Evaluation method of stress corrosion crack resistance in liquid ammonia

By using a controlled method with a reference test piece and specific conditions, SCC in liquid ammonia is accurately reproduced, addressing inefficiencies in existing evaluation methods.

JP2024165863AActive Publication Date: 2024-11-28NIPPON STEEL CORPORATION

Patent Information

Application Number
JP2023082419
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

Existing methods for evaluating stress corrosion cracking (SCC) in liquid ammonia are inefficient, lack strict control over test conditions, and are prone to variations due to impurities and improper handling of oxygen addition, leading to inconsistent and impractical evaluations.

Method used

A method involving a reference test piece and an evaluation test piece, with controlled conditions including specific distances between electrodes, oxygen introduction, and ammonium carbamate concentration, to ensure accurate reproduction of SCC in a laboratory setting.

Benefits of technology

This method allows for the accelerated and reliable reproduction of SCC in steel materials exposed to liquid ammonia, providing a valid evaluation of SCC susceptibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165863000001_ABST
    Figure 2024165863000001_ABST
Patent Text Reader

Abstract

To provide an evaluation method of stress corrosion crack resistance in liquid ammonia, capable of evaluating a SCC sensitivity through accelerating and reproducing a SCC generated in a steel material by liquid ammonia in a laboratory.SOLUTION: An reference-purpose method includes: a step of introducing, into a single pressure container, a reference-purpose test piece and an evaluation-purpose test piece to which a surface strain is applied by a flexure test jig, an ammonia solution of carbamic acid ammonium and an oxygen gas, and compressing and holding for one hour or more; and a step of confirming an existence / nonexistence of a stress corrosion crack after an elapse of testing time. Each test piece is electrically insulated to the flexure test jig and the pressure container. In the reference-purpose test piece, a Vickers hardness is 230 HV or more. Liquid ammonia, the carbamic acid ammonium and the oxygen gas are in a prescribed purity or more. When an occurrence of a stress corrosion crack is recognized in the reference-purpose test piece, an evaluation of a stress corrosion crack to the evaluation-purpose test piece is regarded valid.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for evaluating stress corrosion cracking properties in liquid ammonia. [Background technology]

[0002] Ammonia has been widely used for various purposes, such as raw material for fertilizers and refrigerant. In recent years, the need for global warming countermeasures has increased, and ammonia has attracted attention as a next-generation energy source due to its characteristic of not emitting CO2 when burned. It is expected that CO2 emissions will be reduced through the co-firing and exclusive combustion of ammonia in thermal power generation, industry, engines, etc. In order to supply huge amounts of ammonia for these purposes, efficient storage and transportation of ammonia is necessary, and there is a demand for the construction of large ammonia tanks made of high-strength steel.

[0003] However, ammonia is corrosive to steel, and steel may undergo stress corrosion cracking (hereinafter sometimes referred to as "SCC") in liquid ammonia. For this reason, the strength of steel used in ammonia tanks is currently limited. However, if high-strength steel is used to manufacture large ammonia tanks in the future, the welding residual stress of the welded joints will increase, and the design stress will also increase, increasing the SCC susceptibility. Therefore, it is necessary to properly evaluate the SCC properties of high-strength steel and its welds in liquid ammonia, and then design and manufacture large ammonia tanks made of high-strength steel under conditions where SCC does not occur.

[0004] SCC of steel in liquid ammonia is said to be active path corrosion type SCC, and when a corrosion film is formed on the inner surface of the tank that comes into contact with ammonia during long-term use of the liquid ammonia tank, and the film is locally destroyed by welding residual stress or hoop stress due to internal pressure, a new surface is exposed, and the new surface corrodes and dissolves preferentially, leading to cracks. If we try to accurately reproduce this type of SCC phenomenon, it will take an enormous amount of time (several years to several decades) equivalent to SCC in an actual tank, which makes the test efficiency extremely poor.

[0005] In order to reproduce the SCC phenomenon in a laboratory, for example, Patent Document 1 describes a method for producing a mixture of liquid ammonia at 25°C, saturated CO2 (a sufficient amount of ammonium carbamate: NH4CO2NH2) and 1 kgf / cm3 as an SCC accelerator. 2 A technology has been disclosed that reproduces SCC in 168 hours by adding 100 MPa of O2 and then applying a constant potential (2 V against a platinum electrode, polarization toward the anode side) to a four-point bending test piece in liquid ammonia via a constant potential generator (potentiostat).

[0006] Furthermore, Patent Document 2 discloses a technique in which, although the test specimen is not anodically polarized, the test specimen is bent into a U shape to impart plastic strain, thereby promoting film destruction, and furthermore, by adding CO2 (ammonium carbamate) and oxygen as environmental acceleration factors, the specimen is immersed in liquid ammonia at 25°C for 1,000 hours to reproduce SCC. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 57-137096 [Patent Document 2] Japanese Patent Application Publication No. 11-131178 Summary of the Invention [Problem to be solved by the invention]

[0008] Incidentally, the SCC of steel in liquid ammonia is temperature dependent, with the SCC susceptibility being higher at room temperature (20-25°C) than at low temperatures. However, in order to keep ammonia in a liquid state at room temperature, high pressure (e.g., 0.86 MPa or more at 20°C) is required. Therefore, to perform SCC evaluation tests of steel in liquid ammonia under strict conditions, such as room temperature, a pressure vessel (autoclave) is required, which imposes experimental constraints. In addition, care must be taken to prevent ammonia from leaking during testing, making handling extremely cumbersome.

[0009] Therefore, in both of the techniques described in Patent Document 1 and Patent Document 2, multiple test pieces are simultaneously placed in a relatively small pressure vessel for evaluation, thereby improving the efficiency of the test. However, neither Patent Document 1 nor Patent Document 2 specifies whether the test environment in the same SCC test is appropriately and strictly controlled, and the techniques described in these documents may not strictly control the test conditions. In addition, the addition of oxygen to liquid ammonia is a strong accelerating factor for SCC generation, but the inventor's study revealed that the effect of adding oxygen cannot be obtained unless the SCC test is started after the time until a film is formed after the oxygen addition. However, Patent Document 1 does not specify the time from the addition of oxygen to the start of the SCC test, and in this respect, too, the test conditions may not be strictly controlled. In addition, since the time from the addition of oxygen to the start of the SCC test is not specified, it is unclear whether it is appropriate as an accelerated test.

[0010] Furthermore, the SCC of steel in liquid ammonia is easily affected by trace amounts of impurities mixed into the liquid ammonia, and if the trace impurities in the test environment are not properly controlled, the SCC will not be reproduced, resulting in an inappropriate evaluation. However, it is extremely complicated and unrealistic to analyze the type and concentration of impurities in the environment with high precision for each test. Therefore, a test method is required that shows that the test environment including the evaluation material is properly performed to reproduce the liquid ammonia SCC after appropriately limiting the ammonia purity and the concentration of the added substances used in the test environment in advance. However, neither Patent Document 1 nor Patent Document 2 specifies the purity or concentration of each substance used to reproduce the test environment, and the type and concentration of impurities in the test environment are unclear in the evaluation of SCC in liquid ammonia.

[0011] Incidentally, liquid ammonia has a low electrical conductivity (also called electrical conductivity or electric conductivity) and is difficult to pass electricity through. The present inventor has found that when applying a potential or passing a current in liquid ammonia, the distance between the test piece and the counter electrode, and further between the test piece and the reference electrode, greatly affects the test results. However, Patent Document 1 does not take into account the distance between the test piece and the electrode.

[0012] As described above, the current evaluation of SCC in liquid ammonia is insufficient in terms of the test environment, retention time after oxygen addition, impurity control, and the distance between the test specimen and the counter electrode, as well as between the test specimen and the reference electrode.

[0013] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for evaluating stress corrosion cracking properties in liquid ammonia, which can accelerate and reproduce in a laboratory the SCC caused in steel by liquid ammonia, and evaluate SCC susceptibility. [Means for solving the problem]

[0014] The inventors have come up with the idea of ​​appropriately setting the test environment, the retention time after oxygen addition, the control of impurities, the distance between the test specimen and the counter electrode, and the distance between the test specimen and the reference electrode, which have not been done before, and further placing a reference specimen, which has been confirmed to cause SCC in advance, in the same container as the evaluation specimen. By conducting a test under conditions that cause SCC in the reference specimen and confirming that SCC has occurred in the reference specimen, it is guaranteed that the test environment is appropriately set to reproduce liquid ammonia SCC.

[0015] The gist of the present invention is as follows. [1] A method for evaluating stress corrosion cracking properties in liquid ammonia according to one embodiment of the present invention includes the steps of: placing a reference test piece and an evaluation test piece, to which surface strain has been applied by a bending test jig, and a counter electrode facing the test surfaces of the reference test piece and the evaluation test piece, or placing the reference test piece and the evaluation test piece, the counter electrode, and a reference electrode facing the test surfaces of the reference test piece and the evaluation test piece, in the same pressure vessel; filling the pressure vessel with an ammonia solution containing 3 mass% or more of ammonium carbamate; introducing oxygen gas into the pressure vessel to pressurize the vessel and hold the vessel for one hour or more; and maintaining the pressurized state for a test time during which stress corrosion cracking has occurred in the reference test piece in a previously performed test, and holding the reference test piece and the evaluation test piece at a constant potential at which they are anode polarized at 1.0 V or more relative to the counter electrode, or holding the reference test piece at a current density of 3.0 A / m 2 and a confirmation step of confirming the occurrence of stress corrosion cracking after the test time has elapsed, wherein the reference test piece and the evaluation test piece are electrically insulated from the bending test jig and the pressure vessel, the material of the reference test piece is a steel material having a Vickers hardness of 230 HV or more, or a welded joint including a weld heat affected zone having a Vickers hardness of 230 HV or more, and the distance between the test surface of the reference test piece and the counter electrode and the distance between the test surface of the evaluation test piece and the counter electrode are each 10 0 mm or less, and when held at the constant potential, the distance between the test surface of the reference test piece and the reference electrode and the distance between the test surface of the evaluation test piece and the reference electrode are each 50 mm or less, the purity of the liquid ammonia constituting the ammonia solution is 99.9% or more, the purity of the ammonium carbamate is 97.0% or more, and the purity of the oxygen gas is 99.9% or more, and if the occurrence of stress corrosion cracking is confirmed in the reference test piece in the confirmation process, the evaluation of stress corrosion cracking of the evaluation test piece is valid. [2] In the method for evaluating stress corrosion cracking properties in liquid ammonia described in [1] above, in the holding step and the testing step, the O2 partial pressure in the pressure vessel is set to 0.5 kgf / cm 2 More than 5.0kgf / cm2 The following may also be used. [3] In the method for evaluating stress corrosion cracking properties in liquid ammonia according to the above [1] or [2], the surface strain may be 0.6 times or more the yield strain. [4] In the method for evaluating stress corrosion cracking properties in liquid ammonia according to any one of [1] to [3] above, the bending test jig may be a four-point bending test jig, and the reference test piece and the evaluation test piece may be supported at a constant displacement via ceramic or glass pins. Effect of the Invention

[0016] According to the present invention, it is possible to provide a method for evaluating stress corrosion cracking properties in liquid ammonia, which enables the accelerated reproduction in a laboratory of SCC caused in steel by liquid ammonia and the evaluation of SCC susceptibility. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram showing an example of a test device that can be used in a method for evaluating stress corrosion cracking properties in liquid ammonia according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a plan view of the AA' cross section of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] <Evaluation method for stress corrosion cracking properties in liquid ammonia> The method for evaluating the stress corrosion cracking property in liquid ammonia according to the embodiment of the present invention will be described. The method for evaluating the stress corrosion cracking property in liquid ammonia according to the present embodiment includes the steps of: placing a reference test piece and an evaluation test piece to which surface strain has been applied by a bending test jig, a counter electrode facing the test surfaces of the reference test piece and the evaluation test piece, or the reference test piece and the evaluation test piece, the counter electrode, and a reference electrode facing the test surfaces of the reference test piece and the evaluation test piece in the same pressure vessel; filling the pressure vessel with an ammonia solution containing 3 mass % or more of ammonium carbamate; introducing oxygen gas into the pressure vessel, pressurizing the vessel, and holding the vessel for 1 hour or more; and maintaining the pressurized state for the test time during which stress corrosion cracking occurred in the reference test piece in a previously performed test, and holding the reference test piece and the evaluation test piece at a constant potential at which the reference test piece and the evaluation test piece are anode polarized at 1.0 V or more relative to the counter electrode, or holding the reference test piece at a current density of 3.0 A / m 2 The method includes a test step of maintaining the above constant current while performing anodizing, and a confirmation step of removing the evaluation test piece and the reference test piece from the pressure vessel after the test time has elapsed and confirming whether or not stress corrosion cracking has occurred.

[0019] FIG. 1 is a schematic diagram showing an example of a test apparatus that can be used in the method for evaluating stress corrosion cracking properties in liquid ammonia according to one embodiment of the present invention. FIG. 2 is a plan view of the A-A' section of FIG. 1. FIG. 1 shows a state in which a test piece 2 to which a surface strain is applied by a bending test jig 5, a reference electrode 3, and a counter electrode 4 are installed inside a pressure vessel 1, and a powder of ammonium carbamate 6 and an ammonia solution 7 in which ammonium carbamate is dissolved are placed. FIG. 2 is a plan view (A-A') of the test apparatus shown in FIG. 1, showing a state in which a reference test piece 21 and an evaluation test piece 22 are installed facing the test surfaces of the reference electrode 3 and the counter electrode 4. The reference test piece 21 and the evaluation test piece 22 correspond to the test piece 2 in FIG. 1. The reference test piece 21 and the evaluation test piece 22 are provided with surface strain by a reference test jig 51 and an evaluation test jig 52, respectively. The reference test jig 51 and the evaluation test jig 52 correspond to the bending test jig 5 in FIG. 1. The pressure vessel 1 is equipped with a connection pipe 8 to a gas cylinder for introducing liquid ammonia and O2, and a connection pipe 10 to a pressure gauge for measuring the internal pressure. As shown in Figures 1 and 2, a reference electrode 3 may be installed inside the pressure vessel 1, but it is not necessary to do so. The test piece 2, the reference electrode 3, and the counter electrode 4 are connected by a connection wire 9 to a potentio / galvanostat (not shown) that applies a constant potential or passes a constant current.

[0020] [Installation process] In the installation process, the reference test piece 21 and the evaluation test piece 22, to which surface strain has been applied by the bending test jig 5, and the counter electrode 4 facing the respective test surfaces of the reference test piece 21 and the evaluation test piece 22, or the reference test piece 21 and the evaluation test piece 22, the counter electrode 4, and the reference electrode 3 facing the respective test surfaces of the reference test piece 21 and the evaluation test piece 22 are installed in the same pressure vessel 1.

[0021] The reference test piece 21 is a test piece for determining whether or not a test environment is appropriate in an evaluation test of stress corrosion cracking properties in liquid ammonia. The reference test piece 21 is a steel plate, or a welded joint including a steel plate and a welded heat affected zone. The shape of the reference test piece 21 corresponds to the bending test jig 5. The bending test jig 5 is not particularly limited as long as it can impart surface strain to the reference test piece 21, and examples thereof include a four-point bending test jig, a three-point bending test jig, and a U-bend test jig.

[0022] The material of the reference test piece 21 is a steel material having a Vickers hardness of 230HV or more, or a welded joint having a Vickers hardness of 230HV or more in the heat affected zone (sometimes called HAZ). A large tank for storing a large volume of liquid ammonia requires a high-strength steel material. The reference test piece 21 is required to cause SCC because it is used to ensure that the test environment is appropriately performed to reproduce liquid ammonia SCC. If the Vickers hardness is 230HV or more, SCC in liquid ammonia is likely to occur, so the Vickers hardness of the steel material from which the reference test piece 21 is taken or the Vickers hardness of the HAZ of the welded joint is 230HV or more. In order to make the SCC occurrence condition more severe, it is preferable that the Vickers hardness of the material of the reference test piece 21 is 240HV or more, or 260HV or more. Examples of the material of the reference test piece 21 include low-alloy steel with a total content of alloy elements of 5% or less, and medium-alloy steel with a total content of alloy elements of more than 5% and 10% or less. The Vickers hardness is a value obtained by applying a load of, for example, 9.8 N (1 kgf) in accordance with JIS Z 2244-1:2020.

[0023] The method for evaluating stress corrosion cracking properties in liquid ammonia according to this embodiment is basically carried out under conditions under which stress corrosion cracking occurs in the reference test specimen. The conditions under which stress corrosion cracking occurs in the reference test specimen are determined in advance by confirming the test time and pressurization state under which stress corrosion cracking occurs using the reference test specimen. Then, in the final confirmation step of the series of steps described below, if the occurrence of stress corrosion cracking is confirmed in the reference test specimen, the evaluation of stress corrosion cracking of the evaluation test specimen can be judged to be valid.

[0024] The evaluation test piece 22 is a test piece to be evaluated for stress corrosion cracking properties in liquid ammonia. The evaluation test piece 22 has the same shape as the reference test piece 21. Examples of the material of the evaluation test piece 22 include low-alloy steel with a total content of alloy elements of 5% or less, and medium-alloy steel with a total content of alloy elements of more than 5% and 10% or less. In one evaluation, the material of the evaluation test piece 22 may be the same as the material of the reference test piece 21, or may be different from each other.

[0025] The reference test piece 21 and the evaluation test piece 22 are electrically insulated from each bending test jig 5 and the pressure vessel 1. By electrically insulating the reference test piece 21 and the evaluation test piece 22 from each bending test jig 5 and the pressure vessel 1, it is possible to prevent galvanic corrosion that may occur between them and current flow during anodic polarization, and it is possible to appropriately evaluate SCC in liquid ammonia. In order to electrically insulate the reference test piece 21 and the evaluation test piece 22 from each bending test jig 5, the reference test piece 21 and the evaluation test piece 22 may be supported at a constant displacement via a ceramic or glass pin.

[0026] The surface strain applied to the reference test piece 21 and the evaluation test piece 22 by the bending test jig 5 is preferably 0.6 times or more of the yield strain. If the applied surface strain is 0.6 times or more of the yield strain, the SCC evaluation can be accelerated and the test time can be shortened. On the other hand, in order to set the surface strain applied to the test piece almost uniformly on the test surface, it is necessary to avoid applying a large strain that causes a local portion of the test piece to bulge or shrink significantly. From this viewpoint, the surface strain applied to the reference test piece 21 and the evaluation test piece 22 by the bending test jig 5 is preferably 10 times or less of the yield strain, which corresponds to a U-bend bending test. In the case of a four-point bending test, the surface strain is preferably 1.0 times or less of the yield strain. Moreover, the surface strain applied to the evaluation test piece 22 may be larger than the surface strain applied to the reference test piece 21.

[0027] The yield strain is a value converted into strain using a yield stress previously measured in a tensile test, and may be, for example, the upper yield point or 0.2% proof stress obtained at room temperature in accordance with JIS Z2241: 2022. When the yield strain differs between the base material, the weld heat-affected zone, and the weld metal, such as in a welded joint, the value of a representative portion may be used, for example, the value of the base material.

[0028] Although the method for measuring the surface strain in the reference test piece 21 and the evaluation test piece 22 is not limited, the surface strain in the reference test piece and the evaluation test piece is, for example, a value measured by the following method. That is, a strain gauge connected to a strain measuring device is attached to the surface of the test piece, and the value of the surface strain can be measured by the strain measuring device. In this case, after the surface strain is set to a target value, it is preferable to peel off the strain gauge, wipe off the adhesive used for bonding the strain gauge with an organic solvent, and then polish the surface with fine-grained (e.g., #1000) emery paper until there is no trace of the attached strain gauge.

[0029] The reference test piece 21 and the evaluation test piece 22 are placed in the same pressure vessel 1. The pressure vessel 1 may be a pressure-resistant vessel capable of creating high pressure inside, a so-called autoclave. By placing each test piece in the same pressure vessel 1, the test environment of the reference test piece 21 and the test environment of the evaluation test piece 22 can be made the same, and the variation between these test environments can be suppressed.

[0030] The pressure vessel 1 can accommodate a reference test piece 21 and an evaluation test piece 22, each having a bending test jig 5 attached thereto, and can maintain a high pressure inside. The pressure vessel 1 can accommodate a counter electrode 4 for anodic polarization, and preferably also a reference electrode 3, as shown in FIG. 1. When a constant potential is applied, both the counter electrode 4 and the reference electrode 3 are placed in the pressure vessel 1. When a constant current is applied, only the counter electrode 4 may be placed in the pressure vessel 1. The counter electrode 4 and the reference electrode 3 are preferably made of platinum.

[0031] Liquid ammonia has low electrical conductivity (also called electrical conductivity or electrical conductivity) and does not easily conduct electricity. When applying a potential in liquid ammonia, the distance between the test piece 2 and the reference electrode 3 has a large effect on the test results. At the potential set for anodic polarization, if the distance between the test piece 2 and the reference electrode 3 becomes large, the current that flows becomes lower than the set value, and it is thought that SCC becomes less likely to occur.

[0032] According to the study by the present inventors, when applying a constant potential in the test step described later, it is important that the distance between the test surface of the reference test piece 21 and the reference electrode 3 and the distance between the test surface of the evaluation test piece 33 and the reference electrode 3 are each 50 mm or less. The distance between the test surface of the reference test piece 21 and the reference electrode 3 and the distance between the test surface of the evaluation test piece 22 and the reference electrode 3 are preferably the same within the margin of error, and may be arranged as shown in FIG. 2, for example. For example, the distance from the reference electrode 3 may be 50 mm or less, and the reference test piece 21 and one or more evaluation test pieces 22 may be installed on an arc centered on the reference electrode 3. The distance between the test surface of the reference test piece 21 and the reference electrode 3 and the distance between the test surface of the evaluation test piece 22 and the reference electrode 3 are preferably as close as possible without contact, and although there is no lower limit specified, they are appropriately determined according to the size of the test piece 2 and the jig installed in the pressure vessel 1.

[0033] When the reference electrode 3 and the counter electrode 4 are installed in the pressure vessel 1, the distance from the test piece 2 to the counter electrode 4 is basically greater than the distance from the test piece 2 to the reference electrode 3. However, since liquid ammonia has a property of being difficult to conduct electricity, if the distance from the test piece 2 to the counter electrode 4 becomes too large, the response during anode polarization becomes poor. According to the study by the present inventors, it is important that the distance between the test surface of the reference test piece 21 and the counter electrode 4 and the distance between the test surface of the evaluation test piece 22 and the counter electrode 4 are each 100 mm or less. It is preferable that the distance between the reference test piece and the counter electrode and the distance between the evaluation test piece and the counter electrode are the same within the margin of error, and for example, the arrangement shown in FIG. 2 may be used. For example, the distance from the counter electrode to each test piece is 100 mm or less, and the reference test piece and one or more evaluation test pieces may be installed on an arc centered on the counter electrode. In addition, when a plurality of reference electrodes and counter electrodes can be installed in the pressure vessel 1, the reference electrode and counter electrode may be installed independently on the test surface of the reference test piece and the test piece for evaluation. In the constant current test in the test process described later, when the reference electrode 3 is not installed in the pressure vessel 1, the distance between the test surface of the reference test piece 21 and the test surface of the test piece for evaluation 22 and the counter electrode 4 is preferably as close as possible as long as they do not contact each other. Although there is no lower limit, it is determined appropriately depending on the size of the test piece 2 and the jig installed in the pressure vessel 1. As described above, when the reference electrode 3 and the counter electrode 4 are installed in the pressure vessel 1, the lower limit of the distance from the counter electrode 4 to each test piece 2 is determined appropriately depending on the distance from the reference electrode 3 to each test piece 2 and the size of the test piece 2 and the jig installed in the pressure vessel 1.

[0034] [Filling process] In the filling step, an ammonia solution containing 3% by mass or more of ammonium carbamate is filled into the pressure vessel. If the concentration of ammonium carbamate in the ammonia solution is 3% by mass or more, SCC in liquid ammonia can be promoted. The concentration of ammonium carbamate in the ammonia solution may be 4% by mass or more or 5% by mass or more. There is no particular upper limit to the concentration of ammonium carbamate in the ammonia solution, but if the concentration of ammonium carbamate is too high, the effect of promoting SCC in liquid ammonia is saturated. Therefore, the concentration of ammonium carbamate in the ammonia solution can be, for example, 10% by mass or less in order to save the amount of ammonium carbamate used. The concentration of ammonium carbamate in the ammonia solution may be 9% by mass or less, or 7% by mass or less.

[0035] The purity of ammonium carbamate is 97.0% or more. The purity of the liquid ammonia constituting the ammonia solution is 99.9% or more. This limits the amount of impurities to a small amount, and the effect of impurities on SCC can be suppressed. The purity of ammonium carbamate is preferably 99.5% or more. The purity of the liquid ammonia constituting the ammonia solution is preferably 99.999% or more.

[0036] The method for filling the pressure vessel with an ammonia solution containing 3% by mass or more of ammonium carbamate is not particularly limited, and can be, for example, the following method: For example, after placing ammonium carbamate powder in the pressure vessel, liquid ammonia is added to the pressure vessel to dissolve the ammonium carbamate in the liquid ammonia, thereby preparing an ammonia solution.

[0037] Next, oxygen gas (O2 gas) is introduced into the pressure vessel 1, so that the reference test piece 21 and the evaluation test piece 22 are immersed in an ammonia solution containing 3 mass % or more of ammonium carbamate and O2.

[0038] [Holding process] In the holding step, oxygen gas (O2 gas) is introduced into the pressure vessel 1, pressurized, and held for one hour or more. The holding time is the time from pressurization inside the pressure vessel 1 to the start of the test. As described below, in the case of polarization at a constant potential, the test starts when a constant potential is applied to the reference test piece 21 and the evaluation test piece 22. In the case of polarization at a constant current, the test starts when a constant current is applied to the reference test piece 21 and the evaluation test piece 22.

[0039] The temperature of the ammonia solution is not particularly limited, but is preferably room temperature in consideration of the promotion of SCC and ease of handling of the test environment. The temperature of the ammonia solution may be, for example, 5° C. or higher and 35° C. or lower.

[0040] The purity of the oxygen gas is 99.9% or more. By making the purity of the oxygen gas 99.9% or more, the amount of impurities is limited to a small amount, and the effect of the impurities on SCC can be suppressed. The purity of the oxygen gas is preferably 99.999% or more.

[0041] The pressure in the pressure vessel 1 is maintained at a pressure that keeps the ammonia liquid, but the O2 partial pressure is 0.5 kgf / cm 2 More than 5.0kgf / cm 2 It is preferable that the O2 partial pressure in the pressure vessel 1 is 0.5 kgf / cm or less. The O2 gas in the gas phase dissolves in the ammonia solution at the interface with the ammonia solution and forms a film on the surface of the test piece. In order to form a film that reproduces actual use, the O2 partial pressure in the pressure vessel 1 is 0.5 kgf / cm or less. 2 More preferably, the O2 partial pressure in the pressure vessel 1 is 0.7 kgf / cm or more. 2 More preferably, it is 0.8 kgf / cm 2 Above 0.9kgf / cm 2 Above 1.0kgf / cm 2 That's all. The O2 partial pressure in the pressure vessel 1 is 1.1 kgf / cm 2 It may be 1.2kgf / cm or more. 2 On the other hand, if the coating becomes too thick, cracks are less likely to occur. Therefore, the O2 partial pressure in the pressure vessel 1 is 5.0 kgf / cm 2The O2 partial pressure in the pressure vessel 1 is preferably 1.5 kgf / cm or less. 2 More preferably, it is 1.2 kgf / cm or less. 2 Below, 1.1kgf / cm 2 The O2 partial pressure in the pressure vessel 1 is 1.0 kgf / cm 2 It may be less than 0.9kgf / cm 2 The pressure inside the pressure vessel 1 can be measured by a pressure gauge and adjusted by introducing oxygen gas from a gas cylinder as necessary.

[0042] The holding time is 1 hour or more. By holding for 1 hour or more, a film is stably formed on the surfaces of the reference test piece 21 and the evaluation test piece 22, and SCC susceptibility can be appropriately evaluated. There is no particular upper limit to the holding time, but from the viewpoint of test efficiency, it may be, for example, 96 hours or less, or 24 hours or less.

[0043] [Testing process] In the testing process, the pressurized state is maintained for a test time during which stress corrosion cracking occurs in the reference test piece 21 in a previously performed test. The time during which stress corrosion cracking occurs in the reference test piece 21 varies depending on the shape of the test piece 2, the type of bending test jig 5, and the environment inside the pressure vessel 1 (temperature, pressure, ammonia solution components, etc.).

[0044] In order to promote SCC, the reference test piece 21 and the evaluation test piece 22 are held at a constant potential of 1.0 V or more relative to the counter electrode 4, which is an anodic polarization, or the current density is 3.0 A / m 2 The electrode is maintained at a constant potential of 1.5 V or more while polarizing the electrode anode. The electrode may be maintained at a constant potential of 3.0 V or less or 2.5 V or less. The electrode may be maintained at a constant current of 4.0 A / m or more. 2 It is acceptable to hold the sample at a constant current of 7.0A / m 2 Less than or equal to 6.0A / m 2 You can do it as follows: When maintaining at a constant potential, it is important that the distance between the reference test piece 21 and the evaluation test piece 22 and the reference electrode 3 is 50 mm or less in order to cause SCC. When polarizing at the constant potential, the test time can be, for example, 240 hours (10 days). When polarizing at a constant potential, the test starts when a constant potential is applied to the reference test piece 21 and the evaluation test piece 22. When polarizing at a constant current, the test time can be 168 hours (1 week). When polarizing at a constant current, the test starts when a constant current is applied to the reference test piece 21 and the evaluation test piece 22.

[0045] [Confirmation process] In the confirmation step, the occurrence of stress corrosion cracking is confirmed after the test time has elapsed. The stress corrosion cracking is confirmed by observing the surface of the evaluation test piece 22. For example, the occurrence of stress corrosion cracking may be confirmed by visual observation, or the occurrence of stress corrosion cracking may be confirmed by observing the surface of the evaluation test piece 22 at an arbitrary magnification, for example, 500 times, using an optical microscope. At this time, if the occurrence of stress corrosion cracking is confirmed in the reference test piece 21, it can be determined that an appropriate evaluation has been performed. Therefore, if the occurrence of stress corrosion cracking is confirmed in the reference test piece 21, the evaluation of the stress corrosion cracking of the evaluation test piece 22 is considered to be valid.

[0046] The method for evaluating stress corrosion cracking properties in liquid ammonia has been described above. However, the technical scope of the present invention is not limited to the above-mentioned embodiment, and various modifications can be made without departing from the spirit of the present invention.

[0047] For example, in the confirmation step, the evaluation test piece 22 may be embedded in a resin, polished, and then the surface of the evaluation test piece 22 may be observed. EXAMPLES

[0048] Next, examples of the present invention will be described, although the technical scope of the present invention is not limited to the following examples.

[0049] Reference test pieces were taken from arc welds of high-strength steel HT80 (maximum hardness of welded heat-affected zone exceeds 260HV), pressure vessel steel plate SPV315 (maximum hardness of welded heat-affected zone is 210HV) specified in JIS G3115:2022, and even higher strength HT60 (maximum hardness of welded heat-affected zone is 230HV). Evaluation test pieces were also taken from arc welds of pressure vessel steel plate SPV315 and high-strength steel HT60. For both reference test and evaluation test pieces, a stainless steel four-point bending test jig was used to set the surface strain between the two central points to the size shown in Table 1. In the bending test jig, the reference test piece and the evaluation test piece were brought into contact with a ceramic insulating pin. Several combinations of the evaluation specimen and the reference specimen were prepared, and liquid ammonia, ammonium carbamate, and O2 gas with different purities were prepared, and SCC tests were performed by changing the O2 partial pressure and immersion conditions. The test temperature was controlled at 20°C (±2°C). After immersion, O2 gas was introduced into the pressure vessel and held for 1 hour.

[0050] After immersion, each test piece was placed in a constant potential state of 1.0 V or 2.0 V (vs. Pt electrode) using a potentiostat, or in a constant potential state of 3.0 A / m 2 Or 5.0A / m 2 The conditions were that the anodic polarization was performed under a constant current condition of 100 mm. The distance from the Pt counter electrode was 100 mm or less, and for comparison, some (No. 17 in Table 1) were more than 100 mm. The distance between the test piece and the Pt reference electrode was 50 mm or less, and for comparison, some (No. 16 in Table 1) were more than 50 mm. In addition, some anodic polarization under a constant current condition (Nos. 3, 8, and 10 in Table 1) was performed without placing a reference electrode in the pressure vessel. After the test time shown in Table 1 had elapsed, the test piece was removed from each pressure vessel, and if SCC was found in the reference test piece, the presence or absence of SCC in the evaluation test piece placed in the same vessel as the reference test piece was investigated. The presence or absence of SCC was confirmed specifically by visual observation and by observing the surfaces of the reference test piece and evaluation test piece at 500 times magnification using an optical microscope.

[0051] Table 1 shows a list of SCC test conditions and results.

[0052] [Table 1]

[0053] In all of the inventive examples Nos. 1 to 10, SCC occurred in the reference specimens, indicating that the conditions for reproducing SCC were appropriate, and it was possible to evaluate the presence or absence of SCC susceptibility in the evaluation specimens.

[0054] In the comparative example, No. 11, the SCC susceptibility of the reference test piece was low, so SCC was not reproduced in the reference test piece, and it was therefore inappropriate for the SCC test in liquid ammonia. The test conditions set for No. 11 were the same as those for No. 2, an example of the present invention, except that SPV315 (maximum hardness of the weld heat-affected zone is 210 HV) was used as the reference test piece. However, if SCC is not reproduced in the reference test piece, it is impossible to determine whether the conditions for reproducing SCC in the test process were appropriate, so No. 11 was an inappropriate example.

[0055] In the comparative example, No. 12, the purity of the liquid ammonia was low and it contained impurities that reduced cracking susceptibility, so SCC could not be reproduced in the reference test specimen, making it unsuitable as an SCC test environment in liquid ammonia.

[0056] In the comparative example, No. 13, the purity of the ammonium carbamate was low, and the SCC promotion effect in liquid ammonia was not obtained, so SCC was not reproduced in the reference test piece, making it unsuitable as an SCC test environment in liquid ammonia.

[0057] In the comparative example, No. 14, the concentration of ammonium carbamate was low and the promotion of SCC in liquid ammonia was insufficient, so SCC was not reproduced in the reference test piece and it was unsuitable as an SCC test environment in liquid ammonia.

[0058] In the comparative example, No. 15, the purity of O2 was low and impurities that reduced cracking susceptibility were contained, so SCC could not be reproduced in the reference test piece, making it unsuitable as an SCC test environment in liquid ammonia.

[0059] In the comparative example, No. 16, the distance between the test piece and the reference electrode was large, so SCC was not reproduced on the reference test piece, making it unsuitable as an SCC test environment in liquid ammonia.

[0060] In the comparative example, No. 17, the distance between the test piece and the counter electrode was large, so SCC was not reproduced in the reference test piece, making it unsuitable as an SCC test environment in liquid ammonia.

[0061] In the comparative example, No. 18, the holding time after O2 pressurization was short, so SCC was not reproduced in the reference test specimen, making it unsuitable as an SCC test environment in liquid ammonia. [Explanation of symbols]

[0062] 1. Pressure vessel (autoclave) 2 Test specimens 21 Reference test piece 22 Evaluation specimen 3 Reference electrode 4. Opposite 5. Bending test fixture 51 Reference Test Fixture 52 Evaluation test fixture 6. Ammonium Carbamate 7. Ammonia Solution 8. Gas cylinder connection piping 9 Connecting wires 10. Pressure gauge connection piping

Claims

1. an installation step of installing, in the same pressure vessel, a reference test piece and an evaluation test piece to which a surface strain has been applied by a bending test jig, and a counter electrode facing the respective test surfaces of the reference test piece and the evaluation test piece, or the reference test piece and the evaluation test piece, the counter electrode, and a reference electrode facing the respective test surfaces of the reference test piece and the evaluation test piece; a filling step of filling the pressure vessel with an ammonia solution containing 3% by mass or more of ammonium carbamate; a holding step of introducing oxygen gas into the pressure vessel, pressurizing the vessel, and holding the vessel for one hour or more; The pressurized state is maintained for a test time during which stress corrosion cracking occurs in the reference test piece in a previously performed test, and the reference test piece and the evaluation test piece are held at a constant potential of 1.0 V or more relative to the counter electrode, resulting in an anode polarization, or a current density of 3.0 A / m 2 a test step of maintaining the anode polarization at the constant current; A confirmation step of confirming whether or not stress corrosion cracking occurs after the test time has elapsed; Including, the reference test piece and the evaluation test piece are electrically insulated from the bending test jig and the pressure vessel; The material of the reference test piece is a steel material having a Vickers hardness of 230 HV or more, or a welded joint including a weld heat affected zone having a Vickers hardness of 230 HV or more, the distance between the test surface of the reference test piece and the counter electrode and the distance between the test surface of the evaluation test piece and the counter electrode are each 100 mm or less; During the holding at the constant potential, the distance between the test surface of the reference test piece and the reference electrode and the distance between the test surface of the evaluation test piece and the reference electrode are each 50 mm or less; The purity of the liquid ammonia constituting the ammonia solution is 99.9% or more, The purity of the ammonium carbamate is 97.0% or more, The purity of the oxygen gas is 99.9% or more, When occurrence of stress corrosion cracking is confirmed in the reference test piece in the confirmation step, the evaluation of the stress corrosion cracking of the evaluation test piece is validated. Evaluation method for stress corrosion cracking properties in liquid ammonia.

2. In the holding step and the testing step, the O 2 Partial pressure 0.5 kgf / cm 2 More than 5.0 kgf / cm 2 The following shall apply: The method for evaluating stress corrosion cracking properties in liquid ammonia according to claim 1.

3. The surface strain is 0.6 times or more the yield strain; The method for evaluating stress corrosion cracking properties in liquid ammonia according to claim 1 or 2.

4. The bending test jig is a four-point bending test jig, and supports the reference test piece and the evaluation test piece at a constant displacement via ceramic or glass pins. The method for evaluating stress corrosion cracking properties in liquid ammonia according to claim 1 or 2.

Citation Information

Patent Citations

  • Method and apparatus for manufacturing stress corrosion crack test specimen

    JP2006010427A

  • Corrosion testing apparatus and corrosion testing method

    JP2012093175A

  • Low yield ratio and high-strength steel having excellent stress corrosion cracking resistance and low temperature toughness

    US20180371588A1

  • Low hydrogen type coated electrode

    JP1982137096A

  • Low yield ratio steel plate for low temperature use, excellent in toughness in weld heat-affected zone at large heat input welding as well as in ammonia stress corrosion cracking resistance

    JP1999131178A

Cited By

  • Ammonia stress corrosion cracking acceleration test method

    JP2024179313A

  • Ammonia stress corrosion cracking acceleration test method

    JP2024179321A

  • Ammonia stress corrosion cracking accelerated test method

    JP7782518B2

  • Ammonia stress corrosion cracking accelerated test method

    JP7782519B2

  • Ammonia environment suitability evaluation considering cargo tank environment

    WO2026182556A1