Pile fabric having antifouling property, and method for manufacturing the pile fabric

The pile fabric with silicon-exposed and fluorine-coated parts on flame-retardant fibers addresses the lack of comprehensive stain resistance in existing technologies, providing effective protection against dry and wet stains and maintaining fabric integrity.

JP2024165358APending Publication Date: 2024-11-28AUNDE TEXTILE CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023081500
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing functional fabrics for transportation equipment interiors lack effective stain resistance against both dry and wet stains, with conventional technologies either focusing on water and oil repellency or stain resistance but not both, and also suffer from issues like dry dirt adsorption and fabric texture deterioration.

Method used

A pile fabric with silicon-exposed and fluorine-coated parts, using flame-retardant fibers, where silicon-based fine particles are exposed on the fiber surface and coated with a fluorine-based water and oil repellent, along with a back coat of urethane resin and flame retardant to enhance stain resistance and prevent pile slippage.

Benefits of technology

The fabric achieves improved stain resistance against both dry and wet stains, prevents dry dirt adsorption, maintains fabric texture, and enhances flame retardancy while preventing pile slippage, even after repeated use and washing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165358000001_ABST
    Figure 2024165358000001_ABST
Patent Text Reader

Abstract

To realize "improvement of an antifouling property against both dry and wet stains" or the like by providing: a silicon-exposed part in which silicon-based particulates are exposed from a fiber surface of a pile fabric; a fluorine-coated part in which fluorine-based water-repellent and oil-repellent agent is coated on the silicon-based particulates, and so forth.SOLUTION: A pile fabric 1 in which a flame retardant fiber is used for a pile 2, and a flame non-retardant fiber is used for a base fabric 3, and which has: a silicon-exposed part 4 in which silicon-based particulates attached via binder resin are exposed on a fiber surface; a fluorine-coated part 5 in which fluorine-based water-repellent and oil-repellent agent is coated on the silicon-based particulates; and so forth. A method for manufacturing the pile fabric 1 comprises: a silicon attaching step P1 of applying a mixed liquid of the binder resin and silicon-based particulates to the pile fabric 1 and drying the fabric to provide the silicon-exposed part 4; and a fluorine coating step P2 of applying the fluorine-based water-repellent and oil-repellent agent to the provided silicon exposed part to provide the fluorine-coated part 5 thereon; and so forth.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pile fabric having stain-resistant properties and a method for producing the pile fabric. [Background technology]

[0002] Conventionally, functional fabrics that are applied to the interiors of transportation vehicles such as railway cars are also known (Patent Document 1). This functional fabric is made by forming a fluoropolymer film on the surface of the fibers.

[0003] Conventionally, stain-resistant fabrics for vehicle interior materials, which are used for various parts such as seats, have been known as interior materials for vehicles such as trains (Patent Document 2). This stain-resistant fabric for vehicle interior materials is formed by adhering a stain-resistant agent made of organopolysiloxane fine particles, a binder resin, and a smoothing agent to the fiber surface of a polyester fiber fabric. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-110069 A [Patent Document 2] JP 2011-168905 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the functional fabric described in Patent Document 1 has been surface-treated with a water- and oil-repellent agent, so to speak, and therefore naturally has stain-resistant properties against water-based stains and oil-based stains. However, there is a problem in that the fabric is more likely to adsorb dry stains (dry stains) such as black spots and soil. In addition, the stain-resistant fabric for vehicle interior materials described in Patent Document 2 has stain resistance against dry stains such as black carbon and soil, but does not have water-repellent or oil-repellent properties, and therefore does not have sufficient stain resistance against wet stains (wet stains) such as water-based stains and oil-based stains.

[0006] In view of the above, the present invention aims to provide a pile fabric which achieves "improved stain resistance against both dry and wet stains" by providing a silicon-exposed portion in which silicon-based microparticles are exposed on the fiber surface of the pile fabric, and a fluorine-coated portion in which the silicon-based microparticles are coated with a fluorine-based water- and oil-repellent agent, and a method for producing the pile fabric. [Means for solving the problem]

[0007] The pile fabric 1 according to the present invention is a pile fabric having piles 2 erected from a base fabric 3, the piles 2 being made of flame-retardant fibers and the base fabric 3 being made of non-flame-retardant fibers, and the pile fabric 1 has a first feature in that the fiber surfaces of the flame-retardant and non-flame-retardant fibers have silicon-exposed portions 4 in which silicon-based microparticles adhered to the fiber surface via a binder resin are exposed, and fluorine-coated portions 5 in which the silicon-based microparticles adhered to the fiber surface via the binder resin are coated with a fluorine-based water- and oil-repellent agent.

[0008] A second feature of the pile fabric 1 according to the present invention is that the pile fabric 1 has piles 2 erected from a base fabric 3, the piles 2 and the base fabric 3 are made of non-flame retardant fibers, and the fiber surface of the non-flame retardant fibers has silicon exposed portions 4 where silicon-based fine particles attached to the fiber surface via a binder resin are exposed, flame-retardant exposed portions 4' where a flame retardant attached to the fiber surface via the binder resin is exposed, a fluorine-coated portion 5 where the silicon-based fine particles attached to the fiber surface via the binder resin are coated with a fluorine-based water- and oil-repellent agent, and a fluorine-coated portion 5' where the flame retardant attached to the fiber surface via the binder resin is coated with a fluorine-based water- and oil-repellent agent.

[0009] A third feature of the pile fabric 1 according to the present invention is that, in addition to the above-mentioned first or second feature, the pile fabric 1 further has fiber exposed portions 6 where the fiber surfaces are exposed.

[0010] A fourth feature of the pile fabric 1 according to the present invention is, in addition to the first or second feature described above, that the back surface of the base fabric 3 has a back coat portion 10 coated with a mixture of at least a urethane resin and a flame retardant.

[0011] A fifth feature of the pile fabric 1 according to the present invention is that, in addition to the first or second feature, the amount of the silicon-based fine particles attached is 0.8 g / m 2 More than 4.5g / m 2 The amount of the binder resin adhered is 0.3 g / m or less. 2 More than 1.7g / m 2 The amount of the fluorine-based water / oil repellent agent attached is 0.5 g / m or less. 2 More than 2.9g / m 2 The point is as follows.

[0012] Due to these characteristics, in pile fabric 1 in which flame-retardant fibers are used for pile 2 and non-flame-retardant fibers are used for base fabric 3, by providing silicon-exposed portions 4 in which silicon-based microparticles adhered to the fiber surface via a binder resin are exposed, unlike Patent Document 1, it is possible to suppress adsorption of blackening (black carbon) and dry dirt such as soil onto the fiber surface. At the same time, the pile fabric 1 is provided with a fluorine-coated portion 5 in which silicon-based microparticles attached to the fiber surface via a binder resin are coated with a fluorine-based water- and oil-repellent agent. This makes it possible to impart water- and oil-repellent properties to the pile fabric 1, unlike Patent Document 2, and improves the stain resistance against wet stains such as water-based stains and oil-based stains. The pile fabric 1 can also be said to be a "pile fabric having stain-resistant properties." In addition, in the pile fabric 1, non-flame retardant fibers are used for the pile 2 and base fabric 3, and the pile fabric 1 may be provided with silicon exposed portions 4 and flame retardant exposed portions 4' in which silicon-based particles and flame retardant attached to the fiber surface via a binder resin are exposed, and fluorine-coated portions 5, 5' in which the silicon-based particles and flame retardant attached to the fiber surface via the binder resin are covered with a fluorine-based water- and oil-repellent agent.

[0013] Furthermore, by providing portions 6 where the fiber surface itself is exposed on the fiber surface, deterioration of the feel of the pile fabric 1 can be suppressed. In addition, in the functional fabric described in Patent Document 1, a fluoropolymer film is formed on the fiber surface, which means that the fluoropolymer is adhered to the fiber surface in excess, which can be said to degrade the texture of the fabric.

[0014] In addition, by providing a back coat portion 10 coated with a mixture of at least a urethane resin and a flame retardant on the back surface of the base fabric 3, the pile 2 is prevented from coming off the base fabric 3 and the flame retardancy of the pile fabric 1 is also improved. In addition, the amount of silicon-based particles attached is 0.8 g / m 2 More than 4.5g / m 2 The amount of binder resin attached is 0.3 g / m or less. 2 More than 1.7g / m 2 The amount of fluorine-based water and oil repellent applied is 0.5 g / m 2 More than 2.9g / m 2 The following is also acceptable.

[0015] A manufacturing method for a pile fabric 1 according to the present invention is a manufacturing method for a pile fabric having piles 2 erected from a base fabric 3, the pile fabric 2 being made of a flame-retardant fiber and the base fabric 3 being made of a non-flame-retardant fiber, and the method includes a silicon-imparting step P1 of applying a mixture of at least a binder resin and silicon-based microparticles to the pile fabric and then drying the pile fabric to provide silicon-exposed portions 4 on fiber surfaces of the flame-retardant and non-flame-retardant fibers, where the silicon-based microparticles adhered to the fiber surfaces via the binder resin are exposed, and a fluorine-coating step P2 of applying a fluorine-based water- and oil-repellent agent to the pile fabric after the silicon-imparting step P1 to provide fluorine-coated portions 5 on fiber surfaces of the flame-retardant and non-flame-retardant fibers, where the silicon-based microparticles adhered to the fiber surfaces via the binder resin are covered by the fluorine-based water- and oil-repellent agent.

[0016] A second feature of the method for producing the pile fabric 1 according to the present invention is a method for producing a pile fabric in which a pile 2 is erected from a base fabric 3, the pile 2 and the base fabric 3 are made of non-flame retardant fibers, a mixture of at least a binder resin, silicon-based microparticles, and a flame retardant is applied to the pile fabric, and the pile fabric is then dried to produce silicon exposed portions 4 on the fiber surfaces of the non-flame retardant fibers, where the silicon-based microparticles adhered to the fiber surfaces via the binder resin are exposed, and a mixture of at least a binder resin, silicon-based microparticles, and a flame retardant is applied to the fiber surfaces of the non-flame retardant fibers. and a fluorine-coating process P2' after the silicon / flame-retardant imparting process P1', in which a fluorine-based water / oil repellent agent is applied to the pile fabric to form a fluorine-coated portion 5 on the fiber surface of the non-flame-retardant fiber in which the silicon-based fine particles adhered to the fiber surface via the binder resin are coated with the fluorine-based water / oil repellent agent, and a fluorine-coated portion 5' in which the flame retardant adhered to the fiber surface via the binder resin is coated with the fluorine-based water / oil repellent agent.

[0017] A third feature of the method for producing the pile fabric 1 according to the present invention, in addition to the first or second feature, is that the application of the mixture in the silicon imparting step P1 or the silicon / flame retardant imparting step P1' is carried out in an atmosphere at a predetermined temperature, and the application of the mixture in the fluorine coating steps P2 and P2' is carried out in an atmosphere at a temperature higher than the predetermined temperature.

[0018] A fourth feature of the method for producing the pile fabric 1 according to the present invention, in addition to the first or second feature, is that the application of the mixture in the silicon imparting step P1 or the silicon / flame retardant imparting step P1' and the fluorine coating steps P2, P2' is carried out in an atmosphere at a predetermined temperature, and after the fluorine coating steps P2, P2', a backcoat step P3 is provided on the back surface of the base fabric 3 in an atmosphere at a temperature higher than the predetermined temperature, to provide a backcoat portion 10 coated with a mixture of at least a urethane resin and a flame retardant.

[0019] A fifth feature of the method for producing the pile fabric 1 according to the present invention is that, in addition to the first or second feature, the amount of the silicon-based fine particles applied is 0.8 g / m 2 More than 4.5g / m 2 The amount of the binder resin applied is 0.3 g / m or less. 2 More than 1.7g / m 2 The amount of the fluorine-based water / oil repellent applied is 0.5 g / m or less. 2 More than 2.9g / m 2 The point is as follows.

[0020] Due to these characteristics, a silicon imparting process P1 is provided in which a mixture of binder resin and silicon-based microparticles is imparted to pile fabric 1, in which flame-retardant fibers are used for pile 2 and non-flame-retardant fibers are used for base fabric 3, and then pile fabric 1 is dried to provide silicon exposed portions 4 in which the silicon-based microparticles adhered to the fiber surface via the binder resin are exposed. Unlike Patent Document 1, this makes it possible to suppress adsorption of dry dirt such as blackening (black carbon) and soil onto the fiber surface. In addition, after the silicon imparting step P1, a fluorine-based water- and oil-repellent agent is applied to the pile fabric 1 to provide a fluorine-coated portion 5 in which the silicon-based fine particles adhered to the fiber surface via the binder resin are coated with the fluorine-based water- and oil-repellent agent. As a result, unlike Patent Document 2, the pile fabric 1 can be endowed with water- and oil-repellent properties, and the stain resistance against wet stains such as water-based stains and oil-based stains is improved. The manufacturing method for the pile fabric 1 can also be said to be a "manufacturing method for a pile fabric having stain-resistant properties." The method for producing the pile fabric 1 may further include a silicon / flame retardant imparting step P1' in which a mixture of a binder resin, silicon-based fine particles and a flame retardant is imparted to the pile fabric 1 in which a non-flame retardant fiber is used for the pile 2 and the base fabric 3, and then the pile fabric 1 is dried to provide silicon exposed portions 4 and flame retardant exposed portions 4' on the fiber surface of the non-flame retardant fiber, where the silicon-based fine particles and the flame retardant adhered to the fiber surface via the binder resin are exposed; and a fluorine coating step P2' in which, after the silicon / flame retardant imparting step P1', a fluorine-based water / oil repellent is imparted to the pile fabric 1 to provide fluorine-coated portions 5, 5' in which the silicon-based fine particles and the flame retardant adhered to the fiber surface via the binder resin are covered by the fluorine-based water / oil repellent.

[0021] Furthermore, the application of the mixture in the silicon application step P1 or the silicon / flame retardant application step P1' is carried out in an atmosphere at a predetermined temperature, and the application of the mixture in the fluorine coating steps P2 and P2' is carried out in an atmosphere at a temperature higher than the predetermined temperature, thereby promoting the orientation of fluorine in the fluorine-based water- and oil-repellent agent in the fluorine coating steps P2 and P2' and improving soil resistance. In addition, after the fluorine coating steps P2 and P2', the backcoat step P3 is provided in which a backcoat part 10 is provided on the back surface of the base fabric 3 with a mixture of at least a urethane resin and a flame retardant in an atmosphere at a temperature higher than the predetermined temperature in the silicon attachment step P1 or the silicon / flame retardant attachment step P1' and the fluorine coating steps P2 and P2'. This promotes the orientation of fluorine in the fluorine-based water / oil repellent in the backcoat step P3, improving the water / oil repellency. At the same time, the steps up to the fluorine coating steps P2 and P2' are performed at a temperature lower than the temperature in the backcoat step P3, and since the fluorine is not yet oriented to a large extent in the backcoat step P3, it becomes possible to coat the back surface of the base fabric 3 with a sufficient amount of a mixture of a urethane resin, a flame retardant, etc. At the same time, the pile 2 is prevented from coming off the base fabric 3, and the flame retardancy of the pile fabric 1 is also improved. In addition, the amount of silicon-based fine particles added was 0.8 g / m 2 More than 4.5g / m 2 The amount of binder resin applied is 0.3 g / m or less. 2 More than 1.7g / m 2 The amount of fluorine-based water and oil repellent applied is 0.5 g / m 2 More than 2.9g / m 2 The following is also acceptable. Effect of the Invention

[0022] The pile fabric and the manufacturing method of the pile fabric according to the present invention can achieve "improved stain resistance against both dry and wet stains" by providing silicon-exposed sections in which silicon-based microparticles are exposed on the fiber surface of the pile fabric and fluorine-coated sections in which the silicon-based microparticles are coated with a fluorine-based water- and oil-repellent agent. [Brief description of the drawings]

[0023] [Figure 1] 1 is a schematic diagram showing a cross section of a pile fabric according to a first embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic diagram showing a cross section of a pile fabric according to a second embodiment of the present invention. [Diagram 3] 1 shows a cross section of Example 1 of the pile fabric according to the present invention, where (a) is a photograph substituted for a drawing, (b) is an image showing the position of only silicon in Example 1 with dots, (c) is an image showing the position of only fluorine in Example 1 with dots, and (d) is a superimposed image showing the positions of both silicon and fluorine in Example 1 with dots. [Figure 4] 1 shows a cross section of Example 2 of the pile fabric according to the present invention, where (a) is a photograph substituted for a drawing, (b) is an image showing the position of only silicon in Example 2 as dots, (c) is an image showing the position of only fluorine in Example 2 as dots, and (d) is a superimposed image showing the positions of both silicon and fluorine in Example 2 as dots. [Diagram 5] 1 shows a cross section of Reference Example 1 of the pile fabric according to the present invention, where (a) is a photograph substituted for a drawing, (b) is an image showing the position of only silicon in Reference Example 1 with dots, (c) is an image showing the position of only fluorine in Reference Example 1 with dots, and (d) is a superimposed image showing the positions of both silicon and fluorine in Reference Example 1 with dots. [Figure 6] FIG. 1 is a flowchart showing a method for manufacturing a pile fabric according to the present invention, in which (a) shows a first embodiment, (b) shows a second embodiment, (c) shows a third embodiment, and (d) shows a fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] <Overall structure of pile fabric 1> Hereinafter, an embodiment of the present invention will be described with reference to the drawings. 1 to 5 show a pile fabric 1 according to the present invention, and this pile fabric 1 has pile 2 and a base fabric 3 which will be described later. The pile fabric 1 may have a back coat portion 10 which will be described later. The "surface (fabric surface) 1a" of such pile fabric 1 can also be said to be the surface that is exposed when used as an interior material for railway cars or the like, or as a seat cover for covering seats (chairs). Conversely, the "reverse side (reverse side of fabric) 1b" of the pile fabric 1 can also be said to be the side that is not exposed when the fabric is used as an interior material, seat, or the like for a railway vehicle or the like.

[0025] The pile fabric 1 may have any configuration as long as the pile 2 is erected from the base fabric 3, and may be, for example, a pile woven fabric having warp threads and weft threads, a pile knitted fabric having only warp threads or only weft threads, or a tufted pile fabric in which the pile 2 is tufted into the base fabric 3. In particular, when the pile fabric 1 is a woven pile fabric, any configuration may be used, but for example, the pile 2 may be formed by weaving warp and weft threads in a plain weave, twill weave, satin weave, or the like as the base fabric 3, and weaving pile threads in the warp or weft direction together with this base fabric 3. In addition, a pile fabric in which pile yarns are woven in the warp direction is also called a warp pile fabric, and a pile fabric in which pile yarns are woven in the weft direction is also called a weft pile fabric. Even when the pile fabric 1 is a pile knitted fabric, any configuration is acceptable, but it may be, for example, pile knitted with a weft yarn (a type of weft knit that is a variation of a flat knit, also called pile nap knit or plush knit). In this pile knit, a pile yarn is affixed to the weft yarn, which is the ground yarn, and the sinker loop of this pile yarn is expanded to form the pile 2, and the flat knit fabric knitted with the ground weft yarn becomes the base fabric 3.

[0026] The basis weight of the pile fabric 1 is not particularly limited, but is, for example, 300 g / m 2 More than 900g / m 2 Less than 400 g / m 2 More than 800g / m 2 More preferably, 500 g / m or less 2 More than 700g / m 2 In the present invention, the basis weight, adhesion amount, and application amount (g / m 2 ) means values ​​by dry weight. The pile fabric 1 may have any thickness, for example, from 1 mm to 100 mm, preferably from 1 mm to 50 mm, and more preferably from 2 mm to 40 mm. In addition, the density of the yarns used in the pile fabric 1 may be any value. However, when the pile fabric 1 is the above-mentioned warp pile fabric, the density of the pile yarns (pile 2) woven in the warp direction in the pile fabric 1 may be, for example, 50 yarns / 10 cm or more and 260 yarns / 10 cm or less, preferably 60 yarns / 10 cm or more and 240 yarns / 10 cm or less, and more preferably 70 yarns / 10 cm or more and 220 yarns / 10 cm or less (80 yarns / 10 cm, 90 yarns / 10 cm, 100 yarns / 10 cm, etc.). Furthermore, when the pile fabric 1 is a woven pile fabric, the density of the weft yarns forming the base fabric 3 may be, for example, 100 yarns / 10 cm or more and 260 yarns / 10 cm or less, preferably 120 yarns / 10 cm or more and 240 yarns / 10 cm or less, and more preferably 140 yarns / 10 cm or more and 220 yarns / 10 cm or less (160 yarns / 10 cm, 180 yarns / 10 cm, 200 yarns / 10 cm, etc.). Hereinafter, the pile fabric 1 will be described as being mainly a pile fabric (moquette) 1.

[0027] <First and second embodiments of pile fabric 1> In a first embodiment of the pile fabric 1, a flame-retardant fiber S is used for the pile 2 described later, and a non-flame-retardant fiber S' is used for the base fabric 3 described later, and the fiber surfaces Sa, Sa' of the flame-retardant fiber S and the non-flame-retardant fiber S' have silicon exposed portions 4 and fluorine-coated portions (silicon-coated portions with fluorine) 5 described later (see FIG. 1). In a second embodiment of the pile fabric 1, a non-flame retardant fiber S' is used for both the pile 2 and base fabric 3 described below, and the fiber surface Sa' of the non-flame retardant fiber S' has not only a silicon exposed portion 4 and a fluorine coated portion (a silicon coated portion made of fluorine) 5 described below, but also a flame retardant exposed portion 4' and a fluorine coated portion (a flame retardant coated portion made of fluorine) 5' (see FIG. 2).

[0028] <Pile 2, Base Fabric 3> As shown in FIGS. 1 to 5, the pile 2 is formed from pile yarn or the like as described above, and stands upright from the base fabric 3. The pile 2 may be either a cut pile in which the tip is cut to make it fluffy, or a loop pile in which adjacent piles 2 form loops. In what follows, pile 2 will be described as being cut pile. The pile length of the pile 2 is not particularly limited, but may be, for example, 0.5 mm or more and 10.0 mm or less, preferably 1.0 mm or more and 8.0 mm or less, and more preferably 2.0 mm or more and 6.0 mm or less. The pile height means the height from the surface of the base fabric 3 of the pile fabric 1 to the tip of the pile 2, and in more detail, when the pile 2 is erected (standing upright) at approximately a right angle (approximately 90°) to the base fabric 3 (the angle θ between the pile 2 and the base fabric 3 is approximately 90°), it can be said to be approximately equal to the pile length of the pile 2. Furthermore, when the pile 2 is erected obliquely relative to the base 3 (the angle θ between the pile 2 and the base 3 is less than 90° (for example, 80°, 70°, 60°, 45°, etc.)), the pile height is approximately equal to the pile length x sinθ. Such pile height is not particularly limited, but may be, for example, 0.5 mm or more and 10.0 mm or less, preferably 1.0 mm or more and 8.0 mm or less, and more preferably 2.0 mm or more and 6.0 mm or less.

[0029] On the other hand, as described above, the base fabric 3 is a woven fabric, knitted fabric, or the like, made of warp threads and weft threads, and is in a sheet shape. Here, the "surface (base surface) 3a" of the base fabric 3 can be said to be the surface close to the surface 1a that is exposed when the pile fabric 1 is used to cover the interior fittings of railway vehicles, etc., and the pile 2 is provided on this surface. Conversely, the "reverse side (reverse side of the base fabric) 3b" of the base fabric 3 can also be said to be a surface close to the reverse side 1b that is not exposed when the pile fabric 1 is used to cover the interior fittings of railway vehicles, etc. (if the pile fabric 1 does not have a backcoat portion 10, it is, so to speak, the reverse side 1b of the pile fabric 1 itself). The thickness of the base fabric 3 may also be any value, for example, 0.1 mm or more and 2.0 mm or less, preferably 0.20 mm or more and 1.5 mm or less, and more preferably 0.5 mm or more and 1.0 mm or less.

[0030] <Flame-retardant fiber S, non-flame-retardant fiber S'> The fibers used in the pile 2 and base fabric 3 described so far are, as described above, flame-retardant fiber S or non-flame-retardant fiber S'. The flame-retardant fiber S is, for example, a fiber containing a flame retardant. The flame retardant in the flame-retardant fiber S is a non-halogen-based flame retardant or a phosphorus-based flame retardant kneaded into a material such as a polyester resin described later, a phosphorus-based flame retardant copolymerized with a polyester resin, or a flame retardant described later that is kneaded in or otherwise incorporated therein. On the other hand, the non-flame retardant fiber S' is a fiber that does not contain a flame retardant. In the present invention, the term "fiber" refers to polyethylene terephthalate (PET) fiber, which is a thermoplastic fiber; or fibers having an ester bond, such as polytrimethylene terephthalate (PTT) fiber or polybutylene terephthalate (PBT) fiber; or synthetic fibers, such as nylon (polyamide) fiber, polyolefin fibers such as polyethylene (PE) or polypropylene (PP), rayon fiber, cupra fiber, acetate fiber, acrylic fiber mainly composed of polyacrylonitrile (PAN), polyvinyl alcohol (PVA) fiber (vinylon fiber), or polyurethane (PU) fiber; or glass fiber, wool, silk, or the like, which may be used alone or in combination. The yarns of the pile 2 or base fabric 3 using these fibers may be multifilament yarns, monofilament yarns, or spun yarns.

[0031] In the present invention, "the pile 2 uses a flame-retardant fiber S", "the base fabric 3 uses a non-flame-retardant fiber S'", and "the pile 2 and the base fabric 3 use a non-flame-retardant fiber S'" include not only cases in which the pile 2 or the base fabric 3 has only one flame-retardant fiber S or one non-flame-retardant fiber S', but also cases in which the pile 2 or the base fabric 3 has a plurality of flame-retardant fibers S or one non-flame-retardant fiber S'. Furthermore, the fineness of the fibers constituting the pile 2 and the base fabric 3 may be any value, but may be, for example, a total fineness of 20 dtex or more and 3000 dtex or less. When the fibers constituting the pile 2 and the base fabric 3 are multifilament, the single fiber fineness of each filament is not particularly limited, but may be, for example, 0.1 dtex or more and 50.0 dtex or less.

[0032] <Silicon exposed part 4> As shown in Figures 1 to 5, when the pile fabric 1 is the first embodiment, the silicon-exposed portion 4 is a portion on the fiber surfaces Sa, Sa' of the above-mentioned flame-retardant fiber S and non-flame-retardant fiber S' where the silicon-based microparticles K adhered to the fiber surfaces Sa, Sa' via the binder resin B are exposed, and when the pile fabric 1 is the second embodiment, it is a portion on the fiber surface Sa' of the above-mentioned non-flame-retardant fiber S' where the silicon-based microparticles K adhered to the fiber surface Sa' via the binder resin B are exposed. In the present invention, "on the fiber surfaces Sa, Sa', silicon-based microparticles K adhered to the fiber surfaces Sa, Sa' via the binder resin B are exposed" means that silicon-based microparticles K are adhered to each of the fiber surface Sa of the flame-retardant fiber S and the fiber surface Sa' of the non-flame-retardant fiber S' via the binder resin B, and the silicon surfaces of these silicon-based microparticles K are not covered with the fluorine-based water- and oil-repellent agent F described below. In Figures 3 to 5(d), where the positions of silicon and fluorine are superimposed, the positions where only silicon is present (the positions of silicon that are not overlapped with fluorine) are represented by white dots. The silicon exposed portions 4 described above may be scattered on the fiber surfaces Sa, Sa' of the fibers S, S' used in the pile 2 and base fabric 3 of the pile fabric 1, or may be island portions in the form of sea-islands (see Figures 3(b) and (d)).

[0033] <Silicon-based fine particles K> Here, the silicon-based fine particles K may be fine particles containing silicon (Si) in the form of silicon dioxide (SiO2) such as silica (also called silicic anhydride, silicic acid, or silicon oxide) such as quartz, glass, silica sand, or silica stone, or may be a compound having a siloxane bond (-Si-O-Si-) such as silicone. When the silicon-based fine particles K adhere to the fiber surfaces Sa, Sa' of the fibers S, S' used in the pile 2 and base fabric 3 of the pile fabric 1, they penetrate into gaps and recesses in the fiber surfaces Sa, Sa' or cover the fiber surfaces Sa, Sa', thereby preventing dry dirt such as blackening (black carbon) or soil from adhering to the fiber surfaces Sa, Sa', or, even if such dry dirt does adhere, they can be easily removed from the fiber surfaces Sa, Sa'. The average particle size of the silicon-based fine particles K may be 0.01 μm or more and 2.00 μm or less, preferably 0.05 μm or more and 1.50 μm or less, and more preferably 0.10 μm or more and 1.00 μm or less. The amount of silicon-based fine particles K attached is not particularly limited, but is, for example, 0.8 g / m 2 More than 4.5g / m 2 or less, preferably 1.0 g / m 2 More than 4.0g / m 2 More preferably, 1.5 g / m or less 2 More than 3.5g / m 2 The following is also acceptable.

[0034] <Binder resin B> The binder resin B is not particularly limited, and may be, for example, polyethylene terephthalate (PET) resin, which is a thermoplastic resin, or other resins having ester bonds such as polytrimethylene terephthalate (PTT) resin and polybutylene terephthalate (PBT) resin, acrylic resins mainly composed of polyacrylonitrile (PAN), polyurethane (PU) resin, or other synthetic resins such as nylon (polyamide) resin, polyolefin resins such as polyethylene (PE) and polypropylene (PP), rayon resin, cupra resin, acetate resin, and polyvinyl alcohol (PVA) resin (vinylon resin), and these may be used alone or in combination. The amount of the binder resin B to be applied is not particularly limited, but is, for example, 0.3 g / m 2 More than 1.7g / m 2 or less, preferably 0.4 g / m 2 More than 1.5g / m 2 More preferably, 0.5 g / m or less 2 More than 1.3g / m 2 The following is also acceptable.

[0035] <Flame-retardant exposed part 4'> As shown in FIG. 2, the flame-retardant exposed portion 4' is a portion where the flame retardant N adhered to the fiber surface Sa' via the binder resin B is exposed on the fiber surface Sa' of the non-flame-retardant fiber S' described above only when the pile fabric 1 is of the second embodiment. In the present invention, "on the fiber surface Sa', the flame retardant N adhered to the fiber surface Sa' via the binder resin B is exposed" means that the flame retardant N is adhered to the fiber surface Sa' of the non-flame retardant fiber S' via the binder resin B, and the flame retardant surface of the flame retardant N is not covered with the fluorine-based water- and oil-repellent agent F described later.

[0036] <Flame retardant N> The flame retardant N is not particularly limited, and may be, for example, an alkyl phosphate metal salt such as aluminum trisdiethylphosphinate, aluminum trismethylethylphosphinate, or aluminum trisdiphenylphosphinate; a phosphorus-based flame retardant such as ammonium polyphosphate, a phosphate ester, or tris(1-chloro-2-propyl)phosphate; or a metal hydroxide-based flame retardant such as aluminum hydroxide or magnesium hydroxide; or a non-halogen-based flame retardant. Here, the flame retardant N may be pulverized and in a particulate form, and the average particle size may be 0.10 μm or more and 1.60 μm or less, preferably 0.20 μm or more and 1.20 μm or less, and more preferably 0.30 μm or more and 1.00 μm or less. The amount of the flame retardant N attached is not particularly limited, but for example, 0.10 g / m 2 More than 1.00g / m2 or less, preferably 0.15 g / m 2 More than 0.90g / m 2 More preferably, 0.20 g / m or less 2 More than 0.80g / m 2 The following is also acceptable. The flame-retardant exposed portions 4 ′ described above may also be scattered on the fiber surface Sa′ of the non-flame-retardant fiber S′ used in the pile 2 and base fabric 3 of the pile fabric 1 , or may be island portions in the form of sea islands.

[0037] <Fluorine-coated part (fluorine-coated silicon part) 5> As shown in Figures 1 to 5, when the pile fabric 1 is the first embodiment, the fluorine-coated portion 5 is a portion on the fiber surfaces Sa, Sa' of the above-mentioned flame-retardant fiber S and non-flame-retardant fiber S' where the silicon-based microparticles K adhered to the fiber surfaces Sa, Sa' via the binder resin B are covered with a fluorine-based water- and oil-repellent agent F; when the pile fabric 1 is the second embodiment, the fluorine-coated portion 5 is a portion on the fiber surface Sa' of the above-mentioned non-flame-retardant fiber S' where the silicon-based microparticles K adhered to the fiber surface Sa' via the binder resin B are covered with a fluorine-based water- and oil-repellent agent F, and can be said to be a silicon-coated portion 5 made of fluorine. In the present invention, when the pile fabric 1 is the first embodiment, the phrase "on the fiber surfaces Sa, Sa', the silicon-based fine particles K adhered to the fiber surfaces Sa, Sa' via the binder resin B are coated with a fluorine-based water- and oil-repellent agent F" means that the silicon-based fine particles K are adhered to each of the fiber surface Sa of the flame-retardant fiber S and the fiber surface Sa' of the non-flame-retardant fiber S' via the binder resin B, and at least a part of the silicon surface of the silicon-based fine particles K is coated with a fluorine-based water- and oil-repellent agent F described later. In Figures 3 to 5(d), where the positions of silicon and fluorine are superimposed, the positions where silicon and fluorine overlap are represented by gray dots. In addition, in the present invention, when the pile fabric 1 is the second embodiment, the phrase "on the fiber surface Sa', the silicon-based fine particles K adhered to the fiber surface Sa' via the binder resin B are coated with a fluorine-based water- and oil-repellent agent F" means that the silicon-based fine particles K are adhered to the fiber surface Sa' of the non-flame-retardant fiber S' via the binder resin B, and at least a portion of the silicon surface of the silicon-based fine particles K is coated with the fluorine-based water- and oil-repellent agent F described later. The fluorine-coated portions (fluorine-coated silicon portions) 5 described above may be scattered on the fiber surfaces Sa, Sa' of the fibers S, S' used in the pile 2 and base fabric 3 of the pile fabric 1, or may be in the form of island portions in a sea-island pattern (see Figures 3 to 5(c) and (d)).

[0038] <Fluorine-based water and oil repellent F> Fluorine-based water and oil repellent F is, for example, a perfluoroalkyl group with 6 or less carbon atoms (e.g., 6 or 4 carbon atoms) (CF3-(CF2) n The resin may be a fluorocarbon resin composition having a perfluoroalkyl group, such as a resin having a side chain of a fluorocarbon alkyl group (n is a positive integer, in which all hydrogen atoms in the alkyl chain are replaced with fluorine atoms) and a main chain which is a copolymer of acrylate (acrylic acid ester) and methyl methacrylate (methyl methacrylate, MMA) or a polymer of methyl methacrylate (methyl methacrylate, MMA) (polymethyl methacrylate (PMMA)), or other known fluorine-based water and oil repellents, or a combination of these. The amount of the fluorine-based water- and oil-repellent agent F to be applied is not particularly limited, but may be, for example, 0.5 g / m 2 More than 2.9g / m 2 or less, preferably 0.6 g / m 2 More than 2.6g / m 2 More preferably, 0.8 g / m or less 2 More than 2.4g / m 2 The following is also acceptable. In the present invention, the "amount of fluorine-based water- and oil-repellent agent F adhered" means the amount of fluorine-based water- and oil-repellent agent F, etc., covering the silicon-based microparticles K adhered to the fiber surfaces Sa, Sa' via the binder resin B. Furthermore, the adhesion between the silicon-based microparticles K and the fluorine-based water- and oil-repellent agent F may be achieved by any means, but for example, the main chain of the fluorine-based water- and oil-repellent agent F may be entangled with the silicon-based microparticles K and adhered thereto, or the silicon-based microparticles K and the fluorine-based water- and oil-repellent agent F may be adhered thereto via a specified binder resin.

[0039] <Fluorine-coated part (fluorine-based flame-retardant coating part) 5'> As shown in FIG. 2, the fluorine-coated portion 5′ is a portion where the flame retardant N adhered to the fiber surface Sa′ of the non-flame-retardant fiber S′ via the binder resin B is coated with the fluorine-based water- and oil-repellent agent F only when the pile fabric 1 is of the second embodiment, and can be said to be a fluorine-based flame-retardant coating portion 5′. In the present invention, the phrase "on the fiber surface Sa', the flame retardant N adhered to the fiber surface Sa' via the binder resin B is coated with a fluorine-based water- and oil-repellent agent F" means that the flame retardant N is adhered to the fiber surface Sa' of the non-flame-retardant fiber S' via the binder resin B, and at least a portion of the flame-retardant surface of the flame retardant N is coated with the fluorine-based water- and oil-repellent agent F described later. The meaning and value of the amount of fluorine-based water- and oil-repellent agent F adhered to the fluorine-based flame-retardant coating portion 5', and the adhesion between the flame retardant N and the fluorine-based water- and oil-repellent agent F, are the same as those of the amount of fluorine-based water- and oil-repellent agent F adhered to the fluorine-based silicon coating portion 5. The fluorine-coated portion (fluorine-based flame-retardant coating portion) 5' described above may also be scattered on the fiber surface Sa' of the non-flame-retardant fiber S' used in the pile 2 and base fabric 3 of the pile fabric 1, or may be in the form of sea-island-like island portions.

[0040] <Exposed fiber part 6> As shown in Figures 1 to 5, when the pile fabric 1 is of the first embodiment, the fiber exposed portion 6 is the portion where the fiber surfaces Sa, Sa' of the above-mentioned flame-retardant fiber S and non-flame-retardant fiber S' are exposed, and when the pile fabric 1 is of the second embodiment, it is the portion where the fiber surface Sa' of the above-mentioned non-flame-retardant fiber S' is exposed. In the present invention, when the pile fabric 1 is the first embodiment, "the fiber surfaces Sa, Sa' are exposed" means that at least a portion of each of the fiber surface Sa of the flame-retardant fiber S and the fiber surface Sa' of the non-flame-retardant fiber S' is not covered with the above-mentioned silicon-based fine particles K, flame retardant N, fluorine-based water- and oil-repellent agent F, etc., and in Figures 3 to 5(d), where the positions of silicon and fluorine are superimposed, a position where neither silicon nor fluorine is present is represented by the absence of any dots (white dots, gray dots, black dots). In addition, in the present invention, when the pile fabric 1 is the second embodiment, "the fiber surface Sa' is exposed" means that at least a part of the fiber surface Sa' of the non-flame retardant fiber S' is not covered with the above-mentioned silicon-based microparticles K, flame retardant N, fluorine-based water- and oil-repellent agent F, etc.

[0041] <Backcourt Division 10> As shown in Figures 1 to 5, the backcoat portion 10 is a portion in which the back surface 3b of the above-mentioned base fabric 3 is coated with a mixture of at least a urethane-based resin and the above-mentioned flame retardant N, and may be in the form of a layer of a predetermined thickness. The mixture in the coating section 10 may contain only the crosslinking agent, or may contain both the crosslinking agent and the penetrating agent, in addition to the urethane resin and flame retardant N described above. It may also contain the binder resin B described above, a thickener (e.g., hydroxyethyl cellulose (HEC)), a filler, etc. The proportions of each material mentioned so far (mass % of each material in the mixture of the backcoat portion 10, dry weight) are not particularly limited, but for example, the urethane resin may be 40% or more and 50% or less, the flame retardant N may be 50% or more and 60% or less, the crosslinking agent may be 1% or more and 5% or less, and the penetrating agent may be 1% or more and 5% or less. The amount of the mixture applied to the backcoat portion 10 is not particularly limited, but may be, for example, 70 g / m 2 More than 140g / m 2 or less, preferably 75 g / m 2 More than 130g / m2 More preferably 80 g / m 2 More than 120g / m 2 It may be the following. The thickness of the backcoat portion 10 is not particularly limited, but may be, for example, 0.1 mm or more and 10.0 mm or less, preferably 0.5 mm or more and 5.0 mm or less, and more preferably 1.0 mm or more and 3.0 mm or less.

[0042] <Urethane resin> The urethane resin is a polymer having a urethane bond (-NH·CO·O-) in the repeating unit of the main chain, and is synthesized by polyaddition of a glycol (diol, etc.) having two or more hydroxyl groups and a diisocyanate having two isocyanate groups, and is also called a polyurethane (PU) resin. The urethane resin may have an ester bond (-COO-) or an ether bond (-O-), or may have a functional group such as a carboxy group, an amino group, or a blocked isocyanate group in combination, or may be made into a urethane foam (foamed polyurethane) by adding a foaming agent. In the back coat portion 10, the urethane resin may be, so to speak, a binder, and a mixture of the above-mentioned flame retardant N, etc. may be attached to the back surface 3b of the base fabric 3. The amount of the urethane resin attached to the backcoat portion 10 is not particularly limited, but is, for example, 20 g / m 2 More than 100g / m 2 Less than 30 g / m 2 More than 80g / m 2 More preferably, 40 g / m 2 More than 60g / m 2 It may be the following. The amount of the flame retardant N attached to the backcoat portion 10 is not particularly limited, but is, for example, 30 g / m 2 More than 110g / m 2 Less than 40 g / m 2 More than 90g / m 2 More preferably, 50 g / m 2 More than 70g / m 2 It may be the following.

[0043] <Crosslinking agent> The crosslinking agent is not particularly limited, and may be, for example, a blocked isocyanate crosslinking agent or a carbodiimide crosslinking agent, or may be a polyhydric alcohol such as glycerin, 1,4-butanediol, or diethylene glycol, or an amine such as ethanolamine or polyethylene polyamine, or a small amount of propylene oxide added thereto. It should be noted that the blocked isocyanate crosslinking agent is stable at room temperature and hardens when heated, while the carbodiimide crosslinking agent can crosslink at low temperatures. The amount of the crosslinking agent applied to the backcoat portion 10 is not particularly limited, but may be, for example, 0.1 g / m 2 More than 6.0g / m 2 Less than 1.0 g / m 2 More than 5.0g / m 2 More preferably, 2.0 g / m or less 2 More than 4.0g / m 2 It may be the following.

[0044] <Penetrating agent> The penetrating agent is not particularly limited, and may be, for example, polyoxyalkylene alkyl ether, dialkyl sulfosuccinate salt, or other suitable agents such as alkylnaphthalenesulfonate sodium, alkylbenzenesulfonate sodium, alkyl allyl ether, diethanolamine, alkylnaphthalenesulfonate sodium, alkyl sulfate, metal soap, aliphatic amine, etc. The penetrating agent reduces the contact angle between the back surface 3b of the base fabric 3 and the mixture, and can be said to promote wetting and penetration in the back coating process P3 described later and the like. The method for producing the pile fabric 1 described above will now be described in detail.

[0045] <Manufacturing method of pile fabric 1> As shown in FIG. 6, the manufacturing method of the pile fabric 1 (hereinafter also referred to as "the manufacturing method") includes at least a silicon imparting step P1 or a silicon / flame retardant imparting step P1' described below, and a fluorine coating step P2, P2' described below. The manufacturing method may include a backcoating process P3, which will be described later. Here, in the manufacturing method, if it comprises a silicon imparting step P1 and a fluorine coating step (silicon coating step using fluorine) P2, it is considered to be a first embodiment; if it comprises a silicon imparting step P1, a fluorine coating step (silicon coating step using fluorine) P2, and a backcoat step P3, it is considered to be a second embodiment; if it comprises a silicon / flame retardant imparting step P1' and a fluorine coating step (silicon / flame retardant coating step using fluorine) P2', it is considered to be a third embodiment; and if it comprises a silicon / flame retardant imparting step P1', a fluorine coating step (silicon / flame retardant coating step using fluorine) P2', and a backcoat step P3, it is considered to be a fourth embodiment. In addition, the manufacturing method of the first embodiment including steps P1 and P2 and the third embodiment including steps P1' and P2' can be considered to be a two-stage process, and the second embodiment including steps P1, P2, and P3 and the fourth embodiment including steps P1', P2', and P3 can be considered to be a three-stage process. Additionally, the first to fourth embodiments of the manufacturing method may include a pile fabric forming step, which will be described later, before the silicon imparting step P1 or the silicon / flame retardant imparting step P1'.

[0046] <Silicon imparting process P1> As shown in FIG. 6, the silicon imparting step P1 is a step of imparting a mixture of at least the binder resin B and the silicon-based microparticles K to the pile fabric 1 described above, and then drying the pile fabric 1 to provide silicon exposed portions 4 on the fiber surfaces Sa, Sa' of the flame-retardant fiber S and the non-flame-retardant fiber S' described above, where the silicon-based microparticles K adhered to the fiber surfaces Sa, Sa' via the binder resin B are exposed. The application of the mixture in the silicon application step P1 may be performed under an atmosphere of a predetermined temperature. The "predetermined temperature" for applying the mixture in the silicon application step P1 may be, for example, 120°C or higher and 140°C or lower (or 120°C or higher and lower than 140°C), and may preferably be 125°C or higher and 135°C or lower.

[0047] Here, the means of "adding" in the silicon addition step P1 is not particularly limited, and may be, for example, a padding method (dip-nip method), a dipping method, a spraying method, a kiss roll method, a foam processing method, a coating method, a dropping method, or a printing method. Taking the padding method as an example among the above methods, the padding method involves immersing a pile fabric 1 made of flame-retardant fibers S and non-flame-retardant fibers S' in a dispersion liquid in which a powdery mixture is dispersed in a dispersion medium such as water at a predetermined concentration, or in a solution in which the powdery mixture is dissolved in a solvent such as water, and then squeezing the immersed pile fabric 1 through a pair of mangles (padding rolls). Note that, as long as the mixture can be applied to the pile fabric 1, it is not necessary to first make the mixture in a powder form and then disperse it in a dispersion medium such as water. Also, the means for "applying" the mixture does not have to be the padding method of squeezing with a mangle, and may be an immersion method in which the pile fabric 1 is simply immersed in a solution in which the mixture is dissolved. Here, when dispersing the mixture in a dispersion medium by padding or immersion in the silicon-imparting process P1, the concentration of the mixture of binder resin B and silicon-based microparticles K ((weight of mixture / (weight of dispersion liquid containing mixture and dispersion medium or solution containing solvent)) x 100) may be any value, for example, 0.1% by weight or more and 12.0% by weight or less, preferably 1.0% by weight or more and 10.0% by weight or less, or 2.0% by weight or more and 8.0% by weight or less. In this case, the concentration of only the binder resin B ((weight of binder resin B / (weight of the mixture and the dispersion liquid including the dispersion medium or the solution including the solvent))×100) may be any value, for example, 0.1% by weight or more and 5.0% by weight or less, preferably 0.5% by weight or more and 4.0% by weight or less, or 1.0% by weight or more and 3.0% by weight or less. In this case, the concentration of only the silicon-based microparticles K ((weight of silicon-based microparticles K / (weight of the dispersion of the mixture and the dispersion medium or the solution of the solvent)) x 100) may be any value, but may be, for example, 0.1% by weight or more and 7.0% by weight or less, preferably 0.5% by weight or more and 6.0% by weight or less, or 1.0% by weight or more and 5.0% by weight or less. Furthermore, in the silicon providing step P1, a colloidal solution in which silicon-based fine particles K are dispersed in water using water as a dispersion medium can be used as such colloidal silica.

[0048] Additionally, the means for "drying" in the silicon imparting step P1 is not particularly limited, and for example, the pile fabric 1 may be stretched using a pin tenter and then dried in a dryer at a predetermined drying temperature for a predetermined drying time. The drying temperature is not particularly limited, but may be, for example, 100°C or higher and 200°C or lower, and preferably 120°C or higher and 180°C or lower. The drying time is not particularly limited, but may be, for example, from 0.1 minutes (6 seconds) to 360.0 minutes, preferably from 0.2 minutes (12 seconds) to 10.0 minutes, and more preferably from 0.3 minutes (18 seconds) to 5.0 minutes. Alternatively, the "drying" means in the silicon providing step P1 may be natural drying, blowing air drying (air drying), etc. Even when the "drying" means in the silicon providing step P1 is natural drying, etc., the drying temperature is not particularly limited, and may be, for example, room temperature (about 20°C, etc.), and the drying time may be until moisture evaporates from the pile fabric 1 (for example, 24 hours, etc.).

[0049] The amount of silicon-based fine particles K applied in the silicon application step P1 (in other words, the amount of silicon-based fine particles K attached after drying in the silicon application step P1) is not particularly limited, but is, for example, 0.8 g / m 2 More than 4.5g / m 2 or less, preferably 1.0 g / m 2 More than 4.0g / m 2 More preferably, 1.5 g / m or less 2 More than 3.5g / m 2 The following is also acceptable. The amount of binder resin B applied in the silicon application step P1 (in other words, the amount of binder resin B adhered after drying in the silicon application step P1 (after the silicon application step P1)) is not particularly limited, but may be, for example, 0.3 g / m 2 More than 1.7g / m 2or less, preferably 0.4 g / m 2 More than 1.5g / m 2 More preferably, 0.5 g / m or less 2 More than 1.3g / m 2 The following is also acceptable. Furthermore, the amount (adhesion) of silicon-based microparticles K applied after drying in the silicon application process P1 can also be said to be the sum of the amount (adhesion) of silicon-based microparticles K applied in the silicon-exposed portion 4 described above and the amount (adhesion) of silicon-based microparticles K applied in the fluorine-coated portion (silicon-coated portion by fluorine) 5 described above.

[0050] <Silicon / Flame Retardant Addition Process P1'> As shown in FIG. 6, the silicon / flame retardant imparting process P1' is a process in which a mixture of at least binder resin B, silicon-based microparticles K and flame retardant N is applied to the above-mentioned pile fabric 1, and then the pile fabric 1 is dried to provide, on the fiber surface Sa' of the non-flame retardant fiber S', silicon exposed portions 4 where the silicon-based microparticles K attached to the fiber surface Sa' via the binder resin B are exposed, and flame retardant exposed portions 4' where the flame retardant N attached to the fiber surface Sa' via the binder resin B is exposed. The application of the mixture in the silicon / flame retardant application step P1' may be performed in an atmosphere at a predetermined temperature. The "predetermined temperature" for applying the mixture in the silicon / flame retardant application step P1' may be, for example, 120°C or higher and 140°C or lower (or 120°C or higher and lower than 140°C), and preferably 125°C or higher and 135°C or lower.

[0051] Here, the means for "imparting" in the silicon / flame retardant imparting step P1' is not particularly limited, but may be the same as the means for "imparting" in the silicon imparting step P1, such as the padding method described above. When dispersing the mixture in a dispersion medium by a padding method or the like in the silicon / flame retardant imparting process P1', the concentration of the mixture of binder resin B, silicon-based microparticles K and flame retardant N may be any value, for example, 0.1 wt % or more and 13.0 wt % or less, preferably 1.0 wt % or more and 11.0 wt % or less, or 2.0 wt % or more and 9.0 wt % or less. In this case, the concentration of only the binder resin B, the numerical range of the concentration of only the silicon-based fine particles K, and the colloidal silica may be the same as those in the silicon providing step P1. In this case, the concentration of only the flame retardant N ((weight of flame retardant N / (weight of the dispersion of the mixture and the dispersion medium or the solution of the solvent)) × 100) may be any value, but may be, for example, 0.1% by weight or more and 3.0% by weight or less, preferably 0.2% by weight or more and 2.0% by weight or less, or 0.3% by weight or more and 1.0% by weight or less. In addition, the "drying" means, drying temperature, drying time, etc. in the silicon / flame retardant imparting process P1' are not particularly limited, but may be the same as the "drying" means, drying temperature, drying time, etc. in the silicon imparting process P1 described above.

[0052] The amount of binder resin B and silicon-based microparticles K applied in the silicon / flame retardant application process P1' (in other words, the amount of binder resin B and silicon-based microparticles K adhered after drying in the silicon / flame retardant application process P1' (after the silicon / flame retardant application process P1')) is not particularly limited, but may be similar to the amount of binder resin B and silicon-based microparticles K adhered after drying in the silicon application process P1 described above. The amount of the flame retardant N applied in the silicon / flame retardant application step P1' (in other words, the amount of the flame retardant N attached after drying in the silicon / flame retardant application step P1' (after the silicon / flame retardant application step P1')) is not particularly limited, but may be, for example, 0.10 g / m 2 More than 1.00g / m 2 or less, preferably 0.15 g / m 2 More than 0.90g / m 2 More preferably, 0.20 g / m or less 2 More than 0.80g / m 2 The following is also acceptable. Furthermore, the amount of silicon-based microparticles K adhered after drying in the silicon / flame retardant imparting process P1' can also be said to be the sum of the amount of silicon-based microparticles K adhered in the above-mentioned silicon exposed portion 4 and the amount of silicon-based microparticles K adhered in the above-mentioned fluorine-coated portion (fluorine-coated silicon portion) 5, and the amount of flame retardant N adhered after drying in the silicon / flame retardant imparting process P1' can also be said to be the sum of the amount of flame retardant N adhered in the above-mentioned flame retardant exposed portion 4' and the amount of flame retardant N adhered in the above-mentioned fluorine-coated portion (fluorine-coated flame retardant portion) 5'.

[0053] <Fluorine coating process (silicon coating process with fluorine) P2> As shown in FIG. 6, the fluorine coating step (silicon coating step with fluorine) P2 is a step that follows the silicon imparting step P1 described above, in which a fluorine-based water / oil repellent agent F is applied to the pile fabric 1 described above to provide fluorine-coated portions (silicon-coated portions with fluorine) 5 on fiber surfaces Sa, Sa' of the flame-retardant fiber S and the non-flame-retardant fiber S' in which at least a portion of the silicon surface of the silicon-based microparticles K adhered to the fiber surfaces Sa, Sa' via the binder resin B is covered with the fluorine-based water / oil repellent agent F. The application of the mixture in this fluorine coating step (silicon coating step with fluorine) P2 may be carried out in an atmosphere at a temperature higher than the above-mentioned predetermined temperature if the manufacturing method is the first embodiment, or may be carried out at the above-mentioned predetermined temperature if the manufacturing method is the second embodiment. Furthermore, the "predetermined temperature" for applying the mixture in the fluorine coating process (fluorine-based silicon coating process) P2 may be, for example, 120°C or higher and 140°C or lower (or 120°C or higher and lower than 140°C), and preferably 125°C or higher and 135°C or lower. Furthermore, the "temperature higher than the predetermined temperature" at which the mixture is applied in the fluorine coating step (fluorine-based silicon coating step) P2 may be, for example, 140°C or higher and 160°C or lower, and preferably 145°C or higher and 155°C or lower.

[0054] Here, the means for "imparting" in the fluorine coating step (silicon coating step with fluorine) P2 is not particularly limited, but may be the same as the means for "imparting" in the silicon imparting step P1, such as the padding method (immersion method) described above. When the fluorine-based water- and oil-repellent agent F is dispersed in a dispersion medium by a padding method or the like in the fluorine coating process (fluorine-based silicon coating process) P2, the concentration of the fluorine-based water- and oil-repellent agent F may be any value, for example, from 0.1% by weight to 7.0% by weight, preferably from 0.5% by weight to 6.0% by weight, or from 1.0% by weight to 5.0% by weight. In the fluorine coating step (silicon coating step using fluorine) P2, the pile fabric 1 may be dried after the fluorine-based water / oil repellent agent F is applied. The "drying" means, drying temperature, drying time, etc. in this case are not particularly limited, and may be the same as the "drying" means, drying temperature, drying time, etc. in the silicon application step P1 described above.

[0055] The amount of the fluorine-based water- and oil-repellent agent F applied after the fluorine-based coating step (fluorine-based silicon coating step) P2 (i.e., the amount of the fluorine-based water- and oil-repellent agent F adhered in the fluorine-based coating step (fluorine-based silicon coating step) P2) is not particularly limited, but may be, for example, 0.5 g / m 2 More than 2.9g / m 2 or less, preferably 0.6 g / m 2 More than 2.6g / m 2 More preferably, 0.8 g / m or less 2 More than 2.4g / m 2 The following is also acceptable. In addition, the amount of fluorine-based water- and oil-repellent agent F adhered after the fluorine coating process (fluorine-based silicon coating process) P2 can also be said to be the amount of fluorine-based water- and oil-repellent agent F adhered in the above-mentioned fluorine-coated portion (fluorine-coated portion) 5.

[0056] <Fluorine coating process (fluorine-based silicon / flame-retardant coating process) P2'> As shown in FIG. 6, the fluorine coating process P2' is a process of applying a fluorine-based water / oil repellent agent F to the pile fabric 1 described above after the above-mentioned silicon / flame retardant imparting process P1' to provide, on the fiber surface Sa' of the non-flame retardant fiber S', a fluorine-coated portion (silicon-coated portion by fluorine) 5 in which at least a part of the silicon surface of the silicon-based fine particles K attached to the fiber surface Sa' via the binder resin B is covered with the fluorine-based water / oil repellent agent F, and a fluorine-coated portion (flame-retardant coated portion by fluorine) 5' in which at least a part of the flame-retardant surface of the flame retardant N attached to the fiber surface Sa' via the binder resin B is covered with the fluorine-based water / oil repellent agent F. The application of the mixture in this fluorine coating process (fluorine-based silicon / flame-retardant coating process) P2' may be carried out in an atmosphere at a temperature higher than the above-mentioned predetermined temperature if the manufacturing method is the third embodiment, and may be carried out at the above-mentioned predetermined temperature if the manufacturing method is the fourth embodiment. Furthermore, the "predetermined temperature" for applying the mixture in the fluorine coating process (fluorine-based silicon / flame-retardant coating process) P2' may be, for example, 120°C or higher and 140°C or lower (or 120°C or higher and lower than 140°C), and preferably 125°C or higher and 135°C or lower. Furthermore, the "temperature higher than the predetermined temperature" for applying the mixture in the fluorine coating process (fluorine-based silicon / flame-retardant coating process) P2' may be, for example, 140°C or higher and 160°C or lower, and preferably 145°C or higher and 155°C or lower.

[0057] Here, the means of "imparting" in the fluorine coating process (fluorine-based silicon / flame retardant coating process) P2' is not particularly limited, but may be the same as the means of "imparting" in the silicon imparting process P1, such as the padding method (immersion method) described above. When the fluorine-based water- and oil-repellent agent F is dispersed in a dispersion medium by a padding method or the like in the fluorine-based coating process (fluorine-based silicon / flame-retardant coating process) P2', the numerical range of the concentration of the fluorine-based water- and oil-repellent agent F may be the same as that in the fluorine-based coating process (fluorine-based silicon coating process) P2. In the fluorine coating step (fluorine-based silicon / flame-retardant coating step) P2', the pile fabric 1 may be dried after the fluorine-based water / oil repellent agent F is applied. The "drying" means, drying temperature, drying time, etc. in this case are not particularly limited, and may be the same as the "drying" means, drying temperature, drying time, etc. in the above-mentioned silicon application step P1.

[0058] The numerical range of the amount of fluorine-based water- and oil-repellent agent F applied after the fluorine coating process (fluorine-based silicon / flame-retardant coating process) P2' (in other words, the amount of fluorine-based water- and oil-repellent agent F adhered in the fluorine coating process (fluorine-based silicon / flame-retardant coating process) P2') may be the same as that of the fluorine coating process (fluorine-based silicon coating process) P2. In addition, the amount of fluorine-based water- and oil-repellent agent F adhered after the fluorine coating process (fluorine-based silicon / flame-retardant coating process) P2' can also be said to be the sum of the amount of fluorine-based water- and oil-repellent agent F adhered in the above-mentioned fluorine-coated portion (fluorine-based silicon-coated portion) 5 and the amount of fluorine-based water- and oil-repellent agent F adhered in the fluorine-coated portion (fluorine-based flame-retardant coating portion) 5'.

[0059] <Backcoat process P3> As shown in FIG. 6, the backcoat process P3 is a process that follows the above-mentioned fluorine coating processes (fluorine-based silicon coating process, fluorine-based silicon / flame retardant coating process) P2 and P2', in which a backcoat portion 10 is provided on the back surface 3b of the base fabric 3 in an atmosphere having a temperature higher than the above-mentioned predetermined temperature, in which a mixture of at least a urethane-based resin and a flame retardant N is coated. The "temperature higher than the predetermined temperature" for coating the mixture in this backcoat process P3 may be, for example, 140°C or higher and 160°C or lower, and preferably 145°C or higher and 155°C or lower.

[0060] Here, the means of "coating" in the backcoat process P3 is not particularly limited, but may be, for example, coating, and specific means of coating include coating with a brush or the like, spray coating, comma direct method, gravure direct method, gravure reverse method, reverse roll coating method, air knife coating method, kiss coating method, etc., or a thin film coater, roll print processing machine, inkjet print processing machine, rotor dampening, etc. may also be used. Other "coating" means may be a kiss roll method, a foam processing method, etc. Incidentally, when coating the mixture in the backcoat process P3, a dispersion obtained by dispersing the powdery mixture at a predetermined concentration in a dispersing medium such as water, or a solution obtained by dissolving the mixture in a solvent such as water, is coated by spreading or the like on the back surface 3b of the base fabric 3. In this case, the concentration of the mixture of the urethane resin, flame retardant N, penetrating agent, crosslinking agent, and thickener ((weight of the mixture / (weight of the dispersion mixture of the mixture and the dispersing medium or the solution of the solvent)) x 100) may be any value, but may be, for example, 1% by weight or more and 70% by weight or less, preferably 10% by weight or more and 65% by weight or less, or 20% by weight or more and 60% by weight or less. In this case, the concentration of the urethane resin alone ((weight of urethane resin / (weight of the mixture and the dispersion medium or the solution of the solvent)) × 100) may be any value, for example, from 1 wt % to 50 wt %, preferably from 5 wt % to 4.0 wt %, or from 10 wt % to 30 wt %. In this case, the concentration of only the flame retardant N ((weight of flame retardant N / (weight of the dispersion of the mixture and the dispersion medium or the solution of the solvent)) × 100) may be any value, but may be, for example, 1% by weight or more and 60% by weight or less, preferably 7% by weight or more and 50% by weight or less, or 15% by weight or more and 40% by weight or less. Furthermore, in this case, the concentration of the penetrant alone ((weight of penetrant / (weight of the dispersion of the mixture and the dispersion medium or the solution of the solvent)) × 100) may be any value, but may be, for example, 0.1 wt % or more and 3.0 wt % or less, preferably 0.2 wt % or more and 2.0 wt % or less, or 0.3 wt % or more and 1.0 wt % or less. In addition, the concentration of the crosslinker alone in this case ((weight of crosslinker / (weight of the dispersion of the mixture and the dispersion medium or the solution of the solvent))×100) may be any value, for example, 0.1% by weight or more and 5.0% by weight or less, preferably 0.5% by weight or more and 4.0% by weight or less, or 1.0% by weight or more and 3.0% by weight or less. In addition, the concentration of the thickener alone in this case ((weight of thickener / (weight of the mixture and the dispersion medium or the solution of the solvent)) × 100) may be any value, but may be, for example, 0.01% by weight or more and 0.30% by weight or less, preferably 0.02% by weight or more and 0.20% by weight or less, or 0.03% by weight or more and 0.10% by weight or less. In the backcoating step P3, the pile fabric 1 may be dried after coating with the mixture. The "drying" means, drying temperature, drying time, etc. in this case are not particularly limited, but may be the same as the "drying" means, drying temperature, drying time, etc. in the silicon-imparting step P1 described above.

[0061] The coating amount of the mixture in the backcoating process P3 (in other words, the amount of the mixture adhered after the backcoating process P3) is not particularly limited, but may be, for example, 70 g / m 2 More than 140g / m 2 or less, preferably 75 g / m 2 More than 130g / m 2 More preferably 80 g / m or less 2 More than 120g / m 2 It may be the following. In this case, the amount of the urethane resin applied (adhered amount) is not particularly limited, but may be, for example, 20 g / m 2 More than 100g / m 2 Less than 30 g / m 2More than 80g / m 2 More preferably, 40 g / m 2 More than 60g / m 2 It may be the following. In this case, the amount of the flame retardant N applied (attached) is not particularly limited, but may be, for example, 30 g / m 2 More than 110g / m 2 Less than 40 g / m 2 More than 90g / m 2 More preferably, 50 g / m 2 More than 70g / m 2 It may be the following. Furthermore, the amount of the crosslinking agent applied (adhered amount) in this case is not particularly limited, but may be, for example, 0.1 g / m 2 More than 6.0g / m 2 Less than 1.0 g / m 2 More than 5.0g / m 2 More preferably, 2.0 g / m or less 2 More than 4.0g / m 2 It may be the following.

[0062] <Pile fabric forming process> The pile fabric forming step is a step of forming a pile fabric prior to the above-mentioned silicon imparting step P1 and silicon / flame retardant imparting step P1'. As described above, the pile fabric may be a woven pile fabric, a knitted pile fabric, or a tufted pile fabric. When the pile fabric is a woven pile fabric, the pile fabric forming process can be said to be a woven pile fabric weaving process, when the pile fabric is a knitted pile fabric, the pile fabric forming process can be said to be a knitted pile fabric knitting process, and when the pile fabric is a tufted pile fabric, the pile fabric forming process can be said to be a tufted pile fabric forming process.

[0063] Here, in the case of the pile fabric weaving process, the pile fabric woven in this process may be, for example, a pair of upper and lower fabrics, each of which is woven with warp and weft threads in a plain weave, twill weave, satin weave, etc., and then woven together with the upper and lower fabrics in a warp direction using a pile thread as a connecting thread, and then the connecting thread is cut approximately in the center (center cut). As a result, two pile fabrics are simultaneously produced, with the upper or lower fabric as the base fabric 3 and each of the cut connecting threads (pile threads) as the pile 2, and the pile fabric having such a configuration is also called a moquette 1, and in this case, it is woven by a double moquette loom (jacquard loom, dobby loom, etc.). Alternatively, instead of connecting the upper and lower fabrics with pile threads, the moquette may be woven together with one fabric by hooking the pile thread in the warp direction on a wire extending in the weft direction, and in this case, it is woven by a wire moquette loom. In the case of a pile knitting process, the pile knitted fabric to be knitted in this process may be, for example, a knitted fabric (a type of warp knitting, also called Denbigh knitting or tricot) knitted by a knitting machine having a predetermined number of warp threads (e.g., three reeds) as the base fabric 3, and the pile 2 may be formed by raising one or both sides of this base fabric 3. Furthermore, in the case of the tufted pile fabric forming process, the tufted pile fabric formed in this process is formed, for example, by a tufting machine that tufts (implants) the pile 2 into the base fabric 3 at predetermined intervals. EXAMPLES

[0064] Hereinafter, examples 1 to 5 of the pile fabric 1 according to the present invention, comparative example 1, and reference examples 1 to 3 will be mentioned. These Examples, Comparative Examples, and Reference Examples are used to carry out Tests 1 and 2 described below. Among these Examples, Comparative Examples, and Reference Examples, for Examples 1 and 2 and Reference Example 1, cross-sectional photographs as substitutes for drawings and images showing the positions of silicon and fluorine by dots are shown in Figures 3 to 5.

[0065] <Example 1> The pile fabric 1 of Example 1 is a pile fabric of the first embodiment in which the pile 2 is made of flame-retardant fiber S and the base fabric 3 is made of non-flame-retardant fiber S', and is a pile fabric (moquette) woven in a pile fabric forming process (pile fabric weaving process). In the silicon imparting step P1, a dispersion liquid obtained by mixing a mixture of polyester resin and silicon-based fine particles K as binder resin B with water as a dispersion medium was applied to this pile fabric by padding method (Dip-Nip method) in an atmosphere of 130°C, and then the pile fabric was stretched with a pin tenter and dried at a drying temperature of 150°C in a dryer to provide silicon exposed parts 4. It can be said that the silicon-based fine particles K in the silicon imparting step P1 are used as colloidal silica. After the silicon imparting step P1, in the fluorine coating step (fluorine-based silicon coating step) P2, a dispersion of a fluorine-based water / oil repellent F mixed with water as a dispersion medium was applied to the pile fabric by a dipping method in an atmosphere at 130°C to provide a fluorine-coated part (fluorine-based silicon coated part) 5. After the fluorine coating step (fluorine-based silicon coating step) P2, in the backcoat step P3, a dispersion liquid obtained by mixing at least a urethane resin and a phosphorus-based flame retardant as the flame retardant N with water as a dispersion medium was applied to the back surface 3b of the base fabric 3 of the pile fabric by painting under an atmosphere of 150°C to provide a coating part 10, thereby producing the pile fabric 1 of Example 1. In addition, the pile fabric 1 of Example 1 had an adhesion amount of silicon-based fine particles K of 0.99 g / m 2 The amount of binder resin B attached is 0.38 g / m 2 The amount of fluorine-based water and oil repellent F attached was 0.64 g / m 2 The amount of urethane resin attached was 48.40 g / m 2 The amount of flame retardant N attached is 61.60g / m 2 It is. 3, in the cross section of pile fabric 1 of Example 1, the positions of silicon (silicon-based fine particles K) and fluorine (fluorine-based water / oil repellent agent F) are shifted from each other in some parts and overlap in other parts, and in particular, in FIG. 3(d), silicon-exposed parts 4 are provided at the white dots where only silicon is present, and fluorine-coated parts (silicon-coated parts with fluorine) 5 are provided at least at the grey dots where silicon and fluorine overlap. Furthermore, in FIG. 3(b) to (d), the parts where neither silicon nor fluorine is present can be said to represent fiber-exposed parts 6.

[0066] <Example 2> In the pile fabric 1 of Example 1, the amount of silicon-based fine particles K attached was 1.98 g / m 2 The amount of binder resin B attached was 0.75 g / m 2 The amount of fluorine-based water and oil repellent F applied was 1.28 g / m 2 The adhesion weight of the urethane resin was 50.60 g / m 2 The adhesion amount of flame retardant N was 64.60 g / m 2 The result was pile fabric 1 of Example 2. 4(d) in particular, silicon-exposed portions 4 are provided at the white dot positions where only silicon is present, and fluorine-coated portions 5 are provided at the grey dot positions where silicon and fluorine overlap. Furthermore, in FIGS. 4(b) to 4(d), the portions where neither silicon nor fluorine is present can be said to represent fiber-exposed portions 6.

[0067] <Example 3> In the pile fabric 1 of Example 1, the amount of silicon-based fine particles K attached was 3.96 g / m 2 The amount of binder resin B attached was 1.50 g / m 2 The amount of fluorine-based water and oil repellent F applied was 2.56 g / m 2 The adhesion weight of the urethane resin was 46.20 g / m 2The adhesion amount of flame retardant N was 58.80 g / m 2 The result was designated as pile fabric 1 of Example 3.

[0068] <Example 4> The pile fabric 1 of Example 4 is the pile fabric of the second embodiment in which the non-flame retardant fiber S' is used for the pile 2 and base fabric 3, and is a pile fabric (moquette) woven in the pile fabric forming process (pile fabric weaving process). In the silicon / flame retardant imparting process P1', a dispersion liquid obtained by mixing a mixture of polyester resin as binder resin B, silicon-based fine particles K, and a phosphorus-based flame retardant as flame retardant N with water as a dispersion medium was applied to this pile fabric by padding method (Dip-Nip method) in an atmosphere of 130°C, and then the pile fabric was stretched with a pin tenter and dried in a dryer at a drying temperature of 150°C to provide silicon exposed parts 4 and flame retardant exposed parts 4'. It should be noted that the silicon-based fine particles K in the silicon / flame retardant imparting process P1' can also be said to be used as colloidal silica. After the silicon / flame retardant imparting process P1', in the fluorine coating process (fluorine-based silicon / flame retardant coating process) P2', a dispersion of fluorine-based water / oil repellent F mixed with water as a dispersion medium is applied to the pile fabric by a dipping method in an atmosphere of 130°C to form a fluorine-coated part (fluorine-based silicon coated part) 5 and a fluorine-coated part (fluorine-based flame retardant coated part) 5'. After the fluorine coating step (fluorine-based silicon / flame retardant coating step) P2', in the backcoat step P3, a dispersion obtained by mixing at least a urethane resin, a phosphorus-based flame retardant as the flame retardant N, and a blocked isocyanate-based crosslinking agent as the crosslinking agent and dispersing the mixture in water as a dispersion medium was applied to the back surface 3b of the base fabric 3 of the pile fabric by coating in an atmosphere of 150°C to provide a coating part 10, thereby producing the pile fabric 1 of Example 4. In addition, the pile fabric 1 of Example 4 had an adhesion amount of silicon-based fine particles K of 1.98 g / m 2 The amount of binder resin B attached is 0.5 g / m 2 The amount of flame retardant N attached is 0.35 g / m 2The amount of fluorine-based water and oil repellent F attached was 1.28 g / m 2 The amount of urethane resin attached was 51.90 g / m 2 The amount of flame retardant N attached is 66.10 g / m 2 The amount of crosslinking agent applied is 3.15 g / m 2 It is.

[0069] <Example 5> In pile fabric 1 of Example 4, the amount of urethane resin attached was 48.40 g / m 2 The adhesion amount of flame retardant N was 61.60 g / m 2 The amount of the crosslinking agent, which was a carbodiimide crosslinking agent, attached was 2.93 g / m 2 The result was designated as pile fabric 1 of Example 5.

[0070] <Comparative Example 1> In the pile fabric 1 of Example 1, the binder resin B, the silicon-based fine particles K, and the fluorine-based water- and oil-repellent agent F were not applied to the pile fabric 2 or the base fabric 3, and the amount of the urethane-based resin attached was 48.40 g / m 2 The adhesion amount of flame retardant N was 61.60 g / m 2 As a result, the pile fabric of Comparative Example 1 was prepared.

[0071] <Reference Example 1> In the pile fabric 1 of Example 1, the amount of silicon-based fine particles K attached was 0.59 g / m 2 The amount of binder resin B attached was 0.23 g / m 2 The amount of fluorine-based water and oil repellent F applied was 0.38 g / m 2 The adhesion weight of the urethane resin was 49.30 g / m 2 The adhesion amount of flame retardant N was 62.70 g / m 2 The pile fabric 1 was used as the reference example 1. 5, in the cross section of the pile fabric 1 of Reference Example 1, the silicon and fluorine positions are shifted from each other in some areas and overlap in other areas, and in particular, in FIG. 5(d), silicon-exposed parts 4 are provided at the white dots where only silicon is present, and fluorine-coated parts (silicon-coated parts with fluorine) 5 are provided at least at the grey dots where silicon and fluorine overlap. Furthermore, in FIG. 5(b) to (d), the parts where neither silicon nor fluorine is present can be said to represent fiber-exposed parts 6.

[0072] <Reference Example 2> In the pile fabric 1 of Example 1, the amount of silicon-based fine particles K attached was 4.95 g / m 2 The adhesion amount of binder resin B was 1.88 g / m 2 The amount of fluorine-based water and oil repellent F applied was 3.20 g / m 2 The adhesion weight of the urethane resin was 47.50 g / m 2 The amount of flame retardant N attached was 60.50 g / m 2 The result was pile fabric 1 of Reference Example 2.

[0073] <Reference Example 3> In the pile fabric 1 of Example 4, the flame retardant N and the crosslinking agent were not applied to the pile fabric 2 or the base fabric 3, and the amount of the urethane resin attached was 50.60 g / m 2 The amount of flame retardant N attached was 64.40 g / m 2 As a result, the pile fabric of Reference Example 3 was obtained.

[0074] The amount of each material attached and the material of the pile 2 in the above-mentioned Examples 1 to 5, Comparative Example 1, and Reference Examples 1 to 3 are shown in Table 1 below.

[0075] [Table 1]

[0076] <Anti-stain properties against dry stains> The "stain resistance against dry stains" of the pile fabric 1 in the present invention is measured in accordance with the stain resistance test of JIS-L-1919:2020, Method A-1 (method using a sealed cylindrical container). In addition, in the present invention, "measured in accordance with the soil resistance test of JIS-L-1919:2020, Method A-1 (method using a sealed cylindrical container)" not only includes measurement as described in the soil resistance test of JIS-L-1919:2020, Method A-1 (method using a sealed cylindrical container), but also measurement by applying the description of the A-1 method mutatis mutandis (or with some modifications). The anti-fouling property against such dry stains may be grade 3.5 or higher, preferably grade 4 or higher, in the stain resistance test according to the A-1 method (method using a sealed cylindrical container) of JIS-L-1919:2020.

[0077] <Anti-stain properties against wet stains> Regarding the "stain resistance against wet stains" of the pile fabric 1 in the present invention, the water repellency is measured using the IPA water repellency test method, and the oil repellency is measured using AATCC (The American Association of Textile Chemists and Colorists)-118. In the IPA water repellency test, a mixture of deionized water and isopropyl alcohol (IPA) was gently placed on the pile 2 side (on the pile surface, on the surface 1a of the pile fabric 1) of Examples 1 to 5, Comparative Example 1, and Reference Examples 1 to 3 in the order of 1, 2, 3, ... as droplets of about 3 mm in size (5 or 6 drops) in the order of grades 1, 2, 3, ... shown below, and the state after 30 seconds was observed. The water repellency performance was measured as the highest grade value at which 2 to 3 drops could be maintained. <Grade> IPA / Water (unit: volume %) 1 2 / 98 2 5 / 95 3 10 / 90 4 20 / 80 5 30 / 70 6 40 / 60 7 50 / 50 8 60 / 40 9 70 / 30 10 80 / 20 11 90 / 10 12 100 / 0 In addition, AATCC-118 measures the oil repellency by gently placing several drops (5 or 6 drops) of a mixture of a specified chemical and a special mineral oil on the pile 2 side (on the pile face, on the surface 1a of the pile fabric 1) of about 3 mm in size in the order of 1, 2, 3, ... shown below for Examples 1 to 5, Comparative Example 1, and Reference Examples 1 to 3, and observing the state after 30 seconds. The oil repellency is measured by the highest grade value at which 2 to 3 drops can be maintained. <Grade> Chemicals / Special mineral oil (unit: volume %) Surface tension (unit: dyne / cm) 0 0 / 100 Salad oil (cottonseed oil) 33.0 1 0 / 100 Nujol (liquid paraffin) 32.8 2 n-Hexadecane 35 / 65 Nujol (liquid paraffin) 29.5 3 n-Hexadecane 100 / 0 27.7 4 n-Tetradecane 100 / 0 26.5 5 n-Dodecane 100 / 0 25.4 6 n-Decane 100 / 0 23.9 7 n-Octane 100 / 0 21.7 8 n-Heptane 100 / 0 20.0 The soil resistance against such wet soils may be grade 6 or higher, preferably grade 8 or higher, and more preferably grade 10 or higher, in the IPA water repellency test method, and may be grade 2 or higher, preferably grade 4 or higher, and more preferably grade 5 or higher, in the AATCC-118 method.

[0078] <Test 1 (Anti-stain test)> In Test 1, for <stain resistance against dry stains>, a stain resistance test is performed using the A-1 method of JIS-L-1919:2020 (a method using a sealed cylindrical container) to compare the grades obtained using the A-1 method for the pile fabrics of the above-mentioned Examples 1 to 5, Comparative Example 1, and Reference Examples 1 and 2 in the following states: initial state (no treatment); state after 1000, 1500, and 2500 abrasion treatments using an abrasion tester; and state after 3 washes using a washing tester. In addition, in Test 1, with regard to <soil resistance against wet stains>, the grades determined by the IPA water repellency test method and AATCC-118 for the pile fabrics of the above-mentioned Examples 1 to 5, Comparative Example 1, and Reference Examples 1 and 2 in their initial state (no treatment) are compared, and the grades determined by the IPA water repellency test method and AATCC-118 for the pile fabrics of the above-mentioned Examples 2 and 4 and Comparative Example 1 in their state after three washing treatments using a washing test machine are compared. Here, the abrasion measured using an abrasion tester in Test 1 refers to abrasion measured using an abrasion tester conforming to the A-1 method (flat method) of the A method (universal type method) of JIS-L-1096:2010, and the washing measured using a washing tester in Test 1 refers to washing measured using a washing tester conforming to the A-2 test of JIS-L-0844:2011. In the present invention, "abrasion using an abrasion tester conforming to the A-1 method (flat method) of the A method (universal type method) of JIS-L-1096:2010" includes abrasion using an abrasion tester as described in the A-1 method (flat method) of the A method (universal type method) of JIS-L-1096:2010, as well as abrasion using an abrasion tester that applies the description of the A-1 method mutatis mutandis (or with a partial modification), and "washing using a washing tester conforming to the A-2 test of JIS-L-0844:2011" includes selection using a washing tester as described in the A-2 test of JIS-L-0844:2011, as well as washing using a washing tester that applies the description of the A-2 test mutatis mutandis (or with a partial modification). The measurement results of this test 1 are shown in Table 2 below.

[0079] [Table 2]

[0080] <Evaluation of Test 1 (Anti-stain test)> As shown in Table 2, in Comparative Example 1, none of the binder resin B, silicon-based microparticles K, and fluorine-based water- and oil-repellent agent F are attached to the fiber surfaces Sa and Sa', and the fiber surfaces Sa and Sa' have neither silicon exposed portions 4 nor fluorine-coated portions (silicon-coated portions by fluorine) 5. Therefore, regardless of whether the fiber is in its initial state or has been subjected to treatments such as friction or washing, the <stain resistance against dry stains> is Class 3, and the <stain resistance against wet stains> is Class 0 in both the IPA water repellency test method and AATCC-118, meaning that the stain resistance against both dry and wet stains is insufficient. In contrast, in Examples 1 to 3 and Reference Examples 1 and 2, binder resin B, silicon-based fine particles K, and fluorine-based water- and oil-repellent agent F are adhered to the fiber surfaces Sa and Sa', and the fiber surfaces Sa and Sa' have silicon exposed portions 4 and fluorine-coated portions (fluorine-coated silicon portions) 5. Also, in Examples 4 and 5, binder resin B, silicon-based fine particles K, flame retardant N, and fluorine-based water- and oil-repellent agent F are adhered to the fiber surface Sa', and the fiber surface Sa' has silicon exposed portions 4, fluorine-coated portions (fluorine-coated silicon portions) 5, flame-retardant exposed portions 4', and fluorine-coated portions (fluorine-coated flame-retardant portions) 5'. Therefore, regardless of whether the fiber is in its initial state or has been subjected to treatments such as friction or washing, the <stain resistance against dry stains> is 3.5 or higher, and the <stain resistance against wet stains> is 7 or higher in the IPA water repellency test method and 4 or higher in the AATCC-118 method. Therefore, as in the present invention, by providing silicon exposed portions 4 and fluorine-coated portions (silicon-coated portions with fluorine) 5 on the fiber surfaces Sa, Sa' of the pile fabric 1, and further providing flame-retardant exposed portions 4' and fluorine-coated portions (flame-retardant coated portions with fluorine) 5', "improved stain resistance against both dry and wet stains" is realized. In addition, in the test 1, when comparing Reference Example 1 with Examples 1 to 3, the amount of silicon-based fine particles K attached in Reference Example 1 was 0.8 g / m 2and the amount of binder resin B adhered is less than 0.3 g / m 2 less than 0.5g / m2 and the amount of fluorine-based water / oil repellent F adhered to the surface is less than 0.5g / m2. 2 Therefore, the <anti-soiling property against dry soil> is grade 3.5, and the <anti-soiling property against wet soil> is grade 9 in the IPA water repellency test method and grade 4 in AATCC-118. However, in Examples 1 to 3, the adhesion amount of silicon-based fine particles K is 0.8 g / m 2 With the above, the adhesion amount of binder resin B is 0.3 g / m 2 With the above, the amount of fluorine-based water and oil repellent F adhered is 0.5 g / m 2 Therefore, the <stain resistance against dry stains> is grade 4 or above, and the <stain resistance against wet stains> is grade 10 in the IPA water repellency test method and grade 5 in AATCC-118. Therefore, the adhesion amount of silicon-based fine particles K is 0.8 g / m 2 or more, and the adhesion amount of binder resin B is 0.3 g / m 2 or more, and the amount of fluorine-based water and oil repellent F adhered was 0.5 g / m 2 By doing the above, it is possible to further "improve the stain resistance against both dry and wet stains."

[0081] <Test 2 (Flame retardancy, pile removal, texture test)> In Test 2, for <flame retardancy>, the pile fabrics of Examples 1 to 5, Comparative Example 1, and Reference Examples 1 to 3 described above were compared in the Railway Vehicle Material Flammability Test (described in the Commentary on Technical Standards for Vehicles by the Japan Railway Rolling Stock and Machinery Technology Association, a general incorporated association) to determine pass / fail judgment based on whether the flame during alcohol combustion exceeded the top end of the test specimen, whether there was any residual flame or residual glow after the alcohol combustion, and whether charring or deformation reached the top end of the test specimen (if not, numerical values ​​are given in mm). In Test 2, for <pile loss>, the pile fabrics of the above-mentioned Examples 1 to 5, Comparative Example 1, and Reference Examples 1 and 2 are subjected to 5,000 abrasion tests using an abrasion tester, and then the presence or absence of pile loss is compared. Here, the abrasion measured using the abrasion tester in Test 2 is also measured using an abrasion tester conforming to the A-1 method (flat method) of the A method (universal type method) of JIS-L-1096:2010. In Test 2, the <handle> is judged by visual inspection and touch for the above-mentioned Examples 1 to 5, Comparative Example 1, and Reference Examples 1 to 3. The measurement results of this test 2 are shown in Table 3 below.

[0082] [Table 3]

[0083] <Test 2 (Flame retardancy, pile removal, texture test) evaluation> Regarding <Flame retardancy>, as shown in Table 3, in Reference Example 3, non-flame retardant fiber S' is used for the pile 2 and base fabric 3 (i.e., flame retardant fiber S is not used for the pile 2), and flame retardant N is not attached to the fiber surface Sa' of the non-flame retardant fiber S'. Therefore, the flame during alcohol combustion exceeds the upper end of the test piece, there are residual flames and residual dust after alcohol combustion, and carbonization and deformation reach the upper end of the test piece, resulting in a pass / fail judgment of fail. In contrast, with regard to <Flame retardancy>, in Examples 1 to 3 and Reference Examples 1 and 2, etc., flame-retardant fiber S was used in the pile 2, and flame retardant N was attached to the fiber surfaces Sa and Sa'. In addition, in Examples 4 and 5, non-flame-retardant fiber S' was used in the pile 2 and base fabric 3 (i.e., flame-retardant fiber S was not used in the pile 2), but flame retardant N was attached to the fiber surface Sa' of the non-flame-retardant fiber S'. Therefore, the flame during alcohol combustion did not exceed the top end of the test specimen, there was no residual flame or residual dust after alcohol combustion, the charring or deformation did not reach the top end of the test specimen, and the charring or deformation that occurred was 60 mm or less, resulting in a pass / fail judgment. Therefore, as in the present invention, the pile fabric can be made flame-retardant by using flame-retardant fiber S for the pile 2 or by applying a flame retardant N to the fiber surfaces Sa, Sa'. Regarding <pile loss>, as shown in Table 3, Examples 1 to 5 and Reference Examples 1 and 2, etc. have a back coat portion 10 containing flame retardant N, etc. on the back surface 3b of the base fabric 3, so there is no pile loss even after being subjected to 5,000 abrasion cycles using an abrasion tester. Therefore, by providing the back coat portion 10 containing the flame retardant N or the like, the pile 2 is prevented from coming off the base fabric 3, and the flame retardancy of the pile fabric 1 as a whole is improved. Regarding the feel, as shown in Table 3, in Reference Example 2, the amount of silicon-based fine particles K attached was 4.50 g / m 2 Exceeding 4.95g / m 2 The amount of binder resin B attached is 1.70 g / m 2 Exceeding 1.88g / m 2 The amount of fluorine-based water and oil repellent F attached was 2.90 g / m 2 Exceeding 3.20g / m 2 As a result, the silicon-based microparticles K, binder resin B, and fluorine-based water- and oil-repellent agent F are excessively attached to the fiber surfaces Sa and Sa', which reduces the texture of the pile fabric and results in an evaluation of "X." In contrast, with regard to the <handle>, in Examples 1 to 5 and Reference Examples 1 and 3, the amount of silicon-based fine particles K attached was 4.50 g / m 2 or less, and the adhesion amount of binder resin B is 1.70 g / m 2 or less, and the amount of fluorine-based water / oil repellent F attached is 2.90 g / m 2 Since the above value is less than 100%, the deterioration of the texture of the pile fabric 1 can be suppressed, and the result is judged as "○". Therefore, the amount of silicon-based fine particles K attached is 4.50 g / m 2 and the adhesion amount of binder resin B is 1.70 g / m 2 The amount of fluorine-based water and oil repellent F applied was 2.90 g / m 2 By setting the following, the texture of the pile fabric can be maintained. Considering the texture of this Test 2 and the above Test 1, the amount of silicon-based fine particles K attached is 0.8 g / m 2 More than 4.5g / m 2 or less, and the adhesion amount of binder resin B is 0.3 g / m 2 More than 1.7g / m 2 The amount of fluorine-based water and oil repellent F applied was 0.5 g / m 2 More than 2.9g / m 2By setting the value below, it is possible to achieve both further "improved stain resistance against both dry and wet stains" and "maintaining the texture of the pile fabric."

[0084] <Other> The present invention is not limited to the above-described embodiment. The individual components of the pile fabric 1 and the manufacturing method of the pile fabric 1, as well as the overall structure, shape, dimensions, etc., can be appropriately changed in accordance with the spirit of the present invention. The pile fabric 1 does not necessarily have to have the back coat portion 10. Furthermore, the pile fabric 1 may have a fluorine directly attached portion 7, which will be described later.

[0085] <Fluorine direct attachment part 7> As shown in Figures 1 to 5, when the pile fabric 1 is of the first embodiment, the fluorine-based directly-attached portion 7 is a portion on the fiber surfaces Sa, Sa' of the above-mentioned flame-retardant fiber S and non-flame-retardant fiber S' where the fluorine-based water- and oil-repellent agent F directly adhered to the fiber surfaces Sa, Sa' is exposed; when the pile fabric 1 is of the second embodiment, the fluorine-based directly-attached portion 7 is a portion on the fiber surface Sa' of the above-mentioned non-flame-retardant fiber S' where the fluorine-based water- and oil-repellent agent F directly adhered to the fiber surface Sa' is exposed; in other words, it is a fluorine-exposed portion. In the present invention, "the fluorine-based water- and oil-repellent agent F attached to the fiber surfaces Sa and Sa' is exposed" means that the fluorine-based water- and oil-repellent agent F is directly attached to the fiber surface Sa of the flame-retardant fiber S and the fiber surface Sa' of the non-flame-retardant fiber S', respectively, and the fluorine surface of the fluorine-based water- and oil-repellent agent F is not covered by the silicon-based fine particles K or the like described above. In addition, in the present invention, "the fluorine-based water- and oil-repellent agent F attached directly to the fiber surface Sa' is exposed" means that the fluorine-based water- and oil-repellent agent F is directly attached to the fiber surface Sa' of the non-flame-retardant fiber S', and the fluorine surface of the fluorine-based water- and oil-repellent agent F is not covered by the silicon-based fine particles K or the like described above. In Figures 3 to 5(d), where the positions of silicon and fluorine are superimposed, the positions where only fluorine is present (the positions of fluorine that are not overlapped with silicon) are represented by black dots. Furthermore, when the pile fabric 1 has a fluorine-based directly attached portion 7, the "amount of fluorine-based water- and oil-repellent agent F adhered thereto" in the present invention means not only the amount of fluorine-based water- and oil-repellent agent F covering the silicon-based microparticles K adhered to the fiber surfaces Sa, Sa' via the binder resin B, but also the total amount of fluorine-based water- and oil-repellent agent F directly adhered to the fiber surfaces Sa, Sa'. Furthermore, the adhesion between the silicon-based microparticles K and the fiber surfaces Sa, Sa' may be performed by any means, but for example, the main chain of the fluorine-based water- and oil-repellent agent F may be entangled with the silicon-based microparticles K and adhered thereto, or the silicon-based microparticles K and the fluorine-based water- and oil-repellent agent F may be adhered to each other via a specified binder resin. The fluorine directly attached portions 7 described so far may also be scattered on the fiber surfaces Sa, Sa' of the fibers S, S' used in the pile 2 and base fabric 3 of the pile fabric 1, or may be island portions in a sea-island pattern (see Figures 3 to 5(b) and (d)).

[0086] In addition, the pile fabric 1 can be said to have no portions on the fiber surfaces Sa, Sa' of the above-mentioned flame-retardant fiber S and non-flame-retardant fiber S' where the fluorine-based water- and oil-repellent agent F directly adhered to the fiber surfaces Sa, Sa' is covered by silicon-based microparticles K (i.e., fluorine-coated portions by silicon).Furthermore, in addition to not having the above-mentioned fluorine-coated portions by silicon, the pile fabric 1 can be said to have no portions on the fiber surface Sa' of the above-mentioned non-flame-retardant fiber S' where the fluorine-based water- and oil-repellent agent F directly adhered to the fiber surface Sa' is covered by flame retardant N adhered via binder resin B or the like (i.e., fluorine-coated portions by flame retardant). This can be said to be because the fluorine-based water- and oil-repellent agent F is first directly attached to the fiber surfaces Sa, Sa', and even if silicon-based fine particles K, flame retardant N, binder resin B, etc. try to cover the fluorine-based water- and oil-repellent agent F, the fluorine-based water- and oil-repellent agent F exerts water- and oil-repellent properties and is therefore unable to cover the fluorine-based water- and oil-repellent agent F. Therefore, it can be said that the grey dots in Figures 3 to 5(d), where the positions of silicon and fluorine are superimposed, represent only the fluorine-covered parts (silicon-covered parts by fluorine) 5 described above.

[0087] If desired, the pile fabric 1 may contain any extender pigment or filler (filling material) such as titanium oxide or calcium carbonate, or may be made of a material containing added deodorants, antibacterial agents, antifungal agents, flame retardants, water repellents, stain resistant agents, colorants, fragrances, foaming agents, dispersants, etc. The pile fabric 1 may have any color tone, such as black, brown, blue, white, red, orange, yellow, green, purple, etc., and may have any value of saturation or brightness. The pile fabric 1 may have any pattern, such as a solid color, a plant pattern such as a flower or a plant, an animal pattern, a geometric pattern, or a pattern with a surface irregularity.

[0088] In the first and third embodiments of the manufacturing method for the pile fabric 1 that does not include the backcoat process P3, it is not necessary to apply the mixture of binder resin B and silicon-based fine particles K, or the mixture of binder resin B, silicon-based fine particles K and flame retardant N, and the fluorine-based water- and oil-repellent agent F separately to the pile fabric. For example, as long as the silicon exposed portion 4, the flame-retardant exposed portion 4', the fluorine-coated portion (the silicon-coated portion with fluorine) 5, and the fluorine-coated portion (the flame-retardant coated portion with fluorine) 5' are provided, the mixture of binder resin B and silicon-based fine particles K and the fluorine-based water- and oil-repellent agent F may be applied simultaneously (in a so-called one-stage process). [Industrial Applicability]

[0089] The pile fabric according to the present invention and the pile fabric produced by the method for producing a pile fabric according to the present invention can be used to cover interior materials (inner wall materials, ceiling materials, floor materials, etc.) and seats in the interiors (cabins) of vehicles such as railway cars, automobiles (passenger cars), aircraft, ships, etc., and in the case of railway cars in particular, they can be used to cover seats, chairs, etc., and as other interior materials (inner wall materials, ceiling materials, floor materials). In addition, the pile fabric according to the present invention and the pile fabric produced by the method for producing a pile fabric according to the present invention can be used not only for the interiors of vehicles such as the above-mentioned railway cars, but also for covering interior materials such as wall materials, ceiling materials and flooring materials inside buildings such as houses and buildings, furniture such as chairs and beds, lighting fixtures, etc., and may also be used for industrial material applications and daily necessities such as shoes and clothing. [Explanation of symbols]

[0090] 1 Pile fabric 2 Pile 3 Base fabric 4 Silicon exposed area 4' Flame retardant exposed part 5 Fluorine-coated parts (fluorine-coated silicon parts) 5' Fluorine-coated part (Flame-retardant coating made of fluorine) 6 Exposed fiber area 10 Backcourt P1 Silicon addition process P1' Silicon flame retardant process P2 Fluorine coating process (fluorine-based silicon coating process) P2' Fluorine coating process (fluorine-based silicon / flame-retardant coating process) P3 Backcoat process

Claims

1. A pile fabric in which the pile (2) is erected from a base fabric (3), The pile (2) is made of flame-retardant fiber, The base fabric (3) is made of a non-flame retardant fiber, On the fiber surface of the flame retardant fiber and the non-flame retardant fiber, a silicon-exposed portion (4) in which silicon-based fine particles attached to the fiber surface via a binder resin are exposed; The pile fabric is characterized in having a fluorine-coated portion (5) in which silicon-based fine particles adhered to the fiber surface via a binder resin are coated with a fluorine-based water and oil repellent agent.

2. A pile fabric in which the pile (2) is erected from a base fabric (3), The pile (2) and the base fabric (3) are made of non-flame retardant fibers, On the fiber surface of the non-flame retardant fiber, a silicon-exposed portion (4) in which silicon-based fine particles attached to the fiber surface via a binder resin are exposed; a flame retardant exposed portion (4') in which the flame retardant attached to the fiber surface via the binder resin is exposed; a fluorine-based coating portion (5) in which silicon-based fine particles attached to the fiber surface via a binder resin are coated with a fluorine-based water- and oil-repellent agent; The pile fabric has a fluorine-coated portion (5') in which the flame retardant attached to the fiber surface via a binder resin is coated with a fluorine-based water and oil repellent.

3. 3. The pile fabric according to claim 1 or 2, further comprising an exposed fiber portion (6) on the fiber surface where the fiber surface is exposed.

4. 3. The pile fabric according to claim 1, further comprising a back coat portion (10) on the back surface of the base fabric (3) which is coated with a mixture of at least a urethane resin and a flame retardant.

5. The amount of the silicon-based fine particles attached is 0.8 g / m 2 4.5g / m or more 2 is as follows: The amount of the binder resin attached is 0.3 g / m 2 1.7g / m or more 2 is as follows: The amount of the fluorine-based water- and oil-repellent agent attached is 0.5 g / m 2 2.9g / m or more 2 3. The pile fabric according to claim 1, wherein:

6. A method for manufacturing a pile fabric in which a pile (2) is erected from a base fabric (3), comprising the steps of: The pile (2) is made of flame-retardant fiber, The base fabric (3) is made of a non-flame retardant fiber, a silicon-imparting step (P1) of providing a mixture of at least a binder resin and silicon-based microparticles to the pile fabric, and then drying the pile fabric to provide silicon-exposed portions (4) on the fiber surfaces of the flame-retardant fibers and non-flame-retardant fibers, in which silicon-based microparticles attached to the fiber surfaces via the binder resin are exposed; The method for producing a pile fabric comprises, after the silicon imparting step (P1), a fluorine-based water- and oil-repellent step (P2) of applying a fluorine-based water- and oil-repellent agent to the pile fabric to provide, on fiber surfaces of the flame-retardant fibers and non-flame-retardant fibers, fluorine-coated portions (5) in which the fluorine-based water- and oil-repellent agent covers silicon-based fine particles adhered to the fiber surfaces via a binder resin.

7. A method for manufacturing a pile fabric in which a pile (2) is erected from a base fabric (3), comprising the steps of: The pile (2) and the base fabric (3) are made of non-flame retardant fibers, a silicon / flame retardant imparting step (P1') of imparting a mixture of at least a binder resin, silicon-based microparticles, and a flame retardant to the pile fabric, and then drying the pile fabric to provide, on the fiber surface of the non-flame retardant fiber, a silicon exposed portion (4) where the silicon-based microparticles attached to the fiber surface via the binder resin are exposed, and a flame retardant exposed portion (4') where the flame retardant attached to the fiber surface via the binder resin is exposed; The method for producing a pile fabric comprises a fluorine-based water- and oil-repellent step (P2') of applying a fluorine-based water- and oil-repellent agent to the pile fabric after the silicon / flame-retardant application step (P1') to provide, on the fiber surfaces of the non-flame-retardant fibers, a fluorine-coated portion (5) in which the silicon-based fine particles adhered to the fiber surface via the binder resin are coated with the fluorine-based water- and oil-repellent agent, and a fluorine-coated portion (5') in which the flame retardant adhered to the fiber surface via the binder resin is coated with the fluorine-based water- and oil-repellent agent.

8. The addition of the mixture in the silicon addition step (P1) or the silicon / flame retardant addition step (P1') is carried out in an atmosphere at a predetermined temperature, 8. The method for producing a pile fabric according to claim 6, wherein the mixture is applied in the fluorine coating step (P2, P2') in an atmosphere having a temperature higher than the predetermined temperature.

9. The application of the mixture in the silicon application step (P1) or the silicon / flame retardant application step (P1') and the fluorine coating step (P2, P2') is carried out in an atmosphere at a predetermined temperature, 8. The method for producing pile fabric according to claim 6 or 7, further comprising a backcoat step (P3) of providing a backcoat portion (10) coated with a mixture of at least a urethane resin and a flame retardant on a back surface of the base fabric (3) in an atmosphere having a temperature higher than the predetermined temperature after the fluorine coating step (P2, P2').

10. The amount of the silicon-based fine particles applied is 0.8 g / m 2 4.5g / m or more 2 is as follows: The amount of the binder resin applied is 0.3 g / m 2 1.7g / m or more 2 is as follows: The amount of the fluorine-based water and oil repellent applied is 0.5 g / m 2 2.9g / m or more 2 8. The method for producing a pile fabric according to claim 6, wherein the following is true:

Citation Information

Patent Citations

  • Functional fabric and its production

    JP2000110069A

  • Fabric for stainproof vehicle interior material

    JP2011168905A