Fe-BASED AMORPHOUS ALLOY RIBBON FOR Fe-BASED NANOCRYSTAL ALLOY, AND METHOD FOR PRODUCING Fe-BASED AMORPHOUS ALLOY RIBBON FOR Fe-BASED NANOCRYSTAL ALLOY

By controlling the thickness and space factor of Fe-based amorphous alloy ribbons and using atmospheric gas injection, the manufacturing process minimizes surface irregularities, ensuring continuous production with improved magnetic properties and reduced thickness.

JP2024165702APending Publication Date: 2024-11-28PROTERIAL LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023082109
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing methods for producing Fe-based amorphous alloy ribbons result in air pockets forming on the surface, leading to a decrease in space factor when the ribbon thickness is reduced, which affects the magnetic properties and continuity of the manufacturing process.

Method used

The Fe-based amorphous alloy ribbon is manufactured with a thickness of 11 μm to 14 μm and a space factor of 73% or more, using a single roll method with controlled atmospheric gas injection to minimize surface irregularities and improve adhesion to the cooling roll.

Benefits of technology

This approach maintains a high space factor and reduces surface roughness, allowing for continuous production of ribbons with enhanced magnetic permeability and reduced thickness, preventing breakage and improving magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165702000001_ABST
    Figure 2024165702000001_ABST
Patent Text Reader

Abstract

To provide an Fe-based amorphous alloy ribbon for Fe-based nanocrystal alloy that can suppress the reduction in space factor even if a thickness of the Fe-based amorphous alloy ribbon or the Fe-based nanocrystal alloy ribbon is reduced, and a method for producing the Fe-based amorphous alloy ribbon for Fe-based nanocrystal alloy.SOLUTION: An Fe-based amorphous alloy ribbon for Fe-based nanocrystal alloy has a thickness of 11 μm or more and 14 μm or less, exhibiting a space factor of 73% or more as measured in accordance with IEC60404-8-11:2018.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to Fe-based amorphous alloy ribbons for Fe-based nanocrystalline alloys, which are used in various transformers, various reactors and choke coils, noise suppression components, pulse power magnetic components used in laser power supplies and accelerators, etc., communication pulse transformers, various motor cores, various generators, various magnetic sensors, antenna cores, various current sensors, magnetic shields, etc., and a manufacturing method for Fe-based amorphous alloy ribbons for Fe-based nanocrystalline alloys. [Background technology]

[0002] Silicon steel, ferrite, amorphous alloys, nanocrystalline alloys, etc. are known as soft magnetic materials used in various transformers, various reactors, choke coils, noise suppression parts, laser power supplies, pulse power magnetic parts for accelerators, etc. Ferrite materials have problems with low saturation magnetic flux density and poor temperature characteristics, and ferrite is prone to magnetic saturation and is unsuitable for high power applications designed to have a large operating magnetic flux density. Silicon steel sheets are inexpensive materials and have a high magnetic flux density, but have the problem of large core loss for high frequency applications. Amorphous alloys are usually manufactured by quenching from the liquid or gas phase. Since they have no crystal grains, Fe-based and Co-based amorphous alloys are essentially free of magnetocrystalline anisotropy and are known to exhibit excellent soft magnetic properties. They are used in power transformer cores, choke coils, magnetic heads, current sensors, etc. However, Fe-based amorphous alloys have a problem with large magnetostriction, which means that they do not achieve the same high magnetic permeability as Co-based amorphous alloys, while Co-based amorphous alloys have low magnetostriction and high magnetic permeability, but have a problem with their low saturation magnetic flux density of 1T or less.

[0003] Nanocrystalline alloys are known to have excellent soft magnetic properties comparable to those of Co-based amorphous alloys and high saturation magnetic flux density comparable to those of Fe-based amorphous alloys, and are used in noise countermeasure components such as common mode choke coils, high frequency transformers, pulse transformers, current sensors, and other magnetic cores. Representative compositions include Fe-Cu-(Nb, Ti, Zr, Hf, Mo, W, Ta)-Si-B alloys and Fe-Cu-(Nb, Ti, Zr, Hf, Mo, W, Ta)-B alloys described in Patent Documents 1 and 2. These Fe-based nanocrystalline alloys are usually produced by quenching from the liquid phase or gas phase to form an amorphous alloy, which is then microcrystallized by heat treatment. Methods for quenching from the liquid phase include the single roll method, the twin roll method, the centrifugal quenching method, the spinning in a rotating liquid method, the atomization method, the cavitation method, and the like. Also, methods of quenching from the gas phase include sputtering, vapor deposition, ion plating, etc. Fe-based nanocrystalline alloys are made by microcrystallizing amorphous alloys produced by these methods, and are known to have almost no thermal instability like amorphous alloys, and to have excellent soft magnetic properties with high saturation magnetic flux density and low magnetostriction comparable to Fe-based amorphous alloys. Furthermore, nanocrystalline alloys are known to have little change over time and excellent temperature characteristics.

[0004] When amorphous alloy ribbons made of an amorphous alloy are mass-produced, they are generally manufactured by a molten metal super-quenching method such as the single roll method. In the single roll method, the molten alloy is discharged onto the surface of a cooling roll whose outer circumferential surface is, for example, a copper (Cu) alloy, and is rapidly cooled and solidified. In this way, an amorphous alloy ribbon is manufactured. Then, a nanocrystalline alloy ribbon made of a nanocrystalline alloy is manufactured by heat treating and crystallizing this amorphous alloy ribbon. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 4-4393 [Patent Document 2] Japanese Patent Application Publication No. 1-242755 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, as semiconductor devices have become more frequent, there has been a demand for soft magnetic materials with low loss at high frequencies, as well as higher efficiency, smaller size, and lighter weight. Therefore, it is considered that the loss due to eddy currents can be reduced by reducing the thickness of the Fe-based nanocrystalline alloy ribbon manufactured from the Fe-based amorphous alloy ribbon. However, when manufacturing (casting) the Fe-based amorphous alloy ribbon, air or atmospheric gases are entrained at the interface between the molten alloy and the cooling roll, forming recesses (air pockets) on the surface of the Fe-based amorphous alloy ribbon. When the Fe-based amorphous alloy ribbon is thin, the reduction in the space factor due to the effect of the recesses becomes significant.

[0007] Therefore, the present invention aims to provide an Fe-based amorphous alloy ribbon for Fe-based nanocrystalline alloys, and a manufacturing method for Fe-based amorphous alloy ribbon for Fe-based nanocrystalline alloys, which can suppress a decrease in the space factor even if the thickness of the Fe-based amorphous alloy ribbon or Fe-based nanocrystalline alloy ribbon is reduced. [Means for solving the problem]

[0008] The present invention aims to solve the above-mentioned problems by providing an Fe-based amorphous alloy ribbon for use in an Fe-based nanocrystalline alloy, the ribbon having a thickness of 11 μm or more and 14 μm or less and a space factor of 73% or more as measured in accordance with IEC60404-8-11:2018. Effect of the Invention

[0009] The present invention provides an Fe-based amorphous alloy ribbon for an Fe-based nanocrystalline alloy, and a method for producing an Fe-based amorphous alloy ribbon for an Fe-based nanocrystalline alloy, which can suppress a decrease in the space factor even if the thickness of the Fe-based amorphous alloy ribbon or the Fe-based nanocrystalline alloy ribbon is reduced. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view conceptually showing an example of an Fe-based amorphous alloy ribbon manufacturing apparatus by a single-roll method, which is suitable for an embodiment of the present invention. [Diagram 2] FIG. 2 is an image of the roll surface obtained by an optical microscope in Example 4. [Diagram 3] FIG. 3 is an image of the roll surface obtained by an optical microscope in Comparative Example 1.

MODE FOR CARRYING OUT THE INVENTION

[0011] Hereinafter, the present invention will be specifically described.

[0012] In this specification, the Fe-based amorphous alloy ribbon refers to a ribbon (thin strip) made of an Fe-based amorphous alloy. Further, in this specification, the Fe-based amorphous alloy refers to an amorphous alloy in which the element with the highest content (atomic%) among the contained metal elements is Fe (iron).

[0013] In this specification, the Fe-based nanocrystalline alloy ribbon refers to a ribbon (thin strip) made of an Fe-based nanocrystalline alloy. Further, in this specification, the Fe-based nanocrystalline alloy refers to a nanocrystalline alloy in which the element with the highest content (atomic%) among the contained metal elements is Fe (iron).

[0014] The Fe-based amorphous alloy ribbon for an Fe-based nanocrystalline alloy according to the present disclosure is an Fe-based amorphous alloy ribbon for manufacturing an Fe-based nanocrystalline alloy by crystallizing the Fe-based amorphous alloy ribbon. Hereinafter, the "Fe-based amorphous alloy ribbon for an Fe-based nanocrystalline alloy" according to the present disclosure will also be simply referred to as the "Fe-based amorphous alloy ribbon".

[0015] <Fe-based amorphous alloy ribbon>

[0016] The Fe-based amorphous alloy ribbon is a cooling body of molten metal applied to the surface of a cooling roll during production, and one surface in contact with the cooling roll is formed as the roll surface, and the other surface not in contact with the cooling roll is formed as the free surface. The roll surface and the free surface can be visually distinguished by the gloss of the surface of the Fe-based amorphous alloy ribbon. The roll surface is less glossy than the free surface because it has the irregularities of the cooling roll surface transferred thereto. Therefore, of the two surfaces of the Fe-based amorphous alloy ribbon, the one that is glossier is the free surface, and the one that is not glossy is the roll surface.

[0017] The Fe-based amorphous alloy ribbon has a thickness of 11μm or more and 14μm or less, and a space factor of 73% or more. By making the thickness of the Fe-based amorphous alloy ribbon 11μ or more, the Fe-based amorphous alloy ribbon is less likely to break during casting, and can be wound continuously. By making the thickness of the Fe-based amorphous alloy ribbon 14μm or less, the current loss is reduced and the magnetic permeability in the high frequency range can be increased. The thickness of the Fe-based amorphous alloy ribbon can be calculated from the weight of a 2000mm long sample taken from the casting direction, as well as the ribbon length, ribbon width, and ribbon density, in accordance with IEC 60404-8-11:2018. The space factor of the Fe-based amorphous alloy ribbon can be calculated by stacking 20 sheets of Fe-based amorphous alloy ribbon cut to a length of 100 mm into a laminate in accordance with IEC 60404-8-11:2018, and calculating the ratio of the maximum thickness of the laminate measured with a micrometer to the thickness of the Fe-based amorphous alloy ribbon.

[0018] The Fe-based amorphous alloy ribbon preferably has a dimension in the width direction (direction perpendicular to the casting direction) of 30 mm or more and 300 mm or less.

[0019] The Fe-based amorphous alloy ribbon preferably has an arithmetic mean roughness Ra of the roll surface of 0.1 μm or more and 0.6 μm or less. By setting the arithmetic mean roughness Ra of the roll surface of the Fe-based amorphous alloy ribbon to 0.6 μm or less, the Fe-based amorphous alloy ribbon can have a roll surface with less unevenness. The arithmetic mean roughness Ra is measured in accordance with JIS B 0601:2001, with an evaluation length of 4.0 mm, a cutoff value of 0.8 mm, and a cutoff type of 2RC (phase compensation). Here, the direction of the evaluation length is measured along the width direction at the center of the width direction (direction perpendicular to the casting direction) of the Fe-based amorphous alloy ribbon. The Fe-based amorphous alloy ribbon tends to have a larger arithmetic mean roughness Ra of the free surface than of the roll surface.

[0020] The Fe-based amorphous alloy ribbon preferably has a maximum cross-sectional height Rt of 4 μm or more and 7 μm or less on the roll surface. By setting the maximum cross-sectional height Rt of the roll surface of the Fe-based amorphous alloy ribbon to 4 μm or more, the adhesion of the Fe-based amorphous alloy ribbon to the cooling roll is stable, and the Fe-based amorphous alloy ribbon is less likely to break during casting, and can be continuously wound. By setting the maximum cross-sectional height Rt of the roll surface of the Fe-based amorphous alloy ribbon to 7 μm or less, the Fe-based amorphous alloy ribbon can be made to have a surface with less unevenness on the roll surface, and the space factor is improved. The maximum cross-sectional height Rt is measured (evaluated) in accordance with JIS B 0601:2001, with an evaluation length of 4.0 mm, a cutoff value of 0.8 mm, and a cutoff type of 2RC (phase compensation). Here, the direction of the evaluation length is measured along the width direction at the center of the width direction (direction perpendicular to the casting direction) of the Fe-based amorphous alloy ribbon.

[0021] The Fe-based amorphous alloy ribbon preferably has a maximum peak height Rp of 1.2 μm or more and 2.0 μm or less on the roll surface. By setting the maximum peak height Rp of the Fe-based amorphous alloy ribbon to 1.2 μm or more, the adhesion of the Fe-based amorphous alloy ribbon to the cooling roll is stable, and the Fe-based amorphous alloy ribbon is less likely to break during casting, allowing it to be continuously wound. The maximum peak height Rp is measured (evaluated) in accordance with JIS B 0601:2001, with an evaluation length of 4.0 mm, a cutoff value of 0.8 mm, and a cutoff type of 2RC (phase compensation). Here, the direction of the evaluation length is measured along the width direction at the center of the width direction (direction perpendicular to the casting direction) of the Fe-based amorphous alloy ribbon.

[0022] The Fe-based amorphous alloy ribbon preferably has a maximum valley depth Rv of 0.5 μm or more and 3.7 μm or less on the roll surface. By setting the maximum valley depth Rv of the Fe-based amorphous alloy ribbon on the roll surface to 3.7 μm or less, the Fe-based amorphous alloy ribbon can have fewer concaves on the surface of the roll surface, improving the space factor. The maximum valley depth Rv is measured (evaluated) in accordance with JIS B 0601:2001, with an evaluation length of 4.0 mm, a cutoff value of 0.8 mm, and a cutoff type of 2RC (phase compensation). Here, the direction of the evaluation length is measured along the width direction at the center of the width direction (direction perpendicular to the casting direction) of the Fe-based amorphous alloy ribbon.

[0023] The Fe-based amorphous alloy ribbon preferably has a maximum height Rz of 3.0 μm or more and 5.0 μm or less on the roll surface. By setting the maximum height Rz of the roll surface of the Fe-based amorphous alloy ribbon to 3.0 μm or more, the adhesion of the Fe-based amorphous alloy ribbon to the cooling roll is stable, and the Fe-based amorphous alloy ribbon is less likely to break during casting, and can be continuously wound. By setting the maximum height Rz of the roll surface of the Fe-based amorphous alloy ribbon to 5.0 μm or less, the Fe-based amorphous alloy ribbon can be made to have a surface with less unevenness on the roll surface, and the space factor is improved. The maximum height Rz is measured (evaluated) in accordance with JIS B 0601:2001, with an evaluation length of 4.0 mm, a cutoff value of 0.8 mm, and a cutoff type of 2RC (phase compensation). Here, the direction of the evaluation length is measured along the width direction at the center of the width direction (direction perpendicular to the casting direction) of the Fe-based amorphous alloy ribbon.

[0024] The Fe-based amorphous alloy ribbon preferably has a space thickness of 4.8 μm or less. By setting the space thickness of the Fe-based amorphous alloy ribbon to 4.8 μm or less, when a plurality of Fe-based amorphous alloy ribbons are laminated to form a laminate, the laminate can have a maximum thickness smaller than the thickness of the Fe-based amorphous alloy ribbon. The space thickness can be calculated from the following formula 1 using the thickness (thickness) of the Fe-based amorphous alloy ribbon and the space factor (space factor) of the Fe-based amorphous alloy ribbon.

[0025] [Equation 1] Space thickness = thickness × (100 - space factor) / space factor

[0026] The Fe-based amorphous alloy ribbon preferably has a warpage of 15 mm or less. By making the warpage of the Fe-based amorphous alloy ribbon 15 mm or less, the adhesion of the Fe-based amorphous alloy ribbon to the cooling roll is stabilized, the Fe-based amorphous alloy ribbon is less likely to break during casting, and the ribbon can be wound continuously. The warpage of the Fe-based amorphous alloy ribbon is measured by a laser measuring device to measure the maximum height of the ribbon that is warped and raised in the width direction from the horizontal reference plane when the Fe-based amorphous alloy ribbon is placed so that both ends are placed on the horizontal reference plane.

[0027] The Fe-based amorphous alloy ribbon preferably has a relative permeability of 75,000 or more at a frequency of 1 kHz. The relative permeability of 50,000 or more at a frequency of 10 kHz is preferably. The relative permeability of 100 kHz is preferably 10,000 or more. The relative permeability of the Fe-based amorphous alloy ribbon can be determined by measuring the inductance (LS) using an LCR meter under the conditions of a magnetic field of 0.05 A / m and a turn number of 1 in a nano-crystallized state after a toroidal core made by winding the Fe-based amorphous alloy ribbon is heat-treated at 550°C for 20 minutes. In this case, l in the formula 2 indicates the magnetic path length, A indicates the cross-sectional area, and μ0 indicates the magnetic permeability of a vacuum.

[0028] [Math 2] Relative permeability μr=L S l / A / μ0

[0029] The Fe-based amorphous alloy that constitutes the Fe-based amorphous alloy ribbon preferably has Fe (iron) as the most abundant element (atomic percent) among the metal elements contained therein, and has an Fe-Si-B-Cu-Nb composition.

[0030] The Fe-based amorphous alloy contains at least Fe (iron), but preferably further contains Si (silicon) and B (boron), and more preferably contains copper (Cu) and niobium (Nb) in addition to Fe, Si, and B. The Fe-based amorphous alloy may further contain C (carbon), which is an element contained in pure iron and the like that is the raw material of the molten alloy. Niobium (Nb) can be replaced with molybdenum (Mo) or vanadium (V), and part of the iron (Fe) can be replaced with nickel (Ni) or cobalt (Co).

[0031] An example of an Fe-based amorphous alloy is an Fe-based amorphous alloy in which, when the total content of Fe, Si, B, Cu, Nb, C and unavoidable impurities is taken as 100 atomic %, the Fe content is 72 atomic % to 84 atomic %, the Si content is 2 atomic % to 20 atomic %, the B content is 5 atomic % to 14 atomic %, the Cu content is 0.2 atomic % to 2 atomic %, the Nb content is 0.1 atomic % to 5 atomic %, the C (carbon) content is 0.5 atomic % or less, and the remainder is impurities.

[0032] When the Fe content is 72 atomic % or more, the saturation magnetic flux density of the alloy ribbon is increased, and the increase in size or weight of the magnetic core manufactured using the alloy ribbon is suppressed.When the Fe content is 84 atomic % or less, the decrease in the Curie point and the decrease in the crystallization temperature of the alloy are suppressed, and the stability of the magnetic properties of the magnetic core is improved.

[0033] In addition, when the C (carbon) content is 0.5 atomic % or less, the embrittlement of the alloy ribbon becomes more severe. The C (carbon) content is preferably 0.1 atomic % to 0.5 atomic %. A more preferable C (carbon) content is 0.15 atomic % to 0.35 atomic %. When the C (carbon) content is 0.1 atomic % or more, the productivity of the molten alloy and the alloy ribbon is excellent.

[0034] More preferably, when the total content of Fe, Si, B, Cu, Nb, C and inevitable impurities is 100 atomic%, the content of Si is 12 atomic% to 18 atomic%, the content of B is 5 atomic% to 10 atomic%, the content of Cu is 0.8 atomic% to 1.2 atomic%, the content of Nb is 2.0 atomic% to 4.0 atomic%, the content of C is 0.1 atomic% to 0.5 atomic%, and the balance is an Fe-based amorphous alloy composed of Fe and inevitable impurities. Even more preferably, when the total content of Fe, Si, B, Cu, Nb, C and inevitable impurities is 100 atomic%, the content of Si is 14 atomic% to 16 atomic%, the content of B is 6 atomic% to 9 atomic%, the content of Cu is 0.9 atomic% to 1.1 atomic%, the content of Nb is 2.5 atomic% to 3.5 atomic%, the content of C is 0.15 atomic% to 0.35 atomic%, and the balance is an Fe-based amorphous alloy composed of Fe and inevitable impurities.

[0035] In each of the above-described Fe-based amorphous alloys, the content of C (carbon) is preferably 0.1 atomic% to 0.5 atomic% when the total content of Fe, Si, and B is 100 atomic%.

[0036] <Fe-based nanocrystalline alloy ribbon> The Fe-based nanocrystalline alloy ribbon is obtained by heat-treating the above-described Fe-based amorphous alloy ribbon. The heat treatment of the Fe-based amorphous alloy ribbon can be performed by a known method.

[0037] <Manufacturing method of Fe-based amorphous alloy ribbon> The manufacturing method of the Fe-based amorphous alloy ribbon will be described below.

[0038] FIG. 1 is a schematic cross-sectional view conceptually showing an example of an Fe-based amorphous alloy ribbon manufacturing apparatus by a single-roll method, and shows a cross-section when the alloy ribbon manufacturing apparatus is cut by a plane perpendicular to the axial direction of the cooling roll 30 and the width direction of the alloy ribbon. Here, the alloy ribbon 22C is an example of the Fe-based amorphous alloy ribbon of an embodiment of the present invention. Also, the axial direction of the cooling roll 30 and the width direction of the alloy ribbon 22C are the same direction.

[0039] As shown in FIG. 1, an alloy ribbon production apparatus 100, which is an apparatus for producing an Fe-based amorphous alloy ribbon, includes a crucible 20 equipped with a molten metal nozzle 10, and a cooling roll 30 whose outer peripheral surface faces the tip of the molten metal nozzle 10.

[0040] The crucible 20 has an internal space capable of accommodating the molten alloy 22A that is the raw material of the alloy ribbon 22C, and this internal space is connected to a molten metal flow path in the molten metal nozzle 10. This allows the molten alloy 22A accommodated in the crucible 20 to be discharged onto the chill roll 30 by the molten metal nozzle 10 (in FIG. 1, the discharge direction and flow direction of the molten alloy 22A are indicated by arrows Q). The crucible 20 and the molten metal nozzle 10 may be configured as an integral body or as separate bodies.

[0041] A high-frequency coil 40 serving as a heating means is disposed at least partially around the crucible 20. This makes it possible to heat the crucible 20 containing the master alloy of the alloy ribbon to generate the molten alloy 22A within the crucible 20, and to maintain the liquid state of the molten alloy 22A supplied to the crucible 20 from the outside.

[0042] The molten metal nozzle 10 also has an opening (discharge port) for discharging the molten alloy in the direction of the arrow Q. This opening is preferably a rectangular (slit-shaped) opening.

[0043] The distance (closest distance) between the tip of the molten metal nozzle 10 and the outer circumferential surface of the chill roll 30 is close enough that a puddle 22B (a pool of molten metal) is formed when the molten alloy 22A is discharged by the molten metal nozzle 10.

[0044] The chill roll 30 rotates about its axis in a rotation direction P. A cooling medium such as water flows inside the chill roll 30, so that the coating of the molten alloy formed on the outer circumferential surface of the chill roll 30 can be cooled. By cooling the coating of the molten alloy, an alloy ribbon 22C (Fe-based amorphous alloy ribbon) is produced.

[0045] Examples of materials for the cooling roll 30 include Cu and Cu alloys (Cu-Be alloy, Cu-Cr alloy, Cu-Zr alloy, Cu-Cr-Zr alloy, Cu-Ni alloy, Cu-Ni-Si alloy, Cu-Ni-Si-Cr alloy, Cu-Zn alloy, Cu-Sn alloy, Cu-Ti alloy, etc.), of which a Cu alloy is preferred due to its high thermal conductivity, and a Cu-Be alloy, a Cu-Cr-Zr alloy, a Cu-Ni alloy, a Cu-Ni-Si alloy, or a Cu-Ni-Si-Cr alloy is more preferred.

[0046] Although there is no particular limitation on the surface roughness of the outer peripheral surface of the chill roll 30, the arithmetic mean roughness (Ra) of the outer peripheral surface of the chill roll 30 is preferably 0.1 μm to 0.5 μm, and more preferably 0.1 μm to 0.3 μm. If the arithmetic mean roughness Ra of the outer peripheral surface of the chill roll 30 is 0.5 μm or less, the space factor is improved when manufacturing a wound magnetic core using the alloy ribbon. If the arithmetic mean roughness Ra of the outer peripheral surface of the chill roll 30 is 0.1 μm or more, adjustment of Ra is easier.

[0047] From the viewpoint of cooling capacity, the diameter of the chill roll 30 is preferably 200 mm to 1000 mm, more preferably 300 mm to 800 mm. The rotation speed of the chill roll 30 can be within the range usually set in the single roll method, but the peripheral speed is preferably 10 m / s to 40 m / s, more preferably 20 m / s to 30 m / s.

[0048] The alloy ribbon manufacturing apparatus 100 further includes a peeling gas nozzle 50 as a peeling means for peeling the Fe-based amorphous alloy ribbon from the outer peripheral surface of the chill roll, downstream of the molten metal nozzle 10 in the rotation direction of the chill roll 30 (hereinafter, simply referred to as the "downstream side"). In this example, the peeling gas nozzle 50 blows a peeling gas in the opposite direction to the rotation direction P of the chill roll 30 (the direction of the dashed arrow in FIG. 1) to peel the alloy ribbon 22C from the chill roll 30. As the peeling gas, for example, a high-pressure gas such as nitrogen gas or compressed air can be used.

[0049] The alloy ribbon manufacturing apparatus 100 further includes an abrasive brush roll 60 downstream of the peeling gas nozzle 50 as a polishing means for polishing the outer circumferential surface of the chill roll 30. The abrasive brush roll 60 includes a roll shaft member 61 and an abrasive brush 62 arranged around the roll shaft member 61. The abrasive brush 62 is made of a nonwoven fabric coated with a plurality of abrasive grains. The abrasive brush roll 60 rotates about its axis in the rotation direction R, thereby polishing the outer circumferential surface of the chill roll 30 with the nonwoven fabric of the abrasive brush 62.

[0050] The purpose of polishing by the polishing means (e.g., the polishing brush roll 60) is not necessarily limited to scraping the outer peripheral surface of the chill roll, but also includes removing residues remaining on the outer peripheral surface of the chill roll. The purpose of polishing is preferably at least one of the following first and second purposes.

[0051] The first purpose is to repair the deterioration of the smoothness of the outer peripheral surface of the chill roll. In detail, when the molten alloy and the outer peripheral surface of the chill roll first come into contact, a very small part of the outer peripheral surface of the chill roll (e.g., Cu alloy) dissolves in the molten alloy, and minute recesses (dropped parts) are formed on the outer peripheral surface of the chill roll, which may cause the deterioration of the smoothness of the outer peripheral surface of the chill roll. The deterioration of the smoothness of the outer peripheral surface of the chill roll may cause the deterioration of the smoothness of the roll surface of the alloy ribbon (the surface that was in contact with the outer peripheral surface of the chill roll; the same applies below). Even if the smoothness of the outer peripheral surface of the chill roll is deteriorated, the deterioration of the smoothness of the outer peripheral surface of the chill roll can be repaired by removing the parts that are convex relative to the minute recesses (dropped parts) by the above polishing almost evenly (i.e., the parts where dissolution is suppressed). As a result, the deterioration of the smoothness of the roll surface of the alloy ribbon caused by the deterioration of the smoothness of the outer peripheral surface of the chill roll can be suppressed.

[0052] The second purpose is to remove the residue (alloy) remaining on the outer peripheral surface of the cooling roll after the alloy ribbon is peeled off. The molten alloy discharged onto the outer peripheral surface of the cooling roll is rapidly cooled to form an alloy ribbon, which is then peeled off from the outer peripheral surface of the cooling roll. At this time, a part of the alloy, which is the material of the alloy ribbon, may remain as a residue without being peeled off from the outer peripheral surface of the cooling roll, and this residue may adhere to the outer peripheral surface of the cooling roll to form a convex portion. Since the casting of the alloy ribbon is performed continuously, the molten alloy is discharged again onto the outer peripheral surface of the cooling roll on which the convex portion due to the residue is formed. As a result, on the roll surface of the manufactured alloy ribbon, a concave portion may be formed at a position corresponding to the convex portion, and the smoothness of the roll surface of the alloy ribbon may be deteriorated. In addition, if the thermal conductivity of the residue (alloy) constituting the convex portion is lower than that of the outer peripheral surface of the cooling roll (e.g., Cu alloy), the rapid cooling characteristics by the cooling roll may be locally deteriorated at the convex portion, and the magnetic properties of the alloy ribbon may be deteriorated. Even if the above-mentioned residue remains on the outer peripheral surface of the cooling roll after the alloy ribbon is peeled off, the above-mentioned residue can be removed by the above-mentioned polishing. As a result, it is possible to suppress the deterioration of the smoothness of the roll surface of the alloy ribbon caused by the residue, and also to suppress the deterioration of the magnetic properties of the alloy ribbon caused by the residue.

[0053] The alloy ribbon manufacturing apparatus 100 further includes an atmospheric gas nozzle 70 for injecting (supplying) atmospheric gas onto the surface of the cooling roll onto which the molten alloy is supplied.

[0054] The atmospheric gas jetted from the atmospheric gas nozzle 70 is CO2 gas or CO gas in order to control the gas atmosphere in the vicinity of the roll surface at the tip of the nozzle.

[0055] The alloy ribbon manufacturing apparatus 100 may include other elements in addition to the elements described above (for example, a take-up roll for taking up the manufactured alloy ribbon 22C, etc.).

[0056] Next, an example of a method for manufacturing the alloy ribbon 22C using the alloy ribbon manufacturing apparatus 100 will be described. First, a molten alloy 22A serving as a raw material for the alloy ribbon 22C is prepared in the crucible 20. The temperature of the molten alloy 22A is appropriately set in consideration of the composition of the alloy, and is, for example, 1210°C to 1410°C, and preferably 1280°C to 1400°C.

[0057] Next, the molten alloy is discharged by the molten alloy nozzle 10 onto the outer peripheral surface of the cooling roll 30, which rotates in the rotation direction P, and a coating film is formed by the molten alloy while forming a puddle 22B. The formed coating film is cooled on the outer peripheral surface of the cooling roll 30, and an alloy ribbon 22C is formed on the outer peripheral surface. Next, the alloy ribbon 22C formed on the outer peripheral surface of the cooling roll 30 is peeled off from the outer peripheral surface of the cooling roll 30 by blowing a peeling gas from the peeling gas nozzle 50, and is wound up in a roll by a winding roll (not shown) and collected. Meanwhile, the outer peripheral surface of the cooling roll 30 after the alloy ribbon 22C is peeled off is polished by the polishing brush 62 of the polishing brush roll 60, which rotates in the rotation direction R. The molten alloy is again discharged onto the polished outer peripheral surface of the cooling roll 30. By repeating the above operations, the long alloy ribbon 22C is continuously manufactured (cast). EXAMPLES

[0058] Examples of the present invention will now be described.

[0059] <Production of Fe-based amorphous alloy ribbon> An alloy ribbon manufacturing apparatus similar to the alloy ribbon manufacturing apparatus 100 shown in FIG. 1 was prepared. As the cooling roll, a cooling roll having an outer peripheral surface made of a Cu-Be alloy, a diameter of 400 mm, and an arithmetic mean roughness Ra of the outer peripheral surface of 0.3 μm was used.

[0060] First, an alloy melt (hereinafter, also referred to as "Fe-Si-B-Cu-Nb based alloy melt") composed of Fe, Si, B, Cu, Nb, C and inevitable impurities was prepared in a crucible. Specifically, pure iron, ferrosilicon, and ferroboron were mixed and melted, and when the total content of Fe, Si, B, Cu, Nb, C and inevitable impurities was 100 atomic%, the content of Si was 15 atomic%, the content of B was 7 atomic%, the content of Cu was 1 atomic%, the content of Nb was 3 atomic%, the content of C was 0.2 atomic%, and the balance was an alloy melt composed of Fe and inevitable impurities. The numerical values of atomic% are the amounts measured by ICP emission spectrometry by sampling a part of the alloy from the melt.

[0061] Next, this Fe-Si-B-Cu-Nb based alloy melt was discharged from the opening of a melt nozzle having a rectangular (slit shape) opening with a long side length of 53 mm and a short side length of 0.3 mm onto the outer peripheral surface of a rotating cooling roll and rapidly solidified to produce (cast) 500 kg of an amorphous alloy ribbon with a ribbon width of 53 mm. The casting time was 60 minutes, and the alloy ribbon was continuously cast without break. The above casting was performed while polishing the outer peripheral surface of the cooling roll with a polishing brush (non-woven fabric) of a polishing brush roll.

[0062] The detailed conditions of casting are shown below. <Casting conditions> Alloy melt temperature: 1350 °C to 1390 °C Peripheral speed of cooling roll: 20 m / s to 30 m / s Discharge pressure of alloy melt: Adjusted within the range of 5 kPa to 30 kPa Distance (gap) between the tip of the molten metal nozzle and the outer periphery of the cooling roll: Adjust within the range of 0.1mm to 0.35mm

[0063] In Examples 1 to 8 and Comparative Example 5, the thicknesses were manufactured to the dimensions in Table 1 while a predetermined atmospheric gas was sprayed (supplied) from an atmospheric gas nozzle.

[0064] In Comparative Examples 1 to 4, the atmospheric gas was not sprayed (supplied) from the atmospheric gas nozzle, and the thicknesses were manufactured to the dimensions in Table 1.

[0065] For Examples 1 to 8 and Comparative Examples 1 to 5, the surface roughness (arithmetic mean roughness Ra, maximum peak height Rp, maximum valley depth Rv, maximum height Rz, maximum cross-sectional height Rt), thickness, warpage, space factor, spatial thickness, and relative permeability of the roll surface and free surface were measured. The measurement results for each measured value are shown in Table 1. The measurement method for each measured value was as described above.

[0066] [Table 1]

[0067] As shown in Table 1, in Examples 1 to 8, by injecting (supplying) an atmospheric gas onto the surface of the chill roll to which the molten metal is supplied, it was possible to obtain an Fe-based amorphous alloy ribbon having a space factor of 73% or more even if the ribbon had a thickness of 11 μm or more and 14 μm or less. Also, the space thickness was 4.8 μm or less. Also, FIG. 2 shows an image of the roll surface obtained by an optical microscope in Example 4.

[0068] In Comparative Examples 1 to 3, the atmospheric gas was not sprayed (supplied) to the surface of the chill roll to which the molten metal was supplied, but the thickness exceeded 14 μm, so the space factor was 73% or more. Also, the space thickness exceeded 4.8 μm. Fig. 3 shows an image of the roll surface of Comparative Example 1 obtained by an optical microscope.

[0069] In Comparative Example 4, the atmospheric gas was not injected (supplied) onto the surface of the chill roll to which the molten metal was supplied, and the thickness was set to 14 μm or less, resulting in a space factor of less than 73%. Also, the space thickness was more than 4.8 μm. In Comparative Example 5, the atmospheric gas was injected (supplied) onto the surface of the chill roll to which the molten metal was supplied, but the maximum peak height Rp of the roll surface was less than 1.2 μm, resulting in a space factor of less than 73%. Also, the space thickness was more than 4.8 μm.

[0070] As described above, it is understood that by injecting (supplying) an atmospheric gas onto the surface of the chill roll to which the molten metal is supplied, an Fe-based amorphous alloy ribbon having a space factor of 73% or more can be obtained even if the thickness is 11 μm or more and 14 μm or less. It is also understood that by injecting (supplying) an atmospheric gas onto the surface of the chill roll to which the molten metal is supplied, an Fe-based amorphous alloy ribbon having a space thickness of 4.8 μm or less can be obtained.

[0071] In addition, in Examples 1 to 8, the formation of recesses (air pockets) was suppressed by injecting (supplying) the atmosphere gas onto the surface of the chill roll to which the molten metal was supplied, and the arithmetic mean roughness Ra of the roll surface could be reduced to 0.6 μm or less. Similarly, the maximum peak height Rp, maximum valley depth Rv, maximum height Rz, and maximum cross-sectional height Rt could be reduced by injecting (supplying) the atmosphere gas onto the surface of the chill roll to which the molten metal was supplied. In this way, the formation of recesses (air pockets) was suppressed by injecting (supplying) the atmosphere gas onto the surface of the chill roll to which the molten metal was supplied, and therefore the space factor could be improved (the space thickness could be reduced). From Figs. 2 and 3, it can be seen that the formation of recesses (air pockets) on the roll surface in the Example (Fig. 2) was suppressed compared to the Comparative Example (Fig. 3). [Explanation of symbols]

[0072] 10: Molten metal nozzle 20: Crucible 30: Cooling roll 40: High frequency coil 50: Stripping gas nozzle 60: Abrasive brush roll 70: Atmosphere gas nozzle 100: Alloy ribbon manufacturing equipment

Claims

1. The thickness is 11 μm or more and 14 μm or less, The space factor measured in accordance with IEC 60404-8-11: 2018 is 73% or more. Fe-based amorphous alloy ribbon for Fe-based nanocrystalline alloys.

2. One surface is a roll surface and the other surface is a free surface; The maximum peak height Rp of the roll surface is 1.2 μm or more, and the maximum valley depth Rv is 3.7 μm or less. The Fe-based amorphous alloy ribbon for use in an Fe-based nanocrystalline alloy according to claim 1.

3. The arithmetic average roughness Ra of the roll surface is 0.6 μm or less. The Fe-based amorphous alloy ribbon for use in an Fe-based nanocrystalline alloy according to claim 2.

4. The maximum cross-sectional height Rt of the roll surface is 4 μm or more and 7 μm or less. The Fe-based amorphous alloy ribbon for use in an Fe-based nanocrystalline alloy according to claim 2.

5. A method for producing an Fe-based amorphous alloy ribbon, comprising the steps of: supplying a molten Fe-based alloy to a surface of a cooling roll to produce an Fe-based amorphous alloy ribbon, the method comprising the steps of: An atmospheric gas is sprayed onto a surface of the chill roll onto which the molten alloy is supplied. A method for producing Fe-based amorphous alloy ribbons for use in Fe-based nanocrystalline alloys.

6. The Fe-based amorphous alloy ribbon has a thickness of 11 μm or more and 14 μm or less. A method for producing an Fe-based amorphous alloy ribbon for an Fe-based nanocrystalline alloy according to claim 5.

Citation Information

Patent Citations

  • Fe-based magnetic alloy

    JP1989242755A

  • Vibration control element of piping, piping with vibration control element, and pressure transmitting apparatus with vibration control element

    JP1992004393A