Method of producing alkaline red mud coating for preventing attachment of marine organism

The use of alkaline red mud modified with stearic acid and epoxy resin addresses the environmental and cost issues of existing antifouling paints, providing a sustainable and effective marine biofouling solution.

JP2024164806AActive Publication Date: 2024-11-27TAISHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024048653
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-03-25
Publication Date
2024-11-27
Estimated Expiration
2044-03-25

AI Technical Summary

Technical Problem

Existing antifouling paints for marine biofouling rely on nanomaterials and fluorine-containing substances, which are expensive and environmentally harmful, posing a pollution risk.

Method used

A method using alkaline red mud modified with stearic acid and combined with epoxy resin and a polyamide curing agent to create a low surface energy coating that prevents marine biofouling, utilizing industrial waste as a raw material.

Benefits of technology

The coating is environmentally friendly, non-toxic, and cost-effective, effectively preventing marine organism adhesion while maintaining mechanical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164806000001_ABST
    Figure 2024164806000001_ABST
Patent Text Reader

Abstract

To provide a method of producing an alkaline red mud coating for preventing attachment of marine organisms.SOLUTION: A method of producing an alkaline red mud coating includes the following steps: (1) agitating and mixing a stearic acid and an absolute ethanol to obtain a mixed solution; (2) sufficiently mixing the mixed solution and red mud powder and drying the mixture to obtain modified hydrophobic red mud powder; (3) adding a benzyl glycidyl ether to an epoxy resin, uniformly dispersing it to add hydrophobic red mud powder, uniformly continuing to disperse it, obtaining a blend to grind the blend, and obtaining an antifouling coating; and (4) when used, mixing the antifouling coating and a polyamide hardener, coating a building surface with it, and forming an alkaline red mud coating for preventing attachment of marine organisms. The obtained antifouling coating is an environmentally friendly inorganic coating with low surface energy, hydrophobicity and corrosion resistance.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of marine antifouling paints, and in particular to a method for producing alkaline red mud coatings that prevent marine biofouling. [Background technology]

[0002] Since mankind began to engage in marine-related activities, marine biological fouling has been a troublesome problem facing mankind. Coastal fouling organisms are mainly divided into two types: algae and mollusks. If these fouling organisms grow in large numbers on concrete surfaces and are not cleaned in time, they will accelerate the corrosion of underwater buildings and hinder the inspection, maintenance and repair of underwater buildings.

[0003] Methods for preventing marine fouling organisms are broadly divided into three categories: physical antifouling, chemical antifouling, and biological antifouling. Here, physical antifouling mainly uses physical methods to remove or interfere with the adhesion behavior of marine organisms, and is mostly achieved by antifouling paints. The lower the surface energy of an object, the more difficult it is for marine organisms to attach to it. Therefore, by using a material with low surface energy as a coating, it is possible to make it difficult for fouling organisms to attach and grow on it. Currently, low surface energy antifouling paints for preventing marine organisms from attaching are mainly made of nanomaterials or modified with fluorine-containing organic substances. However, nanomaterials are expensive and have limitations in practical application. Fluorine-containing substances are not only expensive, but also toxic organic substances that are prone to environmental pollution.

[0004] For example, a Chinese patent publication with the publication number CN112625595A discloses a nano-enhanced low surface energy antifouling composition and a preparation method thereof, which firstly uses a dispersant such as ethanol and propylene glycol methyl ether acetate to obtain a nano-zinc oxide slurry, and then mixes the nano-zinc oxide slurry with a resin substrate, ω-hydroxy-terminated polydimethylsiloxane, tetraethyl silicate crosslinker, dibutyltin dilaurate catalyst, and 2,4-pentanedione solvent during application. The organic-inorganic nano-composite polymer material formed by this method has good antifouling ability and scratch resistance to hard objects, but is modified by using nano-materials, has high production costs, and is difficult to widely apply, and the organic substances such as dibutyltin dilaurate used in the preparation method have long-term adverse effects on the aquatic environment. Summary of the Invention [Problem to be solved by the invention]

[0005] Based on the above technical problems, the present invention provides a method for producing an alkaline red mud coating that prevents marine biofouling. [Means for solving the problem]

[0006] The technical solutions used in the present invention are as follows: 1. A method for producing an alkaline red mud coating that inhibits marine biofouling, comprising the steps of: (1) mixing stearic acid and anhydrous ethanol by stirring to obtain a mixed solution; (2) thoroughly mixing the mixed solution in step (1) with red mud powder and drying in a drying process to obtain modified hydrophobic red mud powder; (3) adding benzyl glycidyl ether to epoxy resin and dispersing uniformly, then adding hydrophobic red mud powder in step (2) and continuing to disperse uniformly to obtain a blend, then grinding the blend to obtain an antifouling paint; (4) In use, the antifouling coating in step (4) is mixed with a polyamide hardener and applied to a building surface to form an alkaline red mud coating that prevents marine biofouling.

[0007] Preferably, in step (1), the mass ratio of stearic acid to absolute ethanol is 1:20-30.

[0008] Preferably, in step (1), stearic acid and absolute ethanol are stirred and mixed using a magnetic stirrer, and the stirring time is controlled to 40 minutes to 60 minutes.

[0009] Preferably, in step (2), the mass ratio of the mixed solution to the red mud powder is 2-3:1, and the drying process is carried out in an oven.

[0010] Preferably, in step (3), the epoxy resin is a bisphenol A epoxy resin.

[0011] Preferably, in step (3), the mixing ratio of benzyl glycidyl ether, epoxy resin and hydrophobic red mud powder is 2-6:50-70:15-20 in parts by weight.

[0012] Preferably, in step (4), the amount of the polyamide curing agent added accounts for 2 to 7% by weight of the antifouling coating material. Effect of the Invention

[0013] The beneficial technical effects of the present invention are as follows: The antifouling paint obtained by the present invention is an inorganic paint that has low surface energy, is hydrophobic and corrosion resistant, and is environmentally friendly. The coating formed by application can prevent the adhesion of marine organisms, is environmentally friendly, non-toxic, does not pollute the marine aquatic environment, and has low production costs.

[0014] The present invention creatively uses highly alkaline red mud, which is an industrial solid waste, as a raw material, and by using the red mud, which is a solid waste generated in the alumina manufacturing process, the amount of red mud deposition can be reduced, thereby reducing the manufacturing cost of the coating. At the same time, by effectively utilizing the highly alkaline characteristics of red mud, the proliferation of marine bacteria, fungi, etc. can be inhibited, and the attachment and growth of marine organisms can be effectively prevented.

[0015] The present invention uses stearic acid to modify red mud, which has high alkaline properties, to reduce the surface energy of the red mud while maintaining high alkaline properties, thereby producing a paint with low surface energy and enhancing the effect of preventing marine biofouling. In addition, stearic acid is used as the modified low surface energy material, which is non-toxic, non-polluting, and highly stable.

[0016] The present invention further blends the modified hydrophobic red mud powder with bisphenol A epoxy resin, benzyl glycidyl ether, etc., and limits the amount of each raw material used to obtain an antifouling paint, which is then mixed with a polyamide hardener and painted to obtain an alkaline red mud coating, which not only can effectively prevent the attachment and growth of marine organisms, but also has good mechanical properties. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a process flow diagram of a method for producing an anti-marine biofouling alkaline red mud coating of the present invention. [Diagram 2] FIG. 1 is a mechanism diagram of stearic acid modified red mud. [Diagram 3] FIG. 2: Micromorphology of modified hydrophobic red mud. [Figure 4] FIG. 1 is a graph showing the hydrophobicity of a water droplet on modified red mud powder. [Diagram 5] FIG. 1 is a Fourier data curve diagram of red mud and modified red mud. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Conventional methods for realizing low surface energy antifouling paints include using nanomaterials and using modifiers containing fluorine or silane. Nanomaterials are expensive, difficult to disperse, and require complicated manufacturing processes, fluorine-containing substances are toxic and harmful to the environment, and silane-containing substances have an unstable structure.

[0019] Red mud is a complex, highly alkaline industrial solid waste generated during the refining of alumina. At present, there is no suitable method for treating this waste, and if it is piled up and stored, it will cause soil pollution and will require a large amount of money for maintenance management.

[0020] Based on the above technical problems, the present invention utilizes the high alkalinity and corrosion resistance characteristics of red mud to produce a sustainable marine antifouling coating, which not only solves the problem of utilizing red mud waste, but also reduces the production cost, and the obtained antifouling coating has a high effect of preventing the attachment and growth of marine organisms.

[0021] The present invention will now be described in further detail with reference to specific examples.

[0022] Example 1 As shown in FIG. 1, a method for producing an alkaline red mud coating for preventing marine biofouling includes the following steps:

[0023] (1) Stearic acid and absolute ethanol were stirred and mixed using a magnetic stirrer to obtain a mixed solution. Here, the mass ratio of stearic acid to absolute ethanol was 1:20, and the stirring time was controlled to 40 min.

[0024] (2) The mixed solution in step (1) was thoroughly mixed with red mud powder, the mass ratio of the mixed solution to red mud powder was 2:1, and dried in an oven to obtain modified hydrophobic red mud powder.

[0025] (3) Benzyl glycidyl ether (692 diluent) was added to bisphenol A epoxy resin and dispersed uniformly at low speed using a high-speed disperser, the dispersing speed was 300 rpm. Then the hydrophobic red mud powder in step (2) was added and dispersed uniformly at high speed, the dispersing speed was 900 rpm to obtain a blend. Then the blend was ground to an appropriate fineness using a conical mill to obtain an antifouling paint.

[0026] The mixing ratio of the above benzyl glycidyl ether, bisphenol A epoxy resin and hydrophobic red mud powder was 2:50:20 by weight.

[0027] (4) During use, the antifouling paint in step (4) is mixed with a polyamide hardener, and the amount of polyamide hardener added is controlled to account for 3% of the weight of the antifouling paint. After uniform mixing, the paint is applied to the building surface to form an alkaline red mud coating that prevents marine organisms from fouling.

[0028] Research has shown that an alkaline environment has the effect of inhibiting the growth of marine bacteria, fungi, etc., and marine organisms are less likely to attach to the surface of objects with low surface energy. Therefore, red mud, which has high alkaline characteristics, can be modified with stearic acid to maintain high alkalinity and reduce the surface energy of the red mud to produce a low surface energy paint, which makes it difficult for marine organisms to attach.

[0029] The red mud used in the present invention is a waste product of the alumina manufacturing process, with a large production volume, and its high alkalinity is advantageous for preventing marine biofouling, and the use of red mud is in line with the concept of sustainable development. The present invention further uses stearic acid as a modifier to modify the high alkalinity red mud to obtain a low surface energy material, which is non-toxic, non-polluting, and highly stable.

[0030] Example 2 A method for producing an alkaline red mud coating to prevent marine biofouling, comprising the steps of:

[0031] (1) Stearic acid and absolute ethanol were stirred and mixed using a magnetic stirrer to obtain a mixed solution. Here, the mass ratio of stearic acid to absolute ethanol was 1:30, and the stirring time was controlled to 60 min.

[0032] (2) The mixed solution in step (1) was thoroughly mixed with red mud powder, the mass ratio of the mixed solution to red mud powder was 3:1, and dried in an oven to obtain modified hydrophobic red mud powder.

[0033] (3) Benzyl glycidyl ether (692 diluent) was added to bisphenol A epoxy resin and dispersed uniformly at low speed using a high-speed disperser, the dispersing speed was 300 rpm. Then the hydrophobic red mud powder in step (2) was added and dispersed uniformly at high speed, the dispersing speed was 900 rpm to obtain a blend. Then the blend was ground to an appropriate fineness using a conical mill to obtain an antifouling paint.

[0034] The mixing ratio of the above benzyl glycidyl ether, bisphenol A epoxy resin and hydrophobic red mud powder was 6:50:15 by weight.

[0035] (4) During use, the antifouling paint in step (4) is mixed with a polyamide hardener, and the amount of polyamide hardener added is controlled to account for 2% of the weight of the antifouling paint. After being mixed uniformly, the paint is applied to the building surface to form an alkaline red mud coating that prevents marine organisms from fouling.

[0036] Example 3 A method for producing an alkaline red mud coating to prevent marine biofouling, comprising the steps of:

[0037] (1) Stearic acid and absolute ethanol were stirred and mixed using a magnetic stirrer to obtain a mixed solution, where the mass ratio of stearic acid to absolute ethanol was 1:25, and the stirring time was controlled to 50 min.

[0038] (2) The mixed solution in step (1) was thoroughly mixed with red mud powder, the mass ratio of the mixed solution to red mud powder was 2.5:1, and dried in an oven to obtain modified hydrophobic red mud powder.

[0039] (3) Benzyl glycidyl ether (692 diluent) was added to bisphenol A epoxy resin and dispersed uniformly at low speed using a high-speed disperser, the dispersing speed was 250 rpm. Then the hydrophobic red mud powder in step (2) was added and dispersed uniformly at high speed, the dispersing speed was 800 rpm to obtain a blend. Then the blend was ground to an appropriate fineness using a conical mill to obtain an antifouling paint.

[0040] The mixing ratio of the above benzyl glycidyl ether, bisphenol A epoxy resin and hydrophobic red mud powder was 3:70:20 by weight.

[0041] (4) During use, the antifouling paint in step (4) is mixed with a polyamide hardener, and the amount of polyamide hardener added is controlled to account for 7% of the weight of the antifouling paint. After being mixed uniformly, the paint is applied to the building surface to form an alkaline red mud coating that prevents marine organisms from fouling.

[0042] Example 4 A method for producing an alkaline red mud coating to prevent marine biofouling, comprising the steps of:

[0043] (1) Stearic acid and absolute ethanol were stirred and mixed using a magnetic stirrer to obtain a mixed solution. Here, the mass ratio of stearic acid to absolute ethanol was 1:20, and the stirring time was controlled to 60 min.

[0044] (2) The mixed solution in step (1) was thoroughly mixed with red mud powder, the mass ratio of the mixed solution to red mud powder was 2:1, and dried in an oven to obtain modified hydrophobic red mud powder.

[0045] (3) Benzyl glycidyl ether (692 diluent) was added to bisphenol A epoxy resin and dispersed uniformly at low speed using a high-speed disperser, the dispersing speed was 300 rpm. Then the hydrophobic red mud powder in step (2) was added and dispersed uniformly at high speed, the dispersing speed was 700 rpm to obtain a blend. Then the blend was ground to an appropriate fineness using a conical mill to obtain an antifouling paint.

[0046] The mixing ratio of the above benzyl glycidyl ether, bisphenol A epoxy resin and hydrophobic red mud powder was 2:60:20 by weight.

[0047] (4) During use, the antifouling paint in step (4) is mixed with a polyamide hardener, and the amount of polyamide hardener added is controlled so that it accounts for 5% of the weight of the antifouling paint. After being mixed uniformly, the paint is applied to the building surface to form an alkaline red mud coating that prevents marine organisms from fouling.

[0048] Instead of the benzyl glycidyl ether in Examples 1 to 4 above, phenyl glycidyl ether (690 diluent) may be used.

[0049] Fig. 2 is a mechanism diagram of stearic acid modified red mud in the embodiment of the present invention. As can be seen from the diagram, stearic acid was modified and grafted onto the surface of the red mud particles.

[0050] Figure 3 shows the micro-morphology of the modified hydrophobic red mud of the present invention, i.e. the micro-structure of the modified red mud under a scanning electron microscope at 30,000x magnification. As can be seen from the figure, the red mud particles are roughly spherical, small in size, have a rough surface texture, and have inconspicuous edges. The fine particles in the red mud tend to stick together and form relatively large aggregates.

[0051] Figure 4 shows the hydrophobicity of water droplets on the modified red mud powder. As can be seen from the figure, the water droplets have a spherical shape, indicating that the modified red mud powder has a hydrophobic surface.

[0052] Figure 5 shows the Fourier data curves of red mud and modified red mud. Comparing the two curves, it can be seen that the modified red mud has two more stretching peaks at 2920 cm-1 and 2850 cm-1, which indicates that the modified red mud already has the -COOH hydrophobic group in stearic acid, and the stearic acid has been modified and grafted onto the surface of the red mud, and the red mud has been successfully modified into hydrophobic red mud.

Claims

1. 1. A method for producing an alkaline red mud coating that inhibits marine biofouling, comprising the steps of: (1) mixing stearic acid and anhydrous ethanol by stirring to obtain a mixed solution; (2) mixing the mixed solution in step (1) thoroughly with red mud powder, and drying in a drying process to obtain modified hydrophobic red mud powder; (3) adding benzyl glycidyl ether into epoxy resin and dispersing uniformly, then adding hydrophobic red mud powder in step (2) and continuing to disperse uniformly to obtain a blend, then grinding the blend to obtain an antifouling paint; (4) in use, mixing the antifouling coating in step (4) with a polyamide hardener and applying it to a building surface to form an alkaline red mud coating that prevents marine biofouling; In step (1), the mass ratio of stearic acid to anhydrous ethanol is 1:20-30; In step (2), the mass ratio of the mixed solution to the red mud powder is 2-3:1, and the drying process is carried out in an oven; In step (3), the mixing ratio of benzyl glycidyl ether, epoxy resin and hydrophobic red mud powder is 2-6:50-70:15-20 by weight, In step (4), the amount of the polyamide hardener is 2-7% by weight of the antifouling paint.

2. The method for preparing an alkaline red mud coating for preventing marine biofouling according to claim 1, characterized in that in step (1), the stearic acid and absolute ethanol are stirred and mixed using a magnetic stirrer, and the stirring time is controlled to be 40min-60min.

3. The method for producing an alkaline red mud coating for preventing marine biofouling according to claim 1, characterized in that in step (3), the epoxy resin is bisphenol A epoxy resin.