Separator for alkaline battery

A nonwoven fabric separator with controlled surface oxidation of polyolefin resin fibers addresses mechanical deterioration, enhancing mechanical strength and electrolyte retention while reducing short circuits in alkaline batteries.

JP2024164587APending Publication Date: 2024-11-27JAPAN VILENE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023080183
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-27

AI Technical Summary

Technical Problem

Alkaline battery separators made of polyolefin resin fibers with sulfonic acid groups suffer from mechanical deterioration due to oxidation, leading to increased risk of internal short circuits.

Method used

A nonwoven fabric separator with fibers coated in polyolefin resin containing sulfonic acid groups, where the surface oxidation is minimized by controlling the percentage of COO peak area and sulfur-to-carbon ratio, ensuring high mechanical strength and hydrophilicity.

Benefits of technology

The separator provides enhanced mechanical strength, reduced self-discharge, and improved electrolyte retention, minimizing internal short circuits and maintaining battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164587000001
    Figure 2024164587000001
Patent Text Reader

Abstract

To provide a separator for an alkaline battery, capable of providing the alkaline battery which has a good mechanical strength, and in which an internal short circuit hardly occurs.SOLUTION: A separator for an alkaline battery of the present invention, measures a front surface of fiber which is coated with a polyolefin resin having a sulfonate group contained in the separator for the alkaline battery, with an XPS, and a percentage of a peak area of COO occupying in a sum of peak areas of each peak (C-C, CO, and COO) obtained by performing a waveform separation of a C1s spectrum to be obtained is small so that it is less than 2.0%. That is, a carboxy group (-COOH) provided in the front surface of the fiber is small, a level of oxidation of the polyolefin resin provided in the front surface of the fiber is small. Therefore, the separator for the alkaline battery having the above construction has a good mechanical strength, and can provide the alkaline battery in which an internal short circuit hardly occurs.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator for alkaline batteries. More specifically, the present invention relates to a separator that can be used in alkaline primary batteries such as alkaline manganese batteries, mercury batteries, silver oxide batteries, and air batteries, and alkaline secondary batteries such as nickel-cadmium batteries, silver-zinc batteries, silver-cadmium batteries, nickel-zinc batteries, nickel-hydrogen batteries, and rechargeable alkaline manganese batteries. In particular, the present invention relates to a separator that can be suitably used in batteries that generate oxygen when overcharged, such as nickel-cadmium batteries and nickel-hydrogen batteries. [Background technology]

[0002] Conventionally, a separator has been provided between the positive and negative electrodes of an alkaline battery to prevent short circuits by separating the positive and negative electrodes, and to hold an electrolyte solution to facilitate electromotive reactions. Since this separator for alkaline batteries needs to hold an electrolyte solution consisting of potassium hydroxide or the like, nonwoven fabrics containing fibers containing polyolefin resins, which have excellent alkali resistance, have been used. However, the fibers have low affinity with the electrolyte solution, and separators containing the fibers have problems of poor electrolyte retention and low ionic conductivity. Therefore, nonwoven fabrics containing fibers containing polyolefin resins have been hydrophilized by various methods to improve the electrolyte retention ability.

[0003] For example, as described in Patent Document 1 (JP 2017-107752 A), the applicant of the present application has proposed introducing sulfonic acid groups into the polyethylene resin by a sulfonation treatment for alkaline battery separators in the form of a nonwoven fabric made of core-sheath type composite fibers containing polyethylene, a polyolefin resin, as a sheath component, i.e., the fiber surface is covered with polyethylene. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-107752 A Summary of the Invention [Problem to be solved by the invention]

[0005] In alkaline battery separators according to such conventional technology, the polyolefin resin contained in the constituent fibers has sulfonic acid groups, which improves electrolyte retention and provides high ionic conductivity, allowing the electromotive reaction of the alkaline battery to proceed smoothly. In addition, the sulfonic acid groups adsorb ammonia contained in the electrolyte, thereby suppressing self-discharge of the alkaline battery.

[0006] However, the sulfonation treatment carried out to introduce sulfonic acid groups can oxidize and deteriorate the constituent fibers of the nonwoven fabric constituting the alkaline battery separator, which can result in a decrease in the mechanical strength of the alkaline battery separator, making it more susceptible to tearing and causing an internal short circuit in the alkaline battery.

[0007] The present invention has been made under these circumstances, and aims to provide an alkaline battery separator that is a nonwoven fabric containing fibers whose surfaces are coated with a polyolefin resin having sulfonic acid groups, and that has excellent mechanical strength and can provide an alkaline battery that is less likely to develop internal short circuits. [Means for solving the problem]

[0008] The invention according to claim 1 of the present invention is "an alkaline battery separator comprising a nonwoven fabric containing fibers whose surfaces are coated with a polyolefin resin having sulfonic acid groups, wherein when the surface of the fibers is measured using XPS (X-ray photoelectron spectroscopy) and the resulting C1s spectrum is subjected to waveform separation, the percentage of the peak area of ​​COO in the total peak area of ​​each peak (CC, CO, COO) obtained is less than 2.0%. "

[0009] The invention according to claim 2 of the present invention is "measurement of the surface of the fiber using XPS (X-ray photoelectron spectroscopy) and the obtained S2p 3 / 2 The separator for an alkaline battery according to claim 1, wherein the percentage of the peak area of ​​-SO3 in the total peak area of ​​each peak (-SO3, -SO4) obtained by waveform separation of the spectrum is 50% or more.

[0010] The invention according to claim 3 of the present invention is characterized in that "the alkaline battery separator is measured using a fluorescent X-ray analysis method, and the ratio (S / C) of the number of sulfur atoms (S) to the number of carbon atoms (C) is 1.5×10 -3 ~3.5×10 -3 The separator for an alkaline battery according to claim 1, wherein Effect of the Invention

[0011] In the alkaline battery separator according to claim 1 of the present invention, the surface of a fiber coated with a polyolefin resin having sulfonic acid groups contained in the alkaline battery separator is measured using XPS, and the percentage of the peak area of ​​COO in the total peak area of ​​each peak (CC, CO, COO) obtained by waveform separation of the C1s spectrum obtained is less than 2.0%, which indicates that the surface of the fiber has few carboxy groups (-COOH) and the degree of oxidation of the polyolefin resin on the surface of the fiber is small.

[0012] Therefore, the alkaline battery separator having the above-mentioned configuration has excellent mechanical strength, and therefore, by using the alkaline battery separator, it is possible to provide an alkaline battery that is less susceptible to internal short circuits.

[0013] The alkaline battery separator according to claim 2 of the present invention is characterized in that the surface of a fiber that is included in the alkaline battery separator and is coated with a polyolefin resin having a sulfonic acid group is measured using XPS, and the obtained S2p 3 / 2The percentage of the peak area of ​​-SO3 in the total peak area of ​​each peak (-SO3, -SO4) obtained by waveform separation of the spectrum is large at 50% or more. This indicates that most of the sulfur on the surface of the fiber exists as sulfonic acid groups (-SO3H), and that the polyolefin resin on the surface of the fiber contains many sulfonic acid groups.

[0014] Therefore, an alkaline battery separator having the above-mentioned configuration is highly hydrophilic due to the inclusion of many sulfonic acid groups, and also has excellent self-discharge suppression properties. Therefore, by using this alkaline battery separator, it is possible to provide a high-performance alkaline battery.

[0015] In the alkaline battery separator according to claim 3 of the present invention, the ratio (S / C) of the number of sulfur atoms (S) to the number of carbon atoms (C) measured by fluorescent X-ray analysis is 1.5×10 -3 ~3.5×10 -3 This indicates that the surface of the fibers that make up the alkaline battery separator contains an appropriate amount of sulfonic acid groups (-SO3H).

[0016] Therefore, the separator for alkaline batteries having the above-mentioned configuration has high hydrophilicity due to the inclusion of sulfonic acid groups, and has excellent self-discharge suppression properties, and further has excellent mechanical strength because the polyolefin resin contained in the separator for alkaline batteries is less susceptible to deterioration due to oxidation. As a result, by using the separator for alkaline batteries, it is possible to provide a high-performance alkaline battery that is less susceptible to internal short circuits. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The alkaline battery separator of the present invention contains fibers whose surfaces are coated with a polyolefin resin having sulfonic acid groups. Note that the "surface" of the "surface-coated fibers" does not include both ends of the fibers.

[0018] The polyolefin resin present on the fiber surface may be a known polyolefin resin such as polyethylene, polypropylene, or polymethylpentene. Among these, polyethylene is preferred because it has a tendency to easily introduce sulfonic acid groups by sulfonation treatment and can introduce many sulfonic acid groups. The polyethylene is not particularly limited, but examples include high-density polyethylene, medium-density polyethylene, low-density polyethylene, and linear low-density polyethylene. Among these, high-density polyethylene is preferable because it has a relatively high melting point and is easy to use as a separator at high temperatures, and because high-density polyethylene has a certain degree of hardness, it can be made into a separator with tension and stiffness, and is easy to handle.

[0019] The fiber whose surface is covered with the polyolefin resin having sulfonic acid groups may be a single fiber composed only of the polyolefin resin having sulfonic acid groups, or may be a core-sheath type composite fiber in which the sheath component on the fiber surface is composed of the polyolefin resin having sulfonic acid groups and the core component is composed of another organic resin. Among these, the fiber whose surface is covered with the polyolefin resin having sulfonic acid groups preferably includes a core-sheath type composite fiber whose core component is composed of an organic resin other than the polyolefin resin contained in the sheath component, because the shape of the alkaline battery separator can be firmly held by the core component and the shape stability is excellent. When the fiber whose surface is covered with the polyolefin resin having sulfonic acid groups is a core-sheath type composite fiber, the core component may be a known organic resin, but it is preferable that the core component has a higher melting point than the polyolefin resin having sulfonic acid groups of the sheath component so that the shape of the alkaline battery separator can be firmly held by the core component. In order to provide fibers having a surface coated with a polyolefin resin having sulfonic acid groups with excellent alkali resistance, the core component is preferably a polyolefin resin, and among polyolefin resins, polypropylene, which has excellent chemical resistance and is highly versatile, is more preferable.

[0020] In the case where the fiber having a surface coated with a polyolefin resin having a sulfonic acid group contained in the alkaline battery separator of the present invention is a core-sheath type composite fiber and the core component is polypropylene, the polypropylene can be a homopolymer of propylene or a copolymer of propylene and an α-olefin (e.g., ethylene, 1-butene, etc.). More specifically, for example, an isotactic propylene homopolymer having crystallinity, an ethylene-propylene random copolymer having a low content of ethylene units, a propylene block copolymer composed of a homopolymer portion composed of a propylene homopolymer and a copolymer portion composed of an ethylene-propylene random copolymer having a relatively high content of ethylene units, and further, a crystalline propylene-ethylene-α-olefin copolymer composed of each homopolymer or copolymer portion in the propylene block copolymer further copolymerized with an α-olefin such as 1-butene can be mentioned. Among these, an isotactic propylene homopolymer is preferable because it is easy to have a high degree of crystallinity.

[0021] The fibers having a surface coated with a polyolefin resin having sulfonic acid groups contained in the alkaline battery separator of the present invention can be obtained by carrying out a sulfonation treatment in a fiber state or in a nonwoven fabric state by a conventional method. The polyolefin resin having sulfonic acid groups may also have hydrophilic groups other than sulfonic acid groups (e.g., carboxyl groups, carbonyl groups, etc.). In addition, in order to improve the injectability of the electrolyte, a surfactant may be further contained in addition to the hydrophilic groups containing sulfonic acid groups.

[0022] In the case where the fiber of the alkaline battery separator of the present invention, the surface of which is coated with the polyolefin resin having sulfonic acid groups, is a core-sheath type composite fiber, the core component may be in an eccentric state, but it is preferable that the core component is arranged concentrically in the fiber cross section, since the core-sheath type composite fiber can be fused evenly. The volume ratio of the core component to the sheath component is not particularly limited, but in order to enable the fibers to be firmly fused to each other and to maintain the fiber form during fusion, the volume ratio of the core component to the sheath component is preferably 8:2 to 2:8, more preferably 3:7 to 7:3, and even more preferably 4:6 to 6:4.

[0023] When the fiber having a surface coated with a polyolefin resin having sulfonic acid groups in the alkaline battery separator of the present invention is a sheath-core composite fiber, the fineness of the sheath-core composite fiber is not particularly limited, but is preferably 0.05 to 3.5 dtex, more preferably 0.1 to 2.5 dtex, and even more preferably 0.3 to 2.0 dtex. If the fineness of the sheath-core composite fiber is less than 0.05 dtex, the strength of the alkaline battery separator tends to be insufficient, and if the fineness of the sheath-core composite fiber exceeds 3.5 dtex, the electrolyte retention of the alkaline battery separator tends to be insufficient.

[0024] The fiber length of the core-sheath type composite fiber is not particularly limited, but is preferably 1 to 160 mm, more preferably 3 to 120 mm, and even more preferably 4 to 100 mm, so that the fibers are uniformly dispersed and the alkaline battery separator can uniformly retain the electrolyte.

[0025] The mass percentage of the core-sheath type composite fiber having sulfonic acid groups contained in the alkaline battery separator of the present invention is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 65 mass% or more, so that the constituent fibers of the alkaline battery separator are strongly bonded to each other and the strength of the alkaline battery separator is excellent.

[0026] The fibers of the alkaline battery separator of the present invention, the surface of which is coated with a polyolefin resin having a sulfonic acid group, may contain fibers other than the core-sheath type composite fibers. For example, they may be ultrafine fibers having a fiber diameter of 5 μm or less for the purpose of improving the electrolyte retention of the alkaline battery separator, or single fibers having a fiber diameter of more than 5 μm for the purpose of improving the strength of the alkaline battery separator. The fineness of the fibers other than the core-sheath type composite fibers having a surface coated with a polyolefin resin having a sulfonic acid group is not particularly limited. The fiber length of the fibers other than the core-sheath type composite fibers having a surface coated with a polyolefin resin having a sulfonic acid group is preferably about the same as the fiber length of the core-sheath type composite fibers so that the fibers are uniformly dispersed and the alkaline battery separator can uniformly retain the electrolyte.

[0027] The percentage by mass of fibers other than the core-sheath type composite fibers having sulfonic acid groups contained in the alkaline battery separator of the present invention is preferably 50 mass% or less, more preferably 40 mass% or less, and even more preferably 35 mass% or less, since if it is too high, the content of the core-sheath type composite fibers will be low and the strength of the alkaline battery separator may be inferior.

[0028] The alkaline battery separator of the present invention may contain fibers other than those coated with a polyolefin resin having a sulfonic acid group, for example, fibers coated with a resin other than a polyolefin resin, such as a polyamide resin.

[0029] The alkaline battery separator of the present invention may contain inorganic particles such as alumina and silica in addition to the nonwoven fabric in order to impart functionality such as electrolyte retention and electrical insulation.

[0030] In the alkaline battery separator of the present invention, the surface of the fiber coated with the polyolefin resin having sulfonic acid groups contained in the alkaline battery separator is measured by XPS (X-ray photoelectron spectroscopy), and the percentage of the peak area of ​​COO in the total peak area of ​​each peak (CC, CO, COO) obtained by waveform separation of the C1s spectrum obtained is less than 2.0%. This XPS measurement result shows that the surface of the fiber coated with the polyolefin resin having sulfonic acid groups contained in the alkaline battery separator has few carboxy groups, that is, the deterioration due to oxidation of the polyolefin resin contained in the fiber coated with the polyolefin resin having sulfonic acid groups contained in the alkaline battery separator is small, and the mechanical strength of the alkaline battery separator is excellent. In order to reduce the deterioration due to oxidation of the polyolefin resin contained in the constituent fibers of the alkaline battery separator and to improve the mechanical strength of the alkaline battery separator, the surface of the fiber coated with the polyolefin resin having a sulfonic acid group contained in the alkaline battery separator is measured using XPS, and the percentage of the peak area of ​​COO in the total peak area of ​​each peak (CC, CO, COO) obtained by waveform separation of the C1s spectrum obtained is more preferably 1.5% or less, and even more preferably 1.0% or less. If the peak area of ​​COO in the total peak area of ​​each peak is too small, the hydrophilicity of the fiber coated with the polyolefin resin having a sulfonic acid group is low, and the electrolyte retention of the alkaline battery separator tends to be poor, so 0.01% or more is practical.

[0031] The C1s spectrum by XPS (X-ray photoelectron spectroscopy) is measured under the following conditions after the alkaline battery separator is washed in pure water for 30 minutes or more and air-dried for 24 hours. (1) Excitation source: Mg-Kα (2) Applied voltage value: 10KV (3) Beam current value: 10mA (4) Photoelectron escape angle: 90° The percentage of the COO peak area in the total peak area of ​​each peak (CC, CO, COO) obtained by waveform separation of the obtained C1s spectrum can be calculated by waveform separation of the obtained C1s spectrum into a CC-derived peak, a CO-derived peak, and a COO-derived peak by nonlinear least squares method using a Gaussian-Lorentz mixture function, and obtaining the area of ​​each peak and the total area of ​​each peak.

[0032] The alkaline battery separator of the present invention is characterized in that the surface of the fiber, which is coated with a polyolefin resin having a sulfonic acid group and is contained in the alkaline battery separator, is measured using XPS (X-ray photoelectron spectroscopy) to obtain S2p 3 / 2 The percentage of the peak area of ​​-SO3 in the total peak area of ​​each peak (-SO3, -SO4) obtained by waveform separation of the spectrum is preferably 50% or more. The results of this XPS measurement show that the polyolefin resin on the surface of the fiber, the surface of which is coated with the polyolefin resin having sulfonic acid groups constituting the alkaline battery separator, contains many sulfonic acid groups. Therefore, the alkaline battery separator having this configuration is highly hydrophilic and has excellent self-discharge suppression effect due to the inclusion of many sulfonic acid groups, and therefore, by using this alkaline battery separator, it is possible to provide an alkaline battery with higher performance. The surface of the fiber, the surface of which is coated with the polyolefin resin having sulfonic acid groups contained in the alkaline battery separator so as to have higher hydrophilicity and better self-discharge suppression effect, was measured using XPS (X-ray photoelectron spectroscopy), and the obtained S2p 3 / 2 The percentage of the peak area of ​​-SO3 in the total peak area of ​​each peak (-SO3, -SO4) obtained by waveform separation of the spectrum is more preferably 53% or more, and further preferably 55% or more.

[0033] In addition, S2p by XPS (X-ray photoelectron spectroscopy) 3 / 2 The spectrum is measured under the same conditions as those for measuring the C1s spectrum by XPS.

[0034] The obtained S2p 3 / 2 The percentage of the peak area of ​​-SO3 in the total peak area of ​​each peak (-SO3, -SO4) obtained by waveform separation of the spectrum is the obtained S2p 3 / 2 The spectrum is subjected to waveform separation using the nonlinear least squares method with a Gaussian-Lorentz mixture function to separate the peak due to -SO3 and the peak due to -SO4, and the area of ​​each peak is obtained, so that the area of ​​each peak and the total area of ​​each peak can be calculated.

[0035] The alkaline battery separator of the present invention has a ratio (S / C) of the number of sulfur atoms (S) to the number of carbon atoms (C) measured by X-ray fluorescence analysis of 1.5×10 -3 ~3.5×10 -3 The ratio (S / C) of the number of sulfur atoms (S) to the number of carbon atoms (C) obtained is preferably 1.5×10 -3 If the ratio is less than 3.5×10, the affinity between the alkaline battery separator and the electrolyte tends to be poor, and the ratio (S / C) of the number of sulfur atoms (S) to the number of carbon atoms (C) obtained is 3.5×10 -3 If the temperature exceeds this range, the mechanical strength of the alkaline battery separator tends to decrease.

[0036] This ratio (S / C) is measured by X-ray fluorescence analysis as described above, and is the value obtained by the following procedure.

[0037] First, the alkaline battery separator to be measured is washed in pure water for 30 minutes or more, and then air-dried for 24 hours. Next, the basis weight A (g / m 2 ), and a test piece with a diameter of 44 mm is taken, and the X-ray intensity of the test piece is measured using an X-ray fluorescence device to calculate the amount of sulfur per unit area mS. Next, the amount of sulfur mS is divided by the atomic weight of sulfur (32) (mS / 32) to calculate the number of moles of sulfur (Sm). On the other hand, the test piece is made of polyolefin resin, i.e., -(CH2) nSince the test piece is made up of 1,000,000,000,000,000, the number of moles of carbon (Cm) is calculated by dividing the test piece's basis weight A by the molecular weight of CH2 (14) (A / 14). Next, the number of moles of sulfur is divided by the number of moles of carbon (Sm / Cm) to calculate the ratio (S / C) of the number of sulfur atoms (S) to the number of carbon atoms (C).

[0038] The alkaline battery separator of the present invention includes a nonwoven fabric. Examples of the nonwoven fabric include dry nonwoven fabrics produced by a carding method or an air laying method, wet nonwoven fabrics produced by papermaking, and direct spun nonwoven fabrics (melt blown, spunbond) produced by accumulating directly spun fibers. Among these, wet nonwoven fabrics are thinner than other nonwoven fabrics and can realize an alkaline battery with low electrical resistance, so that the alkaline battery separator of the present invention is preferably a wet nonwoven fabric.

[0039] The basis weight of the separator for alkaline batteries of the present invention is appropriately adjusted, but is preferably 10 to 100 g / m 2 and 20 to 80 g / m 2 and 30 to 70 g / m 2 In the present invention, the "weight" is the weight per square meter of the main surface, which is the widest surface. 2 This refers to the mass per unit.

[0040] In addition, the thickness of the separator for alkaline batteries of the present invention is preferably 10 to 250 μm, more preferably 20 to 230 μm, and even more preferably 30 to 200 μm, since a thinner separator tends to reduce the internal resistance of the battery, but if the thickness is too thin, there is a risk of poor resistance to internal short circuits. Note that the "thickness" in the present invention refers to the average value of measurements at 10 randomly selected points measured under a load of 147 kPa using an outside micrometer (measurement range: 0 to 25 mm) as specified in 3.1 of JIS B 7502 (2016) "Micrometer".

[0041] The cushioning property value of the alkaline battery separator of the present invention, which is obtained by rounding off the value calculated using the following formula to one decimal place, tends to be thinner when subjected to a load of 147 kPa compared to the thickness when no load is applied. This is preferable because the higher the cushioning property value, the thinner the thickness when subjected to a load of 147 kPa compared to the thickness when no load is applied, and the longer the cycle life of the battery tends to be when the alkaline battery separator is incorporated into an alkaline battery. (Formula) = (Thickness of alkaline battery separator under no load (mm)) / (Thickness of alkaline battery separator under 147 kPa load (mm)) This value is preferably 1.4 or more, more preferably 1.5 or more, and even more preferably 1.6 or more. The thickness (mm) of the alkaline battery separator under no load refers to the value obtained by measuring the length between the main surfaces of the alkaline battery separator by freezing the alkaline battery separator, cutting the separator, and observing the cross section of the separator with a scanning electron microscope (SEM).

[0042] The tensile strength of the alkaline battery separator of the present invention is preferably 220 N / 50 mm or more, more preferably 225 N / 50 mm or more, and even more preferably 230 N / 50 mm or more, since the higher the tensile strength, the less oxidative degradation and the better the mechanical strength of the separator. The tensile strength of the alkaline battery separator of the present invention can be determined by the following method. (1) From three randomly selected points on the alkaline battery separator, three rectangular samples measuring 200 mm in the vertical direction (the lengthwise direction of the alkaline battery separator) and 50 mm in the horizontal direction (the direction perpendicular to the vertical direction) are taken. (2) The sample taken in (1) is subjected to a constant-speed extension tensile tester (Orientec Co., Ltd., Tensilon, initial gripping distance: 100 mm, tensile speed: 300 mm / min) and the maximum strength is measured when the sample is pulled until it breaks. The above measurement is performed on three samples, and the arithmetic average value of the three samples is the tensile strength (N / 50 mm) of the alkaline battery separator.

[0043] The tensile elongation of the alkaline battery separator of the present invention is preferably 9% or more, more preferably 10% or more, and even more preferably 11% or more, since the higher the tensile elongation, the less oxidative degradation the separator undergoes, the less likely it is to break, and the greater its mechanical strength. The tensile elongation of the alkaline battery separator of the present invention can be determined by the following method. (1) As in the above (Measurement of tensile strength of alkaline battery separator), three rectangular samples measuring 200 mm in the vertical direction (longitudinal direction of the alkaline battery separator) and 50 mm in the horizontal direction (direction perpendicular to the vertical direction) are taken from three randomly selected points on the alkaline battery separator. (2) The sample taken in (1) is subjected to a constant-speed extension tensile tester (Orientec Co., Ltd., Tensilon, initial gripping distance: 100 mm, tensile speed: 300 mm / min), and the gripping distance (mm) of the sample is measured when the sample is pulled until it breaks. The above measurement is performed for three samples, and the arithmetic average value of the three samples is taken as the average gripping distance L1 of the sample. (3) Calculate the tensile elongation (%) of the alkaline battery separator using the following formula. (Formula)={(L1-100) / 100}×100 The alkaline battery separator of the present invention can be produced, for example, as follows.

[0044] First, prepare fibers whose surfaces are coated with polyolefin resin (such as core-sheath type composite fibers and ultrafine fibers with a fiber diameter of 5 μm or less). Also, prepare fibers whose surfaces are not coated with polyolefin resin as necessary.

[0045] Next, the fibers are blended to form a fiber web. The fiber web can be formed by, for example, a dry method (e.g., carding method, air laying method, etc.) or a wet method. Among these, it is preferable to form the fiber web by a wet method, which is easy to produce a nonwoven fabric (as a separator) in which the fibers are uniformly dispersed and which easily retains the electrolyte uniformly. As the wet method, the fiber web can be formed by a conventionally known method, for example, a horizontal long-net method, an inclined wire-type short-net method, a cylinder method, or a combination of a long-net and a cylinder method. When two or more layers are laminated, it is preferable to laminate fiber webs having the same fiber blend so that a separator with a single layer structure can be produced.

[0046] Next, the fibers constituting this fiber web are bonded together to obtain a nonwoven fabric. Preferably, the fibers constituting the fiber web are bonded together only by fusion. When the fibers are bonded together only by fusion in this manner, the voids in the fiber web are not disturbed, so that the electrolyte is uniformly distributed, and it is easy to manufacture an alkaline battery separator that can manufacture an alkaline battery with low internal resistance. When the fibers constituting this fiber web are fused together by a heat treatment under no pressure, in which the fiber web is sucked from below a support such as a conveyor to bring the fiber web into close contact with the support, hot air is blown onto the fiber web, and a sufficient amount of hot air is passed through, the thickness of the alkaline battery separator tends to be thick, and the alkaline battery separator has high electrolyte retention, which is preferable.

[0047] Next, the nonwoven fabric is subjected to a sulfonation treatment to obtain the alkaline battery separator of the present invention. Examples of the sulfonation treatment include a method of immersing the nonwoven fabric in a solution of fuming sulfuric acid, sulfuric acid, chlorosulfuric acid, or sulfuryl chloride, a method of discharging the nonwoven fabric in the presence of sulfur monoxide gas and / or sulfur dioxide gas, and a method of exposing the nonwoven fabric to sulfur trioxide gas. Any of these methods can introduce sulfonic acid groups. Among these methods, it is preferable to carry out the sulfonation treatment by immersing the nonwoven fabric in a fuming sulfuric acid solution, since this method can suppress oxidation of the polyolefin resin contained in the nonwoven fabric caused by the sulfonation treatment, and can realize an alkaline battery separator with excellent mechanical strength in which the amount of carboxyl groups introduced is small relative to the amount of sulfonic acid groups introduced.

[0048] In addition, if the fuming sulfuric acid solution contains a surfactant, the sulfur trioxide gas in the fuming sulfuric acid reacts easily with the nonwoven fabric in the liquid when the nonwoven fabric is immersed in the fuming sulfuric acid for sulfonation, and the sulfonation process proceeds quickly. This is preferable because the sulfonation process can be performed while suppressing the oxidation of the polyolefin resin, and an alkaline battery separator with excellent mechanical strength can be realized. In addition, the surfactant contained in the fuming sulfuric acid solution can be a known surfactant, and can be an anionic surfactant, a cationic surfactant, an amphoteric surfactant, or a nonionic surfactant. The larger the percentage of the surfactant content in the fuming sulfuric acid solution, the more easily the sulfur trioxide gas in the fuming sulfuric acid reacts with the nonwoven fabric in the liquid, while if the proportion of the surfactant contained in the fuming sulfuric acid solution is too large, the fuming sulfuric acid solution tends to foam easily due to the surfactant, and the efficiency of the sulfonation process may be deteriorated. Therefore, the percentage of the surfactant content is preferably 1 to 10 mass%, more preferably 2 to 7 mass%, and even more preferably 3 to 5 mass%.

[0049] By controlling the conditions of the sulfonation treatment (for example, temperature, reaction time, etc.), it is possible to adjust the percentage of the peak area of ​​COO in the total peak area of ​​each peak (CC, CO, COO) obtained by waveform separation of the C1s spectrum obtained by measuring the alkaline battery separator using XPS, and the ratio (S / C) of the number of sulfur atoms (S) to the number of carbon atoms (C) of the alkaline battery separator. In addition, such a sulfonation treatment does not need to be performed after the formation of a fiber web, and may be performed on the fibers before the formation of the fiber web, and then the fiber web may be formed. Specifically, the temperature in the sulfonation treatment is preferably 40 to 80°C, more preferably 50 to 70°C, and even more preferably 55 to 65°C. In addition, the reaction time in the sulfonation treatment is preferably 20 seconds to 4 minutes, more preferably 30 seconds to 3 minutes, and even more preferably 1 minute to 2 minutes.

[0050] In this way, sulfonic acid groups can be introduced into the nonwoven fabric, but since by-products are also generated when sulfonic acid groups are introduced, these by-products are removed by washing with sulfuric acid, water, or a dilute alkaline solution. Note that if the nonwoven fabric after sulfonation is immediately washed with water, it may generate heat and damage the sheet, so it is preferable to wash it with sulfuric acid of lower concentration in order, and then with water last.

[0051] Then, only the remaining liquid such as water is dried and removed to obtain the separator for alkaline batteries of the present invention. In other words, if heat is applied even after the remaining liquid is removed, the sulfonic acid group (-SO3H) that adsorbs ammonia is denatured and decomposed by heat, and the amount of sulfonic acid groups is reduced, and a separator with excellent self-discharge suppression cannot be obtained due to the reduction in sulfonic acid groups. The method for drying and removing only the remaining liquid varies depending on the type and amount of the remaining liquid, and cannot be generally discussed, but examples of the method include air drying, heating for a short time (preferably 6 minutes or less, more preferably 4 minutes or less), and heating at a low temperature (preferably 105°C or less, more preferably 100°C or less). EXAMPLES

[0052] The present invention will be specifically described below with reference to examples, but the scope of the present invention is not limited thereto.

[0053] Example 1 A fiber web was formed by papermaking using an inclined wire short net method from a slurry in which 100 mass% of core-sheath type composite fused fibers with a tensile strength of 4.5 cN / dtex, a fineness of 0.8 dtex, and a fiber length of 5 mm were dispersed. The core component was made of polypropylene (melting point: 168°C) and the sheath component (fused component) was made of high-density polyethylene (melting point: 135°C). Next, this fiber web was fed into an oven set at a temperature of 140° C. to fuse the sheath components of the core-sheath type composite fibers to produce a nonwoven fabric. Next, this nonwoven fabric was immersed in fuming sulfuric acid of 15% concentration at 60°C for 1 minute and 30 seconds, and then the nonwoven fabric that had been immersed in fuming sulfuric acid was washed successively with sulfuric acid of 75% concentration, sulfuric acid of 50% concentration, and water, thereby carrying out a sulfonation treatment to introduce sulfonic acid groups into the high-density polyethylene derived from the core-sheath composite fiber that covers the surface of the constituent fibers of the nonwoven fabric. The sulfonated nonwoven fabric was then dried by contacting it with a heated roll set at a temperature of 96° C. for 3 minutes. Then, the thickness was adjusted with a pressure roll (at room temperature) to produce an alkaline battery separator (basis weight: 64 g / m 2 , thickness (under 147 kPa load): 0.17 mm) was manufactured.

[0054] Example 2 An alkaline battery separator (basis weight: 64 g / m) was prepared in the same manner as in Example 1, except that the time for immersing the nonwoven fabric in fuming sulfuric acid during the sulfonation treatment was changed from 1 minute 30 seconds to 30 seconds. 2 , thickness (under 147 kPa load): 0.17 mm) was manufactured.

[0055] Example 3 An alkaline battery separator (basis weight: 64 g / m) was produced in the same manner as in Example 1, except that the fuming sulfuric acid contained 5 mass% of polyoxyethylene alkyl ether (nonionic surfactant) when the nonwoven fabric was sulfonated. 2 , thickness (under 147 kPa load): 0.18 mm) was manufactured.

[0056] Example 4 After the nonwoven fabric was sulfonated, an alkaline battery separator (basis weight: 64 g / m) was produced in the same manner as in Example 1, except that the temperature of the heat roll was changed from 96°C to 110°C when drying the nonwoven fabric with the heat roll. 2 , thickness (under 147 kPa load): 0.17 mm) was manufactured.

[0057] Comparative Example 1 An alkaline battery separator (basis weight: 64 g / m) was prepared in the same manner as in Example 1, except that the concentration of fuming sulfuric acid in which the nonwoven fabric was immersed during the sulfonation treatment was changed from 15% to 8%, and the time of immersion in fuming sulfuric acid was changed from 1 minute 30 seconds to 5 minutes. 2 , thickness (under 147 kPa load): 0.17 mm) was manufactured.

[0058] Comparative Example 2 An alkaline battery separator (basis weight: 64 g / m) was prepared in the same manner as in Example 1, except that the same nonwoven fabric as in Example 1 was placed in a reaction tank containing 16 vol. % SO3 gas and 84 vol. % N2 gas (dew point -60°C) and having an internal temperature of 75°C for 30 seconds, and the nonwoven fabric was removed and neutralized by washing with a 2.5 mass % sodium hydroxide aqueous solution, and then thoroughly washed with ion-exchanged water. 2 , thickness (under 147 kPa load): 0.17 mm) was manufactured.

[0059] The physical properties of the alkaline battery separators of the Examples and Comparative Examples are shown in Table 1. The various physical properties were evaluated as follows.

[0060] (Measurement of thickness of alkaline battery separator under no load) The thickness of the alkaline battery separator under no load was measured by the method described above.

[0061] (Cushioning properties of alkaline battery separators) The cushioning property of the alkaline battery separator was determined by the above-mentioned method.

[0062] (XPS (X-ray photoelectron spectroscopy) measurement of alkaline battery separator) Using the method described above, XPS (X-ray photoelectron spectroscopy) measurements were performed on the separator for alkaline batteries, and the C1s spectrum and S2p 3 / 2 The spectrum was obtained. In addition, the percentage of the COO peak area (COO ratio) in the total peak area of ​​each peak (CC, CO, COO) obtained from the obtained C1s spectrum was calculated using the method described above. Furthermore, the obtained S2p 3 / 2 The spectrum was analyzed by the method described above to determine the percentage of the -SO3 peak area (SO3 ratio) in the total peak area of ​​each peak (-SO3, -SO4).

[0063] (Measurement of (S / C) of alkaline battery separator) The ratio (S / C) of the number of sulfur atoms (S) to the number of carbon atoms (C) of the alkaline battery separator was measured by the method described above.

[0064] (Measurement of tensile strength of alkaline battery separator) The tensile strength of the alkaline battery separator was measured by the method described above.

[0065] (Measurement of tensile elongation of alkaline battery separator) The tensile elongation of the alkaline battery separator was measured by the method described above.

[0066] (Measurement of capacity retention rate of nickel-metal hydride batteries incorporating alkaline battery separators) (1) As the electrode current collector, a paste-type nickel positive electrode (33 mm, 182 mm long) using a foamed nickel base material and a paste-type hydrogen storage alloy negative electrode (mesh metal alloy, 33 mm, 247 mm long) were prepared. (2) Next, the alkaline battery separators of the Examples and Comparative Examples cut to a width of 35 mm and a length of 410 mm were sandwiched between the positive and negative electrodes, respectively, and wound in a spiral shape to prepare an SC-type compatible electrode group. (3) This electrode group was placed in an outer can, and then 5 mol / L potassium hydroxide and 1 mol / L lithium hydroxide were poured into the can as electrolyte and the can was sealed to prepare a cylindrical nickel-hydrogen battery. (4) Next, each cylindrical nickel-hydrogen battery was charged to 150% capacity at 0.1 C, and then discharged at 0.1 C, and the initial capacity (A) was measured at the end voltage of 1.0 V. Next, each battery was charged to 150% capacity at 0.1 C, and then left in a thermostatic chamber at 65° C. for 5 days. Thereafter, each battery was discharged again at 0.1 C, and the capacity (B) was measured at the end voltage of 1.0 V. (5) From these results, the capacity retention rate (%) was calculated using the following formula. (Formula)=(B / A)×100

[0067] [Table 1]

[0068] From a comparison between the examples and the comparative examples, the surface of the fiber coated with a polyolefin resin having sulfonic acid groups is measured by XPS (X-ray photoelectron spectroscopy), and the percentage of the peak area of ​​COO in the total peak area of ​​each peak (CC, CO, COO) obtained by waveform separation of the C1s spectrum obtained is less than 2.0%. In the alkaline battery separator of the present invention, the polyolefin resin contained in the fiber coated with a polyolefin resin having sulfonic acid groups is less oxidized and has excellent tensile strength and mechanical strength. From this, it was found that the alkaline battery separator of the present invention can realize an alkaline battery that is less likely to cause internal short circuits when used in an alkaline battery. Furthermore, since the alkaline battery separator of the present invention has little oxidative degradation of the polyolefin resin contained in the fibers whose surfaces are coated with polyolefin resin having sulfonic acid groups, the elasticity of the fibers whose surfaces are coated with polyolefin resin having sulfonic acid groups is high, and the alkaline battery separator has excellent cushioning properties, so that the alkaline battery separator can follow the expansion and contraction of the electrodes of the alkaline battery, thereby realizing an alkaline battery with a long cycle life.

[0069] Furthermore, a comparison between Example 1 and Example 3 indicates that the alkaline battery separator of Example 3, in which a nonwoven fabric was immersed in fuming sulfuric acid containing a surfactant to undergo sulfonation treatment, had an equivalent (S / C) value to the alkaline battery separator of Example 1, but had a smaller percentage of the COO peak area in the total peak area of ​​the peaks (CC, CO, COO) obtained by waveform separation of the C1s spectrum. This indicates that the inclusion of a surfactant in the fuming sulfuric acid enables sulfonation treatment while better suppressing oxidation of the polyolefin resin.

[0070] Furthermore, by comparing Examples 1 to 3 with Example 4, the surface of the fiber coated with a polyolefin resin having a sulfonic acid group was measured using XPS (X-ray photoelectron spectroscopy), and the obtained S2p 3 / 2An alkaline battery separator in which the percentage of the peak area of ​​-SO3 in the total peak area of ​​each peak (-SO3, -SO4) obtained by waveform separation of the spectrum is 50% or more contains many sulfonic acid groups, and the capacity retention rate of an alkaline battery incorporating the alkaline battery separator is high. From this, it was found that the alkaline battery separators of Examples 1 and 2 are excellent in suppressing the self-discharge of an alkaline battery. The cause of this difference is considered to be that the drying temperature after the sulfonation treatment during the production of the alkaline battery separator was different, and the drying temperature was lower in the alkaline battery separators of Examples 1 to 3, so that thermal change of the sulfonic acid groups contained in the alkaline battery separator was less likely to occur. [Industrial Applicability]

[0071] The alkaline battery separator of the present invention can be suitably used as a separator for primary batteries using an alkaline electrolyte, and alkaline secondary batteries such as nickel-metal hydride batteries, nickel-cadmium batteries, and nickel-zinc batteries.

Claims

1. An alkaline battery separator comprising a nonwoven fabric containing fibers whose surfaces are coated with a polyolefin resin having sulfonic acid groups, The surface of the fiber is measured using XPS (X-ray photoelectron spectroscopy), and the percentage of the peak area of ​​COO in the total peak area of ​​each peak (C-C, CO, COO) obtained by waveform separation of the obtained C1s spectrum is less than 2.0%. Separator for alkaline batteries.

2. The surface of the fiber was measured using XPS (X-ray photoelectron spectroscopy), and the obtained S2p 3/2 Each peak (-SO 3 , -SO 4 ) in the total peak area of ​​-SO 3 The percentage of the peak area of ​​is 50% or more. The separator for an alkaline battery according to claim 1 .

3. The alkaline battery separator was measured using a fluorescent X-ray analysis method, and the ratio (S / C) of the number of sulfur atoms (S) to the number of carbon atoms (C) was 1.5×10 -3 ~3.5 x 10 -3 That is, The separator for an alkaline battery according to claim 1 .

Citation Information

Patent Citations

  • Separator for alkaline battery

    JP2001283816A

  • Separator for alkaline battery

    JP2001283817A

  • Nonwoven cloth for battery separator

    JP2015041457A

  • Nonwoven cloth for battery separator

    JP2015041551A

  • Separator for alkali battery and method for manufacturing the same

    JP2017107752A