Method for producing seal member
The manufacturing method for resin seal members with acid washing and crosslinking addresses the high elution issue, producing a seal member with reduced contamination risk for semiconductor applications.
Patent Information
- Application Number
- JP2023080478
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
AI Technical Summary
Resin-based seal members, such as hydrocarbon elastomers, exhibit high elution of components when in contact with chemical solutions, limiting their use in semiconductor manufacturing due to potential contamination and performance deterioration.
A manufacturing method involving a kneading step, acid washing to remove elutable components, a crosslinking agent addition, and molding process to produce a resin seal member with reduced elution properties, using hydrocarbon elastomers and carbon black filler.
The method effectively reduces the content of elutable components, resulting in a seal member with excellent low elution properties suitable for use in semiconductor manufacturing equipment and chemical solution containers, replacing more expensive perfluoro rubber members.
Smart Images

Figure 2024164773000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a seal member, and more particularly to a method for manufacturing a seal member used in a semiconductor manufacturing device or a container for a chemical liquid used in semiconductor manufacturing. [Background technology]
[0002] In the field of semiconductor manufacturing, perfluororubber sealing members are widely used as rubber elastic bodies that have excellent heat resistance, chemical resistance, non-stickiness, low friction properties, etc. For example, a perfluororubber molded body is known whose surface is covered with a sputtered film made of a polyimide polymer (Patent Document 1). In addition, a crosslinkable perfluororubber composition containing an imide-based filler such as polyimide or polyamideimide is known (Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2008-254184 A [Patent Document 2] Patent No. 5487584 Summary of the Invention [Problem to be solved by the invention]
[0004] As the sealing member, in addition to the perfluororubber sealing member, for example, a sealing member made of a resin such as a hydrocarbon-based elastomer is known. Here, in the field of semiconductor manufacturing, the sealing member used in the portion where the chemical liquid may come into contact is required to have excellent chemical resistance in particular.
[0005] Sealing members made of resins such as hydrocarbon-based elastomers are widely used in industrial equipment, chemical containers, electronic devices, etc., but they tend to have a higher tendency for components to leach out (leachability) when in contact with chemicals for long periods of time than sealing members made of perfluororubber. Therefore, in the field of semiconductor manufacturing, where the inclusion of impurities (particularly metal components) can lead to a decrease in product performance, sealing members made of resins other than perfluororubber have been limited to use in areas that do not come into contact with chemicals.
[0006] The present invention has been made to address such problems, and has an object to provide a method for manufacturing a resin sealing member having excellent low elution properties. [Means for solving the problem]
[0007] The manufacturing method of the present invention is a method for manufacturing a resin sealing member, and is characterized by comprising a kneading step of kneading a resin with a filler to obtain a kneaded mixture, an acid washing step of removing leachable components (components contained in the resin that are easily leached) from the kneaded mixture with an acid, and a molding step of molding the kneaded mixture from which the leachable components have been removed into the sealing member.
[0008] The resin has a specific gravity of less than 1.0, the filler has a specific gravity of more than 1.0, and the acid washing step is a step of immersing the kneaded mixture in the acid for washing.
[0009] The method is characterized in that a crosslinking agent kneading step is provided between the acid washing step and the molding step, in which a crosslinking agent is added to the kneaded product from which the elutable components have been removed, and the kneading is performed.
[0010] The method is characterized in that in the acid washing step, the kneaded product is washed with hydrochloric acid.
[0011] The resin is characterized in that it is a hydrocarbon-based elastomer.
[0012] The hydrocarbon elastomer is selected from the group consisting of EPM, EPDM, and EBDM.
[0013] The filler is characterized in that it is carbon black.
[0014] The sealing member is characterized in that it is a sealing member used in semiconductor manufacturing equipment or in a container for a chemical liquid used in semiconductor manufacturing. Effect of the Invention
[0015] The method for manufacturing a sealing member of the present invention includes a kneading step of kneading a resin with a filler to obtain a kneaded mixture, an acid washing step of removing leachable components from the kneaded mixture with an acid, and a molding step of molding the kneaded mixture from which the leachable components have been removed into a sealing member.Therefore, the content of leachable components in the resin molded body can be reduced, and a sealing member with excellent low leachability can be manufactured.
[0016] Since the resin has a specific gravity of less than 1.0 and the filler has a specific gravity of more than 1.0, and the acid washing step is a step of immersing the kneaded material in acid and washing it, the kneaded material is likely to settle in the acid (is not likely to float up) in the acid washing step, and the leachable components are more likely to leach into the acid. This makes it possible to manufacture a sealing member with excellent low leachability.
[0017] Between the acid washing process and the molding process, there is a crosslinking agent kneading process in which a crosslinking agent is added to the kneaded material from which the leachable components have been removed and kneaded. This means that the acid washing is performed before the resin is crosslinked, and the acid easily penetrates into the kneaded material during the acid washing, making it possible to effectively remove the leachable components.
[0018] In the acid washing step, the kneaded material is washed with hydrochloric acid, so that the washing efficiency is excellent. Specifically, hydrochloric acid is a relatively strong acid and has oxidizing properties, so that it can improve the water solubility of elutable components. Hydrochloric acid is less expensive than nitric acid or organic acids, so that it is suitable for washing methods that tend to use a relatively large amount of it, such as when washing by immersion. In addition, since the resin is a hydrocarbon-based elastomer, it has excellent heat resistance and electrical insulation properties, and can be applied to a wide range of applications. Furthermore, since the hydrocarbon-based elastomer is EPDM, it has excellent chemical resistance, and can be applied to applications in which it comes into contact with various chemical solutions. In addition, since the filler is carbon black, it is less likely to be eluted or deteriorated in the acid washing step, and the strength and durability of the sealing member can be improved.
[0019] The sealing member produced by the method of the present invention can be used in semiconductor manufacturing equipment or containers for chemicals used in semiconductor manufacturing, in place of expensive sealing members made of perfluororubber. [Brief description of the drawings]
[0020] [Figure 1] 3A to 3C are process diagrams illustrating an example of a manufacturing process for the sealing member of the present invention. [Diagram 2] 1 shows EDX spectra of a test piece before and after acid washing. [Diagram 3] 1 shows EDX spectra of a test piece before and after acid washing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The method for producing a sealing member of the present invention will be described with reference to FIG. 1. FIG. 1 shows an example of a manufacturing process for a resin sealing member. As shown in FIG. 1, the manufacturing method for a sealing member of the present invention includes a kneading step S1 in which a resin is kneaded with a filler to obtain a kneaded product (hereinafter also referred to as a compound), an acid washing step S2 in which elutable components are removed from the kneaded product with an acid (acid washing), and a molding step S4 in which the acid-washed kneaded product is molded into a sealing member. Here, in this specification, acid means an acidic liquid. Examples of the acidic liquid include an acidic liquid substance alone, an acidic solution in which an acidic substance is dissolved in a liquid, and an acidic aqueous solution in which an acidic substance is dissolved in water. Each step will be described in detail below.
[0022] <Mixing process> In the kneading step S1, first, a resin, a filler, and, if necessary, an additive are prepared as materials to be kneaded (hereinafter, also referred to as kneading materials). The amount of resin mixed can be freely set, and is preferably 50 to 90 mass % and more preferably 60 to 80 mass % based on the total amount of the kneading materials. If the amount of resin mixed is less than 50 mass %, the rubber elasticity of the sealing member will be insufficient (it will be too hard), and the sealing property will be easily deteriorated. On the other hand, if the amount of resin mixed exceeds 90 mass %, the durability of the sealing member may be deteriorated.
[0023] Here, a polymerization catalyst such as a metal catalyst may be used when the resin is synthesized by the resin manufacturer. In this case, the resin manufacturer may not remove the catalyst component from the resin after synthesis from the viewpoint of cost and may sell the product with the catalyst component remaining in the resin. In such a case, it is not easy for the purchaser of the resin product to remove impurities such as the catalyst component after purchase. Therefore, the purchaser of the resin often uses perfluororubber, which has a low content of elutable components and is excellent in low elution properties, for molding the sealing member. The reason why perfluororubber has a low content of elutable components is that it is a special resin with a high selling price, so it is easy to introduce a washing process before drying after salting out after polymerization, and the content of elutable components is low. On the other hand, with general resins, the washing process that leads to an increase in product price is easily omitted, and the resin is easily sold with the elutable components remaining in it.
[0024] As a result of conducting research into a method for allowing purchasers of resin products to easily remove leachable impurities, it was discovered that even if a resin containing a relatively large amount of impurities is used as a kneading material, a sealing member with low leachable properties can be obtained by manufacturing the sealing member in the order of a kneading process, an acid washing process, and a molding process. The present invention is based on this finding.
[0025] Examples of the resin include hydrocarbon elastomers such as olefin elastomers and styrene elastomers, polyurethane elastomers, polyester elastomers, polyvinyl chloride elastomers, silicone elastomers, nitrile rubber, and acrylic rubber.
[0026] From the viewpoint of chemical resistance, hydrocarbon-based elastomers are preferred as resins used in sealing members for semiconductor manufacturing. Examples of hydrocarbon-based elastomers include ethylene propylene rubber (EPM), ethylene propylene diene rubber (EPDM), and ethylene butene diene rubber (EBDM). EPM is a saturated rubber and cannot be crosslinked by sulfur, but is crosslinked only by peroxide crosslinking, so its applications tend to be limited. On the other hand, EPDM and EBDM are unsaturated rubbers and can be easily crosslinked by sulfur or peroxide, making them suitable for a variety of applications. When the sealing member is a crosslinked resin, the resin is unlikely to swell even when it comes into contact with a chemical solution, and is therefore considered to have excellent low elution properties.
[0027] The EPDM is not particularly limited, and a copolymer of ethylene, propylene, and a diene compound can be used. Examples of the diene compound contained in the EPDM include ethylidene norbornene (ENB), 1,4-hexadiene, and dicyclopentadiene. As long as the effect of the present invention is not impaired, the EPDM may contain structural units derived from other copolymerizable monomers.
[0028] Examples of EPDM include EP103AF and EP123 manufactured by ENEOS Materials Corporation, and EPT4021 and EPT4070H manufactured by Mitsui Chemicals, Inc. Examples of EBDM include K-9330 and K-9720 manufactured by Mitsui Chemicals, Inc. The above-mentioned resins may be used alone or in combination of two or more kinds.
[0029] Examples of the filler include inorganic fillers such as carbon black, silicon oxide, titanium oxide, and alumina, and polytetrafluoroethylene powder. The amount of the filler is, for example, 80 parts by mass or less, preferably 1 to 60 parts by mass, more preferably 10 to 60 parts by mass, and even more preferably 15 to 40 parts by mass, when the total amount of the resin is 100 parts by mass. If the amount of the filler exceeds 80 parts by mass, it tends to be difficult to knead the filler into the resin. From the viewpoint of chemical stability, the filler is preferably carbon black.
[0030] Examples of carbon black include Asahi #15, Asahi #35, and Asahi #50 manufactured by Asahi Carbon Co., Ltd., and Seast 3 and Seast S manufactured by Tokai Carbon Co., Ltd. The above-mentioned fillers may be used alone or in combination of two or more kinds.
[0031] It is preferable that the resin has a specific gravity of less than 1.0, and the filler has a specific gravity of more than 1.0. In this case, when the kneaded product is immersed in an acid (particularly an acidic aqueous solution) and washed in the acid washing step described later, it is easy to settle in the acid, and the washing effect is excellent. In particular, it is more preferable that the resin has a specific gravity of 0.80 to 0.95, and the filler has a specific gravity of 1.5 to 4.0, and it is even more preferable that the resin has a specific gravity of 0.80 to 0.90, and the filler has a specific gravity of 1.5 to 2.5. In addition to the above-mentioned resins and fillers, additives such as plasticizers, reinforcing agents, anti-aging agents, colorants, and crosslinking agents can be used as the kneading materials. In this specification, specific gravity means density measured by the method of JIS K6268, and is expressed in g / cm. 3 It is.
[0032] The kneading method may be, for example, roll kneading, kneader kneading, etc. It is preferable to knead the above-mentioned materials to be kneaded in a kneader until they become uniform to obtain a kneaded product.
[0033] <Acid washing process> In the acid washing step S2, the kneaded product obtained in the kneading step, which is the object to be washed, and an acid for removing elutable components such as metal ions from the kneaded product are prepared. The elutable components can be removed from the kneaded product by wiping with acid (wiping with a cloth impregnated with acid), spraying with acid, immersion in acid, or the like. The removal of the elutable components is preferably performed by spraying with acid or immersion in acid, since the process is simple. In this case, the kneaded product is preferably washed after being broken down into pieces of about several mm in size. From the viewpoint of the removal rate of the elutable components (cleaning efficiency), it is preferable to increase the contact area of the kneaded product with the acid. The size of the kneaded product is preferably about 1 to 8 mm, and more preferably about 1 to 5 mm. The shape of the kneaded product can be freely selected from, for example, a cube, a rectangular parallelepiped, a scale, a sphere, an oval sphere, an approximately confetti-like shape, and the like.
[0034] When the kneaded material is washed by immersion in acid, the amount of acid can be, for example, 1 to 10 times the total amount of the kneaded material. The kneaded material may be washed by leaving it in an immersed state in acid, or by immersing it while stirring at a predetermined stirring speed (for example, 100 rpm). Stirring during immersion is preferable from the viewpoint of washing efficiency, since it makes it easier for elutable components to dissolve in the acid. The temperature during washing is, for example, 5 to 100°C, and from the viewpoints of washing efficiency and safety during work, it is preferable to be 15 to 60°C.
[0035] The time for immersing the kneaded material in acid can be freely set within the range of, for example, 1 hour to 7 days, preferably 10 hours to 100 hours, and more preferably 20 hours to 60 hours. When the immersion time is 10 hours or more, the elutable components can be sufficiently removed. When the immersion time is 100 hours or less, the adsorption of the acid components to the filler can be suppressed. The kneaded material may be immersed in acid only once, or may be repeated multiple times. When the kneaded material is repeatedly immersed in acid, it is preferable to, for example, repeatedly immerse the kneaded material in acid for a predetermined time, replace the acid with new acid, and immerse again.
[0036] The acid-washed kneaded material is preferably washed with water such as pure water or ion-exchanged water by wiping, spraying, immersion, etc. The water-washed kneaded material may be left to stand in a room temperature environment and dried at room temperature (air drying), or may be dried by heating under heated conditions (for example, hot air drying). When drying by heating, the material can be dried for about 10 minutes to 3 hours at a temperature range of 50 to 200°C. The water-washed kneaded material may be subjected to acid washing again.
[0037] Examples of acidic substances used as the acid include inorganic acids such as hydrochloric acid, nitric acid, phosphoric acid, sulfuric acid, carbonic acid, and hydrofluoric acid, and organic acids such as acetic acid, oxalic acid, citric acid, and ascorbic acid. From the viewpoints of cost and acidity, it is preferable to use an aqueous solution of hydrochloric acid or nitric acid.
[0038] When an aqueous solution of hydrochloric acid is used for washing, the concentration can be, for example, 5 to 40% by mass. The concentration is preferably 10 to 36% by mass, more preferably 20 to 36% by mass, and even more preferably 30 to 35% by mass. When the hydrochloric acid concentration is 10% by mass or more, elutable components can be removed in a relatively short time. Also, when the hydrochloric acid concentration is 36% by mass or less, washing can be performed without affecting the resin.
[0039] When an aqueous solution of nitric acid is used for washing, the concentration can be, for example, 5 to 70 mass%. The concentration is preferably 5 to 65 mass%, more preferably 10 to 50 mass%, and even more preferably 10 to 40 mass%. When the nitric acid concentration is 5 mass% or more, elutable components can be removed in a relatively short time. Also, when the nitric acid concentration is 65 mass% or less, washing can be performed without affecting the resin.
[0040] <Crosslinking agent kneading process> In the manufacturing process shown in FIG. 1, between the acid washing step S2 and the molding step S4, there is a crosslinking agent kneading step S3 in which a crosslinking agent is added to the acid washed kneaded material and kneaded. Examples of the crosslinking agent include organic peroxides that easily generate peroxy radicals in the presence of heat or an oxidation-reduction system, vulcanizing agents such as sulfur and dithiodimorpholine, and hexamethylenediamine carbamate (HMDC). Examples of the organic peroxide include 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane is preferred. Examples of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane include Perhexa 25B and Perhexa 25B-40 manufactured by NOF Corporation.
[0041] The amount of the crosslinking agent is, for example, 0.05 to 10 parts by mass, preferably 1 to 5 parts by mass, and more preferably 2 to 4 parts by mass, when the total amount of the resin is taken as 100 parts by mass. The above-mentioned crosslinking agents may be used alone or in combination of two or more kinds.
[0042] The kneading method in the crosslinking agent kneading step may be, for example, roll kneading, kneader kneading, etc. The method for producing a sealing member of the present invention does not necessarily have to include the crosslinking agent kneading step S3.
[0043] <Forming process> In the molding step S4, the kneaded product in which the elutable components have been reduced by acid washing is molded into a sealing member. The kneaded product can be molded into a sealing member by a molding method such as compression molding, injection molding, extrusion molding, or transfer molding. When the molding step S4 is performed after the crosslinking agent kneading step S3, crosslinking occurs during molding of the kneaded product containing the crosslinking agent. As crosslinking conditions during molding, a crosslinking temperature of 150 to 190°C and a crosslinking time of 5 to 30 minutes are suitable for the primary crosslinking, and a crosslinking temperature of 130 to 190°C and a crosslinking time of 2 to 10 hours are suitable for the secondary crosslinking. In particular, from the viewpoint of energy saving, a crosslinking temperature of 140 to 180°C and a crosslinking time of 2 to 5 hours are preferred.
[0044] The elution property of the molded sealing member can be confirmed by elemental analysis measurement using a fluorescent X-ray analyzer (EDX). The sealing member of the present invention manufactured by the above process can reduce elements such as calcium, iron, magnesium, aluminum, silicon, potassium, sulfur, and chlorine compared to the case where the acid washing is not performed.
[0045] The sealing member of the present invention has reduced elutable components and is therefore suitable for use in parts of semiconductor manufacturing equipment that may come into contact with chemicals, and for containers for high-purity chemicals used in semiconductor manufacturing, such as resist materials, underlayer film materials, developing solutions, etching solutions, cleaning solutions, CMP slurries, etc. In particular, it can replace sealing members made of perfluororubber, for which there have been no alternatives in the past, leading to reduced costs for equipment and containers. EXAMPLES
[0046] Reference example After five types of hydrocarbon elastomers (EP103AF and EP123 manufactured by ENEOS Materials, Inc., EPT4021, EPT4070H, and K-9330 manufactured by Mitsui Chemicals, Inc.) were washed with acid, the elements contained in each resin were measured before and after the acid washing using an energy dispersive X-ray fluorescence analyzer (EDX-720 manufactured by Shimadzu Corporation). The acid washing was performed according to the following procedure. 10 g of resin was cut into approximately 5 mm squares using scissors and placed in a glass container, and 500 ml of hydrochloric acid (10% by mass) was added. The resin was left to stand for two days while immersed in hydrochloric acid. After that, the test piece was taken out and immersed in pure water to wash it, which was repeated three times while changing the pure water. The test piece after air drying was subjected to EDX measurement. EDX spectra are shown in Figures 2 and 3, and the net intensity (cps / μA) of each element detected is shown in Table 1. In Table 1, ND means below the detection limit.
[0047] [Table 1]
[0048] These results show that when resin is washed alone with acid, the metal components contained in the resin can be significantly reduced. In particular, the change in Ca (calcium) was large, while Mg (magnesium), Al (aluminum), Si (silicon), S (sulfur), and K (potassium) were reduced to below the detection limit after washing. Also, as a trend within the samples analyzed this time, EPDM manufactured by ENEOS Materials Corporation had a relatively low content of metal elements.
[0049] Example 1, Comparative Example 1 Using the kneaded materials shown below, resin molded test pieces were prepared and various evaluations were performed, such as the contained elements, basic physical properties, and heat aging tests (aging resistance). (A) Resin (EPDM) (A-1) EP103AF (manufactured by ENEOS Materials Co., Ltd., Mooney viscosity ML 1+4 (125℃) 87.0) (A-2) EP123 (manufactured by ENEOS Materials Co., Ltd., Mooney viscosity ML 1+4 (125℃) 19.5) (B) Filler (carbon black) (B-1) Asahi #35 (manufactured by Asahi Carbon Co., Ltd.) (C) Crosslinking agent (C-1) Perhexa 25B (manufactured by NOF Corporation)
[0050] The test pieces were prepared according to the following procedure. First, the resin and the filler were mixed in a predetermined ratio, and then kneaded using a rubber roll mill to obtain a compound. 20 g of the compound cut into approximately 5 mm squares using scissors was placed in a glass container, and 100 ml of hydrochloric acid (35% by mass) was added. The compound was left to stand for one day while immersed in hydrochloric acid, and then the acid was replaced with fresh hydrochloric acid of the same concentration, and the compound was left to stand for another day while immersed. In other words, the compound was subjected to two acid washes. After that, the test piece was taken out, immersed in pure water, and washed, which was repeated three times while exchanging the pure water. The compound washed with pure water was left to stand for one hour in a 150°C tank to completely dry it, and after adding a crosslinking agent and kneading it at room temperature, a resin molded body was obtained by heating and crosslinking using a molding machine. Crosslinking during molding was performed under the conditions of primary crosslinking at 170°C for approximately 15 minutes and secondary crosslinking at 150°C for approximately 4 hours. Two types of resin molded bodies were prepared: a 2 mm thick sheet sample and a large test piece (JIS K6262) for measuring compression set. In addition, a dumbbell-shaped No. 3 (JIS K6251) was prepared by punching out the 2 mm thick sheet sample.
[0051] In addition, in Comparative Example 1, a test piece was prepared in the same manner as in Example 1, except that the acid washing step was not performed. Measurement with a Curastometer (registered trademark) confirmed that both the samples of Example 1 and Comparative Example 1 were crosslinked. The composition and evaluation results of each sample are shown in Table 1. In Table 1, the numerical values of each of raw materials A to C refer to the number of parts (parts by mass) when the total amount of resin is 100 parts by mass.
[0052] The obtained test pieces were used to measure the contained elements, basic physical properties, aging resistance, and specific gravity. The contained elements were measured using an energy dispersive X-ray fluorescence analyzer, as in the reference example. The basic physical properties (initial properties) and properties after thermal aging at a temperature of 100°C for 72 hours (aging resistance) were measured by the following method. The hardness was measured at 25°C using a durometer A (JIS K6253-3). The tensile strength, elongation, tensile stress at 50% elongation (50% modulus), and tensile stress at 100% elongation (100% modulus) were measured by the method of JIS K6251. The change in rubber hardness after thermal aging is (value after thermal aging-initial value), and the tensile strength change rate and elongation change rate are [((value after thermal aging-initial value) / initial value) x 100] (JIS K6257). The specific gravity was measured by the method of JIS K6268. The compression set was measured according to the method of JIS K6262 using the following formula: [((initial thickness-thickness after test) / (initial thickness-spacer thickness))×100]. The measurement results are shown in Table 2.
[0053] [Table 2]
[0054] With regard to the amount of contained elements, it was found that Example 1, which was acid-washed, had a sulfur content that was about 30% lower, a calcium content that was about 20% lower, and an iron content that was about 50% lower than Comparative Example 1, which was not acid-washed. Furthermore, with regard to basic physical properties, aging resistance, specific gravity, and compression set, Example 1 showed results equivalent to those of Comparative Example 1. From the above results, it was confirmed that a sealing member with low elution properties can be obtained without affecting various characteristics such as basic physical properties by crosslinking and molding the kneaded material after acid washing in a compound state. [Industrial Applicability]
[0055] According to the method for producing a sealing member of the present invention, a resin sealing member with excellent low elution properties can be produced, and the sealing member can be widely used in the semiconductor manufacturing field, particularly as a member in a portion that comes into contact with semiconductor manufacturing chemicals.
Claims
1. A method for manufacturing a resin seal member, comprising the steps of: A kneading step of kneading a resin with a filler to obtain a kneaded mixture; an acid washing step of removing leachable components from the kneaded material with an acid; a molding step of molding the kneaded material from which the elutable components have been removed into the sealing member; A method for producing a sealing member, comprising the steps of:
2. The resin has a specific gravity of less than 1.0, The filler has a specific gravity greater than 1.0, 2. The method for producing a sealing member according to claim 1, wherein the acid washing step is a step of immersing the kneaded material in the acid and washing it.
3. 3. The method for producing a sealing member according to claim 1, further comprising a crosslinking agent kneading step between the acid washing step and the molding step, in which a crosslinking agent is added to the kneaded material from which leachable components have been removed, and the kneading step is performed.
4. 3. The method for producing a sealing member according to claim 1, wherein in the acid washing step, the kneaded product is washed with hydrochloric acid.
5. 3. The method for producing a seal member according to claim 1, wherein the resin is a hydrocarbon elastomer.
6. 6. The method for producing a seal member according to claim 5, wherein the hydrocarbon elastomer is EPDM.
7. 3. The method for producing a seal member according to claim 1, wherein the filler is carbon black.
8. 3. The method for producing a seal member according to claim 1, wherein the seal member is a seal member used in a semiconductor manufacturing device or a container for a chemical liquid used in semiconductor manufacturing.
Citation Information
Patent Citations
Thermometer for medical treatment
JP1979087584A
Rubber molding and o-ring using it
JP2008254184A