High-strength member for automotive structural component, method for manufacturing high-strength member for automotive structural component, and method for manufacturing steel sheet for high-strength member for automotive structural component
Patent Information
- Application Number
- JP2024138387
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-06-28
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-27
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
【0027】 本発明によれば、耐遅れ破壊特性に優れた高強度部材、高強度部材の製造方法及び高強度部材用鋼板の製造方法を提供することができる。また、本発明の高強度部材を自動車構造部材に適用することにより、自動車用鋼板の高強度化と耐遅れ破壊特性向上との両立が可能となる。即ち、本発明により、自動車車体が高性能化する。
Smart Images

Figure 2024164841000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-strength member used in automobile parts, etc., a manufacturing method for the high-strength member, and a manufacturing method for a steel plate for the high-strength member. More specifically, the present invention relates to a high-strength member having excellent delayed fracture resistance and a manufacturing method thereof. The present invention also relates to a manufacturing method for a steel plate for the high-strength member. [Background technology]
[0002] In recent years, the use of high-strength steel sheets with a tensile strength (TS) of 1320 to 1470 MPa has been increasing for body frame parts such as center pillar R / F (reinforcement), bumpers, impact beam parts, etc. (hereinafter referred to as parts). Furthermore, from the viewpoint of further weight reduction of automobile bodies, the use of steel sheets with a TS of 1800 MPa (1.8 GPa) or more for parts is also being considered.
[0003] As the strength of steel plates increases, there are concerns about the occurrence of delayed fracture. In recent years, there has been concern about delayed fracture from the shear edge of samples machined into part shapes, especially from bent sections where strain is concentrated, and it has become important to suppress delayed fracture originating from such shear edge.
[0004] For example, Patent Document 1 discloses a steel having chemical compositions satisfying the following: C: 0.05-0.3%, Si: 3.0% or less, Mn: 0.01-3.0%, P: 0.02% or less, S: 0.02% or less, Al: 3.0% or less, N: 0.01% or less, with the balance being Fe and unavoidable impurities, and by specifying the grain size and density of Mg oxides, sulfides, complex crystallized products, and complex precipitates, a thin steel sheet having excellent delayed fracture resistance after forming is provided.
[0005] Patent Document 2 provides a manufacturing method for a formed part having excellent delayed fracture resistance by subjecting the sheared end surface of a steel plate having a TS of 1180 MPa or more to shot peening, thereby reducing the residual stress at the end surface. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2003-166035 A [Patent Document 2] JP 2017-125228 A Summary of the Invention [Problem to be solved by the invention]
[0007] The technology disclosed in Patent Document 1 provides a steel sheet with excellent delayed fracture resistance by specifying the chemical composition and the grain size and density of precipitates in the steel. However, the steel sheet of Patent Document 1 has a low C content, and therefore has lower strength than the steel sheet used in the high-strength member of the present invention, with a TS of less than 1470 MPa. Even if the strength of the steel sheet of Patent Document 1 is improved by increasing the C content, the residual stress at the end face also increases as the strength increases, so the delayed fracture resistance is thought to deteriorate.
[0008] In the technology disclosed in Patent Document 2, shot peening is performed on the sheared end face to reduce the residual stress on the end face and provide a formed part with excellent delayed fracture resistance. However, this is larger than the residual stress on the end face of 300 MPa or less specified in the present invention, and the effect of improving delayed fracture resistance is insufficient.
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a high-strength member excellent in delayed fracture resistance and a method for manufacturing the same.
[0010] In the present invention, high strength means that the tensile strength (TS) is 1470 MPa or more.
[0011] In the present invention, excellent delayed fracture resistance means that, as described in the Examples, when a steel sheet is bent and then immersed in hydrochloric acid of pH=1 (25°C) and the maximum load stress at which delayed fracture does not occur is measured as the critical load stress, the critical load stress is 1.10 times or more the yield strength (YS). [Means for solving the problem]
[0012] The present inventors conducted extensive research to solve the above problems. The present inventors discovered that a high-strength component having a bent ridgeline obtained using a steel plate can be made to have excellent delayed fracture resistance by making the tensile strength of the component 1470 MPa or more, making the residual stress at the end face of the bent ridgeline 300 MPa or less, and making the Vickers hardness (HV) at the end face of the bent ridgeline 200 or more and 450 or less, and thus arrived at the present invention. The above problems are solved by the following means.
[0013] [1] A high-strength component having a bent ridge line portion obtained by using a steel plate, The tensile strength of the member is 1470 MPa or more, The residual stress at the end surface of the bent ridge line is 300 MPa or less, and A high-strength member in which the end face of the bent ridge line has a Vickers hardness (HV) of 200 or more and 450 or less.
[0014] [2] The steel plate comprises, in mass%, C: 0.17% or more and 0.35% or less, Si: 0.001% or more and 1.2% or less, Mn: 0.9% or more and 3.2% or less, P: 0.020% or less, S: 0.0010% or less, Al: 0.010% or more and 0.20% or less, and N: 0.010% or less, the balance being iron and unavoidable impurities; and a microstructure in which the area ratio of one or both of bainite containing carbides having an average grain size of 50 nm or less and martensite containing carbides having an average grain size of 50 nm or less in total is 90% or more.
[0015] [3] The steel plate comprises, in mass%, C: 0.17% or more and 0.35% or less, Si: 0.001% or more and 1.2% or less, Mn: 0.9% or more and 3.2% or less, P: 0.020% or less, S: 0.0010% or less, Al: 0.010% or more and 0.20% or less, N: 0.010% or less, and Sb: 0.001% or more and 0.10% or less, with the remainder being iron and unavoidable impurities; and a microstructure in which the area ratio of one or both of bainite containing carbides having an average grain size of 50 nm or less and martensite containing carbides having an average grain size of 50 nm or less in total is 90% or more.
[0016] [4] The composition of the steel plate further comprises, in mass%, B: The high-strength member according to [2] or [3], containing 0.0002% or more and less than 0.0035%.
[0017] [5] The composition of the steel plate further comprises, in mass%, Nb: 0.002% or more and 0.08% or less; The high-strength member according to any one of [2] to [4], containing at least one selected from Ti: 0.002% or more and 0.12% or less.
[0018] [6] The composition of the steel plate further comprises, in mass%, Cu: 0.005% to 1% The high-strength member according to any one of [2] to [5], containing at least one selected from Ni: 0.005% or more and 1% or less.
[0019] [7] The composition of the steel plate further comprises, in mass%, Cr: 0.01% or more and 1.0% or less, Mo: 0.01% or more and less than 0.3% V: 0.003% or more and 0.5% or less, Zr: 0.005% or more and 0.20% or less, and W: the high-strength member according to any one of [2] to [6], containing at least one selected from 0.005% or more and 0.20% or less.
[0020] [8] The composition of the steel plate further comprises, in mass%, Ca: 0.0002% or more and 0.0030% or less, Ce: 0.0002% or more and 0.0030% or less, La: 0.0002% or more and 0.0030% or less, and The high-strength member according to any one of [2] to [7], containing at least one selected from Mg: 0.0002% or more and 0.0030% or less.
[0021] [9] The composition of the steel plate further comprises, in mass%, The high-strength member according to any one of [2] to [8], containing Sn: 0.002% or more and 0.1% or less.
[0022]
[10] A bending process step of cutting out a steel plate having a tensile strength of 1470 MPa or more and bending the steel plate; and an end surface treatment step of heating the end surface produced by the cutting at a temperature of 400°C or higher and 900°C or lower for a period longer than 0 seconds and shorter than 10 seconds after the bending process.
[0023]
[11] A bending process step of cutting out the steel plate according to any one of [2] to [9] and bending the steel plate; and an end surface treatment step of heating the end surface produced by the cutting at a temperature of 400°C or higher and 900°C or lower for a period longer than 0 seconds and shorter than 10 seconds after the bending process.
[0024]
[12] An end surface treatment process in which, after cutting out a steel plate having a tensile strength of 1470 MPa or more, the end surface resulting from the cutting is heated at a temperature of 400°C or more and 900°C or less for a period of more than 0 seconds and less than 10 seconds; and a bending process for bending the steel plate after the end face treatment process.
[0025]
[13] After cutting out the steel plate according to any one of [2] to [9], an end surface treatment process is performed in which the end surface generated by the cutting is heated at a temperature of 400°C or more and 900°C or less for a period of more than 0 seconds and not more than 10 seconds; and a bending process for bending the steel plate after the end face treatment process.
[0026]
[14] A method for producing a steel plate for high strength members, which is obtained by the method for producing a high strength member according to any one of
[10] to
[13] , a hot rolling process for hot rolling a steel material; a cold rolling step of cold rolling the hot-rolled steel sheet obtained by the hot rolling; The cold-rolled steel sheet obtained by the cold rolling is called A C3 and then, in a temperature range from the annealing temperature to 550°C, an average cooling rate is set to 3°C / sec or more and a cooling stop temperature is set to 350°C or less, and then, an annealing step is performed in which the steel sheet is held in a temperature range of 100°C or more and 260°C or less for 20 seconds or more and 1,500 seconds or less. Effect of the Invention
[0027] According to the present invention, it is possible to provide a high-strength member having excellent delayed fracture resistance, a manufacturing method for a high-strength member, and a manufacturing method for a steel plate for a high-strength member. Moreover, by applying the high-strength member of the present invention to an automobile structural member, it is possible to achieve both high strength and improved delayed fracture resistance of the steel plate for the automobile. In other words, the present invention improves the performance of automobile bodies. [Brief description of the drawings]
[0028] [Figure 1] It is a perspective view showing an example of the high-strength member of the present invention. [Diagram 2] In the example, it is a side view showing the state of the members tightened with bolts and nuts. [Diagram 3] In the measurement of the residual stress on the end face of the example, it is an enlarged view of the end face showing the measurement position at the center of the plate thickness and the measurement direction.
Mode for Carrying Out the Invention
[0029] Hereinafter, embodiments of the present invention will be described. Note that the present invention is not limited to the following embodiments.
[0030] The present invention is a high-strength member having a bent ridgeline portion obtained using a steel plate, wherein the tensile strength of the member is 1470 MPa or more, the residual stress on the end face of the bent ridgeline portion is 300 MPa or less, and the Vickers hardness (HV) on the end face of the bent ridgeline portion is 200 or more and 450 or less.
[0031] If a high-strength member satisfying these conditions is obtained, the steel plate used for the high-strength member is not particularly limited. Hereinafter, a preferable steel plate for obtaining the high-strength member of the present invention will be described, but the steel plate used for the high-strength member of the present invention is not limited to the steel plates described below.
[0032] A preferable steel plate for obtaining a high-strength member preferably has a component structure and a microstructure as described below. Note that if the high-strength member of the present invention is obtained, it is not necessarily required to use a steel plate having the component composition and microstructure described below.
[0033] First, the preferable component composition of a preferable steel plate (material steel plate) used for the high-strength member will be described. In the description of the following preferable component composition, the unit “%” of the content of the component means “mass %”.
[0034] <C: 0.17% or more and 0.35% or less> C is an element that improves hardenability. From the perspective of ensuring a total area ratio of one or both of a predetermined martensite and bainite, increasing the strength of martensite and bainite, and ensuring TS≥1470 MPa, the C content is preferably 0.17% or more, more preferably 0.18% or more, and still more preferably 0.19% or more. On the other hand, when the C content exceeds 0.35%, even if heated after bending, the residual stress at the end face of the bending ridge line portion may exceed 300 MPa, which may deteriorate the stress corrosion cracking resistance. Therefore, the C content is preferably 0.35% or less, more preferably 0.33% or less, and still more preferably 0.31% or less.
[0035] <Si: 0.001% or more and 1.2% or less> Si is a strengthening element by solid solution strengthening. Also, when the steel plate is held in a temperature range of 200°C or higher, Si contributes to the improvement of elongation by suppressing the excessive formation of coarse carbides. Furthermore, it contributes to the reduction of Mn segregation in the center of the plate thickness and the suppression of the formation of MnS, improving the stress corrosion cracking resistance. To sufficiently obtain the above effects, the Si content is preferably 0.001% or more, more preferably 0.003% or more, and still more preferably 0.005% or more. On the other hand, if the Si content becomes too high, coarse MnS is likely to form in the plate thickness direction, deteriorating the stress corrosion cracking resistance. Therefore, the Si content is preferably 1.2% or less, more preferably 1.1% or less, and still more preferably 1.0% or less.
[0036] <Mn: 0.9% or more and 3.2% or less> Mn is added to improve the hardenability of the steel and ensure a total area ratio of one or both of a predetermined martensite and bainite. If the Mn content is less than 0.9%, ferrite may be generated in the surface layer of the steel plate, which may reduce the strength. Therefore, the Mn content is preferably 0.9% or more, more preferably 1.0% or more, and still more preferably 1.1% or more. Also, in order not to increase MnS and deteriorate the stress corrosion cracking resistance, the Mn content is preferably 3.2% or less, more preferably 3.1% or less, and still more preferably 3.0% or less.
[0037] <P: 0.020% or less> P is an element that strengthens the steel, but if its content is high, it deteriorates the stress corrosion cracking resistance. Therefore, the P content is preferably 0.020% or less, more preferably 0.015% or less, and still more preferably 0.010% or less. Note that the lower limit of the P content is not particularly limited, but currently, the industrially feasible lower limit is about 0.003%.
[0038] <S: 0.0010% or less> S forms inclusions such as MnS, TiS, and Ti(C,S). In order to suppress the deterioration of the stress corrosion cracking resistance due to these inclusions, the S content is preferably 0.0010% or less. The S content is more preferably 0.0009% or less, still more preferably 0.0007% or less, and particularly preferably 0.0005% or less. Note that the lower limit of the S content is not particularly limited, but currently, the industrially feasible lower limit is about 0.0002%.
[0039] <Al: 0.010% or more and 0.20% or less> Al is added to sufficiently deoxidize and reduce coarse inclusions in the steel. To obtain its effect, the Al content is preferably 0.010% or more, more preferably 0.015% or more. On the other hand, when the Al content exceeds 0.20%, carbides mainly composed of Fe such as cementite generated during coiling after hot rolling are less likely to dissolve in the annealing process, and there is a possibility of generating coarse inclusions and carbides, which may deteriorate the delayed fracture resistance properties. Therefore, the Al content is preferably 0.20% or less, more preferably 0.17% or less, and even more preferably 0.15% or less.
[0040] <N: 0.010% or less> N is an element that forms coarse inclusions such as nitrides and carbonitrides like TiN, (Nb,Ti)(C,N), and AlN in the steel, and deteriorates the delayed fracture resistance properties through the formation of these. To prevent the deterioration of the delayed fracture resistance properties, the N content is preferably 0.010% or less, more preferably 0.007% or less, and even more preferably 0.005% or less. Note that the lower limit of the N content is not particularly limited, but currently, the industrially feasible lower limit is about 0.0006%.
[0041] <Sb: 0.001% or more and 0.10% or less> Sb suppresses oxidation and nitridation of the surface layer of the steel sheet, and suppresses decarburization due to oxidation and nitridation of the surface layer of the steel sheet. By suppressing decarburization, the formation of ferrite in the surface layer of the steel sheet is suppressed, contributing to high strength. Furthermore, the suppression of decarburization also improves the stress corrosion cracking resistance. From such a viewpoint, the Sb content is preferably 0.001% or more, more preferably 0.002% or more, and still more preferably 0.003% or more. On the other hand, if Sb is contained in an amount exceeding 0.10%, it segregates at the prior austenite (γ) grain boundaries and promotes crack generation, which may deteriorate the stress corrosion cracking resistance. Therefore, the Sb content is preferably 0.10% or less, more preferably 0.08% or less, and still more preferably 0.06% or less. Although it is preferable to contain Sb, if the effects of high strength and improvement of stress corrosion cracking resistance of the steel sheet can be sufficiently obtained without containing Sb, Sb may not be contained.
[0042] The preferred steel used for the high-strength member of the present invention preferably basically contains the above components, and the balance is iron and inevitable impurities. The preferred steel used for the high-strength member of the present invention can contain the following optional elements within a range that does not impair the action of the present invention. When the following optional element is contained in an amount less than the following lower limit value, the optional element shall be included as an inevitable impurity.
[0043] <B: 0.0002% or more and less than 0.0035%> B is an element that improves the hardenability of steel and has the advantage of generating martensite and bainite with a predetermined area ratio even when the Mn content is low. To obtain such an effect of B, the B content is preferably 0.0002% or more, more preferably 0.0005% or more, and still more preferably 0.0007% or more. Also, from the viewpoint of fixing N, it is preferable to add it in combination with 0.002% or more of Ti. On the other hand, when the B content becomes 0.0035% or more, the dissolution rate of cementite during annealing is delayed, and carbides mainly composed of Fe such as undissolved cementite remain. As a result, coarse inclusions and carbides are generated, deteriorating the stress corrosion cracking resistance. Therefore, when containing B, the B content is preferably less than 0.0035%, more preferably 0.0030% or less, and still more preferably 0.0025% or less.
[0044] <At least one selected from Nb: 0.002% or more and 0.08% or less and Ti: 0.002% or more and 0.12% or less> Nb and Ti contribute to strengthening through the refinement of prior austenite (γ) grains. From such a viewpoint, the Nb content and the Ti content are each preferably 0.002% or more, more preferably 0.003% or more, and still more preferably 0.005% or more. On the other hand, when a large amount of Nb or Ti is contained, the amount of coarse precipitates of Nb-based such as NbN, Nb(C,N), (Nb,Ti)(C,N) and Ti-based such as TiN, Ti(C,N), Ti(C,S), TiS that remain undissolved during slab heating in the hot rolling process increases, deteriorating the stress corrosion cracking resistance. For this reason, when containing Nb, the Nb content is preferably 0.08% or less, more preferably 0.06% or less, and still more preferably 0.04% or less. Also, when containing Ti, the Ti content is preferably 0.12% or less, more preferably 0.10% or less, and still more preferably 0.08% or less.
[0045] <At least one selected from Cu: 0.005% or more and 1% or less and Ni: 0.005% or more and 1% or less> Cu and Ni can improve the corrosion resistance in the usage environment of automobiles, and have the effect of suppressing hydrogen intrusion into the steel sheet by coating the surface of the steel sheet with corrosion products. Also, from the perspective of improving the stress corrosion cracking resistance, it is preferable to contain 0.005% or more of Cu and Ni respectively, and more preferably 0.008% or more. However, if there is too much Cu or Ni, it will cause the generation of surface defects and deteriorate the plating property and chemical conversion treatment property. Therefore, when containing at least one of Cu and Ni, the Cu content and Ni content are preferably 1% or less respectively, more preferably 0.8% or less, and even more preferably 0.6% or less.
[0046] <At least one selected from Cr: 0.01% or more and 1.0% or less, Mo: 0.01% or more and less than 0.3%, V: 0.003% or more and 0.5% or less, Zr: 0.005% or more and 0.20% or less, and W: 0.005% or more and 0.20% or less> Cr, Mo, and V can be contained for the purpose of improving the hardenability of steel. To obtain such an effect, the Cr content and Mo content are preferably 0.01% or more respectively, more preferably 0.02% or more, and even more preferably 0.03% or more. The V content is preferably 0.003% or more, more preferably 0.005% or more, and even more preferably 0.007% or more. However, if any of these elements is too much, the stress corrosion cracking resistance will be deteriorated due to the coarsening of carbides. Therefore, when containing Cr, the Cr content is preferably 1.0% or less, more preferably 0.4% or less, and even more preferably 0.2% or less. When containing Mo, the Mo content is preferably less than 0.3%, more preferably 0.2% or less, and even more preferably 0.1% or less. When containing V, the V content is preferably 0.5% or less, more preferably 0.4% or less, and even more preferably 0.3% or less.
[0047] Zr and W contribute to the increase in strength through the refinement of prior austenite (γ) grains. From this perspective, the Zr content and the W content are each preferably 0.005% or more, more preferably 0.006% or more, and still more preferably 0.007% or more. However, if a large amount of Zr or W is contained, the amount of coarse precipitates remaining undissolved during slab heating in the hot rolling process increases, deteriorating the stress corrosion cracking resistance. Therefore, when at least one of Zr and W is contained, the Zr content and the W content are each preferably 0.20% or less, more preferably 0.15% or less, and still more preferably 0.10% or less.
[0048] <At least one selected from among Ca: 0.0002% or more and 0.0030% or less, Ce: 0.0002% or more and 0.0030% or less, La: 0.0002% or more and 0.0030% or less, and Mg: 0.0002% or more and 0.0030% or less> Ca, Ce, and La contribute to the improvement of stress corrosion cracking resistance by fixing S as sulfides. Therefore, the content of each of these elements is preferably 0.0002% or more, more preferably 0.0003% or more, and still more preferably 0.0005% or more. On the other hand, if a large amount of these elements is added, the stress corrosion cracking resistance deteriorates due to the coarsening of sulfides. Thus, when at least one of Ca, Ce, and La is contained, the content of each of these elements is preferably 0.0030% or less, more preferably 0.0020% or less, and still more preferably 0.0010% or less.
[0049] Mg fixes O as MgO and serves as a trap site for hydrogen in steel, thus contributing to the improvement of stress corrosion cracking resistance. Therefore, the Mg content is preferably 0.0002% or more, more preferably 0.0003% or more, and still more preferably 0.0005% or more. On the other hand, if a large amount of Mg is added, the stress corrosion cracking resistance deteriorates due to the coarsening of MgO. Therefore, when Mg is contained, the Mg content is preferably 0.0030% or less, more preferably 0.0020% or less, and still more preferably 0.0010% or less.
[0050] <Sn: 0.002% or more and 0.1% or less> Sn suppresses oxidation and nitridation of the surface layer of the steel sheet, and suppresses decarburization due to oxidation and nitridation of the surface layer of the steel sheet. By suppressing decarburization, ferrite formation in the surface layer of the steel sheet is suppressed, contributing to high strength. From such a viewpoint, the Sn content is preferably 0.002% or more, more preferably 0.003% or more, and still more preferably 0.004% or more. On the other hand, when Sn is contained in an amount exceeding 0.1%, it segregates at the prior austenite (γ) grain boundaries and deteriorates the delayed fracture resistance characteristics. Therefore, when Sn is contained, the Sn content is preferably 0.1% or less, more preferably 0.08% or less, and still more preferably 0.06% or less.
[0051] Next, the preferable conditions of the microstructure of the steel sheet used for the high-strength member of the present invention will be described.
[0052] <The area ratio of one or both of bainite containing carbides with an average particle size of 50 nm or less and martensite containing carbides with an average particle size of 50 nm or less is 90% or more in total> In order to obtain a high strength of TS≧1470 MPa, it is preferable that the total area ratio of one or both of bainite containing carbides with an average particle size of 50 nm or less and martensite containing carbides with an average particle size of 50 nm or less is 90% or more with respect to the entire steel sheet structure. If it is less than this, ferrite increases and the strength decreases. Also, from the viewpoint of increasing the strength, the total area ratio is more preferably 91% or more, still more preferably 92% or more, and particularly preferably 93% or more. The total area ratio may be 100% in total. Also, the area ratio of either one may be 90% or more, or the total area ratio of both may be 90% or more.
[0053] Martensite does not include martensite as quenched, but refers to tempered martensite. In the present invention, martensite refers to a hard structure formed from austenite at low temperatures (below the martensite transformation point), and tempered martensite refers to a structure that is tempered when martensite is reheated. Bainite refers to a hard structure formed from austenite at relatively low temperatures (above the martensite transformation point) and in which fine carbides are dispersed in needle-shaped or plate-shaped ferrite.
[0054] The remaining structure other than martensite and bainite is ferrite, pearlite, and retained austenite, and the total amount of these is permissible if it is less than 10%. It may be 0%.
[0055] In the present invention, ferrite is a structure formed by transformation from austenite at relatively high temperatures and consisting of crystal grains with a bcc lattice. Pearlite is a structure formed by lamellar formation of ferrite and cementite. Retained austenite is austenite that does not transform into martensite because the martensite transformation temperature is below room temperature.
[0056] In the present invention, the carbides having an average grain size of 50 nm or less refer to fine carbides that can be observed in bainite and martensite when observed with a SEM. Specific examples of the carbides include Fe carbide, Ti carbide, V carbide, Mo carbide, W carbide, Nb carbide, and Zr carbide.
[0057] The steel sheet may have a plating layer such as a hot-dip galvanized layer. Examples of such a plating layer include an electroplated layer, an electroless plated layer, and a hot-dip plated layer. Furthermore, the steel sheet may have an alloyed plated layer.
[0058] Next, the high-strength member will be described.
[0059] The high-strength member of the present invention is a high-strength member having a bending ridge obtained by using a steel plate, in which the tensile strength of the member is 1470 MPa or more, the residual stress at the end face of the bending ridge is 300 MPa or less, and the Vickers hardness (HV) of the end face of the bending ridge is 200 or more and 450 or less.
[0060] The high-strength member of the present invention is obtained by using a steel plate, and is a formed member obtained by performing processing such as forming and bending so as to have a predetermined shape. The high-strength member of the present invention can be suitably used, for example, for automobile parts.
[0061] The high-strength member of the present invention has a bend ridgeline. In the present invention, the term "bend ridgeline" refers to a region of a steel plate that is no longer flat as a result of bending. An example of a high-strength member 10 shown in FIG. 1 is a steel plate 11 that has been V-bent. The high-strength member 10 has a bend ridgeline 12 on the side of the steel plate 11 in the bent portion. An end face 13 of the bend ridgeline 12 is a plate thickness surface located on the side of the bend ridgeline 12. The bend ridgeline direction D1 in the present invention is a direction parallel to the bend ridgeline 12.
[0062] In the high-strength member of the present invention, the bending angle is not particularly limited as long as the residual stress at the end face of the bend ridgeline is 300 MPa or less and the Vickers hardness (HV) at the end face of the bend ridgeline is 200 or more and 450 or less.
[0063] The example of the high-strength member 10 shown in FIG. 1 is an example in which one portion is bent, but two or more portions may be bent to have two or more bent ridges.
[0064] <Tensile strength of component is 1470MPa or more> The high-strength member has a tensile strength (TS) of 1470 MPa or more. In order to achieve a tensile strength (TS) of 1470 MPa or more, it is preferable to use the above steel plate. The tensile strength (TS) and yield strength (YS) in the present invention are calculated by measuring the flat portion of the high-strength member that is not bent. In addition, if the tensile strength (TS) and yield strength (YS) of the annealed steel sheet before bending (steel sheet after annealing process) are measured, these measured values can be regarded as the measured values of the tensile strength (TS) and yield strength (YS) of the high-strength member obtained using the annealed steel sheet. The strength of the member can be calculated by the method described in the Examples.
[0065] <Residual stress at the end of the bent ridge is 300MPa or less> The residual stress at the end face (plate thickness face) of the bent ridgeline of the high strength member is 300 MPa or less. This makes it difficult for cracks to occur at the end face of the bent ridgeline, so a member with excellent delayed fracture resistance can be obtained. From the viewpoint of suppressing the occurrence of cracks due to delayed fracture, the residual stress is 300 MPa or less, preferably 250 MPa or less, and more preferably 200 MPa or less. There is no particular restriction on the lower limit, and it may be a compressive stress. The residual stress at the end face of the bent ridgeline can be calculated by a method as described in the examples of this specification.
[0066] <Vickers hardness (HV) of the end face of the bent ridge is 200 to 450> The Vickers hardness (HV) of the end face (plate thickness face) of the bent ridgeline of the high strength member is 200 or more and 450 or less. This makes it difficult for cracks to occur at the end face of the bent ridgeline, so that a member with excellent delayed fracture resistance can be obtained. From the viewpoint of suppressing crack generation due to delayed fracture, the hardness is 450 or less, preferably 430 or less, and more preferably 400 or less. In addition, when the hardness of the end face of the bent ridgeline is low, the difference with the base material hardness becomes large, so that the generation of cracks is promoted. Therefore, from the viewpoint of suppressing crack generation due to delayed fracture and obtaining the strength of the member, the Vickers hardness (HV) of the end face is 200 or more. It is preferably 220 or more, and more preferably 250 or more. The Vickers hardness of the end face of the bent ridgeline can be calculated by a method as described in the examples of this specification.
[0067] Next, an embodiment of the method for producing a high-strength component of the present invention will be described.
[0068] One example of an embodiment of a manufacturing method for a high-strength member of the present invention includes a bending process in which a steel plate having a tensile strength of 1470 MPa or more is cut out and bent, and an end surface treatment process in which the end surfaces resulting from the cutting are heated at a temperature of 400°C or more and 900°C or less for more than 0 seconds and not more than 10 seconds after the bending process.
[0069] Another example of an embodiment of the manufacturing method for a high-strength member of the present invention includes a bending process of cutting out a steel plate having the above-mentioned composition and microstructure and bending the steel plate, and an end surface treatment process of heating the end surface generated by the cutting at a temperature of 400°C or more and 900°C or less under conditions of more than 0 seconds and not more than 10 seconds after the bending process.
[0070] Another example of an embodiment of the manufacturing method for a high-strength member of the present invention includes an end face treatment step in which a steel plate having a tensile strength of 1470 MPa or more is cut out, and then the end face resulting from the cutting is heated at a temperature of 400°C or more and 900°C or less for more than 0 seconds and not more than 10 seconds, and a bending step in which the steel plate after the end face treatment step is bent.
[0071] Another example of an embodiment of the method for producing a high-strength member of the present invention includes an end surface treatment step in which a steel plate having the above-mentioned composition and microstructure is cut out, and then the end surface resulting from the cutting is heated at a temperature of 400°C or higher and 900°C or lower for longer than 0 seconds and shorter than 10 seconds, and a bending step in which the steel plate after the end surface treatment step is bent.
[0072] [End surface processing process] As described above, the manufacturing method of the high-strength member of the present invention includes an end surface treatment step of cutting a steel plate and then heating the end surface resulting from the cutting at a temperature of 400°C or more and 900°C or less for more than 0 seconds and not more than 10 seconds. Here, the steel plate to be cut out is, for example, a steel plate having a tensile strength of 1470 MPa or more. In addition, the steel plate to be cut out is, for example, a steel plate having the above-mentioned composition and microstructure.
[0073] Cutting in the present invention includes known cutting methods such as shear cutting (mechanical cutting), laser cutting, electrical cutting such as electric discharge machining, and gas cutting.
[0074] By carrying out the end surface treatment process, residual stress at the end surface of the steel sheet is reduced, and the end surface is softened, making it difficult for cracks to occur at the end surface of the bending ridge line, and a member having excellent delayed fracture resistance can be obtained. The method for heating the end surface is not particularly limited, and for example, heating with a laser is available.
[0075] In order to reduce the residual stress at the end face, the end face of the formed part after bending the steel sheet is heated at a temperature of 400°C or more and 900°C or less. If the heating temperature exceeds 900°C, the formation and coarsening of ferrite becomes significant, so the strength of the formed part decreases, and the part becomes too soft, which deteriorates the delayed fracture resistance. Therefore, the heating temperature is 900°C or less, preferably 870°C or less. If the heating temperature is less than 400°C, the heating capacity is insufficient and the structure does not soften. Therefore, the heating temperature is 400°C or more. It is preferably 450°C or more, more preferably 500°C or more, even more preferably more than 600°C, and particularly preferably 700°C or more. The heating time is 10 seconds or less. If the heating time exceeds 10 seconds, the structure becomes coarse and the delayed fracture resistance deteriorates. Therefore, the heating time is 10 seconds or less. It is preferably 9 seconds or less, more preferably 8 seconds or less. The heating time is not particularly limited as long as the structure is softened and the Vickers hardness of the end face is 200 to 450. Therefore, the heating time is more than 0 seconds, preferably 1 second or more, and more preferably 2 seconds or more.
[0076] The heating range is not particularly limited, but is preferably about 5 mm from the end face of the bent ridge to ensure the strength of the formed part. The heating direction is not particularly limited, but is preferably perpendicular to the plate thickness to eliminate temperature variation in the plate thickness direction.
[0077] [Bending process] The method for producing a high-strength member of the present invention includes a bending step of bending a steel plate. The bending step may be performed before or after the end face treatment step.
[0078] The bending process of the present invention includes at least one of four deformation modes classified into bending deformation, deep drawing deformation, stretch flange deformation, and stretch flange deformation, for example.
[0079] Next, an embodiment of a method for producing a steel plate for high strength members used in the high strength members obtained by the method for producing a high strength member will be described.
[0080] In addition, one example of an embodiment of the manufacturing method of the steel plate for high strength members of the present invention includes a hot rolling step of hot rolling steel (steel material), a cold rolling step of cold rolling the hot rolled steel plate obtained by the hot rolling, and a cold rolling step of rolling the cold rolled steel plate obtained by the cold rolling. C3 The method includes an annealing step in which the steel sheet is heated to an annealing temperature of at least 550°C, and then cooled at an average cooling rate of at least 3°C / sec in the temperature range from the annealing temperature to 550°C, with the cooling stop temperature being at most 350°C, and then held at a temperature range of at least 100°C and at most 260°C for at least 20 seconds and at most 1,500 seconds.
[0081] These steps and a preferred casting step carried out before the hot rolling step will be described below. Note that the temperatures shown below refer to the surface temperatures of the steel material (slab), steel plate, etc. unless otherwise specified.
[0082] [Casting process] A steel having the above-mentioned composition is cast. The casting speed is not particularly limited, but in order to suppress the formation of the above-mentioned inclusions and improve the delayed fracture resistance, the casting speed is preferably 1.80 m / min or less, more preferably 1.75 m / min or less, and even more preferably 1.70 m / min or less. There is no particular lower limit, but from the viewpoint of productivity, it is preferably 1.25 m / min or more, and more preferably 1.30 m / min or more.
[0083] [Hot rolling process] In the hot rolling process, for example, a steel material (slab) having the above-mentioned composition is hot rolled. The slab heating temperature is not particularly limited, but by setting the slab heating temperature at 1200°C or higher, the solid solution of sulfides is promoted and Mn segregation is reduced, the amount of the above-mentioned coarse inclusions is reduced, and the delayed fracture resistance tends to be improved. For this reason, the slab heating temperature is preferably 1200°C or higher, and more preferably 1220°C or higher. In addition, the heating rate during slab heating is preferably 5 to 15°C / min, and the slab soaking time is preferably 30 to 100 minutes.
[0084] The finish rolling end temperature is preferably 840°C or higher. If the finish rolling end temperature is less than 840°C, it takes a long time for the temperature to drop, and inclusions are generated, which not only deteriorates the delayed fracture resistance but also may deteriorate the internal quality of the steel sheet. Therefore, the finish rolling end temperature is preferably 840°C or higher, more preferably 860°C or higher. On the other hand, although there is no particular upper limit, the finish rolling end temperature is preferably 950°C or lower, more preferably 920°C or lower, since it becomes difficult to cool the steel sheet to the coiling temperature later.
[0085] The cooled hot-rolled steel sheet is preferably coiled at a temperature of 630°C or less. If the coiling temperature exceeds 630°C, the surface of the base steel may be decarburized, which may cause a difference in structure between the inside and the surface of the steel sheet and may cause uneven alloy concentration. In addition, the surface decarburization reduces the area ratio of bainite and martensite having carbides in the surface layer of the steel, which tends to make it difficult to ensure the desired strength. Therefore, the coiling temperature is preferably 630°C or less, and more preferably 600°C or less. The lower limit of the coiling temperature is not particularly limited, but it is preferably 500°C or more to prevent a decrease in cold rolling properties.
[0086] [Cold rolling process] In the cold rolling process, the hot-rolled steel sheet obtained by hot rolling is cold-rolled. In the cold rolling process, for example, the hot-rolled steel sheet wound as described above is pickled and then cold-rolled to produce a cold-rolled steel sheet. The pickling conditions are not particularly limited. If the rolling reduction is less than 20%, there is a risk that the surface flatness will be poor and the structure will be non-uniform, so the rolling reduction is preferably 20% or more, more preferably 30% or more, and even more preferably 40% or more.
[0087] [Annealing process] The cold-rolled steel sheet obtained by cold rolling is called A C3 Heat to an annealing temperature above the A point. C3 Below this point, ferrite will form in the structure and the desired strength will not be obtained. C3 5.0 or more points, preferably A C3 point +10℃ or higher, more preferably A C3 The annealing temperature is preferably 900°C or lower from the viewpoint of suppressing the coarsening of austenite and preventing the deterioration of delayed fracture resistance. C3 After heating to an annealing temperature equal to or higher than the annealing point, the steel sheet may be soaked at the annealing temperature.
[0088] A C3 The points are calculated by the following formula: In the formula, (% element symbol) means the content (mass %) of each element. A C3 Point (℃)=910-203√(%C)+45(%Si)-30(%Mn)-20(%Cu)-15(%Ni)+11(%Cr)+32(%Mo)+104(%V)+400(%Ti)+460(%Al)
[0089] As mentioned above, cold-rolled steel sheet A C3 After heating to an annealing temperature equal to or higher than the annealing temperature point, cooling is performed at an average cooling rate of 3°C / sec or more in the temperature range from the annealing temperature to 550°C, and the cooling stop temperature is set to 350°C or less, and then the material is held in a temperature range of 100°C to 260°C for 20 seconds to 1,500 seconds.
[0090] If the average cooling rate in the temperature range from the annealing temperature to 550°C is less than 3°C / s, excessive generation of ferrite occurs, making it difficult to obtain the desired strength. Furthermore, the generation of ferrite in the surface layer makes it difficult to obtain a fraction of bainite or martensite having carbides near the surface layer, deteriorating the delayed fracture resistance. Therefore, the average cooling rate in the temperature range from the annealing temperature to 550°C is 3°C / s or more, preferably 5°C / s or more, and more preferably 10°C / s or more. Although there is no particular upper limit for the average cooling rate, if the rate is too fast, the martensite transformation in the coil width direction is likely to become non-uniform, and the steel sheet may come into contact with the equipment due to shape deterioration, so it is preferable to set the rate to 3000°C / s or less from the viewpoint of obtaining the minimum shape.
[0091] Unless otherwise specified, the average cooling rate in the temperature range from the annealing temperature to 550°C is "(annealing temperature - 550°C) / (cooling time from the annealing temperature to 550°C)".
[0092] The cooling stop temperature is 350°C or less. If the cooling stop temperature exceeds 350°C, tempering does not proceed sufficiently, and as-quenched martensite and residual austenite are generated in the final structure, and the hardness of the end face of the bend ridge line increases, deteriorating the delayed fracture resistance. Therefore, in order to obtain excellent delayed fracture resistance, the cooling stop temperature is 350°C or less, preferably 300°C or less, and more preferably 250°C or less. The lower limit of the cooling stop temperature is not particularly limited, but from the viewpoint of easily securing the temperature when reheating thereafter, 0°C or more is preferable.
[0093] The carbides distributed inside the bainite are formed during holding at low temperatures after quenching, and act as hydrogen trapping sites to capture hydrogen and prevent deterioration of delayed fracture resistance. If the holding temperature is less than 100°C or the holding time is less than 20 seconds, bainite is not formed and as-quenched martensite containing no carbides is formed, which increases the hardness of the end face of the bend ridgeline and prevents the above effect from being obtained.
[0094] Furthermore, if the holding temperature exceeds 260°C or the holding time exceeds 1500 seconds, decarburization occurs and coarse carbides are generated inside the bainite, causing excessive softening and deteriorating delayed fracture resistance.
[0095] Therefore, the holding temperature is 100° C. or higher and 260° C. or lower, and the holding time is 20 seconds or longer and 1500 seconds or shorter. In addition, the holding temperature is preferably 130° C. or higher and 240° C. or lower, and the holding time is preferably 50 seconds or longer and 1000 seconds or shorter.
[0096] In the present invention, "maintained" does not only mean maintaining at a constant temperature, but also includes a case where the temperature changes within the range of the maintained temperature of the present invention.
[0097] The hot-rolled steel sheet after hot rolling may be subjected to a heat treatment for softening the structure. The surface of the steel sheet may be plated with Zn, Al, etc. After annealing and cooling or after plating, the steel sheet may be subjected to temper rolling for shape adjustment. EXAMPLES
[0098] The present invention will be specifically described with reference to examples, but the present invention is not limited to these.
[0099] [Example 1] Steel plates having the tensile strengths shown in Table 1 were sheared into small pieces of 30 mm x 110 mm. For the tensile test, JIS No. 5 test pieces with a gauge length of 50 mm, gauge width of 25 mm, and plate thickness of 1.4 mm were taken from the rolling direction of the steel plate, and the tensile test was performed at a tension speed of 10 mm / min in accordance with JIS Z 2241. The measured tensile strength (TS) and yield strength (YS) are shown in Table 1. For some of the steel plates after shearing, the end surfaces generated by cutting were subjected to end surface treatment under the conditions shown in Table 1. Next, a sample of the steel plate was placed on a die having an angle of 90°, and the steel plate was pressed with a punch having an angle of 90° to perform V-shaped bending. Next, as shown in the side view of FIG. 2, the steel plate (member) after bending was fastened with bolts 20 from both sides of the plate surface of the steel plate 11 using bolts 20, nuts 21, and tapered washers 22. The relationship between the load stress and the tightening amount was calculated by CAE (Computer Aided Engineering) analysis, and the tightening amount was made to match the critical load stress. The critical load stress was measured by the method described later. Next, for some of the steel plates (members) after bending, the end surfaces of the steel plate were subjected to end surface treatment under the conditions shown in Table 1. The end surface treatment conditions are shown in Table 1. In the end surface treatment in Table 1, the column for heat treatment temperature (°C) marked with "-" means that no heat treatment was performed.
[0100] 2. Evaluation Method The delayed fracture resistance of the components obtained under various manufacturing conditions was evaluated by the critical load stress measured by a delayed fracture test. In addition, the residual stress and Vickers hardness of the end faces of the components were measured as follows. The methods of each evaluation are as follows.
[0101] (Measurement of critical load stress) The critical load stress was measured by a delayed fracture test. Specifically, the components obtained under each manufacturing condition were immersed in hydrochloric acid with a pH of 1 (25°C), and the maximum load stress at which delayed fracture did not occur was evaluated as the critical load stress. Delayed fracture was judged by visual inspection and images magnified up to 20 times with a stereomicroscope, and if no cracks occurred after 96 hours of immersion, it was considered that there was no fracture. The term "crack" here refers to the occurrence of cracks with a length of 200 μm or more.
[0102] (Measurement of residual stress on end face) For the components obtained under each manufacturing condition, the residual stress at the end face was measured by X-ray diffraction. The measurement point for the residual stress was the center of the plate thickness at the end face of the bent ridgeline, and the X-ray irradiation diameter was 150 μm. The measurement direction was perpendicular to the plate thickness direction and perpendicular to the bent ridgeline direction. Figure 3 is an enlarged view of the end face of the bent ridgeline, and the plate thickness center C1 and the measurement direction D2 are each indicated with a symbol.
[0103] (Measurement of Vickers hardness on the end surface) The Vickers hardness (HV) of the end face of the members obtained under each manufacturing condition was measured by a Vickers hardness test. The Vickers hardness was measured at a location 100 μm from the end face at the center of the plate thickness of the cross section cut in the bend ridge direction D1 and mirror-polished. The measurement load was 1 kgf.
[0104] 3. Evaluation results The evaluation results are shown in Table 1.
[0105] [Table 1]
[0106] Members with TS≧1470MPa and critical load stress≧1.10×YS were deemed to have passed the test, and are shown in Table 1 as examples of the invention. Members with TS<1470MPa or critical load stress<1.10×YS were deemed to have failed the test, and are shown in Table 1 as comparative examples. In Table 1, "critical load stress / YS" of 1.10 or more means that critical load stress≧1.10×YS. As shown in Table 1, the members of the examples of the invention have high strength and excellent delayed fracture resistance.
[0107] [Example 2] 1. Manufacturing of evaluation components Steel having the composition shown in Table 2, the balance being Fe and unavoidable impurities, was melted in a vacuum melting furnace, and then bloomed to obtain a blooming rolled material having a thickness of 27 mm. The obtained blooming rolled material was hot rolled to a thickness of 4.2 mm to produce a hot rolled steel sheet. Next, the hot rolled steel sheet was ground to a thickness of 3.2 mm, and then cold rolled to a thickness of 2.4 to 1.12 mm to produce a cold rolled steel sheet. Next, the cold rolled steel sheet obtained above was subjected to a heat treatment under the conditions shown in Tables 3 and 4 (annealing process). Note that the blank column of the composition in Table 2 indicates that the component was not intentionally added, and includes not only the case where the component is not contained (0 mass%), but also the case where the component is inevitably contained. Note that the details of the conditions of the hot rolling process, the cold rolling process, and the annealing process are shown in Tables 3 and 4.
[0108] The heat-treated steel plate was sheared into small pieces of 30 mm x 110 mm, and a sample of the steel plate was placed on a die with an angle of 90°, and the steel plate was pressed with a punch with an angle of 90° to perform a V-shaped bending process. Next, as shown in the side view of FIG. 2, the steel plate (member) after bending was tightened from both sides of the plate surface of the steel plate 11 with bolts 20, nuts 21, and tapered washers 22. The relationship between the load stress and the tightening amount was calculated by CAE (Computer Aided Engineering) analysis, and the tightening amount was set to coincide with the critical load stress. The critical load stress was measured by the method described below.
[0109] For Nos. 1 to 72 in Tables 3 and 4, the end faces of the bent ridges were heated at various temperatures after bending. For No. 73 in Table 4, the steel plate was sheared into small pieces, and then the end faces resulting from the cutting were heated before the bending process. The end face treatment conditions are shown in Tables 3 and 4. For end face treatment in Tables 3 and 4, "-" in the heat treatment temperature (°C) column means that no heat treatment was performed.
[0110] [Table 2]
[0111] [Table 3]
[0112] [Table 4]
[0113] 2. Evaluation Method The microstructure fraction of the components obtained under various manufacturing conditions was investigated by analyzing the steel structure (microstructure). Tensile tests were also conducted to evaluate tensile properties such as tensile strength, and delayed fracture resistance was evaluated using the critical load stress measured in a delayed fracture test. Residual stress and Vickers hardness of the end faces of the components were also measured as follows. The methods for each evaluation are as follows.
[0114] (Total area ratio of one or both of bainite containing carbides with an average grain size of 50 nm or less and martensite containing carbides with an average grain size of 50 nm or less) A test piece was taken from the steel sheet obtained in the annealing process (hereinafter referred to as annealed steel sheet) in a direction perpendicular to the sheet thickness L cross section parallel to the rolling direction, mirror-polished, and the structure was revealed with a nital solution. The test piece was then observed using a scanning electron microscope. A 16 mm x 15 mm grid with 4.8 μm intervals was placed on an area of 82 μm x 57 μm in actual length on an SEM image at a magnification of 1500 times, and the area ratios of martensite containing carbides with an average grain size of 50 nm or less and bainite containing carbides with an average grain size of 50 nm or less were calculated by a point counting method in which the number of points on each phase was counted, and the total area ratio was calculated. The area ratio was the average value of three area ratios obtained from separate SEM images at a magnification of 1500 times. Martensite exhibits a white structure, and bainite has fine carbides precipitated inside a black structure. The average grain size of the carbides was calculated as follows. The area ratio was the area ratio relative to the entire observation range, and this was regarded as the area ratio relative to the entire steel sheet structure.
[0115] (Average grain size of carbides in bainite and martensite) Test pieces were taken from the annealed steel sheet in a direction perpendicular to the rolling direction, and the cross section of the thickness L parallel to the rolling direction was mirror-polished and the structure was revealed with nital solution. The specimens were then observed using a scanning electron microscope, and the total area of carbides on the SEM image at a magnification of 5000 times was measured by binarized image analysis, and the average area per carbide was calculated by averaging the total area by number. The circle equivalent diameter calculated from the average area per carbide was taken as the average grain size.
[0116] (Tensile test) JIS No. 5 test pieces with a gauge length of 50 mm, a gauge width of 25 mm, and a plate thickness of 1.4 mm were taken from the rolling direction of the annealed steel sheet, and tensile tests were conducted in accordance with JIS Z 2241 at a tensile speed of 10 mm / min to measure the tensile strength (TS) and yield strength (YS).
[0117] (Measurement of critical load stress) The critical load stress was measured by a delayed fracture test. Specifically, the components obtained under each manufacturing condition were immersed in hydrochloric acid with a pH of 1 (25°C), and the maximum load stress at which delayed fracture did not occur was evaluated as the critical load stress. Delayed fracture was judged by visual inspection and images magnified up to 20 times with a stereomicroscope, and if no cracks occurred after 96 hours of immersion, it was considered that there was no fracture. The term "crack" here refers to the occurrence of cracks with a length of 200 μm or more.
[0118] (Measurement of residual stress on end face) For the components obtained under each manufacturing condition, the residual stress at the end face was measured by X-ray diffraction. The measurement point for the residual stress was the center of the plate thickness at the end face of the bent ridgeline, and the X-ray irradiation diameter was 150 μm. The measurement direction was perpendicular to the plate thickness direction and perpendicular to the bent ridgeline direction. Figure 3 is an enlarged view of the end face of the bent ridgeline, and the plate thickness center C1 and the measurement direction D2 are each indicated with a symbol.
[0119] (Measurement of Vickers hardness on the end surface) The Vickers hardness (HV) of the end face of the members obtained under each manufacturing condition was measured by a Vickers hardness test. The Vickers hardness was measured at a location 100 μm from the end face at the center of the plate thickness of the cross section cut in the bend ridge direction D1 and mirror-polished. The measurement load was 1 kgf.
[0120] 3. Evaluation results The evaluation results are shown in Tables 5 and 6.
[0121] [Table 5]
[0122] [Table 6]
[0123] In this example, members with TS≧1470MPa and critical load stress≧1.10×YS were deemed to pass, and are shown as invention examples in Tables 5 and 6. Members with TS<1470MPa or critical load stress<1.10×YS were deemed to fail, and are shown as comparative examples in Tables 5 and 6. In Tables 5 and 6, "critical load stress / YS" of 1.10 or more means that critical load stress≧1.10×YS. As shown in Tables 5 and 6, the members of the invention examples have high strength and excellent delayed fracture resistance.
[0124] [Example 3] In Example 3, a member was manufactured using a steel type that did not contain Sb and was evaluated. 1. Manufacturing of evaluation components Steel having the composition shown in Table 7 and the balance consisting of Fe and unavoidable impurities was melted in a vacuum melting furnace, and then bloomed to obtain a blooming rolled material with a thickness of 27 mm. The obtained blooming rolled material was hot rolled to a thickness of 4.2 mm to produce a hot rolled steel sheet. Next, the hot rolled steel sheet was ground to a thickness of 3.2 mm, and then cold rolled to a thickness of 2.4 to 1.12 mm to produce a cold rolled steel sheet. Next, the cold rolled steel sheet obtained above was subjected to a heat treatment under the conditions shown in Table 8 (annealing process). Note that the blank column of the composition in Table 7 indicates that the component was not intentionally added, and includes not only the case where the component is not contained (0 mass%) but also the case where the component is inevitably contained. Note that the details of the conditions of the hot rolling process, the cold rolling process, and the annealing process are shown in Table 8.
[0125] The heat-treated steel plate was sheared into small pieces of 30 mm x 110 mm, and a sample of the steel plate was placed on a die with an angle of 90°, and the steel plate was pressed with a punch with an angle of 90° to perform a V-shaped bending process. Next, as shown in the side view of FIG. 2, the steel plate (member) after bending was tightened with bolts 20 from both sides of the plate surface of the steel plate 11 using bolts 20, nuts 21, and tapered washers 22. The relationship between the load stress and the tightening amount was calculated by CAE (Computer Aided Engineering) analysis, and the tightening amount was made to coincide with the critical load stress. The critical load stress was measured by the method described in Example 2.
[0126] After bending, the end faces of the bent ridges were heated at various temperatures. The end face treatment conditions are shown in Table 8.
[0127] [Table 7]
[0128] [Table 8]
[0129] 2. Evaluation Method The members obtained under the various manufacturing conditions were measured and evaluated in the same manner as in Example 2.
[0130] 3. Evaluation results The evaluation results are shown in Table 9.
[0131] [Table 9]
[0132] In this example, members with TS≧1470MPa and critical load stress≧1.10×YS were deemed to pass, and are shown as invention examples in Table 9. Members with TS<1470MPa or critical load stress<1.10×YS were deemed to fail, and are shown as comparative examples in Table 9. In Table 9, "critical load stress / YS" of 1.10 or more means that critical load stress≧1.10×YS. As shown in Table 9, the members of the invention examples have high strength and excellent delayed fracture resistance. [Explanation of symbols]
[0133] 10 High-strength components 11 Steel plate 12 Bend ridge 13 End face of bent ridge 20 Volts 21 Nut 22 Tapered washer C1 center of plate thickness D1 Bending ridge direction D2 Measuring direction
Claims
1. A high-strength member having a bent ridge portion obtained by using a steel plate, The steel plate comprises, in mass%, C: 0.17% or more and 0.35% or less, Si: 0.001% or more and 1.2% or less, Mn: 0.9% or more and 3.2% or less, P: 0.020% or less, Al: 0.010% or more and 0.20% or less, and N: 0.010% or less; The remainder of the composition is iron and unavoidable impurities. The steel plate has a microstructure in which the area ratio of one or both of bainite containing carbides having an average grain size of 50 nm or less and martensite containing carbides having an average grain size of 50 nm or less is 90% or more in total, The tensile strength of the member is 1470 MPa or more, The residual stress at the end surface of the bent ridge line is 300 MPa or less, and The Vickers hardness (HV) of the end surface of the bend ridgeline is 200 or more and 450 or less, A high-strength component for automobile structural components, in which the critical load stress of the component is 1.10 times or more the yield strength when immersed in hydrochloric acid of pH = 1 (25°C) and the maximum load stress at which delayed fracture does not occur is measured as the critical load stress.
2. A high-strength member having a bent ridge portion obtained by using a steel plate, The steel plate comprises, in mass%, C: 0.17% or more and 0.35% or less, Si: 0.001% or more and 1.2% or less, Mn: 0.9% or more and 3.2% or less, P: 0.020% or less, Al: 0.010% or more and 0.20% or less, N: 0.010% or less, and Sb: 0.001% or more and 0.10% or less; The remainder of the composition is iron and unavoidable impurities. The steel plate has a microstructure in which the area ratio of one or both of bainite containing carbides having an average grain size of 50 nm or less and martensite containing carbides having an average grain size of 50 nm or less is 90% or more in total, The tensile strength of the member is 1470 MPa or more, The residual stress at the end surface of the bent ridge line is 300 MPa or less, and The Vickers hardness (HV) of the end surface of the bend ridgeline is 200 or more and 450 or less, A high-strength component for automobile structural components, in which the critical load stress of the component is 1.10 times or more the yield strength when immersed in hydrochloric acid of pH = 1 (25°C) and the maximum load stress at which delayed fracture does not occur is measured as the critical load stress.
3. The composition of the steel sheet further comprises, in mass%, 3. The high-strength member for automobile structural members according to claim 1 or 2, containing 0.0002% or more and less than 0.0035% B.
4. The composition of the steel sheet further comprises, in mass%, Nb: 0.002% or more and 0.08% or less; The high-strength member for automobile structural members according to any one of claims 1 to 3, comprising at least one selected from Ti: 0.002% or more and 0.12% or less.
5. The composition of the steel sheet further comprises, in mass%, Cu: 0.005% or more and 1% or less; The high-strength member for automobile structural members according to any one of claims 1 to 4, comprising at least one selected from Ni: 0.005% or more and 1% or less.
6. The composition of the steel sheet further comprises, in mass%, Cr: 0.01% or more and 1.0% or less, Mo: 0.01% or more and less than 0.3% V: 0.003% or more and 0.5% or less, Zr: 0.005% or more and 0.20% or less, and The high-strength member for automobile structural members according to any one of claims 1 to 5, comprising at least one selected from W: 0.005% or more and 0.20% or less.
7. The composition of the steel sheet further comprises, in mass%, Ca: 0.0002% or more and 0.0030% or less, Ce: 0.0002% or more and 0.0030% or less, La: 0.0002% or more and 0.0030% or less, and The high-strength member for automobile structural members according to any one of claims 1 to 6, comprising at least one selected from Mg: 0.0002% or more and 0.0030% or less.
8. The composition of the steel sheet further comprises, in mass%, The high-strength member for automobile structural members according to any one of claims 1 to 7, containing Sn: 0.002% or more and 0.1% or less.
9. A method for producing a high-strength component for an automobile structural member having a bent ridge line obtained by using a steel plate, comprising the steps of: A bending process step of cutting out the steel plate according to any one of claims 1 to 8 and bending the steel plate; and an end surface treatment step of heating the end surface generated by the cutting at a temperature of 400° C. or more and 900° C. or less for a period of more than 0 seconds and not more than 10 seconds after the bending process. The tensile strength of the member is 1470 MPa or more, The residual stress at the end surface of the bent ridge line is 300 MPa or less, and The Vickers hardness (HV) of the end surface of the bend ridgeline is 200 or more and 450 or less, A method for manufacturing a high-strength component for an automobile structural member, in which the critical load stress of the component is 1.10 times or more the yield strength when the component is immersed in hydrochloric acid of pH = 1 (25°C) and the maximum load stress at which delayed fracture does not occur is measured as the critical load stress.
10. A method for producing a high-strength component for an automobile structural member having a bent ridge line obtained by using a steel plate, comprising the steps of: After cutting out the steel plate according to any one of claims 1 to 8, an end surface treatment step of heating the end surface generated by cutting at a temperature of 400 ° C. or more and 900 ° C. or less under conditions of more than 0 seconds and not more than 10 seconds; A bending process is performed on the steel plate after the end surface treatment process. The tensile strength of the member is 1470 MPa or more, The residual stress at the end surface of the bent ridge line is 300 MPa or less, and The Vickers hardness (HV) of the end surface of the bend ridgeline is 200 or more and 450 or less, A method for manufacturing a high-strength component for an automobile structural member, in which the critical load stress of the component is 1.10 times or more the yield strength when the component is immersed in hydrochloric acid of pH = 1 (25°C) and the maximum load stress at which delayed fracture does not occur is measured as the critical load stress.
11. A method for producing a steel plate according to any one of claims 1 to 8, which is used for a high-strength member obtained by the method for producing a high-strength member for an automobile structural member according to claim 9 or 10, a hot rolling process for hot rolling a steel material; a cold rolling step of cold rolling the hot-rolled steel sheet obtained by the hot rolling; The cold-rolled steel sheet obtained by the cold rolling is C3 and then, an annealing step of heating the steel sheet to an annealing temperature of at least 550°C, cooling the steel sheet at an average cooling rate of at least 3°C / sec in a temperature range from the annealing temperature to 550°C and to a cooling stop temperature of at most 350°C, and then holding the steel sheet in a temperature range of at least 100°C and at most 260°C for at least 20 seconds and at most 1,500 seconds.
Citation Information
Patent Citations
High-strength thin steel sheet superior in delayed fracture resistance after being formed, manufacturing method therefor, and high strength component for automobile made of the high-strength thin steel sheet
JP2003166035A
Manufacturing method of molding member
JP2017125228A