Modified ethylene copolymer, modifier, compatibilizer, modifying method and compatibilizing method
A biomass-derived modified ethylene copolymer with specific properties addresses the limitations of conventional modifiers by improving the appearance and mechanical properties of polymer blends, specifically through enhanced interaction and impact resistance.
Patent Information
- Application Number
- JP2023080221
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
AI Technical Summary
Conventional compatibilizers and modifiers for non-polar and polar polymers, such as polyolefins, fail to achieve both improved appearance and mechanical properties demanded by the market.
A modified ethylene copolymer derived from biomass is used, which is modified with unsaturated carboxylic acids or their derivatives, having a specific modification rate, melt flow rate, and biomass content, to enhance compatibility and mechanical properties.
The modified ethylene copolymer improves the appearance and mechanical properties of molded articles by enhancing the interaction between polar and non-polar polymers, particularly impact resistance.
Smart Images

Figure 2024164611000001 
Figure 2024164611000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a modified ethylene copolymer using a biomass ethylene copolymer, which can be used as a modifier and a compatibilizer, and a modifier and a compatibilizer containing the modified ethylene copolymer. The present invention also relates to a modification method and a compatibilization method using the modified ethylene copolymer. [Background technology]
[0002] Compatibilizers and modifiers are used to disperse organic, inorganic, or biomass fillers or polar polymers in polyolefins, or to improve the properties of polar polymers. Polyolefins having polar groups are usually used as compatibilizers and modifiers.
[0003] When a polyolefin having a polar group is used as a compatibilizer, the polyolefin portion of the polyolefin having a polar group is compatible with a non-polar polymer such as polyolefin, and the polar group portion interacts (chemically bonds, physically bonds) with a filler or a polar polymer, thereby compatibilizing the non-polar polymer such as polyolefin with the filler or polar polymer.
[0004] When a polyolefin having a polar group is used as a modifier, the polar group portion interacts (chemically bonds, physically bonds) with the polar polymer, while the polyolefin portion is incompatible with the polar polymer, so the polar polymer and the polyolefin having a polar group form an island structure. In this way, by mixing a polyolefin having a polar group with a polar polymer, a change in morphology occurs, and functions such as flexibility and impact resistance can be imparted to the polar polymer. In other words, the polar polymer can be modified.
[0005] As an example of the application of such a technique, a polyamide resin composition containing a polyamide resin and a specific acid-modified polyolefin is known (for example, Patent Document 1). Here, a petroleum (fossil fuel)-derived polyolefin is used as the polyolefin to be modified into the acid-modified polyolefin. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2017 / 094720 Summary of the Invention [Problem to be solved by the invention]
[0007] Due to increasing demands on non-polar polymers such as polyolefins and polar polymers, there was room for improvement in conventional compatibilizers and modifiers in terms of achieving both improved appearance and improved mechanical properties as required by the market.
[0008] The present invention has been made in view of the above problems, and an object of the present invention is to provide a modified ethylene copolymer which has an excellent compatibilizing effect between polar polymers and non-polar polymers as a compatibilizer, and also has an excellent modifying effect on polar polymers as a modifier, and which can give molded articles having excellent appearances and mechanical properties. [Means for solving the problem]
[0009] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that, while acid-modified products of petroleum-derived ethylene copolymers have conventionally been used as modifiers or compatibilizers, by using acid-modified products of biomass-derived ethylene copolymers instead, it is possible to improve mechanical properties such as impact resistance while maintaining a good appearance, thus completing the present invention. That is, the present invention has the following features.
[0010] [1] A modified ethylene copolymer obtained by modifying an ethylene copolymer, including a biomass ethylene copolymer, with at least one member selected from the group consisting of unsaturated carboxylic acids and derivatives thereof.
[0011] [2] The modified ethylene copolymer according to [1], having a modification rate of 0.01% by mass or more and 2.50% by mass or less.
[0012] [3] The modified ethylene copolymer according to [1] or [2], having a melt flow rate at 190°C under a load of 2.16 kg of 0.1 g / 10 min or more and 20 g / 10 min or less.
[0013] [4] The modified ethylene copolymer according to any one of [1] to [3], wherein the ethylene copolymer is at least one selected from the group consisting of HDPE and LLDPE.
[0014] [5] The modified ethylene copolymer according to any one of [1] to [4], having a biomass ratio of 20 to 100%.
[0015] [6] A modifier comprising the modified ethylene copolymer according to any one of [1] to [5].
[0016] [7] A compatibilizer comprising the modified ethylene copolymer according to any one of [1] to [5].
[0017] [8] A method for modifying a polar polymer in the presence of the modified ethylene copolymer according to any one of [1] to [5].
[0018] [9] A method for compatibilizing a polar polymer and a non-polar polymer in the presence of the modified ethylene copolymer according to any one of [1] to [5]. Effect of the Invention
[0019] According to the present invention, it is possible to provide a modified ethylene copolymer which, when mixed as a modifier or compatibilizer with a polar polymer or with a polar polymer and a non-polar polymer, can give a molded article having excellent appearance and mechanical properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The following is a detailed description of the embodiments of the present invention, but the present invention is not limited to the following description, and can be modified as desired without departing from the scope of the present invention. In this specification, when a numerical value or physical property value is enclosed before and after "~", the values before and after the "~" are included.
[0021] Hereinafter, the monomer units contained in the copolymer may be simply referred to as "units." For example, a monomer unit based on ethylene and a monomer unit based on an α-olefin may be referred to as an "ethylene unit" and an "α-olefin unit," respectively.
[0022] In the present invention, the melt flow rate (MFR) and density of the ethylene copolymer or modified ethylene copolymer, and the modification rate and biomass degree of the modified ethylene copolymer are values measured as follows.
[0023] <mfr> The MFR is measured in accordance with JIS K7210 under conditions of 190°C and a load of 2.16 kg.
[0024] <density> The density is measured by the underwater displacement method in accordance with JIS K7112.
[0025] <Degeneration rate> The modification rate of the modified ethylene copolymer (also referred to as the graft rate, modification amount, or graft amount; hereinafter referred to as the "graft rate") means the content of unsaturated carboxylic acid and / or its anhydride (hereinafter sometimes referred to as the "unsaturated carboxylic acid component") grafted to the raw material ethylene copolymer described below, as measured with an infrared spectrometer. The content of the unsaturated carboxylic acid component can be measured by, for example, measuring the absorption characteristic of the unsaturated carboxylic acid component in a sample obtained by pressing the modified polymer into a sheet having a thickness of about 100 μm, specifically, 1,900 to 1,600 cm -1 It can be determined by measuring the carbonyl characteristic absorption (C=O stretching vibration band). The graft ratio can also be determined from a calibration curve prepared in advance by the above method.
[0026] <Biomass ratio> The biomass degree of the modified ethylene copolymer is calculated according to ASTM D 6866 based on the 14C content. Specifically, a tandem accelerator-based C-AMS dedicated device (manufactured by NEC Corporation) is used to measure the 14C concentration, after which the biomass degree can be calculated according to ASTM D6866-22. The biomass degree can also be determined by calculation as the content ratio of the biomass ethylene copolymer used in the production of the modified ethylene copolymer in the modified ethylene copolymer.
[0027] [Modified ethylene copolymer] The modified ethylene copolymer of the present invention is a modified ethylene copolymer obtained by modifying an ethylene copolymer including a biomass ethylene copolymer with an unsaturated carboxylic acid component, i.e., at least one selected from the group consisting of unsaturated carboxylic acids and derivatives thereof.
[0028] <Mechanism> The details of the mechanism by which the appearance and mechanical properties can be improved when the modified ethylene copolymer of the present invention is used as a modifier or compatibilizer are not clear; however, it is believed that this is due to the fact that, in the modified ethylene copolymer of the present invention, the biomass ethylene copolymer contained in the ethylene copolymer subjected to modification has a low content of low molecular weight components. On the other hand, in terms of appearance, it is possible to obtain an effect equivalent to that obtained when a petroleum-derived ethylene copolymer is used as the modified ethylene copolymer.
[0029] <Raw material ethylene copolymer> Monomers other than ethylene that constitute the ethylene copolymer (hereinafter sometimes referred to as the "raw material ethylene copolymer"), including the biomass ethylene copolymer, to be subjected to modification with an unsaturated carboxylic acid component, include one or more α-olefin monomers having 3 to 8 carbon atoms, such as propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 4,4-dimethyl-1-pentene, 1-hexene, 4-methyl-1-hexene, 1-heptene, and 1-octene.
[0030] Furthermore, the raw material ethylene copolymer may contain other monomer units in addition to the ethylene monomer and the above-mentioned α-olefin monomer.
[0031] As the raw material ethylene copolymer, from the viewpoint of mechanical properties, HDPE (high density polyethylene) and LLDPE (linear low density polyethylene) are preferred. The density of HDPE is 0.942~0.970g / cm 3 and preferably 0.948 to 0.960 g / cm 3 It is more preferable that: HDPE in the above density range maintains good mechanical properties. The density of LLDPE is 0.910 to 0.928 g / cm 3 and preferably 0.915 to 0.925 g / cm 3 It is more preferable that: LLDPE in the above density range maintains good mechanical properties.
[0032] The MFR (190°C, load 2.16 kg) of the raw material ethylene copolymer is not particularly limited, but is preferably 0.2 to 40 g / 10 min, more preferably 0.5 to 30 g / 10 min. By setting the MFR of the raw material ethylene copolymer within the above range, even when taking into account the change in MFR due to modification, a modified ethylene copolymer having a suitable MFR described below tends to be easily obtained.
[0033] In the present invention, the raw material ethylene copolymer may be used alone or in combination with two or more different types having different physical properties, compositions, etc. In the modified ethylene copolymer of the present invention, the raw material ethylene copolymer subjected to modification may be a mixture containing a petroleum-derived ethylene copolymer together with the biomass ethylene copolymer, within a range that satisfies the suitable biomass degree of the modified ethylene copolymer of the present invention described below. From the viewpoint of satisfying a suitable biomass degree of the modified ethylene copolymer of the present invention described below, the proportion of the biomass ethylene copolymer in the raw material ethylene copolymer is preferably 25 mass% or more, more preferably 30 to 100 mass%, even more preferably 40 to 100 mass%, and most preferably 100 mass%.
[0034] The biomass ethylene copolymer used in the present invention can usually be produced by polymerization or copolymerization using bioethylene obtained by dehydrating ethanol derived from biomass as a raw material, but known commercially available products can also be used. According to the present invention, by using a biomass ethylene copolymer as the raw material ethylene copolymer, as described above, it is possible to improve the appearance and mechanical properties, and also to obtain the effect of enabling a reduction in greenhouse gas emissions by utilizing biomass.
[0035] <Graft modification> Examples of the unsaturated carboxylic acid to be graft-modified to the raw material ethylene copolymer include α,β-ethylenically unsaturated carboxylic acids such as acrylic acid, maleic acid, fumaric acid, tetrahydrofumaric acid, itaconic acid, citraconic acid, crotonic acid, and isocrotonic acid. Examples of the anhydrides of unsaturated carboxylic acids include succinic acid 2-octen-1-yl anhydride, succinic acid 2-dodecen-1-yl anhydride, succinic acid 2-octadecen-1-yl anhydride, maleic acid anhydride, 2,3-dimethylmaleic acid anhydride, bromomaleic acid anhydride, dichloromaleic acid anhydride, citraconic acid anhydride, itaconic acid anhydride, 1-butene-3,4-dicarboxylic acid anhydride, 1-cyclopentene-1,2-dicarboxylic acid anhydride, and 1,2,3,6-tetrahydrophthalic acid. Examples of unsaturated carboxylic acid anhydrides include 3,4,5,6-tetrahydrophthalic anhydride, exo-3,6-epoxy-1,2,3,6-tetrahydrophthalic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, methyl-5-norbornene-2,3-dicarboxylic anhydride, endo-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, and bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic anhydride.
[0036] These unsaturated carboxylic acid components can be appropriately selected depending on the raw material ethylene copolymer to be modified and the modification conditions, and not limited to the case of using one type alone, but two or more types may be used in combination. These unsaturated carboxylic acid components can also be used by dissolving them in an organic solvent or the like.
[0037] The graft modification of the raw material ethylene copolymer can be carried out by adding an unsaturated carboxylic acid component and graft polymerizing the unsaturated carboxylic acid component onto the raw material ethylene copolymer, preferably in the presence of a radical generator.
[0038] Examples of the radical generator used herein include organic and inorganic peroxides such as t-butyl hydroperoxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-bis(t-butyloxy)hexane, 3,5,5-trimethylhexanoyl peroxide, t-butyl peroxybenzoate, benzoyl peroxide, m-toluoyl peroxide, dicumyl peroxide, 1,3-bis(t-butylperoxyisopropyl)benzene, dibutyl peroxide, methyl ethyl ketone peroxide, potassium peroxide, and hydrogen peroxide; azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(isobutylamide)dihalide, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide] and azodi-t-butane; and carbon radical generators such as dicumyl.
[0039] The above radical generator can be appropriately selected depending on the type of raw material ethylene copolymer to be subjected to the modification reaction, the type of unsaturated carboxylic acid component as a modifier, and the modification conditions, and one type may be used alone, or two or more types may be used in combination. The radical generator can also be used after being dissolved in an organic solvent.
[0040] The modification reaction carried out to obtain the modified ethylene copolymer of the present invention can be carried out by various known reaction methods such as a melt-kneading reaction method, a solution reaction method, a suspension dispersion reaction method, etc., but the melt-kneading reaction method is usually preferred.
[0041] In the case of the melt-kneading reaction method, the above-mentioned components are mixed uniformly in a predetermined mixing ratio and then melt-kneaded. For mixing, a Henschel mixer, a ribbon blender, a V-type blender, or the like is used, and for melt-kneading, a Banbury mixer, a kneader, a roll, or a multi-screw kneading extruder such as a single-screw or twin-screw kneading extruder, or the like is used.
[0042] The melt kneading is carried out at a temperature in the range of usually 100°C or higher, preferably 120°C or higher, more preferably 150°C or higher, and usually 300°C or lower, preferably 280°C or lower, more preferably 260°C or lower, so as to prevent thermal degradation of the ethylene copolymer.
[0043] The amount of the unsaturated carboxylic acid component used as a modifier is usually 0.01 parts by mass or more, preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and usually 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 3 parts by mass or less, based on 100 parts by mass of the raw material ethylene copolymer. By setting the amount of the unsaturated carboxylic acid component within the above range, it is economical and sufficient modification can be achieved.
[0044] The amount of the radical generator is usually 0.001 parts by mass or more, preferably 0.005 parts by mass or more, more preferably 0.01 parts by mass or more, and usually 1 part by mass or less, preferably 0.5 parts by mass or less, more preferably 0.1 parts by mass or less, relative to 100 parts by mass of the raw material ethylene copolymer. By setting the amount of the radical generator to be equal to or more than the above lower limit, sufficient modification can be performed. By setting the amount of the radical generator to be equal to or less than the above upper limit, the increase in molecular weight (increase in viscosity) during modification of the raw material ethylene copolymer can be suppressed to a desired range, and the desired modified ethylene copolymer tends to be easily obtained.
[0045] In the modification reaction, a graft polymerization reaction in which an unsaturated carboxylic acid component is added to the raw material ethylene copolymer mainly occurs, but a crosslinking reaction also occurs, and due to this crosslinking, the molecular weight of the resulting modified product tends to increase and the melt viscosity tends to become high. Therefore, if the amount of the radical generator used is too large, the graft polymerization reaction is likely to occur, but at the same time, the crosslinking reaction which leads to such an increase in melt viscosity is also likely to occur, which is not preferable.
[0046] <Grafting rate> The graft ratio of the modified ethylene copolymer of the present invention is preferably 0.01 to 2.50% by mass, more preferably 0.1 to 2.0% by mass, and even more preferably 0.3 to 1.5% by mass. When the graft ratio is equal to or higher than the lower limit, good modification and compatibilization effects can be obtained. However, if the graft ratio is too high, burning and the like increases, which adversely affects the appearance of the composition containing the modified ethylene copolymer and the molded article obtained, so that the graft ratio of the modified ethylene copolymer is preferably equal to or lower than the upper limit.
[0047] <mfr> The melt flow rate (MFR: 190°C, 2.16 kg) of the modified ethylene copolymer of the present invention is preferably 0.1 to 20 g / 10 min, more preferably 0.3 to 15 g / 10 min. When the MFR of the modified ethylene copolymer is within the above range, when the modified ethylene copolymer is added to and mixed with a polar polymer as a modifier or compatibilizer, the modified ethylene copolymer and the polar polymer are well mixed and modified, and when a molded article is formed, the appearance and mechanical properties such as impact resistance are improved.
[0048] <Biomass ratio> The biomass degree of the modified ethylene copolymer of the present invention is preferably 20 to 100%, more preferably 25 to 100%, and even more preferably 40 to 100%. When the biomass degree of the modified ethylene copolymer is 20% or more, the effect of improving the appearance and mechanical properties, especially the effect of improving the mechanical properties, by using the biomass ethylene copolymer as the raw material ethylene copolymer can be effectively obtained.
[0049] <Modified ethylene copolymer composition> When the modified ethylene copolymer of the present invention is used as a modifier or a compatibilizer, it can also be used as a modified ethylene copolymer composition containing other optional additives, polymers, etc. (hereinafter, these are referred to as "other components") according to various purposes within the range that does not significantly impair the effects of the present invention. The other components may be used alone or in any combination and ratio of two or more.
[0050] For example, the additives include heat stabilizers and antioxidants, and hindered phenols, phosphorus compounds, hindered amines, sulfur compounds, copper compounds, and alkali metal halides can be used.
[0051] The mixing method for producing a modified ethylene copolymer composition using the modified ethylene copolymer of the present invention and other components added as necessary is preferably a melt kneading method in practice. In this case, the other components may be added to the raw material ethylene copolymer before modification, and the above-mentioned graft modification may be carried out while mixing the other components, or the other components may be mixed with the modified ethylene copolymer after graft modification.
[0052] A specific example of the melt-kneading method is a method in which the modified ethylene copolymer of the present invention or the starting ethylene copolymer and other components added as necessary are uniformly mixed in a predetermined blending ratio using a Henschel mixer, a ribbon blender, a V-type blender or the like, and then kneaded using a multi-screw kneading extruder, for example, a twin-screw kneading extruder TEX25 manufactured by Japan Steel Works, Ltd.
[0053] The temperature for melt-kneading each component is, like the temperature during the above-mentioned graft modification, usually 100 to 300° C., preferably 120 to 280° C., and more preferably 150 to 260° C. Furthermore, the order and method for kneading each component are not particularly limited, and may be a method in which the modified ethylene copolymer of the present invention or the starting ethylene copolymer and other components used as necessary are kneaded all at once, or a method in which the modified ethylene copolymer of the present invention or the starting ethylene copolymer and some of the other components used as necessary are kneaded in advance, and then the remaining components are kneaded.
[0054] [Modifier] The modifier of the present invention contains the modified ethylene copolymer of the present invention.
[0055] A modifier is an additive that, when mixed with a polar polymer, can change the morphology and impart functions such as flexibility and impact resistance to the polar polymer. In the present invention, by using a modified ethylene copolymer obtained by modifying an ethylene copolymer, including a biomass ethylene copolymer, with an unsaturated carboxylic acid component, a reactive functional group of a polar polymer, such as a polyamide copolymer, reacts with the modified ethylene copolymer, and as a result, the physical properties of the polar polymer, such as a polyamide copolymer, can be modified.
[0056] The content of the modified ethylene copolymer of the present invention in the modifier of the present invention is preferably 5 to 100% by mass from the viewpoint of effectively obtaining the modifying effect of the modified ethylene copolymer of the present invention. The content of the modified ethylene copolymer of the present invention in the modifier of the present invention is more preferably 10% by mass or more, even more preferably 20% by mass or more, and particularly preferably 50% by mass or more.
[0057] [Modification method] The modification method of the present invention is a method of modifying a polar polymer in the presence of the modified ethylene copolymer of the present invention, specifically, a method of adding the modified ethylene copolymer of the present invention to a polar polymer and kneading them under heating.
[0058] Examples of polar polymers include the polyamide copolymers shown below and the ethylene-vinyl alcohol copolymers described below.
[0059] There is no particular restriction on the ratio of the amount of the modified ethylene copolymer to the polar polymer to be modified, and the polar polymer can be modified by adding a wide range of the amount of the modified ethylene copolymer from 0.1 to 50 parts by mass to 100 parts by mass of the polar polymer.
[0060] For the modification of a polar polymer, only one type of the modified ethylene copolymer of the present invention may be used, or two or more types of raw material ethylene copolymers before modification, which differ in type or physical properties, may be mixed and used. The modified ethylene copolymer of the present invention may be used as the above-mentioned modified ethylene copolymer composition.
[0061] <Polyamide polymer> As the polyamide polymer to be modified with the modified ethylene copolymer of the present invention, known polyamide polymers can be used. Specific examples include homopolymers such as polycapramide (nylon 6), poly-ω-aminoheptanoic acid (nylon 7), poly-ω-aminononanoic acid (nylon 9), polyundecaneamide (nylon 11), and polylauryllactam (nylon 12). Polyamide copolymers include polyethylenediamineadipamide (nylon 26), polytetramethyleneadipamide (nylon 46), polyhexamethyleneadipamide (nylon 66), polyhexamethylenesebacamide (nylon 610), polyhexamethylenedodecamamide (nylon 612), polyoctamethyleneadipamide (nylon 86), polydecamethyleneadipamide (nylon 108), caprolactam / lauryl la ... Caprolactam copolymer (nylon 6 / 12), caprolactam / ω-aminononanoic acid copolymer (nylon 6 / 9), caprolactam / hexamethylenediammonium adipate copolymer (nylon 6 / 66), lauryllactam / hexamethylenediammonium adipate copolymer (nylon 12 / 66), ethylenediamine adipamide / hexamethylenediammonium adipate copolymer (nylon 26 / 66), caprolactam / hexamethylenediammonium adipate copolymer (nylon 26 / 66), Examples of the polyamide include aliphatic polyamides such as ethylene diammonium adipate / hexamethylene diammonium adipate / hexamethylene diammonium sebacate copolymer (nylon 66 / 610) and ethylene ammonium adipate / hexamethylene diammonium adipate / hexamethylene diammonium sebacate copolymer (nylon 6 / 66 / 610), aromatic polyamides such as polyhexamethylene isophthalamide, polyhexamethylene terephthalamide, polymetaxylylene adipamide, hexamethylene isophthalamide / terephthalamide copolymer, poly-p-phenylene terephthalamide, and poly-p-phenylene-3,4'-diphenyl ether terephthalamide, amorphous polyamides, and polyamide-based polymers modified with aromatic amines such as methylene benzylamine and metaxylylene diamine, metaxylylene diammonium adipate, and terminal-modified polyamide-based polymers thereof. Among these, terminal-modified polyamide-based polymers are preferred.
[0062] The polyamide polymer preferably has a melt flow rate (MFR: 230°C, 2.16 kg) of 0.1 to 30 g / 10 min. When the MFR of the polyamide polymer is within the above range, it can react optimally with the modified ethylene copolymer of the present invention as a modifier, and can be modified without impairing the properties such as the fluidity of the polyamide polymer.
[0063] The polyamide polymer may be used alone or in combination of two or more types having different copolymer compositions, physical properties, and the like.
[0064] <Other ingredients> In the modification method of the present invention, a polymer composition may be prepared by mixing a polar polymer and a modified ethylene copolymer of the present invention together with a polymer other than the polar polymer and the modified ethylene copolymer of the present invention, and / or any additives (hereinafter, these are referred to as "other components") according to various purposes within a range that does not significantly impair the effects of the present invention. Only one type of other component may be used, or two or more types may be used in any combination and ratio.
[0065] Examples of additives include antioxidants, UV absorbers, plasticizers, lubricants, fillers, and antistatic agents. The total amount of these additives added in the modification method of the present invention is usually 50% by mass or less, preferably 20% by mass or less, and more preferably 10% by mass or less, as the content in the resulting polymer composition.
[0066] [Compatibilizer] The compatibilizer of the present invention contains the modified ethylene copolymer of the present invention.
[0067] The compatibilizer is an agent that makes a non-polar material and a polar material compatible with each other and has the effect of reducing the particle size of the dispersed materials.
[0068] In the present invention, by using an ethylene copolymer including a biomass ethylene copolymer modified with an unsaturated carboxylic acid component, a polar polymer such as a polyamide copolymer is finely dispersed in a non-polar polymer such as a polyolefin, and as a result, the mechanical strength and transparency of a polymer composition or recycled composition in which a polar polymer such as a polyamide copolymer is dispersed can be improved.
[0069] When the object of compatibilization is recycling, the compatibilizer of the present invention is called a recycling aid. For example, scraps generated during the process of producing a multi-layer packaging material using a non-polar polymer such as polyolefin and a polar polymer with barrier properties such as an ethylene-vinyl alcohol copolymer can be collected and pulverized to fine particles, which can then be melt-kneaded using the compatibilizer of the present invention as a recycling aid to make the non-polar polymer such as polyolefin and the polar polymer with barrier properties such as an ethylene-vinyl alcohol copolymer compatible, and the scraps can be recycled as the regrind layer of the multi-layer packaging material by granulation / molding, while suppressing the decrease in transparency and the generation of foreign matter.
[0070] In this way, by using a compatibilizer or recycling aid containing the modified ethylene copolymer of the present invention, it is possible to reduce the dispersed particle size of a barrier polar polymer such as an ethylene-vinyl alcohol copolymer present in a non-polar polymer such as polyolefin, and the effect of improving transparency and mechanical strength is obtained. In addition, since the compatibilizing effect is also exhibited for the polar groups of low molecular weight components generated in the extruder, low molecular weight components can be mixed into the regrind composition. As a result, the amount of low molecular weight components adhering as eye mucus can be reduced, and the amount of foreign matter adhering near the extrusion outlet can be reduced.
[0071] Examples of non-polar polymers include polyolefins such as polypropylene-based polymers and polyethylene-based polymers. The compatibilizer of the present invention is preferably used in the case of compatibilizing a polyethylene-based polymer with a polar polymer.
[0072] The content of the modified ethylene copolymer of the present invention in the compatibilizer of the present invention is preferably 5 to 100 mass% from the viewpoint of effectively obtaining the compatibilizing effect of the modified ethylene copolymer of the present invention, and the content of the modified ethylene copolymer of the present invention in the compatibilizer of the present invention is more preferably 10 mass% or more, even more preferably 20 mass% or more, and particularly preferably 50 mass%.
[0073] [Compatibilization method] The compatibilization method of the present invention is a method for compatibilizing a polar polymer and a non-polar polymer in the presence of the modified ethylene copolymer of the present invention.
[0074] Examples of the non-polar polymer include polyolefin polymers (a) described below, such as polypropylene polymers, polyethylene polymers, etc. The effect of the modified ethylene copolymer of the present invention is particularly effective when the polyethylene polymer is made compatible with a polar polymer. The polar polymer may be a polar polymer (b) described below, preferably a barrier polymer such as an ethylene-vinyl alcohol copolymer.
[0075] There is no particular limitation on the ratio of the polar polymer and the non-polar polymer to be made compatible. As an example of the embodiment, the polar polymer can be made compatible in a wide range of 1 to 50 parts by mass to 100 parts by mass of the non-polar polymer.
[0076] In the compatibilization method of the present invention, the amount of the modified ethylene copolymer of the present invention used is not particularly limited. As an example of the embodiment, it is preferably 0.1 to 25 parts by mass, particularly 0.5 to 15 parts by mass, and particularly 1 to 10 parts by mass, per 100 parts by mass of the non-polar polymer. If the amount of the modified ethylene copolymer used is not less than the above lower limit, the compatibilization effect of the modified ethylene copolymer can be sufficiently obtained. If the amount of the modified ethylene copolymer used is not more than the above upper limit, there is a tendency that the over-reaction between the polar polymer and the modified ethylene copolymer is easily suppressed.
[0077] The modified ethylene copolymer may be used alone or in the form of a mixture of two or more raw ethylene copolymers having different types, physical properties, etc. before modification, or may be used as the modified ethylene copolymer composition described above. In the compatibilization method of the present invention, other components than the modified ethylene copolymer of the present invention, the polar polymer and the non-polar polymer may be present in the compatibilization system.
[0078] [Polymer composition] According to the compatibilization method of the present invention, a polymer composition containing a polar polymer, a non-polar polymer, and the modified ethylene copolymer of the present invention (hereinafter, sometimes referred to as the "polymer composition of the present invention") can be obtained. The polymer composition of the present invention is preferably a polymer composition containing, per 100 parts by mass of a polyolefin polymer (a), 0.1 to 20 parts by mass of a polar polymer (b) such as an ethylene-vinyl alcohol copolymer (b1) (hereinafter, sometimes referred to as "EVOH (b1)") or a polyamide polymer (b2), and 0.1 to 25 parts by mass of the modified ethylene copolymer of the present invention.
[0079] <Polyolefin polymer (a)> Examples of the polyolefin polymer (a) include polypropylene; propylene copolymers obtained by copolymerizing propylene with an α-olefin such as ethylene, 1-butene, 1-hexene, or 4-methyl-1-pentene; polyethylenes such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, and high-density polyethylene; ethylene copolymers obtained by copolymerizing ethylene with an α-olefin such as 1-butene, 1-hexene, or 4-methyl-1-pentene; poly(1-butene), poly(4-methyl-1-pentene), and the like.
[0080] The polyolefin polymer (a) may be used alone or in the form of a mixture of two or more different polymers having different copolymer component compositions, physical properties, and the like.
[0081] Among these, as the polyolefin polymer (a), propylene-based polymers such as polypropylene and propylene-based copolymers, and ethylene-based polymers such as polyethylene and ethylene-based copolymers are preferred. From the viewpoint of obtaining a molded article having excellent heat resistance, the polyolefin polymer (a) is preferably a propylene polymer, more preferably polypropylene. From the viewpoint of obtaining a molded article having excellent transparency, the polyolefin polymer (a) is preferably an ethylene polymer, more preferably polyethylene, and even more preferably high-density polyethylene.
[0082] The melt flow rate (MFR: 190°C or 210°C, 2.16 kg) of the polyolefin polymer (a) is preferably 0.01 to 10 g / 10 min. If the MFR of the polyolefin polymer (a) is 0.01 g / 10 min or more, the difference in melt viscosity between the polar polymer (b) and the polyolefin polymer (a) is not too large, the dispersibility of the polar polymer (b) in the polymer composition is good, and the impact resistance of the obtained molded article is excellent. If the MFR of the polyolefin polymer (a) is 10 g / 10 min or less, the impact resistance of the obtained molded article is good. The MFR of the polyolefin polymer (a) is more preferably 5 g / 10 min or less, further preferably 3 g / 10 min or less, and particularly preferably 2 g / 10 min or less. When the polyolefin polymer (a) is a mixture of a plurality of kinds of polymers, the MFR of the polyolefin polymer (a) is determined as the weighted average of the MFRs of the individual polymers based on the blend mass ratio.
[0083] <Polar polymer (b)> Examples of the polar polymer (b) include barrier polar polymers such as EVOH (b1) and polyamide-based polymer (b2). Examples of the polyamide-based polymer (b2) include the polyamide-based polymers exemplified in the above-mentioned modification method of the present invention. The polar polymer (b) may be a mixture of one or more EVOH (b1) and one or more polyamide polymers (b2). When the EVOH (b1) and the polyamide polymer (b2) are used in combination, there is no particular limitation on the mixing ratio.
[0084] (EVOH(b1)) EVOH (b1) can be obtained by saponifying an ethylene-vinyl ester copolymer. A representative vinyl ester is vinyl acetate, but other fatty acid vinyl esters (vinyl propionate, vinyl pivalate, etc.) can also be used. The ethylene-vinyl ester copolymer can be produced by any known polymerization method, such as solution polymerization, suspension polymerization, emulsion polymerization, etc. The ethylene-vinyl ester copolymer can also be saponified by a known method.
[0085] The ethylene unit content of EVOH (b1), as measured based on ISO14663, is preferably 20 to 60 mol%. When the ethylene unit content is 20 mol% or more, the gas barrier property and melt moldability of EVOH (b1) in the polymer composition at high humidity are good. The ethylene unit content of EVOH (b1) is more preferably 23 mol% or more. When the ethylene unit content is 60 mol% or less, the barrier property is excellent. The ethylene unit content of EVOH (b1) is more preferably 55 mol% or less, further preferably 50 mol% or less, and particularly preferably less than 50 mol%.
[0086] The degree of saponification of the vinyl ester unit of EVOH (b1) is a value measured based on JIS K6726 (wherein EVOH is a solution uniformly dissolved in a water / methanol solvent), and from the viewpoints of barrier property, thermal stability, and moisture resistance, it is preferably 80 mol% or more, more preferably 98 mol% or more, and even more preferably 99 mol% or more.
[0087] The melt flow rate (MFR: 210°C, 2.16 kg) of EVOH (b1) is preferably 0.1 to 100 g / 10 min. If the MFR of EVOH (b1) is 100 g / 10 min or less, the difference in melt viscosity between EVOH (b1) and the acid-modified polyolefin (c) is not too large, the dispersibility of EVOH (b1) in the polymer composition is good, and the thermal stability is excellent. The MFR of EVOH (b1) is more preferably 50 g / 10 min or less, and further preferably 30 g / 10 min or less. If the MFR of EVOH (b1) is 0.1 g / 10 min or more, the difference in viscosity from the modified ethylene copolymer of the present invention is not too large, the dispersibility of EVOH (b1) in the polymer composition is good, and the impact resistance is good. The MFR of EVOH (b1) is more preferably 0.5 g / 10 min or more.
[0088] EVOH (b1) may be copolymerized with polymerizable monomers other than ethylene and vinyl esters within a range that does not impair the effects of the present invention, generally within a range of 5 mol% or less. Examples of such polymerizable monomers include α-olefins such as propylene, isobutene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-butene-1-ol, 4-pentene-1-ol, and 3-butene-1,2-diol, and hydroxyl-containing α-olefin derivatives such as their esters and acylations; hydroxymethylvinylidene diacetates such as 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyronyloxy-2-methylenepropane; unsaturated carboxylic acids or salts thereof, partial alkyl esters, complete alkyl esters, nitriles, amides, or anhydrides; unsaturated sulfonic acids or salts thereof; vinylsilane compounds; vinyl chloride; and styrene.
[0089] As the EVOH (b1), EVOH that has been "post-modified" by urethanization, acetalization, cyanoethylation, oxyalkylenation, or the like can also be used.
[0090] The EVOH (b1) may be used alone or in combination of two or more kinds having different vinyl ester types, ethylene unit contents, physical properties, and the like.
[0091] <Mixing ratio> The polymer composition of the present invention preferably contains 0.1 to 20 parts by mass of the polar polymer (b) and 0.1 to 25 parts by mass of the modified ethylene copolymer of the present invention per 100 parts by mass of the polyolefin polymer (a).
[0092] If the polar polymer (b) is less than 0.1 parts by mass, the barrier properties due to the inclusion of the polar polymer (b) cannot be sufficiently obtained. If the polar polymer (b) is more than 20 parts by mass, the impact resistance of the resulting molded article tends to decrease. The polar polymer (b) is more preferably contained in an amount of 1 to 15 parts by mass, and even more preferably 5 to 10 parts by mass, per 100 parts by mass of the polyolefin polymer (a).
[0093] If the amount of the modified ethylene copolymer of the present invention is less than 0.1 parts by mass, the effect of finely dispersing the polar polymer (b) in the polymer composition cannot be sufficiently obtained, and in particular, in the recycled composition, the decrease in transparency and the generation of foreign matter during the extrusion process cannot be sufficiently prevented. If the amount of the modified ethylene copolymer of the present invention is more than 25 parts by mass, the generation of foreign matter during the extrusion process cannot be sufficiently prevented. The modified ethylene copolymer is more preferably contained in an amount of 0.5 to 15 parts by mass, and even more preferably contained in an amount of 1 to 10 parts by mass, per 100 parts by mass of the polyolefin polymer (a).
[0094] <Other ingredients> The polymer composition of the present invention may contain, depending on various purposes, the polyolefin polymer (a), the polar polymer (b), polymers other than the modified ethylene copolymer of the present invention, and optional additives (hereinafter, these are referred to as "other components"). The other components may be used alone or in any combination and ratio of two or more.
[0095] Examples of the additives include antioxidants, ultraviolet absorbers, plasticizers, lubricants, fillers, and antistatic agents. The total content of these additives in the polymer composition of the present invention is usually 50% by mass or less, preferably 20% by mass or less, and more preferably 10% by mass or less.
[0096] <Method of producing polymer composition> There is no particular limitation on the method for mixing the components to obtain the polymer composition of the present invention, and the following methods can be mentioned. A method in which the polyolefin polymer (a), the polar polymer (b), the modified ethylene copolymer of the present invention, and other components used as necessary are dry-blended at once and melt-kneaded; A method in which the polyolefin polymer (a), the polar polymer (b), the modified ethylene copolymer of the present invention, and a part of other components used as necessary are previously melt-kneaded, and then the other components are blended and melt-kneaded; A method of blending and melt-kneading a multilayer structure containing a polyolefin polymer (a), a polar polymer (b), the modified ethylene copolymer of the present invention, and a part or all of other components used as necessary with other components:
[0097] When the modified ethylene copolymer of the present invention is used as a recycling agent, for example, a method of melt-kneading a recycled multilayer packaging material containing a polyolefin polymer (a) layer and a polar polymer (b) layer with a compatibilizer containing the modified ethylene copolymer of the present invention is suitable as a method for producing the polymer composition of the present invention. Here, the recycled multilayer packaging material refers to scraps such as burrs generated during the production of a molded product made of the multilayer packaging material, or rejected products during molding.
[0098] A specific example of the melt-kneading method is to mix the components uniformly in a predetermined mixing ratio using a Henschel mixer, a ribbon blender, a V-type blender, or the like, and then knead the components using a multi-screw kneading extruder, for example, a twin-screw kneading extruder TEX25 manufactured by Japan Steel Works.
[0099] The temperature for melt-kneading each component is usually 100 to 300°C, preferably 120 to 280°C, more preferably 150 to 260°C, similar to the temperature during graft modification of the modified ethylene copolymer of the present invention.
[0100] [Molded products] A polymer composition containing the modifier or compatibilizer of the present invention can be molded into a molded article (hereinafter, sometimes referred to as the "molded article of the present invention").
[0101] Examples of shapes of the molded article of the present invention include films, sheets, tapes, cups, trays, tubes, bottles, pipes, filaments, irregular cross-section extrusions, various irregular shapes, and the like.
[0102] There is no particular limitation on the method for molding the polymer composition, and any molding method applicable to general polymer compositions can be used. For example, extrusion molding, blow molding, injection molding, thermoforming, and the like can be mentioned.
[0103] During molding, a heat stretching treatment is often performed to improve the physical properties of the molded product or to mold it into a desired container shape. Here, the heat stretching treatment means an operation of uniformly molding a film, sheet, or parison-shaped molded product that has been uniformly heated thermally into a cup, tray, tube, bottle, or film shape by chuck, plug, vacuum force, compressed air force, blow, or the like. Examples of the stretching method include roll stretching, tenter stretching, tubular stretching, stretch blowing, vacuum molding, compressed air molding, and vacuum-compressed air molding. The stretching may be either uniaxial stretching or biaxial stretching. In the case of biaxial stretching, either simultaneous biaxial stretching or sequential biaxial stretching can be used. The stretching temperature is usually 60 to 170°C, and more preferably 80 to 160°C. EXAMPLES
[0104] Hereinafter, specific aspects of the present invention will be described in more detail using examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention. Note that the values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values of the examples.
[0105] In the following Examples and Comparative Examples, the raw materials used in the production of the modified ethylene copolymer and polymer composition are as follows.
[0106] [Raw material ethylene copolymer] <Component (A): HDPE> (Biomass ethylene copolymer) A-1: Braskem SGE7252 (MFR (190°C, load 2.16 kg): 2 g / 10 min, density: 0.952 g / cm 3 ) A-2: Braskem SHA7260 (MFR (190°C, load 2.16 kg): 20 g / 10 min, density: 0.955 g / cm 3 ) (petroleum-derived ethylene copolymer) A-3: JPE HY350 (MFR (190℃, load 2.16kg): 2g / 10min, density: 0.953g / cm 3 ) <Component (B): LLDPE> (Biomass ethylene copolymer) B-1: Braskem SLL118 (MFR (190°C, load 2.16 kg): 1 g / 10 min, density: 0.916 g / cm 3 ) B-2: Braskem SLL218 (MFR (190°C, load 2.16 kg): 2.3 g / 10 min, density: 0.918 g / cm 3 ) (petroleum-derived ethylene copolymer) B-3: SABIC M200024 (MFR (190°C, load 2.16 kg): 20 g / 10 min, density: 0.924 g / cm 3 )
[0107] <Component (C): Radical generator> Organic peroxide: Perhexa 25B, manufactured by Nippon Oil & Fats Co., Ltd.
[0108] <Component (D): Unsaturated Carboxylic Acid Component> Maleic anhydride (commercial product)
[0109] [Polyamide-based polymer composition material] Polyamide polymer: Novamid 2430J manufactured by DSM (MFR (230°C, load 2.16 kg): 2.3 g / 10 min, density: 1.14 g / cm 3 ) Modified ethylene copolymers: (A'-1) to (A'-3), (B'-1) to (B'-3) described below
[0110] [Production of modified ethylene copolymer] <Synthesis Example 1> Component (A-1): 100 parts by mass, component (C): 0.07 parts by mass, and component (D): 1.5 parts by mass were dry blended and mixed, and melt-kneaded using a twin-screw extruder (manufactured by Japan Steel Works, Ltd., TEX25αIII, D=25mmφ, L / D=52.5) at a set temperature of 260°C, a screw speed of 400 rpm, and an extrusion rate of 20 kg / h, and a pellet-shaped modified ethylene copolymer (A'-1) modified with maleic anhydride was obtained by strand cutting. The MFR (190°C, 2.16 kg) and graft ratio of the obtained modified ethylene copolymer (A'-1) were measured by the above-mentioned method. The graft ratio was measured before and after the acetone extraction of the modified ethylene copolymer after melt kneading. The value before acetone extraction is the value including grafted maleic anhydride and free maleic anhydride, and the value after acetone extraction is the value of grafted maleic anhydride. The measurement results are shown in Table 1. The modified ethylene copolymer (A'-1) was prepared by subjecting only the biomass ethylene copolymer to modification, and its biomass degree was about 96%.
[0111] <Synthesis Examples 2 to 6> Modified ethylene copolymers (A'-2), (A'-3), (B'-1), (B'-2), and (B'-3) were obtained in the same manner as in Synthesis Example 1, except that the blending compositions were changed as shown in Table 1. Using the modified ethylene copolymers obtained, the MFR (190°C, 2.16 kg) and graft ratio were measured in the same manner as in Synthesis Example 1. The measurement results are shown in Table 1. The modified ethylene copolymers (A'-2), (B'-1), and (B'-2) were prepared by modifying only biomass ethylene copolymers, and all of them had a biomass ratio of about 85% or more. However, the modified ethylene copolymers (A'-3) and (B'-3) were prepared by using only petroleum-derived ethylene copolymers, and had a biomass ratio of 0%.
[0112] [Table 1]
[0113] [Production and Evaluation of Polyamide Polymer Compositions] <Example 1> 80 parts by mass of Novamid 2430J manufactured by DSM was dry-blended with 20 parts by mass of the modified ethylene copolymer (A'-1) of Synthesis Example 1 as a modifier, and the mixture was melt-kneaded using a twin-screw extruder (TEX25αIII manufactured by Japan Steel Works, D=25mmφ, L / D=52.5) at a set temperature of 260°C, a screw speed of 400 rpm, and an extrusion rate of 20 kg / h, and a pellet-shaped sample was obtained by strand cutting. The pellet-shaped sample obtained was evaluated in the following (1) and (2). The evaluation results are shown in Table 2.
[0114] <Examples 2 and 3, Comparative Examples 1 to 3> Pellet samples were obtained in the same manner as in Example 1, except that the blending composition was changed as shown in Table 2. The obtained pellet samples were evaluated in the following (1) and (2). The evaluation results are shown in Table 2.
[0115] [Evaluation method] (1) Appearance Using a Toshiba Machine Co., Ltd. injection molding machine "IS130GN-5A," injection molded sheets with a thickness of 2 mm were produced at a molding temperature of 260°C and a screw rotation of 30%. The obtained sheets were visually compared, and if the surface was smooth, it was marked with an "O," and if it was not smooth due to surface roughness, etc., it was marked with an "X."
[0116] (2) Impact strength Using the injection molded sheet having a thickness of 2 mm produced above, the IZOD impact strength was measured with reference to JIS K7110 (1984).
[0117] [Table 2]
[0118] [Consideration] As shown in Table 2, Examples 1 to 4, which used the modified ethylene copolymer of the present invention, were excellent in appearance and impact resistance, whereas Comparative Examples 1 and 2 had good appearance but poor impact resistance. The reason why the impact resistance was good when the modified ethylene copolymer of the present invention was used is presumably because the modified ethylene copolymer of the present invention, derived from the biomass ethylene copolymer as the raw material, contained less low molecular weight components than the petroleum-derived modified ethylene copolymer used in the comparative example. That is, low molecular weight components generally have low cohesive strength and therefore cause deterioration of mechanical properties such as impact resistance, but the modified ethylene copolymer of the present invention using the biomass ethylene copolymer has less low molecular weight components and therefore has excellent mechanical properties such as impact resistance.< / mfr> < / mfr>
Claims
1. A modified ethylene copolymer obtained by modifying an ethylene copolymer including a biomass ethylene copolymer with at least one member selected from the group consisting of unsaturated carboxylic acids and derivatives thereof.
2. The modified ethylene copolymer according to claim 1, wherein the modification rate is from 0.01% by mass to 2.50% by mass.
3. The modified ethylene copolymer according to claim 1, which has a melt flow rate at 190° C. under a load of 2.16 kg of 0.1 g / 10 min or more and 20 g / 10 min or less.
4. The modified ethylene copolymer according to claim 1, wherein the ethylene copolymer is at least one selected from the group consisting of HDPE and LLDPE.
5. The modified ethylene copolymer according to claim 1, having a biomass ratio of 20 to 100%.
6. A modifier comprising the modified ethylene copolymer according to any one of claims 1 to 5.
7. A compatibilizer comprising the modified ethylene copolymer according to any one of claims 1 to 5.
8. A method for modifying a polar polymer, comprising the step of modifying the polar polymer in the presence of the modified ethylene copolymer according to any one of claims 1 to 5.
9. A method for compatibilizing a polar polymer and a non-polar polymer in the presence of the modified ethylene copolymer according to any one of claims 1 to 5.
Citation Information
Patent Citations
Polyamide resin composition with high fluidity
WO2017094720A1