Cold storage material for cryogenic freezer, cold storage device for cryogenic freezer and cryogenic freezer
The bismuth-silver regenerator material addresses the brittleness and cracking issues of pure bismuth by adding silver as an additive, improving mechanical strength and refrigerating capacity in cryogenic refrigerators.
Patent Information
- Application Number
- JP2023082576
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Pure bismuth is brittle and prone to cracking during the manufacturing and operation of cryogenic refrigerators due to the forces exerted by the working gas, posing a risk of breakage and reduced refrigerating capacity.
A regenerator material comprising bismuth as a main component with up to 10% by weight of silver as an additive, combined with magnetic cold storage materials at different locations, enhances toughness and mechanical strength.
The bismuth-silver regenerator material improves toughness, reducing the risk of cracking and maintaining or enhancing refrigerating capacity by optimizing the temperature profile and gas absorption in cryogenic refrigerators.
Smart Images

Figure 2024165955000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a regenerator material for a cryogenic refrigerator, and a regenerator for a cryogenic refrigerator and a cryogenic refrigerator using the regenerator material. [Background technology]
[0002] Traditionally, spherical lead has been used as a cold storage material for cryogenic refrigerators. Lead has a higher specific heat than other materials in the low temperature range of approximately 50K or less, and is also inexpensive, so it was widely used in the past. However, the use of lead is now restricted or prohibited due to its adverse effects on the environment and human body. It is known that pure bismuth molded into granules can be used as a cold storage material to replace lead. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-137632 A Summary of the Invention [Problem to be solved by the invention]
[0004] Pure bismuth is brittle, so it can break into powder when it is filled into the regenerator during the manufacturing process of the cryogenic refrigerator. In addition, there is a risk that the pure bismuth regenerator material may break due to the force applied to the regenerator material by the working gas (e.g., helium gas) flowing through the gaps between the regenerator materials during operation of the cryogenic refrigerator.
[0005] An exemplary object of an embodiment of the present invention is to provide a regenerator material for a cryogenic refrigerator having improved toughness, and a regenerator for a cryogenic refrigerator and a cryogenic refrigerator using the regenerator material. [Means for solving the problem]
[0006] According to one embodiment of the present invention, a regenerator material for a cryogenic refrigerator contains bismuth as a main component and at most 10 wt % of silver as an additive.
[0007] According to one embodiment of the present invention, a regenerator for a cryogenic refrigerator comprises a bismuth-silver-based regenerator material having bismuth as its main component and at most 10% by weight of silver as an additive, and a magnetic regenerator material arranged at a different location from the bismuth-silver-based regenerator material in the axial direction of the regenerator.
[0008] According to an aspect of the present invention, a cryogenic refrigerator includes the regenerator for a cryogenic refrigerator of the above aspect. Effect of the Invention
[0009] According to the present invention, it is possible to provide a regenerator material for a cryogenic refrigerator having improved toughness, and a regenerator for a cryogenic refrigerator and a cryogenic refrigerator using the regenerator material. [Brief description of the drawings]
[0010] [Figure 1] 1 is a diagram illustrating a schematic diagram of a cryogenic refrigerator according to an embodiment; [Diagram 2] 1 is a diagram illustrating a schematic diagram of a cryogenic refrigerator according to an embodiment; [Diagram 3] 1 is a graph showing the volumetric specific heat of several metallic materials in accordance with an embodiment. [Figure 4] FIG. 4 is a schematic diagram showing an axial temperature profile of a second regenerator of a cryogenic refrigerator in the embodiment. [Diagram 5] 4 is a graph showing a relationship between the silver content in a bismuth-silver based cold storage material and the cooling temperature of a first stage of a cryogenic refrigerator according to an embodiment. [Figure 6] 4 is a graph showing a relationship between the silver content in a bismuth-silver based regenerator material and the cooling temperature of a second stage of a cryogenic refrigerator according to an embodiment. [Figure 7] FIG. 11 is a schematic diagram showing a second regenerator of a cryogenic refrigerator according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the embodiments for carrying out the present invention will be described in detail with reference to the drawings. In the description and drawings, the same or equivalent components, members, and processes are given the same reference numerals, and duplicated descriptions are omitted as appropriate. The scale and shape of each part shown in the drawings are set for convenience in order to facilitate the description, and are not to be interpreted as being limiting unless otherwise specified. The embodiments are merely examples, and do not limit the scope of the present invention in any way. All features and combinations thereof described in the embodiments are not necessarily essential to the invention.
[0012] 1 and 2 are schematic diagrams illustrating a cryogenic refrigerator 10 according to an embodiment. The cryogenic refrigerator 10 is, as an example, a two-stage Gifford-McMahon (GM) refrigerator. FIG. 1 shows the exterior of the cryogenic refrigerator 10, and FIG. 2 shows the internal structure of the cryogenic refrigerator 10.
[0013] The cryogenic refrigerator 10 includes a compressor 12 and an expander 14. The compressor 12 is configured to recover the working gas of the cryogenic refrigerator 10 from the expander 14, pressurize the recovered working gas, and supply the working gas again to the expander 14. The working gas, also called a refrigerant gas, is typically helium gas, although other suitable gases may be used.
[0014] The expander 14 includes a refrigerator cylinder 16, a displacer assembly 18, and a refrigerator housing 20. The refrigerator housing 20 is coupled to the refrigerator cylinder 16, thereby forming an airtight container that houses the displacer assembly 18. Note that the internal volume of the refrigerator housing 20 may be connected to the low pressure side of the compressor 12 and maintained at low pressure.
[0015] The refrigerator cylinder 16 has a first cylinder 16a and a second cylinder 16b. The first cylinder 16a and the second cylinder 16b are, for example, members having a cylindrical shape, and the second cylinder 16b has a smaller diameter than the first cylinder 16a. The first cylinder 16a and the second cylinder 16b are arranged coaxially, and the lower end of the first cylinder 16a is rigidly connected to the upper end of the second cylinder 16b.
[0016] The displacer assembly 18 has a first displacer 18a and a second displacer 18b. The first displacer 18a and the second displacer 18b are, for example, cylindrical members, and the second displacer 18b has a smaller diameter than the first displacer 18a. The first displacer 18a and the second displacer 18b are arranged coaxially.
[0017] The first displacer 18a is accommodated in the first cylinder 16a, and the second displacer 18b is accommodated in the second cylinder 16b. The first displacer 18a can reciprocate in the axial direction along the first cylinder 16a, and the second displacer 18b can reciprocate in the axial direction along the second cylinder 16b. The first displacer 18a and the second displacer 18b are connected to each other and move together.
[0018] In this document, in order to explain the positional relationship between the components of the cryogenic refrigerator 10, for convenience, the side closer to the top dead center of the axial reciprocating motion of the displacer will be referred to as "top" and the side closer to the bottom dead center as "bottom." The top dead center is the position of the displacer where the volume of the expansion space is maximum, and the bottom dead center is the position of the displacer where the volume of the expansion space is minimum. During operation of the cryogenic refrigerator 10, a temperature gradient occurs in which the temperature decreases from the top to the bottom in the axial direction, so the top side can also be called the high temperature side and the bottom side the low temperature side.
[0019] The first displacer 18a accommodates the first regenerator 26. The cylindrical body of the first displacer 18a serves as a first regenerator container extending in the axial direction. The first regenerator 26 is formed by filling the body of the first displacer 18a with a wire mesh such as copper or other suitable first regenerator material. The upper and lower lids of the first displacer 18a may be provided as separate members from the body of the first displacer 18a, and the upper and lower lids of the first displacer 18a may be fixed to the body by suitable means such as fastening or welding, thereby accommodating the first regenerator material in the first displacer 18a.
[0020] Similarly, the second displacer 18b accommodates the second regenerator 28. The cylindrical body of the second displacer 18b serves as a second regenerator container extending in the axial direction. The upper and lower lids of the second displacer 18b may be provided as separate members from the body of the second displacer 18b, and the upper and lower lids of the second displacer 18b may be fixed to the body by an appropriate means such as fastening or welding, thereby accommodating the second regenerator material in the second displacer 18b.
[0021] The second regenerator 28 includes at least two types of regenerator materials, three types in this example, which are stacked in the axial direction of the second displacer 18b. As shown in Fig. 2, the second regenerator 28 includes a high-temperature side regenerator material 28a, an intermediate regenerator material 28b, and a low-temperature side regenerator material 28c in the axial direction from the high-temperature side to the low-temperature side. To increase the refrigeration capacity of the second stage of the cryogenic refrigerator 10, materials having large specific heats at different temperatures are selected as the regenerator materials.
[0022] The high-temperature side regenerator material 28a may be made of a material having a relatively high volumetric heat capacity (e.g., a volumetric heat capacity higher than that of copper) at the high-temperature side of the second displacer 18b, for example, in a temperature range of 10K to 50K or at least a part thereof. The high-temperature side regenerator material 28a may have a volumetric heat capacity higher than that of copper, which is a regenerator material typically used in the first displacer 18a as described above, in this temperature range. The high-temperature side regenerator material 28a may also have a volumetric heat capacity higher than that of a magnetic regenerator material described below in this temperature range. The high-temperature side regenerator material 28a may be made of a non-magnetic metal material.
[0023] As an example of such a high-temperature side regenerator material 28a, in this embodiment, a bismuth-silver-based regenerator material, for example, a bismuth-silver alloy, is used. The bismuth-silver-based regenerator material contains bismuth as a main component and a small amount of silver as an additive.
[0024] Here, the term "main component" refers to the component that is the largest in the total amount of the heat accumulator composition (e.g., the component with the largest weight percentage). The bismuth silver-based heat accumulator may contain, for example, at least 80 weight percent, at least 90 weight percent, or at least 95 weight percent bismuth. The bismuth silver-based heat accumulator may be entirely bismuth except for the additive (i.e., silver).
[0025] In this embodiment, the bismuth silver-based cold storage material contains at most 10% by weight of silver as an additive. This is because if the ratio of silver exceeds 10% by weight, it becomes difficult or impossible to manufacture the bismuth silver alloy. Since the bismuth silver alloy has a wide solid-liquid coexistence temperature range (262.5 to 350°C), when cooling begins from the solution temperature in the alloy manufacturing process, solidification proceeds while forming dendrites. At this time, bismuth, which is a solute, is discharged into the liquid phase as the dendrites grow. As a result, there is less bismuth in the dendritic solid, and bismuth increases in the remaining liquid phase. Therefore, it is difficult or impossible to stably manufacture a bismuth silver alloy with a silver content exceeding 10% by weight.
[0026] As described below, the bismuth-silver-based cold storage material may contain, for example, at most 5% by weight, or at most 2% by weight, or at most 1% by weight of silver as an additive. The bismuth-silver-based cold storage material may contain at least 0.001% by weight of silver as an additive. The bismuth-silver-based cold storage material may contain only silver as an additive.
[0027] As the intermediate cold storage material 28b, a material different from that of the high-temperature-side cold storage material 28a is used. The intermediate cold storage material 28b may be formed of a material having a relatively high volumetric specific heat in the axial intermediate portion of the second displacer 18b, for example, in a temperature range of 5 K to 10 K or at least a part thereof. Typically, the intermediate cold storage material 28b may be formed of a magnetic cold storage material having a peak of volumetric specific heat associated with a magnetic phase transition in this temperature range. The intermediate cold storage material 28b may be formed of a metallic magnetic material such as HoCu2, Er3Ni, etc.
[0028] As the low-temperature-side cold storage material 28c, a magnetic cold storage material different from that of the intermediate cold storage material 28b is used. The low-temperature-side cold storage material 28c may be formed of a magnetic cold storage material having a relatively high volumetric specific heat in the temperature range of the low-temperature side of the second displacer 18b (i.e., the coldest displacer low end in the displacer assembly 18), for example, in a temperature range of 1 K to 5 K or at least a part thereof.
[0029] The magnetic cold storage material suitable for the low-temperature-side cold storage material 28c has a peak of volumetric specific heat associated with a magnetic phase transition in this temperature range. The magnetic cold storage material may be a non-metallic magnetic material, and the general formula is R x O2S or (R 1-y R′ y ) x O2S (R and R′ are at least one kind of rare earth element, 0.1 ≦ x ≦ 9, 0 < y < 1), or Gd x Al 2-xIt may contain at least one kind of magnetic refrigeration material represented by O3(1≦x<2). The rare earth elements R and R′ may be, for example, yttrium Y, lanthanum La, cerium Ce, praseodymium Pr, neodymium Nd, promethium Pm, samarium Sm, europium Eu, gadolinium Gd, terbium Tb, dysprosium Dy, holmium Ho, erbium Er, thulium Tm, or ytterbium Yb.
[0030] The magnetic refrigeration material used for the low-temperature side refrigeration material 28c may be Gd2O2S (also called GOS), Tb2O2S (also called TBOS), (Gd 1-y Tb y )2O2S(0<y<1, also called GdTbOS), or GdAlO3 (also called GAP), or may contain at least one kind of these.
[0031] As is known, such non-metallic magnetic refrigeration materials have a higher (e.g., several times higher) volumetric specific heat than metallic magnetic refrigeration materials such as HoCu2, for example, in the temperature range of 1K to 5K or at least a part thereof. Therefore, the low-temperature side refrigeration material 28c is suitable for enhancing the refrigeration capacity of the cryogenic refrigerator 10 that provides cryogenic cooling in this temperature range.
[0032] In addition, in order to improve the mechanical strength of the magnetic refrigeration material, additives may be added to the magnetic refrigeration material. The additive may be, for example, at least one of zirconium Zr, aluminum Al, and alumina (Al2O3). The weight ratio of the additive to the magnetic refrigeration material may be, for example, 20% or less, or 15% or less. In this way, without significantly changing the volumetric specific heat of the magnetic refrigeration material (i.e., without significantly affecting the refrigeration capacity of the cryogenic refrigerator 10), the hardness of the magnetic refrigeration material can be increased, and the risk of damage or pulverization due to impact can be reduced.
[0033] The high-temperature side cold storage material 28a, the intermediate cold storage material 28b, and the low-temperature side cold storage material 28c may be granular. The granules constituting such a granular cold storage material may be formed into granules having a size of, for example, 0.01 mm to 3 mm and filled in the second displacer 18b. The particle size of the granules may be, for example, 0.14 mm to 1.6 mm, preferably 0.15 mm to 1.4 mm, and more preferably 0.22 mm to 1.3 mm. The ratio of granules having a particle size of 0.14 mm to 1.6 mm to the total granules may be 70% by weight or more. If the particle size is less than 0.14 mm, the density becomes too high when filling the cold storage device, and the passage resistance of the working gas (e.g., helium gas) may increase rapidly. Also, if the particle size exceeds 1.6 mm, there is a concern that the heat exchange efficiency between the granules and the working gas may be significantly reduced.
[0034] Moreover, the ratio of the maximum diameter to the minimum diameter of the granules (aspect ratio) is 5 or less in any three-dimensional direction, preferably 3 or less, more preferably 2 or less, and further preferably as close to a sphere as possible. If the aspect ratio exceeds 5, the granules are prone to mechanical deformation and destruction, and it becomes difficult to pack them at a high density, which reduces the cooling efficiency. Therefore, the proportion of granules with a ratio of the major axis to the minor axis of 5 or less may be 70% by weight or more of the total granules.
[0035] To protect such particles, the surfaces may be covered with a coating (such as alumina (Al2O3), fluororesin, etc.) having a thickness of, for example, 1 to 50 μm.
[0036] In order to separate the high-temperature side cold accumulator material 28a from the intermediate cold accumulator material 28b, a partition member such as a wire mesh may be disposed at a boundary 29a between the high-temperature side cold accumulator material 28a and the intermediate cold accumulator material 28b. Also, if necessary, a partition member may be disposed at a boundary 29b between the intermediate cold accumulator material 28b and the low-temperature side cold accumulator material 28c.
[0037] Referring to FIG. 2, the displacer assembly 18 forms an upper chamber 30, a first expansion chamber 32, and a second expansion chamber 34 inside the refrigerator cylinder 16. For heat exchange with a desired object or medium to be cooled by the cryogenic refrigerator 10, the expander 14 includes a first cooling stage 33 and a second cooling stage 35. The upper chamber 30 is formed between the upper cover of the first displacer 18a and the upper part of the first cylinder 16a. The first expansion chamber 32 is formed between the lower cover of the first displacer 18a and the first cooling stage 33. The second expansion chamber 34 is formed between the lower cover of the second displacer 18b and the second cooling stage 35. The first cooling stage 33 is fixed to the lower part of the first cylinder 16a so as to surround the first expansion chamber 32, and the second cooling stage 35 is fixed to the lower part of the second cylinder 16b so as to surround the second expansion chamber 34.
[0038] The first regenerator 26 is connected to the upper chamber 30 through a working gas passage 36a formed in the upper lid of the first displacer 18a, and is connected to the first expansion chamber 32 through a working gas passage 36b formed in the lower lid of the first displacer 18a. The second regenerator 28 is connected to the first regenerator 26 through a working gas passage 36c formed from the lower lid of the first displacer 18a to the upper lid of the second displacer 18b. The second regenerator 28 is also connected to the second expansion chamber 34 through a working gas passage 36d formed in the lower lid of the second displacer 18b.
[0039] A first seal 38a and a second seal 38b may be provided so that the working gas flow between the first expansion chamber 32, the second expansion chamber 34 and the upper chamber 30 is guided to the first regenerator 26 and the second regenerator 28, instead of through the clearance between the refrigerator cylinder 16 and the displacer assembly 18. The first seal 38a may be attached to an upper cover of the first displacer 18a so as to be disposed between the first displacer 18a and the first cylinder 16a. The second seal 38b may be attached to an upper cover of the second displacer 18b so as to be disposed between the second displacer 18b and the second cylinder 16b.
[0040] The expander 14 also includes a pressure switching valve 40 and a drive motor 42. The pressure switching valve 40 is accommodated in the refrigerator housing 20, and the drive motor 42 is attached to the refrigerator housing 20.
[0041] As shown in FIG. 2, the pressure switching valve 40 includes a high-pressure valve 40a and a low-pressure valve 40b, and is configured to generate periodic pressure fluctuations in the refrigerator cylinder 16. The working gas discharge port of the compressor 12 is connected to the upper chamber 30 via the high-pressure valve 40a, and the working gas intake port of the compressor 12 is connected to the upper chamber 30 via the low-pressure valve 40b. The high-pressure valve 40a and the low-pressure valve 40b are configured to selectively and alternately open and close (i.e., when one is open, the other is closed). High-pressure (e.g., 2 to 3 MPa) working gas is supplied from the compressor 12 to the expander 14 through the high-pressure valve 40a, and low-pressure (e.g., 0.5 to 1.5 MPa) working gas is collected from the expander 14 to the compressor 12 through the low-pressure valve 40b. For ease of understanding, the flow direction of the working gas is indicated by arrows in FIG. 2.
[0042] The drive motor 42 is provided to drive the reciprocating motion of the displacer assembly 18. The drive motor 42 is connected to a displacer drive shaft 44 via a motion conversion mechanism 43, such as a Scotch yoke mechanism. The motion conversion mechanism 43 is housed in the refrigerator housing 20, as is the pressure switching valve 40. The displacer drive shaft 44 extends from the motion conversion mechanism 43 through the refrigerator housing 20 into the upper chamber 30 and is fixed to the upper cover of the first displacer 18a. A third seal 38c is provided to prevent leakage of the working gas from the upper chamber 30 to the refrigerator housing 20 (which may be maintained at a low pressure as described above). The third seal 38c may be attached to the refrigerator housing 20 so as to be disposed between the refrigerator housing 20 and the displacer drive shaft 44.
[0043] When the drive motor 42 is driven, the rotational output of the drive motor 42 is converted into axial reciprocating motion of the displacer drive shaft 44 by the motion conversion mechanism 43, and the displacer assembly 18 reciprocates in the axial direction inside the refrigerator cylinder 16. In addition, the drive motor 42 is connected to the high pressure valve 40a and the low pressure valve 40b so as to selectively and alternately open and close these valves.
[0044] When the compressor 12 and the drive motor 42 are operated, the cryogenic refrigerator 10 generates periodic volume fluctuations and synchronous pressure fluctuations of the working gas in the first expansion chamber 32 and the second expansion chamber 34, thereby forming a refrigeration cycle, and the first cooling stage 33 and the second cooling stage 35 are cooled to a desired cryogenic temperature. The first cooling stage 33 can be cooled to a first cooling temperature in the range of, for example, about 30K to about 80K. The second cooling stage 35 can be cooled to a second cooling temperature lower than the first cooling temperature, for example, 1K to 20K. The second cooling temperature may be the liquid helium temperature of about 4.2K or a temperature lower than that.
[0045] According to the embodiment, as described above, a bismuth silver-based cold accumulator, for example, a bismuth silver alloy, is used. The table shown below shows the measurement results of Vickers hardness for the granular cold accumulator made of the bismuth silver alloy according to the embodiment. As a comparative example, the table also shows the measurement results of Vickers hardness for a conventional pure bismuth granular cold accumulator. In this specification, pure bismuth may refer to bismuth with a purity of 99.99% or more, a purity of 99.995% or more, or a purity of 99.997% or more.
[0046] [Table 1]
[0047] It can be seen from the table that the granular regenerator material of the bismuth silver alloy according to the embodiment has a larger Vickers hardness measurement value (HV) than the granular regenerator material of pure bismuth in the comparative example. That is, the granular regenerator material of the bismuth silver alloy is harder than the granular regenerator material of pure bismuth. Specifically, the Vickers hardness of the granular regenerator material of pure bismuth was measured to be 19.9 (HV), while the Vickers hardness of the granular regenerator material of Bi-1.0%Ag to which 11.0% by weight of silver was added was measured to be 21.9 (HV), the Vickers hardness of the granular regenerator material of Bi-2.0% by weight of silver was measured to be 28.9 (HV), and the Vickers hardness of the granular regenerator material of Bi-5.0% by weight of silver was measured to be 40.9 (HV). The table also includes the standard deviation for each hardness measurement.
[0048] In this way, by adding a small amount of silver to pure bismuth, the hardness (Vickers hardness, HV) is improved. In other words, the granular cold accumulator of the bismuth-silver alloy according to the embodiment has improved toughness (resistance to cracking) compared to the granular cold accumulator of pure bismuth according to the comparative example.
[0049] Therefore, according to the embodiment, the risk of the granular cold accumulator being crushed (pulverized) is reduced when the granular cold accumulator is filled into the cold accumulator in the manufacturing process of the cryogenic refrigerator 10. Similarly, the risk of the granular cold accumulator being crushed by the force from the working gas (e.g., helium gas) flowing in the cold accumulator during the operation of the cryogenic refrigerator 10 is reduced.
[0050] Fig. 3 is a graph showing the volumetric heat capacity of several metal materials in relation to an embodiment. Fig. 3 shows the temperature change of the volumetric heat capacity of lead (Pb), bismuth (Bi), silver (Ag), and copper (Cu) in the temperature range below 70K.
[0051] Lead has been widely used as a cold storage material in the past because it has a high specific heat at extremely low temperatures below about 60 K, but the use of lead is now restricted or prohibited due to its adverse effects on the environment and human body. Bismuth has a relatively high specific heat at extremely low temperatures (for example, in the temperature range from about 10 K to about 30 K), although not as high as lead, and has been used in recent years as a cold storage material to replace lead. As shown in the figure, silver has a higher specific heat than bismuth at temperatures above about 32 K, but a lower specific heat than bismuth at temperatures lower than that. As is known, copper has a high specific heat at temperatures above about 60 K, but its specific heat is considerably smaller at temperatures lower than that.
[0052] The bismuth-silver-based cold storage material according to the embodiment is made by adding a small amount of silver (for example, at most 10% by weight) to pure bismuth, so its specific heat is considered to be approximately equal to that of pure bismuth. However, the specific heat of this bismuth-silver alloy is considered to be slightly lower than that of pure bismuth at temperatures lower than about 32K, and slightly higher than that of pure bismuth at temperatures higher than about 32K.
[0053] 4 is a schematic diagram showing an axial temperature profile of the second regenerator 28 of the cryogenic refrigerator 10 according to the embodiment. In the figure, the vertical axis indicates temperature (K) and the horizontal axis indicates normalized distance. The normalized distance represents the axial position of the second regenerator 28, with the high temperature end (i.e., the upper end in FIG. 2) of the second regenerator 28 being 0 and the low temperature end (the lower end in FIG. 2) of the second regenerator 28 being 1. For example, a normalized distance of 0.5 represents the midpoint (exactly 1 / 2 position) between the high temperature end and the low temperature end of the second regenerator 28 in the axial direction.
[0054] In FIG. 4, the axial temperature profile of the second regenerator 28 according to the embodiment is shown by a dashed line, and the axial temperature profile of the second regenerator 28 according to the comparative example is shown by a solid line. In the second regenerator 28 according to the embodiment, the high temperature side regenerator material 28a, that is, the bismuth silver alloy according to the embodiment, is filled in the range of 0 to 0.5 in normalized distance. On the other hand, in the second regenerator 28 according to the comparative example, pure bismuth is filled as the high temperature side regenerator material 28a in the range of 0 to 0.5 in normalized distance. In both cases, the intermediate regenerator material 28b is filled in the range of 0.5 to 0.75 in normalized distance, and the low temperature side regenerator material 28c is filled in the range of 0.75 to 1 in normalized distance.
[0055] In the example shown in Fig. 4, the temperature at the high temperature end (position of 0 in normalized distance) of the second regenerator 28 is about 38 K. The temperature at the middle (position of 0.5 in normalized distance) of the second regenerator 28 is about 7 to 8 K, although it is slightly different between the embodiment and the comparative example. As described above, the specific heat of the bismuth silver alloy according to the embodiment is lower than that of pure bismuth in most of this temperature range (precisely, in the temperature range of about 32 K or less).
[0056] Therefore, as shown in the figure, the high temperature side cold storage material 28a according to the embodiment has a slightly higher temperature than the comparative example. More precisely, the axial temperature profile (dashed line) of the second cold storage unit 28 according to the embodiment transitions upward in the axial range (range of 0 to 0.5 in normalized distance) corresponding to the high temperature side cold storage material 28a compared to the axial temperature profile (solid line) of the second cold storage unit 28 according to the comparative example. The temperature profiles of the intermediate cold storage material 28b and the low temperature side cold storage material 28c are roughly the same.
[0057] The density of the working gas (typically helium gas) of the cryogenic refrigerator 10 increases as the temperature decreases from room temperature to cryogenic temperature. During operation of the cryogenic refrigerator 10, the temperature of the second regenerator 28 is lower than that of the first regenerator 26, so the density of the gas in the second regenerator 28 is higher than that of the first regenerator 26. Therefore, the lower the temperature of the second regenerator 28, the more gas of the working gas supplied from the compressor 12 to the expander 14 is absorbed (trapped) from the first regenerator 26 to the second regenerator 28. If an excessive amount of gas is distributed unevenly to the second regenerator 28, the refrigeration capacity of the first stage of the cryogenic refrigerator 10 may decrease.
[0058] As described above, by using the bismuth-silver-based regenerator material according to the embodiment as the high-temperature side regenerator material 28a, the temperature profile of the second regenerator 28 can be increased compared to the pure bismuth of the comparative example. This reduces the amount of gas trapped in the second regenerator 28, and accordingly increases the amount of gas used for cooling in the first regenerator 26. According to the embodiment, there is a possibility that the refrigeration capacity of the first stage of the cryogenic refrigerator 10 can be improved compared to the comparative example.
[0059] However, if the silver content is too high, the specific heat of the bismuth-silver based regenerator material decreases significantly compared to pure bismuth, which may result in a decrease in the refrigeration capacity of the cryogenic refrigerator 10.
[0060] Fig. 5 is a graph showing the relationship between the silver content in the bismuth-silver-based cold storage material and the cooling temperature of the first stage of the cryogenic refrigerator 10 according to the embodiment. Fig. 5 plots the measured temperature T1 of the first cooling stage 33 when the silver content in the bismuth-silver alloy used as the high-temperature side cold storage material 28a of the second cold storage unit 28 is set to 0% (i.e. pure bismuth), 0.01% by weight, 0.25% by weight, 1.0% by weight, 2.0% by weight, and 5.0% by weight.
[0061] The cryogenic refrigerator 10 used in the measurements was a 4K-GM refrigerator (model number RDE-412) and compressor (model number F-50) manufactured by Sumitomo Heavy Industries, Ltd. The charged pressure of the working gas was 1.6 MPa. The cryogenic refrigerator 10 was driven by the power frequency of a commercial power source and operated without load. The pressure during operation was 2.2 MPa on the high pressure side and 0.5 MPa on the low pressure side. The bismuth silver-based regenerator material was formed into granules with a particle size within the above-mentioned numerical range.
[0062] As shown in FIG. 5, in the comparative example, that is, when pure bismuth is used as the high temperature side regenerator material 28a, the measured temperature T1 of the first cooling stage 33 is about 40.2K.
[0063] In contrast, in the bismuth silver-based cold storage material according to the embodiment, the measured temperature T1 is lower than that of the comparative example, regardless of the silver content. Specifically, the measured temperature T1 is about 40.0 K (@0.01 wt% Ag), about 38.9 K (@0.25 wt% Ag), about 39.4 K (@1.0 wt% Ag), about 39.8 K (@2.0 wt% Ag), and about 39.2 K (@5.0 wt% Ag).
[0064] In this way, in the bismuth silver-based cold storage material according to the embodiment, by setting the silver content to at most 5 wt %, the first stage refrigeration capacity of the cryogenic refrigerator 10 can be maintained at the same level or improved compared to the pure bismuth cold storage material of the comparative example. In other words, the decrease in specific heat caused by adding silver to bismuth does not adversely affect the refrigeration capacity of the cryogenic refrigerator 10.
[0065] From the viewpoint of increasing the refrigeration capacity of the first stage and lowering the first stage temperature, the bismuth silver based heat accumulator according to the embodiment may have a silver content of at most 2% by weight, or at most 1% by weight, and may have a silver content of at least 0.01% by weight, or at least 0.1% by weight, or at least 0.25% by weight.
[0066] Fig. 6 is a graph showing the relationship between the silver content in the bismuth silver-based cold storage material and the cooling temperature of the second stage of the cryogenic refrigerator 10 according to the embodiment. Fig. 6 plots the measured temperature T2 of the second cooling stage 35 when the silver content in the bismuth silver alloy used as the high-temperature side cold storage material 28a of the second cold storage unit 28 is 0% (i.e. pure bismuth), 0.25% by weight, 1.0% by weight, 2.0% by weight, and 5.0% by weight. The operating conditions of the cryogenic refrigerator 10 are the same as those of the measurement in Fig. 5.
[0067] As shown in Fig. 6, in the comparative example, that is, when pure bismuth is used as the high-temperature side cold accumulator 28a, the measured temperature T2 of the second cooling stage 35 is about 3.86K. In contrast, in the bismuth silver cold accumulator according to the embodiment, the measured temperature T2 is lower than that of the comparative example, regardless of the silver content. Specifically, the measured temperature T2 is about 3.83K (@0.25 wt% Ag), about 3.82 (@1.0 wt% Ag), about 3.83K (@2.0 wt% Ag), and about 3.83K (@5.0 wt% Ag).
[0068] In this way, in the bismuth silver-based heat accumulator according to the embodiment, the silver content is at most 5 wt %, so that the second stage refrigeration capacity of the cryogenic refrigerator 10 can be maintained at the same level or improved compared to the pure bismuth heat accumulator according to the comparative example. From the viewpoint of increasing the second stage refrigeration capacity and lowering the second stage temperature, the silver content of the bismuth silver-based heat accumulator according to the embodiment may be at most 2 wt %, or at most 1 wt %. The silver content may also be at least 0.01 wt %, or at least 0.1 wt %, or at least 0.25 wt %.
[0069] FIG. 7 is a schematic diagram showing the second regenerator 28 of the cryogenic refrigerator according to the modified example. The second regenerator 28 includes a high-temperature side regenerator material 28a, an intermediate regenerator material 28b, and a low-temperature side regenerator material 28c, as in the above-described embodiment. However, the high-temperature side regenerator material 28a is divided into a first region 28a1 on the high-temperature side and a second region 28a2 on the low-temperature side. The first region 28a1 may be filled with a zinc-based regenerator material, and the second region 28a2 may be filled with a bismuth silver-based regenerator material. The zinc-based regenerator material may be zinc or an alloy mainly composed of zinc. The zinc-based regenerator material may be formed into granules like the bismuth silver-based regenerator material. The zinc-based regenerator material is disposed on the opposite side of the magnetic regenerator material (the intermediate regenerator material 28b and the low-temperature side regenerator material 28c) to the bismuth silver-based regenerator material in the axial direction of the second regenerator 28. In order to separate the first area 28a1 and the second area 28a2, a partition member such as a wire mesh may be disposed at the boundary between them.
[0070] The arrangement area of the bismuth silver-based cold accumulator may be selected from the range of 0 to 0.6 in the normalized distance in the axial direction. When another cold accumulator such as a zinc-based cold accumulator is filled on the high temperature side of the bismuth silver-based cold accumulator, the arrangement area of the bismuth silver-based cold accumulator may be selected from the range of 0.2 to 0.6. For example, the arrangement area of the bismuth silver-based cold accumulator may be in the range of 0.25 to 0.5.
[0071] Even when the second regenerator 28 shown in FIG. 7 is employed, the same effects as those of the above-described embodiment can be achieved.
[0072] The present invention has been described above based on examples. It will be understood by those skilled in the art that the present invention is not limited to the above-described embodiments, that various design changes are possible, that various modifications are possible, and that such modifications are also within the scope of the present invention. Various features described in relation to one embodiment can also be applied to other embodiments. A new embodiment resulting from a combination has the combined effects of each of the combined embodiments.
[0073] For example, the shape of the granular heat exchanger material is not limited to a spherical shape, and the granular heat exchanger material may have a block shape, a pellet shape, or any other shape.
[0074] In addition, the bismuth silver-based cold accumulating material according to the embodiment may have a shape other than granular. For example, the bismuth silver-based cold accumulating material may be processed into a wire mesh or formed into a plate. The bismuth silver-based cold accumulating material may be coated, for example, by plating, on the surface of a wire mesh or plate-shaped member formed of a base material (for example, an appropriate metal material such as copper).
[0075] In addition to silver, a second additive different from silver may be added to the bismuth silver-based heat accumulating material. The second additive may be, for example, at least one of tin (Sn), zinc (Zn), aluminum (Al), and silicon (Si), or any mixture thereof.
[0076] In one embodiment, the regenerator material having bismuth as a main component may also have copper as an additive in addition to or in place of silver.
[0077] In the above embodiment, the GM refrigerator is described as an example, but the present invention is not limited thereto. In an embodiment, the cryocooler 10 may be another type of cryocooler, such as a Solvay refrigerator, a Stirling refrigerator, or a pulse tube refrigerator. The magnetic regenerator foam according to the embodiment may be used as a regenerator of any cooling stage (e.g., the coldest cooling stage) in a multi-stage cryocooler.
[0078] The present invention has been described using specific terms based on the embodiments, but the embodiments merely show one aspect of the principles and applications of the present invention, and many modifications and changes in arrangement are permitted to the embodiments without departing from the spirit of the present invention as defined in the claims. [Explanation of symbols]
[0079] 10 cryogenic refrigerator, 14 expander, 26 first regenerator, 28 second regenerator, 28a high temperature side regenerator material, 28b intermediate regenerator material, 28c low temperature side regenerator material.
Claims
1. It contains bismuth as its main component, A cold storage material for a cryogenic refrigerator, comprising at most 10% by weight of silver as an additive.
2. 2. The regenerator material for a cryogenic refrigerator according to claim 1, further comprising at most 5% by weight of silver as an additive.
3. 2. The regenerator material for a cryogenic refrigerator according to claim 1, further comprising at most 2% by weight of silver as an additive.
4. 2. The regenerator material for a cryogenic refrigerator according to claim 1, further comprising at most 1% by weight of silver as an additive.
5. 2. The regenerator material for a cryogenic refrigerator according to claim 1, characterized in that it contains only silver as an additive.
6. 6. The regenerator material for a cryogenic refrigerator according to claim 1, which is in a granular form.
7. A bismuth-silver-based cold storage material containing bismuth as a main component and containing at most 10% by weight of silver as an additive; a magnetic regenerator material disposed at a position different from the bismuth silver-based regenerator material in the axial direction of the regenerator,
8. The regenerator for a cryogenic refrigerator according to claim 7, further comprising a zinc-based regenerator material arranged on the opposite side of the magnetic regenerator material with respect to the bismuth-silver-based regenerator material in the axial direction of the regenerator.
9. A cryogenic refrigerator comprising the regenerator for a cryogenic refrigerator according to claim 7 or 8.
Citation Information
Patent Citations
Cool accumulator
JP2004225920A
Cold storage medium, cold accumulator, and cryogenic cold storage type refrigerating machine
JP2011137632A
Cold storage material and cold storage type cryogenic refrigerator using same
US20210231349A1