Pipe with inner surface groove for flaring and heat exchange comprising the same

The internally grooved tube with specific dimensions and groove configurations addresses the issue of cracking during flaring in copper tubes, enhancing reliability and performance in heat exchangers by minimizing expansion-related failures.

JP2024164843AInactive Publication Date: 2024-11-27KMCT CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024150712
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-27
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional flaring processes for copper tubes in heat exchangers often result in cracking, particularly for tubes with small diameters, due to the required expansion rate being lower for smaller diameters, leading to potential breakage during flaring.

Method used

An internally grooved tube with specific dimensions and groove configurations, including an outer diameter of 2.0 to 5.5 mm, a wall thickness ratio of 0.057-0.075, a torsion angle of 15 to 27 degrees, and groove parameters satisfying formulas (1) and (2), is used to minimize cracking during flaring.

Benefits of technology

The grooved tube design significantly reduces the likelihood of cracking during flaring, ensuring reliable expansion and maintaining heat transfer performance while meeting lightweight and cost-effective requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164843000001_ABST
    Figure 2024164843000001_ABST
Patent Text Reader

Abstract

To provide a pipe with an inner surface groove for flaring in which cracks are less likely to occur due to pipe expansion through flaring.SOLUTION: A pipe with an inner surface groove for flaring is a seamless pipe with a groove on an inner surface and a flared end part, where an outer diameter D is 2.0 mm or more and 5.5 mm or less, a ratio T / D of a wall thickness T and the outer diameter D is 0.057-0.005D or more and 0.075-0.005D or less, a torsion angle θ of the groove on the inner surface is 15 degrees or more and 27 degrees or less, a radius of curvature r of a tip part of a fin constituting the groove on the inner surface and the number N of the fins in a circumferential direction satisfy a specific formula, and the radius of curvature r of the tip part and the torsion angle θ satisfy a specific formula.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an inner grooved tube for flaring processing and a heat exchanger equipped with the same. [Background technology]

[0002] Conventionally, heat exchangers in room air conditioners (RAC), packaged air conditioners (PAC), refrigerators, hot water heaters, etc., as well as electronic devices such as PCs, smartphones, and game consoles, have contained copper pipes that exchange heat by circulating a heat medium inside.

[0003] For example, in the process of assembling a room air conditioner, first, a number of straight copper tubes are prepared, and each is bent in the longitudinal center to form a U-shaped hairpin tube. Then, each copper tube is inserted into a through hole of an aluminum fin made of a number of laminated aluminum plates, and the straight tube portion of the copper tube is expanded to bring the outer surface of the straight tube portion into close contact with the inner peripheral surface of the through hole of the aluminum fin. Then, the adjacent tube ends protruding from the aluminum fin of each copper tube are connected to each other with a U-shaped bend tube or branch tube. Then, the connected copper tubes become one or more flow paths through which the heat medium flows. Then, the heat of the heat medium in the copper tube is transferred to the aluminum fin, and the temperature of the air or the like in the room is regulated by flowing the air or the like through the gaps between the aluminum plates of the aluminum fin.

[0004] Here, the expansion of the straight pipes of the copper pipes to make them tightly contact the inner circumferential surfaces of the through holes of the aluminum fins is called primary expansion, and the expansion of the pipe ends of each copper pipe to insert the U-shaped bend pipes is called secondary expansion, and the secondarily expanded parts are also called secondary expansion parts. The end of the secondary expansion section is then expanded. This expansion is called tertiary expansion or flaring. The tertiary expansion or flaring section is called the flared section. The bend pipe is inserted into the secondary expansion section through the flared section, and a ring-shaped brazing filler metal is inserted into the gap between the outer surface of the bend pipe and the inner surface of the flared section, after which the brazing filler metal is heated to melt and solidify, thereby joining the bend pipe and the end of the copper pipe. The flared section is formed to ensure a gap for inserting the brazing filler metal.

[0005] Conventionally, this type of flaring could cause cracks at the very end of the copper tube. In particular, when the copper tube has a small outer diameter, for example 6 mm or less, the flaring process could cause the tube to crack. This was thought to be mainly due to the fact that even if the copper tube has a small outer diameter, a certain size is required for the gap in which the brazing material is inserted, so the expansion rate of a copper tube with a small outer diameter is relatively large compared to a copper tube with a large outer diameter.

[0006] In response to this, Patent Document 1 proposes a copper or copper alloy tube for flaring, which is used to flare the end of a seamless tube, characterized in that the outer diameter D is 2.0 to 5.5 mm, the ratio T / D of the wall thickness T to the outer diameter D is (0.057-0.005D) or more (0.075-0.005D) or less, the average crystal grain size is 30 μm or less, and the circumferential elongation is 35% or more. Patent Document 1 also describes that such a copper or copper alloy tube for flaring has an appropriate wall thickness, average crystal grain size, and elongation of the seamless copper tube, and therefore when a small-diameter copper tube with an outer diameter of 2.0 to 5.5 mm is used for flaring, it is possible to prevent cracks from occurring in the expanded tube part of the flared part. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2017-20063 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention provides an inner grooved tube for flaring that is less likely to crack when expanded by flaring, and a heat exchanger including the same. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. The present invention includes the following (I) to (IV). (I) An inner grooved pipe for flaring, which is a seamless pipe having a groove on the inner surface and having an end flared, The outer diameter D is 2.0 mm or more and 5.5 mm or less, The ratio T / D of the wall thickness T to the outside diameter D is 0.057-0.005D or more and 0.075-0.005D or less, The twist angle θ of the groove on the inner surface is 15 degrees or more and 27 degrees or less, The radius of curvature r of the tip of the fin constituting the groove on the inner surface and the number N of the fins in the circumferential direction satisfy the following formula (1), The tip curvature radius r and the twist angle θ satisfy the following formula (2). Formula (1): 0.32≦1 / (r×N)≦0.61 Formula (2): 0.04≦r×(1 / cosθ)≦0.051 (II) The inner grooved pipe for flaring according to the above (I), wherein the tip curvature radius r and the number N of the fins satisfy the following formula (1'). Formula (1´): 0.52≦1 / (r×N)≦0.61 (III) An internally grooved pipe for flaring according to (I) or (II) above, which is made of copper or a copper alloy. (IV) A heat exchanger comprising an inner grooved tube for flaring according to any one of (I) to (III) above. Effect of the Invention

[0010] According to the present invention, it is possible to provide an inner grooved tube for flaring that is less likely to crack due to tube expansion during flaring, and a heat exchanger including the same. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1(a) is a schematic diagram showing the side of a straight grooved tube of the present invention, FIG. 1(b) is a cross-section taken along line AA in FIG. 1(a), and FIG. 1(c) is an enlarged view of one of the eight points (part X) surrounded by dotted lines in FIG. 1(b). [Diagram 2] Figure 2(a) is a schematic side view of a test piece 10 cut out from a portion (a portion of length L in the longitudinal direction) of the grooved tube of the present invention, and Figures 2(b) and 2(c) are schematic side and end views showing the test piece 10 placed on the surface of a metal substrate 20 with a load P applied from above. [Diagram 3] FIG. 3(a) is a schematic side view showing that test piece 10 has been completely crushed by the application of load P, resulting in two plates overlapping each other, FIG. 3(b) is a schematic side view showing the two plates separated, and FIG. 3(c) is a schematic view (schematic front view) of the lower plate (10a) from above after the upper plate (10b) has been removed. [Figure 4] Like FIG. 1(c), this is an enlarged view of one of the eight points (part X) surrounded by dotted lines in FIG. 1(b), and is a schematic view for explaining the fin height, apex angle, and radius of curvature R of the fin base. [Diagram 5] Similar to FIG. 1(c), this is an enlarged view of one of the eight points (part X) surrounded by dotted lines in FIG. 1(b), and is a diagram (schematic diagram) for explaining the radius of curvature R of the fin base portion. [Figure 6] FIG. 2 is a diagram showing an example of a manufacturing apparatus used to manufacture the grooved pipe of the present invention. [Figure 7] FIG. 6 is a partially cutaway front view illustrating a heat exchanger 60 of the present invention, which is a fin-and-tube heat exchanger incorporating the grooved tubes of the present invention. [Figure 8] FIG. 8 is a partially enlarged view (schematic perspective view) of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will now be described. The present invention relates to an internally grooved pipe for flaring, which is a seamless pipe having a groove on its inner surface and having an end flared, wherein the outer diameter D is 2.0 mm or more and 5.5 mm or less, the ratio T / D of the wall thickness T to the outer diameter D is 0.057-0.005D or more and 0.075-0.005D or less, the twist angle θ of the inner surface groove is 15 degrees or more and 27 degrees or less, the tip radius of curvature r of the fins that constitute the inner surface groove and the number N of the fins in the circumferential direction satisfy the following formula (1), and the tip radius of curvature r and the twist angle θ satisfy the following formula (2). Formula (1): 0.32≦1 / (r×N)≦0.61 Formula (2): 0.04≦r×(1 / cosθ)≦0.051 Such an internally grooved pipe for flaring will hereinafter be referred to as the "grooved pipe of the present invention."

[0013] The present invention also relates to a heat exchanger comprising the grooved tube of the present invention. Such a heat exchanger is hereinafter also referred to as "the heat exchanger of the present invention."

[0014] <Grooved pipe of the present invention> The grooved pipe of the present invention will now be described. The grooved pipe of the present invention is an internally grooved pipe for flaring, which is a seamless pipe having a groove on its inner surface and having an end portion flared. The grooved tube of the present invention may be one that has not been flared or one that has been flared. The grooved tube of the present invention provided in the heat exchanger of the present invention is usually one that has been flared.

[0015] The shape of the grooved tube of the present invention is not particularly limited, and may be a straight tube, a straight tube wound into a coil, or a straight tube bent into a U-shape (hairpin tube). The cross-sectional shape is not particularly limited, and the cross section perpendicular to the longitudinal direction of the tube may be elliptical, triangular, rectangular, or any other polygonal shape, but is preferably circular.

[0016] The material of the grooved tube of the present invention is not particularly limited, but it is preferably made of copper or a copper alloy. Examples of copper or copper alloys include C1220 (phosphorus deoxidized copper), C1201 (low phosphorus deoxidized copper), C1020 (oxygen-free copper), C5010, C1862, and C1565 (high strength copper), as specified in JIS H 3300.

[0017] The grooved pipe of the present invention has grooves on the inner surface. The grooves on the inner surface of the grooved pipe of the present invention will be described with reference to FIG. Fig. 1(a) is a schematic diagram showing the side of the grooved tube of the present invention when it is straight and has a circular cross section, in which the central axis of the grooved tube of the present invention is indicated as ω. Fig. 1(b) is a cross section taken along line AA in Fig. 1(a), which is a diagram (schematic cross section) showing a cross section in a direction perpendicular to the longitudinal direction of the tube (a direction parallel to the central axis ω). Here, the eight points enclosed by dotted rectangles in Fig. 1(b) indicate the points at which the outer diameter D, wall thickness T, and fin tip curvature radius r are measured using the method described below, and these points are arranged at approximately equal intervals (approximately 45° intervals) in the circumferential direction in the cross section shown in Fig. 1(b). As described below, these values ​​for the grooved tube of the present invention refer to the simple average values ​​of the measurement results at these eight points. FIG. 1(c) is an enlarged view of one of the eight points (part X) surrounded by dotted lines in FIG. 1(b).

[0018] [Outer diameter D] In the grooved pipe of the present invention, the outer diameter D is 2.0 mm or more and 5.5 mm or less, and preferably 3.5 mm or more and 5.0 mm or less. The outer diameter D is measured at eight points surrounded by dotted lines in Fig. 1(b). In other words, in Fig. 1(b), these eight points consist of four pairs of symmetrical points that face each other with respect to the point indicating the central axis ω, and after obtaining four outer diameter measurements at these eight points (four pairs) that are approximately evenly spaced in the circumferential direction, the simple average of these four measurements is set as the outer diameter D of the grooved pipe of the present invention. The outer diameter is measured using a digital caliper.

[0019] Conventionally, copper tubes with an outer diameter of 7 to 9.52 mm were mainly used for flaring. However, in recent years, there has been a demand for smaller diameters in order to reduce the weight and improve the performance of heat transfer tubes. Also, in order to reduce the global warming potential, the heat transfer medium (refrigerant, etc.) that flows through the tubes is being switched to R32, but because R32 is slightly flammable, there is a demand to reduce the amount of R32 used, and in order to achieve this, there is a demand for smaller diameters. Since the outer diameter D of the grooved pipe of the present invention is in the above-mentioned range, it satisfies the recent demand for smaller diameters.

[0020] [Thickness T] In the grooved pipe of the present invention, the ratio (T / D) of the outer diameter D to the wall thickness T is 0.057-0.005D or more and 0.075-0.005D or less, and preferably 0.059-0.005D or more and 0.071-0.005D or less.

[0021] The thickness T is preferably 0.09 to 0.27 mm, more preferably 0.13 to 0.25 mm, even more preferably 0.17 to 0.23 mm, and further preferably 0.18 to 0.21 mm. In light of the recent rise in copper prices, there is a demand for lightweight internally grooved tubes used in heat exchangers, etc., while still satisfying pressure resistance. The grooved tube of the present invention has the above-mentioned outer diameter D and wall thickness T, and meets this demand.

[0022] The method for measuring the wall thickness T will be described. First, the eight points enclosed by dotted lines in Fig. 1(b) are magnified 10 times using a laser microscope (e.g., Keyence VK-8500) to obtain images or photographs as shown in Fig. 1(c). Next, at each of the eight points shown in Fig. 1(c), the thinnest wall thickness in the radial direction centered on the central axis ω is measured. The value obtained by simply averaging the measurements at the eight points is defined as the wall thickness T of the grooved pipe of the present invention.

[0023] [Tip radius of curvature r] The radius of curvature r of the tip of the fin constituting the groove on the inner surface of the grooved tube of the present invention is preferably 0.030 to 0.045 mm, and taking into consideration heat transfer performance, it is preferably 0.030 to 0.040 mm. Furthermore, when considering productivity, it is more preferably 0.036 to 0.040 mm.

[0024] The method for measuring the radius of curvature r of the tip of the fin will be explained with reference to FIG. 1(b) and FIG. 1(c). First, the eight points enclosed by dotted lines in FIG. 1(b) are magnified 10 times using a laser microscope (for example, VK-8500 manufactured by Keyence Corporation) to obtain an image or photograph as shown in FIG. 1(c). Next, in an image or photograph as shown in Figure 1(c), a curve Y is drawn that is tangent to the tops of the three fins, the fin 1 to be measured and the two adjacent fins 1a and 1b. This curve Y usually overlaps almost exactly with the circumference of a circle centered at ω shown in Figure 1(b). Next, the groove bottom 3a between the fin 1 to be measured and the fin 1a adjacent to it is identified, and similarly, the groove bottom 3b between the fin 1 to be measured and the fin 1b adjacent to it is identified, and then a straight line W that is a tangent to both of these is drawn. 1(c), a line that connects the contour of fin 1 with a point on line W and is perpendicular to line W, and the point on the contour of fin 1 where the line is at its longest is defined as vertex V. Typically, vertex V approximately coincides with the point of contact between the contour of fin 1 and curve Y. Then, a line perpendicular to line W is drawn from vertex V of fin 1. Next, identify the point that bisects the perpendicular line drawn from vertex V to line W, and draw a line that passes through this point and is parallel to line W. Let 5a and 5b be the points where this line intersects with the contour of fin 1. Then, let Za be the tangent line that passes through point 5a and touches the contour of fin 1, and similarly, let Zb be the tangent line that passes through point 5b and touches the contour of fin 1. Next, a circle that passes through the vertex V and is tangent to the tangent lines Za and Zb is drawn on the outer periphery of the vertex V. The radius of the circle thus drawn is taken as the radius of curvature r of the tip of the fin.

[0025] [Number of fins N] The number of fins N constituting the grooves on the inner surface of the grooved pipe of the present invention is preferably 36-69, and more preferably 37-52.

[0026] The number N of fins constituting the grooves on the inner surface of the grooved pipe of the present invention is measured in a cross section as shown in Fig. 1(b). That is, the number N of fins present in the circumferential direction is measured visually in a cross section perpendicular to the longitudinal direction of the pipe (parallel to the central axis ω).

[0027] [Twist angle θ] The twist angle θ of the grooves on the inner surface of the grooved pipe of the present invention is 15 degrees or more and 27 degrees or less, and preferably 20 degrees or more and 27 degrees or less. If the twist angle θ is too large, the pressure loss of the heat transfer medium (refrigerant, etc.) flowing inside the tube increases, which may lead to an increase in the power required for the compressor in an air conditioner unit, etc. In that case, the coefficient of performance (COP) of the equipment decreases. Also, there is a risk of fin collapse during the primary expansion. If the twist angle θ is too small, cracks are likely to occur due to the expansion caused by flaring. Also, the heat transfer coefficient inside the tube decreases, which may result in a decrease in heat exchange performance.

[0028] The method for measuring the twist angle θ will be described with reference to FIGS. Fig. 2(a) is a schematic side view showing a test piece 10 obtained by cutting out a portion (a portion having a length L in the longitudinal direction) from the grooved pipe of the present invention. Fig. 2(b) and Fig. 2(c) are a schematic side view and a schematic end view showing the state in which the test piece 10 is placed on the surface of a metal substrate 20 and a load P is applied from above. Fig. 3(a) is a schematic side view showing the test piece 10 completely crushed by the application of load P, resulting in two overlapping plates, Fig. 3(b) is a schematic side view showing the two plates separated, and Fig. 3(c) shows a schematic view (schematic front view) of the lower plate (10a) from above after the upper plate (10b) of the two plates has been removed.

[0029] 2(a), a part is cut out from the grooved pipe of the present invention to obtain a test piece 10. Specifically, a part is cut out so that the length L in the longitudinal direction is 15 to 30 mm. 2(b) and 2(c), the test piece 10 is placed on the surface of the metal substrate 20, and a load P is applied from above to the test piece 10. Here, the load P is set to about 0.14 to 0.20 kN. Here, the metal substrate 20 may be any material having a hardness sufficient to prevent the test piece 10 from being dented when a load P is applied thereto, and may be, for example, a plate made of stainless steel.

[0030] When the load P is applied to the test piece 10 as described above, the test piece 10 is completely crushed, and the two plates (10a, 10b) are stacked as shown in Fig. 3(a). Then, the two plates are separated as shown in Fig. 3(b). In the state shown in Fig. 3(a), the two plates (10a and 10b) may be connected at both ends (both ends in a direction parallel to the main surface of the substrate 20 in Fig. 3(a)). In such a case, the two plates can be separated by polishing the connected portion with abrasive paper or the like. Then, grooves appear that have been formed (transferred) by pressing the fins of the upper plate 10b onto the fins 15 of the lower plate 10a. If the grooves are connected by a straight line, the straight line (shown by a dotted line in FIG. 3(c)) indicates the position where the fins 16 of the upper plate 10b existed when the two plates (10a, 10b) were overlapped as shown in FIG. 3(a). The angle between the fins 15 and 16 is measured and defined as 2θ. The value obtained by dividing the angle by 2 is defined as the twist angle (θ).

[0031] [Formula 1] In the grooved pipe of the present invention, the radius of curvature r of the tip of the fin and the number N of the fins in the circumferential direction satisfy the following formula (1). Formula (1): 0.32≦1 / (r×N)≦0.61

[0032] It is preferable that these further satisfy the following formula (1'). Formula (1´): 0.52≦1 / (r×N)≦0.61

[0033] If formula (1) is satisfied, cracks are less likely to occur due to tube expansion through flaring. When formula (1´) is satisfied, this tendency becomes even more pronounced.

[0034] As shown in FIG. 1(b) and FIG. 1(c), in the cross section perpendicular to the longitudinal direction (parallel to the central axis ω) of the grooved pipe of the present invention, the grooves and the fins are alternately arranged in the circumferential direction. Here, the latter part is called (i) the groove bottom thick part + fin, and the former part is called (ii) the groove bottom thick part. When flaring is performed, the material elongation of the part (i) is smaller than that of the part (ii). In other words, the part (ii) is elongated more. Therefore, in order to suppress breakage in the part (ii), it is necessary to widen the width of the part (ii) (the groove bottom width shown in FIG. 4 described later). If the number of fins N is reduced or the radius of curvature r of the tip of the fin is reduced so as to satisfy the above formula (1), it is possible to widen the width of the part (ii), and cracks during flaring can be suppressed.

[0035] Furthermore, when the number of fins N is large or the radius of curvature r of the fin tips is large, if the ratio of the groove bottom width to the fin height (groove bottom width / fin height) is below a certain value, the grooved plug tends to be easily damaged during the manufacturing process. If the grooved plug is damaged, the formation of the fin at the damaged location will be incomplete, or the damaged location will become a resistance and the grooved pipe will break. In other words, the product cannot be manufactured. If the number of fins N and the radius of curvature r of the fin tips are determined so as to satisfy the above formula (1), the grooved plug will be less likely to be damaged during the manufacturing process.

[0036] Furthermore, if the radius of curvature r of the fin tips is too large or the number of fins N is too large, the unit mass of the internally grooved tube becomes heavy, leading to increased costs. Furthermore, if the radius of curvature r of the fin tips is too large, the surface area of ​​the internally grooved tube that contributes to the heat transfer effect decreases, leading to reduced heat transfer performance. If the number of fins N and the radius of curvature r of the fin tips are determined so as to satisfy the above formula (1), such problems are less likely to occur.

[0037] [Formula 2] In the grooved pipe of the present invention, the radius of curvature r of the tip portion of the fin and the twist angle θ as described above satisfy the following formula (2). Formula (2): 0.04≦r×(1 / cosθ)≦0.051

[0038] When the twist angle θ is small and the value of cosθ is large, the distance between any fin and its adjacent fin in the longitudinal direction of the tube is large. When flaring is performed, the aforementioned (ii) groove bottom thick part, which is the thinnest part, must withstand flaring cracks, and the tensile strength in the circumferential direction of the tube is the lowest in the (ii) groove bottom thick part. Therefore, the larger the distance between any fin and its adjacent fin in the longitudinal direction of the tube, the more likely it is that flaring cracks will occur in the (ii) groove bottom thick part. On the other hand, when the twist angle θ is large and cosθ is small, the distance between any fin and the adjacent fin in the longitudinal direction of the tube is small, so (ii) the thick groove bottom portion becomes narrow. In this case, when the tool for flaring is inserted, as it progresses, the tool reaches (i) the thick groove bottom portion + the fin before flare expansion cracks occur in (ii) the thick groove bottom portion. In other words, (ii) the thick groove bottom portion is supported by the fin before it breaks, and flaring cracks can be suppressed. Furthermore, if the value of r×(1 / cos θ) is too large, the heat transfer performance tends to decrease, and the productivity also tends to decrease. From this point of view, the grooved pipe of the present invention which satisfies the above formula (2) is less likely to crack when expanded by flaring.

[0039] The method for measuring the fin root curvature radius R will be described with reference to FIG. Fig. 5 is an enlarged schematic diagram of one of the eight areas (part X) surrounded by dotted lines in Fig. 1(b), similar to Fig. 1(c). Note that the same parts are denoted by the same reference numerals in Fig. 5 and Fig. 1(c). First, the point of contact between the straight line W described with reference to FIG. Next, the intersection point of the tangent line Za and the straight line W is designated as point O. Then, a circle is drawn with point O as its center and tangent to the contour of the fin 1, and the point of contact between the circle and the contour of the fin 1 is designated as point S. Next, a circle is drawn with point O as its center and passing through point Q, and the point of intersection between the circle and the tangent Za that is closer to fin 5a of fin 1 is designated as point P. Then, draw a circle passing through the three points P, Q, and S, and define the radius of that circle as the "fin root curvature radius R."

[0040] Such a grooved pipe of the present invention is less likely to crack when expanded by flaring.

[0041] <Manufacturing method> The method for producing the grooved pipe of the present invention is not particularly limited. The grooved pipe of the present invention can be produced, for example, by using a production apparatus shown in FIG. The manufacturing apparatus shown in FIG. 6 will be described. FIG. 6 is a schematic cross-sectional view of a manufacturing apparatus 30 capable of manufacturing the grooved pipe of the present invention. The manufacturing apparatus 30 has a retaining plug 32 to be inserted inside the mother tube 31. The retaining plug 32 has a truncated cone shape, and is inserted so that the end of the retaining plug 32 with a smaller diameter is located downstream in the direction in which the mother tube 31 is pulled out. In addition, a holding die 33 is provided at a position on the outer circumferential side of the holding plug 32, and the mother tube 31 is disposed so as to be sandwiched between the holding plug 32 and the holding die 33 from the inside and outside. The mother tube 31 is subjected to diameter reduction processing by being sandwiched between the holding plug 32 and the holding die 33. A grooved plug 35 is connected to the retaining plug 32 via a rod-shaped plug shaft 34. A groove having a shape to be formed on the inner circumferential surface of the mother tube 31 is formed on the outer circumferential surface of the grooved plug 35. The grooved plug 35 can freely rotate about the plug shaft 34. The grooved plug 35 has a number of rolling balls 36 located on the outer periphery thereof, and the mother tube 31 is sandwiched between the grooved plug 35 and the rolling balls 36 from the inside and outside. The rolling balls 36 are arranged so as to be able to revolve around the tube axis (the same as the central axis ω) of the mother tube 31 in the circumferential direction of the tube. The rolling balls 36 are also held by a processing ring 40. Each rolling ball 36 can rotate on its own axis, and each rolling ball 36 can perform planetary rotation within the processing ring 40 while in contact with the outer surface of the mother tube 31. The grooved plug 35 and the rolling balls 36 form a rolling section 37. Furthermore, a shaping die (not shown) is provided downstream of the rolling section 37 in the drawing direction of the mother tube 31 to reduce the outer diameter of the mother tube 31, which has grooves formed on its inner surface, to a predetermined dimension.

[0042] Next, a method for producing the grooved pipe of the present invention using such a production apparatus will be described. First, the blank tube 31 is subjected to diameter reduction processing by a holding plug 32 and a holding die 33 . Next, the diameter of this reduced mother tube 31 is reduced by pressing it with rolling balls 36 that rotate in planetary rotation around the outside of the mother tube 31, and at the same time, the inner surface of the mother tube 31 is pressed against the grooved plug 35. As a result, the grooves of the grooved plug 35 are transferred to the inner surface of the mother tube 31, and spirally extending fins 39 are formed. At this time, the grooved plug 35 rotates due to the fins 39 that it itself formed on the inner surface of the mother tube 31. In addition, the grooved plug 35 is connected to the retaining plug 32 via the plug shaft 34, and this retaining plug 32 remains in a position on the inner side of the retaining die 33 due to the frictional force caused by the drawing of the mother tube 31 and the resistance force from the retaining die 33, so that the grooved plug 35 also stops in a position on the inner side of the rolling balls 36. Next, the blank tube 31 having grooves formed on its inner surface that has passed through the rolling section 37 is further reduced in diameter by a shaping die (not shown) to become the grooved tube of the present invention. The internally grooved pipe thus formed is usually wound into a coil, which is then annealed and shipped to air conditioner manufacturers and the like.

[0043] <Heat exchanger of the present invention> The heat exchanger of the present invention will now be described. The heat exchanger of the present invention is not particularly limited as long as it is a heat exchanger equipped with the grooved tube of the present invention. For example, FIG. 7 is a partially cutaway front view illustrating a heat exchanger 60 of the present invention, which is a fin-and-tube type heat exchanger incorporating the grooved tube of the present invention, and FIG. 8 is a partially enlarged view (schematic perspective view) thereof. As shown in Figs. 7 and 8, in the heat exchanger 60 of the present invention, the grooved tube 52 of the present invention is processed into a hairpin tube. The heat exchanger 60 has a plurality of aluminum fins 50 stacked in parallel and a grooved tube 52 of the present invention, and the grooved tube 52 of the present invention is inserted into each of a plurality of holes provided in the aluminum fins 50, and is fixed by primary expansion. A return bend tube 54 is interposed between the two grooved tubes 52 of the present invention to connect the two grooved tubes 52 of the present invention, and the grooved tube 52 of the present invention forms a flow path for the heat medium to flow over a long distance. Although a smooth tube is usually used as the return bend tube 54, the grooved tube of the present invention may be processed into a return bend tube for use. Air, etc. flows between the aluminum fins 50, and heat exchange is performed between the heat medium and the air, etc. by flowing a heat medium such as a fluorocarbon-based refrigerant inside the grooved tube 52 of the present invention. EXAMPLES

[0044] The present invention will be described with reference to examples, but the present invention is not limited to the embodiments described below.

[0045] Inner grooved pipes for flaring were manufactured according to Examples 1 to 7 and Comparative Examples 1 to 8, having the features shown in Table 1. All of them were seamless copper pipes made of C1020 (oxygen-free copper specified in JIS H 3300).

[0046] The outer diameter D, wall thickness T, radius of curvature r of the fin tip, and number of fins N of each of the inner grooved tubes for flaring shown in Table 1 are values ​​obtained by measuring, by the above-mentioned method, the ring-shaped cut surface obtained by cutting each inner grooved tube for flaring in a direction perpendicular to the tube axis. 2) was also measured and calculated using the method described above. Furthermore, the twist angles (θ) in Table 1 are also values ​​obtained by measurement using the method described above.

[0047] Each of the inner grooved pipes for flaring according to Examples 1 to 7 and Comparative Examples 1 to 8 was subjected to a push-expansion test. The expansion test involves gradually expanding the ends of each internally grooved tube for flaring using a flaring tool with a cone angle of 60 degrees until flaring cracks occur. Five of each of the inner grooved tubes for flaring were prepared, and their ends were gradually expanded using the flaring tool. The outer diameter at which a flaring crack occurred was determined in the same manner as in measuring the outer diameter D described above. That is, the outer diameter at which a flaring crack occurred (the outer diameter at the expanded end) was measured at eight locations (four pairs) that were approximately equal in the circumferential direction using a digital caliper, and the four measured values ​​were simply averaged to determine the value. The outer diameters (simple average values) of the five identical inner grooved tubes for flaring were then simply averaged, and the obtained value was determined as the outer diameter D' of the inner grooved tube for flaring after expansion.

[0048] The performance of the inner grooved pipe for flaring was evaluated based on the relationship between the obtained outer diameter D' and the outer diameter D before expanding. Specifically, if D'-D ≥ 2 was not satisfied, it was judged as failing (×), and if D'-D ≥ 2 was satisfied, it was judged as passing (◯). Furthermore, among the passing cases, if D'-D ≥ 2.32 was also satisfied, it was judged as being particularly good (◎).

[0049] Here, the reason why D'-D≧2 is considered acceptable will be explained. The wire diameter of the ring filler is usually φ1.4 mm. When fitting a U-shaped bent pipe to an inner grooved pipe for flaring with an outer diameter D of φ5.00 mm, in order to prevent the filler from leaking, it is necessary for the flare processing part to be expanded by about 1.0 mm on one side, which is equivalent to about 72% of the wire diameter of the ring filler, that is, to an outer diameter of 7.0 mm.

[0050] [Table 1] [Explanation of symbols]

[0051] 1, 1a, 1b fins 3a, 3b groove bottom Points 5a and 5b 10, 10a, 10b Test pieces 15 Fin of test piece (plate) 10a 16 Fin of test piece (plate) 10b 20 Substrate 30 Manufacturing equipment 31 Plain Tube 32 Retaining plug 33 Holding Dice 34 Plug shaft 35 Grooved plug 36 Rolling ball 37 Rolling section 39 Finn 40 Processing Ring 50 Aluminum fins 52 Grooved pipe of the present invention 54 Return bend pipe 60 Heat exchanger of the present invention

Claims

1. A seamless pipe having a groove on its inner surface and a flare at its end, The outer diameter D is 2.0 mm or more and 5.5 mm or less, The ratio T / D of the wall thickness T to the outer diameter D is 0.057-0.005D or more and 0.075-0.005D or less, The thickness T is 0.17 to 0.27 mm, The twist angle θ of the groove on the inner surface is 15 degrees or more and 27 degrees or less, The radius of curvature r of the tip of the fin constituting the groove on the inner surface and the number N of the fins in the circumferential direction satisfy the following formula (1), The tip curvature radius r and the twist angle θ satisfy the following formula (2), The tip curvature radius r is 0.036 to 0.045 mm, The number N of fins is 37 to 52, An inner grooved pipe for flaring, made of C1220 (phosphorus deoxidized copper), C1201 (low phosphorus deoxidized copper), or C1020 (oxygen-free copper) as specified in JIS H 3300. Formula (1): 0.500≦1 / (r×N)≦0.61 Formula (2): 0.046≦r×(1 / cosθ)≦0.051

2. A seamless pipe having a groove on its inner surface and a flare at its end, The outer diameter D is 2.0 mm or more and 5.5 mm or less, The ratio T / D of the wall thickness T to the outer diameter D is 0.057-0.005D or more and 0.075-0.005D or less, The thickness T is 0.17 to 0.27 mm, The twist angle θ of the groove on the inner surface is 15 degrees or more and 27 degrees or less, The radius of curvature r of the tip of the fin constituting the groove on the inner surface and the number N of the fins in the circumferential direction satisfy the following formula (1'), The tip curvature radius r and the twist angle θ satisfy the following formula (2'), The tip curvature radius r is 0.036 to 0.045 mm, The number N of fins is 37 to 52, An inner grooved pipe for flaring, made of C1220 (phosphorus deoxidized copper), C1201 (low phosphorus deoxidized copper), or C1020 (oxygen-free copper) as specified in JIS H 3300. Formula (1'): 0.52≦1 / (r×N)≦0.61 Formula (2'): 0.04≦r×(1 / cosθ)≦0.051

3. A heat exchanger comprising the inner grooved tube for flaring processing according to claim 1 or 2.

Citation Information

Patent Citations

  • Copper and copper alloy tube for flare processing