Greening base material
A greening base material with controlled fluorine and chromium elution levels in paper sludge ash, combined with gypsum and resin, addresses environmental pollution and enhances plant growth in slope greening applications.
Patent Information
- Application Number
- JP2023080612
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-28
AI Technical Summary
Existing greening base materials containing paper sludge ash (PS ash) suffer from high environmental pollution due to harmful components like coal, refuse derived paper and plastics, which inhibit plant growth and pose ecological risks.
A greening base material comprising paper sludge ash with controlled elution levels of fluorine (0.8 mg/L or less) and hexavalent chromium (0.05 mg/L or less), combined with a bonding material such as gypsum and synthetic resin, to enhance plant growth and reduce environmental impact.
The solution provides a low-pollution, cost-effective greening base material that supports plant germination and growth, effectively utilizing waste while minimizing environmental harm and maintaining soil integrity on slopes.
Smart Images

Figure 2024164897000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a greening base material. [Background technology]
[0002] Greening base materials ensure the retention of slopes by providing a base for plant growth. General greening base materials are mainly composed of base materials (bark compost, peat moss, etc.) and bonding materials (cement, synthetic resin, etc.), and may also contain plant seeds, chemical fertilizers, water-absorbing materials, etc.
[0003] The greening base material disclosed in Patent Document 1 may contain paper sludge ash (hereinafter also referred to as "PS ash") obtained by incinerating paper sludge (PS) as a water-absorbing material. PS is a waste product generated in the papermaking process. Therefore, the use of PS ash obtained from PS is an effective use of waste.
[0004] However, regular PS ash contains a large amount of harmful substances originating from coal, RPF (refuse derived paper and plastics densified fuel), wood chips, etc., which are incinerated together with PS. Therefore, greening base materials containing regular PS ash have the problem of being highly environmentally polluting. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-280075 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is to provide a greening base material that can effectively utilize waste, has low environmental pollution, and is suitable for greening slopes. [Means for solving the problem]
[0007] The invention described in claim 1 is a greening base material containing a base material and a bonding material, The bonding material contains at least paper sludge ash, The paper sludge ash is characterized in that the amount of fluorine eluted is 0.8 mg / L or less and the amount of hexavalent chromium eluted is 0.05 mg / L or less.
[0008] The invention described in claim 2 is the greening base material described in claim 1, The bonding material further contains gypsum.
[0009] The invention described in claim 3 is the greening base material described in claim 2, The bonding material further contains a synthetic resin.
[0010] The invention described in claim 4 is the greening base material described in claim 1, The content of the paper sludge ash is within a range of 15 to 30 kg per 1000 L of base material. Effect of the Invention
[0011] According to the present invention, it is possible to provide a greening base material which allows for effective use of waste, is less likely to pollute the environment, and is suitable for greening slopes. [Brief description of the drawings]
[0012] [Figure 1] Paper sludge ash photo [Diagram 2] Photograph of spraying greening base material [Diagram 3] Graph showing soil hardness measurement results in laboratory tests [Figure 4] Graph showing soil pH measurement results in laboratory tests [Diagram 5] Graph showing germination rate measurements in laboratory tests [Figure 6]Graph showing the results of measuring grass height in indoor tests [Figure 7] Photo of the slope after construction in the field test DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The following describes the embodiments of the present invention. However, the embodiments described below are subject to various technically preferable limitations for carrying out the present invention, but the scope of the invention is not limited to the embodiments described below.
[0014] The greening base material of the present invention is a greening base material containing a base material and a bonding material, and is characterized in that the bonding material contains at least paper sludge ash, and the paper sludge ash has a fluorine elution amount of 0.8 mg / L or less and a hexavalent chromium elution amount of 0.05 mg / L or less.
[0015] <Base material> As the base material, any base material generally used as a base material for greening base materials can be used without any restrictions. Examples of base materials include bark compost, peat moss, etc. Two or more types of base materials can be mixed and used. For example, bark compost and peat moss can be mixed and used as the base material.
[0016] <Binding material; PS ash> The greening base material of the present invention is characterized in that it contains at least paper sludge ash (PS ash) as a bonding material. The PS ash of the present invention is characterized in that the amount of fluorine eluted is 0.8 mg / L or less and the amount of hexavalent chromium eluted is 0.05 mg / L or less.
[0017] PS ash is ash obtained by incinerating paper sludge (PS). The main component of PS ash is quicklime (calcium oxide: CaO). Figure 1 is a photograph of PS ash.
[0018] PS ash gains strength when its main component, quicklime, absorbs water, preventing the greening base material from being washed away by rainfall, etc.
[0019] The amounts of fluorine and hexavalent chromium eluted are values measured in accordance with Ministry of the Environment Notification No. 46. Specifically, PS ash is used as a sample, and the amounts of elution are measured by preparing a sample solution, eluting, creating a test solution, and detecting the target components in accordance with Ministry of the Environment Notification No. 46.
[0020] PS ash in which the amount of fluorine elution and hexavalent chromium elution meet the above conditions can be obtained, for example, by incinerating PS alone, rather than together with other waste (coal, RPF, wood chips, etc.).
[0021] PS ash having fluorine elution and hexavalent chromium elution amounts that satisfy the above conditions can be obtained, for example, from Kaminoyama Paper Co., Ltd. The amounts of fluorine elution and hexavalent chromium elution from samples 1 to 6 of PS ash obtained from Kaminoyama Paper Co., Ltd. are shown in Table I below.
[0022] [Table 1]
[0023] The content of PS ash in the greening base material is not particularly limited, but is preferably within the range of 15 to 30 kg per 1000 L of base material. When the content of PS ash is within this range, the germination rate of plants is good.
[0024] <Binding material; other than PS ash> The greening base material of the present invention may further contain a bonding material other than PS ash. Examples of bonding materials other than PS ash include synthetic resin, gypsum, cement, etc.
[0025] From the viewpoint of the germination rate of plants, the greening base material of the present invention preferably further contains gypsum as a bonding material. Also, from the viewpoint of the germination rate and growth of plants, the greening base material of the present invention preferably further contains gypsum and a synthetic resin as bonding materials.
[0026] An example of a synthetic resin that can be suitably used for the greening base material of the present invention is an ethylene-vinyl acetate copolymer.
[0027] The content of the bonding material other than PS ash in the greening base material is not particularly limited. The content of the gypsum may be, for example, within the range of 1.5 to 3 kg per 1000 L of the base material. The content of the synthetic resin may be, for example, within the range of 0.4 to 1.5 kg per 1000 L of the base material. The content of the cement may be, for example, within the range of 7.5 to 15 kg per 1000 L of the base material.
[0028] <Plant seeds> The greening base material of the present invention may further contain plant seeds. As the plant seeds, those that are usually used for greening slopes can be used without any restrictions. Specific examples of the plant seeds include seeds of tall fescue, Kentucky bluegrass, etc.
[0029] In addition, the plant seeds may not be included in the greening base material, but may be scattered separately after the greening base material is sprayed. Also, since the plant seeds may be carried by wind or birds, it is not necessary to include them in the greening base material or to scatter them separately.
[0030] When plant seeds are contained in the greening base material, the content of the plant seeds may be within a range of, for example, 0.01 to 10 kg per 1000 L of base material.
[0031] <Other ingredients> In addition to the above-mentioned components, the greening base material may contain appropriate components such as natural fertilizers, chemical fertilizers, water-absorbent materials, etc., within limits that do not impair the effects of the present invention.
[0032] <Uses of greening base materials> The greening base material of the present invention can be suitably used in a slope greening method. The slope greening method can be carried out, for example, by spraying the greening base material onto the slope and allowing plants to germinate and grow on the greening base material. Figure 2 is a photograph of a photo of the greening base material spraying work. In one example of spraying the greening base material, the greening base material is compressed by air through a hose and sprayed onto the slope from a nozzle gun.
[0033] The greening base material of the present invention contains PS ash, which is waste from paper mills. Therefore, by using the greening base material of the present invention in a greening method, the waste can be effectively utilized. By being able to effectively utilize the waste, the greening base material of the present invention can be manufactured at low cost. In addition, by being able to effectively utilize the waste, the greening base material of the present invention contributes to resource circulation and reduction of carbon dioxide emissions.
[0034] The greening base material of the present invention contains PS ash with a fluorine elution amount of 0.8 mg / L or less and a hexavalent chromium elution amount of 0.05 mg / L or less. Because the elution amounts of fluorine and hexavalent chromium in the PS ash are low, the greening base material of the present invention is less environmentally polluting and less likely to inhibit plant germination and growth when used in greening techniques, compared with greening base materials containing normal PS ash.
[0035] PS ash imparts a soil hardness of 10 to 25 mm to the greening base material after construction. A greening base material with a soil hardness of 10 mm or more is less likely to flow away and is easily retained even when applied to a steep slope. A greening base material with a soil hardness of 25 mm or more is less likely to inhibit the growth of plant roots, and therefore is less likely to inhibit the germination and growth of plants. It is particularly preferable that the soil hardness of the greening base material after construction is within the range of 11 to 20 mm.
[0036] The soil hardness of the greening base material after construction can be measured with a Yamanaka soil hardness tester. Specifically, first, the cone of the soil hardness tester is pressed firmly vertically against the soil cross section until the brim is in close contact with the soil cross section. Next, the cone is gently pulled out so that the floating indicator does not move, and the hardness scale (mm or kg / cm) is read. 2 ) value. The measurement should be repeated three times for the same layer. The average of the three values should be used as the soil hardness. EXAMPLES
[0037] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0038] <Material> Details of the materials used in the examples are as follows: ·PS Ash Obtained from Kaminoyama Paper Co., Ltd. Fluorine elution amount measured according to Ministry of the Environment Notification No. 46: 0.66 mg / L Hexavalent chromium elution amount measured according to Ministry of the Environment Notification No. 46: below detection limit (0.005 mg / L) Calcium oxide content measured by fluorescent X-ray test: 59.9% ·Bark compost Agritech Co., Ltd., Greentech No. 1 Synthetic resin Japan Coating Resin Co., Ltd., Lunasol S, ethylene-vinyl acetate copolymer ·plaster Calcined plaster of Paris, manufactured by Kanto Chemical Co., Ltd. ·cement Portland cement ·Chemical fertilizer 1 Fukuei Fertilizer Co., Ltd., Advanced Chemical 555 ·Chemical fertilizer 2 Birdie Green, manufactured by JCAM AGRI
[0039] <Laboratory testing> Starting in October 2021, indoor testing was conducted following the procedure below.
[0040] The materials were mixed to obtain the compositions shown in Tables II to IV below to produce each of the greening base materials (Comparative Examples 1 to 4, Examples 1 to 10). Among the composition values shown in Tables II to IV, the values in parentheses are converted into amounts per 1000 L of base material.
[0041] A greening base material was laid in each container having an area of 265 mm x 183 mm. 15 plant seeds were sown on the greening base material in each container. Tall fescue seeds and Kentucky bluegrass seeds were used as the plant seeds. In each comparative example and example, a sample sown with tall fescue seeds and a sample sown with Kentucky bluegrass seeds were prepared.
[0042] The seeds were grown in a simple greenhouse outdoors, with adequate watering. The seeds were observed twice a week during cultivation, and the germination rate was measured. The germination rate is the ratio of germinated seeds out of the total number of seeds sown (15 seeds). The germination rates of each plant on each greening base material are shown in Tables II to IV.
[0043] Cultivation was continued, and two months after sowing, the soil hardness, soil pH, and plant height of each plant in each greening base material were measured. Soil hardness was measured by the method described above using a Yamanaka soil hardness meter. Soil pH was measured by inserting a sensor directly into the soil using a soil pH meter (FUSO, PH-212). Plant height was the average height of the plants grown in each greening base material at the time of measurement. The soil hardness, soil pH, and plant height of each plant in each greening base material were as shown in Tables II to IV.
[0044] [Table 2]
[0045] [Table 3]
[0046] [Table 4]
[0047] 3 to 6 are graphs showing the results of the evaluations in the laboratory tests. From the results of the laboratory tests, it was confirmed that the germination rate was better in the examples, particularly when the content of PS ash was within the range of 15 to 30 kg per 1000 L of base material, or when gypsum was further contained in addition to PS ash. It was also confirmed that the germination rate and growth were better in the examples, particularly when gypsum and synthetic resin were further contained in addition to PS ash.
[0048] <Field Test> Field testing was conducted from July 2022, following the procedure below.
[0049] Each greening base material (Comparative Example 5, Examples 11 and 12) was manufactured by mixing the materials to obtain the composition shown in Table V below. Among the composition values shown in Table V, the values in parentheses are values converted as the amount per 1000 L of base material.
[0050] The field test was carried out on a slope with a gradient of 80% (approximately 50°) and multiple frames formed on it. The size of each frame was 1.7m x 1.7m.
[0051] The greening base material thus produced was sprayed onto eight slope frames per sample to a thickness of 7 cm. Figure 7 shows a photograph of the slope after construction. Of the six slope frames constructed, the two on the left side were slope frames constructed with the greening base material of Comparative Example 5, the two in the middle with the greening base material of Example 11, and the two on the right side with the greening base material of Example 12.
[0052] The material cost was reduced by 2.5% in Example 11 and increased by 0.7% in Example 12, based on Comparative Example 5.
[0053] The workability of both Example 11 and Example 12 was equivalent to that of Comparative Example 5, which was the benchmark.
[0054] After application, the state of plant growth was checked approximately once every two months. The growth performance of Example 11 was equivalent to that of Comparative Example 5, which was the benchmark, while that of Example 12 was slightly inferior to that of Comparative Example 5, which was the benchmark.
[0055] Two months after application, the soil hardness of each greening base material was measured using the Yamanaka soil hardness meter as described above. The soil hardness of each greening base material is shown in Table V.
[0056] [Table 5]
[0057] As a result of the field test, it was confirmed that the greening base material of the present invention can be used in the field without any problems.
Claims
1. A greening base material containing a base material and a bonding material, The bonding material contains at least paper sludge ash, The paper sludge ash has a fluorine elution amount of 0.8 mg / L or less and a hexavalent chromium elution amount of 0.05 mg / L or less. A greening base material characterized by the above.
2. The bonding material further contains gypsum.
2. The greening base material according to claim 1.
3. The bonding material further contains a synthetic resin.
3. The greening base material according to claim 2.
4. The content of the paper sludge ash is within the range of 15 to 30 kg per 1000 L of base material.
2. The greening base material according to claim 1.
Citation Information
Patent Citations
Tree planting foundation bed material and tree planting construction method employing it
JP1999280075A