Polyethylene microporous membrane, method for manufacturing the same, and separator including that microporous membrane
A microporous polyethylene membrane with controlled molecular weight and biaxial stretching enhances heat resistance and mechanical strength, addressing safety issues in high-temperature batteries and enabling high-capacity applications.
Patent Information
- Application Number
- JP2024078102
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2044-05-13
AI Technical Summary
Microporous polyethylene membranes used in secondary batteries lack sufficient heat resistance, mechanical strength, and permeability, especially in high-temperature environments, posing safety risks and limiting their application in larger batteries.
A microporous polyethylene membrane with specific molecular weight, thickness, perforation strength, gas permeability, and tensile strength ratios, produced through a sequential biaxial stretching process, ensuring high mechanical strength, permeability, and improved heat resistance.
The membrane provides excellent thermal safety in high-temperature environments, preventing smoke or ignition, and supports high-capacity, high-output batteries by maintaining mechanical integrity and permeability.
Smart Images

Figure 2024166119000001 
Figure 2024166119000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a polyethylene microporous membrane, a method for producing the same, and a separator including the microporous membrane. According to one aspect, the present disclosure relates to a polyethylene microporous membrane having improved heat resistance, a method for producing the same, and a separator including the microporous membrane. [Background technology]
[0002] Microporous polyethylene membranes are used in a variety of fields, such as separation filters, secondary battery separators, fuel cell separators, supercapacitor separators, etc. In particular, they are widely used as secondary battery separators because of their excellent electrical insulation properties, ion permeability, etc.
[0003] In recent years, secondary batteries have become larger and larger in capacity for application in electric vehicles, ESS (Energy Storage Systems), etc., and ensuring the safety of the battery has become an even more important factor. For example, when a battery is exposed to or operated in a high-temperature environment, the separator may shrink, causing an internal short circuit, which may cause a fire. Therefore, there is a need to develop a polyethylene microporous membrane with excellent heat resistance that can withstand the temperature rise of the battery. In addition to heat resistance, high mechanical strength is required to improve safety during the manufacturing process and use of the battery, and high permeability is required to improve capacity and output.
[0004] As a method for enhancing such safety, Korean Patent Publication No. 10-2016-0106177 discloses a method for improving the half-crystallization time t 1 / 2However, such a microporous membrane has a shrinkage rate in the lateral direction of only about 6% at 105°C, and is inferior in safety to batteries in a high-temperature environment such as a hot-box evaluation, so that it is not suitable for application to high-capacity and large-sized batteries.
[0005] Therefore, there is a need for the development of a polyethylene microporous membrane that not only has high mechanical strength and permeability and significantly improved heat resistance at higher temperatures, but also can achieve excellent battery safety, particularly in a hot box evaluation at 130°C, which is an evaluation index for high-temperature safety. Summary of the Invention [Problem to be solved by the invention]
[0006] In order to solve the above-mentioned problems, an object of the present disclosure is to provide a polyethylene microporous membrane that has excellent mechanical strength and permeability as well as significantly improved heat resistance at high temperatures, a production method thereof, and a separator including the microporous membrane.
[0007] In particular, the objective of the present invention is to provide a microporous polyethylene membrane that can achieve excellent battery safety even in a hot box evaluation at 130°C after the battery is assembled.
[0008] The microporous membrane of the present disclosure can be widely applied to green technology fields such as electric vehicles, battery charging stations, and other battery-based solar and wind power generation. In addition, the microporous membrane of the present disclosure can be used in eco-friendly electric vehicles, hybrid vehicles, and the like to reduce air pollution and greenhouse gas emissions and prevent climate change. The microporous membrane can be used as a separator for a secondary battery. [Means for solving the problem]
[0009] As one means for achieving the above object, the present disclosure provides a polymer having a weight average molecular weight of 1×10 5 g / mol~10×10 5 g / mol of polyethylene, the microporous membrane has a thickness of 3 μm to 20 μm, a puncture strength of 0.25 N / μm or more, and a gas permeability of 1.5×10 -5 Darcy or more, the transverse shrinkage rate measured after leaving it at 131℃ for 1 hour is 10% or less, and the longitudinal tensile strength (TS MD ) is 1500kg / cm 2 The transverse tensile strength (TS TD ) is 2000kg / cm 2 The ratio of the tensile strength in the longitudinal direction to the tensile strength in the transverse direction (TS MD / TS TD ) is 0.5 to 0.7.
[0010] In one embodiment, the polyethylene microporous membrane has a tensile strength in the longitudinal direction of 2000 kg / cm 2 The tensile strength in the transverse direction is 2800kg / cm 2 It may be more than that.
[0011] In one embodiment, the average longitudinal tensile strength and transverse tensile strength are 2500 kg / cm 2 The average value may be (TS MD +TS TD ) / 2.
[0012] In one embodiment, the polyethylene microporous membrane may have a puncture strength of 0.50 N / μm or more.
[0013] In one embodiment, the microporous polyethylene membrane may have a porosity of 30% to 70%.
[0014] In one embodiment, the polyethylene microporous membrane may be produced by a wet process including a sequential biaxial stretching step.
[0015] In addition, as another means for achieving the above object, the present disclosure provides a method for producing a polymerizable composition comprising the steps of: (a) providing a polymerizable composition having a weight average molecular weight of 1×10 5 g / mol~10×10 5 (b) melt-kneading a mixture containing a polyethylene resin having a molecular weight of 1000 g / mol and a diluent in an extruder to produce a melt; (b) extruding the melt into a sheet; (c) sequentially biaxially stretching the sheet in the longitudinal and transverse directions to form a film; (d) extracting the diluent from the stretched film and drying it; and (e) heat-treating the dried film at a temperature at which 20% to 50% of the crystals of the dried film are melted, and the stretch ratio (SR) in the longitudinal direction of the step (c) is 1000 g / mol. MD ) is 4.0 times or more, and the transverse stretch ratio (SR TD ) is 5.3 times or more, and the ratio of the longitudinal stretch ratio to the transverse stretch ratio (SR MD / SR TD ) is 0.5 to 0.75.
[0016] In one embodiment, the temperature at which 20% to 50% of the crystals in the film dried in step (e) melt may be 133°C to 145°C.
[0017] In another aspect of the present disclosure, a separator is provided that includes the polyethylene microporous membrane. Fabricating a separator from the microporous membrane may include cutting the microporous membrane to a desired size depending on the application. Also, the porosity and thickness of the microporous membrane may be adjusted within the porosity and thickness range depending on the specific application.
[0018] In one embodiment, an electrochemical device is provided that includes the separator.
[0019] In one embodiment, the electrochemical device may be a secondary battery including the separator between a positive electrode and a negative electrode.
[0020] As another means for achieving the above-mentioned object, the present disclosure provides a separator including the above-mentioned polyethylene microporous membrane. Effect of the Invention
[0021] The polyethylene microporous membrane according to the present disclosure has excellent mechanical strength and permeability, and can ensure significantly improved heat resistance at high temperatures.
[0022] In addition, the polyethylene microporous membrane according to the present disclosure has a puncture strength of 0.25 N / μm or more and a tensile strength in the machine direction (MD) of 1500 kg / cm 2 The tensile strength in the transverse direction (TD) is 2000kg / cm 2 or more, and the gas permeability is 1.5×10 -5 It could be better than Darcy.
[0023] Additionally, the polyethylene microporous membrane according to the present disclosure may have a transverse shrinkage percentage of 10% or less measured after being left at 131° C. for 1 hour.
[0024] In addition, the present disclosure can provide a battery having excellent high-temperature thermal safety, in which the battery does not emit smoke or catch fire in a high-temperature environment, by including the polyethylene microporous membrane according to one embodiment. In particular, the present disclosure can provide a battery having excellent high-temperature thermal safety, in which the battery does not emit smoke or catch fire in a hot box evaluation at a high temperature of 130°C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The embodiments described herein may be modified into various other forms, and the technology according to one aspect is not limited to the embodiments described below. In addition, the embodiments of one aspect are provided to more completely explain the present disclosure to those having average knowledge in the art.
[0026] Additionally, as used in the specification and the appended claims, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context indicates otherwise.
[0027] In addition, the numerical ranges used herein include lower and upper limits, and all values within the ranges, increments logically derived in the form and width of the ranges defined, all values that are doubly limited, and all possible combinations of upper and lower limits of numerical ranges that are mutually limited in different ways. Unless otherwise defined herein, values outside the numerical ranges that may occur due to experimental error or rounding up are also included in the numerical ranges defined.
[0028] Furthermore, throughout the specification, unless otherwise specified to the contrary, "comprising" an element means that it may further include other elements, rather than excluding other elements.
[0029] The present disclosure relates to a method for determining the longitudinal tensile strength (TS MD ) and transverse tensile strength (TS TD ) ratio (TS MD / TS TD This was devised with the understanding that when the thickness of a glass is controlled within a specific range, it is possible to obtain excellent mechanical strength and transmittance even with a very thin thickness, and also to ensure significantly improved heat resistance at high temperatures.
[0030] According to one embodiment, the weight average molecular weight is 1×10 5 g / mol~10×10 5 g / mol of polyethylene, and has a longitudinal tensile strength (TS MD ) and transverse tensile strength (TS TD ) and the ratio of longitudinal tensile strength to transverse tensile strength (TS MD / TS TD ) within a specific range, even if the thickness is as thin as 3μm to 20μm, the puncture strength is 0.25N / μm or more and the gas permeability is 1.5×10 -5 It is possible to provide a microporous polyethylene membrane having a shrinkage rate of 10% or less in the transverse direction measured after standing at 131° C. for 1 hour.
[0031] A secondary battery according to one embodiment includes a polyethylene microporous membrane that satisfies all of the above-mentioned physical properties, thereby ensuring both excellent battery performance and safety. In particular, the present disclosure can provide a battery that has excellent high-temperature thermal safety, in which the battery does not emit smoke or catch fire in a hot box evaluation at a high temperature of 130°C. In other words, the polyethylene microporous membrane of the present disclosure is suitable for use in high-power / high-capacity batteries by satisfying all of the above-mentioned physical properties.
[0032] In one aspect, a polyethylene microporous membrane satisfying all of the above-mentioned physical properties can be produced by a stretching process under specific conditions, whereby the ratio of tensile strength in the longitudinal direction to tensile strength in the transverse direction is realized within a specific range.
[0033] In one aspect, the polyethylene microporous membrane can be produced by a stretching process under specific conditions and a heat setting process under specific conditions, so that the ratio of tensile strength in the longitudinal direction to tensile strength in the transverse direction is realized in a specific range.
[0034] In one aspect, the polyethylene microporous membrane may be produced by a wet process including a successive biaxial stretching step at a specific stretch ratio or more, which can provide a polyethylene microporous membrane that satisfies all of the above-mentioned physical properties.
[0035] Specifically, the polyethylene microporous membrane is produced by extruding a mixture obtained by dissolving a diluent in a polyethylene resin, and sequentially biaxially stretching the mixture to a specific stretch ratio to produce a film, and then extracting the diluent from the film. The polyethylene microporous membrane may be produced by a wet method including a typical sequential biaxial stretching step known to those skilled in the art, and is not limited as long as it can produce a microporous membrane having the above-mentioned physical properties.
[0036] In one embodiment, the longitudinal stretch ratio (SR MD ) is 4.0 times or more, and the transverse stretch ratio (SR TD ) is 5.3 times or more, and the ratio of the longitudinal stretch ratio to the transverse stretch ratio (SR MD / SR TD) may be 0.5 to 0.75. This allows the polyethylene microporous membrane to have excellent mechanical strength and permeability even when it is thin, and also has significantly improved heat resistance at high temperatures.
[0037] The microporous polyethylene membrane will be described in more detail below.
[0038] In one embodiment, the ratio of the longitudinal tensile strength to the transverse tensile strength (TS MD / TS TD ) may be 0.5 or more and 0.65 or less, or 0.7 or less, for example, 0.5 to 0.7 or 0.5 to 0.65.
[0039] In one embodiment, the polyethylene microporous membrane has a longitudinal tensile strength (TS MD ) is 1500kg / cm 2 More than 1800kg / cm 2 or more than 2000kg / cm 2 TS may be more than MD The upper limit of the value is not particularly limited, but for example, 3500 kg / cm 2 Below 3000kg / cm 2 In a specific embodiment, the TS MD The value is 1500kg / cm 2 ~3500kg / cm 2 , 1800kg / cm 2 ~3500kg / cm 2 , or 2000 kg / cm 2 ~3000kg / cm 2 It may be, but is not limited to this.
[0040] In one embodiment, the disclosed microporous membrane has a transverse tensile strength (TS TD ) is 2000kg / cm 2 More than 2500kg / cm 2 More than 2800kg / cm 2 or more than 3000kg / cm 2 TS may be more than TDThe upper limit of the value is not particularly limited, but for example, 5000 kg / cm 2 Below 4500kg / cm 2 In a specific embodiment, the TS TD The value is 2000kg / cm 2 ~5000kg / cm 2 , 2500kg / cm 2 ~5000kg / cm 2 , 2800kg / cm 2 ~4500kg / cm 2 , or 3000 kg / cm 2 ~4500kg / cm 2 It may be, but is not limited to this.
[0041] In one embodiment, the average value of the tensile strength in the longitudinal direction and the tensile strength in the transverse direction is 2500 kg / cm 2 More than 2600kg / cm 2 or more than 2700kg / cm 2 The upper limit of the average value is not particularly limited, but may be, for example, 4250 kg / cm 2 Below 4000kg / cm 2 or less than 3750kg / cm 2 In a specific embodiment, the average value is 2500 kg / cm 2 ~4250kg / cm 2 , 2600kg / cm 2 ~4000kg / cm 2 , or 2700 kg / cm 2 ~3750kg / cm 2 It may be, but is not limited to this.
[0042] TS in the above range MD Value, T.S. TD These values and average values can be achieved by controlling the longitudinal stretch ratio and the transverse stretch ratio in the stretching step to a specific ratio, or by controlling the temperature in the heat setting step to a specific range, in the production of the polyethylene microporous membrane, but are not necessarily limited thereto.
[0043] The microporous membrane according to one embodiment has a small thickness but has a TS in the above range. MD / TS TD The microporous membrane according to the present disclosure has a high tensile strength and a low thermal shrinkage, which significantly improves the heat resistance. That is, the following high-temperature hot box evaluation was performed on a battery manufactured using the microporous membrane according to one embodiment as a separator, and the battery did not emit smoke or fire in a high-temperature environment, so that the battery has excellent battery safety. The manufacturing and evaluation method of the battery for the evaluation is as follows. A positive electrode using NCM622 (Ni:Co:Mn=6:2:2) as an active material and a negative electrode using graphite carbon as an active material are wound together with the microporous membrane according to the present disclosure and placed in an aluminum pouch to manufacture a battery. Next, an electrolyte solution in which 1M lithium hexafluorophosphate (LiPF6) is dissolved in a solution containing ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate in a volume ratio of 3:5:2 is injected into the inside of the battery and sealed to manufacture a battery with a capacity of 2 Ah. Next, after aging and degassing the battery, it was fully charged to 4.2V, placed in an oven and heated at 5°C / min. After reaching 130°C, it was left for 30 minutes and checked to see if the battery emitted smoke or caught fire.
[0044] In one embodiment, the thickness of the polyethylene microporous membrane may be 3 μm to 20 μm, specifically 3 μm to 15 μm, more specifically 3 μm to 10 μm, and even more specifically 3 μm to 7 μm. The microporous membrane of the present disclosure can achieve excellent puncture strength, gas permeability, heat shrinkage rate, and tensile strength even in a very thin film state with a thickness in the above-mentioned range, and in particular, it has been revealed that it can have excellent thermal safety in a hot box evaluation according to the evaluation method of the following examples. In addition, it has excellent resistance to external stress generated during battery manufacturing, and temperature rise and dendrites generated during battery charging and discharging, and has low internal resistance of the battery, thereby improving the charge and discharge performance of the battery.
[0045] In one embodiment, the polyethylene microporous membrane may have a puncture strength of 0.25 N / μm or more even if it has a thickness in the above range. Specifically, the puncture strength may be 0.40 N / μm or more or 0.50 N / μm or more, and the upper limit is not particularly limited, but may be, for example, 1.0 N / μm or less. In a specific embodiment, the puncture strength may be 0.25 N / μm to 1.0 N / μm, 0.40 N / μm to 1.0 N / μm, or 0.50 N / μm to 1.0 N / μm, but is not limited thereto. By satisfying the puncture strength in the above range, the membrane has excellent resistance to external stress generated during the manufacture of the battery and dendrites generated during the charge and discharge of the battery, and the safety of the battery can be ensured. In addition, the membrane can be thinned as a separator for a secondary battery, and is suitable for use in high-capacity / high-output batteries.
[0046] In one embodiment, the polyethylene microporous membrane has a pore size of 1.5×10 -5 Darcy or more, and specifically, the gas permeability is 1.6 × 10 -5 Darcy or higher, 3.0×10 -5 Darcy or less, or 5.0×10 -5 Darcy or less. In a specific embodiment, the gas permeability is 1.5×10 -5 Darcy~5.0×10 -5 Darcy or 1.6×10 -5 Darcy~3.0×10 -5 By satisfying the gas permeability in the above range, it is possible to have excellent ion conductivity, and the charge / discharge characteristics of the battery can be improved due to the low internal resistance of the battery.
[0047] In one aspect, the polyethylene microporous membrane may have a transverse shrinkage percentage measured after standing at 131°C for 1 hour of 10% or less, 8% or less, or 6% or less, and the lower limit is not particularly limited, but may be, for example, 0.1%, 0.5%, or 1%. In a specific aspect, the shrinkage percentage may be, but is not limited to, 0.1% to 10%, 0.5% to 8%, or 1% to 6%.
[0048] In one embodiment, the polyethylene microporous membrane may have a porosity of 30% to 70%, 40% to 70%, or 50% to 70%, but is not limited thereto, in terms of mechanical strength and ionic conductivity. The porosity is calculated by the following mathematical formula. Specifically, a sample with a width of A cm, a length of B cm, and a thickness of T cm is prepared, and the mass is measured, and the porosity is calculated from the ratio of the resin mass and the microporous membrane mass of the same volume.
[0049] Porosity (%)=100×{1-M / (A×B×T×ρ)} In the above formula, M is the mass of the microporous membrane (g), ρ is the density of the polyethylene resin constituting the microporous membrane (g / cm 3 ).
[0050] In one aspect, the polyethylene microporous membrane may be produced by a wet process including a successive biaxial stretching step, which can provide a polyethylene microporous membrane that satisfies all of the above-mentioned physical properties.
[0051] Specifically, the polyethylene microporous membrane is produced by extruding and sequentially biaxially stretching a mixture obtained by dissolving a diluent in a polyethylene resin into a film, and extracting the diluent from the film. The polyethylene microporous membrane may be produced by a wet method including a typical sequential biaxial stretching process known to those skilled in the art, and is not limited as long as it can produce a microporous membrane having the above-mentioned physical properties.
[0052] In one embodiment, the longitudinal stretch ratio (SR MD ) is 4.0 times or more, and the transverse stretch ratio (SR TD) is 5.3 times or more, and the ratio of the longitudinal stretch ratio to the transverse stretch ratio (SR MD / SR TD ) may be 0.5 to 0.75. This allows the polyethylene microporous membrane to have excellent mechanical strength and permeability even when it is thin, and also has significantly improved heat resistance at high temperatures.
[0053] Hereinafter, the method for producing the polyethylene microporous membrane of the present disclosure will be described.
[0054] A method for producing a polyethylene microporous membrane according to one embodiment includes: (a) producing a polyethylene microporous membrane having a weight average molecular weight of 1×10 5 g / mol~10×10 5 (b) melt-kneading a mixture containing a polyethylene resin having a molecular weight of 1000 g / mol and a diluent in an extruder to produce a melt; (b) extruding the melt into a sheet; (c) sequentially biaxially stretching the sheet in the longitudinal and transverse directions to form a film; (d) extracting the diluent from the stretched film and drying it; and (e) heat-treating the dried film at a temperature at which 20% to 50% of the crystals of the dried film are melted, and the stretch ratio (SR) in the longitudinal direction of the step (c) is 1000 g / mol. MD ) is 4.0 times or more, and the transverse stretch ratio (SR TD ) is 5.3 times or more, and the ratio of the longitudinal stretch ratio to the transverse stretch ratio (SR MD / SR TD ) may be 0.5 to 0.75.
[0055] Each manufacturing step will now be described.
[0056] First, step (a) is a step of melt-kneading a mixture containing a polyethylene resin and a diluent by an extruder to produce a melt, and the mixture contains the polyethylene resin and the diluent in a weight ratio of 10-60:90-40 in order to form pores, and specifically, may contain the diluent in a weight ratio of 20-40:80-60, but is not particularly limited as long as the object of the present disclosure is achieved. When the weight ratio satisfies the above range, the melt has sufficient fluidity, and a uniform sheet can be easily formed in the subsequent step, and sufficient orientation is achieved during the stretching process, and mechanical strength is easily ensured, so that problems such as breakage during the stretching process can be prevented.
[0057] The polyethylene resin may be or contain high density polyethylene from the viewpoints of strength, extrusion kneadability, stretchability, heat resistance of the final microporous membrane, and the like.
[0058] In one embodiment, the polyethylene resin has a weight average molecular weight of 1×10 5 g / mol~10×10 5 g / mol, specifically 3×10 5 g / mol~8×10 5 It may be in g / mol, but is not necessarily limited thereto.
[0059] In one embodiment, the polyethylene resin may have a melting temperature of 130° C. or higher, specifically, 130° C. to 140° C., but is not necessarily limited thereto. The melting temperature of the polyethylene resin can be determined by DSC.
[0060] In one embodiment, the diluent can be any organic compound that forms a single phase with the polyethylene resin at the extrusion temperature without any limitations. For example, the diluent may be one or a combination of two or more selected from the group consisting of aliphatic or cyclic hydrocarbons such as nonane, decane, decalin, paraffin oil, and paraffin wax; phthalic acid esters such as dibutyl phthalate and dioctyl phthalate; C10-C20 fatty acids such as palmitic acid, stearic acid, oleic acid, linoleic acid, and linolenic acid; and C10-C20 fatty alcohols such as cetyl alcohol, stearyl alcohol, and oleyl alcohol. A specific example of the diluent is paraffin oil having a kinetic viscosity at 40° C. of 20 cSt to 200 cSt, but is not limited thereto.
[0061] In addition, the mixture may further contain one or more conventional additives for improving specific functions, such as an oxidation stabilizer, a UV stabilizer, and an antistatic agent, within a range that does not significantly deteriorate the properties of the microporous membrane.
[0062] Step (b) is a step of extruding the molten material to form it into a sheet, and may be performed by any method known to those skilled in the art without limitation. For example, the molten material may be extruded through a T-die, cooled to a temperature of 10°C to 80°C, and then formed into a sheet by a casting or calendaring method.
[0063] In step (c), the longitudinal stretch ratio (SR MD ) is 4.0 times or more, and the transverse stretch ratio (SR TD ) is 5.3 times or more, and the ratio of the longitudinal stretch ratio to the transverse stretch ratio (SR MD / SR TD ) may be 0.5 to 0.75. This allows the longitudinal tensile strength (TS MD ) and transverse tensile strength (TS TD ) ratio (TS MD / TS TD ) can be controlled within a specific range, making it possible to produce a microporous polyethylene membrane that has excellent mechanical strength and permeability even at a thin thickness and also has significantly improved heat resistance at high temperatures.
[0064] The stretch ratio in the longitudinal direction may be specifically 4 to 10, more specifically 5 to 8, and the stretch ratio in the transverse direction may be 5.3 to 15, more specifically 6 to 10. When the stretch ratios in each direction satisfy the above-mentioned ranges, a polyethylene microporous membrane having the physical properties targeted in the present disclosure can be produced.
[0065] The SR MD / SR TD By satisfying the range of 0.5 to 0.75, the ratio of tensile strength in the longitudinal direction to the transverse direction that the present disclosure aims to achieve, and the tensile strength of 1500 kg / cm 2 Tensile strength in the longitudinal direction of 2000kg / cm 2 The above lateral tensile strength can be ensured.
[0066] The stretching in step (c) may be performed by a sequential stretching method using a roll or a tenter, and may be performed at a temperature in the range of 60°C lower than the melting temperature of polyethylene to the melting temperature of polyethylene. When the stretching is performed at a temperature in the above range, the fluidity of the polyethylene resin for effective stretching can be ensured. In particular, the sheet is stretched uniformly over the entire sheet, and no breakage due to stretching occurs, so that the stretching can be performed stably. This allows the production of a high-quality microporous membrane having uniform physical properties such as gas permeability, puncture strength, and tensile strength over the entire membrane. As an example, the stretching may be performed at 80°C to 140°C or 90°C to 120°C, but is not limited thereto.
[0067] Step (d) is a step of extracting and drying the diluent from the stretched film, and is carried out by extracting the diluent in the film using an organic solvent, and drying the organic solvent with the film in which the diluent has been replaced with the organic solvent. The organic solvent can be used without any particular limitation as long as it can extract the diluent. Specifically, methyl ethyl ketone, methylene chloride, hexane, etc. may be used as the organic solvent because of its high extraction efficiency and fast drying.
[0068] Step (d) is preferably carried out at a high temperature due to the increased solubility of the diluent and the organic solvent, but may be carried out at a temperature of 40° C. or less from the standpoint of safety due to the boiling of the organic solvent.
[0069] Step (e) is a step of heat-treating the dried film at a temperature at which 20% to 50% of the crystals in the dried film melt. Heat is applied while the film is forcibly held using a roll or tenter device so as not to cause dimensional changes in the longitudinal and transverse directions, thereby removing residual stress in the film and reducing the heat shrinkage rate of the finally produced polyethylene microporous membrane.
[0070] The ratio of the longitudinal stretch ratio to the transverse stretch ratio (SR MD / SR TD) is heat-treated under the above-mentioned temperature conditions to produce a polyethylene microporous membrane that has properties that cannot be achieved by microporous membranes produced by conventional methods. A microporous membrane with such properties is suitable for use in high-power / high-capacity batteries. A high-power / high-capacity battery refers to a secondary battery that can transmit a significant amount of power during discharge and can be used in applications requiring high power, such as electric vehicles, power tools, energy storage systems, and portable electronic devices.
[0071] In one embodiment, the temperature at which 20% to 50% of the crystals of the dried film melts varies depending on the molecular weight of the polyethylene used and the stretching ratio of the film. In the present disclosure, by using a polyethylene with a high molecular weight as the polyethylene resin for producing a polyethylene microporous membrane, the temperature at which 20% to 50% of the film crystals melts may be 133°C to 145°C, specifically 135°C to 140°C. Conventionally, heat treatment was performed at a temperature below 133°C, but the microporous membrane produced by heat treatment at this temperature has a drawback of not satisfying sufficient physical properties. In contrast, in the present disclosure, the above physical properties can be obtained by using a highly crystalline polyethylene with a high melting point. For example, conventional microporous membranes do not satisfy sufficient levels of gas permeability and puncture strength, or even if they are excellent in gas permeability and puncture strength, they have a drawback of being unsuitable for use as a separator for a secondary battery because of poor heat shrinkage.
[0072] In one aspect, the heat treatment in step (e) may be performed at a temperature in the range of 133° C. to 145° C., specifically, at a temperature in the range of 135° C. to 140° C. By performing the heat treatment at a temperature in the above range, a polyethylene microporous membrane satisfying all of the physical properties targeted by the present disclosure can be produced.
[0073] In one embodiment, step (e) may be heat-setting by heat stretching and heat-relaxing. That is, the tension during heat treatment may be adjusted and heat treatment may be performed in various ways. The heat treatment may be repeated 1 to 3 times, but is not necessarily limited thereto.
[0074] The step (e) may include, for example, a heat stretching step of stretching in the longitudinal or transverse direction, a heat setting step of fixing the length / width in the longitudinal and transverse directions and applying heat, and a heat relaxing step of relaxing (shrinking) in the longitudinal or transverse direction. As an example, the heat relaxing step may be relaxing to 80% to 99% or 90% to 99% of the transverse width before the heat relaxing step, and the heat stretching step may be stretching to 120% to 160% or 140% to 160% of the transverse width before the heat stretching step.
[0075] The present disclosure provides a separator including the polyethylene microporous membrane as described above, and the separator may be a separator used in any known energy storage device, and is not particularly limited, but a non-limiting example is a separator used in a lithium secondary battery.
[0076] Examples and experimental examples are specifically illustrated below. However, the examples and experimental examples described below are merely a partial example, and the technology described in this specification is not limited thereto.
[0077] [Physical property measurement method] 1. Weight average molecular weight (g / mol) Weight average molecular weight (Mw) was measured using high temperature gel permeation chromatography (GPC) from Agilent Technologies, Inc. Analysis was performed at 140°C using PLgel Guard and PLgel Olexis as GPC columns, 1,2,4-trichlorobenzene (TCB) as a solvent, and polystyrene as a standard sample.
[0078] 2. Thickness of microporous membrane (μm) The thickness of the microporous membrane was measured using a contact type thickness gauge with a thickness precision of 0.1 μm. The measurement pressure was 0.63 N using a TESA Mu-Hite Electronic Height Gauge manufactured by TESA.
[0079] 3.Punching strength (N / μm) The puncture strength was measured by pressing the microporous membrane at a speed of 120 mm / min using a pin tip with a diameter of 1.0 mm and a curvature radius of 0.5 mm attached to an INSTRON Universal Test Machine (UTM) 3345. The puncture strength was calculated by dividing the load (N) at which the microporous membrane broke by the thickness (μm) of the microporous membrane.
[0080] 4. Gas permeability (Darcy) The gas permeability was measured using a porometer (CFP-1500-AEL, manufactured by PMI). Generally, the gas permeability is expressed by the Gurley number, but since the Gurley number does not correct for the influence of thickness, it is difficult to understand the relative permeability due to the pore structure. To solve this problem, the gas permeability of the present disclosure is measured using the Darcy permeability constant calculated by the following mathematical formula 1. Nitrogen was used as the gas, and the average value of the Darcy permeability constant measured in the range of 100 to 200 psi was calculated.
[0081] [Mathematical formula 1] Darcy transmission constant (C)=(8F·T·V) / (πD 2 (P 2 -1) F=Flow rate (cc / min) T = sample thickness (mm) V = gas viscosity (0.185 cp for N2) D = sample diameter (mm) P = pressure (psi)
[0082] 5. Tensile strength (kg / cm 2 ) The tensile strength was measured in accordance with ASTM D882 using an INSTRON Universal Test Machine (UTM) 3345, by pulling the microporous membrane in both the transverse and machine directions at a speed of 100 mm / min, at which the microporous membrane broke.
[0083] 6. Transverse shrinkage rate (%) A 15 cm x 15 cm microporous membrane with a length of 10 cm and a marking on the vertical and horizontal directions was left in an oven (Yamato Scientific Co., Ltd. DKN612) stabilized at 131°C for 1 hour, and then the change in length was measured and the horizontal shrinkage rate was calculated according to the following Equation 2.
[0084] [Mathematical formula 2] Transverse shrinkage rate (%) = {(transverse length before heating - transverse length after heating) / transverse length before heating} x 100
[0085] 7. Hotbox Evaluation The hot box evaluation was performed using a battery assembled by applying a polyethylene microporous membrane to the separator. Specifically, a positive electrode using NCM622 (Ni:Co:Mn=6:2:2) as an active material and a negative electrode using graphite carbon as an active material were wound together with the prepared microporous membrane and placed in an aluminum pouch, and then an electrolyte solution in which 1M lithium hexafluorophosphate (LiPF6) was dissolved in a solution containing ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate in a volume ratio of 3:5:2 was injected and sealed to assemble a battery with a capacity of 2 Ah. After aging and degassing, the assembled battery was fully charged to 4.2 V, placed in an oven and heated at 5°C / min until it reached 130°C, and then left for 30 minutes to measure the changes in the battery.
[0086] If the battery emitted smoke or caught fire after being left at 130°C for 30 minutes, it was rated as Fail; if there was no change in the battery voltage / current and no smoke or fire occurred, it was rated as Pass.
[0087] 8. Thermal property analysis of the film The phenomenon of the crystals of the film introduced into the heat setting device melting due to temperature was analyzed using a differential scanning calorimeter (DSC) Discovery DSC250 from TA Instruments, with a sample weight of 5 mg and a scan rate of 10° C. / min.
[0088] In detail, the temperature at which 20% of the crystals of the film introduced into the heat fixing device melts (T m1 ) and the temperature at which it melts by 50% (T m2 ) are the temperatures (T m1 ) and the temperature at the point where the heat capacity is 50% (T m2 ) was measured using a method to calculate the
[0089] 9.Porosity (%) The porosity was calculated according to the following mathematical formula: Specifically, a sample with a width of A cm, a length of B cm, and a thickness of T cm was prepared, and its mass was measured. The porosity was calculated from the ratio of the mass of the resin and the mass of the microporous membrane of the same volume.
[0090] Porosity (%)=100×{1-M / (A×B×T×ρ)} In the above formula, M is the mass of the microporous membrane (g), ρ is the density of the polyethylene resin constituting the microporous membrane (g / cm 3 ).
[0091] <Example 1> Weight average molecular weight is 5.0×10 5 g / mol and a high-density polyethylene resin (0.95 g / cm 3 A mixture containing 30:70 by weight of 1,2-dichlorophenyl ether (COOH) and paraffin oil having a kinetic viscosity of 80 cSt at 40° C. was melt-kneaded in a twin-screw extruder to produce a molten product.
[0092] The melt was continuously extruded by a T-die, and a sheet having a width of 300 mm and an average thickness of 700 μm was produced using a casting roll set at 30° C. The sheet was stretched in the longitudinal direction by a roll method to 6 times at a stretching temperature of 100° C., and then guided to a tenter and stretched in the transverse direction to 8 times at a stretching temperature of 118° C.
[0093] Paraffin oil was extracted from the film that had been stretched in the machine direction and the transverse direction at 25°C using methylene chloride, and the film from which the paraffin oil had been extracted was dried at 50°C. The dried film was heat-stretched in the transverse direction to 150% at 136°C, the temperature at which 38% of the crystals of the dried film melt, using a tenter-type heat setting device, and then heat-set for 10 seconds and heat-relaxed (shrunk) to 93% of the width before the heat-relaxing process to produce a microporous membrane with a thickness of 5 μm. The melting temperature was measured using a differential scanning calorimeter (DSC) Discovery DSC250 provided by TA Instruments, and was measured under conditions of a sample weight of 5 mg and a scan speed of 10°C / min.
[0094] The properties of the final microporous membrane and the performance of the battery using the same are shown in Table 2 below.
[0095] <Examples 2 to 4 and Comparative Examples 1 to 5> A polyethylene microporous membrane was produced in the same manner as in Example 1, except that the longitudinal / transverse stretch ratio and heat setting temperature were changed to the conditions shown in Table 1. The physical properties of the finally produced microporous membrane and the performance of the battery using the same are recorded in Table 2 below.
[0096] [Table 1]
[0097] [Table 2]
[0098] Referring to Tables 1 and 2, the microporous membranes of the examples satisfied all of the physical properties targeted by the present disclosure, and the batteries using the microporous membranes passed the hot box test and achieved excellent thermal safety.
[0099] The microporous membranes of Comparative Example 1 and Comparative Example 2 have a ratio of longitudinal stretch ratio to transverse stretch ratio (SR MD / SR TD As a result of the stretching step, the ratio of the tensile strength in the longitudinal direction to the tensile strength in the transverse direction (TS MD / TS TD ) exceeds 0.7 and the lateral shrinkage rate at 131°C exceeds 10%, which significantly reduces the thermal safety of the battery to which it is applied.
[0100] The microporous membrane of Comparative Example 3 had a longitudinal stretch ratio to transverse stretch ratio (SR MD / SR TD ), but the heat setting temperature was lower than in the examples. As a result, the ratio of the tensile strength in the machine direction to the tensile strength in the transverse direction (TS MD / TS TD ) exceeds 0.7 and the lateral shrinkage rate at 131°C exceeds 10%, which significantly reduces the thermal safety of the battery to which it is applied.
[0101] The microporous membrane of Comparative Example 4 had a longitudinal stretch ratio of less than 4.0 times and a longitudinal / transverse stretch ratio ratio (SR MD / SR TD ) the stretching step was performed, but the tensile strength in the machine direction was so low that the film broke during the process, making it impossible to manufacture the film.
[0102] The microporous membrane of Comparative Example 5 had a transverse stretch ratio of less than 5.3 times and a ratio of the longitudinal stretch ratio to the transverse stretch ratio (SR MD / SR TD ) the stretching step is performed, the gas permeability targeted by the present disclosure cannot be achieved, and the battery using this has the drawback of being unable to achieve the required battery performance and having significantly reduced thermal safety.
[0103] As described above, the present disclosure has been described in the present specification by using specific details and limited embodiments, but this is merely provided for a more general understanding of the present disclosure, and the present disclosure is not limited to the above embodiments. A person having ordinary knowledge in the field to which the present disclosure belongs can make various modifications and variations from such descriptions.
Claims
1. Weight average molecular weight is 1×10 5 g / mol~10×10 5 g / mol polyethylene, The microporous membrane has a thickness of 3 μm to 20 μm, a puncture strength of 0.25 N / μm or more, and a gas permeability of 1.5×10 -5 Darcy or more, the transverse shrinkage rate measured after leaving at 131° C. for 1 hour is 10% or less, and the tensile strength in the longitudinal direction (TS MD ) is 1500 kg / cm 2 The tensile strength in the transverse direction (TS TD ) is 2000 kg / cm 2 or more, and the ratio of the tensile strength in the longitudinal direction to the tensile strength in the transverse direction (TS MD / TS TD ) is 0.5 to 0.
7.
2. Tensile strength in the longitudinal direction is 2000 kg / cm 2 or more, and the tensile strength in the transverse direction is 2800 kg / cm 2 The polyethylene microporous membrane according to claim 1,
3. The average longitudinal and transverse tensile strength is 2500 kg / cm 2 The polyethylene microporous membrane according to claim 1,
4. The polyethylene microporous membrane according to claim 1, having a puncture strength of 0.50 N / μm or more.
5. The polyethylene microporous membrane according to claim 1, having a porosity of 30% to 70%.
6. The polyethylene microporous membrane according to claim 1, produced by a wet process including a successive biaxial stretching step.
7. (a) Weight average molecular weight is 1×10 5 g / mol~10×10 5 A step of melt-kneading a mixture containing a polyethylene resin having a molecular weight of 100 g / mol and a diluent in an extruder to produce a melt; (b) extruding the melt into a sheet; (c) sequentially biaxially stretching the sheet in the machine and transverse directions to form a film; (d) extracting the diluent from the stretched film and drying; (e) heat treating the dried film at a temperature at which 20% to 50% of the crystals in the dried film melt; The stretch ratio (SR) in the longitudinal direction in the step (c) MD ) is 4.0 times or more, and the transverse stretch ratio (SR TD ) is 5.3 times or more, and the ratio of the longitudinal stretch ratio to the transverse stretch ratio (SR MD / SR TD ) is 0.5 to 0.
75.
8. The method for producing a microporous polyethylene membrane according to claim 7, wherein in step (e), a temperature at which 20% to 50% of the crystals of the dried film melt is 133°C to 145°C.
9. A separator comprising the polyethylene microporous membrane according to any one of claims 1 to 6.
10. An electrochemical device comprising the separator according to claim 9.
11. The electrochemical element according to claim 10, which is a secondary battery including the separator between a positive electrode and a negative electrode.
Citation Information
Patent Citations
Polyolefin microporous membrane
CN115149204A
Microporous membrane, method for manufacturing the same membrane, and method for using the same membrane.
JP2012525991A
A method for producing polyolefin microporous membranes with excellent productivity and easily controllable physical properties.
JP2013530261A
High-strength separator
JP2021193177A
Polyolefin microporous film
WO2018164056A1