Surface-modified negative electrode active material particle, negative electrode mixture, lithium ion battery, and production method of negative electrode mixture

Surface-modified silicon particles with fluoroalkyl groups enhance the affinity between silicon and fluorine-containing binders, reducing resistance and improving lithium ion battery performance.

JP2024165021AInactive Publication Date: 2024-11-28TOYOTA JIDOSHA KK
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023080827
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium ion batteries face high resistance issues due to the interaction between silicon particles and binders in the negative electrode composite material.

Method used

Surface modification of silicon particles with fluoroalkyl groups improves the affinity between silicon particles and fluorine-containing binders, resulting in a negative electrode composite material with reduced resistance.

Benefits of technology

The modified silicon particles lead to a more uniform charge distribution and lower resistance in lithium ion batteries, enhancing their performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165021000001_ABST
    Figure 2024165021000001_ABST
Patent Text Reader

Abstract

To provide: surface-modified negative electrode active material particles having low resistance; a negative electrode mixture including such surface-modified negative electrode active material particles; a lithium ion battery including such surface-modified negative electrode active material particles; and a production method of such surface-modified negative electrode active material particles.SOLUTION: Surface-modified negative electrode active material particles of the present disclosure have silicon particles and a fluoroalkyl group that modifies the surface of the silicon particles. A negative electrode mixture of the present disclosure includes surface-modified negative electrode active material particles and a fluorine-containing binder. In addition, the surface-modified negative electrode active material particles included in the negative electrode mixture of the present disclosure have silicon particles and a fluoroalkyl group that modifies the surface of the silicon particles. A lithium ion battery of the present disclosure has a negative electrode active material layer containing a negative electrode mixture. A method of the present disclosure for producing surface-modified negative electrode active material particles includes modifying the surface of the silicon particles with the fluoroalkyl group.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to surface-modified negative electrode active material particles, a negative electrode mixture, a lithium ion battery, and a method for producing the negative electrode mixture. [Background technology]

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is known as a negative electrode active material for batteries.

[0003] Patent Document 1 describes a carbon-based negative electrode active material and a porous SiO x particles (0≦x<2), x The particles include an oxide layer coated on the surface, and the porous SiO x The particles are porous silicon particles, the thickness of the oxide film layer is 40 nm or more and 200 nm or less, and the porous SiO x The specific surface area of ​​the particles is 5m 2 / g to 50m 2 / g. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-120866 A Summary of the Invention [Problem to be solved by the invention]

[0005] In lithium ion batteries, it is desirable to reduce resistance.

[0006] An object of the present disclosure is to provide surface-modified negative electrode active material particles having low resistance, a negative electrode composite including such surface-modified negative electrode active material particles, a lithium ion battery including such surface-modified negative electrode active material particles, and a method for producing such surface-modified negative electrode active material particles. [Means for solving the problem]

[0007] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> Silicon particles, and The fluoroalkyl group modifying the surface of the silicon particle The surface-modified negative electrode active material particles have the following structure: <Aspect 2> 2. The surface-modified negative electrode active material particle according to aspect 1, having a silicon-oxygen-silicon-carbon bond, the silicon not bonded to the carbon being the silicon of the silicon particle, and the carbon being the carbon of a fluoroalkyl group. <Aspect 3> 2. The surface-modified negative electrode active material particles according to aspect 1, wherein the fluoroalkyl group has 3 or more and 12 or less carbon atoms. <Aspect 4> The surface-modified negative electrode active material particles according to any one of aspects 1 to 3, and Contains a fluorine-containing binder, Negative electrode composite material. <Aspect 5> 5. The negative electrode composite of claim 4, wherein the fluorine-containing binder is a polyvinylidene fluoride-based binder. <Aspect 6> A negative electrode active material layer is provided, and The negative electrode active material layer contains the negative electrode mixture according to aspect 4 or 5. Lithium-ion battery. Aspect 7 modifying the surface of silicon particles with fluoroalkyl groups; A method for producing surface-modified negative electrode active material particles. <Aspect 8> The method according to embodiment 7, wherein the surface of the silicon particle is modified with a fluoroalkyl group by dehydration condensation between a silanol group on the surface of the silicon particle and a silanol group generated by hydrolyzing a hydrolyzable group-containing silane having a fluoroalkyl group. Effect of the Invention

[0008] According to the present disclosure, it is possible to provide surface-modified negative electrode active material particles having low resistance, a negative electrode composite including such surface-modified negative electrode active material particles, a lithium ion battery including such surface-modified negative electrode active material particles, and a method for producing such surface-modified negative electrode active material particles. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 shows the results of XPS measurement (Si(2p)) of Comparative Synthesis Examples 1 to 3 and Synthesis Examples 1 and 2. [Diagram 2] FIG. 2 shows the results of XPS measurement (F(1s)) of Comparative Synthesis Examples 1 to 3 and Synthesis Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0011] 《Surface modified negative electrode active material particles》 The surface-modified negative electrode active material particles of the present disclosure have silicon particles and fluoroalkyl groups modifying the surfaces of the silicon particles.

[0012] The present inventors have found that a lithium ion battery containing silicon particles whose surfaces are modified with fluoroalkyl groups as a negative electrode active material has low resistance. The reason for this is presumed to be as follows, without intending to be bound by any theory. That is, it is believed that by modifying the surfaces of the silicon particles, the affinity between the silicon particles and the fluorine-containing binder in the negative electrode mixture is improved. And, it is believed that a battery made using this negative electrode mixture is easily charged uniformly, and therefore has low resistance.

[0013] <Silicon particles> The surface-modified negative electrode active material particles of the present disclosure include silicon particles.

[0014] The composition of the silicon particles is not particularly limited. The proportion of silicon element in all elements contained in the silicon particles may be, for example, 50 mol % or more, 70 mol % or more, or 90 mol % or more.

[0015] The silicon particles may contain other elements such as Li element in addition to Si element. Examples of other elements include Sn element, Fe element, Co element, Ni element, Ti element, Cr element, B element, and P element in addition to Li element.

[0016] The silicon particles may contain impurities such as oxides.

[0017] The silicon particles may be amorphous or crystalline, and the crystal phase contained in the silicon particles is not particularly limited.

[0018] The shape and size of the silicon particles are not particularly limited. The average particle size of the silicon particles may be, for example, 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and may be 10 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. The average particle size can be determined by observation with an electron microscope such as an SEM, and is determined, for example, as the average value of the maximum Feret diameters of each of a plurality of particles. The number of samples is preferably large, for example, 20 or more, 50 or more, or 100 or more. The average particle size can be appropriately adjusted, for example, by appropriately changing the manufacturing conditions of the silicon particles described later or by performing a classification process.

[0019] The silicon particles contained in the surface-modified negative electrode active material particles may be porous silicon particles. The porous silicon particles contain silicon having a plurality of voids. There is no particular limitation on the shape of the voids in the porous silicon particles.

[0020] The porous silicon particles may be particles containing nanoporous silicon. Nanoporous silicon refers to silicon having a plurality of pores with pore diameters on the nanometer order (less than 1000 nm, preferably 100 nm or less).

[0021] <Fluoroalkyl Group> The surface-modified negative electrode active material particles of the present disclosure have fluoroalkyl groups modifying the surfaces of silicon particles.

[0022] The number of carbon atoms in the fluoroalkyl group may be 3 or more and 15 or less. The number of carbon atoms may be 4 or more, 5 or more, 6 or more, 7 or more, or 8 or more, and may be 14 or less, 13 or less, 12 or less, 11 or less, or 10 or less. The fluoroalkyl group may have a linear, branched, or cyclic structure, but is preferably a linear fluoroalkyl group. The fluoroalkyl group may be a perfluoroalkyl group, and may be an alkyl group in which some of the hydrogen atoms are substituted with fluorine (for example, -(CH 2 ) 2 (CF 2) n CF 3 (n is an integer of 0 to 12), but is preferably -(CH 2 ) 2 (CF 2 ) n CF 3 (n is an integer of 0 to 12).

[0023] The surface-modified negative electrode active material particles of the present disclosure have a silicon-oxygen-silicon-carbon bond, and the silicon not bonded to the carbon may be silicon of a silicon particle, and the carbon may be carbon of a fluoroalkyl group. That is, the carbon of a fluoroalkyl group may be bonded to silicon on the surface of a silicon particle via oxygen and silicon.

[0024] <<Method for producing surface-modified negative electrode active material particles>> The disclosed method of making surface-modified negative electrode active material particles includes modifying the surfaces of silicon particles with fluoroalkyl groups.

[0025] The surfaces of the silicon particles may be modified with fluoroalkyl groups by dehydration condensation between silanol groups on the surfaces of the silicon particles and silanol groups generated by hydrolysis of a hydrolyzable group-containing silane having a fluoroalkyl group.

[0026] As the hydrolyzable group-containing silane, a hydrolyzable group-containing silane having a structure corresponding to the above description of the fluoroalkyl group in the present disclosure can be used.

[0027] 《Negative electrode mixture》 The negative electrode mixture of the present disclosure includes surface-modified negative electrode active material particles and a fluorine-containing binder. The surface-modified negative electrode active material particles included in the negative electrode mixture of the present disclosure include silicon particles and fluoroalkyl groups that modify the surfaces of the silicon particles.

[0028] Without intending to be bound by any theory, it is believed that by making both the surface modifying group and the binder fluorine-based, the silicon particles and the binder are firmly bonded via the surface modifying group, and the peel strength between the negative electrode active material layer and the negative electrode current collector layer is improved, thereby suppressing cracking of the negative electrode active material layer, and as a result, the resistance is reduced.

[0029] In the present disclosure, the term "negative electrode mixture" refers to a composition that can form a negative active material layer as it is or by further containing other components. In the present disclosure, the term "negative electrode mixture slurry" refers to a slurry that contains a dispersion medium in addition to the "negative electrode mixture" and can be applied and dried to form a negative electrode active material layer.

[0030] <Surface modified negative electrode active material particles> The negative electrode mixture of the present disclosure includes surface-modified negative electrode active material particles. For the surface-modified negative electrode active material particles, reference can be made to the above description of the surface-modified negative electrode active material particles of the present disclosure.

[0031] <Fluorine-containing binder> The negative electrode mixture of the present disclosure includes a fluorine-containing binder. Examples of the fluorine-containing binder include polyvinylidene fluoride (PVdF)-based binders and polytetrafluoroethylene (PTFE)-based binders. The fluorine-containing binder is preferably a PVdF-based binder. The PVdF-based binder may be a copolymer having a unit derived from a monomer other than VdF.

[0032] The negative electrode mixture of the present disclosure also optionally includes an electrolyte, a conductive aid, and a binder other than the fluorine-containing binder.

[0033] <Electrolyte> The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.

[0034] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li 2 SP 2 S 5 System (Li 7 P 3 S 11 , Li 3 P.S. 4 , Li 8 P 2 S 9 etc.), Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 SP 2 S 5 , LiI-LiBr-Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -GeS 2 (Li 13 GeP 3 S 16 , Li 10 GeP 2 S 12 etc.), LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 , Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.

[0035] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).

[0036] In addition, when the negative electrode composite material contains a solid electrolyte, the mass ratio of the surface-modified negative electrode active material particles to the solid electrolyte in the negative electrode composite material (mass of the surface-modified negative electrode active material particles:mass of the solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0037] The electrolyte preferably contains a supporting salt and a solvent.

[0038] As a supporting salt (lithium salt) of the electrolyte having lithium ion conductivity, for example, LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 Inorganic lithium salts such as LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(FSO 2 ) 2 , LiC(CF 3 SO 2 ) 3 Examples of organic lithium salts include:

[0039] Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.

[0040] <Conductive assistant> The conductive assistant is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.

[0041] <Binders other than fluorine-containing binders> The binder other than the fluorine-containing binder is not particularly limited. For example, the binder may be a material such as butadiene rubber (BR) or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto. The ratio of the mass of the binder other than the fluorine-containing binder to the total mass of the binder may be less than 50 mass%, less than 40 mass%, less than 30 mass%, less than 20 mass%, or less than 10 mass%, or may be 0 mass%. Lithium-ion battery The lithium ion battery of the present disclosure has a negative electrode active material layer, and the negative electrode active material layer contains the negative electrode mixture of the present disclosure. The lithium ion battery of the present disclosure may have, in this order, a negative electrode current collector layer, a negative electrode active material layer containing the negative electrode mixture of the present disclosure, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.

[0042] The lithium ion battery of the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be a solid battery having a solid electrolyte layer as an electrolyte layer. In the present disclosure, a "solid-state battery" means a battery using at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery using only a solid electrolyte as an electrolyte.

[0043] The lithium ion battery may be a primary battery or a secondary battery.

[0044] Examples of the shape of the lithium ion battery include a coin type, a laminate type, a cylindrical type, and a square type.

[0045] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.

[0046] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0047] <Negative electrode active material layer> The negative electrode active material layer of the present disclosure contains the negative electrode mixture of the present disclosure. For the negative electrode mixture, the above description of the negative electrode mixture of the present disclosure can be referenced.

[0048] The thickness of the negative electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0049] <Electrolyte layer> The electrolyte layer includes at least an electrolyte. In addition to the electrolyte, the electrolyte layer may include a binder or the like as necessary. For the electrolyte, the above description of the negative electrode mixture of the present disclosure can be referred to. The binder may be, for example, polyvinylidene fluoride (PVdF), butadiene rubber (BR), styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.

[0050] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.

[0051] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally an electrolyte, a conductive assistant, a binder, and the like.

[0052] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material is lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganate (LiMn 2 O 4 ), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O 2 , Li 1+x Mn 2-x-y MyO 4 Li-Mn spinel substituted with different elements having a composition represented by the formula (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO 4 , M may be one or more metals selected from Fe, Mn, Co, and Ni), but is not limited thereto.

[0053] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials that constitute the coating layer include LiNbO 3 In addition, Li 4 Ti 5 O 12 , Li 3 PO 4 These include, but are not limited to, the following.

[0054] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0055] For the electrolyte and the conductive assistant, the above description of the negative electrode mixture of the present disclosure can be referred to. For the binder, the above description of the electrolyte layer of the present disclosure can be referred to.

[0056] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.

[0057] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0058] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc. may be used, but is not limited to these.

[0059] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred. EXAMPLES

[0060] <<Preparation of surface-modified negative electrode active material particles>> Preparation of Silicon Particles (Comparative Synthesis Example 1) Silicon particles were prepared as a silicon (Si) source. The silicon particles and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed silicon particles and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere to obtain porous silicon particles.

[0061] <Modification with Fluoroalkyl Groups> (Synthesis Example 1) In an argon (Ar)-substituted glove box, 2 g of porous silicon particles, 20 g of ultra-dehydrated ethanol (Fujifilm Wako Pure Chemical Industries, Ltd.), and a fluoroalkyl group (-C 2 H 4 (CF 2 ) 5 CF 3 0.15 g of trimethoxy(1H,1H,2H,2H-tridecafluoro-n-octyl)silane (Tokyo Chemical Industry Co., Ltd.), a silane coupling agent having a fluoroalkyl group, was weighed out and placed in a sealed reaction vessel and stirred at 50°C for 16 hours to dehydrate and condense the silanol groups on the surfaces of the silicon particles with the silanol groups generated by hydrolysis of the silane coupling agent having a fluoroalkyl group. The solution after the reaction was suction filtered, washed with 30 mL of ethanol, and filtered, and this operation was repeated five times. The obtained solid was vacuum dried at 100°C for 12 hours to remove the -C from the surfaces of the silicon particles. 2 H 4 (CF 2 ) 5 CF 3 Thus, surface-modified negative electrode active material particles were obtained.

[0062] (Synthesis Example 2) The silane coupling agent is a fluoroalkyl group (-C 2 H 4 (CF 2 ) 7 CF 3 The surface of the silicon particles was coated with -C in the same manner as in Synthesis Example 1, except that 0.18 g of trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane (manufactured by Tokyo Chemical Industry Co., Ltd.) was used. 2 H 4 (CF 2 ) 7 CF 3 Thus, surface-modified negative electrode active material particles were prepared.

[0063] (Comparative Synthesis Example 2) The silane coupling agent is a silane having an alkyl group (-(CH 2 ) 5 CH 3The surface of the silicon particles was coated with -(CH 2 ) 5 CH 3 Thus, surface-modified negative electrode active material particles were prepared.

[0064] (Comparative Synthesis Example 3) The silane coupling agent is a silane having an alkyl group (-(CH 2 ) 7 CH 3 The surface of the silicon particles was coated with -(CH 2 ) 7 CH 3 Thus, surface-modified negative electrode active material particles were prepared.

[0065] Making a Battery Preparation of Positive Electrode Mixture A polypropylene (PP) container is filled with butyl butyrate, a 5 wt% butyl butyrate solution of polyvinylidene fluoride (PVDF) binder, and LiNi as the positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 (average particle size: 6μm), Li as sulfide solid electrolyte 2 SP 2 S 5 The glass ceramic and vapor grown carbon fiber (VGCF) as a conductive additive were added to the container and stirred for 30 seconds with an ultrasonic disperser (UH-50, manufactured by SMT). Next, the container was shaken for 3 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) and stirred for 30 seconds with the ultrasonic disperser. It was further shaken for 3 minutes with the shaker to obtain a slurry-like positive electrode mixture (positive electrode mixture slurry).

[0066] <Formation of Positive Electrode Active Material Layer> The obtained slurry was applied to an aluminum (Al) foil (manufactured by Showa Denko) as a positive electrode current collector layer by a blade method using an applicator. The applied slurry was dried for 30 minutes on a hot plate at 100° C. As a result, a positive electrode active material layer was formed on the positive electrode current collector layer.

[0067] <Preparation of negative electrode mixture> (Comparative Examples 1 to 3, and Examples 1 and 2) A polypropylene (PP) container was filled with diisobutyl ketone, a 5 wt% diisobutyl ketone solution of a PVDF-based binder (Kureha Corporation: KF8300), VGCF as a conductive additive, and Li as a solid electrolyte. 2 SP 2 S 5 The glass ceramics and the silicon particles of Comparative Synthesis Examples 1 to 3 and Synthesis Examples 1 and 2 as negative electrode active materials were added to a container and stirred for 30 seconds with an ultrasonic dispersing device (UH-50, manufactured by SMT Co., Ltd.). The container was then shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain the slurry-like negative electrode composites (negative electrode composite slurries) of Comparative Examples 1 to 3 and Examples 1 and 2.

[0068] (Comparative Examples 4 and 5) Negative electrode mixture slurries of Comparative Examples 4 and 5 were prepared in the same manner as in Examples 1 and 2, except that the binder was changed to a 5 wt % diisobutyl ketone solution of a styrene butadiene rubber (SBR)-based binder.

[0069] <Formation of negative electrode active material layer> The obtained slurry was applied onto a nickel (Ni) foil as a negative electrode current collector by a blade method using an applicator. The applied slurry was dried for 30 minutes on a hot plate at 100° C. This formed a negative electrode active material layer on the negative electrode current collector layer.

[0070] <Formation of solid electrolyte layer> A polypropylene (PP) container is filled with heptane, a 5 wt% heptane solution of SBR binder, and Li as a solid electrolyte. 2 SP 2 S5 A glass ceramic based on the system was added and stirred for 30 seconds with an ultrasonic dispersing device (UH-50 manufactured by SMT). The container was then shaken for 30 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) to obtain a solid electrolyte slurry. The obtained slurry was applied to an Al foil by a blade method using an applicator. The applied slurry was dried for 30 minutes on a hot plate at 100°C. This formed a solid electrolyte layer. Three solid electrolyte layers were produced.

[0071] <Battery Assembly> The positive electrode current collector layer, the positive electrode active material layer, and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. in the first pressing step to obtain a positive electrode laminate.

[0072] The negative electrode current collector layer, the negative electrode active material layer, and the second solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. in the second pressing step to obtain a negative electrode laminate.

[0073] The negative electrode laminate and the positive electrode laminate were fabricated so that the area of ​​the negative electrode laminate was larger than the area of ​​the positive electrode laminate.

[0074] Further, an Al foil as a release sheet, an intermediate solid electrolyte layer formed on the Al foil, and the negative electrode laminate were laminated so that the solid electrolyte layers were in contact with each other. The laminate was set in a flat uniaxial press and temporarily pressed for 10 seconds at a pressure of 100 MPa and a temperature of 25° C. The Al foil was peeled off from the intermediate solid electrolyte layer of the laminate to obtain a negative electrode laminate further laminated with an intermediate solid electrolyte layer.

[0075] The positive electrode laminate and the negative electrode laminate further having an intermediate solid electrolyte layer laminated thereon were laminated so that the solid electrolyte layers were in contact with each other. This laminate was set in a flat uniaxial press and pressed for 1 minute at a pressure of 200 MPa and a temperature of 120°C in the third pressing step. This produced an all-solid-state battery.

[0076] "evaluation" Analysis of the surface properties of silicon particles The carbon content of silicon particles of the synthesis example and the comparative synthesis example was measured by high-frequency combustion infrared absorption method (apparatus used: LECO, CSLS600). In addition, the fluorine content of silicon particles of each example was measured by combustion ion chromatography (apparatus used: Thermo Fisher Scientific, ICS-1500 type ion chromatograph, Nitto Seiko Analytech, AQF-100 type automatic sample combustion apparatus).

[0077] Furthermore, the surface of the silicon particles of each example was analyzed by X-ray photoelectron spectroscopy (XPS) (apparatus used: PHI 5000 Versaprobe II, manufactured by ULVAC-PHI). Measurements were performed under the following conditions: X-ray source: AlKα, 15 kV, 3 mA, energy step: 0.1 eV, number of sweeps: 4 times. The peak areas of XPS were measured by drawing a baseline for each peak using XPS analysis software (MultiPak, manufactured by ULVAC-PHI), and obtaining the integrated intensity (area) of each peak. The area ratio of F(1s) / Si(2p) was calculated from the obtained areas (F(1s): 684-692 eV, Si(2p): 95-107 eV).

[0078] <DCIR Measurement> The prepared battery was restrained at a predetermined restraining pressure using a restraining jig, and was charged at a constant current and constant voltage at 1 / 10C to 4.55V (1 / 100C cut), and then discharged at 1C to 3.0V. Then, it was charged at a constant current and constant voltage at 1 / 3C to 4.35V (1 / 100C cut), and then discharged at a constant current and constant voltage at 1 / 3C to 3.00V (1 / 100C cut). Furthermore, it was charged at a constant current and constant voltage at 1 / 3C to 4.35V (1 / 100C cut), and then discharged at a constant current and constant voltage at 1 / 3C to 3.14V (1 / 100C cut). Then, a constant current of 5C was applied for 10s, and the direct current internal resistance (DCIR) was measured.

[0079] "result" Analysis of the surface properties of silicon particles The results of quantitative analysis of the carbon amount and fluorine amount of the silicon particles of the Comparative Synthesis Example and Synthesis Example are shown in Table 1. The results of XPS analysis of each silicon particle are shown in Table 1 and in FIGS.

[0080] [Table 1]

[0081] As shown in Table 1, the silicon particles of the synthesis examples had larger carbon and fluorine amounts on the particle surface, and larger values ​​of F(1s) / Si(2p) than the silicon particles of Comparative Synthesis Example 1. From these facts, it is considered that the surface of the silicon particles of the examples was modified with fluoroalkyl groups. In addition, since the silicon particles of Comparative Synthesis Examples 2 and 3 had larger carbon amounts on the particle surface than the silicon particles of Comparative Synthesis Example 1, it is considered that the surface of these silicon particles was modified with alkyl groups.

[0082] <DCIR Measurement> The results of the DCIR measurement of the batteries of each example are shown in Table 2. The DCIR value of each example is expressed as a relative value when the measurement result of Comparative Example 1 is set to 1.00.

[0083] [Table 2]

[0084] As shown in Table 2, the DCIR values ​​were small in the batteries of the Examples in which both the surface modifying group and the binder were fluorine-based. In contrast, the DCIR values ​​in the batteries of Comparative Examples 2 to 5 in which either the surface modifying group or the binder was non-fluorine-based were equivalent to that of Comparative Example 1 in which unmodified silicon particles were used.

Claims

1. Silicon particles, and The fluoroalkyl group modifying the surface of the silicon particle The surface-modified negative electrode active material particles have the following structure:

2. 2. The surface-modified negative electrode active material particle according to claim 1, having a silicon-oxygen-silicon-carbon bond, the silicon not bonded to the carbon being silicon of the silicon particle, and the carbon being carbon of a fluoroalkyl group.

3. The surface-modified negative electrode active material particles according to claim 1 , wherein the fluoroalkyl group has 3 or more and 12 or less carbon atoms.

4. The surface-modified negative electrode active material particles according to claim 1 , and Contains a fluorine-containing binder, Negative electrode composite material.

5. 5. The negative electrode mixture of claim 4, wherein the fluorine-containing binder is a polyvinylidene fluoride-based binder.

6. A negative electrode active material layer is provided, and The negative electrode active material layer contains the negative electrode mixture according to claim 4 or 5. Lithium-ion battery.

7. modifying the surface of silicon particles with fluoroalkyl groups; A method for producing surface-modified negative electrode active material particles.

8. The method according to claim 7, wherein the surface of the silicon particle is modified with the fluoroalkyl group by dehydration condensation between the silanol group on the surface of the silicon particle and the silanol group generated by hydrolyzing a hydrolyzable group-containing silane having a fluoroalkyl group.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery and manufacture for electrode

    JP1999354104A

  • Negativee active material for lithium secondary battery, manufacturing method therefor, and lithium secondary battery containing the material

    JP2008130570A

  • Negative electrode material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    JP2013069531A

  • Negative electrode material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    JP2014002956A

  • Electrode and secondary battery

    JP2017174692A