area weight of about 5 to about 50 grams per square foot; the glass fibers have a diameter range ranging from about 9HT to about 35HT; the glass fibers have a length range of from about 0.25 inches to about 10.0 inches; 1. A binderless fiberglass web, comprising from 99% to 100% glass, or from 99% to 100% glass and an inert ingredient that does not bond the glass fibers to one another.
28. 1. A laminated binderless web of glass fibers, comprising: a first web of glass fibers; at least one additional web of glass fibers deposited on said first web of glass fibers; the first web having a weight per square foot of about 5 to about 50 grams per square foot; the glass fibers have a diameter range ranging from about 9HT to about 35HT; the glass fibers have a length range of from about 0.25 inches to about 10.0 inches; 1. A laminated binderless web of fiberglass, characterized in that the laminated web of fiberglass comprises from 99% to 100% glass, or from 99% to 100% glass and an inert ingredient that does not bond the glass fibers to one another.
Citation Information
Patent Citations
High silica glass fiber punched felt
CN2633912Y
Glass fiber mat
JP1977124977A
Fibrous heat insulating material and its production
JP1993286786A
Method of producing core material for vacuum heat insulation material
JP2003293256A
Insulation panel based on mineral fibers, its method of manufacture and use