Polypropylene microporous membrane, method for manufacturing the same, and separator including that microporous membrane

The production of a microporous polypropylene membrane with specific properties through a wet method and controlled heat treatment addresses the issues of low strength and heat resistance in conventional membranes, ensuring battery safety and performance in high-temperature environments.

JP2024166169AActive Publication Date: 2024-11-28SK IE TECH CO LTD

Patent Information

Application Number
JP2024080229
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-16
Publication Date
2024-11-28
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

Conventional microporous polypropylene membranes used in secondary batteries suffer from low perforation strength, uneven pore sizes, and inadequate heat resistance, making them unsuitable for high-capacity and large-sized batteries, particularly in high-temperature environments.

Method used

A microporous polypropylene membrane is produced with a viscosity average molecular weight of 1×10^6 g/mol to 3×10^6 g/mol, thickness of 3μm to 30μm, perforation strength of 0.20N/μm or more, gas permeability of 1.0×10^-5 Darcy or higher, porosity of 25% to 60%, and average pore size of 25nm to 50nm, achieved through a wet method involving sequential biaxial stretching and controlled heat treatment.

Benefits of technology

The membrane exhibits excellent perforation strength, permeability, and heat resistance, ensuring battery safety and performance in high-temperature environments, preventing smoke or ignition in hot box evaluations at 140°C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166169000001_ABST
    Figure 2024166169000001_ABST
Patent Text Reader

Abstract

To provide a polypropylene microporous membrane excellent in the puncture strength and permeability and significantly improved in the heat resistance at high temperature, a method for manufacturing the same, and a separator including the microporous membrane.SOLUTION: A polypropylene microporous membrane contains a polypropylene with a viscosity average molecular weight of 1×106 g / mol to 3×106 g / mol. The microporous membrane has a thickness of 3 μm to 30 μm, and a puncture strength of 0.20 N / μm or more, a gas permeability of 1.0×10-5 Darcy or more, a porosity of 25% to 60%, an average pore size of 25 nm to 50 nm, and a shrinkage rate in the transverse direction of 20% or less as measured after being left at 150°C for 1 hour.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polypropylene microporous membrane, a method for producing the same, and a separator including the microporous membrane. According to one aspect, the present disclosure relates to a polypropylene microporous membrane having excellent puncture strength and permeability as well as improved heat resistance, a method for producing the same, and a separator including the microporous membrane. [Background technology]

[0002] Polyolefin microporous membranes are used in a variety of fields, such as separation filters, secondary battery separators, fuel cell separators, supercapacitor separators, etc. In particular, they are widely used as secondary battery separators because of their excellent electrical insulation properties and ion permeability.

[0003] In recent years, secondary batteries have become larger and larger in capacity to be applied to electric vehicles, ESS (Energy Storage Systems), etc., and ensuring the safety of the battery has become an even more important factor. For example, when a battery is exposed to or operated in a high-temperature environment, the separator may shrink, causing an internal short circuit, which may cause a fire. Therefore, there is a need to develop a polyolefin-based microporous membrane with excellent heat resistance that can withstand the temperature rise of the battery. In addition to heat resistance, high mechanical strength is required to improve safety during the manufacturing process and use of the battery, and high permeability is required to improve capacity and output.

[0004] The high molecular weight polyethylene used as the main material for secondary battery separators has a low melting temperature of about 140°C and has limited heat resistance. To overcome this, polypropylene, which has a high melting temperature, is used as the material for secondary battery separators.

[0005] However, conventional polypropylene microporous membranes are manufactured by a dry process, and such dry polypropylene microporous membranes have a low longitudinal / transverse stretch ratio or are mainly stretched in one direction due to the characteristics of the dry process, and have relatively low puncture strength, so that they can only be supplemented by a method of increasing thickness. In addition, the pores of the microporous membrane obtained by the dry process have characteristics of being linear and large in size, and the uniformity of the pore size is low. These characteristics have a negative effect on the performance of the battery, so that the dry polypropylene microporous membrane is not suitable for use in the field of secondary batteries.

[0006] To solve this problem, Korean Patent Publication No. 10-2011-0101202 discloses a polypropylene microporous membrane that is manufactured by a wet process and has excellent heat resistance and strength. However, this microporous membrane has a remarkably low puncture strength of less than 0.05 N / μm and does not have a significantly improved thermal shrinkage stability compared to conventional membranes, and therefore has poor battery safety in high-temperature environments such as hot-box evaluations, making it unsuitable for use in high-capacity and large-sized batteries.

[0007] Therefore, from the viewpoints of battery performance and safety, there is a need for the development of a polypropylene microporous membrane that has high puncture strength and permeability, and significantly improved heat resistance at higher temperatures, and in particular, can achieve excellent battery safety even in a hot box evaluation at 140°C, which is an evaluation index for high-temperature safety. Summary of the Invention [Problem to be solved by the invention]

[0008] In order to solve the above problems, an object of the present disclosure is to provide a polypropylene microporous membrane that has excellent puncture strength and permeability as well as significantly improved heat resistance at high temperatures, a production method thereof, and a separator including the microporous membrane.

[0009] In particular, the objective of the present invention is to provide a microporous polypropylene membrane that can achieve excellent battery safety even in a hot box evaluation at 140°C after the assembly of the battery.

[0010] The polypropylene microporous membrane of the present disclosure can be widely applied to green technology fields such as electric vehicles, battery charging stations, and other battery-based solar and wind power generation, etc. In addition, the polypropylene microporous membrane of the present disclosure can be used in eco-friendly electric vehicles, hybrid vehicles, etc. to reduce air pollution and greenhouse gas emissions and prevent climate change. [Means for solving the problem]

[0011] As one means for achieving the above object, the present disclosure provides a polymer having a viscosity average molecular weight of 1×10 6 g / mol~3×10 6 g / mol of polypropylene, the microporous membrane has a thickness of 3 μm to 30 μm, a puncture strength of 0.20 N / μm or more, and a gas permeability of 1.0 × 10 -5 Provided is a polypropylene microporous membrane having a porosity of 25% to 60%, an average pore size of 25 nm to 50 nm, and a transverse shrinkage rate of 20% or less measured after standing at 150°C for 1 hour. The porosity means the proportion of free space or pores in the volume of the microporous membrane. The polypropylene resin may be homopolypropylene. For example, the homopolypropylene resin may have high crystallinity of 40% or more, 50% or more, 60% or more, or 70% or more. For example, the highly crystalline homopolypropylene resin may have a melting point of 160 to 170°C.

[0012] In one embodiment, the polypropylene microporous membrane may have a melt rupture temperature of 165° C. or higher.

[0013] In one embodiment, the polypropylene microporous membrane may have a transverse shrinkage rate of 15% or less.

[0014] In one embodiment, the polypropylene microporous membrane may be produced by a wet process including a sequential biaxial stretching step.

[0015] In addition, as another means for achieving the above-mentioned object, the present disclosure provides a method for producing a polymerizable composition comprising the steps of: (a) providing a polymerizable composition having a viscosity average molecular weight of 1×10 6 g / mol~3×10 6 The present invention provides a method for producing a microporous polypropylene membrane, comprising the steps of: (a) melt-kneading a mixture containing polypropylene resin and a diluent having a molecular weight of 1000 g / mol in an extruder to produce a melt; (b) extruding the melt into a sheet; (c) sequentially biaxially stretching the sheet in the longitudinal and transverse directions to form a film; (d) extracting the diluent from the stretched film and drying it; and (e) heat-stretching the dried film at a temperature at which 2% to 5% of the polypropylene resin crystals melt, and heat-setting and heat-relaxing the heat-stretched film at a temperature at which 25% to 60% of the polypropylene resin crystals melt.

[0016] In one embodiment, the hot stretching in step (e) may be carried out at a temperature of 125°C to 135°C.

[0017] In one embodiment, the heat setting and heat relaxation in step (e) may be carried out at a temperature of 155°C to 165°C.

[0018] In another aspect of the present disclosure, there is provided a microporous polypropylene membrane produced by the above production method.

[0019] In another embodiment of the present disclosure, the viscosity average molecular weight is 1×10 6 g / mol~3×10 6 g / mol of polypropylene, the microporous membrane has a thickness of 3 μm to 30 μm, a puncture strength of 0.20 N / μm or more, and a gas permeability of 1.0 × 10 -5 The present invention provides a microporous membrane for use as a separator in a secondary battery, which has a porosity of 25% to 60%, an average pore size of 25 nm to 50 nm, and a lateral shrinkage rate of 20% or less measured after being left at 150°C for 1 hour.

[0020] In one embodiment, the microporous membrane for a separator of a secondary battery may have a melt rupture temperature of 165° C. or higher.

[0021] In another aspect of the present disclosure, there is provided a secondary battery including a positive electrode, a negative electrode, and the separator according to the above aspect.

[0022] As another means for achieving the above object, the present disclosure provides a separator including the above-mentioned polypropylene microporous membrane. Effect of the Invention

[0023] The microporous polypropylene membrane according to the present disclosure has excellent puncture strength and permeability, and can ensure significantly improved heat resistance at high temperatures.

[0024] In addition, the polypropylene microporous membrane according to the present disclosure has a puncture strength of 0.20 N / μm or more and a gas permeability of 1.0×10 -5 It can be more than Darcy.

[0025] Additionally, the microporous polypropylene membrane according to the present disclosure can have a transverse shrinkage percentage of 20% or less when measured after standing at 150° C. for 1 hour.

[0026] In addition, the present disclosure can provide a battery having excellent safety, in which the polypropylene microporous membrane according to one embodiment ensures excellent battery performance and does not emit smoke or catch fire in a high-temperature environment. In particular, the present disclosure can provide a battery having excellent safety, in which the battery does not emit smoke or catch fire in a hot box evaluation at a high temperature of 140°C. [Brief description of the drawings]

[0027] [Figure 1] FIG. 2 shows a frame for measuring the melt rupture temperature of a microporous membrane produced in one embodiment. [Diagram 2]FIG. 2 shows a microporous membrane fixed with tape to a frame for measuring the melt rupture temperature of the microporous membrane produced in one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] The embodiments described herein may be modified into various other forms, and the technology according to one aspect is not limited to the embodiments described below. In addition, the embodiments of one aspect are provided to more completely explain the present disclosure to those having average knowledge in the art.

[0029] Additionally, as used in the specification and the appended claims, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context indicates otherwise.

[0030] In addition, the numerical ranges used herein include lower and upper limits, and all values ​​within the ranges, increments logically derived in the form and width of the ranges defined, all values ​​that are doubly limited, and all possible combinations of upper and lower limits of numerical ranges that are mutually limited in different ways. Unless otherwise defined herein, values ​​outside the numerical ranges that may occur due to experimental error or rounding up are also included in the numerical ranges defined.

[0031] Furthermore, throughout the specification, unless otherwise specified to the contrary, "comprising" an element means that it may further include other elements, rather than excluding other elements.

[0032] The present disclosure relates to a polymer having a viscosity average molecular weight of 1×10 6 g / mol~3×10 6 g / mol of polypropylene, the microporous membrane has a thickness of 3 μm to 30 μm, a puncture strength of 0.20 N / μm or more, and a gas permeability of 1.0 × 10 -5 Provided is a polypropylene microporous membrane having a Darcy or greater, a porosity of 25% to 60%, an average pore size of 25 nm to 50 nm, and a transverse shrinkage rate of 20% or less measured after standing at 150°C for 1 hour.

[0033] In recent years, secondary batteries are required to satisfy better battery performance and safety as their capacity and size increase, and therefore secondary battery separators are required to have both higher levels of heat resistance and transmittance. For this purpose, polypropylene with a high melting temperature is used as a material for secondary battery separators, but polypropylene microporous membranes produced by dry processes are not suitable for use in the field of secondary batteries due to their low puncture strength and excessively large and non-uniform pore size. In addition, polypropylene microporous membranes produced by wet processes also have low puncture strength and are not significantly improved in heat shrinkage stability compared to conventional membranes, and therefore have poor battery safety in high-temperature environments such as hot box evaluation, making them unsuitable for use in high-capacity and large-sized batteries.

[0034] As a result of extensive research by the inventors, it was found that the puncture strength is 0.20 N / μm or more, and 1.0×10 -5 It was confirmed that it is possible to produce a polypropylene microporous membrane that has excellent puncture strength and permeability as well as significantly improved heat resistance at high temperatures by achieving a gas permeability of Darcy or higher, a porosity of 25% to 60%, an average pore size of 25nm to 50nm, and a transverse shrinkage rate of 20% or less measured after leaving it at 150°C for 1 hour.

[0035] A secondary battery according to one embodiment includes a polypropylene microporous membrane that satisfies all of the above physical properties, thereby ensuring both excellent battery performance and safety at high temperatures. In particular, the present disclosure can provide a battery that has excellent thermal safety at high temperatures, in which the battery does not emit smoke or catch fire in a hot box evaluation at a high temperature of 140°C. The manufacturing and evaluation method of the battery for the evaluation is as follows. A positive electrode using NCM622 (Ni:Co:Mn=6:2:2) as an active material and a negative electrode using graphite carbon as an active material are wound together with the microporous membrane of the present disclosure and placed in an aluminum pouch to manufacture a battery. Next, 1M lithium hexafluorophosphate (LiPF 6 ) is dissolved in an electrolyte solution, which is then injected into the battery and sealed to produce a battery with a capacity of 2 Ah. The battery is then aged and degassed, fully charged to 4.2 V, and placed in an oven to heat at a rate of 5° C. / min. After reaching 140° C., the battery is left for 30 minutes to check whether smoke or fire occurs. In other words, the polypropylene microporous membrane of the present disclosure satisfies both of the above-mentioned physical properties and is therefore suitable for use in high-output / high-capacity batteries.

[0036] In one embodiment, a polypropylene microporous membrane satisfying all of the above physical properties can be produced by using a polypropylene resin having a viscosity average molecular weight in a specific range or by heat treating the diluent at a specific temperature after extraction.

[0037] In one embodiment, the polypropylene resin contained in the polypropylene microporous membrane has a viscosity average molecular weight of 1×10 6 g / mol~3×10 6 g / mol, specifically 1.2×10 6 g / mol~2.5×10 6 g / mol, more specifically 1.3×10 6 g / mol~2.2×10 6 It may be in g / mol.

[0038] In one embodiment, the heat treatment at a particular temperature after extraction of the diluent may comprise heat stretching the film obtained after extraction of the diluent at a first temperature, and heat setting and heat relaxing the heat stretched film at a second temperature higher than the first temperature.

[0039] This allows the polypropylene microporous membrane to have excellent puncture strength and permeability, as well as significantly improved heat resistance at high temperatures.

[0040] The polypropylene microporous membrane will be described in more detail below.

[0041] In one embodiment, the thickness of the polypropylene microporous membrane may be 3 μm to 30 μm, specifically 5 μm to 20 μm, more specifically 5 μm to 15 μm. The microporous membrane of the present disclosure can achieve excellent puncture strength, gas permeability, and heat shrinkage even if it has a thickness in the above range, and in particular, it has been found to exhibit excellent battery safety in a hot box evaluation according to the evaluation method of the following embodiment. In addition, it has excellent resistance to external stress generated during battery production, and temperature rise and dendrites generated during battery charge and discharge, and has low internal resistance of the battery, thereby improving the charge and discharge performance of the battery.

[0042] In one embodiment, the polypropylene microporous membrane may have a puncture strength of 0.20 N / μm or more even if it has a thickness in the above range. Specifically, the puncture strength may be 0.25 N / μm or more, or 0.30 N / μm or more, and the upper limit is not particularly limited, but may be, for example, 1.0 N / μm or less. In a specific embodiment, the puncture strength may be 0.20 N / μm to 1.0 N / μm, 0.25 N / μm to 1.0 N / μm, or 0.30 N / μm to 1.0 N / μm, but is not limited thereto. By satisfying the puncture strength in the above range, the resistance against external stress generated during the manufacture of the battery and dendrites generated during the charge and discharge of the battery is excellent, and the battery safety can be ensured. In addition, the separator for the secondary battery can be thinned, and is suitable for use in high-capacity / high-output batteries.

[0043] In one embodiment, the polypropylene microporous membrane has a pore size of 1.0×10 -5 Darcy or more, and specifically, the gas permeability is 1.3×10 -5 Darcy or higher, 1.5×10 -5 Darcy or higher, 3.0×10 -5 Darcy or less, or 5.0×10 -5 Darcy or less. In a specific embodiment, the gas permeability is 1.0×10 -5 Darcy~5.0×10 -5 Darcy, or 1.3 × 10 -5 Darcy~3.0×10 -5 By satisfying the gas permeability in the above range, it is possible to have excellent ion conductivity, and the charge / discharge characteristics of the battery can be improved due to the low internal resistance of the battery.

[0044] In one embodiment, the polypropylene microporous membrane may have a porosity of 25% to 60%, specifically 30% to 50% or 35% to 39%, in terms of mechanical strength and ionic conductivity, but is not limited thereto.

[0045] In one embodiment, the polypropylene microporous membrane may have an average pore size of 25 nm to 50 nm, specifically 25 nm to 40 nm, more specifically 25 nm to 35 nm. In this case, the average pore size may be measured using a half-dry method. In one embodiment, the average pore size can be measured using a porometer according to ASTM F316-03.

[0046] In one embodiment, the polypropylene microporous membrane may have a transverse shrinkage rate of 20% or less, 15% or less, or 13% or less, measured after standing at 150° C. for 1 hour, and the lower limit is not particularly limited, but may be, for example, 0.1%, 0.5%, or 1%. In a specific embodiment, the shrinkage rate may be, but is not limited to, 0.1% to 20%, 0.5% to 15%, or 1% to 13%.

[0047] In one embodiment, the polypropylene microporous membrane may have a melt rupture temperature of 165° C. or more, or 170° C. or more, and the upper limit is not particularly limited, but may be, for example, 250° C. In a specific embodiment, the melt rupture temperature may be 165° C. to 250° C. or 170° C. to 250° C., but is not limited thereto.

[0048] In one embodiment, the polypropylene microporous membrane may be produced by a wet process including a successive biaxial stretching step, which can provide a polypropylene microporous membrane that satisfies all of the above-mentioned physical properties.

[0049] Specifically, the polypropylene microporous membrane is produced by extruding and sequentially biaxially stretching a mixture obtained by dissolving a diluent in a polypropylene resin into a film, and extracting the diluent from the film. The polypropylene microporous membrane may be produced by a wet method including a typical sequential biaxial stretching process known to those skilled in the art, and is not limited as long as it can produce a microporous membrane having the above-mentioned physical properties.

[0050] In one embodiment, a polypropylene microporous membrane satisfying all of the above physical properties can be produced by using a polypropylene resin having a viscosity average molecular weight in a specific range, or by heat treatment at a specific temperature after diluent extraction. As a result, the polypropylene microporous membrane can have excellent puncture strength and permeability, as well as significantly improved heat resistance at high temperatures. By including a polypropylene microporous membrane satisfying all of the above physical properties, the present disclosure can provide a battery that has excellent thermal safety at high temperatures, in which the battery does not smoke or catch fire in a hot box evaluation at a high temperature of 140°C while ensuring excellent battery performance.

[0051] In one embodiment, the polypropylene resin contained in the polypropylene microporous membrane has a viscosity average molecular weight of 1×10 6 g / mol~3×10 6 g / mol, specifically 1.2×10 6 g / mol~2.5×10 6 g / mol, more specifically 1.3×10 6 g / mol~2.2×10 6 It may be in g / mol.

[0052] In one embodiment, the heat treatment at a particular temperature after extraction of the diluent may comprise heat stretching the film obtained after extraction of the diluent at a first temperature, and heat setting and heat relaxing the heat stretched film at a second temperature higher than the first temperature.

[0053] Hereinafter, the method for producing the polypropylene microporous membrane of the present disclosure will be described.

[0054] According to one embodiment, a method for producing a microporous polypropylene membrane includes: (a) producing a microporous polypropylene membrane having a viscosity average molecular weight of 1×10 6 g / mol~3×10 6The method may include the steps of: (a) melt-kneading a mixture containing polypropylene resin and diluents (g / mol) in an extruder to produce a molten material; (b) extruding the molten material to form a sheet; (c) sequentially biaxially stretching the sheet in the longitudinal and transverse directions to form a film; (d) extracting the diluents from the stretched film and drying it; and (e) heat-stretching the dried film at a temperature at which 2% to 5% of the polypropylene resin crystals melt, and heat-setting and heat-relaxing the heat-stretched film at a temperature at which 25% to 60% of the polypropylene resin crystals melt.

[0055] Each manufacturing step will now be described.

[0056] First, step (a) is a step of melt-kneading a mixture containing polypropylene resin and diluent by an extruder to produce a melt, and the mixture contains polypropylene resin and diluent in a weight ratio of 10-60:90-40 in order to form pores, and specifically, may contain them in a weight ratio of 20-40:80-60, but is not particularly limited as long as the object of the present disclosure is achieved. When the weight ratio satisfies the above range, the melt has sufficient fluidity, and a uniform sheet can be easily formed in the subsequent step, and sufficient orientation is achieved during the stretching process, and mechanical strength is easily ensured, so that problems such as breakage during the stretching process can be prevented.

[0057] The polypropylene resin has a viscosity average molecular weight of 1×10 6 g / mol~3×10 6 g / mol, preferably 1.2×10 6 g / mol~2.5×10 6 g / mol, more preferably 1.3×10 6 g / mol~2.2×10 6The microporous membrane may be a polypropylene having a viscosity average molecular weight of 100 g / mol or may contain a polypropylene having a viscosity average molecular weight in the above range. By having a viscosity average molecular weight in the above range, the physical properties targeted by the present disclosure can be realized. A battery using a microporous membrane satisfying the above physical properties has low initial resistance and excellent battery performance, and can achieve excellent thermal safety in a hot box test.

[0058] In one embodiment, the polypropylene resin may have a melting temperature of 160° C. or more, specifically, 160° C. to 170° C., but is not necessarily limited thereto. The melting temperature of the polypropylene resin can be determined by DSC.

[0059] In one embodiment, the diluent can be any organic compound that forms a single phase with the polypropylene resin at the extrusion temperature without any limitations. For example, the diluent may be one or a combination of two or more selected from the group consisting of aliphatic or cyclic hydrocarbons such as nonane, decane, decalin, paraffin oil, and paraffin wax; phthalic acid esters such as dibutyl phthalate and dioctyl phthalate; C10-C20 fatty acids such as palmitic acid, stearic acid, oleic acid, linoleic acid, and linolenic acid; and C10-C20 fatty alcohols such as cetyl alcohol, stearyl alcohol, and oleyl alcohol. A specific example of the diluent is paraffin oil having a kinetic viscosity of 20 cSt to 200 cSt at 40° C., but is not limited thereto. Alternatively, other diluents having the same or similar kinetic viscosity at an appropriate extrusion temperature may be used. For example, a diluent having a kinetic viscosity of 1 cSt to 1000 cSt or 10 cSt to 500 cSt may be used.

[0060] In addition, the mixture may further contain one or more conventional additives for improving specific functions, such as an oxidation stabilizer, a UV stabilizer, and an antistatic agent, within a range that does not significantly deteriorate the properties of the microporous membrane.

[0061] Step (b) is a step of extruding the molten material to form it into a sheet, and may be performed by any method known to those skilled in the art without limitation. For example, the molten material may be extruded through a T-die, cooled to a temperature of 10°C to 80°C, and then formed into a sheet by a casting or calendaring method.

[0062] The stretch ratios in the longitudinal and transverse directions in step (c) may each independently be 4 times or more, 6 times or more, and 10 times or less, or 15 times or less, for example, 4 times to 15 times, or 6 times to 10 times. When the stretch ratios in the longitudinal and transverse directions satisfy the above-mentioned ranges, a polypropylene microporous membrane having the physical properties targeted in the present disclosure can be produced.

[0063] The stretching in step (c) may be performed by a sequential stretching method using a roll or a tenter, and may be performed at a temperature in the range of 80°C lower than the melting temperature of polypropylene to the melting temperature of polypropylene. When the stretching is performed at a temperature in the above range, the fluidity of the polypropylene resin for effective stretching can be ensured. In particular, the sheet is stretched uniformly over the entire sheet, and no breakage due to stretching occurs, so that the stretching can be performed stably. This allows the production of a high-quality microporous membrane having uniform physical properties such as gas permeability and puncture strength over the entire membrane. As an example, the stretching may be performed at 100°C to 170°C or 110°C to 160°C, but is not limited thereto.

[0064] Step (d) is a step of extracting and drying the diluent from the stretched film, and is carried out by extracting the diluent in the film using an organic solvent, and drying the organic solvent with the film in which the diluent has been replaced with the organic solvent. The organic solvent can be used without any particular limitation as long as it can extract the diluent. Specifically, methyl ethyl ketone, methylene chloride, hexane, etc. may be used as the organic solvent because of its high extraction efficiency and fast drying.

[0065] Step (d) is preferably carried out at a high temperature due to the increased solubility of the diluent and the organic solvent, but may be carried out at a temperature of 40° C. or less from the standpoint of safety due to the boiling of the organic solvent.

[0066] Step (e) is a step of heat-treating the dried film by using a roll-type or tenter-type device at a temperature at which 2% to 5% of the polypropylene resin crystals melt, and heat-setting and heat-relaxing the heat-stretched film at a temperature at which 25% to 60% of the polypropylene resin crystals melt. By heat-treating at the above-mentioned temperature, the physical properties targeted by the present disclosure can be realized. A microporous membrane having such physical properties is suitably applied to a high-output / high-capacity battery. In detail, a battery using a microporous membrane satisfying the above-mentioned physical properties has low initial resistance and excellent battery performance, and can achieve excellent thermal safety in a hot box test.

[0067] In one embodiment, the temperature at which the crystals of the polypropylene resin melt to a certain level may vary depending on the viscosity average molecular weight and crystallinity of the polypropylene used. In the present disclosure, since a polypropylene having a viscosity average molecular weight in the above range is used as the polypropylene resin for producing a polypropylene microporous membrane, the heat stretching in the step (e) may be performed at a temperature of 125°C to 135°C, specifically, at a temperature of 127°C to 133°C. In addition, the heat setting and heat relaxation in the step (e) may be performed at a temperature of 155°C to 165°C, specifically, at a temperature of 157°C to 165°C.

[0068] The heat stretching in step (e) is, for example, stretching in the longitudinal or transverse direction, and from the viewpoint of the thermal shrinkage rate, it may be stretching in the transverse direction, or it may be stretching to 120% to 160% or 130% to 150% of the transverse width before the heat stretching.

[0069] The thermal relaxation in step (e) is relaxation (shrinkage) in the longitudinal or transverse direction, and from the viewpoint of the thermal shrinkage rate, it may be relaxation in the transverse direction, or relaxation to 80% to 99% or 90% to 99% of the transverse width before thermal relaxation.

[0070] The present disclosure provides a separator including the polypropylene microporous membrane as described above, and the separator may be a separator used in any known energy storage device, and is not particularly limited, but a non-limiting example is a separator used in a lithium secondary battery.

[0071] Examples and experimental examples are specifically illustrated below. However, the examples and experimental examples described below are merely a partial example, and the technology described in this specification is not limited thereto.

[0072] [Physical property measurement method] 1.Viscosity average molecular weight (g / mol) The viscosity average molecular weight (Mv) of polypropylene was measured by measuring the intrinsic viscosity (η) at 165°C using a Polymer Char's Crystex QC model in accordance with ISO16152:2022, and calculating it using the Margolies-equation shown in the following mathematical formula 1. The intrinsic viscosity was measured using 1,2,4-trichlorobenzene (TCB) as a solvent.

[0073] [Mathematical formula 1] Mv=5.37x10 4 x[η] 1.49

[0074] 2. Thickness of microporous membrane (μm) The thickness of the microporous membrane was measured using a contact type thickness gauge with a thickness precision of 0.1 μm. The measurement pressure was 0.63 N using a TESA Mu-Hite Electronic Height Gauge manufactured by TESA.

[0075] 3.Punching strength (N / μm) The puncture strength was measured by pressing the microporous membrane at a speed of 120 mm / min using a pin tip with a diameter of 1.0 mm and a curvature radius of 0.5 mm attached to an INSTRON Universal Test Machine (UTM) 3345. The puncture strength was calculated by dividing the load (N) at which the microporous membrane broke by the thickness (μm) of the microporous membrane.

[0076] 4. Gas permeability (Darcy) The gas permeability was measured using a porosity measuring device (CFP-1500-AEL by Porous Materials Inc. (PMI)). Generally, gas permeability is expressed by the Gurley number, but since the Gurley number does not correct for the influence of thickness, it is difficult to understand the relative permeability due to the pore structure. To solve this problem, the gas permeability of the present disclosure is measured using the Darcy permeability constant calculated by the following mathematical formula 2. Nitrogen was used as the gas, and the average value of the Darcy permeability constant measured in the range of 100 to 200 psi was calculated.

[0077] [Mathematical formula 2] Darcy transmission constant (C)=(8F·T·V) / (πD 2 (P 2 -1) F=Flow rate (cc / cm) T = sample thickness (mm) V = Viscosity of gas (0.185 cP at 20℃ for N 2 ) D = sample diameter (mm) P = pressure (psi)

[0078] 5. Transverse shrinkage rate (%) A 15 cm x 15 cm microporous membrane with a length of 10 cm and a marking on the vertical and horizontal directions was left in an oven (Yamato Scientific Co., Ltd. DKN612) stabilized at 150°C for 1 hour, and then the change in length was measured and the horizontal shrinkage rate was calculated according to Equation 3 below.

[0079] [Mathematical formula 3] Transverse shrinkage rate (%) = {(transverse length before heating - transverse length after heating) / transverse length before heating} x 100

[0080] 6.Average pore size (nm) The average pore size was measured using a porometer (CFP-1500-AEL, PMI) in accordance with ASTM F316-03. The average pore size was measured using the half-dry method (ASTM F316-03), and Galwick liquid (surface tension: 15.9 dyne / cm) provided by PMI was used to measure the pore size.

[0081] 7. Melt rupture temperature The melt rupture temperature of the microporous membrane was measured by fixing a microporous membrane 12 (5 cm x 5 cm) as shown in Figure 2 to a frame 10 (outer diameter: 7.5 cm x 7.5 cm, inner diameter: 2.5 cm x 2.5 cm) as shown in Figure 1 with polyimide tape 14, leaving it in a convection oven maintained at a set temperature for 10 minutes, and then observing whether the microporous membrane ruptured. The highest temperature at which the microporous membrane did not rupture after 10 minutes was defined as the melt rupture temperature.

[0082] 8.Initial resistance test The initial resistance test was performed using a battery assembled by applying a polypropylene microporous membrane to the separator. Specifically, a positive electrode using NCM622 (Ni:Co:Mn=6:2:2) as an active material and a negative electrode using graphite carbon as an active material were wound up together with the prepared microporous membrane and placed in an aluminum pouch. The battery was then placed in a solution containing ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate in a volume ratio of 3:5:2, and 1M lithium hexafluorophosphate (LiPF 6 The battery was then sealed to assemble a 2 Ah capacity battery. After aging and degassing, the assembled battery was fully charged to 4.2 V and the initial resistance (mΩ) was measured.

[0083] If the initial resistance is 50 mΩ or less, it is confirmed that the capacity is maintained at 20% or more in a 2C-rate discharge test, and the initial resistance value is used as an evaluation index for the output characteristics.

[0084] 9. Hotbox Evaluation The hot box evaluation was carried out using a battery assembled by applying a polypropylene microporous membrane to the separator. Specifically, a positive electrode using NCM622 (Ni:Co:Mn=6:2:2) as an active material and a negative electrode using graphite carbon as an active material were wound up together with the prepared microporous membrane and placed in an aluminum pouch. The battery was then dissolved in 1M lithium hexafluorophosphate (LiPF 6 ) was dissolved in electrolyte and sealed to assemble a battery with a capacity of 2 Ah. After aging and degassing the assembled battery, it was fully charged to 4.2 V and placed in an oven where the temperature was increased at 5°C / min. After reaching 140°C, the battery was left for 30 minutes and the changes in the battery were measured.

[0085] If the battery emitted smoke or caught fire after being left at 140°C for 30 minutes, it was rated as Fail; if there was no change in the battery voltage / current and no smoke or fire occurred, it was rated as Pass.

[0086] 10. Thermal property analysis of the film The phenomenon in which polypropylene resin crystals melt due to temperature was analyzed using a TA Instruments differential scanning calorimeter (DSC), Discovery DSC250, under conditions of a sample weight of 5 mg and a scan speed of 10°C / min.

[0087] The temperature at which n% of polypropylene resin crystals melt (T n) was measured by calculating the temperature at the point showing n% of the heat capacity relative to the total heat capacity (Heat of fusion). In this disclosure, T 2 , T 5 , T 25 , and T 60 was measured and recorded in Table 1.

[0088] 11.Porosity (%) The porosity was calculated according to the following mathematical formula: Specifically, a sample with a width of A cm (e.g., 30 cm), a length of B cm (e.g., 20 cm), and a thickness of T cm (e.g., 0.0003 to 0.002 cm) was prepared, its mass was measured, and the porosity was calculated from the ratio of the mass of the resin and the mass of the microporous membrane of the same volume.

[0089] Porosity (%)=100×{1-M / (A×B×T×ρ)} In the above formula, M is the mass of the microporous membrane (g), ρ is the density of the polypropylene resin constituting the microporous membrane (g / cm 3 ).

[0090] <Example 1> Viscosity average molecular weight is 1.5×10 6 A mixture containing polypropylene resin with a melting temperature of 165°C (g / mol) and paraffin oil with a kinematic viscosity of 80cSt at 40°C in a weight ratio of 30:70 was melt-kneaded using a twin-screw extruder to produce a melt. The melting temperature was measured using a differential scanning calorimeter (DSC) Discovery DSC250 provided by TA Instruments, with a sample weight of 5mg and a scan speed of 10°C / min.

[0091] The melt was continuously extruded by a T-die, and a sheet having a width of 300 mm and an average thickness of 1100 μm was produced using a casting roll set at 30° C. The sheet was stretched in the longitudinal direction by a roll method to 6 times at a stretching temperature of 115° C., and then guided to a tenter and stretched in the transverse direction to 6 times at a stretching temperature of 140° C.

[0092] Paraffin oil was extracted from the film which had been completely stretched in the machine direction and the transverse direction at 25°C using methylene chloride, and the film from which the paraffin oil had been extracted was dried at 60°C.

[0093] The dried film was heat stretched to 145% in the transverse direction using a tenter type heat setting device at 130°C, a temperature at which 3% of the polypropylene resin crystals melt, and then heat set for 10 seconds at 160°C, a temperature at which 35% of the polypropylene resin crystals melt, and heat relaxed (shrunk) to 93% of the width before the heat relaxing process to produce a microporous membrane with a thickness of 12.8 μm.

[0094] The properties of the final microporous membrane and the performance of the battery using the same are shown in Table 2 below.

[0095] <Examples 2 to 3 and Comparative Examples 1 to 6> A polypropylene microporous membrane was prepared in the same manner as in Example 1, except that the viscosity average molecular weight (PP Mv) of the polypropylene resin used, the longitudinal / transverse stretch ratio, and the heat treatment temperature were changed to the conditions shown in Table 1. The physical properties of the final microporous membrane and the performance of the battery using the same are recorded in Table 2 below.

[0096] [Table 1]

[0097] [Table 2]

[0098] Referring to Tables 1 and 2, the microporous membranes of the examples satisfy all of the physical properties targeted by the present disclosure, and the batteries using the microporous membranes have initial resistances of 50 mΩ or less and pass hot box tests, achieving excellent battery performance and safety in high temperature environments.

[0099] The microporous membrane of Comparative Example 1 had a particle size of 1.0 × 10 6 As a result of using a polypropylene resin with a viscosity average molecular weight of less than g / mol, the chains were less entangled, and the film broke during the heat stretching in the heat treatment step.

[0100] The microporous membrane of Comparative Example 2 had a particle size of 3.0 × 10 6 When a polypropylene resin having a viscosity average molecular weight exceeding 100 g / mol is used, the mixing of the resin and the diluent is not uniform, resulting in a sheet of uneven thickness and uneven product quality.

[0101] The microporous membranes of Comparative Example 3 and Comparative Example 4 were heat-stretched in the heat treatment step at a temperature at which 5% of the crystals of the film introduced into the heat setting device melt (T 5 ) and the gas permeability, porosity, and average pore size were 1.0 × 10 -5 Since it is less than Darcy, less than 25%, and less than 24 nm, the thermal safety of a battery using it is equivalent to that of the present disclosure, but the initial resistance is 55 mΩ or more, resulting in poor battery performance.

[0102] The microporous membrane of Comparative Example 5 was heat-set and heat-relaxed in the heat treatment step at a temperature at which 25% of the crystals of the film introduced into the heat-set device melt (T 25 ) and found that the physical properties such as gas permeability were met, but the lateral shrinkage rate was 25.1%, meaning that batteries using this material have the disadvantage of being significantly less safe in high-temperature environments.

[0103] The microporous membrane of Comparative Example 6 was heat-set and heat-relaxed in the heat treatment step at a temperature at which 60% of the crystals of the film introduced into the heat-set device melt (T 60 ) and the gas permeability, porosity, and average pore size were 0.2 × 10 -5 Since it is less than Darcy, less than 16%, and less than 19 nm, the thermal safety of a battery using it is equivalent to that of the present disclosure, but the initial resistance is 65 mΩ, which is a drawback in that the battery performance is inferior.

[0104] As described above, the present disclosure has been described in the present specification by using specific details and limited embodiments, but this is merely provided for a more general understanding of the present disclosure, and the present disclosure is not limited to the above embodiments. A person having ordinary knowledge in the field to which the present disclosure belongs can make various modifications and variations from such descriptions.

Claims

1. Viscosity average molecular weight is 1×10 6 g / mol ~ 3 x 10 6 g / mol of polypropylene, the microporous membrane has a thickness of 3 μm to 30 μm, a puncture strength of 0.20 N / μm or more, and a gas permeability of 1.0×10 -5 A microporous polypropylene membrane having a Darcy or more, a porosity of 25% to 60%, an average pore size of 25 nm to 50 nm, and a transverse shrinkage rate of 20% or less measured after standing at 150° C. for 1 hour.

2. The microporous polypropylene membrane of claim 1, having a melt rupture temperature of 165°C or higher.

3. The microporous polypropylene membrane of claim 1, wherein the transverse shrinkage rate is 15% or less.

4. The microporous polypropylene membrane according to claim 1, produced by a wet process including a successive biaxial stretching step.

5. (a) Viscosity average molecular weight of 1×10 6 g / mol ~ 3 x 10 6 A step of melt-kneading a mixture containing a polypropylene resin having a molecular weight of 100 g / mol and a diluent in an extruder to produce a melt; (b) extruding the melt into a sheet; (c) sequentially biaxially stretching the sheet in the machine and transverse directions to form a film; (d) extracting the diluent from the stretched film and drying; (e) heat-stretching the dried film at a temperature at which 2% to 5% of the polypropylene resin crystals melt, and heat-treating the heat-stretched film by heat-setting and heat-relaxing at a temperature at which 25% to 60% of the polypropylene resin crystals melt.

6. The method for producing a polypropylene microporous membrane according to claim 5, wherein the hot stretching in step (e) is performed at a temperature of 125°C to 135°C.

7. The method for producing a microporous polypropylene membrane according to claim 5, wherein the heat setting and heat relaxing in step (e) are carried out at a temperature of 155°C to 165°C.

8. A separator comprising the microporous polypropylene membrane according to any one of claims 1 to 4.

9. Viscosity average molecular weight is 1×10 6 g / mol ~ 3 x 10 6 g / mol of polypropylene, the microporous membrane has a thickness of 3 μm to 30 μm, a puncture strength of 0.20 N / μm or more, and a gas permeability of 1.0×10 -5 A microporous membrane for a separator of a secondary battery, having a Darcy or more, a porosity of 25% to 60%, an average pore size of 25 nm to 50 nm, and a lateral shrinkage rate of 20% or less measured after being left at 150° C. for 1 hour.

10. The microporous membrane for a separator of a secondary battery according to claim 9 , which has a melt-rupture temperature of 165° C. or higher.

11. A microporous polypropylene membrane produced by the method according to any one of claims 5 to 7.

12. A secondary battery comprising a positive electrode, a negative electrode, and the separator according to claim 8.

Citation Information

Patent Citations

  • System And Process For Producing A Multilayer Microporous Membrane

    EP2111910A1

  • Porous polypropylene film, separator for electricity storage device, and electricity storage device

    WO2012105661A1

  • Polyolefin microporous membrane, method for producing same, and battery separator

    WO2016104789A1

  • Polyolefin microporous film and lithium-ion secondary cell in which same is used

    WO2019074122A1

Cited By

  • Microporous polyolefin film, method for preparing the same, and secondary battery comprising the same

    JP2026047143A