Aromatic polyamide film and diaphragm including the same

Aromatic polyamide films with controlled thickness and modulus are produced to prevent curling and slack during transportation and lamination, achieving wrinkle-free and streak-free films with enhanced mechanical properties.

JP2024164586AInactive Publication Date: 2024-11-27TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023080182
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-27
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Thin aromatic polyamide films with high strength face issues of curling and slack during transportation and lamination due to increased transport tension, which can lead to wrinkles and streaks, and existing methods for thickness control are inadequate for films thinner than 3 μm.

Method used

Aromatic polyamide films with a thickness of 2 μm or more and less than 3 μm, Young's modulus of 8 GPa or more and 20 GPa or less, and controlled thickness unevenness in the width direction of 0.05 μm or less, achieved through precise lamination and stretching processes.

Benefits of technology

The solution prevents curling and slack during transportation and lamination, ensuring wrinkle-free and streak-free films with improved mechanical properties and dimensional stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164586000001
    Figure 2024164586000001
  • Figure 2024164586000002
    Figure 2024164586000002
  • Figure 2024164586000003
    Figure 2024164586000003
Patent Text Reader

Abstract

To provide an aromatic polyamide film that prevents slack during transportation without requiring higher transport tension in lamination and other processes, and also reduces wrinkles and streaks during lamination.SOLUTION: An aromatic polyamide film for metal foil lamination has a film thickness of 2 μm or more and less than 3 μm and a Young's modulus of 8 GPa or more and 20 GPa or less in both the longitudinal and width directions, where the thickness variation in the width direction is 0.05 μm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an industrial thin film having excellent transportability and processability, which is supplied for various industrial uses. [Background technology]

[0002] Aromatic polyamides, especially those made of para-oriented aromatics, have high mechanical properties such as rigidity and strength, and are very advantageous for thin film production, so they are used as magnetic recording media. They also have heat resistance second only to polyimides, so they are used in industrial materials such as heat-resistant processing paper, flexible circuit boards, speaker diaphragms, and capacitors.

[0003] In industrial material applications, the film may be coated with a resin and then laminated to another substrate. If the aromatic polyamide film is loose, wrinkles or streaks may occur during lamination.

[0004] In general, increasing the transport tension is effective in suppressing slack in the film. However, in the case of a thin aromatic polyamide film having high strength, increasing the transport tension may cause curling of the film after lamination, which may affect the quality.

[0005] It is known that sagging of a film is caused by uneven thickness.

[0006] A method for suppressing thickness unevenness in aromatic polyamide films is known in which the closest distance between the die and the support is set to 1.6 mm or less (Patent Document 1). Another known method involves measuring the diameter of a film roll wound around a cylindrical core in the roll width direction, determining the thickness per film sheet, and adjusting a thickness adjustment bolt so that the thickness falls within a specified range.

[0007] However, the aromatic polyamide films disclosed in Patent Documents 1 and 2 have a thickness of 3 μm or more, and when a thin film with a thickness of less than 3 μm is used, it may not be possible to produce it with good productivity by bonding it with other materials. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2002-210820 A [Patent Document 2] JP 2001-023160 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention aims to provide a thin aromatic polyamide film that takes advantage of the excellent heat resistance of aromatic polyamides, is less likely to sag during transport even without increasing the transport tension in a lamination process or the like, and can suppress wrinkles and streaks when laminated. [Means for solving the problem]

[0010] In order to solve such problems, the present invention comprises the following configuration.

[0011] An aromatic polyamide film for metal foil lamination, characterized in that the thickness of the film is 2 μm or more and less than 3 μm, and the Young's modulus in the longitudinal and transverse directions is 8 GPa or more and 20 GPa or less, respectively, and the thickness unevenness in the transverse direction is 0.05 μm or less. Effect of the Invention

[0012] The aromatic polyamide film of the present invention takes advantage of the excellent heat resistance of aromatic polyamides, and can provide a thin aromatic polyamide film that is less likely to sag during transport even without increasing the transport tension, and can suppress wrinkles and streaks when laminated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below together with preferred embodiments, but the present invention is not limited thereto. The aromatic polyamide film of the present invention preferably has repeating units represented by the following chemical formula (1) and / or chemical formula (2), for example.

[0014] [ka]

[0015] [ka]

[0016] Here, examples of the groups Ar1, Ar2, and Ar3 include those represented by the following chemical formula (3).

[0017] [ka]

[0018] The X and Y groups are selected from, but are not limited to, -O-, -CH2-, -CO-, -CO2-, -S-, -SO2-, -C(CH3)2-, etc. Furthermore, those in which some of the hydrogen atoms on these aromatic rings are substituted with a halogen group (especially chlorine) such as fluorine, bromine, or chlorine, a nitro group, an alkyl group (especially methyl group) such as methyl, ethyl, or propyl, or an alkoxy group such as methoxy, ethoxy, or propoxy, etc., are preferred because they reduce the moisture absorption rate and reduce dimensional changes due to humidity changes. In addition, hydrogen in the amide bond constituting the polymer may be substituted with another substituent. In the aromatic polyamide used in the present invention, it is preferable that the aromatic rings having the above-mentioned para orientation occupy 80 mol % or more, more preferably 90 mol % or more of the total aromatic rings. The para orientation referred to here means a state in which the divalent bonds constituting the main chain on the aromatic ring are coaxial or parallel to each other. If the para orientation is less than 80 mol %, the rigidity and heat resistance of the film may be insufficient. Furthermore, when the aromatic polyamide contains 60 mol % or more of the repeating unit represented by the following chemical formula (4), the stretchability and film properties are particularly excellent, which is preferable.

[0019] [ka]

[0020] Furthermore, the film of the present invention has an average light transmittance of 70% or more and 100% or less in the wavelength range of 400 nm to 750 nm, which suppresses the yellowish tinge of the film, making it preferable as a glass replacement.

[0021] In order to make the average light transmittance in the wavelength range of 400 nm to 750 nm 70% or more and 100% or less, it is preferable to have a structural unit represented by any one of the following chemical formulas (5) to (9).

[0022] [ka]

[0023] R1 , R 2 is -H, an aliphatic group having 1 to 5 carbon atoms, -CF3, -CCl3, -OH, -F, -Cl, -Br, -OCH3, a silyl group, or a group containing an aromatic ring, preferably -CF3, -F, -Cl, or a group containing an aromatic ring.

[0024] [ka]

[0025] R 3 is a group containing Si, a group containing P, a group containing S, a halogenated hydrocarbon group, a group containing an aromatic ring, or a group containing an ether bond (however, structural units having these groups may be present in the molecule).Preferably, it is a group containing Si, a halogenated hydrocarbon group, a group containing an aromatic ring, or a group containing an ether bond.

[0026] [ka]

[0027] R 4 is any group. Although not particularly limited, it is preferably -H, -Cl, or -F.

[0028] [ka]

[0029] R 5 is any aromatic group or any alicyclic group. Although not particularly limited, more preferred are phenyl, biphenyl, cyclohexane, and decalin.

[0030] Furthermore, among the above, when the structural unit represented by chemical formula (5) or (6) is present, a thin film having excellent rigidity is easily obtained, and an intermediate layer is easily formed, so that excellent surface hardness, impact resistance, and flex resistance can be easily achieved after the cured layer is provided.

[0031] Among the above, it is particularly preferable that the compound has a structural unit represented by the following chemical formula (9).

[0032] [ka]

[0033] R 6 is any group. Although not particularly limited, it is preferably -H, -Cl, or -F.

[0034] The structural unit represented by the above chemical formula (9) preferably accounts for 20 to 100 mol %, more preferably 50 to 100 mol %, and further preferably 80 to 100 mol %, of the aromatic nitrogen-containing polymer constituting the film of the present invention.

[0035] Regarding the method for producing the film of the present invention, an aromatic polyamide film will be exemplified below, but the present invention is not limited thereto.

[0036] For example, when an aromatic polyamide is obtained from an acid chloride and a diamine, it is synthesized by solution polymerization in an aprotic organic polar solvent such as N-methylpyrrolidone (NMP), dimethylacetamide (DMAc), or dimethylformamide (DMF), or by interfacial polymerization using an aqueous medium. When an acid chloride and a diamine are used as monomers in a polymer solution, hydrogen chloride is by-produced, and to neutralize this, inorganic neutralizing agents such as calcium hydroxide, calcium carbonate, or lithium carbonate, or organic neutralizing agents such as ethylene oxide, propylene oxide, ammonia, triethylamine, triethanolamine, or diethanolamine are used. When an aromatic polyamide is obtained from the reaction of an isocyanate with a carboxylic acid, the reaction is carried out in an aprotic organic polar solvent in the presence of a catalyst.

[0037] These polymer solutions may be used as they are as a membrane-forming stock solution, or the polymer may be isolated and then redissolved in the above-mentioned organic solvents or an inorganic solvent such as sulfuric acid to prepare a membrane-forming stock solution.

[0038] To obtain the aromatic polyamide film of the present invention, the intrinsic viscosity ηjnh of the polymer (a value measured at 30° C. by dissolving 0.5 g of the polymer in 100 ml of 98% sulfuric acid) is preferably 0.5 (dl / g) or more.

[0039] The method of adding the particles includes a method in which the particles are sufficiently slurried in a solvent in advance and then used as a polymerization solvent or dilution solvent, and a method in which the particles are directly added to a film-forming stock solution prepared.

[0040] In some cases, inorganic salts such as calcium chloride, magnesium chloride, lithium chloride, and lithium nitrate may be added to the film-forming solution as a dissolving aid. The film-forming solution may be the neutralized polymer solution as it is, or the polymer may be isolated and then redissolved in a solvent. As the solvent, organic polar solvents such as N-methyl-2-pyrrolidone, dimethylacetamide, and dimethylformamide are preferred because they are easy to handle, but strong acidic solvents such as concentrated sulfuric acid, concentrated nitric acid, and polyphosphoric acid may also be used. The polymer concentration in the film-forming solution is preferably about 2 to 40% by mass.

[0041] The film-forming solution prepared as described above is formed into a film by a so-called solution film-forming method. Solution film-forming methods include a dry-wet method, a dry method, and a wet method. When inorganic salts are contained in the polymer solution, a wet process is required to extract the salts, and therefore the dry-wet method is used.

[0042] When forming a film by a dry-wet method, the raw solution is extruded from a die onto an endless belt as a support to form a sheet, and then the solvent is evaporated from the sheet, and the sheet is dried until the polymer concentration (PC) reaches 35 to 60% by mass, at which the sheet has self-supporting properties. The sheet that has completed the dry process is cooled, peeled off from the support, and introduced into a wet bath in the next wet process, where desalting and desolvation are performed. The composition of the wet bath is not particularly limited as long as it is a poor solvent for the polymer, but water or a mixed system of organic solvent / water can be used. In this case, in order to reduce impurities in the sheet, the composition ratio of the organic solvent / water mixed system (the following values ​​are based on mass) is organic solvent / water = 70 / 30 to 0 / 100, but preferably 60 / 40 to 30 / 70, and the bath temperature is preferably 40°C or higher. The wet bath may contain inorganic salts, but it is preferable to finally extract the solvent and inorganic salts contained in the sheet with a large amount of water.

[0043] The sheet that has passed through the wet process is then dried and heat-treated in a tenter, and it is preferable to dry the sheet until the solvent content in the sheet is less than 5% by mass before heat-treatment in the tenter. If the sheet is subjected to the heat-treatment process with a solvent content of 5% by mass or more, unevenness in the heat treatment is likely to occur, resulting in uneven physical properties in the film width direction and making the sheet more likely to break during the stretching process. It is more preferable that the solvent content is low, and it is desirable to completely dry the sheet to approximately 0% by mass.

[0044] The sheet formed as described above is stretched in the wet process to improve the mechanical properties and dimensional stability of the sheet during the heat treatment process. The stretching can be performed by first stretching in the longitudinal direction of the sheet and then in the width direction, or by stretching in the width direction and then in the longitudinal direction in a sequential biaxial stretching method, or by stretching in the longitudinal direction and the width direction at the same time in a simultaneous biaxial stretching method. These stretching methods are well known as stretching methods in melt film formation performed in the production of films of polyethylene, polypropylene, polyester, etc., but in the case of a film obtained by solution film formation as in the present invention, the sheet contains solvents and wet bath components, and the process involves the movement of these components outside the sheet, so it is preferable to adopt the method described below in order to obtain the desired film.

[0045] As the stretching method, the sequential biaxial stretching method is preferred from the viewpoint of the apparatus and operability. As the stretching conditions, it is necessary to select appropriate conditions depending on the polymer composition, etc., but it is preferable that the stretching ratio in the longitudinal direction of the sheet is 1.0 to 1.5 times and the stretching ratio in the transverse direction is 1.1 to 2.0 times in order to obtain the desired dimensional stability. In addition, the stretching temperature is preferably 270 ° C or more for 3 seconds or more, and more preferably 270 to 320 ° C for 3 seconds or more. If the stretching temperature is less than 270 ° C, crystallization is insufficient, and sufficient dimensional properties such as moisture absorption rate and tensile strength may not be obtained. Note that, if the stretching temperature exceeds 320 ° C, the crystallization degree increases too much, making the film brittle and the film prone to tearing. In addition, the solvent content in the sheet during stretching is preferably less than 5 mass %. Note that it is effective to slowly cool the film after stretching or heat treatment, and cooling at a rate of 50 ° C / sec or less is effective in reducing the thermal shrinkage rate. By adjusting the above-mentioned stretching ratio, etc., the Young's modulus can be adjusted to 8 to 20 GPa.

[0046] The aromatic polyamide film of the present invention may be a single-layer film, but may also be a laminated film. For example, in the case of two layers, a method of dividing a polymerized aromatic polyamide solution into two, adding different particles to each, and then laminating them is one example. The same applies to the case of three or more layers. Examples of these lamination methods include lamination in a die, lamination in a composite pipe, and a method of forming one layer first and then forming another layer on it.

[0047] It is important that the thickness unevenness in the width direction of the aromatic polyamide film of the present invention is 0.05 μm or less. If the thickness unevenness exceeds 0.05 μm, slackness may occur during low tension conveyance of 5 N, and wrinkles or streaks may occur during lamination. More preferably, the thickness unevenness is 0.03 μm or less.

[0048] In order to obtain a thickness and widthwise thickness variation of 0.05 μm or less for the aromatic polyamide film of the present invention, it is preferable that the lip gap of the die is 1.0 mm on average, and the thickness can be made 2 to 3 μm by adjusting this lip gap. In order to obtain the above-mentioned thickness variation, it is preferable that the ON rate difference between adjacent bolts in the heat bolts of the automatic die that adjusts the lip gap is |5%| or less.

[0049] If the ON rate difference between adjacent heat bolts of the automatic cap exceeds |5%|, it is not preferable because the thickness unevenness in the width direction may exceed 0.05 μm. More preferably, the ON rate difference between adjacent heat bolts of the automatic cap is |3%| or less. EXAMPLES

[0050] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.

[0051] (Film thickness X) Using a high-precision digital micrometer MDH-25MB (manufactured by Mitutoyo Corporation), measurements were taken at 10 mm intervals in the direction perpendicular to the film transport direction (MD) with 10 sheets stacked together, excluding 50 mm from the edge portions, and the average value divided by the number of sheets stacked was taken as the film thickness.

[0052] (Thickness unevenness R) Using a high-precision digital micrometer MDH-25MB (manufactured by Mitutoyo Corporation), measurements were taken at 10 mm intervals in the direction perpendicular to the film transport direction (MD) with 10 sheets stacked together, excluding 50 mm from the edge portions, and the value was divided by the number of sheets stacked together. The difference between the maximum and minimum measured values ​​obtained was rounded off to two decimal places to determine the thickness unevenness.

[0053] (Young's Modulus) The film was divided into 5 parts in the width direction, and 5 film samples, each 10 mm wide, were taken from the center of each part so that the length in the measurement direction was 150 mm in both the longitudinal and transverse directions of the film.

[0054] Using an Orientec Robot Tensilon RTF-1210, the collected films were set in the device with a chuck distance of 100 mm, and a tensile test was performed under conditions of a tensile speed of 200 mm / min, a temperature of 23°C, and a relative humidity of 65%. The longitudinal Young's modulus and transverse Young's modulus were calculated from the tangent to the rising part of the obtained load-elongation curve, and the average value was used for evaluation.

[0055] (Talmi Evaluation) The aromatic polyamide film was unwound from the roll with a tension of 30 N / m, and the tension of the film subjected to tension between the rolls was evaluated using the following index. ○: No sagging △: Slight localized sagging ×: Sagging

[0056] (Aromatic polyamide solution A) 85 mol % of 2-chloroparaphenylenediamine (hereinafter, CPA) and 15 mol % of diphenyl ether (hereinafter, DPE) were dissolved in N-methyl-2-pyrrolidone (hereinafter, NMP), and the solution was filtered through a polypropylene filter with a filtration accuracy of 1.0 μm, and then transferred to a polymerization tank. 98.5 mol % of chloroterephthalic acid chloride (hereinafter, CTPC) that had been passed through a polypropylene filter with a filtration accuracy of 1.0 μm was added to this, and before polymerization, silica particles with an average particle size of 80 nm were added so as to be 0.02 mass % relative to the aromatic diamine component, and organic particles with an average particle size of 100 nm were added so as to be 6.0 mass % relative to the aromatic diamine component, and the mixture was stirred at 30° C. or less for 2 hours to obtain a polymerized polymer.

[0057] Next, 98.5 mol% lithium carbonate was added to the hydrogen chloride in the polymer and neutralized for 4 hours, and 10 mol% triethanolamine was added to the hydrogen chloride in the polymer and stirred for 1 hour to obtain an aromatic polyamide solution A with a polymer concentration of 10.8 mass%.

[0058] (Aromatic polyamide solution B) 85 mol % of CPA and 15 mol % of DPE were dissolved in NMP, and the solution was filtered through a polypropylene filter with a filtration accuracy of 1.0 μm and then transferred to a polymerization tank. 98.5 mol % of CTPC that had been passed through a polypropylene filter with a filtration accuracy of 1.0 μm was added to the solution, and the mixture was stirred at 30° C. or less for 2 hours to obtain a polymerized polymer.

[0059] Next, 98.5 mol% of lithium carbonate was added to the hydrogen chloride in the polymer and neutralized for 4 hours, and then 1.6 mass% of silica having an average primary particle size of 16 nm ("AEROSIL" R972 type manufactured by Nippon Aerosil Co., Ltd.) was added to the polymer and stirred for 1 hour. After that, 10 mol% of triethanolamine was added to the hydrogen chloride in the polymer and stirred for 1 hour to obtain an aromatic polyamide solution B with a polymer concentration of 10.8 mass%.

[0060] Example 1 Aromatic polyamide solution A was passed through a stainless steel metal fiber filter with a filtration accuracy of 1.2 μm, and aromatic polyamide solution B was passed through a stainless steel metal fiber filter with a filtration accuracy of 5.0 μm, and then laminated inside the die. The lamination ratio (thickness ratio) of aromatic polyamide solutions A and B was set to 50% each. The lip gap of the nozzle was 1.0 mm on average, and the ON rate difference between adjacent bolts of the automatic nozzle heat bolts was set to |3%| or less.

[0061] Next, the laminated polymer solution was cast onto a stainless steel belt with a mirror-like surface, and the belt was heated with hot air at 180°C for 2 minutes on the downstream side of the spinneret in the running direction to evaporate the solvent, and the self-supporting film was continuously peeled off from the belt. At this time, the layer in contact with the stainless steel belt was laminated so that aromatic polyamide solution B was the layer.

[0062] Next, the membrane was introduced into a tank of a solvent extraction treatment device, and stretched 1.08 times in the MD direction while extracting the remaining solvent and inorganic salts produced by neutralization with water.

[0063] The obtained film was then held by the clips of a transverse stretching machine to dry off moisture and heat-treat, and then dried and heat-treated at 280°C for 1.5 minutes and stretched 1.14 times in the TD direction. It was then gradually cooled at a rate of 20°C / sec, the film edges were removed, and the film was wound up on a core with an oscillation of 60 mm to obtain a jumbo roll of aromatic polyamide film with an average thickness of 2.4 μm.

[0064] Next, the film was slit into a narrow width (660 mm) using a slitter at a winding speed of 30 m / min, a winding surface pressure of 200 N / m, and a winding tension of 100 N / m, and wound in a roll onto a cylindrical core of fiber reinforced plastic (FWP) core A (manufactured by Tenryu Kogyo Co., Ltd.) FWP10 having a cylindricity of 0.05 mm, a width direction elastic modulus of 14.5 GPa, a bending strength of 210 MPa, a surface hardness of 85, an outer diameter of 167 mm, and an inner diameter of 152.5 mm, with the aromatic polyamide solution A on the inner surface of the winding, and an aromatic polyamide film in which the film was wound onto the cylindrical core was obtained. The results are shown in Table 1.

[0065] [Table 1]

[0066] Example 2 The same procedure as in Example 1 was carried out except that the average thickness was set to 2.3 μm.

[0067] The results are shown in Table 1.

[0068] Example 3 The same procedure as in Example 1 was carried out, except that the difference in ON rate between adjacent bolts of the automatic mouthpiece was set to |5%| or less.

[0069] The results are shown in Table 1.

[0070] Comparative Example 1 The same procedure as in Example 1 was carried out, except that the difference in ON rate between adjacent bolts of the automatic mouthpiece was set to |8%| or less.

[0071] The results are shown in Table 1.

[0072] Comparative Example 2 The same procedure as in Example 1 was carried out, except that the difference in ON rate between adjacent bolts of the automatic mouthpiece was set to |10%| or less.

[0073] The results are shown in Table 1.

[0074] Comparative Example 3 The same procedure as in Example 1 was carried out except that the average thickness was set to 2.3 μm and the ON rate difference between adjacent bolts of the automatic nozzle was set to |8%| or less.

[0075] The results are shown in Table 1.

Claims

1. The film thickness is 2 μm or more and less than 3 μm, The Young's modulus in the longitudinal direction and the width direction is 8 GPa or more and 20 GPa or less, respectively. In the aromatic polyamide film, The thickness variation in the width direction is 0.05 μm or less. Aromatic polyamide film for laminating metal foil.

2. A diaphragm comprising the aromatic polyamide film according to claim 1 , at least one surface of which is coated with a resin, and the aromatic polyamide film is laminated to another substrate.

Citation Information

Patent Citations

  • Film roll for magnetic recording medium having high elastic modulus and manufacture of magnetic recording medium

    JP2001023160A

  • Aromatic polyamide film and magnetic recording medium made thereof

    JP2002210820A