Modified PTFE with controlled breaking strength and specific gravity, produced via emulsion polymerization, addresses the challenge of high strength and low pressure, enhancing moldability and flexibility for diverse applications.
Patent Information
- Application Number
- JP2024141092
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-08-10
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
AI Technical Summary
Existing polytetrafluoroethylene (PTFE) materials face challenges in achieving high breaking strength while maintaining low extrusion pressure, leading to issues with moldability and extrusion difficulties.
Modified PTFE with specific breaking strength and standard specific gravity ranges, incorporating tetrafluoroethylene and vinylidene fluoride units, is produced through controlled emulsion polymerization to achieve low extrusion pressure and excellent moldability.
The modified PTFE exhibits high breaking strength with low extrusion pressure, enabling improved moldability and flexibility, suitable for various applications including filtration and textile products.
Smart Images

Figure 2024164150000001 
Figure 2024164150000002 
Figure 2024164150000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to modified polytetrafluoroethylene and aqueous dispersions. [Background technology]
[0002] When polytetrafluoroethylene is molded and highly stretched in an unsintered state, a porous polytetrafluoroethylene film is obtained. This porous film allows gases such as water vapor to pass through, but does not allow water droplets to pass through due to the strong water repellency of polytetrafluoroethylene. Taking advantage of this unique property, it is used in clothing, separation membranes, etc.
[0003] Patent Document 1 describes a fine powder made of a tetrafluoroethylene homopolymer having a given standard specific gravity and breaking strength.
[0004] Patent Document 2 describes modified polytetrafluoroethylene having units based on perfluoro(propyl vinyl ether) or hexafluoropropylene. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2002-201217 A [Patent Document 2] JP 2006-117912 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present disclosure is to provide a modified polytetrafluoroethylene and an aqueous dispersion that have high breaking strength yet low extrusion pressure. [Means for solving the problem]
[0007] The present disclosure (1) is a modified polytetrafluoroethylene having a breaking strength of more than 32.8 N and a standard specific gravity of 2.150 or more.
[0008] The present disclosure (2) is the modified polytetrafluoroethylene according to the present disclosure (1), having a strength ratio expressed as breaking strength (N) / extrusion pressure (MPa) of more than 1.90 N / MPa.
[0009] The present disclosure (3) is the modified polytetrafluoroethylene according to the present disclosure (1) or (2), which has a breaking strength of more than 37.0 N.
[0010] The present disclosure (4) is a modified polytetrafluoroethylene having a standard specific gravity of 2.155 or more, which is any combination with any of the present disclosures (1) to (3).
[0011] The present disclosure (5) is a modified polytetrafluoroethylene having a standard specific gravity of 2.160 or more, which is any combination with any of the present disclosures (1) to (4).
[0012] The present disclosure (6) is a modified polytetrafluoroethylene having a standard specific gravity of 2.150 or more and a strength ratio expressed as breaking strength (N) / extrusion pressure (MPa) of more than 1.90 N / MPa.
[0013] The present disclosure (7) is a modified polytetrafluoroethylene that contains tetrafluoroethylene units and vinylidene fluoride units, and in which the amount of the vinylidene fluoride units is 1.0 mass% or less based on the total polymerized units.
[0014] The present disclosure (8) is a modified polytetrafluoroethylene in any combination with any of the present disclosures (1) to (7) in powder form.
[0015] The present disclosure (9) is a modified polytetrafluoroethylene in any combination with any of the present disclosures (1) to (8) which are fine powders.
[0016] The present disclosure (10) is an aqueous dispersion containing particles of modified polytetrafluoroethylene in any combination with any of the present disclosures (1) to (7). Effect of the Invention
[0017] According to the present disclosure, it is possible to provide a modified polytetrafluoroethylene and an aqueous dispersion that can be extruded at a low pressure despite having high breaking strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Generally, the breaking strength of polytetrafluoroethylene (PTFE) can be increased by increasing the extrusion pressure, but the paste extrudate tends to become hard and the moldability of the extrudate tends to deteriorate. However, as a result of extensive research, it was discovered that by using modified PTFE and controlling the breaking strength and standard specific gravity, it is possible to obtain PTFE that has a high breaking strength but a low extrusion pressure, contrary to common technical knowledge.
[0019] The present disclosure will now be described in detail.
[0020] The present disclosure provides a modified PTFE (hereinafter also referred to as a first modified PTFE) having a breaking strength of more than 32.8 N and a standard specific gravity of 2.150 or more. The first modified PTFE has the above-mentioned structure, and therefore has high breaking strength, but also has low extrusion pressure and excellent moldability. The reason for this is unclear, but it is speculated that the high standard density (low molecular weight) gives flexibility to the molded product and allows it to be molded uniformly even at low extrusion pressure. It is also speculated that the modified PTFE allows the fibrillated molecules to bond more tightly during paste extrusion compared to homo-PTFE, resulting in high breaking strength.
[0021] The first modified PTFE has a breaking strength of more than 32.8 N. The breaking strength is preferably 33.0 N or more, more preferably 35.0 N or more, even more preferably 37.0 N or more, even more preferably more than 37.0 N, even more preferably 38.0 N or more, particularly preferably 40.0 N or more, and most preferably 42.0 N or more. The higher the breaking strength, the better, but it may be 100.0 N or less, 80.0 N or less, or 50.0 N or less. The breaking strength is a value determined by the following method. The stretched bead (produced by stretching the bead) obtained in the stretching test carried out at a stretch speed of 100% / sec described below is clamped and fixed in a movable jaw having a gauge length of 5.0 cm, and a tensile test is carried out at 25°C and a speed of 300 mm / min, and the strength at the time of break is measured as the breaking strength.
[0022] The first modified PTFE has a standard specific gravity (SSG) of 2.150 or more. In terms of being able to further increase the breaking strength and further reduce the extrusion pressure, the standard specific gravity is preferably 2.155 or more, more preferably 2.160 or more, even more preferably 2.165 or more, even more preferably 2.170 or more, particularly preferably 2.175 or more, most preferably 2.180 or more, and is preferably 2.250 or less, more preferably 2.240 or less, even more preferably 2.230 or less, even more preferably 2.220 or less, particularly preferably 2.210 or less. The standard specific gravity is measured by a water displacement method according to ASTM D 792 using a sample molded according to ASTM D 4895.
[0023] The strength ratio of the first modified PTFE, expressed as breaking strength (N) / extrusion pressure (MPa), is preferably more than 1.90 N / MPa, more preferably 1.95 N / MPa or more, even more preferably 2.00 N / MPa or more, even more preferably 2.05 N / MPa or more, even more preferably 2.10 N / MPa or more, even more preferably 2.20 N / MPa or more, and particularly preferably 2.25 N / MPa or more. The higher the strength ratio, the better, but it may be 5.00 N / MPa or less, or 4.00 N / MPa or less. A higher strength ratio means a higher breaking strength and a lower extrusion pressure. The breaking strength is a value determined by the method described above. The above extrusion pressure is a value determined by the following method. 21.7 g of lubricant (trade name: Isopar H (registered trademark), manufactured by Exxon Corp.) is added to 100 g of modified PTFE powder, and mixed at room temperature for 3 minutes to obtain a PTFE fine powder mixture. The obtained PTFE fine powder mixture is then left at room temperature (25°C) for at least 1 hour before extrusion, and then paste extruded at room temperature through an orifice (diameter 2.5 mm, land length 11 mm, introduction angle 30°) at a reduction ratio of 100:1 (ratio of cross-sectional area of the inlet and outlet of the die) to obtain a uniform bead (beading; extrusion molded body). The extrusion speed, i.e., the ram speed, is 20 inches / min (51 cm / min). The extrusion pressure is the value obtained by measuring the load when the extrusion load reaches equilibrium in the paste extrusion and dividing it by the cross-sectional area of the cylinder used for the paste extrusion.
[0024] The first modified PTFE is preferably stretchable. In this specification, "stretchable" is determined according to the following criteria. The bead obtained by the above paste extrusion is heated at 230°C for 30 minutes to remove the lubricant from the bead. The bead (extrudate) is then cut to the appropriate length, clamped at each end with a clamp distance of 2.0 inches (51 mm) between the clamps, and heated to 300°C in an air circulating oven. The clamps are then moved apart at a desired speed (stretch rate) until a separation distance corresponding to the desired stretch (total stretch) is achieved, and a stretch test is performed. The stretching method essentially follows that disclosed in U.S. Pat. No. 4,576,869, except for the extrusion speed (51 cm / min instead of 84 cm / min). "Stretch" is the increase in length due to stretching, and is usually expressed in relation to the original length. In the above preparation method, the stretch rate is 1000% / sec and the total stretch is 2400%. A stretchable material is considered to be stretchable if it does not break before the stretch is completed.
[0025] In the above-mentioned production method, the modified PTFE of the present disclosure is preferably subjected to a stretch test under conditions of a stretch rate of 100% / sec and a total stretch of 2400%, and does not break before the above-mentioned stretching is completed.
[0026] The first modified PTFE contains polymerization units (TFE units) based on tetrafluoroethylene (TFE) and polymerization units (modified monomer units) based on a modified monomer. In this specification, the term "modified PTFE" refers to a PTFE having a content of modified monomer units of 1.0 mass% or less based on the total polymerization units. The content of TFE units in the modified PTFE may be 99.0% by mass or more. The modified PTFE may consist of only TFE units and modified monomer units.
[0027] The content of the modified monomer unit is 1.0% by mass or less based on the total polymerized units, but in terms of lowering the extrusion pressure and increasing the breaking strength, it is preferably 0.80% by mass or less based on the total polymerized units, more preferably 0.50% by mass or less, even more preferably 0.40% by mass or less, even more preferably 0.30% by mass or less, even more preferably 0.20% by mass or less, even more preferably 0.10% by mass or less, even more preferably 0.08% by mass or less, particularly preferably 0.05% by mass or less, and most preferably 0.03% by mass or less. The content of the modified monomer unit may be 0.0001% by mass or more, 0.001% by mass or more, or 0.005% by mass or more, based on the total polymerized units. In this specification, the modified monomer unit means a portion of the molecular structure of the modified PTFE that is derived from the modified monomer.
[0028] The content of each of the above-mentioned polymer units can be calculated by appropriately combining NMR, FT-IR, elemental analysis, and X-ray fluorescence analysis depending on the type of monomer.
[0029] The above-mentioned modified monomer is not particularly limited as long as it can be copolymerized with TFE, and examples thereof include perfluoroolefins such as hexafluoropropylene [HFP], hydrogen-containing fluoroolefins such as trifluoroethylene and vinylidene fluoride [VDF], perhaloolefins such as chlorotrifluoroethylene, perfluorovinyl ether, perfluoroallyl ether, (perfluoroalkyl)ethylene, ethylene, etc. The modified monomer used may be one type or multiple types.
[0030] The perfluorovinyl ether is not particularly limited, and examples thereof include perfluorovinyl ethers represented by the following general formula (A): CF2=CF-ORf (A) (wherein Rf represents a perfluoro organic group). In this specification, the "perfluoro organic group" refers to an organic group in which all hydrogen atoms bonded to carbon atoms are replaced with fluorine atoms. The perfluoro organic group may have an ether oxygen.
[0031] An example of the perfluorovinyl ether is perfluoro(alkyl vinyl ether) [PAVE], where Rf in the general formula (A) is a perfluoroalkyl group having 1 to 10 carbon atoms. The number of carbon atoms in the perfluoroalkyl group is preferably 1 to 5.
[0032] Examples of the perfluoroalkyl group in the PAVE include a perfluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, and a perfluorohexyl group.
[0033] The perfluorovinyl ether further includes those in which Rf in the above general formula (A) is a perfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms, and those in which Rf is the following formula:
[0034] [ka]
[0035] (wherein m represents 0 or an integer of 1 to 4), Rf is a group represented by the following formula:
[0036] [ka]
[0037] (wherein n represents an integer of 1 to 4).
[0038] The (perfluoroalkyl)ethylene (PFAE) is not particularly limited, and examples thereof include (perfluorobutyl)ethylene (PFBE) and (perfluorohexyl)ethylene.
[0039] The perfluoroallyl ether may, for example, be a compound represented by the general formula (B): CF2=CF-CF2-ORf 1 (B) (In the formula, Rf 1 represents a perfluoro organic group.
[0040] Above Rf 1 is preferably a perfluoroalkyl group having 1 to 10 carbon atoms or a perfluoroalkoxyalkyl group having 1 to 10 carbon atoms. The perfluoroallyl ether is preferably at least one selected from the group consisting of CF2=CF-CF2-O-CF3, CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9, more preferably at least one selected from the group consisting of CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9, and further preferably CF2=CF-CF2-O-CF2CF2CF3.
[0041] As the above-mentioned modifying monomer, at least one selected from the group consisting of VDF, CTFE, PAVE and HFP is preferred, since it is easy to adjust the breaking strength and standard specific gravity within the above-mentioned ranges, at least one selected from the group consisting of VDF, CTFE and HFP is more preferred, and at least one selected from the group consisting of VDF and HFP is even more preferred, and VDF is particularly preferred, since it allows for a lower extrusion pressure and a higher breaking strength, and allows for high breaking strength and elongation to be obtained even when processed at low temperature. In terms of improving heat resistance, it is also preferable to use both VDF and HFP as the modifying monomer.
[0042] The first modified PTFE generally has non-melt secondary processability. The non-melt secondary processability means that the melt flow rate cannot be measured at a temperature higher than the melting point according to ASTM D-1238 and D-2116, in other words, the PTFE does not flow easily even in the melting temperature range.
[0043] It is preferable that the first modified PTFE has no history of being heated to a temperature of 300°C or higher, and in a heat of fusion curve measured by a differential scanning calorimeter (DSC) at a temperature rise rate of 10°C / min, shows one or more endothermic peaks in the range of 333 to 347°C, and the heat of fusion at 290 to 350°C calculated from the heat of fusion curve is 62 mJ / mg or more.
[0044] The first modified PTFE can be produced, for example, by a production method including a step (A) of emulsion polymerizing TFE and a modifying monomer.
[0045] The above emulsion polymerization can be carried out, for example, in an aqueous medium in the presence of an anionic fluorine-containing surfactant and a polymerization initiator. The emulsion polymerization can be carried out by charging an aqueous medium, the anionic fluorine-containing surfactant, monomers and, if necessary, other additives into a polymerization reactor, stirring the contents of the reactor, maintaining the reactor at a predetermined polymerization temperature, and then adding a predetermined amount of polymerization initiator to initiate the polymerization reaction. After the start of the polymerization reaction, monomers, polymerization initiators, chain transfer agents, the surfactants and the like may be additionally added depending on the purpose.
[0046] In terms of easily obtaining each of the above-mentioned physical properties, the modified monomer (preferably VDF) concentration in the gas in the reactor at the start of polymerization (at the time of adding the initiator) is preferably 0.001 mol% or more, more preferably 0.01 mol% or more. The above concentration may also be 15 mol% or less, preferably 6.0 mol% or less, more preferably 5.0 mol% or less, even more preferably 3.0 mol% or less, and particularly preferably 1.0 mol% or less. The modified monomer concentration may be maintained thereafter until the end of the polymerization reaction, or depressurization may be performed during the reaction. The modified monomer is preferably charged all at once before the start of polymerization, but a portion of it may be added continuously or intermittently after the start of polymerization.
[0047] The polymerization initiator is not particularly limited as long as it can generate radicals within the polymerization temperature range, and known oil-soluble and / or water-soluble polymerization initiators can be used. Furthermore, it can also be combined with a reducing agent or the like to initiate polymerization as a redox. The concentration of the polymerization initiator is appropriately determined depending on the type of monomer, the molecular weight of the desired modified PTFE, and the reaction rate.
[0048] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical polymerization initiator can be used.
[0049] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, for example, dialkyl peroxycarbonates such as diisopropyl peroxydicarbonate and disec-butyl peroxydicarbonate, peroxyesters such as t-butyl peroxyisobutyrate and t-butyl peroxypivalate, dialkyl peroxides such as di-t-butyl peroxide, and the like. In addition, di(ω-hydro-dodecafluoroheptanoyl) peroxide, di(ω-hydro-tetradecafluoroheptanoyl) peroxide, di(ω-hydro-hexadecafluorononanoyl) peroxide, di(perfluorobutyryl) peroxide, di(perfluorovaleryl) peroxide, di(perfluorohexanoyl) peroxide, di(perfluoroheptanoyl) peroxide, di(perfluorooctanoyl) peroxide, di(perfluorononanoyl) peroxide, di(ω-chloro Representative examples include di[perfluoro(or fluorochloro)acyl]peroxides such as di(ω-hexafluorobutyryl) peroxide, di(ω-chloro-decafluorohexanoyl) peroxide, di(ω-chloro-tetradecafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexadecafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydrododecafluoroheptanoyl-perfluorobutyryl-peroxide, di(dichloropentafluorobutanoyl) peroxide, di(trichlorooctafluorohexanoyl) peroxide, di(tetrachloroundecafluorooctanoyl) peroxide, di(pentachlorotetradecafluorodecanoyl) peroxide, and di(undecachlorodotriacontafluorodocosanoyl) peroxide.
[0050] The water-soluble radical polymerization initiator may be a known water-soluble peroxide, such as ammonium salts, potassium salts, or sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, or percarbonic acid, t-butyl permaleate, or t-butyl hydroperoxide, etc. A reducing agent such as sulfites or sulfites may also be contained, and the amount used may be 0.1 to 20 times that of the peroxide.
[0051] For example, when polymerization is carried out at a low temperature of 30° C. or less, it is preferable to use a redox initiator that combines an oxidizing agent and a reducing agent as the polymerization initiator. Examples of the oxidizing agent include persulfates, organic peroxides, potassium permanganate, manganese triacetate, cerium ammonium nitrate, and bromates. Examples of the reducing agent include sulfites, bisulfites, bromates, diimines, and oxalic acid. Examples of the persulfates include ammonium persulfate and potassium persulfate. Examples of the sulfites include sodium sulfite and ammonium sulfite. In order to increase the decomposition rate of the initiator, it is also preferable to add a copper salt or an iron salt to the combination of the redox initiator. Examples of the copper salt include copper(II) sulfate, and examples of the iron salt include iron(II) sulfate.
[0052] As the redox initiator, it is preferred that the oxidizing agent is permanganic acid or a salt thereof, a persulfate, manganese triacetate, a cerium (IV) salt, or bromic acid or a salt thereof, and the reducing agent is a dicarboxylic acid or a salt thereof, or a diimine. More preferably, the oxidizing agent is permanganic acid or a salt thereof, a persulfate, or bromic acid or a salt thereof, and the reducing agent is a dicarboxylic acid or a salt thereof.
[0053] Examples of the redox initiator include combinations of potassium permanganate / oxalic acid, potassium permanganate / ammonium oxalate, manganese triacetate / oxalic acid, manganese triacetate / ammonium oxalate, cerium ammonium nitrate / oxalic acid, and cerium ammonium nitrate / ammonium oxalate. When a redox initiator is used, either the oxidizing agent or the reducing agent may be charged in advance in a polymerization tank, and then the other may be added continuously or intermittently to initiate polymerization. For example, when potassium permanganate / ammonium oxalate is used, it is preferable to charge ammonium oxalate in a polymerization tank and continuously add potassium permanganate thereto. In this specification, when the redox initiator is described as "potassium permanganate / ammonium oxalate," it means a combination of potassium permanganate and ammonium oxalate. The same applies to other compounds.
[0054] The redox initiator is particularly preferably a combination of an oxidizing agent that is a salt and a reducing agent that is a salt. For example, the oxidizing agent which is the salt is more preferably at least one selected from the group consisting of persulfates, permanganates, cerium (IV) salts, and bromates, further preferably permanganates, and particularly preferably potassium permanganate. The reducing agent which is the salt is more preferably at least one selected from the group consisting of oxalates, malonates, succinates, glutarates and bromates, further preferably oxalates, and particularly preferably ammonium oxalate.
[0055] Specifically, the redox initiator is preferably at least one selected from the group consisting of potassium permanganate / oxalic acid, potassium permanganate / ammonium oxalate, potassium bromate / ammonium sulfite, manganese triacetate / ammonium oxalate, and cerium ammonium nitrate / ammonium oxalate, more preferably at least one selected from the group consisting of potassium permanganate / oxalic acid, potassium permanganate / ammonium oxalate, potassium bromate / ammonium sulfite, and cerium ammonium nitrate / ammonium oxalate, and even more preferably potassium permanganate / oxalic acid.
[0056] When a redox initiator is used, the oxidizing agent and the reducing agent may be added all at once at the beginning of the polymerization, the reducing agent may be added all at once at the beginning of the polymerization and the oxidizing agent may be added continuously, the oxidizing agent may be added all at once at the beginning of the polymerization and the reducing agent may be added continuously, or both the oxidizing agent and the reducing agent may be added continuously.
[0057] When a redox initiator is used as a polymerization initiator, the amount of the oxidizing agent added is preferably 5 ppm or more, more preferably 10 ppm or more, and preferably 10000 ppm or less, more preferably 1000 ppm or less, relative to the aqueous medium. The amount of the reducing agent added is preferably 5 ppm or more, more preferably 10 ppm or more, and preferably 10000 ppm or less, more preferably 1000 ppm or less. In order to easily obtain a modified PTFE suitable for stretching applications, the amount of the oxidizing agent added to the aqueous medium is preferably 0.1 ppm or more, more preferably 1.0 ppm or more, and preferably 100 ppm or less, more preferably 10 ppm or less. The amount of the reducing agent added is preferably 0.1 ppm or more, more preferably 1.0 ppm or more, and preferably 100 ppm or less, more preferably 10 ppm or less. When a redox initiator is used in the emulsion polymerization, the polymerization temperature is preferably 100° C. or lower, more preferably 95° C. or lower, and even more preferably 90° C. or lower. The polymerization temperature is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher.
[0058] As the polymerization initiator, a water-soluble radical polymerization initiator and a redox initiator are preferred, since it is easy to adjust the breaking strength and standard specific gravity within the above-mentioned ranges.
[0059] The amount of polymerization initiator to be added is not particularly limited, but may be added all at once, stepwise, or continuously at the beginning of polymerization in an amount (for example, several ppm to water concentration) that does not significantly reduce the polymerization rate. The upper limit is a range in which the reaction temperature may be increased while removing heat from the equipment side by the polymerization reaction heat, and a more preferred upper limit is a range in which the polymerization reaction heat can be removed from the equipment side. More specifically, for example, the amount is preferably 1 ppm or more, more preferably 10 ppm or more, and even more preferably 50 ppm or more, relative to the aqueous medium. Also, 100,000 ppm or less is preferable, 10,000 ppm or less is more preferable, and 5,000 ppm or less is even more preferable. In terms of easily obtaining the above-mentioned physical properties, the amount of the polymerization initiator added is preferably an amount equivalent to 0.1 ppm or more, more preferably an amount equivalent to 1.0 ppm or more, and is preferably an amount equivalent to 100 ppm or less, more preferably an amount equivalent to 10 ppm or less, relative to the aqueous medium.
[0060] The aqueous medium is a reaction medium for polymerization, and refers to a liquid containing water. The aqueous medium is not particularly limited as long as it contains water, and may contain water and, for example, a fluorine-free organic solvent such as an alcohol, ether, or ketone, and / or a fluorine-containing organic solvent having a boiling point of 40° C. or less.
[0061] In the above emulsion polymerization, a nucleating agent, a chain transfer agent, a buffering agent, a pH adjusting agent, a stabilizing aid, a dispersion stabilizer, a radical scavenger, a decomposing agent for the polymerization initiator, and the like may be used, if necessary.
[0062] The emulsion polymerization is preferably carried out with the addition of a nucleating agent for the purpose of adjusting the particle size. The nucleating agent is preferably added before the start of the polymerization reaction. As the nucleating agent, a known agent can be used. For example, it is preferable that the nucleating agent is at least one selected from the group consisting of fluoropolyethers, nonionic surfactants, and chain transfer agents, and it is more preferable that the nucleating agent is a nonionic surfactant.
[0063] The fluoropolyether may, for example, be a perfluoropolyether (PFPE) acid or a salt thereof. The perfluoropolyether (PFPE) acid or salt thereof may have any chain structure in which oxygen atoms in the backbone of the molecule are separated by saturated fluorocarbon groups having 1 to 3 carbon atoms. Also, two or more types of fluorocarbon groups may be present in the molecule. A representative structure has a repeating unit represented by the following formula: (-CFCF3-CF2-O-) n (-CF2-CF2-CF2-O-) n (-CF2-CF2-O-) n -(-CF2-O-) m (-CF2-CFCF3-O-) n -(-CF2-O-) m
[0064] These structures are described by Kasai in J. Appl. Polymer Sci. 57, 797 (1995). As disclosed therein, the PFPE acid or its salt may have a carboxylic acid group or its salt at one or both ends. The PFPE acid or its salt may also have a sulfonic acid, phosphonic acid group or their salt at one or both ends. The PFPE acid or its salt may also have a different group at each end. For monofunctional PFPEs, the other end of the molecule is usually perfluorinated, but may contain hydrogen or chlorine atoms. The PFPE acid or its salt has at least two ether oxygens, preferably at least four ether oxygens, and even more preferably at least six ether oxygens. Preferably, at least one of the fluorocarbon groups separating the ether oxygens, more preferably at least two of such fluorocarbon groups, has two or three carbon atoms. Even more preferably, at least 50% of the fluorocarbon groups separating the ether oxygens have 2 or 3 carbon atoms. Also preferably, the PFPE acid or salt thereof has a total of at least 15 carbon atoms, for example, the preferred minimum value of n or n+m in the repeating unit structure above is at least 5. Two or more of the PFPE acids or salts thereof having an acid group at one or both termini may be used in the manufacturing method of the present disclosure. The PFPE acid or salt thereof preferably has a number average molecular weight of less than 6000 g / mol.
[0065] The emulsion polymerization is preferably carried out by adding a radical scavenger or a decomposer of the polymerization initiator, since it is possible to further increase the molecular weight of the modified PTFE and improve the stretchability. The radical scavenger or the decomposer of the polymerization initiator is preferably added after the start of the polymerization reaction, preferably before 10% by mass or more, preferably 20% by mass or more of the total TFE consumed in the polymerization reaction is polymerized, and preferably before 50% by mass or less, preferably 40% by mass or less is polymerized. When depressurization and repressurization are performed as described below, it is preferable to add it after that.
[0066] The radical scavenger is a compound that does not have the ability to restart after addition or chain transfer to the free radical in the polymerization system. Specifically, a compound that easily undergoes a chain transfer reaction with a primary radical or a growing radical, and then generates a stable radical that does not react with a monomer, or a compound that easily undergoes an addition reaction with a primary radical or a growing radical, and generates a stable radical, is used. Generally, the activity of what is called a chain transfer agent is characterized by the chain transfer constant and the reinitiation efficiency, but among chain transfer agents, those with a reinitiation efficiency of almost 0% are called radical scavengers. The radical scavenger can be, for example, a compound whose chain transfer constant with TFE at the polymerization temperature is greater than the polymerization rate constant and whose reinitiation efficiency is substantially zero percent. "Reinitiation efficiency is substantially zero percent" means that the generated radicals turn the radical scavenger into stable radicals. Preferably, the compound has a chain transfer constant (Cs) with TFE at the polymerization temperature (=chain transfer rate constant (kc) / polymerization rate constant (kp)) of more than 0.1. The above compound has a chain transfer constant (Cs) of more preferably 0.5 or more, even more preferably 1.0 or more, even more preferably 5.0 or more, and particularly preferably 10 or more.
[0067] The radical scavenger is preferably at least one selected from the group consisting of, for example, aromatic hydroxy compounds, aromatic amines, N,N-diethylhydroxylamine, quinone compounds, terpenes, thiocyanates, and cupric chloride (CuCl2). Examples of the aromatic hydroxy compound include unsubstituted phenol, polyhydric phenol, salicylic acid, m- or p-salicylic acid, gallic acid, and naphthol. The unsubstituted phenols include o-, m-, or p-nitrophenol, o-, m-, or p-aminophenol, p-nitrosophenol, etc. The polyhydric phenols include catechol, resorcinol, hydroquinone, pyrogallol, phloroglucinol, naphthresorcinol, etc. Examples of aromatic amines include o-, m- or p-phenylenediamine, benzidine, and the like. Examples of the quinone compound include o-, m- or p-benzoquinone, 1,4-naphthoquinone, alizarin, and the like. Examples of thiocyanates include ammonium thiocyanate (NH4SCN), potassium thiocyanate (KSCN), and sodium thiocyanate (NaSCN). Of the above radical scavengers, aromatic hydroxy compounds are preferred, unsubstituted phenols or polyhydric phenols are more preferred, and hydroquinone is even more preferred.
[0068] The amount of the radical scavenger added is preferably an amount equivalent to 3 to 500% (molar basis) of the polymerization initiator concentration from the viewpoint of appropriately reducing the standard specific gravity. A more preferred lower limit is 10% (molar basis), and even more preferred is 15% (molar basis). A more preferred upper limit is 400% (molar basis), and even more preferred is 300% (molar basis).
[0069] The decomposer for the polymerization initiator may be any compound capable of decomposing the polymerization initiator used, and is preferably at least one selected from the group consisting of sulfites, bisulfites, bromates, diimines, diimine salts, oxalic acid, oxalates, copper salts, and iron salts. Examples of sulfites include sodium sulfite and ammonium sulfite. Examples of copper salts include copper(II) sulfate, and examples of iron salts include iron(II) sulfate. The amount of the decomposition agent added is preferably an amount equivalent to 3 to 500% (molar basis) of the initiator concentration from the viewpoint of appropriately reducing the standard specific gravity. A more preferred lower limit is 10% (molar basis), and even more preferred is 15% (molar basis). A more preferred upper limit is 400% (molar basis), and even more preferred is 300% (molar basis).
[0070] In the above emulsion polymerization, the polymerization temperature and polymerization pressure are appropriately determined depending on the type of monomer used, the molecular weight of the desired modified PTFE, and the reaction rate. Usually, the polymerization temperature is 5 to 150°C, preferably 10°C or higher, more preferably 30°C or higher, and even more preferably 50°C or higher. Also, it is more preferably 120°C or lower, and even more preferably 100°C or lower. The polymerization pressure is 0.05 to 10 MPaG. The polymerization pressure is more preferably 0.3 MPaG or more, and even more preferably 0.5 MPaG or more. Also, the polymerization pressure is more preferably 5.0 MPaG or less, and even more preferably 3.0 MPaG or less.
[0071] In the emulsion polymerization, it is preferable not to release the pressure after the modified monomer is charged into the polymerization vessel until the polymerization is completed, so that the modified monomer can be left in the system until the end of the polymerization, and the breaking strength of the resulting modified PTFE can be further increased.
[0072] The above-mentioned production method may include a step (B) of coagulating the above-mentioned aqueous dispersion to obtain a wet powder of the above-mentioned modified PTFE. The above-mentioned coagulation can be carried out by a known method.
[0073] The above-mentioned manufacturing method may include a step (C) of drying the above-mentioned wet powder. The above-mentioned drying is usually carried out by using a means such as vacuum, high frequency, or hot air while keeping the above-mentioned wet powder in a state where it is not very fluid, preferably in a state where it is left stationary. Friction between powders, especially at high temperatures, generally has an undesirable effect on fine powder-type PTFE. This is because particles made of this type of PTFE have the property of easily fibrillating even with a small shear force and losing the original stable particle structure state. The drying temperature is preferably 300° C. or less, more preferably 250° C. or less, even more preferably 230° C. or less, even more preferably 210° C. or less, even more preferably 190° C. or less, and particularly preferably 170° C. or less, from the viewpoint of reducing the extrusion pressure. From the viewpoint of improving the breaking strength, the temperature is preferably 10° C. or more, more preferably 100° C. or more, even more preferably 150° C. or more, even more preferably 170° C. or more, even more preferably 190° C. or more, and particularly preferably 210° C. or more. In order to further increase the strength ratio, it is preferable to appropriately adjust the temperature within this temperature range.
[0074] The present disclosure also provides a modified PTFE (hereinafter also referred to as a second modified PTFE) having a standard specific gravity of 2.150 or more and a strength ratio expressed as breaking strength (N) / extrusion pressure (MPa) of more than 1.90 N / MPa. The second modified PTFE has the above-mentioned structure, and therefore has high breaking strength, but also has low extrusion pressure and excellent moldability.
[0075] The second modified PTFE has a standard specific gravity (SSG) of 2.150 or more. In terms of being able to further increase the breaking strength and further reduce the extrusion pressure, the standard specific gravity is preferably 2.155 or more, more preferably 2.160 or more, even more preferably 2.165 or more, even more preferably 2.170 or more, particularly preferably 2.175 or more, most preferably 2.180 or more, and is preferably 2.250 or less, more preferably 2.240 or less, even more preferably 2.230 or less, even more preferably 2.220 or less, particularly preferably 2.210 or less.
[0076] The second modified PTFE has a strength ratio expressed by breaking strength (N) / extrusion pressure (MPa) of more than 1.90 N / MPa, preferably 1.95 N / MPa or more, more preferably 2.00 N / MPa or more, even more preferably 2.05 N / MPa or more, even more preferably 2.10 N / MPa or more, even more preferably 2.20 N / MPa or more, and particularly preferably 2.25 N / MPa or more. The higher the strength ratio, the better, but it may be 5.00 N / MPa or less, or 4.00 N / MPa or less.
[0077] The second modified PTFE preferably has a breaking strength of more than 32.8 N, more preferably 33.0 N or more, even more preferably 35.0 N or more, even more preferably 37.0 N or more, even more preferably 37.0 N or more, even more preferably 38.0 N or more, particularly preferably 40.0 N or more, and most preferably 42.0 N or more. The higher the breaking strength, the better, but it may be 100.0 N or less, 80.0 N or less, or 50.0 N or less.
[0078] The second modified PTFE is preferably expandable.
[0079] The second modified PTFE contains a TFE unit and a modified monomer unit. The modified monomer may be any of those exemplified for the first modified PTFE. The content of the modified monomer unit may be within the same range as that of the first modified PTFE.
[0080] The second modified PTFE may have similar physical properties to the first modified PTFE, except that the strength ratio is greater than 1.90 N / MPa.
[0081] The second modified PTFE can be produced by the production method explained for the first modified PTFE.
[0082] The present disclosure also provides a modified PTFE (hereinafter also referred to as a third modified PTFE) which contains tetrafluoroethylene (TFE) units and vinylidene fluoride (VDF) units, and in which the amount of the VDF units is 1.0 mass % or less based on the total polymerized units. The third modified PTFE has the above-mentioned structure, and therefore has high breaking strength, but also has low extrusion pressure and excellent moldability. In addition, the third modified PTFE has high breaking strength and breaking elongation even when processed at low temperature. When a modified monomer such as perfluoro(alkyl vinyl ether) or hexafluoropropylene is used, the breaking strength and breaking elongation also decrease as the processing (e.g., baking) temperature decreases, but it has been surprisingly found that when a VDF unit is used as the modified monomer, high breaking strength and breaking elongation can be obtained even when processed at a low temperature (e.g., 340°C or lower).
[0083] The content of the VDF units is 1.0% by mass or less based on the total polymerization units, but in terms of lowering the extrusion pressure and increasing the breaking strength, it is preferably 0.80% by mass or less based on the total polymerization units, more preferably 0.50% by mass or less, even more preferably 0.40% by mass or less, even more preferably 0.30% by mass or less, even more preferably 0.20% by mass or less, even more preferably 0.10% by mass or less, even more preferably 0.08% by mass or less, particularly preferably 0.05% by mass or less, and most preferably 0.03% by mass or less. The content of the VDF units may be 0.0001% by mass or more, 0.001% by mass or more, or 0.005% by mass or more, based on the total polymerized units. In this specification, the VDF unit means a portion of the molecular structure of the modified PTFE that is derived from VDF.
[0084] The content of TFE units in the third modified PTFE may be 99.0% by mass or more.
[0085] The third modified PTFE may consist of only TFE units and VDF units, but may also contain, in addition to the TFE units and VDF units, polymerized units based on a modifying monomer other than VDF (other modifying monomer units). Examples of the other modifying monomer include the modifying monomers exemplified for the first modified PTFE, and among them, HFP is preferred from the viewpoint of improving heat resistance. When the second modified PTFE contains the other modified monomer units, the total amount of the VDF units and the other modified monomer units is preferably 1.0 mass % or less based on the total polymerized units. In one preferred embodiment, the second modified PTFE contains TFE units, VDF units and HFP units, and the total amount of the VDF units and the HFP units is 1.0 mass % or less based on the total polymerized units.
[0086] The third modified PTFE preferably has a breaking strength of more than 32.8 N, more preferably 33.0 N or more, even more preferably 35.0 N or more, even more preferably 37.0 N or more, even more preferably 37.0 N or more, even more preferably 38.0 N or more, particularly preferably 40.0 N or more, and most preferably 42.0 N or more. The higher the breaking strength, the better, but it may be 100.0 N or less, 80.0 N or less, or 50.0 N or less.
[0087] The third modified PTFE preferably has a standard specific gravity (SSG) of 2.150 or more, more preferably 2.155 or more, even more preferably 2.160 or more, even more preferably 2.165 or more, even more preferably 2.170 or more, particularly preferably 2.175 or more, most preferably 2.180 or more, and preferably 2.250 or less, more preferably 2.240 or less, even more preferably 2.230 or less, even more preferably 2.220 or less, particularly preferably 2.210 or less.
[0088] The third modified PTFE has a strength ratio expressed by breaking strength (N) / extrusion pressure (MPa) of preferably more than 1.90 N / MPa, more preferably 1.95 N / MPa or more, even more preferably 2.00 N / MPa or more, even more preferably 2.05 N / MPa or more, even more preferably 2.10 N / MPa or more, even more preferably 2.20 N / MPa or more, and particularly preferably 2.25 N / MPa or more. The higher the strength ratio, the better, but it may be 5.00 N / MPa or less, or 4.00 N / MPa or less.
[0089] The third modified PTFE is preferably expandable.
[0090] The third modified PTFE may have similar physical properties to the first modified PTFE, except that the modifying monomer is VDF.
[0091] The third modified PTFE can be produced by the production method explained for the first modified PTFE, except that VDF is used as the modified monomer.
[0092] The first, second and third modified PTFEs are preferably in the form of a powder, more preferably a fine powder.
[0093] The first, second and third modified PTFEs can also be provided in the form of an aqueous dispersion. An aqueous dispersion containing any of the first, second and third modified PTFE particles is also a preferred embodiment of the present disclosure. The aqueous dispersion of the present disclosure can form a coating film that is less likely to crack.
[0094] The first, second and third modified PTFEs preferably have an average primary particle size of 500 nm or less, more preferably 350 nm or less, even more preferably 300 nm or less, and particularly preferably 280 nm or less, and preferably 100 nm or more, more preferably 150 nm or more, even more preferably 170 nm or more, and particularly preferably 200 nm or more. The average primary particle size is measured by the following method. The modified PTFE aqueous dispersion is diluted with water until the solid content is 0.15% by mass, and the transmittance of the 550 nm projected light per unit length of the diluted latex obtained and the number-based length average particle diameter determined by measuring a specific direction using a transmission electron microscope photograph are measured to create a calibration curve. Using this calibration curve, the number-average particle diameter is determined from the measured transmittance of the 550 nm projected light of each sample, and is taken as the average primary particle diameter.
[0095] The first, second and third modified PTFEs may have an average aspect ratio of primary particles of 2.0 or less, preferably 1.8 or less, more preferably 1.7 or less, even more preferably 1.6 or less, even more preferably 1.5 or less, even more preferably 1.4 or less, especially preferably 1.3 or less, particularly preferably 1.2 or less, and most preferably 1.1 or less. The average aspect ratio may also be 1.0 or more. The above average aspect ratio is determined by observing the fluororesin powder or an aqueous fluororesin dispersion diluted to a solid content of approximately 1% by mass with a scanning electron microscope (SEM), processing the images of 200 or more particles randomly selected, and averaging the ratio of the long axis to the short axis.
[0096] The first, second and third modified PTFEs preferably have an average secondary particle size of 100 μm or more, more preferably 200 μm or more, and even more preferably 300 μm or more, and preferably 2000 μm or less, more preferably 1000 μm or less, even more preferably 800 μm or less, and particularly preferably 700 μm or less. The average secondary particle size is measured in accordance with JIS K 6891.
[0097] The first, second and third modified PTFEs are particularly useful as raw materials for the elongated body. The elongated body formed from any of the first, second and third modified PTFEs is also a preferred embodiment of the present disclosure.
[0098] The above-mentioned stretched body can be obtained by stretching the first, second and third modified PTFEs.
[0099] The above-mentioned stretched body is also preferably in the form of a film, a tube, a fiber, or a rod.
[0100] When the stretched body is a membrane (stretched membrane or porous membrane), it can be stretched by a known PTFE stretching method. Preferably, a sheet-like or rod-like paste extrudate is roll-stretched in the extrusion direction to obtain a uniaxially stretched film. Furthermore, a biaxially stretched film can also be obtained by stretching the film in the width direction using a tenter or the like. It is also preferable to carry out a semi-baking treatment before stretching.
[0101] The stretched body can be made into a porous body having a high porosity, and can be suitably used as a filter medium for various precision filters such as air filters and chemical filters, a support material for polymer electrolyte membranes, and the like. They are also useful as materials for products used in the fields of textiles, medicine, electrochemicals, sealing materials, air filtration, ventilation / internal pressure regulation, liquid filtration, and general consumer goods. Specific applications are given below as examples.
[0102] Electrochemical Field Dielectric material prepreg, EMI shielding material, heat transfer material, etc. More specifically, printed wiring board, electromagnetic shielding material, insulating heat transfer material, insulating material, etc. Sealing materials field Gaskets, packing, pump diaphragms, pump tubes, aircraft sealing materials, etc.
[0103] Air Filtration Field ULPA filters (for semiconductor manufacturing), HEPA filters (for hospitals and semiconductor manufacturing), cylindrical cartridge filters (for industrial use), bag filters (for industrial use), heat-resistant bag filters (for exhaust gas treatment), heat-resistant pleated filters (for exhaust gas treatment), SINBRAN filters (for industrial use), catalyst filters (for exhaust gas treatment), adsorbent filters (for HDD installation), adsorbent vent filters (for HDD installation), vent filters (for HDD installation and others), vacuum cleaner filters (for vacuum cleaners), general-purpose multi-layer felt material, GT cartridge filters (for GT compatible products), cooling filters (for electronic device housings), etc.
[0104] Ventilation / internal pressure regulation field Freeze-drying materials such as freeze-drying containers, automotive ventilation materials for electronic circuits and lamps, container applications such as container caps, protective ventilation applications for electronic devices including small terminals such as tablet terminals and mobile phones, medical ventilation applications, etc.
[0105] Liquid Filtration Semiconductor liquid filtration filters (for semiconductor manufacturing), hydrophilic PTFE filters (for semiconductor manufacturing), chemical filters (for chemical liquid treatment), pure water production line filters (for pure water production), backwash type liquid filtration filters (for industrial wastewater treatment), etc.
[0106] General consumer goods field Clothing, cable guides (movable wires for motorcycles), motorcycle clothing, cast liners (medical supporters), vacuum cleaner filters, bagpipes (musical instruments), cables (signal cables for guitars, etc.), strings (for stringed instruments), etc.
[0107] Textiles PTFE fiber (textile material), sewing thread (textile), weaving thread (textile), rope, etc.
[0108] Medical field Internal implants (extended products), artificial blood vessels, catheters, general surgery (tissue reinforcement materials), head and neck products (dura substitutes), oral health (tissue regenerative medicine), orthopedics (bandages), etc.
[0109] The first, second and third modified PTFEs can also be suitably used as various additives such as dust-proof additives, drip prevention agents and battery binders, in coating applications and in glass cloth impregnation processing applications. In addition, the aqueous dispersions containing the particles of the first, second and third modified PTFEs can be used in a variety of applications, for example, as a surface coating agent for cooking utensils, or for impregnating glass fiber, carbon fiber, Kevlar (registered trademark) fiber and the like to produce impregnated bodies such as roofing materials, and can also be used to form films by applying the same to an object to be coated and baking it in applications such as high-frequency printed circuit boards, conveyor belts and packing.
[0110] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims. EXAMPLES
[0111] The present disclosure will now be described in more detail with reference to examples, but the present disclosure is not limited to these examples.
[0112] Various physical properties were measured by the following methods.
[0113] Polymer Solids Content 1 g of the modified PTFE aqueous dispersion was dried in a blower dryer at 150° C. for 60 minutes, and the ratio of the mass of the heating residue to the mass (1 g) of the aqueous dispersion was expressed as a percentage.
[0114] Modified Monomer Content The VDF content was determined by the following method. 19 F-NMR was measured. In addition, a thin film disk was produced by pressing the PTFE powder, and the infrared absorbance measured by FT-IR was 1429 cm -1 / 2360cm -1 The absorbance ratio was calculated. 19 A calibration curve was prepared from the F-NMR measurements and the above absorbance ratios, and the VDF content was calculated from this calibration curve. The HFP content was determined by press-molding PTFE powder to create a thin-film disk, and the infrared absorbance of the thin-film disk was measured by FT-IR. -1 Absorbance at / 935cm -1 The absorbance ratio was calculated by multiplying the absorbance ratio at The CTFE content was determined by press-molding PTFE powder to create a thin film disk, measuring the infrared absorbance of the thin film disk by FT-IR, and determining the CTFE content at 957 cm -1 Absorbance / 2360cm -1 The absorbance ratio was calculated by multiplying the absorbance by 0.58.
[0115] Standard specific gravity (SSG) The measurements were made using samples formed in accordance with ASTM D 4895 and by the water displacement method in accordance with ASTM D 792.
[0116] Average primary particle size The modified PTFE aqueous dispersion was diluted with water to a solid content concentration of 0.15% by mass, and the transmittance of the 550 nm projected light relative to the unit length of the obtained diluted latex and the number-based length average particle diameter determined by measuring a specific direction using a transmission electron microscope photograph were measured to create a calibration curve. Using this calibration curve, the number-average particle diameter was determined from the measured transmittance of the 550 nm projected light of each sample, and was taken as the average primary particle diameter.
[0117] Extrusion Pressure 21.7 g of lubricant (trade name: Isopar H (registered trademark), manufactured by Exxon Corp.) was added to 100 g of modified PTFE powder, and mixed at room temperature for 3 minutes to obtain a PTFE fine powder mixture. The obtained PTFE fine powder mixture was then left at room temperature (25°C) for at least 1 hour before extrusion, and then paste extruded at room temperature through an orifice (diameter 2.5 mm, land length 11 mm, introduction angle 30°) at a reduction ratio of 100:1 (ratio of cross-sectional area of the inlet and outlet of the die) to obtain a uniform bead (beading; extrusion molded body). The extrusion speed, i.e., the ram speed, was 20 inches / min (51 cm / min). The extrusion pressure was determined by measuring the load when the extrusion load reached equilibrium in the paste extrusion and dividing it by the cross-sectional area of the cylinder used for paste extrusion.
[0118] Extension test The bead obtained by the above paste extrusion was heated at 230°C for 30 minutes to remove the lubricant from the bead. The bead (extrudate) was then cut to the appropriate length, clamped at each end with a clamp distance of 2.0 inches (51 mm) between the clamps, and heated to 300°C in an air circulating oven. The clamps were then moved apart at a desired speed (stretch rate) until a separation distance corresponding to the desired stretch (total stretch) was achieved, and stretch testing was performed. The stretching method essentially follows that disclosed in U.S. Pat. No. 4,576,869, except for the extrusion speed (51 cm / min instead of 84 cm / min). "Stretch" is the increase in length due to drawing, and is usually expressed in relation to the original length. In the above preparation method, the stretch rate is 100% / sec and the total stretch is 2400%.
[0119] Breaking Strength The stretched bead (produced by stretching the bead) obtained in the above stretching test was clamped and fixed in a movable jaw having a gauge length of 5.0 cm, and a tensile test was performed at 25°C and a speed of 300 mm / min, and the strength at the time of break was measured as the breaking strength.
[0120] strength ratio It was calculated by breaking strength (N) / extrusion pressure (MPa).
[0121] Synthesis Example 1 A white solid A was obtained by the method described in Synthesis Example 1 of WO 2021 / 045228.
[0122] Example 1 In a 6L stainless steel reactor equipped with a stirrer, 3600g of deionized water, 180g of paraffin wax, 5.4g of white solid A, and 0.0265g of oxalic acid were placed. The contents of the reactor were then heated to 70°C while being aspirated, and purged with tetrafluoroethylene (TFE) to remove oxygen from the reactor, and the contents were stirred. 1.70g of vinylidene fluoride (VDF) was pressurized into the reactor with TFE, and TFE was then added to make the pressure 2.70MPaG. An aqueous solution of potassium permanganate, in which 3.4mg of potassium permanganate was dissolved in deionized water, was continuously added to the reactor as an initiator. After the injection of the initiator, a drop in pressure occurred and the start of polymerization was observed. TFE was added to the reactor to keep the pressure constant at 2.70MPaG. When the amount of TFE charged reached 430g, the charging of the aqueous potassium permanganate solution was stopped. When the amount of TFE charged reached 1815 g, the supply of TFE was stopped, stirring was stopped, and the reaction was terminated. After that, the pressure in the reactor was evacuated until it reached normal pressure, and nitrogen replacement was performed, and the contents were removed from the reactor and cooled. The paraffin wax was removed to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 33.3 mass%, and the average primary particle size was 251 nm. The obtained PTFE aqueous dispersion was diluted to a solid content concentration of 13% by mass and coagulated by vigorously stirring in a container equipped with a stirrer. The coagulated wet powder was taken out and dried at 210°C for 18 hours to obtain a PTFE powder. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0123] Example 2 Polymerization was carried out under the same conditions as in Example 1, except that the amount of VDF charged was changed to 0.4 g, the amount of potassium permanganate was changed from 3.4 mg to 5.6 mg, and the charging of the aqueous potassium permanganate solution was stopped when the amount of TFE charged reached 870 g. The solid content concentration of the obtained aqueous PTFE dispersion was 33.4 mass%, and the average primary particle size was 263 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 1. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0124] Example 3 The same conditions as in Example 1 were used except that the VDF charge amount was changed to 2.56 g, the potassium permanganate to 3.7 mg, and when the TFE charge amount reached 430 g, stirring was stopped and the inside of the polymerization tank was depressurized to atmospheric pressure, and then TFE was introduced to set the pressure to 2.7 MPaG and stirring was resumed. The solid content concentration of the obtained PTFE aqueous dispersion was 33.9 mass%, and the average primary particle size was 246 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 1. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0125] Example 4 Polymerization was carried out under the same conditions as in Example 1, except that the amount of VDF charged was changed to 32.0 g and the amount of potassium permanganate was changed from 3.4 mg to 3.9 mg. The solid content concentration of the obtained PTFE aqueous dispersion was 33.5 mass%, and the average primary particle diameter was 224 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 1. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0126] Example 5 In a 6L stainless steel reactor equipped with a stirrer, 3600g of deionized water, 180g of paraffin wax, and 5.4g of white solid A were placed. The reactor contents were then heated to 80°C while being aspirated, and purged with tetrafluoroethylene (TFE) to remove oxygen from the reactor, and the contents were stirred. 5.82g of vinylidene fluoride (VDF) was pressurized into the reactor with TFE, and TFE was then added to bring the pressure to 2.70MPaG. An aqueous solution of 7.2mg of ammonium persulfate (APS) dissolved in deionized water as an initiator was added to the reactor. After the initiator was injected, a pressure drop occurred and the start of polymerization was observed. TFE was added to the reactor to keep the pressure constant at 2.70MPaG. When the amount of TFE charged reached 430g, an aqueous solution of 36.0mg of hydroquinone dissolved in deionized water was added. When the amount of TFE charged reached 1580 g, the supply of TFE was stopped, stirring was stopped, and the reaction was terminated. After that, the pressure in the reactor was evacuated until it reached normal pressure, and nitrogen replacement was performed, and the contents were removed from the reactor and cooled. The paraffin wax was removed to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 30.2 mass%, and the average primary particle size was 214 nm. The obtained PTFE aqueous dispersion was diluted to a solid content concentration of 13% by mass and coagulated by vigorously stirring in a container equipped with a stirrer. The coagulated wet powder was taken out and dried at 210°C for 18 hours to obtain a PTFE powder. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0127] Example 6 Polymerization was carried out under the same conditions as in Example 5, except that the amount of VDF charged was changed to 3.1 g and the amount of hydroquinone charged was changed to 18.2 mg, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 30.3 mass%, and the average primary particle size was 223 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 5. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0128] Example 7 Polymerization was carried out under the same conditions as in Example 5, except that the amount of VDF charged was changed to 0.19 g and the amount of hydroquinone charged was changed to 11.0 mg, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 30.3 mass%, and the average primary particle size was 265 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 5. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0129] Example 8 Polymerization was carried out under the same conditions as in Example 5, except that the amount of VDF charged was changed to 0.36 g, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 29.8 mass%, and the average primary particle size was 261 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 5. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0130] Example 9 Polymerization was carried out under the same conditions as in Example 5, except that the VDF charge amount was changed to 2.1 g, the hydroquinone charge amount was changed to 18.0 mg, and stirring was stopped when the TFE charge amount reached 430 g, the inside of the polymerization tank was depressurized to atmospheric pressure, and then TFE was introduced and stirring was resumed under a pressure of 2.7 MPaG. The solid content concentration of the obtained PTFE aqueous dispersion was 30.3 mass%, and the average primary particle size was 226 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 5. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0131] Example 10 Polymerization was carried out under the same conditions as in Example 5, except that the VDF was changed to 0.52 g, the ammonium persulfate (APS) to 15.4 mg, the amount of hydroquinone charged to 17.9 mg, the polymerization pressure was changed to 0.80 MPa, the polymerization temperature was changed to 70° C., and the final amount of TFE was changed to 1520 g, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 29.8 mass%, and the average primary particle size was 278 nm. The obtained PTFE aqueous dispersion was used to coagulate in the same manner as in Example 5, and the resulting wet powder was taken out and dried at 180° C. for 18 hours to obtain a PTFE powder. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0132] Example 11 Polymerization was carried out under the same conditions as in Example 1, except that VDF was changed to 1.28 g of CTFE, the amount of potassium permanganate charged was changed to 3.87 mg, and the final amount of TFE was changed to 1790 g, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 33.0 mass%, and the average primary particle size was 263 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 1. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0133] Example 12 Polymerization was carried out under the same conditions as in Example 1, except that VDF was changed to 2.60 g of CTFE and the final amount of TFE was changed to 1660 g, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 31.4 mass%, and the average primary particle size was 248 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 1. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0134] Example 13 Polymerization was carried out under the same conditions as in Example 5, except that VDF was changed to 0.11 g of HFP, ammonium persulfate (APS) was changed to 15.4 mg, the amount of hydroquinone charged was changed to 17.9 mg, the polymerization pressure was changed to 0.80 MPa, the polymerization temperature was changed to 70° C., and the final amount of TFE was changed to 1540 g, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 29.8 mass%, and the average primary particle size was 312 nm. The obtained PTFE aqueous dispersion was used to coagulate in the same manner as in Example 5, and the resulting wet powder was taken out and dried at 180° C. for 18 hours to obtain a PTFE powder. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0135] Comparative Example 1 Polymerization was carried out under the same conditions as in Example 1, except that the amount of VDF charged was changed to 55.7 g and the amount of potassium permanganate charged was changed to 4.46 mg, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 33.1 mass%, and the average primary particle diameter was 224 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 1. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1. Furthermore, a sample formed in accordance with ASTM D 4895 using the obtained PTFE powder was subjected to heat treatment at 380° C. for 6 hours, and when it was cooled to room temperature, the sample showed severe foaming.
[0136] Comparative Example 2 Polymerization was carried out under the same conditions as in Example 1, except that VDF was not charged, the amount of white solid A charged was changed to 13 g, the amount of succinic acid charged was changed to 0.108 g, the amount of potassium permanganate charged was changed to 3.5 mg, and the final amount of TFE was changed to 1500 g, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 29.5 mass%, and the average primary particle size was 380 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 1. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.
[0137] [Table 1]
[0138] Crack limit film thickness Approximately 5 ml of PTFE aqueous dispersion was dropped onto an aluminum plate measuring 20 cm long x 10 cm wide x 1.5 mm thick, and flow-coated, then air-dried using an inclined plate at approximately 80 degrees, dried at 110°C for 15 minutes, and baked at 380°C for 15 minutes to produce a PTFE coating. The film thickness at the crack occurrence location confirmed by microscopic observation was measured with an eddy current film thickness meter (SWT-9100, manufactured by Sanko Electronics Laboratory). The average value of 10 measurements on each of the two coating plates was taken as the crack limit film thickness.
[0139] Example 14 In a 6L stainless steel reactor equipped with a stirrer, 3600g of deionized water, 180g of paraffin wax, and 1.18g of white solid A were placed. The reactor contents were then heated to 80°C while being aspirated, and purged with tetrafluoroethylene (TFE) to remove oxygen from the reactor, and the contents were stirred. 5.82g of vinylidene fluoride (VDF) was pressurized into the reactor with TFE, and TFE was then added to make the pressure 2.70MPaG. An aqueous solution of 7.2mg of ammonium persulfate (APS) dissolved in deionized water as an initiator was added to the reactor. After the initiator was injected, a pressure drop occurred and the start of polymerization was observed. TFE was added to the reactor to keep the pressure constant at 2.70MPaG. When the amount of TFE charged reached 460g, an aqueous solution of 25.0mg of hydroquinone dissolved in deionized water and a deionized aqueous solution of 3.24g of white solid A dissolved therein were added. When the amount of TFE charged reached about 1950 g, the supply of TFE was stopped, stirring was stopped, and the reaction was terminated. After that, the pressure in the reactor was evacuated until it reached normal pressure, and nitrogen replacement was performed, and the contents were removed from the reactor and cooled. The paraffin wax was removed to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 35.3 mass%, and the average primary particle size was 263 nm. Pure water was added to the obtained aqueous dispersion and stirred at high speed to obtain a wet PTFE powder. The obtained wet PTFE powder was dried at 150°C for 18 hours to obtain a PTFE powder. The SSG of the obtained PTFE was 2.228 and the VDF content was 0.049% by mass. To 1000 g of the obtained PTFE aqueous dispersion, 40 g of surfactant TDS-80 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene alkyl ether) and 160 g of pure water were added, and the mixture was left to stand at 70°C to obtain a PTFE aqueous dispersion concentrate having a PTFE resin solid content concentration of 65 mass% or more. To this, surfactant TDS-120 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene alkyl ether) and pure water were added to prepare a modified PTFE aqueous dispersion composition having a modified PTFE resin solid content concentration of 63 mass% and a surfactant amount of 5 mass% relative to the modified PTFE. The obtained modified PTFE aqueous dispersion composition had a crack limit film thickness of 4 μm.
Claims
1. A modified polytetrafluoroethylene having a breaking strength of more than 32.8 N and a standard specific gravity of 2.150 or more.
2. The modified polytetrafluoroethylene according to claim 1, having a strength ratio expressed as breaking strength (N) / extrusion pressure (MPa) of more than 1.90 N / MPa.
3. The modified polytetrafluoroethylene according to claim 1 or 2, having a breaking strength of more than 37.0 N.
4. 3. The modified polytetrafluoroethylene according to claim 1, having a standard specific gravity of 2.155 or more.
5. 3. The modified polytetrafluoroethylene according to claim 1, having a standard specific gravity of 2.160 or more.
6. A modified polytetrafluoroethylene having a standard specific gravity of 2.150 or more and a strength ratio expressed as breaking strength (N) / extrusion pressure (MPa) of more than 1.90 N / MPa.
7. A modified polytetrafluoroethylene comprising tetrafluoroethylene units and vinylidene fluoride units, the amount of said vinylidene fluoride units being 1.0 mass% or less based on the total polymerized units.
8. The modified polytetrafluoroethylene according to claim 1 or 2, in the form of a powder.
9. The modified polytetrafluoroethylene according to claim 1 or 2, which is in the form of a fine powder.
10. 3. An aqueous dispersion comprising particles of the modified polytetrafluoroethylene according to claim 1 or 2.
Citation Information
Patent Citations
Tetrafluoroethylene polymer having excellent strength
JP2002201217A
Modified polytetrafluoroethylene and method for producing the same
JP2006117912A