Polyethylene microporous membrane, method for manufacturing the same, and separator including that microporous membrane
The polyethylene microporous membrane with targeted physical properties and manufacturing process addresses the inverse relationship between permeability and heat resistance, achieving enhanced output and thermal safety in high-capacity batteries.
Patent Information
- Application Number
- JP2024078105
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2044-05-13
AI Technical Summary
Conventional microporous polyethylene membranes used in secondary batteries face challenges in achieving both high gas permeability and heat resistance, which are inversely related, leading to compromised thermal safety and output characteristics, especially in high-capacity and large-sized batteries.
A polyethylene microporous membrane with specific physical properties, including a thickness of 3 μm to 30 μm, perforation strength of 0.15 N/μm or more, transverse shrinkage rate of 5% or less, and a PS index of 110 or more, achieved through a manufacturing process involving sequential biaxial stretching and controlled thermal relaxation.
The membrane ensures high gas permeability, porosity, and improved heat resistance, enhancing battery output characteristics and thermal safety, particularly in high-output/high-capacity batteries, as demonstrated by passing hot-box evaluation at 125°C.
Smart Images

Figure 2024164827000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a polyethylene microporous membrane, a method for producing the same, and a separator including the microporous membrane. According to one aspect, the present disclosure relates to a polyethylene microporous membrane having significantly high gas permeability and porosity as well as improved heat resistance, a method for producing the same, and a separator including the microporous membrane. [Background technology]
[0002] Microporous polyethylene membranes are used in a variety of fields, such as separation filters, secondary battery separators, fuel cell separators, supercapacitor separators, etc. In particular, they are widely used as secondary battery separators because of their excellent electrical insulation properties, ion permeability, etc.
[0003] In recent years, secondary batteries have become larger and larger in capacity to be applied to electric vehicles, ESS (Energy Storage Systems), etc., and ensuring the safety of the battery has become an even more important factor. For example, when a battery is exposed to or operated in a high-temperature environment, the separator may shrink, causing an internal short circuit, which may cause a fire. Therefore, there is a need to develop a polyethylene microporous membrane with excellent heat resistance that can withstand the temperature rise of the battery. In addition to heat resistance, high mechanical strength is required to improve safety during the manufacturing process and use of the battery, and high permeability and high porosity are required to improve capacity and output.
[0004] In particular, in view of the recent trend toward larger and higher capacity batteries, there is a strong need to develop separators that have both higher levels of heat resistance and permeability. However, because high permeability is inversely related to excellent heat resistance and / or strength, conventional separators that have achieved high permeability have the disadvantage of reduced thermal safety, even if they have excellent capacity and output characteristics.
[0005] As a method for solving the above problems, Korean Patent Publication No. 10-2012-0032539 discloses a polyolefin microporous membrane with large pore size, excellent electrical properties, and excellent strength and low heat shrinkage. However, this microporous membrane only has a heat shrinkage rate of 20% or less in the width direction at 130°C, a porosity of 40-50%, and a gas permeability of only 100-200 sec / 100 ml, so the physical properties required for application to batteries with higher capacity and power are not sufficient.
[0006] Therefore, there is a need for the development of a microporous polyethylene membrane that has extremely high permeability and porosity, as well as significantly improved heat resistance at high temperatures. Summary of the Invention [Problem to be solved by the invention]
[0007] In order to solve the above-mentioned problems, an object of the present disclosure is to provide a polyethylene microporous membrane that has extremely high gas permeability and porosity and also has significantly improved heat resistance at high temperatures, a production method thereof, and a separator including the microporous membrane.
[0008] The separator of the present disclosure is widely applicable to the green technology field such as electric vehicles, battery charging stations, solar power generation using batteries, wind power generation, etc. In addition, the separator of the present disclosure can be used in eco-friendly electric vehicles, hybrid vehicles, etc. to reduce air pollution and greenhouse gas emissions and prevent climate change. [Means for solving the problem]
[0009] As one means for achieving the above-mentioned object, the present disclosure provides a polyethylene microporous membrane having a thickness of 3 μm to 30 μm, a puncture strength of 0.15 N / μm or more, a transverse shrinkage rate measured after standing at 121°C for 1 hour of 5% or less, and a PS index, represented by the following formula 1, of 110 or more.
[0010] [Formula 1] PS index = [gas permeability x porosity] ÷ [121°C lateral shrinkage rate]
[0011] In the above formula 1, the unit of gas permeability is "×10 -5 The unit of the shrinkage in the transverse direction at 121°C is "%".
[0012] In one embodiment, the polyethylene microporous membrane has a gas permeability of 10.0×10 -5 It could be better than Darcy.
[0013] In one embodiment, the microporous polyethylene membrane may have a porosity of 55% to 70%, specifically 60% to 70%.
[0014] In one embodiment, the polyethylene microporous membrane may have a PS index of 220 or more, specifically 400 or more.
[0015] In one embodiment, the polyethylene microporous membrane has a weight average molecular weight of 1×10 5 g / mol~10×10 5 g / mol polyethylene.
[0016] In one embodiment, the polyethylene microporous membrane may be produced by a wet process including a sequential biaxial stretching step.
[0017] In addition, as another means for achieving the above-mentioned object, the present disclosure provides a method for producing a polyethylene microporous membrane, comprising the steps of: (a) melt-kneading a mixture containing a polyethylene resin and a diluent in an extruder to produce a molten material; (b) extruding the molten material to form a sheet; (c) stretching the sheet in the longitudinal direction by at least four times its size; (d) extracting the diluent from the longitudinally stretched sheet and drying it; (e) stretching the dried sheet in the transverse direction by at least four times its size to form a film; and (f) heat-treating the transversely stretched film.
[0018] In one embodiment, the step (f) includes a heat-relaxing step in which the length in the longitudinal direction is fixed and the width in the transverse direction is reduced, and the heat-relaxing step may relax the width in the transverse direction to 80% to 95% of the width before the heat-relaxing step.
[0019] In another aspect of the present disclosure, a separator is provided comprising the microporous polyethylene membrane.
[0020] In another aspect of the present disclosure, there is provided an electrochemical device comprising the separator.
[0021] In one embodiment, the electrochemical device may be a secondary battery including the separator between a positive electrode and a negative electrode.
[0022] As another means for achieving the above-mentioned object, the present disclosure provides a separator including the above-mentioned polyethylene microporous membrane. Effect of the Invention
[0023] The polyethylene microporous membrane according to the present disclosure has high gas permeability and porosity, and can ensure significantly improved heat resistance at high temperatures.
[0024] In addition, the polyethylene microporous membrane according to the present disclosure has a puncture strength of 0.15 N / μm or more, a transverse shrinkage rate of 5% or less measured after standing at 121°C for 1 hour, and can have significantly high gas permeability and porosity.
[0025] Therefore, the present disclosure can provide a battery having improved output characteristics and thermal safety at high temperatures by including the above-mentioned polyethylene microporous membrane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The embodiments described herein may be modified into various other forms, and the technology according to one aspect is not limited to the embodiments described below. In addition, the embodiments of one aspect are provided to more completely explain the present disclosure to those having average knowledge in the art.
[0027] Additionally, as used in the specification and the appended claims, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context indicates otherwise.
[0028] In addition, the numerical ranges used herein include lower and upper limits, and all values within the ranges, increments logically derived in the form and width of the ranges defined, all values that are doubly limited, and all possible combinations of upper and lower limits of numerical ranges that are mutually limited in different ways. Unless otherwise defined herein, values outside the numerical ranges that may occur due to experimental error or rounding up are also included in the numerical ranges defined.
[0029] Furthermore, throughout the specification, unless otherwise specified to the contrary, "comprising" an element means that it may further include other elements, rather than excluding other elements.
[0030] The present disclosure provides a polyethylene microporous membrane having a thickness of 3 μm to 30 μm, a puncture strength of 0.15 N / μm or more, a transverse shrinkage rate measured after standing at 121°C for 1 hour of 5% or less, and a PS index, represented by the following formula 1, of 110 or more.
[0031] [Formula 1] PS index = [gas permeability (× 10 -5 Darcy) × void ratio (%) ÷ [121℃ transverse shrinkage rate (%)]
[0032] In recent years, secondary batteries have been required to satisfy better output characteristics and thermal safety as their capacity and size increase, and therefore separators for secondary batteries are required to have both higher levels of heat resistance and transmittance. However, conventional separators have been limited in achieving both heat resistance and transmittance at a certain level or higher because it is impossible to achieve both high transmittance and heat resistance at the same time.
[0033] As a result of extensive research, the inventors have found that it is possible to produce a polyethylene microporous membrane that has a transverse shrinkage rate of 5% or less when measured after being left at 121°C for 1 hour, a PS index of 110 or more according to Equation 1, and has extremely high gas permeability, high porosity, and extremely improved heat resistance at high temperatures.
[0034] A secondary battery according to an embodiment includes a polyethylene microporous film that satisfies both of the above-mentioned physical properties, thereby ensuring both excellent output characteristics and thermal safety. In particular, the present disclosure can provide a battery that has excellent thermal safety at high temperatures, in which the battery does not smoke or catch fire in a hot-box evaluation at a high temperature of 125°C. The manufacturing and evaluation method of the battery for the evaluation is as follows. A positive electrode using NCM622 (Ni:Co:Mn=6:2:2) as an active material and a negative electrode using graphite carbon as an active material are wound together with the microporous film of the present disclosure and placed in an aluminum pouch to manufacture a battery. Then, an electrolyte solution in which 1M lithium hexafluorophosphate (LiPF6) is dissolved in a solution containing ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate in a volume ratio of 3:5:2 is injected into the inside of the battery and sealed to prepare a battery with a capacity of 2 Ah. Next, the battery is subjected to aging and degassing, fully charged to 4.2 V, placed in an oven and heated at 5° C. / min, and left for 30 minutes after reaching 125° C., and then checked for the occurrence of smoke or fire in the battery. That is, the polyethylene microporous membrane of the present disclosure satisfies all of the above-mentioned physical properties and is therefore suitable for use in high-output / high-capacity batteries.
[0035] The above-mentioned physical properties of the polyethylene microporous membrane of the present disclosure can be achieved by, but are not necessarily limited to, performing a diluent extraction step or a transverse heat treatment step under specific conditions before the transverse stretching step in the production of the polyethylene microporous membrane.
[0036] The PS index according to formula 1 increases as the gas permeability and porosity increase and the transverse heat shrinkage decreases, and may be 110 or more. Specifically, it may be 220 or more, more specifically, 400 or more, and even more specifically, 500 or more. The higher the PS index, the more preferable it is, and the upper limit is not particularly limited, but may be, for example, 2000 or 1500. In a specific embodiment, the PS index may be 110 to 2000, 220 to 2000, 400 to 1500, or 500 to 1500, but is not limited thereto. When the PS index satisfies the above range, the gas permeability and porosity are high and the heat resistance is excellent, so that it can be suitably applied to high-output / high-capacity batteries.
[0037] In one embodiment, the polyethylene microporous membrane has a PS index in the above-mentioned range and a transverse shrinkage rate measured after standing at 121°C for 1 hour of 5% or less, 3% or less, or 2.5% or less, and the lower limit is not particularly limited, but may be, for example, 0.1%, 0.5%, or 1%. In a specific embodiment, the shrinkage rate may be 0.1% to 5%, 0.5% to 5%, 1% to 3%, or 1% to 2.5%, but is not limited thereto.
[0038] In one embodiment, the thickness of the polyethylene microporous membrane may be 3 μm to 30 μm, specifically 5 μm to 20 μm, and more specifically 5 μm to 15 μm. Even if the microporous membrane of the present disclosure has a thickness in the above range, it can achieve excellent levels of puncture strength, gas permeability, and heat shrinkage. As a result, it has excellent resistance to external stress generated during battery production, and to temperature rise and dendrites generated during battery charge and discharge, and has low internal resistance of the battery, thereby improving the charge and discharge performance of the battery.
[0039] In one embodiment, the polyethylene microporous membrane may have a puncture strength of 0.15 N / μm or more even if it has a thickness in the above range. Specifically, the puncture strength may be 0.17 N / μm or more, 0.26 N / μm or more, and the upper limit is not particularly limited, but may be, for example, 1.0 N / μm or less. In a specific embodiment, the puncture strength may be 0.15 N / μm to 1.0 N / μm, 0.17 N / μm to 1.0 N / μm, or 0.26 N / μm to 1.0 N / μm, but is not limited thereto. By satisfying the above-mentioned range of puncture strength, the membrane has excellent resistance to external stress generated during battery production and dendrites generated during battery charge and discharge, and battery safety can be ensured. In addition, the membrane can be thinned as a separator for secondary batteries, and is suitable for use in high-capacity / high-output batteries.
[0040] In one embodiment, the polyethylene microporous membrane has a porosity of 10.0 × 10 -5 Darcy or more, and specifically, the gas permeability is 15.0 × 10 -5 Darcy or higher, more specifically 20.0×10 -5 Darcy or higher, more specifically 25.0×10 -5 The upper limit of the gas permeability is not particularly limited, but may be, for example, 50.0×10 -5 Below Darcy, 40.0×10 -5 Darcy or less, or 35.0 x 10 -5 Darcy or less. In a specific embodiment, the gas permeability is 10.0×10 -5 Darcy~50.0×10 -5 Darcy, 15.0×10 -5 Darcy~50.0×10 -5 Darcy, 20.0×10 -5 Darcy~40.0×10 -5 Darcy, or 25.0×10 -5 Darcy~35.0×10 -5By satisfying the gas permeability in the above range, it is possible to have excellent ion conductivity, and the output characteristics of the battery can be significantly improved due to the low internal resistance of the battery.
[0041] In one embodiment, the polyethylene microporous membrane may have a porosity of 55% to 70%, specifically 60% to 70%. When the porosity is within the above range, the battery's internal resistance is low, and the output characteristics of the battery can be significantly improved.
[0042] In one embodiment, the polyethylene microporous membrane has a weight average molecular weight of 1×10 5 g / mol~10×10 5 g / mol of polyethylene, specifically 3×10 5 g / mol~8×10 5 g / mol polyethylene.
[0043] In one aspect, the polyethylene microporous membrane may be produced by a wet process including a successive biaxial stretching step, and a polyethylene microporous membrane satisfying all of the above-mentioned physical properties can be provided by adopting a specific step order or changing the conditions of a specific heat treatment step.
[0044] In one aspect, the polyethylene microporous membrane can be produced by a method of stretching in one direction and then extracting the diluent and stretching in the other direction, a method of sequentially biaxially stretching a film and heat-treating the film under specific conditions, or a combination thereof.
[0045] Specifically, the polyethylene microporous membrane may be produced by performing a step of extracting a diluent after longitudinal stretching and before transverse stretching in the production of a polyethylene microporous membrane, but is not necessarily limited thereto as long as a microporous membrane having the above-mentioned physical properties can be produced.
[0046] Hereinafter, the method for producing the polyethylene microporous membrane of the present disclosure will be described.
[0047] A method for producing a polyethylene microporous membrane according to one embodiment may include the steps of: (a) melt-kneading a mixture containing a polyethylene resin and a diluent in an extruder to produce a molten material; (b) extruding the molten material to form a sheet; (c) stretching the sheet in the longitudinal direction by at least four times its original size; (d) extracting the diluent from the longitudinally stretched sheet and drying it; (e) stretching the dried sheet in the transverse direction by at least four times its original size to form a film; and (f) heat-treating the film.
[0048] Unlike the conventional method in which a diluent extraction process is performed after the longitudinal and transverse stretching processes, the present disclosure performs transverse stretching after extracting the diluent from a sheet that has been completed longitudinal stretching, thereby allowing the pores to be significantly expanded by stretching, thereby producing a polyethylene microporous membrane having extremely high porosity and gas permeability, and also having high heat resistance.
[0049] Each manufacturing step will now be described.
[0050] First, step (a) is a step of melt-kneading a mixture containing a polyethylene resin and a diluent by an extruder to produce a melt, and the mixture contains the polyethylene resin and the diluent in a weight ratio of 10-60:90-40 in order to form pores, and specifically, may contain the diluent in a weight ratio of 20-40:80-60, but is not particularly limited as long as the object of the present disclosure is achieved. When the weight ratio satisfies the above range, the melt has sufficient fluidity, and a uniform sheet can be easily formed in the subsequent step, and sufficient orientation is achieved during the stretching process, and mechanical strength is easily ensured, so that problems such as breakage during the stretching process can be prevented.
[0051] The polyethylene resin may be or contain high density polyethylene from the viewpoints of strength, extrusion kneadability, stretchability, heat resistance of the final microporous membrane, and the like.
[0052] In one embodiment, the polyethylene resin has a weight average molecular weight of 1×10 5 g / mol~10×10 5 g / mol, specifically 3×10 5 g / mol~8×10 5 It may be in g / mol, but is not necessarily limited thereto.
[0053] In one embodiment, the polyethylene resin may have a melting temperature of 130° C. or higher, specifically, 130° C. to 140° C., but is not necessarily limited thereto. The melting temperature of the polyethylene resin can be measured by DSC.
[0054] In one embodiment, the diluent can be any organic compound that forms a single phase with the polyethylene resin at the extrusion temperature without any limitations. For example, the diluent may be one or a combination of two or more selected from the group consisting of aliphatic or cyclic hydrocarbons such as nonane, decane, decalin, paraffin oil, and paraffin wax; phthalic acid esters such as dibutyl phthalate and dioctyl phthalate; C10-C20 fatty acids such as palmitic acid, stearic acid, oleic acid, linoleic acid, and linolenic acid; and C10-C20 fatty alcohols such as cetyl alcohol, stearyl alcohol, and oleyl alcohol. A specific example of the diluent is paraffin oil having a kinetic viscosity at 40° C. of 20 cSt to 200 cSt, but is not limited thereto.
[0055] In addition, the mixture may further contain one or more conventional additives for improving specific functions, such as an oxidation stabilizer, a UV stabilizer, and an antistatic agent, within a range that does not significantly deteriorate the properties of the microporous membrane.
[0056] Step (b) is a step of extruding the molten material to form it into a sheet, and may be performed by any method known to those skilled in the art without limitation. For example, the molten material may be extruded through a T-die, cooled to a temperature of 10°C to 80°C, and then formed into a sheet by a casting or calendaring method.
[0057] The longitudinal stretch ratio in step (c) may be specifically 4 times or more, 4 times to 15 times, more specifically 6 times to 10 times. When the longitudinal stretch ratio satisfies the above-mentioned range, a polyethylene microporous membrane having the physical properties targeted in the present disclosure can be produced.
[0058] The stretching in step (c) may be performed by a roll method or a tenter method at a temperature in the range of 60°C lower than the melting temperature of polyethylene to the melting temperature of polyethylene. When the stretching is performed at a temperature in the above range, the fluidity of the polyethylene resin for effective stretching can be ensured. In particular, the sheet is stretched uniformly over the entire sheet, and no breakage due to stretching occurs, so that the stretching can be performed stably. This makes it possible to produce a high-quality microporous membrane having uniform physical properties such as gas permeability, punch strength, and porosity over the entire membrane. As an example, the stretching may be performed at 80°C to 140°C or 90°C to 125°C, but is not limited thereto.
[0059] Step (d) is a step of extracting and drying the diluent from the sheet stretched in the longitudinal direction, and is carried out by extracting the diluent in the film using an organic solvent, and drying the organic solvent with the film in which the diluent has been replaced with the organic solvent. The organic solvent can be used without any particular limitation as long as it can extract the diluent. Specifically, methyl ethyl ketone, methylene chloride, hexane, etc. may be used as the organic solvent because of its high extraction efficiency and fast drying.
[0060] Step (d) is preferably carried out at a high temperature due to the increased solubility of the diluent and the organic solvent, but may be carried out at a temperature of 40° C. or less from the standpoint of safety due to the boiling of the organic solvent.
[0061] Step (e) is a step of stretching the dried sheet in the transverse direction by 4 times or more to form a film, and the stretch ratio, stretching method, and stretching temperature for the transverse stretching are the same as those for the longitudinal stretching, so detailed explanations will be omitted. For example, the stretching may be performed at 80°C to 140°C or 90°C to 125°C, but is not limited thereto.
[0062] Step (f) is a step of heat-treating the film stretched in the transverse direction, which may be performed using a roll-type or tenter-type device, and may be performed at a temperature of 120°C to 140°C, for example.
[0063] In one embodiment, step (f) may include a heat-relaxing step in which the length of the transversely stretched film is fixed in the machine direction and the width of the transverse direction is relaxed (shrunk). By including the heat-relaxing step, a polyolefin microporous membrane having the physical properties targeted in the present disclosure can be produced.
[0064] Specifically, the polyethylene microporous membrane according to one embodiment is produced by including the above-mentioned heat-relaxing step, and thus has properties of increased porosity (or gas permeability) and significantly improved heat resistance. In particular, a battery using the above-mentioned microporous membrane has low initial resistance and can achieve excellent thermal safety in a hot box test.
[0065] The heat-relaxing step may be performed to relax the width in the lateral direction to 80% to 100% of the width before the heat-relaxing step.
[0066] The thermal relaxation step may be relaxation to 80% to 95% or 90% to 95% in order to more effectively achieve the physical properties targeted by the present disclosure.
[0067] In one embodiment, step (f) may include a heat stretching step of fixing the length in the machine direction of the transversely stretched film and stretching the width in the transverse direction, a heat setting step of fixing the length / width in the machine direction and applying heat, and the above-mentioned heat relaxation step. Without being limited thereto, the heat stretching step may stretch the film to 120% to 160% or 120% to 140% of the width in the transverse direction before the heat stretching step.
[0068] When the film stretched in the order of the longitudinal stretching step, the extraction step, and the transverse stretching step is heat-treated under the above-mentioned conditions, a polyethylene microporous membrane can be produced that has extremely high gas permeability and porosity as well as extremely improved heat resistance at high temperatures, contrary to the conventional belief that it is difficult to achieve both heat resistance and permeability at a certain level due to the incompatibility of high permeability and heat resistance. A microporous membrane with such properties can be suitably applied to high-power / high-capacity batteries.
[0069] The present disclosure provides a separator including the polyethylene microporous membrane as described above, and the separator may be a separator used in any known energy storage device, and is not particularly limited, but a non-limiting example is a separator used in a lithium secondary battery.
[0070] Examples and experimental examples are specifically illustrated below. However, the examples and experimental examples described below are merely a partial example, and the technology described in this specification is not limited thereto.
[0071] [Physical property measurement method] 1. Weight average molecular weight (g / mol) Weight average molecular weight (Mw) was measured using a high temperature GPC (Gel Permeation Chromatography) model name PL220 manufactured by Agilent Technologies. Analysis was performed at 140°C using PLgel Guard and PLgel Olexis as GPC columns, 1,2,4-trichlorobenzene (TCB) as a solvent, and polystyrene as a standard sample.
[0072] 2. Thickness of the microporous membrane (μm) The thickness of the microporous membrane was measured using a contact type thickness gauge with a thickness precision of 0.1 μm. The thickness was measured using a TESA μ-Hite Electronic Height Gauge manufactured by TESA Corporation at a measurement pressure of 0.63 N.
[0073] 3.Punching strength (N / μm) The puncture strength was measured by pressing the microporous membrane at a speed of 120 mm / min using a pin tip with a diameter of 1.0 mm and a curvature radius of 0.5 mm attached to an INSTRON Universal Test Machine (UTM) 3345. The puncture strength was calculated by dividing the load (N) at which the microporous membrane broke by the thickness (μm) of the microporous membrane.
[0074] 4. Gas permeability (Darcy) The gas permeability was measured using a porometer (CFP-1500-AEL, manufactured by PMI). Generally, the gas permeability is expressed by the Gurley number, but since the Gurley number does not correct for the influence of thickness, it is difficult to understand the relative permeability due to the pore structure. To solve this problem, the gas permeability of the present disclosure is measured using the Darcy permeability constant calculated by the following mathematical formula 1. Nitrogen was used as the gas, and the average value of the Darcy permeability constant measured in the range of 100 to 200 psi was calculated.
[0075] [Mathematical formula 1] Darcy transmission constant (C)=(8F·T·V) / (πD 2 (P 2 -1) F=Flow rate (cc / min) T = sample thickness (mm) V = gas viscosity (0.185 cP for N2) D = sample diameter (mm) P = pressure (psi)
[0076] 5.Porosity (%) The porosity of the microporous membrane was calculated according to the following mathematical formula 2. Specifically, a sample with a width of A cm, a length of B cm, and a thickness of T cm was prepared, and its mass was measured. The porosity was calculated from the ratio of the mass of the resin and the mass of the microporous membrane of the same volume.
[0077] [Mathematical formula 2] Porosity (%)=100×{1-M / (A×B×T×ρ)} In Equation 2, M is the mass of the microporous membrane (g), ρ is the density of the polyethylene resin constituting the microporous membrane (g / cm 3 ).
[0078] 6. Transverse shrinkage rate (%) A 15 cm x 15 cm microporous membrane with a length of 10 cm and a marking on the vertical and horizontal directions was left in an oven (Yamato Scientific Co., Ltd. DKN612) stabilized at 121°C for 1 hour, and then the change in length was measured and the horizontal shrinkage rate was calculated according to Equation 3 below.
[0079] [Mathematical formula 3] Transverse shrinkage rate (%) = {(transverse length before heating - transverse length after heating) / transverse length before heating} x 100
[0080] 7.PS Index (Performance & Safety Index) The PS index of a microporous membrane is an index for evaluating both output performance and safety, and was calculated according to the following formula 1.
[0081] [Formula 1] PS index = [gas permeability (× 10 -5 Darcy) × void ratio (%) ÷ [121℃ transverse shrinkage rate (%)]
[0082] 8.Initial resistance test The initial resistance test was performed using a battery assembled by applying a polyethylene microporous membrane to the separator. Specifically, a positive electrode using NCM622 (Ni:Co:Mn=6:2:2) as an active material and a negative electrode using graphite carbon as an active material were wound together with the prepared microporous membrane and placed in an aluminum pouch, and then an electrolyte solution in which 1M lithium hexafluorophosphate (LiPF6) was dissolved in a solution containing ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate in a volume ratio of 3:5:2 was injected and sealed to assemble a battery with a capacity of 2 Ah. After aging and degassing, the assembled battery was fully charged to 4.2 V and the initial resistance (mΩ) was measured.
[0083] If the initial resistance is 30mΩ or less, it is confirmed that the capacity is maintained at 50% or more in a 3C-rate discharge test, and the initial resistance value is used as an evaluation index for the output characteristics.
[0084] 9. Hotbox Evaluation The hot box evaluation was carried out using a battery assembled by applying a polyethylene microporous membrane to the separator. Specifically, a positive electrode using NCM622 (Ni:Co:Mn=6:2:2) as an active material and a negative electrode using graphite carbon as an active material were wound together with the prepared microporous membrane and placed in an aluminum pouch, and then an electrolyte solution in which 1M lithium hexafluorophosphate (LiPF6) was dissolved in a solution containing ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate in a volume ratio of 3:5:2 was injected and sealed to assemble a battery with a capacity of 2 Ah. After aging and degassing, the assembled battery was fully charged to 4.2 V and placed in an oven and heated at 5°C / min. After reaching 125°C, it was left for 30 minutes and the changes in the battery were measured.
[0085] If the battery emitted smoke or caught fire after being left at 125°C for 30 minutes, it was rated as Fail; if there was no change in the battery voltage / current and no smoke or fire occurred, it was rated as Pass.
[0086] <Example 1> Weight average molecular weight is 5.0×10 5 g / mol and a high-density polyethylene resin (0.95 g / cm 3 A mixture containing 30:70 by weight of 100% ethylenediaminetetraacetate (EPO) and paraffin oil having a kinematic viscosity of 80 cSt at 40°C was melt-kneaded using a twin-screw extruder to produce a melt. The melt temperature was measured using a differential scanning calorimeter (DSC) Discovery DSC250 provided by TA Instruments, with a sample weight of 5 mg and a scan rate of 10°C / min.
[0087] The melt was continuously extruded through a T-die and a casting roll set at 30° C. was used to produce a sheet having a width of 300 mm and an average thickness of 1100 μm.
[0088] The sheet was stretched in the longitudinal direction by a roll method to 7 times at a stretching temperature of 95°C, and paraffin oil was extracted from the sheet after the longitudinal stretching was completed at 25°C using methylene chloride. The sheet from which the paraffin oil was extracted was dried at 60°C. The dried sheet was stretched in the transverse direction by a tenter method to 8 times at a stretching temperature of 122°C.
[0089] The film that had been stretched in the transverse direction was heat-treated in the transverse direction at 130°C using a tenter-type heat setting device while keeping the length in the longitudinal direction fixed, to produce a microporous membrane with a thickness of 11.5 μm. In detail, the heat treatment in the transverse direction was performed by heat-stretching the film to 135% in the transverse direction, heat-setting it for 10 seconds, and then heat-relaxing (shrinking) it to 93% of the width before the heat-relaxing step.
[0090] The properties of the final microporous membrane and the performance of the battery using the same are shown in Table 1 below.
[0091] <Example 2> A microporous polyethylene membrane was produced in the same manner as in Example 1, except that the heat treatment was performed while both the longitudinal and transverse directions were fixed, and the results were recorded in Table 1.
[0092] <Comparative Example 1> Weight average molecular weight is 3.0×10 5 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that a high-density polyethylene resin having a molecular weight of 0.01 g / mol was used, the extraction step was performed after sequential stretching to 8 times in each of the machine direction and the transverse direction, and the heat treatment was performed at 130.5°C, and the results are recorded in Table 1.
[0093] <Comparative Example 2> A polyethylene microporous membrane was produced in the same manner as in Example 1, except that the membrane was successively stretched 8 times in each of the machine direction and the transverse direction, and then the extraction step was performed, and the membrane was heat-treated at 132°C to be heat-stretched to 155% in the transverse direction, heat-set for 10 seconds, and heat-relaxed (shrunk) to 97% of the width before the heat-relaxing step, and the results are recorded in Table 1.
[0094] [Table 1]
[0095] Referring to Table 1, the microporous membranes of Examples 1 and 2 had a transverse shrinkage rate of 5% or less and a PS index of 110 or more when measured after being left at 121° C. for 1 hour. As a result, the batteries using the microporous membranes had an initial resistance of 30 mΩ or less and passed the hot box test, achieving both excellent output characteristics and thermal safety.
[0096] In particular, since Example 1 was heat-treated in the horizontal direction while the length in the vertical direction was fixed, it has better gas permeability, porosity, and heat shrinkage rate than Example 2 in which heat treatment was performed while both the vertical and horizontal directions were fixed, and it can be seen that it has a PS index that is about 5 times higher than that of Example 2.
[0097] The microporous membrane of Comparative Example 1 was subjected to a diluent extraction step after the conventional longitudinal and transverse stretching steps, and the transverse shrinkage rate measured after leaving it at 121°C for 1 hour was 5% or less, but the PS index was less than 110. Therefore, the battery using it has excellent thermal safety but has the drawback of significantly reduced output characteristics.
[0098] The microporous membrane of Comparative Example 2 was subjected to a diluent extraction step after the conventional longitudinal and transverse stretching steps, and as a result, the transverse shrinkage rate measured after leaving it at 121°C for 1 hour exceeded 5% and the PS index was less than 110. Therefore, the battery using it had poor thermal safety and output characteristics.
[0099] As described above, the present disclosure has been described in the present specification by using specific details and limited embodiments, but this is merely provided for a more general understanding of the present disclosure, and the present disclosure is not limited to the above embodiments. A person having ordinary knowledge in the field to which the present disclosure belongs can make various modifications and variations from such descriptions.
Claims
1. A polyethylene microporous membrane having a thickness of 3 μm to 30 μm, a puncture strength of 0.15 N / μm or more, a transverse shrinkage rate measured after being left at 121° C. for 1 hour of 5% or less, and a PS index represented by the following formula 1 of 110 or more. [Formula 1] PS index = [gas permeability (x 10 -5 Darcy × void ratio (%) ÷ [121°C transverse shrinkage (%)]
2. Gas permeability is 10.0 x 10 -5 The polyethylene microporous membrane of claim 1, having a Darcy or greater.
3. The polyethylene microporous membrane according to claim 1, having a porosity of 55% to 70%.
4. The polyethylene microporous membrane according to claim 1, having a porosity of 60% to 70%.
5. The polyethylene microporous membrane according to claim 1, wherein the PS index is 220 or more.
6. The polyethylene microporous membrane according to claim 1, wherein the PS index is 400 or more.
7. Weight average molecular weight is 1×10 5 g / mol~10×10 5 The microporous polyethylene membrane of claim 1, comprising a polyethylene having a molecular weight of 1.0 g / mol.
8. The polyethylene microporous membrane according to claim 1, produced by a wet process including a successive biaxial stretching step.
9. (a) melt-kneading a mixture containing a polyethylene resin and a diluent in an extruder to produce a melt; (b) extruding the melt into a sheet; (c) stretching the sheet in the machine direction by at least 4 times; (d) extracting the diluent from the longitudinally stretched sheet and drying; (e) stretching the dried sheet in the transverse direction by at least 4 times to form a film; (f) heat-treating the transversely stretched film.
10. The method for producing a polyethylene microporous membrane according to claim 9, wherein the step (f) includes a heat-relaxing step of fixing the length in the longitudinal direction and shrinking the width in the transverse direction, and the heat-relaxing step relaxes the width in the transverse direction to 80% to 95% of the width before the heat-relaxing step.
11. A separator comprising the polyethylene microporous membrane according to any one of claims 1 to 8.
12. An electrochemical device comprising the separator according to claim 11.
13. 13. The electrochemical device according to claim 12, which is a secondary battery including the separator between a positive electrode and a negative electrode.
Citation Information
Patent Citations
Ultrathin high strength polyolefin microporous membrane and preparation method thereof
CN109517210A
Polyethylene microporous film excellent in high temperature strength and permeability
JP2009070823A
Microporous polyolefin film possessing good mechanical properties and thermal stability
JP2009132904A
Multilayer porous film with excellent heat resistance
JP2013517969A
Polyolefin microporous membrane, production method for polyolefin microporous membrane, battery separator, and battery
WO2017170289A1