Polyarylate resin
By integrating a controlled amount of formate into the polyarylate resin, the issues of color tone and thermal deterioration are addressed, resulting in a resin with enhanced color stability and reduced yellowing.
Patent Information
- Application Number
- JP2023206772
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2023-12-07
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional polyarylate resins suffer from insufficient color tone and thermal deterioration during melt molding, leading to discoloration and yellowing, particularly when used in applications requiring transparency and heat resistance.
Incorporating a controlled amount of formate, specifically sodium formate, into the polyarylate resin composition during polymerization, with a content ranging from 0.1 to 2.0 ppm, enhances the resin's color tone and suppresses thermal degradation.
The polyarylate resin achieves superior color stability and reduced thermal discoloration, maintaining excellent color tone and transparency even under high-temperature conditions.
Smart Images

Figure 2024166046000001 
Figure 2024166046000002 
Figure 2024166046000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyarylate resin and a method for producing the same. [Background technology]
[0002] Polyarylate resins, which are made up of aromatic dicarboxylic acid components and dihydric phenol components, are amorphous, transparent, and have excellent heat resistance, and are used in a variety of applications. Among them, amorphous polyarylate resins, which are made up of residues of terephthalic acid and isophthalic acid and residues of 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), are one of the few super engineering plastics, and because they are transparent, highly heat-resistant, and have excellent mechanical strength and dimensional stability, their molded articles are widely used in fields such as electrical and electronics, automobiles, and machinery.
[0003] However, due to its excellent heat resistance, polyarylate resins are often melt-molded at higher temperatures than general-purpose polymers, and are prone to thermal degradation and coloration during melting. In addition, molded products tend to turn yellow when used for long periods at high temperatures. For this reason, their use has been restricted in some cases to applications where color tone and transparency are required and color change over time is undesirable, such as automobile lamp lenses and camera lenses for in-car or mobile phones.
[0004] In order to solve the above problems, various methods have been investigated in which modifiers such as dyes, pigments, and antioxidants are added during melt molding or melt kneading. For example, Patent Document 1 proposes a method of melt-kneading a dye or pigment and a sulfur-containing carboxylate ester into a polycarbonate resin. For example, Patent Document 2 proposes a method of melt-kneading a polyarylate resin with a phenol-based compound, a phosphorus-based compound, and a lactone-based compound. However, these methods are merely modifications using additives added during melt kneading, and therefore there is a need to improve the color tone and thermal discoloration of the polyarylate resin itself, from the standpoint of reducing the number of types and amounts of additives used.
[0005] In order to improve the color tone and thermal discoloration of polyarylate resin itself, it is necessary to devise a method for producing polyarylate resin from raw materials.As the polymerization method of polyarylate resin, melt polymerization method, solution polymerization method, and interfacial polymerization method are known.In particular, interfacial polymerization method is suitable for making polyarylate resin excellent in color tone because even if the polymer has high heat resistance, the reaction proceeds to a high degree of polymerization at a temperature close to room temperature, and the transparency and heat resistance that are the inherent characteristics of polyarylate resin are fully utilized.
[0006] Furthermore, as described in Patent Document 3, although not limited to the interfacial polymerization method, adding a reducing agent such as sodium hydrosulfite during the polymerization step is effective in preventing discoloration of the dihydric phenol compound, which is a monomer, and further, coloring of the obtained polyarylate resin.
[0007] On the other hand, Patent Document 4 discloses a technique for producing an aromatic polycarbonate having excellent color tone and heat resistance by using sodium hydrosulfite as a reducing agent added during the polymerization step.
[0008] Patent Document 5 discloses a technique for producing polycarbonate with excellent hue by controlling the sodium formate content in sodium hydrosulfite used in the production of polycarbonate to 0.3% by weight or less. In particular, Patent Document 5 proposes that if the sodium formate content in the sodium hydrosulfite used in the production of polycarbonate is more than 0.3% by weight, this causes deterioration of the hue of the resin when heated. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 4-120164 [Patent Document 2] JP 2002-265766 A [Patent Document 3] Special Publication No. 1-18939 [Patent Document 4] Japanese Patent Application Publication No. 7-233253 [Patent Document 5] Patent No. 5544681 Summary of the Invention [Problem to be solved by the invention]
[0010] However, the conventional techniques sometimes have the following problems. It is not possible to obtain polyarylate resin with a sufficiently excellent color tone. When molding using polyarylate resin, coloring due to thermal degradation during melt molding cannot be sufficiently suppressed.
[0011] An object of the present invention is to provide a polyarylate resin which is capable of more sufficiently suppressing coloration due to thermal degradation during melt molding and has a more sufficiently excellent color tone. [Means for solving the problem]
[0012] As a result of extensive research to solve the problem, the inventors have found that when a polyarylate resin contains an appropriate amount of formate, the color tone of the polyarylate resin is sufficiently excellent and coloration due to thermal degradation during melt molding can be more sufficiently suppressed.
[0013] The gist of the present invention is as follows. <1> Contains an aromatic dicarboxylic acid component and a dihydric phenol component as monomer components, A polyarylate resin having a formate content of 0.1 to 2.0 ppm. <2> The polyarylate resin has a color difference a value of -1.0 to 0.5. <1> The polyarylate resin according to claim 1. <3> The polyarylate resin has a powdery or granular shape. <1> or <2> The polyarylate resin according to claim 1. <4> The formate salt is sodium formate. <1> ~ <3> The polyarylate resin according to any one of claims 1 to 5. <5> A molded plate having a thickness of 3 mm molded by injection molding the polyarylate resin has a YI value of 22 or less. <1> ~ <4> The polyarylate resin according to any one of claims 1 to 5. <6> A method for producing a polyarylate resin by polymerizing an aromatic dicarboxylic acid component and a dihydric phenol component, comprising the steps of: A method for producing a polyarylate resin, comprising adding a dithionite having a formate content of 0.4 to 1.5% by mass in an amount of 0.05 to 4.0% by mass based on the dihydric phenol component. <7> The dithionite is sodium dithionite (also known as sodium hydrosulfite) produced by the sodium formate method. <6> A method for producing the polyarylate resin described in claim 1. <8> <1> ~ <5> The polyarylate resin according to any one of the above is produced. <6> or <7> A method for producing the polyarylate resin described in claim 1. Effect of the Invention
[0014] The polyarylate resin of the present invention has a sufficiently good color tone of the polyarylate resin itself, and can more sufficiently suppress coloration due to thermal deterioration during melt molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below. The polyarylate resin of the present invention is an aromatic polyester resin obtained from an aromatic dicarboxylic acid component (including its functional derivative) and a dihydric phenol component, and contains these components as monomer components. Therefore, the polyarylate resin of the present invention can also be expressed as containing residues of an aromatic dicarboxylic acid component and a dihydric phenol component. The structure of the polyarylate resin of the present invention is not particularly limited, and the present invention is applicable to polyarylate resins of any structure. The functional derivative means an organic compound in which the carboxyl group of an aromatic dicarboxylic acid is replaced with a more reactive substituent, and includes, for example, an acid halide having an acid halide group described later.
[0016] The aromatic dicarboxylic acid component for introducing aromatic dicarboxylic acid residues constituting the polyarylate resin is an organic compound containing an aromatic ring and two carboxyl groups per molecule. The carboxyl group may be an acid halide group. An acid halide group is a group in which the hydroxyl group of a carboxyl group is replaced with a halogen atom. Specific examples of such aromatic dicarboxylic acid components include terephthalic acid, isophthalic acid, phthalic acid, chlorophthalic acid, nitrophthalic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, methylterephthalic acid, 4,4'-biphenyldicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 4,4'-diphenylisopropylidenedicarboxylic acid, 1,2-bis(4-carboxyphenoxy)ethane, 5-sodium sulfoisophthalic acid, diphenic acid, and derivatives thereof (e.g., acid halides). These aromatic dicarboxylic acids can be used alone or in combination of two or more. Of these, from the viewpoint of further improving color tone and resistance to discoloration, it is preferred that the polyarylate resin contains at least one of terephthalic acid and isophthalic acid, and preferably both.
[0017] In this specification, the color tone refers to the color tone of the polyarylate resin itself, and is the characteristic of having a smaller color difference a value measured by a color difference meter. Discoloration resistance is a property that more sufficiently suppresses discoloration due to thermal deterioration during melt molding of a polyarylate resin, and refers to a property in which the yellow index (YI) value of the obtained molded product measured with a color tone measuring device is smaller.
[0018] The total content of terephthalic acid and isophthalic acid in the polyarylate resin is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and sufficiently preferably 100% by mass, based on the total amount of aromatic dicarboxylic acid components. The total content of terephthalic acid and isophthalic acid may be the total content of residues of terephthalic acid and isophthalic acid.
[0019] When the polyarylate resin contains terephthalic acid and isophthalic acid as aromatic dicarboxylic acid components, the content ratio thereof is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, the mass ratio of terephthalic acid / isophthalic acid is preferably 0 / 100 to 100 / 0, more preferably 20 / 80 to 80 / 20, even more preferably 40 / 60 to 60 / 40, particularly preferably 45 / 55 to 55 / 45, and sufficiently preferably 50 / 50. The content ratio of terephthalic acid and isophthalic acid may be the content ratio of residues of terephthalic acid and isophthalic acid.
[0020] The dihydric phenol component for introducing the dihydric phenol residue constituting the polyarylate resin is an organic compound containing two phenolic hydroxyl groups per molecule. The phenolic hydroxyl group is a hydroxyl group directly bonded to an aromatic ring. Specific examples of such dihydric phenol components include, for example, 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 2,2-bis(3-methyl-4-hydroxyphenyl)propane (bisphenol C), 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z), 1,1-bis(4-hydroxyphenyl)-1-phenylethane (bisphenol AP), 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, and 2,2-bis(4-hydroxy-3,5-dibromophenyl). Examples of the compounds include propane, 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxybiphenyl [4,4'-biphenol], 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (bisphenol TMC), 4,4'-(1,3-dimethylbutylidene)diphenol, resorcinol, etc. These compounds may be used alone or in combination of two or more. From the viewpoint of further improving color tone and resistance to discoloration, the polyarylate resin preferably contains one or more dihydric phenol components selected from the group consisting of bisphenol A, bisphenol C, bisphenol Z, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, and bisphenol TMC, and more preferably contains bisphenol A.
[0021] The content of bisphenol A in the polyarylate resin is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 0 to 100 mass%, more preferably 40 to 100 mass%, further preferably 60 to 100 mass%, particularly preferably 80 to 100 mass%, and sufficiently preferably 100 mass% based on the total amount of dihydric phenol components. The content of bisphenol A may be the content of bisphenol A residues.
[0022] The polyarylate resin may contain at least one dihydric alcohol component selected from the group consisting of ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, dodecanediol, neopentyl glycol, cyclohexanediol, 1,4-dihydroxymethylcyclohexane, and the like, in place of a portion of the dihydric phenol component, as long as the characteristics and effects of the present invention are not impaired.
[0023] The content of the dihydric alcohol component in the polyarylate resin is not particularly limited, and may be, for example, 50% by mass or less based on the total amount of the dihydric phenol components, and from the viewpoint of further improving color tone and discoloration resistance, is preferably 20% by mass or less, more preferably 10% by mass or less, further preferably 5% by mass or less, particularly preferably 1% by mass or less, and sufficiently preferably 0% by mass. The content of the dihydric alcohol component may be the content of the residue of the dihydric alcohol component.
[0024] The polyarylate resin may further contain a polyfunctional or higher polyvalent monomer component within a range that does not impair the characteristics and effects of the present invention. When the polyarylate resin contains a polyfunctional or higher polyvalent monomer component, a branched structure is introduced into the polyarylate resin. Examples of the polyfunctional or higher polyvalent monomer component include a tricarboxylic acid component such as 1,3,5-benzenecarboxylic acid; and a triol component such as 4,4',4''-trihydroxytriphenylmethane.
[0025] The content of the polyvalent monomer component in the polyarylate resin is not particularly limited, and may be, for example, 20% by mass or less based on the total amount of the dihydric phenol component and the aromatic dicarboxylic acid component, and from the viewpoint of further improving the color tone and discoloration resistance, is preferably 10% by mass or less, more preferably 5% by mass or less, further preferably 2% by mass or less, particularly preferably 1% by mass or less, and sufficiently preferably 0% by mass. The content of the polyvalent monomer component may be the content of the residue of the polyvalent monomer component.
[0026] The polyarylate resin may contain a terminal blocking agent to adjust the molecular weight. Examples of the terminal blocking agent include one or more compounds selected from the group consisting of monohydric phenols such as phenol, cresol, p-tert-butylphenol, 2,3,5-trimethylphenol, 2,3,6-trimethylphenol, and cumylphenol; monohydric acid chlorides such as benzoic acid chloride, methanesulfonyl chloride, and phenyl chloroformate; monohydric alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-butanol, pentanol, hexanol, dodecyl alcohol, stearyl alcohol, benzyl alcohol, and phenethyl alcohol; and monohydric carboxylic acids such as acetic acid, propionic acid, octanoic acid, cyclohexane carboxylic acid, benzoic acid, toluic acid, phenyl acetic acid, p-tert-butyl benzoic acid, and p-methoxyphenyl acetic acid. From the viewpoint of further improving color tone and resistance to discoloration, the end-capping agent is preferably a monohydric phenol (particularly p-tert-butylphenol).
[0027] The content of the terminal blocking agent in the polyarylate resin is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 0.2 to 20 parts by mass, more preferably 0.6 to 10 parts by mass, further preferably 1.2 to 6 parts by mass, and particularly preferably 2 to 5 parts by mass, relative to 100 parts by mass of the dihydric phenol component. The content of the terminal blocking agent may be the content of residues of the terminal blocking agent.
[0028] The polyarylate resin of the present invention contains 0.1 to 2.0 ppm of formate, and from the viewpoint of further improving color tone and discoloration resistance, the content of formate is preferably 0.1 to 1.5 ppm, more preferably 0.1 to 0.8 ppm, even more preferably 0.1 to 0.5 ppm, and particularly preferably 0.2 to 0.4 ppm. In the present invention, by the polyarylate resin containing the formate in the appropriate amount as described above, not only the color tone of the polyarylate resin itself is sufficiently excellent, but also the discoloration resistance of the molded article containing the polyarylate resin is sufficiently excellent. If the content of formate exceeds 2 ppm, thermal deterioration during melt molding is promoted, and yellowing of the resin molded article becomes significant. On the other hand, if the content of formate in the polyarylate resin is less than 0.1 ppm, the color difference a value of the powder or granule becomes very low, but the effect of suppressing thermal discoloration during melt molding becomes insufficient, and yellowing of the resin molded article becomes significant.
[0029] The formate may be an alkali metal salt of formic acid, such as sodium formate, potassium formate, etc. From the viewpoint of further improving color tone and discoloration resistance, the formate is preferably sodium formate, and the above content is preferably the content of sodium formate.
[0030] The content of formate is determined by extracting the formate from 0.5 g of polyarylate resin with 50 mL of ultrapure water and quantitatively analyzing the extracted formate by ion chromatography (IC).
[0031] The formate contained in the polyarylate resin of the present invention may be a residue of the formate contained in a reducing agent (e.g., a dithionite (particularly sodium hydrosulfite)) used during the production of the polyarylate resin, or it may be an additive newly added after the production of the polyarylate resin.
[0032] The formate content can be controlled by the following methods; The polyarylate resin is dissolved and washed with an organic solvent capable of dissolving the polyarylate resin. This can reduce the content of formate. There are various organic solvents capable of dissolving the polyarylate resin depending on the monomer components constituting the polyarylate resin. Examples of the organic solvents include aliphatic chlorine-based solvents such as dichloromethane, 1,2-dichloroethane, chloroform, 1,1,1-trichloroethane, 1,1,2,2-tetrachloroethane, dibromomethane, tribromomethane, bromoethane, 1,1-dibromoethane, and 1-bromopropane, aromatic chlorine-based solvents such as chlorobenzene, o-dichlorobenzene, m-dichlorobenzene, and p-dichlorobenzene, amide-based solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, ether-based solvents such as 1,4-dioxane, 1,3-dioxolane, and tetrahydrofuran, aromatic hydrocarbon-based solvents such as benzene, toluene, and xylene, and mixtures thereof. During the production of polyarylate resin, the formate content contained in dithionite (particularly sodium hydrosulfite) as a reducing agent is adjusted. For example, by reducing the formate content of dithionite (particularly sodium hydrosulfite), the formate content of the polyarylate resin can be reduced. Also, by increasing the formate content of dithionite (particularly sodium hydrosulfite), the formate content of the polyarylate resin can be increased. During the production of polyarylate resin, the amount of dithionite (particularly sodium hydrosulfite) used as a reducing agent is adjusted. For example, by reducing the amount of dithionite (particularly sodium hydrosulfite) used, the formate content of the polyarylate resin can be reduced. Also, for example, by increasing the amount of dithionite (particularly sodium hydrosulfite) used, the formate content of the polyarylate resin can be increased. During the production of polyarylate resin, the formate content in the polyarylate resin can be reduced by strengthening the washing process with pure water (for example, by extending the washing time). By employing one or more of the above-mentioned methods, or by employing two or more of them in combination, the content of formate in the polyarylate resin can be controlled.
[0033] The color difference a value of the polyarylate resin of the present invention is usually -1.0 to 0.5, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably -1.0 to 0.2, more preferably -1.0 to -0.1, still more preferably -1.0 to -0.4, and particularly preferably -0.8 to -0.45.
[0034] The color difference a value is obtained by filling a measurement container with polyarylate resin so that there are no gaps, and measuring in reflection mode with a colorimeter (for example, a colorimeter (ZE6000) manufactured by Nippon Denshoku Industries Co., Ltd.) The polyarylate resin used in the measurement has a particulate shape, and the particle diameter of the particles is 0.7 to 5.0 mm (some may contain fine powder).
[0035] The YI value of a 3 mm thick plate obtained by injection molding the polyarylate resin of the present invention is usually 22 or less, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 19.5 or less, more preferably 14 or less, even more preferably 10 or less, and particularly preferably 9 or less. There is no particular restriction on the lower limit of the YI value, and the YI value is usually 1 or more, particularly 4 or more.
[0036] The YI value is measured by subjecting a 3 mm thick plate obtained by injection molding a polyarylate resin at a resin temperature of 360° C. using a general injection molding machine (e.g., J110AD injection molding machine manufactured by JSW Corporation) to a color tone measuring device (e.g., SZ-Σ90 type colorimeter manufactured by Nippon Denshoku Industries Co., Ltd.). The polyarylate resin used for molding has a particulate shape, and the particle diameter of the particles is 0.7 to 5.0 mm (some may contain fine powder).
[0037] In general, from the viewpoints of mechanical properties and workability during melt molding and melt kneading, the polyarylate resin of the present invention preferably has an inherent viscosity of 0.40 to 1.30 dl / g, more preferably 0.45 to 1.10 dl / g, even more preferably 0.45 to 0.90 dl / g, particularly preferably 0.50 to 0.80 dl / g, and sufficiently preferably 0.50 to 0.60 dl / g.
[0038] The inherent viscosity (ηinh) is an index of molecular weight, and the value measured by the following method is used. A resin solution of polyarylate resin is prepared using 1,1,2,2-tetrachloroethane as a solvent so that the concentration is 1 g / dl, and the relative viscosity (ηrel) is measured at a temperature of 25°C. The inherent viscosity is calculated from the obtained relative viscosity using the following formula. ηinh(dl / g) = Ln(ηrel) / c (c: concentration)
[0039] The polymerization method for the polyarylate resin is not particularly limited as long as the resulting polyarylate resin has the above-mentioned properties, and may be a known method, for example, the following method: A solution polymerization method in which a dicarboxylic acid halide containing an aromatic dicarboxylic acid component is reacted with a diol containing a dihydric phenol component in an organic solvent; A melt polymerization method in which the dicarboxylic acid and the diol are heated in the presence of acetic anhydride or diallyl carbonate; and An interfacial polymerization method in which a divalent carboxylic acid halide dissolved in an organic solvent that is not compatible with water is mixed with a diol dissolved in an alkaline aqueous solution.
[0040] From the viewpoint of further improving color tone and resistance to discoloration, the polymerization method for the polyarylate resin used in the present invention is preferably an interfacial polymerization method, since the reaction proceeds to a high degree of polymerization at a relatively low temperature.
[0041] When the interfacial polymerization method is applied, the organic solvent used is not particularly limited as long as it is incompatible with water and dissolves the divalent carboxylic acid halide used and the polyarylate resin produced. Suitable organic solvents include, for example, aliphatic chlorine-based solvents such as dichloromethane, 1,2-dichloroethane, chloroform, 1,1,1-trichloroethane, and tetrachloroethane; aromatic chlorine-based solvents such as chlorobenzene and o-dichlorobenzene; and mixtures thereof. In the isolation and drying process of the produced polyarylate resin, it is better to avoid organic solvents with too high a boiling point. Among them, aliphatic chlorine-based solvents (especially dichloromethane) are preferable as organic solvents.
[0042] In the interfacial polymerization method, it is preferable to use a dithionite produced by a sodium formate method as a reducing agent, because the formate content in the polyarylate resin described above can be easily achieved, and as a result, the polyarylate resin of the present invention having excellent color tone and resistance to discoloration can be easily produced.
[0043] The dithionite may be an alkali metal salt of dithionous acid, such as sodium dithionite (also known as sodium hydrosulfite), potassium dithionite, etc. From the viewpoint of further improving color tone and discoloration resistance, the dithionite is preferably sodium hydrosulfite.
[0044] From the viewpoint of further improving color tone and discoloration resistance, the dithionite is preferably sodium hydrosulfite produced by the sodium formate method. Dithionite produced by a method other than the sodium formate method (e.g., an electrolytic method) does not contain formate itself.
[0045] The sodium formate method is a method for producing sodium hydrosulfite using sodium formate. More specifically, sodium formate is dissolved in aqueous alcohol (e.g. aqueous methanol), and sodium hydroxide and sulfurous anhydride are added to cause a reaction.
[0046] The content of formate contained in the dithionite (particularly, the content of sodium formate contained in sodium hydrosulfite produced by the sodium formate method) is preferably 0.4 to 1.5 mass%, more preferably 0.4 to 1.0 mass%, further preferably 0.5 to 1.0 mass%, and particularly preferably 0.5 to 0.8 mass%, from the viewpoint of further improving color tone and discoloration resistance. If the content of the formate (particularly, sodium formate) is too small or too large, it becomes difficult for the obtained polyarylate resin to achieve the formate content of the polyarylate resin of the present invention, and coloring due to thermal deterioration during melt molding cannot be sufficiently suppressed. The content of the formate (particularly, sodium formate) is a ratio to the total amount of dithionite (particularly the total amount of sodium hydrosulfite). The total amount of dithionite refers to the total amount of dithionite and formate contained in said dithionite, and in particular, when by-products and decomposition products are contained in the dithionite, the total amount including said by-products and decomposition products. The total amount of sodium hydrosulfite refers to the total amount of sodium hydrosulfite and sodium formate contained in said sodium hydrosulfite, and in particular, when by-products and decomposition products are contained in the sodium hydrosulfite, the total amount including said by-products and decomposition products.
[0047] Methods for quantifying formate contained in dithionite (particularly, methods for quantifying formate contained in sodium hydrosulfite produced by the sodium formate method) include the method specified in "Standards and Criteria for Food Additives (Ministry of Health and Welfare Notification No. 370 of 1959) Article 2 Additives (as of November 30, 2017)" and a method for detecting organic acids by ion chromatography. In the present invention, a method for detecting organic acids by ion chromatography is adopted.
[0048] The content of formate contained in dithionite (particularly sodium hydrosulfite) can be controlled, for example, by washing and purifying the dithionite (particularly the obtained sodium hydrosulfite) with an aqueous methanol solution. In detail, the content of formate (particularly sodium formate) can be controlled by adjusting the number of washings with the aqueous methanol solution and the methanol concentration of the aqueous methanol solution. For example, the more the number of washings, the lower the content of formate (especially sodium formate), whereas the less the number of washings, the higher the content of formate (especially sodium formate). For example, the higher the methanol concentration of the aqueous methanol solution, the lower the content of formate (particularly, sodium formate), whereas the lower the methanol concentration of the aqueous methanol solution, the higher the content of formate (particularly, sodium formate).
[0049] The amount of the reducing agent (e.g., dithionite (particularly sodium hydrosulfite produced by the formate sodium method)) added is preferably 0.05 to 4.0 mass% relative to the mass of the dihydric phenol component used, more preferably 0.1 to 2.0 mass%, even more preferably 0.2 to 1.5 mass%, sufficiently preferably 0.2 to 1.1 mass%, and more preferably 0.3 to 0.8 mass%, from the viewpoint of further improving color tone and discoloration resistance. If the amount of the reducing agent added is too small or too large, it becomes difficult to achieve the formate content of the polyarylate resin of the present invention. For example, if the amount added is less than 0.05 mass%, the effect of preventing discoloration of the dihydric phenol component is insufficient, and discoloration due to thermal deterioration during melt molding cannot be sufficiently suppressed. On the other hand, if the amount added is increased to more than 4.0 mass%, the formate content of the polyarylate resin of the present invention is too high, and discoloration due to thermal deterioration during melt molding cannot be sufficiently suppressed.
[0050] In the interfacial polymerization method, a polymerization catalyst may be used.The polymerization catalyst in the interfacial polymerization method may include tertiary amines such as trimethylamine, triethylamine, tri-n-butylamine, tri-n-propylamine, tri-isopropylamine, trihexylamine, tridecylamine, N,N-dimethylcyclohexylamine, pyridine, quinoline, dimethylaniline, etc.; quaternary ammonium salts such as trimethylbenzylammonium halide, triethylbenzylammonium halide, tri-n-propylbenzylammonium halide, tri-n-butylbenzylammonium halide, etc.; quaternary phosphonium salts such as trimethylbenzylphosphonium halide, tetramethylbenzylphosphonium halide, triethylbenzylphosphonium halide, tri-n-butylbenzylphosphonium halide, tetra-n-butylphosphonium halide, triphenylbenzylphosphonium halide, tetraphenylphosphonium halide, etc.; crown ethers such as 18-crown-6, 18-benzocrown-6, 18-dibenzocrown-6, 15-crown-5, etc. In particular, from the standpoint of polymerization rate and cost, quaternary ammonium salts (particularly trimethylbenzylammonium halide and tri-n-butylbenzylammonium halide) are preferred.
[0051] The amount of the polymerization catalyst used is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 0.1 to 5 mass %, more preferably 0.1 to 3 mass %, and even more preferably 0.1 to 1.5 mass % based on the dihydric phenol component.
[0052] When the polyarylate resin of the present invention is produced by the interfacial polymerization method, it is preferable to employ the following method. A dihydric phenol component, end-capping agent, reducing agent, and polymerization catalyst are dissolved in an alkaline aqueous solution to obtain an aqueous layer. Separately, an aromatic dicarboxylic acid component is dissolved in an organic solvent to obtain an organic layer. The two incompatible liquids (the aqueous layer and organic layer described above) are mixed under strong stirring, and a polymerization reaction is carried out until a high degree of polymerization is reached due to interlayer migration of the dihydric phenol component and the end-capping agent component in the aqueous layer. After the reaction is completed, stirring is stopped and the organic layer is separated into a state in which the produced polyarylate resin is dissolved, and an aqueous layer in which by-products such as salts and unreacted monomers are dissolved, and the organic layer is then neutralized with an inorganic acid such as acetic acid or phosphoric acid.
[0053] The organic layer after neutralization contains unreacted monomers, low molecular weight polyarylate resins, by-product salts, and other impurities, and in order to remove them, the organic layer is thoroughly washed with pure water using means such as a static separation method or a centrifugation method. Both the static separation method and the centrifugation method utilize extraction of various impurities contained in the organic layer into pure water, and either method may be used as appropriate. Washing with pure water can reduce the content of formate in the polyarylate resin. In addition, the content of formate can be further reduced by increasing the number of times of washing with pure water or the washing time.
[0054] The process of granulating the polyarylate resin from the organic layer in which the thoroughly washed polyarylate resin is dissolved includes the hot water granulation method of distilling off the organic solvent in hot water, the kneader method of heating with a kneader or the like to evaporate the organic solvent and pulverize the remaining polymer, the spray dry method of spraying the organic solvent with a spray to instantly evaporate the organic solvent, and the reprecipitation method of pouring an organic solvent solution into a poor solvent for the polyarylate resin to precipitate and precipitate the polymer content, etc. Any method may be appropriately adopted, but in the present invention, it is preferable to carry out the process using the hot water granulation method in view of the properties of the particles obtained and the simplicity of the device.
[0055] When dichloromethane is used as the organic solvent, in hot water granulation, 50°C hot water is placed in a hot water jacketed tank equipped with an agitator, stirred, and then the hot water is withdrawn from the bottom of the tank and introduced into a wet grinder and returned to the same tank while circulating, while supplying an organic solvent solution in which polyarylate resin has been dissolved, and while maintaining the liquid temperature in the tank at 50°C, the organic solvent is distilled off to granulate the polyarylate resin, and a polyarylate / hot water slurry is obtained in the wet grinder on the circulation line, taking care not to generate large particles, and this slurry is withdrawn through a filter to obtain only the polyarylate resin powder.
[0056] The granulated polyarylate resin powder is dried by a suitable method using a suitable dryer depending on the production amount, etc. At this time, if the drying temperature exceeds 140°C, the vaporized dichloromethane undergoes thermal decomposition, and hydrogen chloride is generated, causing severe corrosion of the inner wall of the dryer, so operation at 140°C or less (particularly 120 to 135°C) is desirable. By setting the drying temperature at 120 to 135°C, the formate content of the polyarylate resin can be kept within the above-mentioned range, while moisture and dichloromethane can be sufficiently removed.
[0057] When the polyarylate resin of the present invention has a powdery or granular shape (or a powdery or granular form), the particle diameter of the particles is 0.7 to 5.0 mm (some particles may be fine powders). Furthermore, the polyarylate resin of the present invention may contain some particles in which two or more particles are pressed together.
[0058] The particle size of the polyarylate resin is a value obtained by measuring 50 random particles of the polyarylate resin using a microscope (VHX-6000) manufactured by Keyence Corporation.
[0059] The polyarylate resin of the present invention can be melt-kneaded with various thermoplastic resins and various additives to form a polyarylate resin composition with characteristic properties. As a kneading method, there are methods using a general extruder, such as a single-screw extruder, a twin-screw extruder, a roll kneader, a Brabender, etc., and among them, a method using a twin-screw extruder is preferable because it improves the kneading state of multiple raw materials. It is also preferable to use a static mixer or a dynamic mixer in combination. The raw materials may be added from a hopper or a side feeder. The resin composition obtained by melt kneading is preferably in the form of pellets. The polyarylate resin composition includes the polyarylate resin of the present invention and may further include at least one selected from a thermoplastic resin and an additive. For example, the polyarylate resin composition may include only a polyarylate resin, a thermoplastic resin, and an additive. At this time, the polyarylate resin composition may or may not include a thermoplastic resin and an additive independently.
[0060] Examples of the thermoplastic resin include nylon resin, polycarbonate resin, polyester resin, polyphenylene ether resin, polystyrene resin, etc. The polyester resin refers to polyester other than the polyarylate resin of the present invention.
[0061] The content of the thermoplastic resin in the polyarylate resin composition is not particularly limited, and may be, for example, 100% by mass or less, particularly 50% by mass or less, based on the polyarylate resin, and from the viewpoint of further improving color tone and discoloration resistance, is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less. The lower limit of the content of the thermoplastic resin is not particularly limited, and the content of the thermoplastic resin may be 0% by mass.
[0062] As the additives, additives that may be conventionally added to polyarylate resins can be used, such as antioxidants, lubricants, dyes and pigments, flow improvers, flame retardants, and fillers. Examples of the antioxidant include various antioxidants such as hindered phenol-based, hindered amine-based, thioether-based, and phosphorus-based antioxidants. The lubricant may be, for example, a fatty acid salt such as a stearate salt. Examples of the dyes and pigments include metal complex dyes, anthraquinone dyes, perinone dyes, inorganic pigments such as carbon black and inorganic metals, and organic pigments containing organic compounds such as azo pigments and polycyclic pigments. Examples of the flow improver include inorganic compounds such as fatty acid salts, and organic compounds including fluorine-based and amide-based compounds. Examples of the flame retardant include various types of halogen-based, phosphorus-based, nitrogen-based and hydrated metal-based flame retardants. Examples of the filler include inorganic fillers such as glass, mica, talc, and silica.
[0063] The content of additives in the polyarylate resin composition is not particularly limited, and may be, for example, 50% by mass or less, particularly 30% by mass or less, based on the polyarylate resin, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, particularly preferably 0.8% by mass or less, sufficiently preferably 0.4% by mass or less, and even more preferably 0% by mass. When two or more kinds of additives are contained, the total content thereof may be within the above range. The lower limit of the content of additives is not particularly limited, and the content of additives may be 0% by mass.
[0064] In particular, the content of the antioxidant in the polyarylate resin composition is not particularly limited, but the polyarylate resin composition of the present invention is sufficiently excellent in color tone and discoloration resistance even without the antioxidant. Therefore, the content of the antioxidant in the polyarylate resin composition may be 20 mass% or less, particularly 10 mass% or less, based on the polyarylate resin, and from the viewpoint of further improving the color tone and discoloration resistance, it is preferably 5 mass% or less, more preferably 1 mass% or less, even more preferably 0.4 mass% or less, particularly preferably 0.2 mass% or less, and sufficiently preferably 0 mass%. When two or more kinds of antioxidants are contained, the total content thereof may be within the above range. EXAMPLES
[0065] The present invention will be described in detail with reference to examples. However, the present invention is not limited to these examples, and various modifications and applications are possible without departing from the spirit of the present invention.
[0066] <Method for determining formate in sodium hydrosulfite> (1) Quantitative determination of sodium formate in sodium hydrosulfite Approximately 0.1 g of sodium hydrosulfite was weighed into a PP container, 20 mL of ultrapure water was added, and the mixture was left to stand overnight at room temperature to dissolve. The solution was then diluted 100 times with ultrapure water, and the diluted solution was filtered through a 0.2 μm membrane filter and quantitatively analyzed by ion chromatography (IC). A calibration curve method (multiple calibration curve) was used for quantification.
[0067] <Evaluation method for polyarylate resin powder> (1) Method for determining residual sodium formate in polyarylate resin powder Approximately 0.5 g of the freeze-pulverized polyarylate resin powder was weighed in a PP (polypropylene) container. The shape of the freeze-pulverized polyarylate resin was composed of particles with a particle diameter of 0.3 to 1.5 mm, including fine powder of 0.3 mm or less. The particle diameter was obtained by measuring 50 random particles using a Keyence microscope (VHX-6000). Next, 50 mL of ultrapure water was added, and extraction was performed by heating for 1 hour in a dryer set at 120°C. After that, the mixture was filtered through a 0.2 μm membrane filter, and quantitative analysis was performed by ion chromatography (IC). For quantification, a calibration curve method (single-point calibration curve) was used to calculate the amount of formate ions using the following formula 1, and the amount of sodium formate was converted using formula 2.
[0068]
number
[0069] A = Concentration of calibration standard (formic acid) B = IC peak area of the sample being analyzed C = Blank IC peak area D = dilution ratio E = IC peak area of calibration standard F = weight of sample to be analyzed
[0070]
number
[0071] G = amount of formate ions H = sodium formate formula weight (68.01) I = formate ion formula weight (45.02)
[0072] (2) Color difference a value of polyarylate resin powder A colorimeter (ZE6000) manufactured by Nippon Denshoku Industries Co., Ltd. was used. The polyarylate resin powder was packed into a measurement container so that there were no gaps, set on a sample holder, and measured in reflection mode. The particle diameter of the particles was 0.7 to 5.0 mm (some may contain fine powder).
[0073] (3) Yellow Index YI Value of Injection Molded Polyarylate Resin Powder The obtained polyarylate resin powder was molded into a 3 mm thick sample plate at a resin temperature of 360°C using a general injection molding machine (e.g., JSW J110AD injection molding machine), and the color was measured using a colorimeter (Nippon Denshoku Kogyo SZ-Σ90 colorimeter). Evaluation was performed according to the following criteria. ◎◎: 10 or less (excellent); ◎: Over 10, 14 or less (excellent); ○: Over 14, 19.5 or less (good); △: Over 19.5, 22 or less (Pass: No practical problems); ×: Over 22 (Failed: Problems in practical use).
[0074] <Sodium hydrosulfite> Sodium hydrosulfite was prepared by the following method.
[0075] Sodium hydrosulfite A (manufacturing method: sodium formate method) (sodium formate content 0.7% by mass) and sodium hydrosulfite B (manufacturing method: sodium formate method) (sodium formate content 0.9% by mass). Sodium hydrosulfite was produced by the sodium formate method. The amount of sodium formate contained in the produced sodium hydrosulfite was quantitatively analyzed by ion chromatography (IC). The sodium formate content differed slightly depending on the production lot, and the one with a content of 0.7% by mass was designated as sodium hydrosulfite A, and the one with a content of 0.9% by mass was designated as sodium hydrosulfite B.
[0076] Sodium hydrosulfite C (manufacturing method: sodium formate method): sodium formate content 3.0 mass% (used in Comparative Examples 1 and 2). Sodium hydrosulfite C was produced by blending commercially available sodium formate with sodium hydrosulfite A (sodium formate content: 0.7% by mass) so that the sodium formate content was 3.0% by mass.
[0077] Sodium hydrosulfite D (manufacturing method: electrolytic method): sodium formate content 0 mass% (used in Comparative Example 5). Sodium hydrosulfite D was produced by electrolysis.
[0078] <Inherent viscosity of polyarylate resin> A resin solution was prepared using 1,1,2,2-tetrachloroethane as a solvent to give a concentration of 1 g / dl, and the relative viscosity (ηrel) was measured at a temperature of 25° C. The inherent viscosity was calculated from the obtained relative viscosity using the following formula. ηinh(dl / g) = Ln(ηrel) / c (c: concentration)
[0079] Example 1 (Method of synthesizing polyarylate resin powder) In a reaction vessel equipped with a stirrer, 100 parts by mass of 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 3.8 parts by mass of p-tert-butylphenol, 37 parts by mass of sodium hydroxide, 0.6 parts by mass of trimethylbenzylammonium chloride, and sodium hydrosulfite A were charged at 0.5% by mass relative to the mass of the dihydric phenol component, and dissolved in 1103 parts by mass of water to obtain an aqueous layer. Separately, 92 parts by mass of a 1 / 1 mixture of terephthalic acid chloride / isophthalic acid chloride was dissolved in 895 parts by mass of dichloromethane to obtain an organic layer. This organic layer was added to the aqueous layer previously prepared under strong stirring, and a polymerization reaction was carried out at 15°C for 2 hours. After this, the aqueous layer and the organic layer were separated, and 10 parts by mass of acetic acid was added to the organic layer to stop the reaction, and further washing with water was repeated until it became neutral, to obtain a 17% by mass dichloromethane solution of polyarylate. The dichloromethane solution of polyarylate was granulated by hot water granulation method, and the water and dichloromethane were thoroughly dried using a paddle type hot air dryer at 120 to 135°C to obtain the polyarylate resin powder of Example 1. The particle diameter of the particles was 0.7 to 5.0 mm (some may contain fine powder). Other characteristic values of the obtained polyarylate resin powder were as shown in Table 1.
[0080] Example 2 Polyarylate resin powder particles were synthesized in the same manner as in the "method of synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite A was added in an amount of 1.0 mass% relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.6 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some may contain fine powder). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0081] Example 3 Polyarylate resin powder particles were synthesized in the same manner as in the "method of synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite B was added in an amount of 1.2 mass% relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some may contain fine powder). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0082] Example 4 Polyarylate resin powder particles were synthesized in the same manner as in the "method of synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite B was added in an amount of 3.0 mass% relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 0.9 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some may contain fine powder). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0083] Comparative Example 1 Polyarylate resin powder particles were synthesized in the same manner as in the "method of synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite C was added in an amount of 3.0% by mass relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some particles may contain fine powder). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0084] Comparative Example 2 Polyarylate resin powder particles were synthesized in the same manner as in the "method of synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite C was added in an amount of 0.5% by mass relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some particles may contain fine powder). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0085] Comparative Example 3 Polyarylate resin powder particles were synthesized in the same manner as in the "method of synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite B was added in an amount of 7.0 mass% relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some particles may contain fine powder). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0086] Comparative Example 4 Polyarylate resin powder particles were synthesized in the same manner as in the "method of synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite A was added in an amount of 0.1 mass% relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some particles may contain fine powder). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0087] Comparative Example 5 Polyarylate resin powder particles were synthesized in the same manner as in the "method of synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite D was added in an amount of 0.5% by mass relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some particles may contain fine powder). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0088] [Table 1]
[0089] The above examples and comparative examples reveal the following: By adjusting the amount of sodium formate contained in the polyarylate resin to an appropriate amount, the color tone of the polyarylate resin itself becomes good, and yellowing of molded products caused by thermal deterioration due to heat melting can be more sufficiently reduced; and The polyarylate resin of the present invention can be produced by using a specific amount of sodium hydrosulfite having a specific sodium formate content. [Industrial Applicability]
[0090] The polyarylate resin of the present invention is useful in various applications requiring prevention of yellowing of molded products, such as lamp covers and camera lenses mounted on automobiles, camera lenses mounted on mobile phones and smartphones, modules constituting electronic substrates, and replacement of plastic materials for parts mainly made of glass members.
Claims
1. Contains an aromatic dicarboxylic acid component and a dihydric phenol component as monomer components, A polyarylate resin having a formate content of 0.1 to 2.0 ppm.
2. The polyarylate resin according to claim 1, wherein the polyarylate resin has a color difference a value of -1.0 to 0.
5.
3. The polyarylate resin according to claim 1 , wherein the polyarylate resin has a powdery or granular shape.
4. 2. The polyarylate resin of claim 1, wherein the formate is sodium formate.
5. 2. The polyarylate resin according to claim 1, wherein a molded plate having a thickness of 3 mm obtained by injection molding the polyarylate resin has a YI value of 22 or less.
6. A method for producing a polyarylate resin by polymerizing an aromatic dicarboxylic acid component and a dihydric phenol component, comprising the steps of: A method for producing a polyarylate resin, comprising adding a dithionite having a formate content of 0.4 to 1.5% by mass in an amount of 0.05 to 4.0% by mass based on the dihydric phenol component.
7. The method for producing a polyarylate resin according to claim 6, wherein the dithionite is sodium dithionite produced by a sodium formate method.
8. A method for producing the polyarylate resin according to claim 6, which produces the polyarylate resin according to any one of claims 1 to 5.
Citation Information
Patent Citations
Tool correction system
JP1980044681A
Borosilicate glass
JP1989018939A
Colored polycarbonate resin composition
JP1992120164A
Production of aromatic polycarbonate
JP1995233253A
Polyarylate resin composition
JP2002265766A