Chloroprene rubber composition and dust cover for ball joints
Patent Information
- Application Number
- JP2023081982
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
【0010】 本発明によれば、クロロプレンゴム100重量部に対して、融点90℃以下の炭化水素系ワックスを3.5~10重量部と、芳香族第二級アミン系老化防止剤を5~12重量部とを配合せしめることにより、金属との接着性にすぐれ、さらにはオゾン濃度が50pphmで0~30%伸長の動的オゾン劣化試験(JIS K 6259)で500時間以上亀裂の生じないクロロプレンゴム組成物を得ることができ、これをボールジョイント用ダストカバーに適用することで、一段と高い耐オゾン性を有するダストカバーを提供することができる。
Smart Images

Figure 2024165629000008 
Figure 2024165629000001 
Figure 2024165629000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a chloroprene rubber composition, and more particularly to a chloroprene rubber composition suitable for use in a dust cover for preventing the intrusion of foreign matter such as dust and rainwater into a ball joint for an automobile. [Background technology]
[0002] 2. Description of the Related Art As disclosed in Patent Document 1, for example, a dust cover is attached to an automobile ball joint to prevent the intrusion of foreign matter such as dust and rainwater.
[0003] Rubber materials are generally used as materials for such ball joint dust covers, and among them, chloroprene rubber is particularly suitable as a rubber material with excellent heat resistance and ozone resistance. As a product similar to ball joint dust covers, Patent Document 2 discloses a constant velocity joint boot made of chloroprene rubber, which describes a chloroprene rubber composition in which 3 parts by weight or less of p-phenylenediamine and 0.8 parts by weight or less of paraffin wax are added to 100 parts by weight of chloroprene rubber. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2011-252519 A [Patent Document 2] JP 2000-291798 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when the chloroprene rubber composition of Patent Document 2 is applied to a dust cover for a ball joint, the adhesion between the rubber and metal becomes an issue. That is, as disclosed in Patent Document 1, a dust cover for a ball joint has a metal ring disposed inside the rubber, and it is necessary for the rubber and the metal ring to be reliably adhered to each other, but Patent Document 2 does not take this into consideration.
[0006] Furthermore, in recent years, due to the deterioration of the global environment and the associated demand for improved reliability, dust covers for ball joints are now required to have even higher ozone resistance.That is, in the past, a chloroprene rubber composition that did not crack for 500 hours or more in a static ozone degradation test (JIS K 6259) with an ozone concentration of 50 pphm and 30% elongation was sufficient, but in recent years this has not been sufficient, and there has been a demand for dust covers made of a chloroprene rubber composition that does not crack for 500 hours or more in a dynamic ozone degradation test (JIS K 6259) with an ozone concentration of 50 pphm and 0 to 30% elongation.
[0007] The present invention has been made in consideration of the above-mentioned points, and an object of the present invention is to provide a chloroprene rubber composition used in a dust cover for a ball joint, which uses chloroprene rubber to improve heat resistance and ozone resistance, and which has excellent adhesion to metal and further high ozone resistance. [Means for solving the problem]
[0008] In order to achieve this object, the present inventors conducted extensive research and found that by blending 3.5 to 10 parts by weight of a hydrocarbon wax having a melting point of 90°C or less and 5 to 12 parts by weight of an aromatic secondary amine-based antiaging agent with 100 parts by weight of chloroprene rubber, the rubber has good adhesion to metal and no cracks are generated for 500 hours or more in a dynamic ozone degradation test (JIS K 6259) with an ozone concentration of 50 pphm and 0 to 30% elongation, thereby completing the present invention.
[0009] That is, the chloroprene rubber composition of the first invention is characterized in that 3.5 to 10 parts by weight, preferably 4 to 6 parts by weight, of a hydrocarbon wax having a melting point of 90°C or less and 5 to 12 parts by weight, preferably 8 to 10 parts by weight of an aromatic secondary amine-based antiaging agent are blended with respect to 100 parts by weight of chloroprene rubber. A second invention is characterized in that, in the first invention, the hydrocarbon wax having a melting point of 90° C. or less is a microcrystalline wax. The third invention is characterized in that, in the first or second invention, the aromatic secondary amine-based antiaging agent is N-phenyl-N'-isopropyl-p-phenylenediamine or N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine. A fourth invention is characterized in that it is a dust cover for a ball joint made of the chloroprene rubber composition according to the first invention. Effect of the Invention
[0010] According to the present invention, by blending 3.5 to 10 parts by weight of a hydrocarbon wax having a melting point of 90°C or less and 5 to 12 parts by weight of an aromatic secondary amine-based antiaging agent with 100 parts by weight of chloroprene rubber, it is possible to obtain a chloroprene rubber composition which has excellent adhesion to metal and which does not crack for 500 hours or more in a dynamic ozone degradation test (JIS K 6259) of 0 to 30% elongation at an ozone concentration of 50 pphm. By applying this composition to a dust cover for a ball joint, it is possible to provide a dust cover with even higher ozone resistance. [Brief description of the drawings]
[0011] [Figure 1] 1 is an overall vertical sectional view of a ball joint to which the present invention is applied; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described in detail. 1 is used, for example, between the steering device and wheels of an automobile, and has a housing 2 on the steering device side, a bearing member 3 provided in the housing 2, and a ball stud 4 having at one end a ball portion 4a that is supported by the bearing member 3 so as to be tiltable and rotatable. A knuckle arm 5 on the wheel side is fixed to the shaft portion 4b of the ball stud 4 by fastening means 6a, 6b, so that the knuckle arm 5 is connected to the housing 2 so as to be tiltable and rotatable with the ball portion 4a as a fulcrum.
[0013] In this ball joint 1, a rubber dust cover 7 is attached between the housing 2 and the knuckle arm 5 to prevent foreign matter such as dust and rainwater from entering from the outside. The dust cover 7 is generally shaped like a cylindrical bag, and is integrally formed with a large diameter portion 7a at one end, a small diameter portion 7b at the other end, and a central portion 7c that bulges outward. The large diameter portion 7a is press-fitted and fixed into the seat portion 2a of the housing 2, and the small diameter portion 7b is press-fitted and fixed into the shaft portion 4b of the ball stud 4 so as to contact the knuckle arm 5. To ensure this press-fitting and fixing, metal rings 8a and 8b are provided inside the large diameter portion 7a and the small diameter portion 7b of the dust cover 7, respectively. Grease is sealed inside the dust cover 7 to lubricate the space between the bearing member 3 of the housing 2 and the ball portion 4a of the ball stud 4.
[0014] The chloroprene rubber composition of the present invention is suitable for use in the dust cover 7 of the ball joint 1 constructed as described above, and a new compounding is adopted in the rubber composition in order to further improve ozone resistance while ensuring excellent adhesion between the rubber and the metal ring. That is, the present invention is obtained by blending 3.5 to 10 parts by weight, preferably 4 to 6 parts by weight, of a hydrocarbon wax having a melting point of 90°C or less, and 5 to 12 parts by weight, preferably 8 to 10 parts by weight, of an aromatic secondary amine-based antiaging agent, per 100 parts by weight of chloroprene rubber.
[0015] Chloroprene rubber is a rubber obtained by polymerizing chloroprene (2-chloro-1,3-butadiene), and is a general-purpose special synthetic rubber that is excellent in heat aging resistance, weather resistance, chemical resistance, etc. In the present invention, the chloroprene rubber may be a commercially available product such as Denka Chloroprene M-40, M-120, EM-40, S-40V, DCR-30, DCR-35, DCR-36, DCR-37, DCR-40A, DCR-42A, DCR-66, PM-40NS (all of which are product names manufactured by Denka Co., Ltd.), Skyprene 505, 630, 640, B-5, B-5A, B-10, B-10H, B-11, B-12, B-25, B-30, B-31, E-20, E-20H, E-33, R-10, R-22, TSR-41, TSR-42, TSR-43, TSR-44, TSR-45, TSR-46, TSR-47, TSR-48, TSR-49, TSR-50, TSR-51, TSR-52, TSR-53, TSR-54, TSR-55, TSR-56, TSR-57, TSR-58, TSR-59 ...9, TSR-59, TSR-59, TSR-59, TSR-59, TSR-59, TSR-59, TSR-59, TSR-59, TSR-59, TSR-59, TSR-59, TSR-59, TSR-5 Examples include SR-42, TSR-44, TSR-48, TSR-51, TSR-52, TSR-54, TSR-57, TSR-61, TSR-70, P-90, Y-30S, Y-31 (all of which are product names manufactured by Tosoh Corporation), Showpren GW, SND5, SND22, SND37, TRT, TW, TW100, W, WB, WHV, WHV100, WK, WRT, WXJ, WXJK (all of which are product names manufactured by Showa Denko K.K.), and these chloroprene rubbers are used alone or in the form of a blend of several grades.
[0016] The hydrocarbon wax, which is an essential component in the present invention, is classified into high-purity paraffin wax containing linear paraffin as the main component, and microcrystalline wax containing a large number of minor components such as branched paraffins and cyclic paraffins in addition to linear paraffin. Examples of paraffin waxes include paraffin wax 115°F (melting point 48°C), 120°F (melting point 50°C), 125°F (melting point 53°C), 130°F (melting point 56°C), 135°F (melting point 59°C), 140°F (melting point 61°C), 145°F (melting point 63°C), 150°F (melting point 66°C), and 155°F (melting point 69°C) (all product names manufactured by Nippon Seiro Co., Ltd.). Examples of microcrystalline waxes include Suntite R (melting point 68°C), Suntite C (melting point 72°C), Suntite S (melting point 73°C), Suntite Z (melting point 81°C) (all product names manufactured by Seiko Chemical Co., Ltd.), Sunnock P (melting point 70°C), Sunnock (melting point 77°C) (all product names manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), and among hydrocarbon waxes, microcrystalline wax has better ozone resistance than paraffin wax. In the present invention, a hydrocarbon wax having a melting point of 90° C. or less is used, and if a wax having a melting point higher than this is used, it becomes difficult to achieve the effect of ozone resistance. The melting point of the microcrystalline wax referred to here was measured by TGA (thermogravimetric analysis).
[0017] In the present invention, the hydrocarbon wax is used in a ratio of 3.5 to 10 parts by weight per 100 parts by weight of the chloroprene rubber. If the wax is used in a ratio greater than this, the adhesion to metal deteriorates, while if it is used in a ratio less than this, it becomes difficult to achieve the effect of ozone resistance.
[0018] The present invention is characterized in that the aromatic secondary amine-based antiaging agent is N-phenyl-N'-isopropyl-p-phenylenediamine or N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine. That is, the aromatic secondary amine-based antiaging agent, which is another essential component in the present invention, is a compound in which two hydrogen atoms of ammonia are substituted with a hydrocarbon group or an aromatic atomic group, and N-phenyl-N'-isopropyl-p-phenylenediamine (Nocrac 810-NA (trade name of Ouchi Shinko Chemical Industry Co., Ltd.), Ozonone 3C (trade name of Seiko Chemical Industry Co., Ltd.), Antage 3C (trade name of Kawaguchi Chemical Industry Co., Ltd.)) or N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (Nocrac 6C (trade name of Ouchi Shinko Chemical Industry Co., Ltd.), Ozonone 6C (trade name of Seiko Chemical Industry Co., Ltd.), Antage 6C (trade name of Kawaguchi Chemical Industry Co., Ltd.)) are preferably used. Other examples include phenyl-1-naphthylamine (Nocrac PA (trade name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)), octylated diphenylamine (Nocrac AD-F (trade name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), Nonflex OD-3 (trade name, manufactured by Seiko Chemical Co., Ltd.)), 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (Nocrac CD (trade name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)), p-(p-toluenesulfonylamido)diphenylamine (Nocrac TD (trade name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)), N,N'-di-2-naphthyl-p-furan Phenylenediamine (Nocrac White (product name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), Nonflex F (product name, manufactured by Seiko Chemical Industry Co., Ltd.)), N,N'-diphenyl-p-phenylenediamine (Nocrac DP (product name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), Nonflex H (product name, manufactured by Seiko Chemical Industry Co., Ltd.), Antage DP (product name, manufactured by Kawaguchi Chemical Industry Co., Ltd.)), N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine (Nocrac G-1 (product name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)), and the like may also be used.
[0019] In the present invention, the aromatic secondary amine-based antioxidant is used in a ratio of 5 to 12 parts by weight based on 100 parts by weight of the chloroprene rubber. If the aromatic secondary amine-based antioxidant is used in a ratio greater than this, problems such as scorching may occur, while if it is used in a ratio less than this, it becomes difficult to achieve the effect of ozone resistance.
[0020] In addition to the essential components of the hydrocarbon wax and aromatic secondary amine antioxidant, various compounding agents generally used in the rubber industry, such as a reinforcing material, an extender filler, a vulcanizing agent, a vulcanization accelerator, an acid acceptor, and an antioxidant, are appropriately added to the chloroprene rubber composition.
[0021] In the present invention, 0 to 80 parts by weight, preferably 0 to 40 parts by weight, of a reinforcing agent such as carbon black or a silica-based filler may be added to 100 parts by weight of the chloroprene rubber. The use of more than 80 parts by weight is not preferred because it deteriorates the kneadability of the rubber.
[0022] Examples of carbon black include SAF carbon (average particle size 18 to 22 μm) such as Asahi #90 (trade name of Asahi Carbon Co., Ltd.), Show Black N110, N134 (all of which are trade names of Showa Cabot Co., Ltd.), Seast 9 (trade name of Tokai Carbon Co., Ltd.), and Diamond Black-A (trade name of Mitsubishi Chemical Co., Ltd.), SAF-HS carbon (average particle size about 20 μm) such as Seast 9H (trade name of Tokai Carbon Co., Ltd.), Asahi #80 (trade name of Asahi Carbon Co., Ltd.), Show Black N220 (trade name of Showa Cabot Co., Ltd.), Seast 6 (trade name of Tokai Carbon Co., Ltd.), Diamond Black I,ISAF carbon (average particle size 19-29μm) such as N220M (all of the above are product names manufactured by Mitsubishi Chemical Corporation), N-339 carbon (average particle size 24μm) such as Asahi #75 (product name manufactured by Asahi Carbon Co., Ltd.), Show Black N339 (product name manufactured by Showa Cabot Co., Ltd.), Seast KH (product name manufactured by Tokai Carbon Co., Ltd.), and Dia Black N339 (product name manufactured by Mitsubishi Chemical Corporation), ISAF-LS carbon (average particle size 21-24μm) such as Asahi #80L (product name manufactured by Asahi Carbon Co., Ltd.), Show Black N219 (product name manufactured by Showa Cabot Co., Ltd.), Seast 600 (product name manufactured by Tokai Carbon Co., Ltd.), and Dia Black LI (product name manufactured by Mitsubishi Chemical Corporation), Asahi #78 (product name manufactured by Asahi Carbon Co., Ltd.), Seast 5H (product name manufactured by Tokai Carbon Co., Ltd.), and Dia Black I-ISAF-HS carbon (average particle size 21-31 μm) such as II (product name of Mitsubishi Chemical Corporation), HAF carbon (26-30 μm) such as Asahi #70 (product name of Asahi Carbon Co., Ltd.), Show Black N330 (product name of Showa Cabot Co., Ltd.), Seast S (product name of Tokai Carbon Co., Ltd.), and Dia Black-H (product name of Mitsubishi Chemical Corporation), HAF-HS carbon (average particle size 22-30 μm) such as Asahi #70H (product name of Asahi Carbon Co., Ltd.), Seast 3H (product name of Tokai Carbon Co., Ltd.), and Dia Black-SH (product name of Mitsubishi Chemical Corporation), Asahi #70IH (product name of Asahi Carbon Co., Ltd.), Show Black N351 (product name of Showa Cabot Co., Ltd.), Seast NH (product name of Tokai Carbon Co., Ltd.), and HAF-HS carbon (average particle size 22-30 μm) such as ... N-351 carbon (average particle size: about 29 μm) such as Asahi 70L (product name of Asahi Carbon Co., Ltd.), Show Black N326 (product name of Showa Cabot Co., Ltd.), Seast 300 (product name of Tokai Carbon Co., Ltd.), Dia Black LH (product name of Mitsubishi Chemical Co., Ltd.) and other HAF-LS carbon (average particle size: 25 to 29 μm) such as Asahi 70IN (product name of Asahi Carbon Co., Ltd.), Seast N (product name of Tokai Carbon Co., Ltd.) and other LI-HAF carbon (average particle size: about 29 μm) such as Asahi 60H (product name of Asahi Carbon Co., Ltd.), Show Black MAF (product name of Showa Cabot Co., Ltd.), Seast 116 (product name of Tokai Carbon Co., Ltd.), Dia Black N550M, SF,Examples include MAF carbons (average particle size 30-35 μm) such as Asahi #60 and #60U (both of which are product names manufactured by Asahi Carbon Co., Ltd.), Show Black N550 (product name manufactured by Showa Cabot Co., Ltd.), Seast SO and FM (both of which are product names manufactured by Tokai Carbon Co., Ltd.), and Dia Black-E and EY (both of which are product names manufactured by Mitsubishi Chemical Co., Ltd.), FEF carbons (average particle size 40-52 μm) such as Asahi #50, #50U and #51 (both of which are product names manufactured by Asahi Carbon Co., Ltd.), Seast S (product name manufactured by Tokai Carbon Co., Ltd.), and Dia Black R (product name manufactured by Mitsubishi Chemical Co., Ltd.), SRF carbons (average particle size 58-94 μm) such as Asahi #35 (product name manufactured by Asahi Carbon Co., Ltd.), and Dia Black N760M and LR (both of which are product names manufactured by Mitsubishi Chemical Co., Ltd.), and GPF carbons (49-84 μm) such as Asahi #55 (product name manufactured by Asahi Carbon Co., Ltd.), and Seast V (product name manufactured by Tokai Carbon Co., Ltd.). ,
[0023] Examples of silica-based fillers include dry silica such as Aerosil 130, 200, 300, 380, R972, and R974 (all of which are product names manufactured by Nippon Aerosil Co., Ltd.) and Reolosil QS13, QS30, QS38, and QS102 (all of which are product names manufactured by Tokuyama Corporation); Carplex #67, #80, #100, #1120, XR, 22S, CS-5, and CS-7 (all of which are product names manufactured by Shionogi Pharmaceutical Co., Ltd.); Silton A and R-2 (all of which are product names manufactured by Mizusawa Chemical Industry Co., Ltd.); Tokuseal AL-1, Gu, U, UR, and US (all of which are product names manufactured by Tokuyama Corporation); Nipsil AQ, ER, LP, NA, NP, NS-K, and VN3 (all of which are product names manufactured by Nippon Silica Co., Ltd.); and Ultrasil Examples include wet silica such as VN3 (trade name manufactured by Degussa, Germany) and Hi-Sil233 (trade name manufactured by PPG Industries, USA).
[0024] In addition, activated calcium carbonate such as Hakuenka CC, DD, O, U (all of which are product names manufactured by Shiraishi Kogyo Co., Ltd.), special calcium carbonate such as Hakuenka A, AA (all of which are product names manufactured by Shiraishi Kogyo Co., Ltd.), magnesium silicate such as Mistron Paper (product name manufactured by Nippon Mistron Co., Ltd.), magnesium silicate such as Hitron, Hitron A, Microlite, US-100, US-150S, US-150SS, Hilac, Hilac SS (all of which are product names manufactured by Takehara Chemical Industry Co., Ltd.), and the like may be used in combination as appropriate.
[0025] If necessary, about 5 to 100 parts by weight of an extender filler may be added to the chloroprene rubber composition of the present invention for the purpose of dimensional stability and low cost, per 100 parts by weight of the base rubber.
[0026] Examples of the extender filler include light calcium carbonate such as Green Ball (product name of Inoue Sekikogyo Co., Ltd.), Tama Pearl TP-121, TP-121R, TP222H, TP-222HS, TP-123, TP-123CS (all of which are product names of Okutama Kogyo Co., Ltd.), and Silver W (product name of Shiraishi Kogyo Co., Ltd.), Whiteron SSB, SB, S (all of which are product names of Shiraishi Calcium Co., Ltd.), Sunlight #100, #300, #700, #800, #1000, #1500, #2000, #2200, #2500 (all of which are product names of Takehara Chemical Industry Co., Ltd.), and NS#100, NS Heavy calcium carbonate such as #200, NS#400, NS#600, NS#1000, NS#2300, NS#2500, NS#2700, NS#3000, SS#30, SS#80, NN#200, NN#500 (all of which are product names manufactured by Nitto Funka Kogyo Co., Ltd.) and Super S, SS, SSS, 4S, #1500, #1700, #2000 (all of which are product names manufactured by Maruo Calcium Co., Ltd.), JET-S (product name manufactured by Asada Flour Milling Co., Ltd.), Crystallite AA, VX-S, VX-S-2, VX-SR (all of which are product names manufactured by Tatsumori Co., Ltd.), and Min-U-Sil 5, 10, 15, 30 (all of which are product names manufactured by US Silica (USquartz powder such as Imsil A-10, A-15, A-25, A-108 (all of which are product names of Illinois Minerals, Inc., USA); wollastonite (calcium metasilicate) such as JA-30W, 325M (all of which are product names of Asada Flour Milling Co., Ltd., USA) and NYAD325, 400, 1250, G (all of which are product names of NYCO, Inc., USA); Celite 270, 281, 501, 503, 505, 535, 545, 560, 577, FC, SSC, Super Examples include diatomaceous earth such as Floss and SnowFloss (all trade names manufactured by Johns-Manville (USA)), Radiolite #100, #200, #300, #500, #500S, #600, #700, #800, #800-S, #900, F, SPF, Fine Flow A, and Fine Flow B (all trade names manufactured by Showa Chemical Industry Co., Ltd.), zinc oxide such as zinc oxide type 2 (trade name manufactured by Sakai Chemical Industry Co., Ltd.), aluminum sulfate, barium sulfate, calcium sulfate, titanium oxide, and molybdenum disulfide, and usually one or several types are used in combination with a reinforcing filler.
[0027] As the vulcanization accelerator, a thiourea-based compound is used, and specific examples thereof include thiocarbamate (Noccela C (product name of Ouchi Shinko Chemical Industry Co., Ltd.)), ethylene thiourea (Accel 22-S (product name of Kawaguchi Chemical Industry Co., Ltd.), Suncerer 22-C (product name of Sanshin Chemical Industry Co., Ltd.)), diethyl thiourea (Noccela EUR (product name of Ouchi Shinko Chemical Industry Co., Ltd.), Accel EUR (product name of Kawaguchi Chemical Industry Co., Ltd.), Suncerer EUR (product name of Sanshin Chemical Industry Co., Ltd.)), dibutyl thiourea (Accel BUR-F (product name of Kawaguchi Chemical Industry Co., Ltd.), Suncerer BUR (product name of Sanshin Chemical Industry Co., Ltd.)), dilauryl thiourea (Accel LUR (product name of Kawaguchi Chemical Industry Co., Ltd.)), trimethyl thiourea (Noccela TMU (product name of Ouchi Shinko Chemical Industry Co., Ltd.), Suncerer TMU (product name of Sanshin Chemical Industry Co., Ltd.)), and the like. These thiourea compounds are used in a proportion of about 0.25 to 5 parts by weight, preferably 0.5 to 1 part by weight, per 100 parts by weight of the chloroprene rubber.
[0028] As the vulcanization accelerator, dibenzothiazyl disulfide (Noccela DM (trade name of Ouchi Shinko Chemical Industry Co., Ltd.), Accel DM (trade name of Kawaguchi Chemical Industry Co., Ltd.), Suncerer DM (trade name of Sanshin Chemical Industry Co., Ltd.), tetramethylthiuram monosulfide (Noccela TS (trade name of Ouchi Shinko Chemical Industry Co., Ltd.), Accel TS (trade name of Kawaguchi Chemical Industry Co., Ltd.), Suncerer TS (trade name of Sanshin Chemical Industry Co., Ltd.)), tetramethylthiuram disulfide (Noccela TT (trade name of Ouchi Shinko Chemical Industry Co., Ltd.), Accel TMT (trade name of Kawaguchi Chemical Industry Co., Ltd.), Suncerer TT (trade name of Sanshin Chemical Industry Co., Ltd.)) and the like are used in an amount of about 0.5 to 1 part by weight per 100 parts by weight of chloroprene rubber. If the amount of crosslinking accelerator is more than this, the storage stability of the unvulcanized rubber is impaired, which is not preferable.
[0029] It is necessary to add a metal oxide to the composition of the present invention in order to improve processing stability, adjust the vulcanization rate, or act as an acid acceptor to improve aging resistance. Usually, about 4 parts by weight of magnesium oxide and about 5 parts by weight of zinc oxide are added per 100 parts by weight of chloroprene rubber.
[0030] In the present invention, in order to improve roll workability and mold releasability, fatty acids such as stearic acid and zinc stearate or metal salts thereof may be added in an amount of about 0.5 to 5 parts by weight based on 100 parts by weight of the chloroprene rubber.
[0031] In the present invention, a plasticizer may be added to adjust hardness or impart plasticity. There are no particular limitations on the plasticizer as long as it is compatible with chloroprene rubber, and specific examples include vegetable oils such as rapeseed oil, phthalate plasticizers, DUP (diundecyl phthalate), DOS (dioctyl sebacate), DOA (dioctyl adipate), ester plasticizers, ether ester plasticizers, thioether plasticizers, aromatic oils, naphthenic oils, etc., and the amount of the plasticizer added is about 5 to 50 parts by weight based on 100 parts by weight of chloroprene rubber.
[0032] The chloroprene rubber composition prepared by the above-mentioned blending is vulcanized and molded, for example, by press crosslinking at about 150-200° C. for about 3-30 minutes, to produce a dust cover 7 for a ball joint 1 as shown in FIG. EXAMPLES
[0033] Next, examples of the present invention are shown in Tables 1 to 4.
[0034] [Table 1]
[0035] [Table 2]
[0036] [Table 3]
[0037] [Table 4]
[0038] Example 1 Chloroprene rubber (Showa Denko's Showpren W) 100 parts by weight Zinc oxide 5 parts by weight Magnesium oxide 4 parts by weight FEF carbon black 40 parts by weight Plasticizer (rapeseed oil) 20 parts by weight Vulcanization accelerator (Axel 22-S manufactured by Kawaguchi Chemical) 1 part by weight Vulcanization accelerator (Noccela TT, manufactured by Ouchi Shinko Chemical) 1 part by weight Anti-aging agent (Nocrac 810-NA, manufactured by Ouchi Shinko Chemical) 5 parts by weight Wax (Santite S, manufactured by Seiko Chemical) 3.5 parts by weight
[0039] The above components were kneaded by an open roll, and the resulting chloroprene rubber composition was crosslinked by heating at 170° C. for 10 minutes to prepare a test piece having a thickness of 2 mm. Additionally, the obtained chloroprene rubber composition was injection molded to mold a dust cover for a ball joint as shown in FIG.
[0040] The test pieces thus created were used to evaluate the specimens in a static ozone degradation test (JIS K 6259) with an ozone concentration of 50 ppm and 30% elongation, and in a dynamic ozone degradation test (JIS K 6259) with an ozone concentration of 50 ppm and 0 to 30% elongation. In both the static and dynamic ozone degradation tests, the specimens were found to be NC (no cracks) after 500 hours or more. Furthermore, in the molded dust cover, the rubber and the metal ring were securely bonded together, and no particular problems were found.
[0041] Example 2 The blending amount of the antioxidant Nocrac 810-NA manufactured by Ouchi Shinko Chemical Co., Ltd. was changed to 8 parts by weight from Example 1, and evaluation was performed in the same manner as in Example 1. In both the static ozone degradation test and the dynamic ozone degradation test, the result was NC (no cracks) after 500 hours or more. As in Example 1, the rubber and metal ring of the molded dust cover were securely bonded together, and no particular problems were found.
[0042] [Examples 3 to 28] Similarly, when the composition of the antioxidant and wax was changed to that shown in the table and evaluated (in Examples 17 to 28, the wax was changed to Sunnock manufactured by Ouchi Shinko Chemical), both the static ozone degradation test and the dynamic ozone degradation test were NC (no cracks) after 500 hours or more. As in Example 1, the rubber and metal ring of the molded dust cover were securely bonded together, and no particular problems were found.
[0043] As described above, it is possible to produce a dust cover for a ball joint made of a chloroprene rubber composition. Next, comparative examples for the above examples are shown in Tables 5 to 7.
[0044] [Table 5]
[0045] [Table 6]
[0046] [Table 7]
[0047] [Comparative Examples 1 to 17] When the results shown in Tables 5 to 7 were evaluated in the same manner as in the Examples, the static ozone degradation test was NC (no cracks) after 500 hours or more, but the dynamic ozone degradation test showed cracks at the times shown in the tables, indicating poor durability.
[0048] From the above results, the effect of the present invention, that is, by blending 3.5 to 10 parts by weight of a hydrocarbon wax having a melting point of 90°C or less and 5 to 12 parts by weight of an aromatic secondary amine antioxidant with respect to 100 parts by weight of chloroprene rubber, no cracks were generated for 500 hours or more in the dynamic ozone deterioration test (JIS K 6259), and the effect of excellent ozone resistance was confirmed. Therefore, by applying this rubber composition to a dust cover for a ball joint, a high-quality dust cover that does not generate cracks due to ozone for a long period of time can be obtained. This makes it possible in the present invention to provide a dust cover for a ball joint made of the chloroprene rubber composition. [Industrial Applicability]
[0049] The crosslinked rubber using the chloroprene rubber composition of the present invention has good ozone resistance, particularly excellent dynamic ozone resistance, and therefore can be effectively applied not only to dust covers for ball joints but also to various other cover members. [Explanation of symbols]
[0050] 1 Ball joint 2. Housing 2a Seat area 3 Bearing materials 4 Ball Studs 4a Ball section 4b Shaft 5 Knuckle Arm 6a, 6b Fastening means 7 Dust cover 7a Large diameter section 7b Small diameter section 7c central part 8a,8b Metal ring
Claims
1. A chloroprene rubber composition comprising 100 parts by weight of chloroprene rubber, 3.5 to 10 parts by weight, preferably 4 to 6 parts by weight, of a hydrocarbon wax having a melting point of 90°C or less, and 5 to 12 parts by weight, preferably 8 to 10 parts by weight, of an aromatic secondary amine-based antiaging agent.
2. 2. The chloroprene rubber composition according to claim 1, wherein the hydrocarbon wax having a melting point of 90° C. or less is a microcrystalline wax.
3. 3. The chloroprene rubber composition according to claim 1, wherein the aromatic secondary amine-based antioxidant is N-phenyl-N'-isopropyl-p-phenylenediamine or N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine.
4. A dust cover for a ball joint, comprising the chloroprene rubber composition according to claim 1.
Citation Information
Patent Citations
Chloroprene rubber constant velocity joint boot
JP2000291798A
Dust cover for ball joint
JP2011252519A