Hydraulic composition

Incorporating a neutralization inhibitor with calcium nitrate into environmentally friendly cement compositions suppresses carbonation, addressing the increased carbonation issue in these cements, ensuring structural integrity and workability without significant cost or composition changes.

JP2024166423AActive Publication Date: 2024-11-28TAISEI CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024164019
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-03-15
Filing Date
2024-09-20
Publication Date
2024-11-28
Estimated Expiration
2040-01-16

AI Technical Summary

Technical Problem

Environmentally friendly cement compositions exhibit increased carbonation rates compared to traditional cement, leading to reduced structural integrity due to corrosion of reinforcing bars, and existing methods to suppress carbonation, such as increasing cement amounts or reducing water-cement ratios, are costly and affect workability.

Method used

Incorporation of a neutralization inhibitor containing calcium nitrate into hydraulic compositions, with a specific nitrate ion content of 0.8% to 5.0% by mass, to suppress carbonation without altering the overall composition or cement amounts.

Benefits of technology

The hydraulic composition effectively inhibits carbonation progression, maintaining structural integrity while keeping costs manageable and workability intact, demonstrated in both accelerated and natural environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166423000012
    Figure 2024166423000012
  • Figure 2024166423000013
    Figure 2024166423000013
  • Figure 2024166423000014
    Figure 2024166423000014
Patent Text Reader

Abstract

To provide a hydraulic composition with suppressed propagation of neutralization reaction.SOLUTION: Disclosed is a hydraulic composition including a hydraulic powder including Portland cement and a neutralization suppression agent including calcium nitrate. A blending ratio of the Portland cement in all powders is 10 mass% or over and 70 mass% or under. Preferably, to all powder amounts, the neutralization suppression agent in nitrate ion (NO3-, formula weight 62) conversion of 0.8 mass% or over and 5.0 mass% or under is included therein. Preferably, the hydraulic powder further includes at least one of a blast furnace slag and a fly ash.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hydraulic composition. [Background technology]

[0002] Cement hardens through a hydration reaction with water to become a hardened body. The clinker minerals that make up part or all of the cement react with water to produce hydrates such as calcium hydroxide, which is strongly alkaline, and the pore solution in the hardened body exhibits a strong alkaline nature. If the hardened body is left in the atmosphere, carbon dioxide that penetrates the body reacts with calcium salts such as calcium hydroxide to produce calcium carbonate, and the pore solution changes from strongly alkaline to neutral, a process known as "neutralization." Neutralization proceeds from the surface of the hardened body that comes into contact with the air. When cement is used to build a reinforced concrete structure, if neutralization progresses to the vicinity of the reinforcing bars inside the structure, it destroys the passive film that covers the reinforcing bars, which is one of the causes of reinforcing bar corrosion. The reinforcing bars expand compared to before corrosion, causing cracks and destruction of the hardened body, and corrosion causes cross-sectional defects in the reinforcing bars, reducing the strength of the reinforced concrete structure.

[0003] In recent years, environmentally friendly cements that emit less carbon dioxide during production have been proposed. Environmentally friendly cements are hydraulic compositions that have the same composition as those in which 20 to 100% of a mixture of one or more types of cement (Portland cement, blast furnace cement, fly ash cement, silica cement, ecocement) specified in JIS R5210, R5211, R5212, R5213, and R5214 is replaced with slag, fly ash, silica fume, gypsum dihydrate, gypsum hemihydrate, anhydrous gypsum, limestone fine powder, slaked lime, expansive material, siliceous admixture, or calcium salt or sodium salt, and concrete using environmentally friendly cement is called environmentally friendly concrete. For example, Patent Document 1 proposes a hydraulic composition consisting of ground granulated blast furnace slag, ground limestone, and two or more types of stimulants with different calcium ion elution rates as environmentally friendly cement, while Patent Document 2 proposes a slag hardening composition consisting mainly of fine aggregate, coarse aggregate, ground limestone, ground granulated slag, sodium carbonate, and chemical admixtures as environmentally friendly concrete. Non-Patent Document 1 reports an example of environmentally friendly concrete in which 20 to 80% of Portland cement has been replaced with an admixture whose main component is blast furnace slag. However, there is a problem that hardened bodies and concrete using environmentally friendly cement use less Portland cement and are more prone to carbonation than hardened bodies and concrete using only Portland cement. For example, the environmentally friendly cement shown in Patent Document 1 is said to be able to suppress carbonation by selecting a reaction stimulant necessary for hardening the blast-furnace cement, but the carbonation rate of this environmentally friendly cement is faster than that of hardened bodies using only Portland cement.

[0004] A known technique for preventing carbonation is to increase the amount of cement and reduce the water-cement ratio to make the hardened body denser and less susceptible to carbon dioxide penetration. However, this increases the amount of cement used, which increases costs. Also, a low water-cement ratio results in poor fluidity and reduced workability. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-148434 A [Patent Document 2] Patent No. 5743650 [Non-patent literature]

[0006] [Non-Patent Document 1] Hiroshi Jinnai, Masaki Kato, Kaori Tateyama, Kenji Kondo: Realization of buildings constructed with environmentally friendly concrete as main structural members and their CO2 reduction effects, Concrete Engineering, vol.52, No.6, pp.528-533, June 2014. Summary of the Invention [Problem to be solved by the invention]

[0007] The object of the present invention is to provide a hydraulic composition in which the progress of a neutralization reaction is suppressed. [Means for solving the problem]

[0008] The means for solving the problems of the present invention are as follows. 1. A concrete mixture comprising hydraulic powder containing Portland cement and a carbonation inhibitor containing calcium nitrate, the Portland cement content of the total powder being 10% by mass or more and 70% by mass or less, and the carbonation inhibitor being mixed in an amount of nitrate ions (NO3 - %, calculated as a formula weight 62), of 0.8 mass % or more and 5.0 mass % or less, and the powder further contains at least one of blast furnace slag and fly ash. 2. A concrete mixture comprising hydraulic powder containing Portland cement and blast furnace slag, and a carbonation inhibitor containing calcium nitrate, the Portland cement content of the total powder being 10% by mass or more and 32.7% by mass or less, and the carbonation inhibitor being mixed with nitrate ions (NO3 - %, calculated as a formula weight 62), of 0.8 mass % or more and 5.0 mass % or less, and the powder further contains at least one of silica fume and anhydrous gypsum. Effect of the Invention

[0009] The hydraulic composition of the present invention can suppress the progress of carbonation in the hardened body by including a carbonation inhibitor containing calcium nitrate. Carbonation of the hardened body can be suppressed by replacing a part of the water added during hardening with an aqueous solution of a nitrate compound, by dissolving a nitrate compound in a part or all of the water added during hardening, or by simply adding or mixing the nitrate compound as a solid. The hydraulic composition of the present invention can suppress carbonation with the conventional composition without changing the composition and amount of powder consisting of one or both of cement and admixture other than the nitrate compound, and the total amount of powder.

[0010] The amount of neutralization inhibitor mixed is determined by the amount of nitrate ions (NO3 - The effect can be obtained by adding 0.8 mass% or more, calculated as formula weight 62). The inhibitory effect increases as the addition rate increases, but if the addition rate exceeds 5.0 mass%, a sufficient effect can be obtained, but the rate of decrease in the carbonation rate with increasing addition rate becomes small and the cost becomes high. For this reason, it is preferable to adjust the amount to a range of 0.8 mass% or more and 5.0 mass% or less. By adding a carbonation inhibitor, the progress of carbonation can be controlled to match the required performance of the structure. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 shows the results of the accelerated neutralization test in Experiment 1. [Diagram 2] FIG. 1 shows the results of the accelerated neutralization test in Experiment 2. [Diagram 3] Graph showing neutralization depth after 3.8 years of exposure in Experiment 2. [Figure 4] FIG. 1 shows the results of the accelerated neutralization test in Experiment 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] "Hydraulic composition" The hydraulic composition of the present invention contains cement and a carbonation inhibitor comprising a nitrate compound. The hydraulic composition of the present invention only needs to contain cement and a carbonation inhibitor consisting of a nitrate compound, and may contain a mineral admixture. Here, in this specification, the cement and the mineral admixture are collectively referred to as powder, and the total amount thereof is referred to as the total amount of powder. The hydraulic composition of the present invention may contain, in addition to cement and a carbonation inhibitor, or cement, an admixture and a carbonation inhibitor, chemical admixtures such as air-enhancing agents, water-reducing agents, air-enhancing water-reducing agents, high-performance water-reducing agents, high-performance air-enhancing water-reducing agents, retarders, foaming agents, waterproofing agents, colorants, cold resistance agents, early-strengthening agents and thickeners; fine and coarse aggregates such as gravel, sand, sea sand, crushed stone, crushed sand, various slag aggregates, heavy aggregates, lightweight aggregates and recycled aggregates; additives such as vinylon fibers, polypropylene fibers, glass fibers, steel fibers and carbon fibers; and water such as tap water, river water, lake water, groundwater, recovered water from ready-mixed concrete plants, water contained in chemical admixtures and crystallization water contained in carbonation inhibitors.

[0013] ·cement As the cement contained in the hydraulic composition of the present invention, any hydraulic powder that hardens by reacting with water can be used without any particular limitation. For example, Examples of the cement include portland cement, blast furnace cement, fly ash cement, silica cement, and eco-cement. Environmentally friendly cement can also be used. Among these, cement in which the blending ratio of portland cement in the total powder is 80 mass% or less, which is prone to neutralization, blast furnace cement, fly ash cement, and environmentally friendly cement are preferable.

[0014] ·Admixture Slag, fly ash, silica fume, gypsum dihydrate, gypsum hemihydrate, anhydrous gypsum, limestone fine powder, hydrated lime, expansive agents, and siliceous admixtures are mixtures or small-amount mixtures of cement and environmentally friendly cement specified by the JIS, but they can also be used as admixtures when making mortar or concrete using cement.

[0015] Neutralization inhibitor The hydraulic composition of the present invention contains a carbonation inhibitor made of a nitrate compound. As the nitrate compound, any compound that can be incorporated into a hydraulic composition can be used without any particular limitation, and examples of the nitrate compound that can be used include calcium nitrate, magnesium nitrate, sodium nitrate, potassium nitrate, ammonium nitrate, and aluminum nitrate. In addition, a carbonation inhibitor other than a nitrate compound can be used in combination as long as it does not impede the effects of the present invention.

[0016] The hydraulic composition of the present invention contains a carbonation inhibitor in the form of nitrate ions (NO3 - It is preferable that the amount of the carbonation inhibitor is 0.8 mass% or more and 5.0 mass% or less, calculated as a formula weight 62). If the amount of the carbonation inhibitor is less than 0.8 mass% calculated as a nitrate ion, the effect of inhibiting the progress of carbonation may be insufficient. If the amount of the carbonation inhibitor is more than 5.0 mass% calculated as a nitrate ion, a sufficient carbonation inhibition effect can be obtained, but the improvement in the carbonation inhibition effect with an increase in the amount of the carbonation inhibitor reaches a plateau, and the cost becomes high.

[0017] The hydraulic composition of the present invention can be used as a paste by using water and / or a chemical admixture, or as mortar or concrete by using fine aggregate, coarse aggregate and / or a chemical admixture. Concrete can be used in the form of pre-mixed concrete, ready-mixed concrete, and concrete products such as concrete blocks, box culverts, and segments for shield tunnels.

[0018] The hydraulic composition of the present invention is hardened by mixing with water. The carbonation inhibitor may be mixed in advance as a part of the hydraulic composition of the present invention in the hydraulic mixture, or may be mixed in advance with the water to be mixed, or may be added and mixed when mixing the hydraulic composition other than the carbonation inhibitor with water. When the nitrate compound is mixed in a solid state with the hydraulic composition, it is preferably in a powder form that can be mixed uniformly. When the nitrate compound is mixed with the water for hardening, it is preferably dissolved in order to be mixed uniformly. The manufacturing method of the hydraulic composition of the present invention may be performed by a conventional method except for adding the nitrate compound. That is, when used as a paste, mortar, or concrete, the water containing the carbonation inhibitor and other constituent materials may be mixed and kneaded in a concrete mixer or mortar mixer, or the carbonation inhibitor, water, and other constituent materials may be mixed and kneaded, or further, other constituent materials excluding the carbonation inhibitor may be kneaded, and after producing a paste, mortar, or concrete, the carbonation inhibitor may be added and kneaded again. When producing a paste, mortar, or concrete, the hydraulic composition of the present invention may be premixed (premixed) with some or all of the other constituent materials excluding water before pouring water. EXAMPLES

[0019] "Experiment 1" Environmentally friendly cement An environmentally friendly cement containing 77.2% by mass of blast furnace slag relative to the total powder amount was hardened using aqueous solutions containing calcium nitrate, a carbonation inhibitor, dissolved at different concentrations. Of the materials, the blast furnace slag satisfies JIS A 6206, the expansive agent JIS A 6202, the slaked lime JIS R 9001, and the limestone fine powder JIS A 5008, and the calcium nitrate used was a special grade reagent (calcium nitrate tetrahydrate (Ca(NO3)2·4H2O)) manufactured by Kanto Chemical Co., Ltd. Note that Examples 1 and 2 are reference examples.

[0020] [Table 1]

[0021] Water: Yokohama City Water Bureau, tap water Blast furnace slag (with gypsum): Manufactured by DC Corporation, product name: Cerament A (anhydrous Gypsum additive: SO3 equivalent = 2.1%) Expansion material: Manufactured by Pacific Materials Co., Ltd., Product name: Expan Slaked lime: Manufactured by Okutama Kogyo Co., Ltd. Product name: Special slaked lime Limestone powder: Manufactured by Miyagi Lime Industry Co., Ltd. Calcium nitrate tetrahydrate: Special grade reagent manufactured by Kanto Chemical Co., Ltd.

[0022] Using this cement paste, a test specimen measuring approximately 3 cm in diameter and 5 cm in height was made, which was then sealed and cured. It was demolded when it was 28 days old, and stored at 20°C and 60% RH for 7 days. After that, all sides except for the bottom surface were coated with aluminum adhesive tape, and it was left in an environment of 20°C, 60% RH, and 5% CO2 concentration to carry out an accelerated carbonation test. After a specified period of time had passed, the specimen was split and a 1% alcohol solution of phenolphthalein was sprayed onto the cross section, and the area where no coloration occurred was considered to be the area where neutralization had progressed, and the accelerated carbonation depth was measured. The results are shown in Figure 1. It is known that carbonation progresses in proportion to the square root of the carbonation period, and when the relationship between the change in accelerated carbonation depth and the square root of the carbonation period is approximated by a straight line (linear approximation), the slope of the line can be taken as the carbonation rate. In other words, the carbonation rate indicates the ratio of change in carbonation depth to the change in the square root of the accelerated carbonation period.

[0023] For the paste using environmentally friendly cement, the carbonation rate ratio was obtained when the carbonation inhibitor was added to the carbonation rate of Comparative Example 1, which did not contain the carbonation inhibitor. Comparative Example 2, which contained 0.5 in terms of nitrate ions, i.e., 0.5 mass% of the total powder amount, had a carbonation rate ratio of 1.7, and no effect of addition was observed. On the other hand, Example 1, which contained 1.0 in terms of nitrate ions, i.e., 1.0 mass% of the total powder amount, had a suppressed carbonation rate of about 0.78, and Example 2, which contained 2.0 in terms of nitrate ions, i.e., 2.0 mass% of the total powder amount, had a carbonation rate ratio of 0.59, and it was confirmed that carbonation was suppressed.

[0024] "Experiment 2" Concrete was prepared by adding fine aggregate and coarse aggregate to a paste prepared by using 8.3 mass% (2.0 mass% in terms of nitrate ions) of a chemical admixture for concrete containing calcium nitrate (manufactured by BASF Japan Ltd., product name: Masterset FZP99, nitrate ion content: 24 mass%) instead of calcium nitrate with respect to the total powder amount. This mixture is designated as Example 3. Furthermore, a mixture obtained by removing the chemical admixture for concrete containing calcium nitrate from Example 3 is designated as Comparative Example 3. In Example 3 and Comparative Example 3, fine aggregate having a density of 2.63 g / cm according to JIS A 5308 Annex A was used. 3 The crushed sand and the coarse aggregate used were crushed stone conforming to JIS A 5005 with a Gmax of 20 mm, the fine aggregate rate was 43%, and the water-powder ratio was 0.36. Example 3 is a reference example.

[0025] [Table 2]

[0026] In Example 3 and Comparative Example 3, a high-performance air-entraining water-reducing agent, a retarder, and an air-entraining agent were added, and it was confirmed that the slump and air content satisfied the target values ​​of 15±2.5 cm and 6.0±1.5%, respectively. The high-performance air-entraining water-reducing agent used was a polycarboxylate ether type (manufactured by BASF Japan, product name: Masterglanium SP8SV), the retarder was a complex of a modified lignin sulfonate compound and an oxycarboxylate compound (manufactured by BASF Japan, product name: Master Pozzolith No. 89), and the air-entraining agent was a high alkyl carboxylate type anionic surfactant (manufactured by BASF Japan, product name: Master Air 775). Test specimens were prepared by casting Example 3 and Comparative Example 3 into a formwork with inner dimensions of 100 x 100 x 400 mm. The specimens were demolded after 3 days and cured in water at 20°C until they were 28 days old. They were then stored in an environment of 20°C and 60% RH until they were 56 days old, after which they were covered with aluminum adhesive tape except for one side of the 100 x 400 mm dimensions. After covering, they were left to stand in an environment of 20°C, 60% RH, and a CO2 concentration of 5%, and an accelerated carbonation test was performed. After the specified accelerated test period had elapsed, the test specimen was broken, and a 1% alcohol solution of phenolphthalein was sprayed onto the cross section to measure the carbonation depth. The results are shown in Figure 2.

[0027] Additionally, a test specimen prepared in the same manner as above and cured for 56 days was covered with epoxy resin except for one side of a 100 x 400 mm surface. After covering, it was exposed to rain outdoors for 3.8 years with the exposed surface facing vertically and outward from the building, and the carbonation depth of the exposed surface was measured. The average annual precipitation during the exposure period was 1777 mm / year, and the atmospheric carbon dioxide concentration was 0.041%. The results are shown in Figure 3.

[0028] For the total powder amount, the neutralization inhibitor is added as nitrate ions (NO3 -By adding 2.0 mass% calculated as formula weight 62), the carbonation rate ratio of Example 3 to Comparative Example 3 was about 0.36, and about 0.43 in the exposure environment. From this, it was confirmed that the carbonation inhibition effect was not only in the paste but also in concrete containing fine aggregate and coarse aggregate, and not only in the accelerated environment but also in the actual environment.

[0029] "Experiment 3" Various cements The materials shown below were mixed with various cements or mixtures of cement and admixtures in the mass ratios shown in Tables 3 to 9 to prepare cement pastes. Among the materials, ordinary Portland cement and high-early-strength Portland cement were made to satisfy JIS R 5210, blast-furnace cement was made to satisfy JIS R 5211, blast-furnace slag was made to satisfy JIS A 6206, silica fume was made to satisfy JIS A 6207, fly ash was made to satisfy JIS A 6201, and anhydrous gypsum was made to satisfy JIS R 9151. As calcium nitrate, a special grade reagent (calcium nitrate tetrahydrate (Ca(NO3)2·4H2O)) manufactured by Kanto Chemical Co., Ltd. was used, and the crystal water contained in calcium nitrate tetrahydrate was counted as water in Tables 3 to 9. Calcium nitrate was dissolved in advance in water to be added to harden the hydraulic composition, and then added to the hydraulic composition. Example 4 is a reference example.

[0030] Water: Yokohama City Water Bureau, tap water Ordinary Portland cement: Manufactured by Taiheiyo Cement Corporation High-early-strength Portland cement: Manufactured by Taiheiyo Cement Corporation Blast furnace slag (without gypsum): manufactured by DC Corporation, product name: Cerament Blast furnace slag (with gypsum): Manufactured by DC Corporation, product name: Cerament A (anhydrous gypsum) Addition of copper (2.1% in terms of SO3) Silica fume: manufactured by DC Corporation Fly ash: Techno Chubu Co., Ltd., Type II Anhydrous gypsum: manufactured by DC Corporation Calcium nitrate: Kanto Chemical Co., Ltd., special grade reagent, tetrahydrate

[0031] Ordinary Portland Cement [Table 3]

[0032] Equivalent to blast furnace cement (type C), Portland cement 30% by mass [Table 4]

[0033] Fly ash cement (type C) equivalent, Portland cement 70% by mass [Table 5]

[0034] Environmentally friendly cement (1), Portland cement 10% by mass [Table 6]

[0035] Environmentally friendly cement (2), Portland cement 25% by mass [Table 7]

[0036] Environmentally friendly cement (3), Portland cement 25% by mass [Table 8]

[0037] Environmentally friendly cement (4), Portland cement 32.7% by mass [Table 9]

[0038] In Tables 3 to 9, Table 3 is ordinary Portland cement, Table 4 is a mixture of ordinary Portland cement and blast furnace slag equivalent to blast furnace cement Type C, Table 5 is a mixture of ordinary Portland cement and fly ash equivalent to fly ash cement Type C, and Tables 6 to 9 are environmentally friendly cement.

[0039] Using each of the hydraulic compositions shown in Tables 3 to 9, an accelerated carbonation test was carried out in the same manner as in Experiment 1. From the results up to 28 days of the accelerated carbonation period, the carbonation rate was calculated, and for each, the carbonation rate ratio was calculated against the corresponding Comparative Example to which no carbonation inhibitor was added (the "Comparative Example" is followed by the same number as the number followed by the "Example", and the combination of the corresponding Example and Comparative Example is shown in the same table. For example, Example 4 corresponds to Comparative Example 4, and the combination is shown in Table 3). For each hydraulic composition, the carbonation rates of the Comparative Examples and the corresponding Examples and the calculated carbonation rate ratio are shown in Table 10.

[0040] [Table 10]

[0041] It was confirmed that the progress of carbonation can be suppressed in hydraulic compositions with a low Portland cement blend ratio, in which carbonation is likely to progress. Note that the progress of carbonation is also expected to be suppressed in Portland cement, but since Portland cement is difficult to carbonate in the first place, it is presumed that the measured value of the carbonation rate ratio is significantly affected by measurement errors.

[0042] "Experiment 4" Types of nitrate compounds To the mixture of Comparative Example 1, magnesium nitrate (hexahydrate), ammonium nitrate, sodium nitrate, and potassium nitrate were added in the mixing ratios shown in Table 11 to prepare cement paste. All of these nitrates were special grade reagents manufactured by Kanto Chemical Co., Ltd. Examples 11 to 14 are reference examples.

[0043] [Table 11]

[0044] Using each hydraulic composition shown in Table 11, an accelerated carbonation test was carried out in the same manner as in Experiment 1. The neutralization rate coefficient was calculated from the results up to the 28th day of the neutralization period. The relationship between the amount of neutralization inhibitor converted to nitrate ions and the neutralization rate coefficient was obtained. The ratios of the neutralization rate coefficients of Examples 11 to 14 to the neutralization rate coefficient of Comparative Example 1, in which no neutralization inhibitor was added, are shown in FIG. 4.

[0045] The neutralization rate was reduced by 0.4 to 0.9 times by adding magnesium nitrate, ammonium nitrate, sodium nitrate, and potassium nitrate. It was confirmed that the carbonation inhibitors made of nitrate compounds can suppress the progress of carbonation in various cements. It was also confirmed that the progress of carbonation can be further suppressed by increasing the amount of carbonation inhibitor. Even if the composition of the powder in the paste, mortar, and concrete was changed, the carbonation depth could be reduced by the carbonation inhibitor. In other words, it was confirmed that the carbonation inhibitor of the present invention can suppress the progress of carbonation in various types and blends of cement paste, mortar, and concrete.

Claims

1. The present invention includes a hydraulic powder containing Portland cement and a carbonation inhibitor containing calcium nitrate, The blending ratio of Portland cement in the total powder is 10% by mass or more and 70% by mass or less, The neutralization inhibitor is added to the total powder amount in the form of nitrate ions (NO 3 - , Formula weight 62) is 0.8% by mass or more and 5.0% by mass or less, The hydraulic composition, wherein the powder further contains at least one of blast furnace slag and fly ash.

2. The present invention includes a hydraulic powder containing Portland cement and blast furnace slag, and a carbonation inhibitor containing calcium nitrate, The blending ratio of Portland cement in the total powder is 10% by mass or more and 32.7% by mass or less, The neutralization inhibitor is added to the total powder amount in the form of nitrate ions (NO 3 - , Formula weight 62) is 0.8% by mass or more and 5.0% by mass or less, The hydraulic composition further comprises at least one of silica fume and anhydrous gypsum.

Citation Information

Patent Citations

  • Cement admixture and cement composition

    JP1993330877A

  • Low environmental load type ultra high early strength concrete

    JP2001039758A

  • Shrinkage reduction agent for hydraulic material

    JP2005187278A

  • Cement composition

    JP2006083039A

  • Pre-blended cement composition containing a non-chloride accelerator

    JP2008515759A