Li2o-al2o3-sio2-based crystallized glass
Optimized Li2O-Al2O3-SiO2 glass composition reduces TiO2 to minimize yellow tint and uses ZrO2 for enhanced nucleation, achieving transparent and mechanically strong glass with reduced thermal expansion and no toxic fining agents.
Patent Information
- Application Number
- JP2024138507
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-03-22
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-03-18
AI Technical Summary
Existing Li2O-Al2O3-SiO2 crystallized glass used in applications such as front windows for stoves and optical lenses suffers from yellowish tint due to TiO2 content, leading to undesirable coloration and reduced transparency, while traditional fining agents like As2O3 and Sb2O3 are toxic and environmentally harmful.
The glass composition is optimized by reducing TiO2 content and incorporating ZrO2 to enhance crystal nucleation, with specific ratios of components to maintain transparency and suppress yellow coloration, using non-toxic alternatives for fining agents.
The resulting glass achieves a colorless and transparent appearance with high ultraviolet transparency, reduced thermal expansion, and improved mechanical strength, while eliminating environmental hazards from toxic fining agents.
Smart Images

Figure 2024164110000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to Li2O-Al2O3-SiO2 crystallized glass. In particular, the present invention relates to Li2O-Al2O3-SiO2 crystallized glass suitable for use as a material for, for example, front windows of oil stoves, wood stoves, etc., substrates for high-tech products such as color filters and substrates for image sensors, setters for firing electronic components, light diffusion plates, furnace tubes for semiconductor manufacturing, masks for semiconductor manufacturing, optical lenses, members for dimensional measurement, members for communication, members for construction, containers for chemical reactions, top plates for electromagnetic cooking, heat-resistant tableware, heat-resistant covers, window glass for fire doors, members for astronomical telescopes, members for space optics, etc. [Background technology]
[0002] Li2O-Al2O3-SiO2 crystallized glass has been used as a material for front windows of oil stoves, wood stoves, etc., substrates for high-tech products such as color filters and substrates for image sensors, setters for firing electronic components, light diffusion plates, furnace tubes for semiconductor manufacturing, masks for semiconductor manufacturing, optical lenses, members for dimensional measurement, members for communication, building members, containers for chemical reactions, top plates for electromagnetic cooking, heat-resistant tableware, heat-resistant covers, window glass for fire doors, members for astronomical telescopes, members for space optics, etc. For example, Patent Documents 1 to 3 disclose Li2O-Al2O3-SiO2 crystallized glass obtained by precipitating Li2O-Al2O3-SiO2 crystals such as β-quartz solid solution (Li2O·Al2O3·nSiO2 [2≦n≦4]) and β-spodumene solid solution (Li2O·Al2O3·nSiO2 [n≧4]) as the main crystals.
[0003] Li2O-Al2O3-SiO2 crystallized glass has excellent thermal properties due to its low thermal expansion coefficient and high mechanical strength. In addition, by adjusting the heat treatment conditions in the crystallization process, it is possible to control the type of precipitated crystals, and transparent crystallized glass (β-quartz solid solution precipitated) can be easily produced.
[0004] However, when producing this type of crystallized glass, it is necessary to melt it at a high temperature exceeding 1400°C. For this reason, As2O3 and Sb2O3 are used as fining agents added to the glass batch, which can generate a large amount of fining gas when melted at high temperatures. However, As2O3 and Sb2O3 are highly toxic and may pollute the environment during the glass manufacturing process or waste glass treatment.
[0005] In view of this, SnO2 and Cl have been proposed as alternative fining agents to As2O3 and SB2O3 (see, for example, Patent Documents 4 and 5). However, Cl is likely to corrode dies and metal rolls during glass molding, and as a result, there is a risk of deteriorating the surface quality of the glass. [Prior art documents] [Patent documents]
[0006] Patent Document 1: Japanese Patent Publication No. 39-21049 Patent Document 2: Japanese Patent Publication No. 40-20182 Patent Document 3: Japanese Patent Application Laid-open No. 1-308845 Patent document 4: Japanese Patent Application Laid-Open No. 11-228180 Patent document 5: Japanese Patent Application Laid-Open No. 11-228181 Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, Li2O-Al2O3-SiO2 crystallized glass has a problem in that it is colored due to TiO2, Fe2O3, etc., has a yellowish tinge, and is not desirable in appearance.
[0008] An object of the present invention is to provide a Li2O-Al2O3-SiO2 based crystallized glass in which yellow coloring due to TiO2, Fe2O3, etc. is suppressed. [Means for solving the problem]
[0009] To improve the yellow coloring of transparent crystallized glass, it is sufficient to reduce the TiO2 content, but if the TiO2 content is reduced, the optimal firing temperature range in the crystallization process becomes narrower, and the amount of crystal nuclei generated tends to decrease. As a result, the amount of coarse crystals increases, the crystallized glass becomes cloudy, and transparency is easily impaired. However, it has been found that the lack of crystal nuclei generated due to the reduction of the TiO2 content can be compensated for by adding a large amount of ZrO2, such as 1 mass% or more.
[0010] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention is characterized by containing, by mass%, 40-90% SiO2, 5-30% Al2O3, 1-10% Li2O, 0-20% SnO2, 1-20% ZrO2, 0-10% MgO, 50-10% P2O, and less than 0-2% TiO2.
[0011] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably further contains, by mass%, 0-10% Na2O, 0-10% K2O, 0-10% CaO, 0-10% SrO, 0-10% BaO, 0-10% ZnO, and 0-10% B2O3.
[0012] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably further contains, by mass %, 0.1% or less of Fe2O3.
[0013] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a mass ratio of SnO2 / (SnO2+ZrO2+P2O5+TiO2+B2O3) of 0.06 or more. Here, "SnO2 / (SnO2+ZrO2+P2O5+TiO2+B2O3)" is the value obtained by dividing the content of SnO2 by the total amount of SnO2, ZrO2, P2O5, TiO2, and B2O3.
[0014] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a mass ratio of Al2O3 / (SnO2+ZrO2) of 7.1 or less, where "Al2O3 / (SnO2+ZrO2)" is the value obtained by dividing the content of Al2O3 by the combined amount of SnO2 and ZrO2.
[0015] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a mass ratio of SnO2 / (SnO2+ZrO2) of 0.01 to 0.99, where "SnO2 / (SnO2+ZrO2)" is the value obtained by dividing the content of SnO2 by the combined amount of SnO2 and ZrO2.
[0016] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably contains, by mass%, 8% or less of Na2O+K2O+CaO+SrO+BaO, where "Na2O+K2O+CaO+SrO+BaO" refers to the total amount of Na2O, K2O, CaO, SrO, and BaO.
[0017] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a mass ratio of (SiO2+Al2O3) / Li2O of at least 20. Here, "(SiO2+Al2O3) / Li2O" is the value obtained by dividing the total amount of SiO2 and Al2O3 by the content of Li2O.
[0018] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a mass ratio of (SiO2+Al2O3) / SnO2 of at least 44. Here, "(SiO2+Al2O3) / SnO2" is the value obtained by dividing the total amount of SiO2 and Al2O3 by the content of SnO2.
[0019] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a mass ratio of (MgO+ZnO) / Li2O of less than 0.395 or more than 0.754. Here, "MgO+ZnO) / Li2O" is the value obtained by dividing the total amount of MgO and ZnO by the content of Li2O.
[0020] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a mass ratio of (Li2O+Na2O+K2O) / ZrO2 of 2.0 or less, where "(Li2O+Na2O+K2O) / ZrO2" is the value obtained by dividing the total amount of Li2O, Na2O, and K2O by the content of ZrO2.
[0021] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a mass ratio of TiO2 / ZrO2 of 0.0001 to 5.0, where "TiO2 / ZrO2" is the value obtained by dividing the TiO2 content by the ZrO2 content.
[0022] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a mass ratio of TiO2 / TiO2+Fe2O3 of 0.001 to 0.999, where "TiO2 / (TiO2+Fe2O3)" is the value obtained by dividing the TiO2 content by the TiO2 and Fe2O3 contents.
[0023] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably contains, by mass%, less than 0.05% of HfO2+Ta2O5, where "HfO2+Ta2O5" refers to the total amount of HfO2 and Ta2O5.
[0024] The Li2O-Al2O3-SiO2 based crystallized glass of the present invention preferably contains, by mass %, 7 ppm or less of Pt.
[0025] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably contains, by mass %, 7 ppm or less of Rh.
[0026] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably contains, by mass %, 9 ppm or less of Pt+Rh, where "Pt+Rh" refers to the total amount of Pt and Rh.
[0027] The Li2O-Al2O3-SiO2 crystallized glass of the present invention preferably has a colorless and transparent appearance.
[0028] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a thickness of 3 mm and a transmittance of 10% or more at a wavelength of 300 nm, making it suitable for use in a variety of applications requiring ultraviolet transmittance.
[0029] In the Li2O-Al2O3-SiO2 crystallized glass of the present invention, it is preferable that β-quartz solid solution is precipitated as the main crystal, which makes it easy to obtain crystallized glass with a low thermal expansion coefficient.
[0030] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a thermal expansion coefficient of 30×10 -7 / ° C. or less. In this way, the composition can be suitably used in various applications requiring low expansion properties.
[0031] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a thermal expansion coefficient of 30×10 -7 / ° C. or less. This allows the composition to be suitably used in various applications requiring low expansion properties over a wide temperature range.
[0032] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a thickness of 3 mm, a transmittance of 10% or more at a wavelength of 300 nm, and a thermal expansion coefficient of 30×10 -7 / °C or less.
[0033] In the Li2O-Al2O3-SiO2-based crystallized glass of the present invention, the change in transmittance before and after crystallization at a thickness of 3 mm and a wavelength of 300 nm is preferably 50% or less. Here, "change in transmittance before and after crystallization" means {(transmittance before crystallization (%) - transmittance after crystallization (%)) / transmittance before crystallization (%)} x 100 (%). Effect of the Invention
[0034] According to the present invention, it is possible to provide Li2O-Al2O3-SiO2-based crystallized glass in which yellow coloring due to TiO2, Fe2O3, etc. is suppressed. [Brief description of the drawings]
[0035] [Figure 1] 1 is a transmittance curve of sample No. 29 before crystallization. [Diagram 2] 1 is a transmittance curve of sample No. 29 after crystallization. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] The Li2O-Al2O3-SiO2 crystallized glass of the present invention contains, in mass%, 40-90% SiO2, 5-30% Al2O3, 1-10% Li2O, 0-20% SnO2, 1-20% ZrO2, 0-10% MgO, 50-10% P2O, and less than 0-2% TiO2. The reasons for limiting the glass composition as above are as follows. In the following explanation of the content of each component, "%" means "mass%" unless otherwise specified.
[0037] SiO2 is a component that forms the skeleton of glass and also constitutes Li2O-Al2O3-SiO2 crystals. The content of SiO2 is preferably 40-90%, 52-80%, 55-75%, 56-70%, 59-70%, 60-70%, 60-69.5%, 60.5-69.5%, 61-69.5%, 61.5-69.5%, 62-69.5%, 62.5-69.5%, 63-69.5%, and particularly 63.5-69.5%. If the content of SiO2 is too low, the thermal expansion coefficient tends to be high, making it difficult to obtain crystallized glass with excellent thermal shock resistance. In addition, chemical durability tends to decrease. On the other hand, if the content of SiO2 is too high, the meltability of glass decreases, the viscosity of the glass melt increases, making it difficult to clarify or mold the glass, and productivity tends to decrease. In addition, the time required for crystallization becomes longer, which tends to reduce productivity.
[0038] Al2O3 is a component that forms the skeleton of glass and constitutes Li2O-Al2O3-SiO2 crystals. In addition, Al2O3 is a component that coordinates around the crystal nucleus and forms a core-shell structure. The presence of the core-shell structure makes it difficult for crystal nucleus components to be supplied from outside the shell, making it difficult for the crystal nucleus to enlarge, and facilitating the formation of a large number of fine crystal nuclei. The content of Al2O3 is preferably 5 to 30%, 8 to 30%, 9 to 28%, 10 to 27%, 12 to 27%, 14 to 7%, 16 to 27%, 17 to 27%, 18 to 27%, 18 to 26.5%, 18.1 to 26.5%, 19 to 26.5%, 19.5 to 26.5%, 20 to 26.5%, 20.5 to 26.5%, and particularly 20.8 to 25.8%. If the content of Al2O3 is too low, the thermal expansion coefficient tends to be high, making it difficult to obtain crystallized glass with excellent thermal shock resistance. Also, chemical durability tends to decrease. Furthermore, the crystal nuclei become large, and the crystallized glass tends to become cloudy. On the other hand, if the content of Al2O3 is too high, the meltability of the glass decreases, the viscosity of the glass melt increases, making it difficult to clarify and mold the glass, and productivity tends to decrease. Also, mullite crystals tend to precipitate, causing the glass to devitrify, and the crystallized glass tends to break.
[0039] Li2O is a component that constitutes Li2O-Al2O3-SiO2 crystals, and has a large effect on crystallinity, and also reduces the viscosity of glass, improving the meltability and formability of glass. The content of Li2O is preferably 1-10%, 2-10%, 2-8%, 2.5-6%, 2.8-5.5%, 2.8-5%, 3-5%, 3-4.5%, 3-4.2%, and particularly 3.2-4%. If the content of Li2O is too low, mullite crystals tend to precipitate and the glass tends to devitrify. In addition, when crystallizing glass, Li2O-Al2O3-SiO2 crystals are difficult to precipitate, making it difficult to obtain crystallized glass with excellent thermal shock resistance. Furthermore, the meltability of glass decreases, the viscosity of the glass melt increases, making it difficult to clarify the glass, and making it difficult to mold the glass, which tends to reduce productivity. On the other hand, if the Li2O content is too high, the crystallinity becomes too strong, the glass tends to become easily devitrified, and the crystallized glass becomes easily broken.
[0040] SiO2, Al2O3, and Li2O are the main components of the β-quartz solid solution, which is the main crystal, and Li2O and Al2O3 compensate for each other's charges to form a solid solution in the SiO2 skeleton. By containing these three components in an appropriate ratio, crystallization proceeds efficiently, making it possible to manufacture at low cost. It is preferable that (SiO2+Al2O3) / Li2O is 20 or more, 20.2 or more, 20.4 or more, 20.6 or more, 20.8 or more, and especially 21 or more.
[0041] SnO2 acts as a clarifier. It is also a necessary component for efficient crystal precipitation during the crystallization process. On the other hand, if it is contained in a large amount, it significantly intensifies the coloring of glass. The SnO2 content is 0-20%, over 0-20%, 0.05-20%, 0.1-10%, 0.1-5%, 0.1-4%, 0.1-3%, 0.15-3%, 0.2-3%, 0.2-2.7%, 0.2-2.4%, 0.25-2.4%, 0.3-2.4%, 0.35-2.4%, 0.4-2.4%, 0.45-2.4%, 0.5-2.4%, 0. It is preferable that the content of SnO2 is 5 to 2.35%, 0.5 to 2.3%, 0.5 to 2.2%, 0.5 to 2.1%, 0.5 to 2.05%, 0.5 to 2%, 0.5 to 1.95%, 0.5 to 1.93%, 0.5 to 1.91%, 0.5 to 1.9%, 0.5 to 1.88%, 0.5 to 1.85%, 0.5 to 1.83%, 0.5 to 1.81%, and particularly 0.5 to 1.8%. If the content of SnO2 is too low, it becomes difficult to clarify the glass, and the productivity is likely to decrease. In addition, crystal nuclei are not sufficiently formed, and coarse crystals are precipitated, which may cause the glass to become cloudy or break. On the other hand, if the content of SnO2 is too high, the coloring of the crystallized glass may become strong. In addition, the amount of SnO2 evaporated during production increases, which tends to increase the environmental load.
[0042] ZrO2 is a nucleation component for precipitating crystals during the crystallization process. The ZrO2 content is 1-20%, 1-15%, 1-10%, 1-5%, 1.5-5%, 1.75-4.5%, 1.75-4.4%, 1.75-4.3%, 1.75-4.2%, 1.75-4.1%, 1.75-4%, 1.8-4%, 1.85-4%, 1.9-4%, 1.95-4%, 2-4%, 2.05-4%, It is preferable that the content of ZrO2 is 2.1 to 4%, 2.15 to 4%, 2.2 to 4%, 2.25 to 4%, 2.3 to 4%, 2.3 to 3.95%, 2.3 to 3.9%, 2.3 to 3.95%, 2.3 to 3.9%, 2.3 to 3.85%, 2.3 to 3.8%, more than 2.7 to 3.8%, 2.8 to 3.8%, 2.9 to 3.8%, and particularly 3 to 3.8%. If the content of ZrO2 is too low, crystal nuclei are not sufficiently formed, and coarse crystals are precipitated, which may cause the crystallized glass to become cloudy or break. On the other hand, if the content of ZrO2 is too high, coarse ZrO2 crystals are precipitated, which makes the glass more likely to devitrify and the crystallized glass more likely to break.
[0043] SnO2+ZrO2 is preferably 1-30%, 1.1-30%, 1.1-27%, 1.1-24%, 1.1-21%, 1.1-20%, 1.1-17%, 1.1-14%, 1.1-11%, 1.1-9%, 1.1-7.5%, 1.4-7.5%, 1.8-7.5%, 2.0-7.5%, 2.2-7%, 2.2-6.4%, 2.2-6.2%, 2.2-6%, 2.3-6%, 2.4-6%, 2.5-6%, and particularly 2.8-6%. If SnO2+ZrO2 is too small, crystal nuclei are difficult to precipitate and crystallization is difficult. On the other hand, if SnO2+ZrO2 is too large, the crystal nuclei become large and the crystallized glass becomes easily cloudy.
[0044] SnO2 has the effect of promoting phase separation of ZrO2. In order to efficiently cause phase separation while keeping the liquidus temperature low (while reducing the risk of devitrification due to initial phase precipitation) and to rapidly perform nucleation and crystal growth in the subsequent steps, the mass ratio of SnO2 / (SnO2+ZrO2) is preferably 0.01 to 0.99, 0.01 to 0.98, 0.01 to 0.94, 0.01 to 0.90, 0.01 to 0.86, 0.01 to 0.82, 0.01 to 0.78, 0.01 to 0.74, 0.01 to 0.70, 0.03 to 0.70, and particularly preferably 0.05 to 0.70.
[0045] In addition, SnO2 reacts with SnO2 → SnO + 1 / 2O2 at high temperatures, releasing O2 gas into the molten glass. This reaction is known as the fining mechanism of SnO2, and the O2 gas released during the reaction enlarges the tiny bubbles present in the molten glass and releases them outside the glass system, and also has a "stirring effect" of mixing the molten glass. In the Li2O-Al2O3-SiO2-based crystallized glass of the present invention, the content of SiO2 and Al2O3 accounts for the majority, and since these components are difficult to dissolve, it is necessary to contain these three components in a suitable ratio in order to efficiently form a homogeneous molten glass. (SiO2 + Al2O3) / SnO2 is 44 or more, 44.3 or more, 44.7 or more, 45 or more, or 45.2 or more. It is preferable that it is 45.4 or more, 45.6 or more, 45.8 or more, and especially 46 or more.
[0046] Al2O3 / (SnO2+ZrO2) is preferably 7.1 or less, 7.05 or less, 7.0 or less, 6.95 or less, 66.9 or less, 6.85 or less, 6.8 or less, 6.75 or less, 6.7 or less, 6.65 or less, 6.6 or less, 6.55 or less, 6.5 or less, 6.45 or less, 6.4 or less, 6.35 or less, 6.3 or less, 6.25 or less, 6.15 or less, 6.1 or less, 6.05 or less, 6.0 or less, 5.98 or less, 5.95 or less, 5.92 or less, 5.9 or less, 5.8 or less, 5.7 or less, 5.6 or less, and particularly preferably 5.5 or less. If Al2O3 / (SnO2+ZrO2) is too large, nucleation does not proceed efficiently, making it difficult to crystallize efficiently. This tendency is more likely to occur when TiO2 is less than 0.2%. On the other hand, if Al2O3 / (SnO2+ZrO2) is too small, the crystal nuclei become large and the crystallized glass becomes cloudy. Therefore, the lower limit of Al2O3 / (SnO2+ZrO2) is preferably 0.01 or more.
[0047] MgO is a component that dissolves in Li2O-Al2O3-SiO2 crystals and increases the thermal expansion coefficient of the Li2O-Al2O3-SiO2 crystals. The content of MgO is preferably 0-10%, 0-8%, 0-6%, 0-5%, 0-4.5%, 0-4%, 0-3.5%, 0.02-3.5%, 0.05-3.5%, 0.08-3.5%, 0.1-3.5%, 0.1-3.3%, 0.1-3%, 0.13-3%, 0.15-3%, 0.17-3%, 0.19-3%, 0.2-2.9%, 0.2-2.7%, 0.2-2.5%, 0.2-2.3%, 0.2-2.2%, 0.2-2.1%, and particularly preferably 0.2-2%. If the content of MgO is too low, the thermal expansion coefficient tends to be too low. Also, volumetric shrinkage occurs during crystal precipitation, but the amount of volumetric shrinkage may be too large. Also, the difference in thermal expansion coefficient between the crystal phase after crystallization and the remaining glass phase becomes large, so the crystallized glass may be easily broken. If the content of MgO is too high, the crystallinity becomes too strong, making it prone to devitrification and the crystallized glass to be easily broken. Also, the thermal expansion coefficient tends to be too high.
[0048] P2O5 is a component that suppresses the precipitation of coarse ZrO2 crystals. The content of P2O5 is preferably 0 to 10%, 0 to 8%, 0 to 6%, 0 to 5%, 0 to 4%, 0 to 3.5%, 0.02 to 3.5%, 0.05 to 3.5%, 0.08 to 3.5%, 0.1 to 3.5%, 0.1 to 3.3%, 0.1 to 3%, 0.13 to 3%, 0.15 to 3%, 0.17 to 3%, 0.19 to 3%, 0.2 to 2.9%, 0.2 to 2.7%, 0.2 to 2.5%, 0.2 to 2.3%, 0.2 to 2.2%, 0.2 to 2.1%, 0.2 to 2%, and particularly preferably 0.3 to 1.8%. If the P2O5 content is too low, coarse ZrO2 crystals will precipitate, causing the glass to devitrify and the crystallized glass to break easily.On the other hand, if the P2O5 content is too high, the amount of Li2O-Al2O3-SiO2 crystals precipitated will decrease, and the thermal expansion coefficient will tend to increase.
[0049] TiO2 is a nucleation component for precipitating crystals during the crystallization process. On the other hand, when it is contained in a large amount, it significantly intensifies the coloring of glass. In particular, zirconia titanate crystals containing ZrO2 and TiO2 act as crystal nuclei, but electrons transfer from the valence band of the ligand oxygen to the conduction band of the central metal zirconia and titanium (LMCT transition), which contributes to the coloring of the crystallized glass. In addition, if titanium remains in the remaining glass phase, an LMCT transition can occur from the valence band of the SiO2 skeleton to the conduction band of the tetravalent titanium in the remaining glass phase. In addition, a dd transition occurs in the trivalent titanium in the remaining glass phase, which contributes to the coloring of the crystallized glass. Furthermore, when titanium and iron coexist, an ilmenite (FeTiO3)-like coloring appears. It is also known that when titanium and tin coexist, the yellow color is intensified. Therefore, the TiO2 content is 0~4%, 0~3.5%, 0~3%, 0~2.5%, 0~2.2%, 0~2.1%, 0~2%, 0~1.95%, 0~1.9%, 0~1.8%, 0~1.7%, 0~1.6%, 0~1.5%, 0~1.4%, 0~1.3%, 0~1.2%, 0~1.1%, 0~1.05%, 0~1%, 0~0.95%, 0~0.9%, 0~0.85%, 0~0.8%, 0~0.75%, 0~0.7%, 0~0.65%. %, 0-0.6%, 0-0.55%, 0-0.5%, 0-0.48%, 0-0.46%, 0-0.44%, 0-0.42%, 0-0.4%, 0-0.38%, 0-0.36%, 0-0.34%, 0-0.32%, 0-0.3%, 0-0.28%, 0-0.26%, 0-0.24%, 0-0.22%, 0-0.2%, 0-0.18%, 0-0.16%, 0-0.14%, 0-0.12%, and especially 0-0.1%. However, since TiO2 is easily mixed in as an impurity, if TiO2 is to be completely removed, the raw material batch becomes expensive and the manufacturing cost tends to increase. In order to suppress an increase in manufacturing costs, the lower limit of the TiO2 content is preferably 0.0003% or more, 0.0005% or more, 0.001% or more, 0.005% or more, 0.01% or more, particularly preferably 0.02% or more.
[0050] TiO2 and ZrO2 are components that can function as crystal nuclei. Ti and Zr are homologous elements, and have similar electronegativity and ionic radius. For this reason, they tend to have similar molecular conformations as oxides, and it is known that in the coexistence of TiO2 and ZrO2, phase separation is likely to occur in the early stages of crystallization. For this reason, within the range in which coloring is permitted, TiO2 / ZrO2 is preferably 0.0001 to 5.0, 0.0001 to 4.0, 0.0001 to 3.0, 0.0001 to 2.5, 0.0001 to 2.0, 0.0001 to 1.5, 0.0001 to 1.0, 0.0001 to 0.5, 0.0001 to 0.4, and particularly 0.0001 to 0.3. If TiO2 / ZrO2 is too small, the raw material batch becomes expensive and the manufacturing cost tends to increase. On the other hand, if TiO2 / ZrO2 is too large, the crystal nucleation rate will be slow, which may increase the production cost.
[0051] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention may contain the following components in addition to the above components in the glass composition.
[0052] Na2O is a component that can be dissolved in Li2O-Al2O3-SiO2 crystals, and has a large effect on crystallinity, and also reduces the viscosity of glass to improve the melting and moldability of glass. It is also a component for adjusting the thermal expansion coefficient and refractive index of crystallized glass. The content of Na2O is preferably 0-10%, 0-8%, 0-6%, 0-5%, 0-4.5%, 0-4%, 0-3.5%, 0-3%, 0-2.7%, 0-2.4%, 0-2.1%, 0-1.8%, and particularly 0-1.5%. If the content of Na2O is too high, the crystallinity becomes too strong, the glass becomes easily devitrified, and the crystallized glass becomes easily broken. In addition, the ionic radius of Na cations is larger than that of Li cations and Mg cations, which are the main crystal constituents, and is therefore difficult to be incorporated into the crystals, so that Na cations after crystallization tend to remain in the remaining glass (glass matrix). Therefore, if the content of Na2O is too high, the refractive index difference between the crystal phase and the remaining glass is likely to occur, and the crystallized glass tends to be cloudy. However, since Na2O is easily mixed in as an impurity, if Na2O is to be completely removed, the raw material batch becomes expensive and the manufacturing cost tends to increase. In order to suppress the increase in manufacturing cost, the lower limit of the content of Na2O is preferably 0.0003% or more, 0.0005% or more, and particularly 0.001% or more.
[0053] K2O is a component that can be dissolved in Li2O-Al2O3-SiO2 crystals, and has a large effect on crystallinity, and also reduces the viscosity of glass to improve the melting and moldability of glass. It is also a component for adjusting the thermal expansion coefficient and refractive index of crystallized glass. The content of K2O is 0-10%, 0-8%, 0-6%, 0-5%, 0-4.5%, 0-4%, 0-3.5%, 0-3%, 0-2.7%, 0-2.4%, 0-2.1%, 0-1.8%, 0-1.5%, 0-1.4%, 0-1.3%, 0-1.2%. It is preferably 0-1.1%, 0-1%, 0-0.9%, and particularly preferably 0.1-0.8%. If the content of K2O is too high, the crystallinity becomes too strong, the glass becomes easily devitrified, and the crystallized glass becomes easily broken. In addition, the ionic radius of K cation is larger than that of Li cation and Mg cation, which are the main crystal constituents, and is difficult to be incorporated into the crystal, so that K cation after crystallization is likely to remain in the remaining glass. Therefore, if the content of K2O is too high, the refractive index difference between the crystal phase and the remaining glass is likely to occur, and the crystallized glass tends to become cloudy. However, since K2O is easily mixed in as an impurity, if K2O is to be completely removed, the raw material batch becomes expensive and the manufacturing cost tends to increase. In order to suppress the increase in manufacturing cost, the lower limit of the content of K2O is preferably 0.0003% or more, 0.0005% or more, and particularly 0.001% or more.
[0054] Li2O, Na2O, and K2O are components that improve the melting and moldability of glass, but if the content of these components is too high, the low-temperature viscosity will drop too much, and the glass may flow too much during crystallization. Li2O, Na2O, and K2O are also components that can deteriorate the weather resistance, water resistance, chemical resistance, etc. of glass before crystallization. If the glass before crystallization is deteriorated by moisture, etc., the desired crystallization behavior and therefore the desired properties may not be obtained. On the other hand, ZrO2 is a component that functions as a nucleating agent, and has the effect of crystallizing preferentially at the beginning of crystallization and suppressing the flow of the remaining glass. In addition, ZrO2 efficiently fills the voids in the glass network, which is mainly composed of SiO2 skeleton, and has the effect of inhibiting the diffusion of protons and various chemical components in the glass network, improving the weather resistance, water resistance, chemical resistance, etc. of glass before crystallization. In order to obtain crystallized glass with the desired shape and properties, (Li2O+Na2O+K2O) / ZrO2 should be appropriately controlled. It is preferable that (Li2O+Na2O+K2O) / ZrO2 be 2.0 or less, 1.98 or less, 1.96 or less, 1.94 or less, 1.92 or less, and particularly preferably 1.90 or less.
[0055] CaO is a component that reduces the viscosity of glass and improves the melting and moldability of glass. It is also a component for adjusting the thermal expansion coefficient and refractive index of crystallized glass. The content of CaO is preferably 0-10%, 0-8%, 0-6%, 0-5%, 0-4.5%, 0-4%, 0-3.5%, 0-3%, 0-2.7%, 0-2.4%, 0-2.1%, 0-1.8%, and particularly 0-1.5%. If the content of CaO is too high, the glass is easily devitrified and the crystallized glass is easily broken. In addition, the ionic radius of Ca cations is larger than that of Li cations and Mg cations, which are the main crystal constituents, and is difficult to be incorporated into the crystal, so that Ca cations after crystallization are likely to remain in the remaining glass. For this reason, if the content of CaO is too high, a refractive index difference between the crystal phase and the remaining glass is easily generated, and the crystallized glass tends to become cloudy. However, since CaO is easily mixed in as an impurity, if one tries to completely remove CaO, the raw material batch becomes expensive and the manufacturing cost tends to increase. In order to suppress the increase in manufacturing cost, the lower limit of the CaO content is preferably 0.0001% or more, 0.0003% or more, and particularly 0.0005% or more.
[0056] SrO is a component that reduces the viscosity of glass and improves the melting and moldability of glass. It is also a component for adjusting the thermal expansion coefficient and refractive index of crystallized glass. The content of SrO is preferably 0-10%, 0-8%, 0-6%, 0-5%, 0-4.5%, 0-4%, 0-3.5%, 0-3%, 0-2.7%, 0-2.4%, 0-2.1%, 0-1.8%, 0-1.5%, and particularly 0-1%. If the content of SrO is too high, the glass is easily devitrified and the crystallized glass is easily broken. In addition, the ionic radius of Sr cation is larger than that of Li cation and Mg cation, which are the main crystal constituents, and is difficult to be incorporated into the crystal, so that Sr cation after crystallization is likely to remain in the remaining glass. For this reason, if the content of SrO is too high, a refractive index difference between the crystal phase and the remaining glass is easily generated, and the crystallized glass tends to become cloudy. However, since SrO is easily mixed in as an impurity, if one tries to completely remove SrO, the raw material batch becomes expensive and the manufacturing cost tends to increase. In order to suppress the increase in manufacturing cost, the lower limit of the SrO content is preferably 0.0001% or more, 0.0003% or more, and particularly preferably 0.0005% or more.
[0057] BaO is a component that reduces the viscosity of glass and improves the melting and moldability of glass. It is also a component for adjusting the thermal expansion coefficient and refractive index of crystallized glass. The content of BaO is preferably 0-10%, 0-8%, 0-6%, 0-5%, 0-4.5%, 0-4%, 0-3.5%, 0-3%, 0-2.7%, 0-2.4%, 0-2.1%, 0-1.8%, 0-1.5%, and particularly 0-1%. If the content of BaO is too high, crystals containing Ba are precipitated, the glass is easily devitrified, and the crystallized glass is easily broken. In addition, the ionic radius of Ba cations is larger than that of Li cations and Mg cations, which are the main crystal constituents, and Ba cations are not easily incorporated into the crystals, so that Ba cations after crystallization tend to remain in the remaining glass. For this reason, if the content of BaO is too high, a refractive index difference between the crystal phase and the remaining glass is easily generated, and the crystallized glass tends to become cloudy. However, since BaO is easily mixed in as an impurity, if BaO is to be completely removed, the raw material batch becomes expensive and the manufacturing cost tends to increase. In order to suppress the increase in manufacturing cost, the lower limit of the BaO content is preferably 0.0001% or more, 0.0003% or more, and particularly preferably 0.0005% or more.
[0058] MgO, CaO, SrO, and BaO are components that improve the meltability and moldability of glass, but if the content of these components is too high, the low-temperature viscosity will drop too much, and the glass may flow too much during crystallization. On the other hand, ZrO2 is a component that functions as a nucleating agent, and has the effect of crystallizing preferentially at the beginning of crystallization and suppressing the flow of the remaining glass. In order to obtain crystallized glass with the desired shape and characteristics, (MgO+CaO+SrO+BaO) / ZrO2 should be appropriately controlled. (MgO+CaO+SrO+BaO) / ZrO2 is preferably 0 to 3, 0 to 2.8, 0 to 2.6, 0 to 2.4, 0 to 2.2, 0 to 2.1, 0 to 2, 0 to 1.8, 0 to 1.7, 0 to 1.6, and particularly 0 to 1.5. Na2O, K2O, CaO, SrO, and BaO tend to remain in the remaining glass after crystallization. Therefore, if the total amount of these is too large, the refractive index difference between the crystal phase and the remaining glass is likely to occur, and the crystallized glass is likely to become cloudy. Therefore, Na2O+K2O+CaO+SrO+BaO is preferably 8% or less, 7% or less, 6% or less, 5% or less, 4.5% or less, 4% or less, 3.5% or less, 3% or less, 2.7% or less, 2.42% or less, 2.415% or less, 2.410% or less, 2.405% or less, and particularly 2.4% or less.
[0059] Li2O, Na2O, K2O, MgO, CaO, SrO, and BaO are components that improve the meltability and formability of glass. In addition, glass melts containing a large amount of MgO, CaO, SrO, and BaO tend to have a gradual change in viscosity (viscosity curve) relative to temperature, while glass melts containing a large amount of Li2O, Na2O, and K2O tend to have a rapid change. If the change in the viscosity curve is too gradual, the glass will continue to flow even after being molded into a desired shape, making it difficult to obtain the desired shape. On the other hand, if the change in the viscosity curve is too rapid, the glass melt will solidify during molding, making it difficult to obtain the desired shape. For this reason, (MgO+CaO+SrO+BaO) / (Li2O+Na2O+K2O) should be appropriately controlled. (MgO+CaO+SrO+BaO) / (Li2O+Na2O+K2O) is preferably 0 to 2, 0 to 1.8, 0 to 1.5, 0 to 1.2, 0 to 1, 0 to 0.9, 0 to 0.8, 0 to 0.7, 0 to 0.6, 0 to 0.5, and particularly preferably 0 to 0.45.
[0060] ZnO is a component that dissolves in Li2O-Al2O3-SiO2 crystals and has a large effect on crystallinity. It is also a component for adjusting the thermal expansion coefficient and refractive index of the crystallized glass. The content of ZnO is preferably 0-10%, 0-8%, 0-6%, 0-5%, 0-4.5%, 0-4%, 0-3.5%, 0-3%, 0-2.7%, 0-2.4%, 0-2.1%, 0-1.8%, 0-1.5%, and particularly preferably 0-1%. If the content of ZnO is too high, the crystallinity becomes too strong, which makes the glass prone to devitrification and breakage. However, since ZnO is easily mixed in as an impurity, if ZnO is to be completely removed, the raw material batch becomes expensive and the manufacturing cost tends to increase. In order to suppress the increase in manufacturing cost, the lower limit of the content of ZnO is preferably 0.0001% or more, 0.0003% or more, and particularly preferably 0.0005% or more.
[0061] In Li2O-Al2O3-SiO2 crystallized glass, Li cations, Mg cations, and Zn cations are components that are easily dissolved in β-quartz solid solutions, and compared with Ba cations, they are considered to be components that contribute less to the increase in the refractive index of the remaining glass after crystallization. In addition, Li2O, MgO, and ZnO function as fluxes when vitrifying raw materials, so they can be said to be important components in producing colorless and transparent crystallized glass at low temperatures. Li2O is an essential component for achieving low expansion, and must be contained at 1% or more. In order to achieve the desired thermal expansion coefficient, etc., the necessary amount of Li2O must be contained, but if the contents of MgO and ZnO are also increased accordingly, the viscosity of the glass may decrease too much. If the low-temperature viscosity decreases too much, the softening fluidity of the glass during firing may become too large, making it difficult to crystallize into the desired shape. In addition, if the high-temperature viscosity decreases too much, the thermal load on the manufacturing equipment decreases, but the convection speed during heating increases, and there is a risk that refractories and the like may be easily physically eroded. Therefore, it is preferable to control the content ratio of Li2O, MgO, and ZnO, and in particular, it is preferable to control the total amount of MgO and ZnO relative to Li2O, which has a high function as a flux. Therefore, it is preferable to make the mass ratio of (MgO+ZnO) / Li2O small, such as 0.394 or less, 0.393 or less, 0.392 or less, 0.391 or less, and especially 0.390 or less, or to make it large, such as 0.755 or more, 0.756 or more, 0.757 or more, 0.758 or more, and especially 0.759 or more.
[0062] B2O3 is a component that reduces the viscosity of glass and improves the meltability and moldability of glass. It is also a component that may be involved in the ease of phase separation during crystal nucleation. The content of B2O3 is preferably 0-10%, 0-8%, 0-6%, 0-5%, 0-4.5%, 0-4%, 0-3.5%, 0-3%, 0-2.7%, 0-2.4%, 0-2.1%, 0-1.8%, and particularly 0-1.5%. If the content of B2O3 is too high, the amount of B2O3 evaporated during melting increases, which increases the environmental load. However, since B2O3 is easily mixed in as an impurity, if B2O3 is to be completely removed, the raw material batch becomes expensive and the manufacturing cost tends to increase. In order to suppress the increase in manufacturing cost, B2O3 may be contained in an amount of 0.0001% or more, 0.0003% or more, and particularly 0.0005% or more.
[0063] It is known that in Li2O-Al2O3-SiO2 crystallized glass, a phase separation region is formed in the glass before the formation of crystal nuclei, and then crystal nuclei composed of TiO2, ZrO2, etc. are formed in the phase separation region. Since SnO2, ZrO2, P2O5, TiO2, and B2O3 are strongly involved in the phase separation formation, the ratios of SnO2+ZrO2+P2O5+TiO2+B2O3 are 1.5-30%, 1.5-26%, 1.5-22%, 1.5-20%, 1.5-18%, 1.5-16%, 1.5-15%, 1.8-15%, 2.1-15%, 2.4-15%, 2.5-15%, 2.8-15%, 2.8-13%, 2.8-12%, 2.8-1 ... 10%, 3 to 9.5%, 3 to 9.2%, particularly 3 to 9%, are preferred, and SnO2 / (SnO2+ZrO2+P2O5+TiO2+B2O3) is preferably 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, 0.1 or more, 0.103 or more, 0.106 or more, 0.11 or more, 0.112 or more, 0.115 or more, 0.118 or more, 0.121 or more, 0.124 or more, 0.127 or more, 0.128 or more, particularly 0.13 or more. If P2O5+B2O3+SnO2+TiO2+ZrO2 is too small, it becomes difficult to form a phase separation region and crystallize. On the other hand, if P2O5+B2O3+SnO2+TiO2+ZrO2 is too much and / or SnO2 / (SnO2+ZrO2+P2O5+TiO2+B2O3) is too small, the phase separation region becomes large and the crystallized glass becomes easily cloudy. The upper limit of SnO2 / (SnO2+ZrO2+P2O5+TiO2+B2O3) is not particularly limited, but is practically 0.9 or less.
[0064] Fe2O3 is a component that enhances the coloring of glass, especially a component that significantly enhances coloring by interacting with TiO2 and SnO2. The content of Fe2O3 is preferably 0.10% or less, 0.08% or less, 0.06% or less, 0.05% or less, 0.04% or less, 0.035% or less, 0.03% or less, 0.02% or less, 0.015% or less, 0.013% or less, 0.012% or less, 0.011% or less, 0.01% or less, 0.009% or less, 0.008% or less, 0.007% or less, 0.006% or less, 0.005% or less, 0.004% or less, 0.003% or less, and especially 0.002% or less. However, since Fe2O3 is easily mixed in as an impurity, if Fe2O3 is to be completely removed, the raw material batch becomes expensive and the manufacturing cost tends to increase. In order to suppress an increase in production costs, the lower limit of the Fe2O3 content is preferably 0.0001% or more, 0.0002% or more, 0.0003% or more, 0.0005% or more, and particularly preferably 0.001% or more.
[0065] When titanium and iron coexist, ilmenite (FeTiO3)-like coloring may occur. In particular, in Li2O-Al2O3-SiO2 crystallized glass, titanium and iron components that do not precipitate as crystal nuclei or main crystals after crystallization remain in the remaining glass, and the occurrence of the above coloring may be promoted. In terms of design, it is possible to reduce the amount of these components, but since TiO2 and Fe2O3 are easily mixed in as impurities, if they are to be completely removed, the raw material batch becomes expensive and the manufacturing cost tends to increase. Therefore, in order to suppress the manufacturing cost, TiO2 and Fe2O3 may be contained within the above-mentioned range, and in order to make the manufacturing cost cheaper, both components may be contained within the range in which coloring is allowed. In such a case, TiO2 / (TiO2+Fe2O3) is preferably 0.001 to 0.999, 0.003 to 0.997, 0.005 to 0.995, 0.007 to 0.993, 0.009 to 0.991, 0.01 to 0.99, 0.1 to 0.9, 0.15 to 0.85, 0.2 to 0.8, 0.25 to 0.25, 0.3 to 0.7, 0.35 to 0.65, and particularly preferably 0.4 to 0.6. This makes it easier to obtain colorless and highly transparent crystallized glass at low cost.
[0066] Pt is a component that can be mixed into glass in the form of ions, colloids, metals, etc., and causes a yellow to brown coloration. This tendency becomes more pronounced after crystallization. Furthermore, after careful investigation, it was found that the inclusion of Pt may affect the nucleation and crystallization behavior of the crystallized glass, making it more likely to become cloudy. For this reason, the Pt content is preferably 7 ppm or less, 6 ppm or less, 5 ppm or less, 4 ppm or less, 3 ppm or less, 2 ppm or less, 1.6 ppm or less, 1.4 ppm or less, 1.2 ppm or less, 1 ppm or less, 0.9 ppm or less, 0.8 ppm or less, 0.7 ppm or less, 0.6 ppm or less, 0.5 ppm or less, 0.45 ppm or less, 0.40 ppm or less, 0.35 ppm or less, and particularly 0.30 ppm or less. Although the inclusion of Pt should be avoided as much as possible, when using general melting equipment, it may be necessary to use Pt members to obtain homogeneous glass. For this reason, if Pt is completely removed, the manufacturing cost tends to increase. In the case where coloring is not adversely affected, in order to suppress an increase in manufacturing cost, the lower limit of the Pt content is preferably 0.0001 ppm or more, 0.001 ppm or more, 0.005 ppm or more, 0.01 ppm or more, 0.02 ppm or more, 0.03 ppm or more, 0.04 ppm or more, 0.05 ppm or more, 0.06 ppm or more, and particularly 0.07 ppm or more. In addition, in the case where coloring is permitted, Pt may be used as a nucleation agent that promotes the precipitation of main crystals, similar to ZrO2 and TiO2. In that case, Pt may be used as a nucleation agent alone, or may be used as a nucleation agent in combination with other components. In addition, when Pt is used as a nucleation agent, the form is not particularly important (colloid, metal crystal, etc.).
[0067] Rh is a component that can be mixed into glass in the form of ions, colloids, metals, etc., and tends to cause yellow to brown coloring and make crystallized glass opaque, similar to Pt. Therefore, the content of Rh is preferably 7 ppm or less, 6 ppm or less, 5 ppm or less, 4 ppm or less, 3 ppm or less, 2 ppm or less, 1.6 ppm or less, 1.4 ppm or less, 1.2 ppm or less, 1 ppm or less, 0.9 ppm or less, 0.8 ppm or less, 0.7 ppm or less, 0.6 ppm or less, 0.5 ppm or less, 0.45 ppm or less, 0.40 ppm or less, 0.35 ppm or less, and particularly 0.30 ppm or less. Although the mixing of Rh should be avoided as much as possible, when using general melting equipment, it may be necessary to use Rh components to obtain homogeneous glass. Therefore, if Rh is to be completely removed, the manufacturing cost tends to increase. In the case where coloring is not adversely affected, in order to suppress an increase in manufacturing costs, the lower limit of the Rh content is preferably 0.0001 ppm or more, 0.001 ppm or more, 0.005 ppm or more, 0.01 ppm or more, 0.02 ppm or more, 0.03 ppm or more, 0.04 ppm or more, 0.05 ppm or more, 0.06 ppm or more, and particularly 0.07 ppm or more. In addition, in the case where coloring is permitted, Rh may be used as a nucleating agent similar to ZrO2 or TiO2. In that case, Rh may be used alone as a nucleating agent, or may be used as a nucleating agent in combination with other components. In addition, when Rh is used as a nucleating agent to promote the precipitation of main crystals, the form is not particularly important (colloid, metal crystal, etc.).
[0068] In addition, Pt+Rh is 9ppm or less, 8ppm or less, 7ppm or less, 6ppm or less, 5ppm or less, 4.75ppm or less, 4.5ppm or less, 4.25ppm or less, 4ppm or less, 3.75ppm or less, 3.5ppm or less, 3.25ppm or less, 3ppm or less, 2.75ppm or less, 2.5ppm or less, 2.25ppm or less, 2ppm or less, 1.75ppm or less, 1.5ppm It is preferable that the concentration is 1.25 ppm or less, 1 ppm or less, 0.95 ppm or less, 0.9 ppm or less, 0.85 ppm or less, 0.8 ppm or less, 0.75 ppm or less, 0.7 ppm or less, 0.65 ppm or less, 0.60 ppm or less, 0.55 ppm or less, 0.50 ppm or less, 0.45 ppm or less, 0.40 ppm or less, 0.35 ppm or less, and particularly 0.30 ppm or less. Although the inclusion of Pt and Rh should be avoided as much as possible, when using general melting equipment, it may be necessary to use Pt and Rh components to obtain homogeneous glass. Therefore, if Pt and Rh are to be completely removed, the manufacturing cost tends to increase. In the case where there is no adverse effect on coloration, in order to suppress an increase in production costs, the lower limit of Pt+Rh is preferably 0.0001 ppm or more, 0.001 ppm or more, 0.005 ppm or more, 0.01 ppm or more, 0.02 ppm or more, 0.03 ppm or more, 0.04 ppm or more, 0.05 ppm or more, 0.06 ppm or more, and particularly preferably 0.07 ppm or more.
[0069] In developing glass materials, it is common to use various crucibles to produce glasses of various compositions. For this reason, platinum and rhodium that have evaporated from the crucible are often present inside the electric furnace used for melting. It has been confirmed that Pt and Rh present inside the electric furnace are mixed into the glass. In order to control the amount of Pt and Rh mixed in, it is possible to control the Pt and Rh content in the glass by selecting the raw materials and crucible materials used, attaching a quartz lid to the crucible, lowering the melting temperature, shortening the melting time, etc.
[0070] As2O3 and SB2O3 are highly toxic and may pollute the environment during the glass manufacturing process, waste glass processing, etc. For this reason, it is preferable that the Li2O-Al2O3-SiO2-based crystallized glass of the present invention does not substantially contain these components (specifically, less than 0.1 mass %).
[0071] The Li2O-Al2O3-SiO2 crystallized glass of the present invention may contain, in addition to the above components, trace components such as H2, CO2, CO, H2O, He, Ne, Ar, and N2 up to 0.1% each, as long as they do not adversely affect coloring. In addition, if Ag, Au, Pd, Ir, V, Cr, Sc, Ce, Pr, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Ac, Th, Pa, U, etc. are intentionally added to the glass, the raw material cost tends to increase and the manufacturing cost tends to increase. On the other hand, when glass containing Ag, Au, etc. is irradiated with light or heat treated, aggregates of these components are formed, and crystallization can be promoted from these aggregates. In addition, Pd, etc. have various catalytic effects, and by containing them, it is possible to impart unique functions to glass or crystallized glass. In consideration of these circumstances, when the purpose is to promote crystallization or to impart other functions, the above components may be contained in an amount of 1% or less, 0.5% or less, 0.3% or less, or 0.1% or less, respectively, and if not, the amount is preferably 500 ppm or less, 300 ppm or less, 100 ppm or less, and particularly preferably 10 ppm or less.
[0072] Furthermore, as long as there is no adverse effect on coloration, the Li2O-Al2O3-SiO2-based crystallized glass of the present invention may contain up to 10% in total of SO3, MnO, Cl2, Y2O3, MoO3, La2O3, WO3, HfO2, Ta2O5, Nd2O3, Nb2O5, RfO2, etc. However, since the raw material batches of the above components are expensive and tend to increase the manufacturing cost, they do not have to be added unless there are special circumstances. In particular, since HfO2 has a high raw material cost and Ta2O5 can be a conflict mineral, it is preferable that the total amount of these components be, by mass, 5% or less, 4% or less, 3% or less, 2% or less, 1% or less, 0.5% or less, 0.4% or less, 0.3% or less, 0.2% or less, 0.1% or less, 0.05% or less, less than 0.05%, 0.049% or less, 0.048% or less, 0.047% or less, 0.046% or less, and especially 0.045% or less.
[0073] That is, the preferred composition ranges for implementing the Li2O-Al2O3-SiO2-based crystallized glass of the present invention are 50-75% SiO2, 10-30% Al2O3, 1-8% Li2O, 0-5% SnO2, 1-5% ZrO2, 0-10% MgO, 50-5% P2O, 0-less than 2% TiO2, (Li2O+Na2O+K2O) / ZrO2 0-1.5, TiO2 / (TiO2+Fe2O3) 0.01-0.99, (MgO+ZnO) / Li2O 0-0.8, and more preferably 50-75% SiO2, 10-30% Al2O3, 1-8% Li2O, over 0-5% SnO2, 1-5% ZrO2, and 0-10% MgO. 0-10%, P2O50-5%, TiO20-less than 2%, (Li2O+Na2O+K2O) / ZrO20-1.5, TiO2 / (TiO2+Fe2O3) 0.01-0.99, (MgO+ZnO) / Li2O 0-0.8, (MgO+CaO+SrO+BaO) / (Li2O+Na2O+K2O) 0-0.5, and more preferably SiO250-75%, Al2O310-30%, Li2O 1-8%, SnO20-5%, ZrO21-5%, MgO 0-10%, P2O50-5%, TiO20-less than 2%, (Li2O+Na2O+K2O) / ZrO20-1.5, TiO2 / (TiO2+Fe2O3) 0.01-0.99, (MgO+ZnO) / Li2O 0-0.8, (MgO+CaO+SrO+BaO) / (Li2O+Na2O+K2O) 0-0.5, (MgO+CaO+SrO+BaO) / ZrO2 0-2, and more preferably SiO2 50-75%, Al2O3 10-30%, Li2O 1-8%, SnO2 more than 5%, ZrO2 1-5%, MgO 0-10%, P2O 50-5%, TiO2 0-less than 2%, (Li2O+Na2O+K2O) / ZrO2 0-1.5, TiO2 / (TiO2+Fe2O3) 0.01-0.99, (MgO+ZnO) / Li2O 0~0.8, (MgO+CaO+SrO+BaO) / (Li2O+Na2O+K2O) 0~0.5, (MgO+CaO+SrO+BaO) / ZrO20~2, SnO2 / (SnO2+ZrO2+P2O5+TiO2+B2O3) 0.06~0.9, and more preferably, SiO2 50-75%, Al2O3 10-30%, Li2O 1-8%, SnO20-5%, ZrO2 1-5%, MgO 0-10%, P2O 50-5%, TiO2 0-less than 2%, (Li2O+Na2O+K2O) / ZrO2 0-1.5, TiO2 / (TiO2+Fe2O3) 0.01-0.99, (MgO+ZnO) / Li2O 0-0.8, (MgO+CaO+SrO+BaO) / (Li2O+Na2O+K2O) 0-0.5, (MgO+CaO+SrO+BaO) / ZrO2 0-2, SnO2 / (SnO2+ZrO2+P2O5+TiO2+B2O3) 0.06-0.9, Pt+Rh 0-5ppm, and more preferably, SiO2 50-75%, Al2O3 10-30%, Li2O 1-8%, SnO2 over 0-5%, ZrO2 1-5%, MgO 0-10%, P2O 50-5%, TiO2 0-less than 2%, (Li2O+Na2O+K2O) / ZrO2 0-1.5, TiO2 / (TiO2+Fe2O3) 0.01-0.99, (MgO+ZnO) / Li2O 0-0.394, (MgO+CaO+SrO+BaO) / (Li2O+Na2O+K2O) 0-0.5, (MgO+CaO+SrO+BaO) / ZrO20-2, SnO2 / (SnO2+ZrO2+P2O5+TiO2+B2O3) 0.06-0.9, Pt+Rh 0-5 ppm, and particularly preferred are SiO2 50-75%, Al2O3 10-30%, Li2O 1-8%, SnO20-5%, ZrO2 1-5%, MgO 0-10%, P2O 50-5%, TiO20-less than 2%, (Li2O+Na2O+K2O) / ZrO20-1.5, TiO2 / (TiO2+Fe2O3) 0.01-0.99, (MgO+ZnO) / Li2O 0~0.394, (MgO+CaO+SrO+BaO) / (Li2O+Na2O+K2O) 0~0.5, (MgO+CaO+SrO+BaO) / ZrO2 0~2, SnO2 / (SnO2+ZrO2+P2O5+TiO2+B2O3) 0.06~0.9, Pt+Rh 0~5ppm, HfO2+Ta2O5 0~less than 0.05%.
[0074] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention having the above composition tends to have a colorless and transparent appearance.
[0075] The Li2O-Al2O3-SiO2 crystallized glass of the present invention has a thickness of 3 mm and a transmittance at a wavelength of 200 nm of 0% or more, 2.5% or more, 5% or more, 10% or more, 12% or more, 14% or more, 16% or more, 18% or more, 20% or more, 22% or more, 24% or more, 26% or more, 28% or more, 30% or more, 32% or more, 34% or more, 36% or more, 38% or more, 40% or more, 40.5% or more, 41% or more, 41.5% or more, 42% or more, 42.5% or more, 43% or more, 43.5% or more, 44% or more, 44.5% or more, and particularly 45% or more. In the case of an application that requires transmission of ultraviolet light, if the transmittance at a wavelength of 200 nm is too low, there is a risk that the desired transmittance cannot be obtained. In particular, when used for optical cleaning using an ozone lamp or the like, or for medical or exposure applications using an excimer laser, a high transmittance at a wavelength of 200 nm is preferred.
[0076] The Li2O-Al2O3-SiO2 crystallized glass of the present invention has a thickness of 3 mm and a transmittance at a wavelength of 250 nm of 0% or more, 1% or more, 2% or more, 3% or more, 4% or more, 5% or more, 6% or more, 7% or more, 8% or more, 9% or more, 10% or more, 10.5% or more, 11% or more, 11.5% or more, 12% or more, 12.5% or more, 13% or more, 13.5% or more, 14% or more, 14.5% or more, 15% or more, 15.5% or more, and particularly preferably 16% or more. In the case of applications that require the transmission of ultraviolet light, if the transmittance at a wavelength of 250 nm is too low, there is a risk that the desired transmittance cannot be obtained. In particular, when used for sterilization applications using low-pressure mercury lamps or processing applications using YAG lasers, etc., it is preferable that the transmittance at a wavelength of 250 nm is high.
[0077] The Li2O-Al2O3-SiO2 crystallized glass of the present invention has a thickness of 3 mm and a transmittance at a wavelength of 300 nm of 0% or more, 2.5% or more, 5% or more, 10% or more, 12% or more, 14% or more, 16% or more, 18% or more, 20% or more, 22% or more, 24% or more, 26% or more, 28% or more, 30% or more, 32% or more, 34% or more, 36% or more, 38% or more, 40% or more, 40.5% or more, 41% or more, 41.5% or more, 42% or more, 42.5% or more, 43% or more, 43.5% or more, 44% or more, 44.5% or more, and particularly 45% or more. In particular, when used for UV curing, adhesion, drying (UV curing), fluorescent detection of printed matter, insect attraction applications, etc., the higher the transmittance at a wavelength of 300 nm, the more preferable.
[0078] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a thickness of 3 mm and a transmittance at a wavelength of 325 nm of preferably 0% or more, 2.5% or more, 5% or more, 10% or more, 12% or more, 14% or more, 16% or more, 18% or more, 20% or more, 22% or more, 24% or more, 26% or more, 28% or more, 30% or more, 32% or more, 34% or more, 36% or more, 38% or more, 40% or more, 42% or more, 44% or more, 46% or more, 48% or more, 50% or more, 52% or more, 54% or more, 56% or more, 57% or more, 58% or more, 59% or more, 60% or more, 61% or more, 62% or more, 63% or more, 64% or more, and particularly preferably 65% or more. In particular, when used for UV curing, adhesion, drying (UV curing), fluorescent detection of printed matter, and insect attraction applications, a high transmittance at a wavelength of 325 nm is preferable.
[0079] The Li2O-Al2O3-SiO2 crystallized glass of the present invention has a thickness of 3 mm and a transmittance at a wavelength of 350 nm of 0% or more, 5% or more, 10% or more, 15% or more, 20% or more, 25% or more, 30% or more, 35% or more, 40% or more, 45% or more, 50% or more, 55% or more, 60% or more, 65% or more, 70% or more, 71% or more, 72% or more, 73% or more, 74% or more, 75% or more, 76% or more, 77% or more, 78% or more, 80% or more, 81% or more, 82% or more, 83% or more, and particularly 84% or more. In particular, when used in processing using YAG laser or the like, the transmittance at a wavelength of 350 nm is preferably high.
[0080] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a thickness of 3 mm and a transmittance at a wavelength of 380 nm of preferably 50% or more, 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 78% or more, 80% or more, 81% or more, 82% or more, 83% or more, and particularly preferably 84% or more. If the transmittance at a wavelength of 380 nm is too low, the yellow coloring becomes strong and the transparency of the crystallized glass decreases, which may make it impossible to obtain the desired transmittance.
[0081] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a thickness of 3 mm and a transmittance at a wavelength of 800 nm of preferably 50% or more, 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 78% or more, 80% or more, 81% or more, 82% or more, 83% or more, 84% or more, 85% or more, 86% or more, 87% or more, and particularly preferably 88% or more. If the transmittance at a wavelength of 800 nm is too low, it tends to turn green. In particular, when used for medical purposes such as vein authentication, the transmittance at a wavelength of 800 nm is preferably high.
[0082] The Li2O-Al2O3-SiO2 crystallized glass of the present invention has a thickness of 3 mm and a transmittance at a wavelength of 1200 nm of 50% or more, 55% or more, 60% or more, 65% or more, 70% or more, 72% or more, 74% or more, 76% or more, 78% or more, 80% or more, 81% or more, 82% or more, 83% or more, 84% or more, 85% or more, 86% or more, 87% or more, 88% or more, and particularly 89% or more. If the transmittance at a wavelength of 1200 nm is too low, it tends to become green. In particular, when used for infrared communication applications such as infrared cameras and remote controls, the transmittance at a wavelength of 1200 nm is preferably high.
[0083] The Li2O-Al2O3-SiO2 crystallized glass of the present invention has a transmittance change rate before and after crystallization at a thickness of 3 mm and a wavelength of 300 nm of 50% or less, 48% or less, 46% or less, 44% or less, 42% or less, 40% or less, 38% or less, 37.5% or less, 37% or less, 36.5% or less, 36% or less, 35.5% or less, and particularly 35% or less. If the transmittance change rate before and after crystallization is small, it becomes possible to predict and control the transmittance after crystallization before crystallization, and it becomes easier to obtain the desired transmittance after crystallization. It is preferable that the transmittance change rate before and after crystallization is small not only at a wavelength of 300 nm but also in the entire wavelength range.
[0084] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a lightness L * is preferably 50 or more, 60 or more, 65 or more, 70% or more, 75 or more, 80 or more, 85 or more, 90 or more, 91 or more, 92 or more, 93 or more, 94 or more, 95 or more, 96 or more, 96.1 or more, 96.3 or more, and particularly preferably 96.5 or more. * If is too small, the color tends to look grayish and dark regardless of the chromaticity.
[0085] The Li2O-Al2O3-SiO2 crystallized glass of the present invention has a chromaticity of *is preferably within ±5.0, ±4.5, ±4, ±3.6, ±3.2, ±2.8, ±2.4, ±2, ±1.8, ±1.6, ±1.4, ±1.2, ±1, ±0.9, ±0.8, ±0.7, ±0.6, and particularly preferably within ±0.5. * If it is too negative, it tends to look green, and if it is too positive, it tends to look red.
[0086] The Li2O-Al2O3-SiO2 crystallized glass of the present invention has a chromaticity of b * is preferably within ±5.0, ±4.5, ±4, ±3.6, ±3.2, ±2.8, ±2.4, ±2, ±1.8, ±1.6, ±1.4, ±1.2, ±1, ±0.9, ±0.8, ±0.7, ±0.6, and particularly preferably within ±0.5. * If it is too negative, it tends to look blue, and if it is too positive, it tends to look yellow.
[0087] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a strain point (temperature at which the viscosity of the glass corresponds to approximately 1014.5 dPa s) in a glass state before crystallization of 600° C. or higher, 605° C. or higher, 610° C. or higher, 615° C. or higher, 620° C. or higher, 630° C. or higher, 635° C. or higher, 640° C. or higher, 645° C. or higher, 650° C. or higher, and particularly preferably 655° C. or higher. If the strain point temperature is too low, the glass before crystallization is likely to break when molded.
[0088] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention, in a glass state before crystallization, preferably has an annealing point (the temperature at which the viscosity of the glass corresponds to approximately 1013 dPa s) of 680° C. or higher, 685° C. or higher, 690° C. or higher, 695° C. or higher, 700° C. or higher, 705° C. or higher, 710° C. or higher, 715° C. or higher, 720° C. or higher, and particularly preferably 725° C. or higher. If the annealing point temperature is too low, the glass before crystallization is likely to break when molded.
[0089] The Li2O-Al2O3-SiO2 crystallized glass of the present invention is easily crystallized by heat treatment, so it is not easy to measure the softening point temperature (the temperature at which the viscosity of the glass is about 107.6 dPa·s) as with common glasses such as soda-lime glass. Therefore, in the Li2O-Al2O3-SiO2 crystallized glass of the present invention, the temperature at which the slope of the thermal expansion curve of the glass before crystallization changes is taken as the glass transition temperature and is treated as a substitute for the softening point. The Li2O-Al2O3-SiO2 crystallized glass of the present invention preferably has a glass transition temperature of 680°C or higher, 685°C or higher, 690°C or higher, 695°C or higher, 700°C or higher, 705°C or higher, 710°C or higher, 715°C or higher, 720°C or higher, and particularly 725°C or higher in the glass state before crystallization. If the glass transition temperature is too low, the glass will flow too much during crystallization, making it difficult to mold it into a desired shape.
[0090] The liquidus temperature of the Li2O-Al2O3-SiO2 crystallized glass of the present invention is preferably 1540°C or less, 1535°C or less, 1530°C or less, 1525°C or less, 1520°C or less, 1515°C or less, 1510°C or less, 1505°C or less, 1500°C or less, 1495°C or less, 1490°C or less, 1485°C or less, 1480°C or less, 1475°C or less, 1470°C or less, 1465°C or less, 1460°C or less, 1455°C or less, 1450°C or less, 1445°C or less, 1440°C or less, 1435°C or less, 1430°C or less, 1425°C or less, 1420°C or less, 1415°C or less, and particularly 1410°C or less. If the liquidus temperature is too high, devitrification is likely to occur during production. On the other hand, if the temperature is 1480°C or lower, it is easy to manufacture using the roll method, etc., if the temperature is 1450°C or lower, it is easy to manufacture using the casting method, etc., and if the temperature is 1410°C or lower, it is easy to manufacture using the fusion method, etc.
[0091] The Li2O-Al2O3-SiO2 crystallized glass of the present invention has a liquidus viscosity (logarithm of viscosity corresponding to liquidus temperature) of 2.70 or more, 2.75 or more, 2.80 or more, 2.85 or more, 2.90 or more, 2.95 or more, 3.00 or more, 3.05 or more, 3.10 or more, 3.15 or more, 3.20 or more, 3.25 or more, 3.30 or more, 3.35 or more, 3.40 or more, 3.45 or more, 3.50 or more, 3.55 or more, 3.60 or more, 3.65 or more, and particularly 3.70 or more. If the liquidus viscosity is too low, it is likely to devitrify during production. On the other hand, if it is 3.40 or more, it becomes easy to produce it by the roll method, etc., if it is 3.50 or more, it becomes easy to produce it by the casting method, etc., and if it is 3.70 or more, it becomes easy to produce it by the fusion method, etc.
[0092] The Li2O-Al2O3-SiO2 crystallized glass of the present invention preferably has β-quartz solid solution precipitated as the main crystal. If β-quartz solid solution is precipitated as the main crystal, the crystal grain size is easily small, so that the crystallized glass is easily transparent to visible light and the transparency is easily increased. In addition, it is easy to make the thermal expansion coefficient of the glass close to zero. In addition, the Li2O-Al2O3-SiO2 crystallized glass of the present invention is heat-treated at a higher temperature than the crystallization conditions for precipitating β-quartz solid solution, so that β-spodumene solid solution is precipitated. The crystal grain size of β-spodumene solid solution is easily larger than that of β-quartz solid solution, and generally tends to become cloudy when made into crystallized glass, but by suitably adjusting the glass composition and firing conditions, the refractive index difference between the crystal phase containing β-spodumene solid solution and the remaining glass phase may be reduced, and in this case, the crystallized glass is less likely to become cloudy. The Li2O-Al2O3-SiO2-based crystallized glass of the present invention may contain crystals such as β-spodumene solid solution, so long as they do not adversely affect coloring or the like.
[0093] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a thermal expansion coefficient of 30×10 -7 / ℃ or less, 25×10 -7 / ℃ or less, 20×10 -7 / ℃ or less, 18×10 -7 / ℃ or less, 16×10-7 / ℃ or less, 14×10 -7 / ℃ or less, 13×10 -7 / ℃ or less, 12×10 -7 / ℃ or less, 11×10 -7 / ℃ or less, 10×10 -7 / ℃ or less, 9×10 -7 / ℃ or less, 8×10 -7 / ℃ or less, 7×10 -7 / ℃ or less, 6×10 -7 / ℃ or less, 5×10 -7 / ℃ or less, 4×10 -7 / ℃ or less, 3×10 -7 / ℃ or less, especially 2×10 -7 / °C or less. When dimensional stability and / or thermal shock resistance are particularly required, it is preferable that the temperature is -5×10 -7 / ℃~5×10 -7 / ℃, -3×10 -7 / ℃~3×10 -7 / ℃, -2.5×10 -7 / ℃~2.5×10 -7 / ℃, -2×10 -7 / ℃~2×10 -7 / ℃, -1.5×10 -7 / ℃~1.5×10 -7 / ℃, -1×10 -7 / ℃~1×10 -7 / ℃, especially -0.5×10 -7 / ℃~0.5×10 -7 / °C.
[0094] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a thermal expansion coefficient of 30×10 -7 / ℃ or less, 25×10 -7 / ℃ or less, 20×10 -7 / ℃ or less, 18×10 -7 / ℃ or less, 16×10 -7 / ℃ or less, 14×10 -7 / ℃ or less, 13×10 -7 / ℃ or less, 12×10 -7 / ℃ or less, 11×10 -7 / ℃ or less, 10×10 -7 / ℃ or less, 9×10 -7 / ℃ or less, 8×10 -7 / ℃ or less, 7×10 -7 / ℃ or less, 6×10 -7 / ℃ or less, 5×10 -7 / ℃ or less, 4×10 -7 / ℃ or less, especially 3×10 -7 / °C or less. In addition, when dimensional stability and / or thermal shock resistance are particularly required, it is preferable that the temperature is -15×10 -7 / ℃~15×10 -7 / ℃, -12×10 -7 / ℃~12×10 -7 / ℃, -10×10 -7 / ℃~10×10 -7 / ℃, -8×10 -7 / ℃~8×10 -7 / ℃, -6×10 -7 / ℃~6×10 -7 / ℃, -5×10 -7 / ℃~5×10 -7 / ℃, -4.5×10 -7 / ℃~4.5×10 -7 / ℃, -4×10 -7 / ℃~4×10 -7 / ℃, -3.5×10 -7 / ℃~3.5×10 -7 / ℃, -3×10 -7 / ℃~3×10 -7 / ℃, -2.5×10 -7 / ℃~2.5×10 -7 / ℃, -2×10 -7 / ℃~2×10 -7 / ℃, -1.5×10 -7 / ℃~1.5×10 -7 / ℃, -1×10 -7 / ℃~1×10 -7 / ℃, especially -0.5×10 -7 / ℃~0.5×10 -7 / °C.
[0095] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a Young's modulus of 60 to 120 GPa, 70 to 110 GPa, 75 to 110 GPa, 75 to 105 GPa, or 80 to 105 GPa, particularly preferably 80 to 100 GPa. If the Young's modulus is too low or too high, the crystallized glass becomes easily broken.
[0096] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a modulus of rigidity of 25 to 50 GPa, 27 to 48 GPa, or 29 to 46 GPa, particularly preferably 30 to 45 GPa. If the modulus of rigidity is too low or too high, the crystallized glass becomes easily broken.
[0097] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention preferably has a Poisson's ratio of 0.35 or less, 0.32 or less, 0.3 or less, 0.28 or less, 0.26 or less, and particularly preferably 0.25 or less. If the Poisson's ratio is too large, the crystallized glass becomes easily broken.
[0098] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention has a density of 2.30 to 2.60 g / cm 3 , 2.32~2.58g / cm 3 , 2.34~2.56g / cm 3 , 2.36~2.54g / cm 3 , 2.38~2.52g / cm 3 , 2.39~2.51g / cm 3 , especially 2.40~2.50g / cm 3 If the density of the crystallizable glass is too low, the gas permeability before crystallization is deteriorated, and the glass may be contaminated during storage. On the other hand, if the density of the crystallizable glass is too high, the weight per unit area is large, and handling becomes difficult.
[0099] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention (after crystallization) has a density of 2.40 to 2.80 g / cm 3 , 2.42~2.78g / cm 3 , 2.44~2.76g / cm 3, 2.46~2.74g / cm 3 , especially 2.47 to 2.73 g / cm 3 If the density of the crystallized glass is too low, the gas permeability of the crystallized glass may deteriorate, whereas if the density of the crystallized glass is too high, the weight per unit area increases, making handling difficult.
[0100] The density change rate of the Li2O-Al2O3-SiO2-based crystallized glass of the present invention is {(density after crystallization (g / cm 3 )-Density before crystallization (g / cm 3 ) / density before crystallization (g / cm 3 )}×100(%), where the density before crystallization is the density after the glass after melting is held at 700°C for 30 minutes and cooled to room temperature at 3°C / min, and the density after crystallization is the density after crystallization treatment under a specified condition. The density change rate is preferably 0.01 to 10%, 0.05 to 8%, 0.1 to 8%, 0.3 to 8%, 0.5 to 8%, 0.9 to 8%, 1 to 7.8%, 1 to 7.4%, 1 to 7%, 1.2 to 7%, 1.6 to 7%, 2 to 7%, 2 to 6.8%, 2 to 6.5%, 2 to 6.3%, 2 to 6.2%, 2 to 6.1%, 2 to 6%, 2.5 to 5%, 2.6 to 4.5%, or 2.8 to 3.8%. If the density change rate before and after crystallization is reduced, the breakage rate after crystallization can be reduced, and scattering between the glass and the glass matrix can be reduced, making it possible to obtain crystallized glass with high transmittance. In particular, in the region where the TiO2 content is 2% or less (preferably 1% or less, 0.5% or less, and particularly 0.05% or less), scattering can be significantly reduced in reducing coloring factors other than absorption of TiO2, etc., which contributes to improving transmittance.
[0101] The Li2O-Al2O3-SiO2 crystallized glass of the present invention may be subjected to chemical strengthening or the like. The conditions of the chemical strengthening treatment may be appropriately selected by considering the glass composition, the degree of crystallization, the type of molten salt, and the like, and the treatment time and temperature. For example, a glass composition containing a large amount of Na2O that may be contained in the remaining glass may be selected so that chemical strengthening after crystallization is easy, or the degree of crystallization may be intentionally reduced. The molten salt may contain an alkali metal such as Li, Na, or K alone or in combination. Furthermore, not only the usual one-stage strengthening but also multi-stage chemical strengthening may be selected. In addition, the Li2O-Al2O3-SiO2 crystallized glass of the present invention may be treated by chemical strengthening or the like before crystallization, so that the Li2O content on the sample surface can be reduced more than that inside the sample. When such glass is crystallized, the crystallization degree of the sample surface becomes lower than that inside the sample, the thermal expansion coefficient of the sample surface becomes relatively high, and compressive stress due to the thermal expansion difference can be applied to the sample surface. Furthermore, when the crystallinity of the sample surface is low, the glass phase increases on the surface, and chemical resistance and gas barrier properties can be improved by selecting the glass composition.
[0102] Next, a method for producing the Li2O-Al2O3-SiO2 system crystallized glass of the present invention will be described.
[0103] First, a raw material batch prepared to obtain glass of the above composition is put into a glass melting furnace, melted at 1500 to 1750°C, and then molded. The glass may be melted by a flame melting method using a burner or an electric melting method using electric heating. Melting by laser irradiation or plasma is also possible. The sample shape may be a plate, fiber, film, powder, sphere, hollow, or the like, and is not particularly limited.
[0104] Next, the obtained crystallizable glass (crystallizable glass before crystallization) is heat-treated to crystallize. As for the crystallization conditions, first, nucleation is performed at 700 to 950°C (preferably 750 to 900°C) for 0.1 to 100 hours (preferably 1 to 60 hours), followed by crystal growth at 800 to 1050°C (preferably 800 to 1000°C) for 0.1 to 50 hours (preferably 0.2 to 10 hours). In this way, a transparent Li2O-Al2O3-SiO2-based crystallized glass in which β-quartz solid solution crystals are precipitated as the main crystals can be obtained. The heat treatment may be performed only at a certain temperature, or may be performed stepwise by holding at two or more levels of temperature, or may be heated while applying a temperature gradient.
[0105] Crystallization may also be promoted by applying or irradiating sound waves or electromagnetic waves. Furthermore, the cooling rate of the crystallized glass at a high temperature may be performed at a certain temperature gradient, or may be performed at two or more levels of temperature gradient. If sufficient thermal shock resistance is desired, it is desirable to control the cooling rate to sufficiently relax the structure of the remaining glass phase. The average cooling rate from 800°C to 25°C is preferably 3000°C / min, 1000°C / min or less, 500°C / min or less, 400°C / min or less, 300°C / min or less, 200°C / min or less, 100°C / min or less, 50°C / min or less, 25°C / min or less, 10°C / min or less, and particularly 5°C / min or less in the inner part of the thickness farthest from the surface of the crystallized glass. In addition, when dimensional stability over a long period of time is desired, the cooling rate is preferably 2.5°C / min or less, 1°C / min or less, 0.5°C / min or less, 0.1°C / min or less, 0.05°C / min or less, 0.01°C / min or less, 0.005°C / min or less, 0.001°C / min or less, 0.0005°C / min or less, and particularly preferably 0.0001°C / min or less. Except for the case of physical strengthening treatment by air cooling, water cooling, etc., it is desirable that the cooling rate of the crystallized glass is close to the cooling rate from the surface to the part of the inner thickness farthest from the surface. The value obtained by dividing the cooling rate of the part of the inner thickness farthest from the surface by the cooling rate of the surface is preferably 0.0001 to 1, 0.001 to 1, 0.01 to 1, 0.1 to 1, 0.5 to 1, 0.8 to 1, 0.9 to 1, and particularly preferably 1. By being close to 1, residual strain is unlikely to occur at all positions of the crystallized glass sample, and long-term dimensional stability is easily obtained. The cooling rate of the surface can be estimated using a contact thermometer or a radiation thermometer, and the internal temperature can be estimated by placing the high-temperature crystallized glass in a cooling medium and measuring the heat quantity and rate of heat change of the cooling medium, and then using this numerical data and the specific heat and thermal conductivity of the crystallized glass and the cooling medium. EXAMPLES
[0106] The present invention will be described below based on examples, but the present invention is not limited to the following examples. Tables 1 to 18 show examples of the present invention (samples Nos. 1 to 5, 8 to 63) and comparative examples (samples Nos. 6 and 7).
[0107] [Table 1]
[0108]
Table 2
[0109]
Table 3
[0110]
Table 4
[0111]
Table 5
[0112]
Table 6
[0113]
Table 7
[0114]
Table 8
[0115]
Table 9
[0116]
Table 10
[0117]
Table 11
[0118] [Table 12]
[0119] [Table 13]
[0120] [Table 14]
[0121] [Table 15]
[0122] [Table 16]
[0123] [Table 17]
[0124] [Table 18]
[0125] First, each raw material was mixed in the form of oxide, hydroxide, carbonate, nitrate, etc. to obtain a glass having the composition shown in each table, and a glass batch was obtained (the composition shown in each table is the analytical value of the glass actually produced). The obtained glass batch was placed in a crucible containing platinum and rhodium, a reinforced platinum crucible not containing rhodium, a refractory crucible, or a quartz crucible, and melted at 1600°C for 4 to 100 hours, then heated to 1650 to 1680°C and melted for 0.5 to 20 hours, rolled to a thickness of 5 mm, and further heat-treated at 700°C for 30 minutes in an annealing furnace, and the annealing furnace was cooled to room temperature at 100°C / h to obtain a crystallizable glass. The melting was performed by an electric melting method that is widely used in the development of glass materials.
[0126] It has been confirmed that the glass composition of sample No. 29 can be melted by laser irradiation when it is in contact with a liquid or solid. It has also been confirmed that the glass composition can be melted by laser irradiation when it is in contact with only the gas while the glass sample is suspended by feeding gas from around the glass sample. It has also been confirmed that the glass composition can be melted in advance in an electric furnace or the like, and then formed into a hemispherical, spherical, fibrous, powdery, or other shape by a press method, a redraw method, a spray method, or the like. It has also been confirmed that the glass compositions of sample Nos. 30 to 51 can be melted in a continuous furnace combining burner heating and electric current heating, and that the glass compositions can be formed into a block, flake, hollow, or other shape by a roll method, a film method, a lot method using dielectric heating, or the like. It has also been confirmed that the glass composition of sample No. 17 can be formed into a thin plate, tube, or bulb shape by an updraw method, a downdraw method, a slit method, an overflow (fusion) method, a hand-blowing method, or the like. Furthermore, it was confirmed that the glass composition of sample No. 61 could be used to pour a molten glass onto a liquid having a higher specific gravity than that of sample No. 61, and then solidified into a plate by cooling. Note that the glasses produced by either method could be crystallized under the conditions shown in the table.
[0127] The Pt and Rh contents of the samples were analyzed using an ICP-MS device (Agilent8800, manufactured by AGILEINT TECH NOLOGY). First, the prepared glass samples were crushed and wetted with pure water, and then perchloric acid, nitric acid, sulfuric acid, hydrofluoric acid, etc. were added to melt them. The Pt and Rh contents of the samples were then measured using an ICP-MS. The Pt and Rh contents of each measurement sample were determined based on a calibration curve prepared using a previously prepared Pt and Rh solution with known concentrations. The measurement modes were Pt:He gas / HMI (low mode) and Rh:HEHe gas / HMI (medium mode), and the mass numbers were Pt:198 and Rh:103. The Li2O content of the prepared samples was analyzed using an atomic absorption spectrometer (ContrAA600, manufactured by Analytik Jena). The flow of melting the glass samples and the use of the calibration curves were basically the same as for the Pt and Rh analysis. As for other components, they were measured by ICP-MS or atomic absorption spectrometry in the same way as Pt, Rh, and Li2O, or glass samples with known concentrations previously examined using an ICP-MS or atomic absorption spectrometry were used as calibration curve samples, and calibration curves were then created using an XRF analyzer (RIGAKU ZSX PrimusIV) and the actual content of each component was determined from the XRF analysis values of the measurement sample based on the calibration curve. During XRF analysis, the tube voltage, tube current, exposure time, etc. were adjusted as necessary depending on the components being analyzed.
[0128] The crystallized glasses shown in each table were heat-treated at 750-900°C for 0.75-60 hours to form nuclei, and then further heat-treated at 800-1000°C for 0.25-3 hours to crystallize. Then, the glasses were heat-treated at 700°C for 30 minutes, and cooled to room temperature at 100°C / h. The obtained crystallized glasses were evaluated for transmittance, diffuse transmittance, brightness, chromaticity, precipitated crystals, average crystallite size, thermal expansion coefficient, density, Young's modulus, rigidity modulus, Poisson's ratio, and appearance. The transmittance, brightness, chromaticity, etc. of the crystallized glasses before crystallization were measured in the same manner as the crystallized glasses. The viscosity and liquidus temperature of the crystallized glasses were also measured.
[0129] The transmittance, brightness and chromaticity were evaluated by measuring a crystallized glass plate with a thickness of 3 mm, both sides of which were optically polished, using a spectrophotometer. A spectrophotometer V-670 manufactured by JASCO was used for the measurement. The V-670 was equipped with an integrating sphere unit "ISN-723", and the measured transmittance corresponds to the total light transmittance. The measurement wavelength range was 200 to 1500 nm, the scan speed was 200 nm / min, the sampling pitch was 1 nm, and the bandwidth was 5 nm in the wavelength range of 200 to 800 nm and 20 nm in other wavelength ranges. Before the measurement, baseline correction (100% adjustment) and dark measurement (0% adjustment) were performed. The dark measurement was performed with the barium sulfate plate attached to the ISN-723 removed. Using the measured transmittance, tristimulus values XYZ were calculated based on JISZ8781-42013 and corresponding international standards, and lightness and chromaticity were calculated from each stimulus value (illuminant C / 10°). The diffuse transmittance of crystallized glass was measured using the same model as above, with the barium sulfate plate attached to the ISN-723 removed and the measurement sample placed on the instrument.
[0130] The precipitated crystals were evaluated using an X-ray diffractometer (Rigaku Smart Lab, fully automatic multipurpose horizontal X-ray diffractometer). The scan mode was 2θ / θ measurement, the scan type was continuous scan, the scattering and divergence slit width was 1°, the receiving slit width was 0.2°, the measurement range was 10-60°, the measurement step was 0.1°, and the scan speed was 5° / min. The main crystals and crystal grain size were evaluated using the analysis software installed in the package of the same model. As the precipitated crystal species identified as the main crystals, β-quartz solid solution is shown in the table as "β-Q". In addition, the average crystallite size of the main crystals was calculated using the measured X-ray diffraction peaks based on the Debeye-Scherrer method. In the measurement for calculating the average crystallite size, the scan speed was 1° / min.
[0131] The thermal expansion coefficient was evaluated by the average linear thermal expansion coefficient measured in the temperature ranges of 30 to 380°C and 30 to 750°C using a crystallized glass sample processed to 20mm x 3.8mmφ. A NETZSCH dilatometer was used for the measurement. In addition, the same measuring device was used to measure the thermal expansion curve in the temperature range of 30 to 750°C, and the glass transition point of the crystallized glass before crystallization was evaluated by calculating the inflection point.
[0132] The Young's modulus, rigidity modulus, and Poisson's ratio were measured at room temperature using a free resonance type elastic modulus measuring device (JE-RT3, manufactured by Nippon Technoplus) for plate samples (40 mm x 20 mm x 20 mm) whose surfaces had been polished with a polishing solution containing dispersed No. 1200 alumina powder.
[0133] The density was evaluated by the Archimedes method.
[0134] The strain point and annealing point were evaluated by the fiber elongation method. The crystallizable glass was prepared into fiber samples by hand drawing.
[0135] The high-temperature viscosity was evaluated by the platinum ball pulling method. For the evaluation, the lump glass sample was crushed to the appropriate size and placed in an alumina crucible while taking care to avoid the inclusion of air bubbles as much as possible. The alumina crucible was then heated to turn the sample into a molten liquid, and the viscosity of the glass was measured at multiple temperatures. The constants of the Vogel-Fulcher equation were calculated to create a viscosity curve, and the temperature at each viscosity was calculated.
[0136] The liquidus temperature was evaluated by the following method. First, a platinum boat of about 120 x 20 x 10 mm was filled with glass powder aligned to 300 to 500 micrometers, which was then placed in an electric furnace and melted at 1600 ° C for 30 minutes. After that, it was transferred to an electric furnace with a linear temperature gradient and placed in it for 20 hours to precipitate devitrification. After the measurement sample was air-cooled to room temperature, the devitrification precipitated at the interface between the platinum boat and the glass was observed, and the temperature at the devitrification point was calculated from the temperature gradient graph of the electric furnace to determine the liquidus temperature. In addition, the obtained liquidus temperature was inserted into the high-temperature viscosity curve of the glass, and the viscosity corresponding to the liquidus temperature was determined as the liquidus viscosity. It was found that the initial phase of the glass listed in each table was mainly ZrO2 based on the results of X-ray diffraction, composition analysis, etc. (Hitachi scanning electron microscope Hitachi S3400N TyPE2, Horiba EMAX ENERGY EX250X).
[0137] The appearance was evaluated by visually checking the color tone of the crystallized glass. Visual inspection was performed against a white background and a black background, under indoor lighting and sunlight (8:00, 12:00, and 16:00 on sunny and cloudy days in January, April, July, and October). The color tone was judged comprehensively from the results of each visual inspection.
[0138] As is clear from Tables 1 to 12, the crystallized glass of Samples No. 1 to 5 and 8 to 45, which are examples, had a colorless and transparent appearance, high transmittance, and a thermal expansion coefficient of almost 0. In addition, the rate of change in transmittance before and after crystallization was small. Furthermore, the Young's modulus was 92 to 93 GPa, the rigidity modulus was 37 to 38 GPa, and the Poisson's ratio was 0.22 to 0.23. On the other hand, the crystallized glass of Samples No. 6 and 7, which are comparative examples, had a yellow appearance, low transmittance in the short wavelength range, and a large rate of change in transmittance before and after crystallization.
[0139] Figure 1 shows the transmittance curve before crystallization of sample No. 29, and Figure 2 shows the transmittance curve after crystallization of sample No. 29. It is clear from Figures 1 and 2 that the rate of change in transmittance before and after crystallization is small.
[0140] As is clear from samples No. 31 to No. 36 in Table 10, the lower the Pt and Rh content, the higher the total light transmittance and the lower the diffuse transmittance. This suggests that the presence of Pt and Rh in the sample makes it easier for absorption to occur in a wide wavelength range after crystallization, and that Pt and Rh affect nucleation and crystal growth, causing segregation of the main crystals, an increase in the refractive index difference between the crystal phase and the remaining glass phase, and enlargement of the crystallite size or crystal particles (polycrystals formed by agglomeration of crystallites), etc., inside the crystallized glass, making it easier for light to be scattered.
[0141] As is clear from Tables 11 and 12, the Li2O-Al2O3-SiO2 crystallized glass of the present invention can obtain high transmittance even when crystallized in a short time. Therefore, since it can be crystallized at a process speed comparable to that of the conventionally used Li2O-Al2O3-SiO2 crystallized glass, it can be manufactured at low cost using existing equipment. In addition, the thermal expansion coefficient of the Li2O-Al2O3-SiO2 crystallized glass of the present invention can be adjusted by changing the crystal nucleus formation temperature, crystal growth temperature, and holding time in each temperature range.
[0142] Incidentally, when sample No. 41, which does not contain Pt or Rh, was nucleated at 825°C for 0.75 hours and crystallized at 935°C for 0.25 hours, the density change rate before and after crystallization was about 3.4%. On the other hand, when sample No. 40, which has the same composition but contains 0.01 ppm Pt and 0.03 ppm Rh, was processed under the same crystallization conditions, the density change rate before and after crystallization was about 3.7%. This shows that Pt and Rh promoted crystallization. As mentioned above, if coloring is acceptable, Pt and Rh may be used as crystallization promoters.
[0143] In addition, when the crystallized glass of sample No. 27 was immersed in molten KNO3 at 475°C for 7 hours, a compressive stress layer was formed on the surface of the sample (compressive stress: 110 MPa, compression depth: 10 micrometers). [Industrial Applicability]
[0144] The Li2O-Al2O3-SiO2-based crystallized glass of the present invention is suitable for use as front windows for oil stoves, wood stoves, etc., substrates for high-tech products such as color filters and image sensor substrates, setters for firing electronic components, light diffusers, furnace tubes for semiconductor manufacturing, masks for semiconductor manufacturing, optical lenses, components for dimensional measurement, components for communication, components for construction, containers for chemical reactions, top plates for electromagnetic cooking, heat-resistant tableware, heat-resistant covers, window glass for fire doors, components for astronomical telescopes, components for space optics, etc.
Claims
【Request 1】 In mass%, SiO 2 55-75%, Al 2 O 3 18-27%, Li 2 O 1-10%, SnO 2 0.05-20%, ZrO 2 1-20%, MgO 0-10%, P 2 O 5 0-10%, TiO 2 0 to 4%, CaO 0.0001% or more, Fe 2 O 3 0 to 0.1%, Pt 0 to 7 ppm, Rh 0 to 7 ppm, and (Li 2 O+Na 2 O+K 2 O) / ZrO 2 is 1.98 or less, (MgO + ZnO) / Li 2 O is 0.394 or less, SnO 2 / (SnO 2 + ZrO 2 ) is 0.05 to 0.70 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 2】 In mass%, ZrO 2 The Li according to claim 1, wherein the Li content is 1 to 5%. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 3】 Furthermore, in mass%, Na 2 O 0-10%, K 2 O 0-10%, CaO 0.0001-10%, SrO 0-10%, BaO 0-10%, ZnO 0-10%, B 2 O 3 3. The Li according to claim 1, wherein the Li content is 0 to 10%. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 4】 In terms of mass ratio, SnO 2 / (SnO 2 + ZrO 2 +P 2 O 5 + TiO 2 +B 2 O 3 ) is 0.06 or more, 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 5】 In terms of mass ratio, Al 2 O 3 / (SnO 2 + ZrO 2 ) is 7.1 or less. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. [Request 6] In mass%, Na 2 O+K 2 The Li alloy according to any one of claims 1 to 5, characterized in that it contains 8% or less of O+CaO+SrO+BaO. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 7】 In terms of mass ratio, (SiO 2 +Al 2 O 3 ) / Li 2 Li according to any one of claims 1 to 6, characterized in that O is 20 or more. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 8】 In terms of mass ratio, (SiO 2 +Al 2 O 3 ) / SnO 2 The Li according to any one of claims 1 to 7, wherein the Li 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 9】 In terms of mass ratio, TiO 2 / ZrO 2 The Li according to any one of claims 1 to 8, wherein 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 10】 In mass%, HfO 2 +Ta 2 O 5 The Li according to any one of claims 1 to 9, containing less than 0.05% 2 O-Al 2 O 3 -SiO 2 Glass-ceramics.
11. The Li-based lithium-ion battery according to any one of claims 1 to 10, characterized in that it contains, in mass%, Pt + Rh of 9 ppm or less. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 12】 The Li-based electrolytic capacitor according to any one of claims 1 to 11, characterized in that the appearance is colorless and transparent. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. [Request 13] The Li-based film according to any one of claims 1 to 12, which has a thickness of 3 mm and a transmittance of 10% or more at a wavelength of 300 nm. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. [Request 14] The Li alloy according to any one of claims 1 to 13, characterized in that β-quartz solid solution is precipitated as the main crystal. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. 【Request 15】 The thermal expansion coefficient at 30 to 380°C is 30 x 10 -7 / °C or less. 2 O-Al 2 O 3 -SiO 2 Glass-ceramics. [Request 16] The thermal expansion coefficient at 30 to 750°C is 30 x 10 -7 The Li according to any one of claims 1 to 15, wherein the Li 2 O-Al 2 O 3 -SiO 2 Glass-ceramics.
Citation Information
Patent Citations
Crystallized glass
JP2001342038A
Li2O-Al2O3-SiO2-BASED CRYSTALLIZED GLASS
JP2012056829A
Li2O-Al2O3-SiO2-BASED CRYSTALLIZED GLASS
JP2015074596A