Polyethylene fiber

A bimodal ethylene resin with optimized molecular weight distribution and melting characteristics addresses the mechanical and processability issues of polyethylene fibers, enhancing their performance in both melt and gel spinning applications.

JP2024166533APending Publication Date: 2024-11-29TOSOH CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023082690
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing polyethylene fibers face challenges with mechanical properties and processability, particularly in melt spinning applications, limiting their versatility and effectiveness.

Method used

Development of a polyethylene fiber using a bimodal ethylene resin with specific molecular weight distribution and melting characteristics, achieved through a combination of ultra-high molecular weight and low molecular weight components, optimized using metallocene catalysts and controlled polymerization methods.

Benefits of technology

The resulting polyethylene fiber exhibits excellent tensile strength, elastic modulus, and processability, suitable for both melt and gel spinning, with improved mechanical properties and reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166533000001
    Figure 2024166533000001
  • Figure 2024166533000002
    Figure 2024166533000002
  • Figure 2024166533000003
    Figure 2024166533000003
Patent Text Reader

Abstract

To provide a polyethylene fiber which is converted into a high-molecular-weight ethylenic resin having a bimodal molecular weight and melting property, preferably, a composition of the ethylenic resin and polyethylene, and thereby is excellent in mechanical characteristics such as tensile braking stress and elastic modulus, and is also excellent in workability.SOLUTION: A polyethylene fiber is made of an ethylenic resin having an HLMFR at a temperature of 190°C and a load of 21.6 kg of 0.01 to 100 g / 10 min and a bimodal elution curve measured by GPC, preferably, is made of a composition containing polyethylene having an MFR at a temperature of 190°C and a load of 2.16 kg of 0.01 to 10 g / 10 min and a density of 930 to 980 kg / m3.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a specific polyethylene fiber, and more specifically, to a polyethylene fiber which contains a high molecular weight ethylene-based resin having bimodal molecular weight and meltability, and thereby has excellent mechanical properties such as tensile break stress and elastic modulus as well as excellent processability. [Background technology]

[0002] Polyethylene is a resin used in a wide range of applications, and in order to make it suitable for each application, technologies have been proposed to control the molecular weight distribution and composition by combining two or more resin components, thereby improving various physical properties and appearance. For example, an increase in higher molecular weight components improves mechanical strength but decreases moldability, while an increase in lower molecular weight components decreases mechanical strength but improves moldability.

[0003] As a method for combining two or more types of polyethylene components, there have been proposed a method in which each component is polymerized and then blended by melt kneading or dry blending, a method in which multi-stage polymerization is carried out continuously, a method in which two or more types of polyethylene components are simultaneously produced by adding a plurality of transition metal catalysts to a polymerization system, a method in which a combination of these is carried out, etc. In addition, a resin modifier has also been proposed (see, for example, Patent Document 1) that is blended with a target material to modify the physical properties, appearance, etc. of the target material.

[0004] Ultra-high molecular weight polyethylene, which has attracted attention in recent years (see, for example, Patent Documents 2 and 3), has an extremely high molecular weight equivalent to a viscosity average molecular weight (hereinafter sometimes referred to as Mv) of 1 million or more, and therefore has excellent impact resistance, self-lubrication, abrasion resistance, weather resistance, chemical resistance, dimensional stability, etc., and has high physical properties comparable to those of engineering plastics. For this reason, attempts have been made to apply it to uses such as sheets, films, high-strength fibers, sliding members, lining materials, line parts in the food industry, machine parts, artificial joints, sporting goods, microporous membranes, and separators by various molding methods.

[0005] Furthermore, polyethylene fibers made of polyethylene have attracted attention because they exhibit excellent performance despite being made of a general-purpose material called polyethylene. Proposed fibers with excellent cut resistance include those made of polyethylene with an aspect ratio of less than 3 and hard particles with an average particle size of 3.0 to 15.0 μm blended with polyethylene having an [η] = 0.8 to 4.9 dl / g (see, for example, Patent Document 4), and fibers with extremely excellent creep resistance include those made of ultra-high molecular weight polyethylene having specific ethyl branches in the side chains (see, for example, Patent Document 5). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-179304 A [Patent Document 2] Patent No. 4868853 [Patent Document 3] Patent No. 6405888 [Patent Document 4] International Patent Publication No. 2018 / 181309 [Patent Document 5] Patent Publication No. 2021-70902 Summary of the Invention [Problem to be solved by the invention]

[0007] However, while the modifier proposed in Patent Document 1 was effective in improving processability to a certain extent, further improvement is required in terms of improving mechanical strength, and Patent Documents 2 and 3 merely propose ultra-high molecular weight polyethylene, leaving room for problems in terms of molding processability.

[0008] The polyethylene fiber proposed in Patent Document 4 is applicable to melt spinning, but has problems with mechanical properties. Also, it is difficult to apply the polyethylene fiber proposed in Patent Document 5 to melt spinning, which has excellent processability.

[0009] Therefore, the emergence of polyethylene fibers that have excellent processability that can be applied to not only gel spinning but also melt spinning and that also have excellent mechanical properties has been anticipated. [Means for solving the problem]

[0010] Means for Solving the Problems The present inventors conducted intensive studies to solve the above problems and found that an ethylene-based resin having specific melting properties and molecular weight configuration can be applied to melt spinning and can be made into a polyethylene fiber having excellent tensile properties such as tensile breaking stress and elastic modulus, thereby completing the present invention.

[0011] That is, the present invention relates to (1) a polyethylene fiber, characterized in that it contains an ethylene-based resin which has a high melt flow rate (HLMFR) of 0.01 to 100 g / 10 min at a temperature of 190°C under a load of 21.6 kg and a bimodal elution curve measured by gel permeation chromatography in accordance with JIS 6922-2:1997.

[0012] The present invention will be described in detail below.

[0013] The polyethylene fiber of the present invention is (1) a polyethylene fiber made of an ethylene-based resin comprising an ethylene-based resin (c) having a melt flow rate (hereinafter sometimes referred to as HLMFR) of 0.01 to 100 g / 10 min at a temperature of 190° C. and a load of 21.6 kg in accordance with JIS 6922-2:1997 and a bimodal elution curve measured by gel permeation chromatography (hereinafter sometimes referred to as GPC). The ethylene-based resin (c) may be a bimodal ethylene-based resin having a relatively high molecular weight that exhibits melting behavior and an elution curve measured by GPC that exhibits a bimodal elution curve, and examples of the ethylene-based resin include ethylene homopolymers and ethylene-α-olefin copolymers. Examples of the α-olefins in this case include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, etc., and ethylene homopolymers are preferable because they result in polyethylene fibers with particularly excellent tensile properties.

[0014] The ethylene-based resin (iii) has (1) an HLMFR of 0.01 to 100 g / 10 min and exhibits melt fluidity. If the HLMFR is less than 0.01 g / 10 min, the melt fluidity is poor and the processability during melt spinning is poor. On the other hand, if the HLMFR is more than 100 g / 10 min, the resulting fiber has poor mechanical properties.

[0015] The ethylene resin (iii) constituting the polyethylene fiber of the present invention is an ethylene polymer having a bimodal molecular weight distribution, and preferably contains a specific ultra-high molecular weight polyethylene component (i) as a specific component, since it results in a polyethylene fiber having an excellent balance between processability and tensile properties. In this case, the bimodal molecular weight distribution is preferably one in which the elution curve measured by GPC has two peaks, and when the elution curve is expressed as a differential molecular weight distribution (x-axis: Log [M], y-axis: differential distribution value) and the peaks are divided into two normal distributions (normal distribution of ultra-high molecular weight polyethylene component (i) and normal distribution of polyethylene component (ii)) according to the following formula (i), it satisfies (2-1) to (2-3). f(x)=a×(1 / (2π(σ 2 )) (1 / 2) ) exp(-((x-μ) 2 ) / (2(σ 2 ))) Formula (i) (Here, a is the peak intensity, σ is the standard deviation, x is the variable, and μ is the mean.) (2-1) The ultra-high molecular weight polyethylene component (a) (hereinafter may be referred to as component (a)) represented as a high molecular weight peak component has a weight average molecular weight (hereinafter may be referred to as Mw) of 900,000 to 5,000,000 and a molecular weight distribution expressed as weight average molecular weight / number average molecular weight (hereinafter may be referred to as Mw / Mn) of 2.0 to 5.0, (2-2) The polyethylene component (b) (hereinafter may be referred to as component (b)) represented as a low molecular weight peak component has an Mw of 10,000 to 500,000 and an Mw / Mn of 2.0 to 5.0, and (2-3) the component (a) / component (b) (weight ratio) is greater than 5 / 95 and less than 80 / 20, and it is particularly preferable that the component (a) / component (b) (weight ratio) is 10 / 90 to 50 / 50.

[0016] When the ethylene-based resin (iii) is one in which the ultra-high molecular weight component (i) and the low molecular weight component (ii) coexist in a specific ratio, the ethylene-based resin has excellent melting properties. In addition, when blended with polyethylene, the component (i) can be highly dispersed, making it possible to highly modify the tensile properties of the polyethylene fiber without impairing the appearance.

[0017] In order to obtain a polyethylene fiber having a particularly excellent balance between dispersibility in polyethylene and improved mechanical properties, the ethylene-based resin (c) preferably has (3) Mw / Mn, calculated as linear polyethylene as measured by GPC, of ​​4.0 or more and less than 50, and particularly preferably 4.0 or more and 30 or less.

[0018] In addition, since the components (A) and (B) are different from a simple blend in which each component is independently dispersed, the ethylene-based resin (C) is (4) measured using a differential scanning calorimeter (hereinafter sometimes referred to as DSC) by heating from 0°C to 230°C at a heating rate of 10°C / min (hereinafter sometimes referred to as 1st scan) at a crystal melting peak (hereinafter referred to as Tm 1 It is preferable that the peak intensity distribution is unimodal.

[0019] The ethylene-based resin (iii) constituting the polyethylene fiber of the present invention may be any resin as long as it satisfies the above-mentioned characteristics. In particular, it is preferable that the ethylene-based resin (iii) is produced using a metallocene catalyst, since it is easy to control the molecular weight and molecular weight distribution and to produce an (ultra)high molecular weight. Among these, examples of a method for producing the ethylene-based resin (iii) having both the component (i) and the component (ii) include a method using a co-supported catalyst in which two or more types of metallocene complexes are supported on a carrier as the catalyst system, and a method using a multi-stage polymerization of two or more stages.

[0020] The polymerization method of the ethylene-based resin (iii) may be, for example, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, a slurry polymerization method, etc., among which, the slurry polymerization method is preferable since it enables the production of an ethylene-based resin with a regular particle shape. The solvent used in the slurry polymerization method may be any organic solvent that is generally used, for example, benzene, toluene, xylene, pentane, hexane, heptane, etc., and liquefied gases such as isobutane and propane, and olefins such as 1-butene and 1-hexene can also be used as the solvent.

[0021] The production catalyst used to produce the ethylene-based resin (iii) may be any catalyst capable of producing the ethylene-based resin. For example, in the case of multi-stage polymerization, a metallocene catalyst obtained from at least a transition metal compound (A-1), an organically modified clay modified with an aliphatic salt (B), and an organoaluminum compound (C) may be used. For example, in the case of a co-supported catalyst method, a metallocene catalyst obtained from at least a transition metal compound (A-1), a transition metal compound (A-2), an organically modified clay modified with an aliphatic salt (B), and an organoaluminum compound (C) may be used.

[0022] Examples of the transition metal compound (A-1) include transition metal compounds having a (substituted) cyclopentadienyl group and a (substituted) fluorenyl group, transition metal compounds having a (substituted) cyclopentadienyl group and a (substituted) indenyl group, transition metal compounds having a (substituted) indenyl group and a (substituted) fluorenyl group, and the like. In this case, examples of the transition metal include zirconium and hafnium, and among these, zirconium compounds having a (substituted) cyclopentadienyl group and an amino group-substituted fluorenyl group and hafnium compounds having a (substituted) cyclopentadienyl group and an amino group-substituted fluorenyl group are preferred, as they enable efficient production of an ethylene-based resin suitable for polyethylene fibers.

[0023] More specifically, for example, diphenylmethylene(1-indenyl)(9-fluorenyl)zirconium dichloride, diphenylmethylene(1-indenyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(4-phenyl-1-indenyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2-(dimethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2-(dimethylamino)-9-fluorenyl)zirconium dichloride, )(2-(diethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2-(dibenzylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2,7-bis(dimethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2,7-bis(diethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2,7-bis (dibenzylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(4-(dimethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(4-(diethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(4-(dibenzylamino)-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-9-fluorenyl)zirconium dichloride diphenylmethylene(cyclopentadienyl)(2-(diethylamino)-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(diethylamino)-7-ethyl-9-fluorenyl)zirconium dichloride,Diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-7-ethyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-7-ethyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-7-n-propyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(diethylamino)-7-n-propyl-9-fluorenyl)zirconium dichloride diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-7-n-propyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-7-n-propyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-7-isopropyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(diphenylmethylene)(cyclopentadienyl)(2-(diphenylmethylene)(cyclopentadienyl) diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-7-isopropyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-7-isopropyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-7-n-butyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-7-n-butyl-9-fluorenyl)zirconium dichloride Examples of zirconium compounds include diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-7-t-butyl-9-fluorenyl)zirconium dichloride and diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-7-t-butyl-9-fluorenyl)zirconium dichloride; zirconium compounds in which the dichloro form of these compounds is replaced with a dimethyl form, a diethyl form, a dihydro form, a diphenyl form or a dibenzyl form; and hafnium compounds in which the zirconium of these compounds is replaced with hafnium.

[0024] Examples of the transition metal compound (A-2) include a transition metal compound having a (substituted) cyclopentadienyl group and a (substituted) fluorenyl group, a transition metal compound having a (substituted) cyclopentadienyl group and a (substituted) indenyl group, and a transition metal compound having a (substituted) indenyl group and a (substituted) indenyl group.

[0025] More specifically, dimethylsilanediylbis(cyclopentadienyl)zirconium dichloride, diethylsilanediylbis(cyclopentadienyl)zirconium dichloride, dicyclohexylsilanediylbis(cyclopentadienyl)zirconium dichloride, diphenylsilanediylbis(cyclopentadienyl)zirconium dichloride, dimethylsilanediylbis(methylcyclopentadienyl)zirconium dichloride, diethylsilanediylbis(methylcyclopentadienyl)zirconium dichloride, dicyclohexylsilanediylbis(cyclopentadienyl)zirconium dichloride, Silanediylbis(methylcyclopentadienyl)zirconium dichloride, diphenylsilanediylbis(methylcyclopentadienyl)zirconium dichloride, dimethylsilanediylbis(2,4-dimethylcyclopentadienyl)zirconium dichloride, diethylsilanediylbis(2,4-dimethylcyclopentadienyl)zirconium dichloride, dicyclohexylsilanediylbis(2,4-dimethylcyclopentadienyl)zirconium dichloride, diphenylsilanediylbis(2,4-dimethylcyclopentadienyl)zirconium dichloride silanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, dimethylsilanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, diethylsilanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, dicyclohexylsilanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, diphenylsilanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, dimethylsilanediyl[(cyclopentadienyl)(4,7-dimethylindenyl)]zirconium dichloride silanediyl[(cyclopentadienyl)(4,7-dimethylindenyl)]zirconium dichloride, dicyclohexylsilanediyl[(cyclopentadienyl)(4,7-dimethylindenyl)]zirconium dichloride, diphenylsilanediyl[(cyclopentadienyl)(4,7-dimethylindenyl)]zirconium dichloride, dimethylsilanediyl[(cyclopentadienyl)(2,4,7-trimethylindenyl)]zirconium dichloride, diethylsilanediyl[(cyclopentadienyl)(2,4,7-trimethylindenyl)]zirconium dichloride, dicyclohexylsilanediyl[(cyclopentadienyl)(2,4,7-trimethylindenyl)]zirconium dichloride, diphenylsilanediyl[(cyclopentadienyl)(2,4,7-trimethylindenyl)]zirconium dichloride, bis(indenyl)zirconium dichloride, isopropylidenebis(indenyl)zirconium dichloride, (methyl)(phenyl)methylenebis(indenyl)zirconium dichloride, diphenyl Phenylmethylene bis(indenyl)zirconium dichloride, ethylene bis(indenyl)zirconium dichloride, isopropylidene bis(2-methylindenyl)zirconium dichloride, (methyl)(phenyl)methylene bis(2-methylindenyl)zirconium dichloride, diphenylmethylene bis(2-methylindenyl)zirconium dichloride, ethylene bis(2-methylindenyl)zirconium dichloride, isopropylidene bis(tetrahydroindenyl)zirconium dichloride , (methyl)(phenyl)methylenebis(tetrahydroindenyl)zirconium dichloride, diphenylmethylenebis(tetrahydroindenyl)zirconium dichloride, ethylenebis(tetrahydroindenyl)zirconium dichloride, isopropylidene(cyclopentadienyl)(fluorenyl)zirconium dichloride, (methyl)(phenyl)methylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride dichloride, ethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, isopropylidene(cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride, (methyl)(phenyl)methylene(cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride, ethylene(cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride; zirconium compounds in which the dichloro form of these compounds is replaced with a dimethyl form, a diethyl form, a dihydro form, a diphenyl form, or a dibenzyl form; and hafnium compounds in which the zirconium of these compounds is replaced with hafnium.

[0026] Examples of the organically modified clay (B) modified with an aliphatic salt include N,N-dimethyl-behenylamine hydrochloride, N-methyl-N-ethyl-behenylamine hydrochloride, N-methyl-Nn-propyl-behenylamine hydrochloride, N,N-dioleyl-methylamine hydrochloride, N,N-dimethyl-behenylamine hydrofluoride, N-methyl-N-ethyl-behenylamine hydrofluoride, N-methyl-Nn-propyl-behenylamine hydrofluoride, N,N-dioleyl-methylamine hydrofluoride, N,N-dimethyl-behenyl ... behenylamine hydrobromide, N-methyl-N-ethyl-behenylamine hydrobromide, N-methyl-Nn-propyl-behenylamine hydrobromide, N,N-dioleyl-methylamine hydrobromide, N,N-dimethyl-behenylamine hydroiodide, N-methyl-N-ethyl-behenylamine hydroiodide, N-methyl-Nn-propyl-behenylamine hydroiodide, N,N-dioleyl-methylamine hydroiodide, N,N-dimethyl-behenylamine sulfate, N-methyl-N-ethyl-behenylamine sulfate aliphatic amine salts such as N-methyl-Nn-propyl-behenylamine sulfate and N,N-dioleyl-methylamine sulfate; P,P-dimethyl-behenylphosphine hydrochloride, P,P-diethyl-behenylphosphine hydrochloride, P,P-dipropyl-behenylphosphine hydrochloride, P,P-dimethyl-behenylphosphine hydrofluoride, P,P-diethyl-behenylphosphine hydrofluoride, P,P-dipropyl-behenylphosphine hydrofluoride, P,P-dimethyl-behenylphosphine hydrobromide, P,P- Examples of the clay modified with an aliphatic salt include aliphatic phosphonium salts such as diethyl-behenylphosphine hydrobromide, P,P-dipropyl-behenylphosphine hydrobromide, P,P-dimethyl-behenylphosphine hydroiodide, P,P-diethyl-behenylphosphine hydroiodide, P,P-dipropyl-behenylphosphine hydroiodide, P,P-dimethyl-behenylphosphine sulfate, P,P-diethyl-behenylphosphine sulfate, and P,P-dipropyl-behenylphosphine sulfate.

[0027] The clay compound constituting the organically modified clay (B) may be any compound as long as it belongs to the category of clay compounds. In general, the organically modified clay (B) is formed by stacking many layers called silicate layers, which are composed of a tetrahedral sheet of silica tetrahedrons connected in two dimensions and an octahedral sheet of alumina octahedrons or magnesia octahedrons connected in two dimensions in a 1:1 or 2:1 ratio. The Si in some of the silica tetrahedra is replaced by Al, the Al in the alumina octahedrons by Mg, and the Mg in the magnesia octahedrons by Li, etc., resulting in a lack of positive charges within the layers and the layers as a whole being negatively charged. In order to compensate for this negative charge, Na is introduced between the layers. + Or Ca 2+ As the clay compound, there are natural or synthetic products such as kaolinite, talc, smectite, vermiculite, mica, brittle mica, and malachite, and these can be used, among which smectite is preferred because of its ease of availability and ease of organic modification, and among smectites, hectorite or montmorillonite is even more preferred.

[0028] The organically modified clay (B) can be obtained by introducing the aliphatic salt between the layers of the clay compound to form an ion complex. When preparing the organically modified clay (B), it is preferable to select conditions of a clay compound concentration of 0.1 to 30% by weight and a treatment temperature of 0 to 150°C. The aliphatic salt may be prepared as a solid and dissolved in a solvent for use, or a solution of the aliphatic salt may be prepared by chemical reaction in a solvent and used as is. As for the reaction ratio of the clay compound and the aliphatic salt, it is preferable to use an equivalent or greater amount of aliphatic salt relative to the exchangeable cations of the clay compound. Examples of the treatment solvent that can be used include aliphatic hydrocarbons such as pentane, hexane, and heptane; aromatic hydrocarbons such as benzene and toluene; alcohols such as ethyl alcohol and methyl alcohol; ethers such as ethyl ether and n-butyl ether; halogenated hydrocarbons such as methylene chloride and chloroform; acetone; 1,4-dioxane; tetrahydrofuran; water, and the like. It is preferable to use alcohols or water alone or as one component of the solvent.

[0029] In addition, the particle size of the organically modified clay (B) constituting the production catalyst is not limited, and is preferably 1 to 100 μm, since it is excellent in efficiency during catalyst preparation and efficiency during ethylene-based resin production. There is also no limit to the method of adjusting the particle size, and large particles may be crushed to an appropriate particle size, small particles may be granulated to an appropriate particle size, or crushing and granulation may be combined. In addition, the particle size may be adjusted either on the clay before organic modification or on the organically modified clay after modification.

[0030] As the organoaluminum compound (C), any compound that belongs to the category called an organoaluminum compound can be used, and examples thereof include alkylaluminum such as trimethylaluminum, triethylaluminum, and triisobutylaluminum.

[0031] The proportions of the transition metal compounds (A-1) and (A-2) (hereinafter, the transition metal compounds (A-1) and (A-2) are collectively referred to as component (A)), the organically modified clay (B) (hereinafter, also referred to as component (B)), and the organoaluminum compound (C) (hereinafter, also referred to as component (C)) constituting the production catalyst are not subject to any restrictions as long as they can be used as a production catalyst. In particular, in order to provide a production catalyst capable of efficiently producing the ethylene-based resin (C), the molar ratio per metal atom of component (A) to component (C) is preferably in the range of component (A):component (C)=100:1 to 1:100,000, and more preferably in the range of 1:1 to 1:10,000. Furthermore, the weight ratio of component (A) to component (B) is preferably component (A):component (B)=10:1 to 1:10000, and more preferably in the range of 3:1 to 1:1000.

[0032] Regarding the preparation method of the production catalyst, any method may be used as long as it is possible to prepare a production catalyst containing the (A) component, the (B) component, and the (C) component, and for example, a method of mixing the (A), (B), and (C) components in a solvent inert to the respective components, or using the monomer to be polymerized as a solvent, can be mentioned. In addition, there is no restriction on the order in which these components are reacted, and there is no restriction on the temperature and time of this treatment. In addition, it is also possible to prepare a production catalyst using two or more kinds of each of the (A), (B), and (C) components.

[0033] The polymerization conditions such as polymerization temperature, polymerization time, polymerization pressure, and monomer concentration when producing the ethylene resin (iii) can be arbitrarily selected, and among them, it is preferable to carry out the polymerization at a polymerization temperature of 0 to 100°C, for a polymerization time of 10 seconds to 20 hours, and at a polymerization pressure of normal pressure to 100 MPa. It is also possible to adjust the molecular weight by using hydrogen or the like during the polymerization. The polymerization can be carried out by any method such as a batch method, a semi-continuous method, or a continuous method, and it is also possible to carry out the polymerization in two or more stages by changing the polymerization conditions. The polymer particles obtained after the polymerization is completed can be separated and recovered from the polymerization solvent by a conventionally known method, and dried to obtain the product.

[0034] The polyethylene fiber of the present invention is preferably a melt-spun polyethylene fiber, which is suitable for an excellent processing method, and in this case, it is of course made of the ethylene resin (iii), but it is preferably made of a composition (e) containing the ethylene resin (iii) and polyethylene (iv) because it has particularly excellent melting properties. The polyethylene (iv) in this case may be any polyethylene that belongs to the category of polyethylene, for example, ethylene homopolymer and ethylene-α-olefin copolymer, and examples of the α-olefin in this case include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, etc., and among them, ethylene homopolymer is preferred because it will result in a polyethylene fiber with excellent tensile properties, and in particular, polyethylene fiber with an MFR of 0.01 to 10 g / 10 min and a density of 930 to 980 kg / m because it will result in a polyethylene fiber with an excellent balance between processability and mechanical properties. 3 Preferably, the polyethylene is a polyethylene having a molecular weight of 100 or more, more preferably a high density polyethylene. An example of such a polyethylene is Nipolon Hard (trade name, manufactured by Tosoh Corporation).

[0035] The blending amount in the case of forming the composition (E) is arbitrary as long as excellent tensile properties as a polyethylene fiber are expressed, and in particular, since the balance between its mechanical properties and processability is excellent, it is preferable to form the composition (E) containing 1 to 100 parts by weight of the ethylene-based resin (C) per 100 parts by weight of the polyethylene (D), and particularly preferably 5 to 50 parts by weight. The method for preparing the composition (E) in this case can be prepared by any method, and for example, a method can be mentioned in which 1 to 100 parts by weight of the ethylene-based resin (C) is blended per 100 parts by weight of the polyethylene (D), and further additives normally used in polyolefins, such as weather resistance stabilizers, heat resistance stabilizers, antistatic agents, antislip agents, antiblocking agents, antifogging agents, lubricants, pigments, nucleating agents, plasticizers, antioxidants, antioxidants, ultraviolet absorbers, neutralizing agents, surfactants, slip agents, inorganic or organic fillers, etc., are blended and kneaded by a kneading machine or the like. The conditions for this process may be any as long as it enables the formation of the composition (E). For example, an example of the process includes a method in which the ethylene-based resin (C), and, in some cases, the polyethylene (D) and / or other additives, etc. are heated, melted, and kneaded at a temperature in the range of 190°C to 250°C for about 20 to 30 seconds using a single-screw or twin-screw melt kneader or the like, and the mixture is then cut into granular pellets to be used as a polyethylene fiber material.

[0036] The polyethylene fiber of the present invention can be prepared by any method, for example, melt spinning, gel spinning, etc., and melt spinning is preferred because it has better processability and does not require a step of removing the solvent after spinning, resulting in less environmental impact.

[0037] As the melt spinning, for example, ethylene resin (c), ethylene resin (c) and the above-mentioned compounding agent are mixed, and further ethylene resin (c) and polyethylene (d) are mixed, and the mixture is extruded from a spinning nozzle by an extruder at a temperature 50°C or more higher than the melting point of ethylene resin (c) as it is or after it is made into a composition (e), to obtain an undrawn extruded yarn. As the gel spinning, for example, ethylene resin (c), ethylene resin (c) and the above-mentioned compounding agent are mixed, and further ethylene resin (c) and polyethylene (d) are mixed, and the mixture is extruded from a spinning nozzle by an extruder at a temperature 10°C or more higher than the melting point of ethylene resin (c) as it is or after it is made into a composition (e), to obtain an undrawn extruded yarn. Furthermore, a method may be used in which an undrawn yarn is drawn in a single-stage or multi-stage drawing process to form a drawn yarn, and the draw ratio in this case may be 2 to 100. The fiber diameter in this case may be appropriately selected, and may be, for example, 10 to 500 μm.

[0038] Since the polyethylene fiber of the present invention is particularly excellent in the effect of improving heat resistance, it is preferable that the difference (Tmd-Tm0) between the crystalline melting peak temperature (Tm0) of the undrawn yarn before drawing and the crystalline melting peak temperature (Tmd) of the drawn polyethylene fiber, which is the drawn yarn, is 5° C.≦Tmd-Tm0. The crystalline melting peak temperature can be measured using a DSC as the crystalline melting peak temperature in the 1st scan when the temperature is raised from 0° C. to 230° C. at a heating rate of 10° C. / min (1st scan).

[0039] The polyethylene fiber of the present invention may be any fibrous material, such as yarn, monofilament, multifilament, etc., and may have a circular or elliptical shape as well as a core-sheath structure, a star shape, a polygonal shape, a hollow shape, etc. The polyethylene fiber can be used, for example, for gloves, vests, tapes, sheets, braids, twisted threads, fishing lines, ropes, nets, etc. Effect of the Invention

[0040] This polyethylene fiber has excellent processability and mechanical strength, and is expected to be lightweight and have a long life, making it suitable for a variety of applications. EXAMPLES

[0041] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples as long as the gist of the present invention is not exceeded.

[0042] Unless otherwise specified, the reagents used were either commercially available or synthesized according to known methods.

[0043] The organically modified clay was pulverized using a jet mill (product name: CO-JET SYSTEM α MARK III, manufactured by Seishin Enterprise Co., Ltd.), and the particle size after pulverization was measured using a Microtrack particle size distribution measuring device (product name: MT3000, manufactured by Nikkiso Co., Ltd.) using ethanol as a dispersant.

[0044] The preparation of the catalyst for production, the production of the ethylene resin, and the purification of the solvent were all carried out under an inert gas atmosphere. The hexane solution (20 wt%) of triisobutylaluminum manufactured by Toso Finechem Co., Ltd. was used.

[0045] Furthermore, various physical properties of the ethylene resin and polyethylene were measured by the methods shown below.

[0046] ~Measurement of intrinsic viscosity ([η])~ The measurements were performed using an Ubbelohde viscometer, decahydronaphthalene as a solvent, at 135° C., and an ethylene resin concentration of 0.005 wt %.

[0047] ~Measurement of Mw and Mn~ Measurements were performed using an ultra-high temperature GPC (SSC-7110, manufactured by Senshu Scientific Co., Ltd.) equipped with a column (TSKgel GMHHR-H(S)HT, manufactured by Tosoh Corporation) with 1-chloronaphthalene as the eluent at a column temperature of 210°C, a sample concentration of 0.5 mg / ml, and an injection volume of 0.2 ml. The molecular weight calibration curve was calibrated using a standard polystyrene sample, and Mw and Mn were converted to linear polyethylene.

[0048] ~MFR~ The melt flow rate was measured at a temperature of 190° C. under a load of 2.16 kg in accordance with JIS6922-2:1997.

[0049] ~HLMFR~ The melt flow rate was measured at a temperature of 190° C. and a load of 21.6 kg in accordance with JIS6922-2:1997.

[0050] ~Measurement of thermal melting of ethylene resin~ Using a DSC (manufactured by SII NanoTechnology, Inc., product name: DSC6220), the temperature was raised from 0°C to 230°C at a heating rate of 10°C / min (1st scan), and the crystal melting peak (Tm 1 ), heat of fusion (ΔH 1 ) measurements were carried out.

[0051] Furthermore, various physical properties of the polyethylene fibers were measured by the methods shown below.

[0052] ~Tensile properties~ Using a tensile tester (manufactured by BALDWIN (product name) UTM-2.5T-PL), polyethylene fibers were cut into lengths of 3 cm at 25° C. and 50 mm / min, and the 1% tensile modulus and tensile breaking stress were measured. ~Measurement of thermal melting of polyethylene fibers~ Using a DSC (DSC6220 (product name) manufactured by SII Nano Technology Co., Ltd.), the temperature was raised from 0°C to 230°C at a heating rate of 10°C / min (1st scan), and the crystal melting peak (Tm) and heat of fusion (ΔH) of the 1st scan were measured. The amount of polyethylene sample was 6 mg. The Tm of unstretched polyethylene fiber was Tm0, and the Tm of stretched polyethylene fiber was Tmd. Fibers with a difference between Tm0 and Tmd (Tmd-Tm0) of 5°C or less than Tmd-Tm0 were considered to have a high heat resistance improvement effect due to stretching.

[0053] Preparation Example 1 (1) Preparation of organically modified clay 300 ml of industrial alcohol (manufactured by Japan Alcohol Sales Co., Ltd., (trade name) Ekinen F-3) and 300 ml of distilled water were placed in a 1-liter flask, 15.0 g of concentrated hydrochloric acid and 42.4 g (120 mmol) of dimethylbehenylamine (manufactured by Lion Specialty Chemicals, (trade name) Lipomin DM22D) were added, and the mixture was heated to 45°C to disperse 100 g of synthetic hectorite (manufactured by BYK Additives Limited, (trade name) Laponite RDS), and then the mixture was heated to 60°C and stirred for 1 hour while maintaining the temperature. After filtering the slurry, it was washed twice with 600 ml of hot water at 60°C and dried in a dryer at 85°C for 12 hours to obtain 125 g of organically modified clay. This organically modified clay was pulverized in a jet mill to a median diameter of 10 μm.

[0054] (2) Preparation of catalyst suspension for production After replacing the air in a 300 ml flask equipped with a thermometer and reflux condenser with nitrogen, 25.0 g of the organically modified clay obtained in (1) and 108 ml of hexane were added, followed by 0.628 g of diphenylmethylene(cyclopentadienyl)(2-diethylamino-9-fluorenyl)zirconium dichloride and 142 ml of a hexane solution of 20 wt% triisobutylaluminum, and the mixture was stirred at 60°C for 3 hours. After cooling to 45°C, the supernatant was removed and washed twice with 200 ml of hexane, and then 200 ml of hexane was added to obtain a suspension of a catalyst for production (solid weight content: 12.5 wt%).

[0055] Preparation Example 2 (1) Preparation of organically modified clay The same procedure as in Preparation Example 1 was followed.

[0056] (2) Preparation of catalyst suspension for production After replacing the air in a 300 ml flask equipped with a thermometer and a reflux condenser with nitrogen, 25.0 g of the organically modified clay obtained in (1) and 108 ml of hexane were added, followed by 0.669 g of diphenylmethylene(cyclopentadienyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride and 142 ml of a hexane solution of 20 wt% triisobutylaluminum, and the mixture was stirred at 60°C for 3 hours. After cooling to 45°C, the supernatant was removed and washed twice with 200 ml of hexane, and then 200 ml of hexane was added to obtain a suspension of a catalyst for production (solid weight content: 12.5 wt%).

[0057] Preparation Example 3 (1) Preparation of organically modified clay In a 1-liter flask, 300 ml of industrial alcohol (product name Ekinen F-3, manufactured by Japan Alcohol Sales Co., Ltd.) and 300 ml of distilled water were added, and 15.0 g of concentrated hydrochloric acid and dioleylmethylamine ((C 18 H 35 ) 2 (CH 3 )N, 63.7g (120mmol) of (trade name) Lipomin MO (manufactured by Lion Specialty Chemicals Co., Ltd.) was added and heated to 45℃, after which 100g of synthetic hectorite (trade name Laponite RD, manufactured by BYK) was dispersed, and the temperature was raised to 60℃ and stirred for 1 hour while maintaining the temperature. After filtering the slurry, it was washed twice with 600ml of water at 60℃ and dried in a dryer at 85℃ for 12 hours to obtain 130g of organically modified clay. This organically modified clay was pulverized in a jet mill to a median diameter of 15μm.

[0058] (2) Preparation of catalyst suspension for production After replacing the air in a 300 ml flask equipped with a thermometer and a reflux condenser with nitrogen, 25.0 g of the organically modified clay obtained in (1) and 108 ml of hexane were added, followed by the addition of 0.392 g (1 mmol) of bis(indenyl)zirconium dichloride and 142 ml of a 20 wt% hexane solution of triisobutylaluminum, and stirring for 3 hours at 60°C. After cooling to room temperature, the supernatant was removed and washed twice with 220 ml of hexane, followed by the addition of 220 ml of hexane to obtain a suspension of a catalyst for production (solid weight content: 12.0 wt%).

[0059] Manufacturing Example 1 As described below, a bimodal polyethylene ethylene-based resin (III-1) was produced by two-stage polymerization in which the polymerization of component (III-1) was successively carried out after the polymerization of component (III-1). The ethylene-based resin (III-1) had an HLMFR of 2.3 g / 10 min and an [η] of 6.5 dl / g.

[0060] Manufacturing of component (A-1) 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 1 were added to a 10-liter autoclave, and the temperature was raised to 60°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 1 hour. 100 g of ethylene was consumed during the polymerization in terms of polyethylene, and the [η] of component (A-1) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 22 dl / g.

[0061] Manufacture of component (B-1) and ethylene resin (C-1) After polymerizing component (a-1), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.50MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 9 hours to polymerize component (b-1), thereby producing ethylene-based resin (c-1), which is an ethylene homopolymer. During the polymerization, 900g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-1) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0062] Manufacturing Example 2 As described below, a bimodal polyethylene ethylene-based resin (III-2) was produced by two-stage polymerization in which the polymerization of component (III-2) was successively carried out after the polymerization of component (III-2). The ethylene-based resin (III-2) had an HLMFR of 0.08 g / 10 min and an [η] of 7.5 dl / g.

[0063] Manufacturing of component (A-2) In a 10-liter autoclave, 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 1 were added, and the temperature was raised to 60°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 2 hours. During the polymerization, 200 g of ethylene was consumed in terms of polyethylene, and the [η] of component (A-2) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 22 dl / g.

[0064] Manufacture of component (B-2) and ethylene resin (B-2) After polymerizing component (a-2), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.50MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 8 hours to polymerize component (b-2), thereby producing ethylene-based resin (c-2), which is an ethylene homopolymer. During the polymerization, 800g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-2) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0065] Production Example 3 As described below, an ethylene resin (III-3), which is a bimodal polyethylene, was produced by two-stage polymerization in which the polymerization of component (III-3) was successively carried out after the polymerization of component (III-3). The ethylene polymer (III-3) had an HLMFR of 3.1 g / 10 min and an [η] of 4.1 dl / g.

[0066] Manufacturing of component (A-3) 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 2 were added to a 10-liter autoclave, and the temperature was raised to 70°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 1 hour. During the polymerization, 200 g of ethylene was consumed in terms of polyethylene, and the [η] of component (A-3) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 10 dl / g.

[0067] Manufacture of component (B-3) and ethylene resin (B-3) After polymerizing component (a-3), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.87MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 4 hours to polymerize component (b-3), thereby producing ethylene-based resin (c-3), which is an ethylene homopolymer. During the polymerization, 800g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-3) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0068] Production Example 4 As described below, a bimodal polyethylene ethylene resin (III-4) was produced by two-stage polymerization in which the polymerization of component (III-4) was successively carried out after the polymerization of component (III-4). The ethylene resin (III-4) had an HLMFR of 7.2 g / 10 min and an [η] of 3.2 dl / g.

[0069] Manufacturing of component (A-4) In a 10-liter autoclave, 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 2 were added, and the temperature was raised to 70°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 0.5 hours. 100 g of ethylene was consumed during the polymerization in terms of polyethylene, and the [η] of component (A-4) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 10 dl / g.

[0070] Manufacture of component (B-4) and ethylene resin (B-4) After polymerization of component (a-4), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.87MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 4.5 hours to polymerize component (b-4), thereby producing ethylene-based resin (c-4), which is an ethylene homopolymer. During the polymerization, 900g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-4) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0071] Production Example 5 As described below, a bimodal polyethylene ethylene resin (III-5) was produced by two-stage polymerization in which the polymerization of component (III-5) was successively carried out after the polymerization of component (III-5). The ethylene resin (III-5) had an HLMFR of 0.23 g / 10 min and an [η] of 6.6 dl / g.

[0072] Manufacturing of component (A-5) In a 10-liter autoclave, 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 2 were added, and the temperature was raised to 70°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 2.5 hours. During the polymerization, 500 g of ethylene was consumed in terms of polyethylene, and the [η] of component (A-5) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 10 dl / g.

[0073] Manufacture of components (Ro-5) and ethylene-based resins (Ha-5) After polymerization of component (a-5), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.87MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 2.5 hours to polymerize component (b-5), thereby producing ethylene-based resin (c-5), which is an ethylene homopolymer. During the polymerization, 500g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-5) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0074] Production Example 6 In a 10-liter autoclave, 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (corresponding to 310 mg of solid content) of the suspension of the catalyst for production obtained in Preparation Example 3 were added, and the temperature was raised to 85°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.90 MPa, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 100 ppm, and slurry polymerization was carried out for 1.5 hours to produce polyethylene, an ethylene homopolymer. The polyethylene had MFR=0.68 g / 10 min, HLMFR=10 g / 10 min, and [η]=2.4 dl / g.

[0075] [Table 1]

[0076] Example 1 The ethylene-based resin (Ha-1) obtained in Production Example 1 was dry-blended with an antioxidant (manufactured by BASF, product name: Irganox B225), and then a filamentous material was extruded from a single-hole nozzle having an orifice diameter of 0.6 mm at 280°C and a screw rotation speed of 15 rpm using a single-screw extruder (manufactured by Toyo Seiki, product name: Labo Plastomill), and cooled by air, and then wound up to obtain an undrawn yarn.

[0077] The resulting undrawn yarn was drawn 6 times between two driven rolls while being heated at 120° C., to obtain a polyethylene fiber as a wound drawn yarn.

[0078] The resulting polyethylene fiber had a fiber diameter of 143 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 5.8 GPa and 332 MPa, respectively.

[0079] Example 2 Polyethylene fibers were obtained in the same manner as in Example 1, except that the ethylene resin (III-2) obtained in Production Example 2 was used.

[0080] The resulting polyethylene fiber had a fiber diameter of 151 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 6.0 GPa and 354 MPa, respectively.

[0081] Example 3 The ethylene resin (III-1) obtained in Production Example 1 and decalin were mixed in a weight ratio of 15:85, and an antioxidant (manufactured by BASF, (product name) Irganox B225) was added to obtain a slurry solution.

[0082] The obtained slurry liquid was melted at 200°C with a screw rotation speed of 15 rpm using a twin-screw extruder (Toyo Seiki Co., Ltd., product name: Labo Plastomill) and a filamentous material was extruded from a single-hole nozzle with an orifice diameter of 0.6 mm. The filamentous material was collected and cooled in a water-cooled bath to obtain an undrawn yarn (gel yarn).

[0083] The resulting undrawn yarn was dried at 110° C., and then drawn 4 times between two driven rolls while being heated at 100° C. to obtain a polyethylene fiber that was a wound drawn yarn.

[0084] The resulting polyethylene fiber had a fiber diameter of 122 μm, and a tensile test revealed that the tensile modulus, tensile strength and tensile breaking stress were 5.3 GPa and 301 MPa, respectively.

[0085] Example 4 500 g of the ethylene-based resin (H-1) obtained in Production Example 1, polyethylene (manufactured by Tosoh Corporation, (product name) Nipolon Hard 5110 (MFR = 0.9 g / 10 min, density = 961 kg / m 3 500g of NH5110 (hereinafter sometimes referred to as NH5110) and 2g of an antioxidant (BASF, (trade name) Irganox B225) were dry blended, and then melt-kneaded at 220°C, 30 rpm, and a discharge rate of 0.8 kg / h using a twin-screw extruder (Toyo Seiki Seisakusho, (trade name) Labo Plastomill Parallel Twin-screw Extruder 2D25S) to obtain composition (E-1). The MFR of composition (E-1) was 0.11 g / 10 min.

[0086] The obtained composition (E-1) was extruded into a filamentous material from a single-hole nozzle having an orifice diameter of 0.6 mm at 280°C and a screw rotation speed of 15 rpm using a single-screw extruder (Toyo Seiki Co., Ltd., product name: Labo Plastomill), and the extruded material was cooled by air and then wound up to obtain an undrawn filament.

[0087] The resulting undrawn yarn was drawn 10 times between two driven rolls while being heated at 120° C., to obtain a polyethylene fiber that was a wound drawn yarn.

[0088] The resulting polyethylene fiber had a fiber diameter of 103 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 7.2 GPa and 428 MPa, respectively.

[0089] Example 5 A polyethylene fiber was obtained in the same manner as in Example 4, except that 500 g of the ethylene resin (III-2) obtained in Production Example 2 was used to prepare a composition (III-2), which was then stretched 11 times between two driving rolls while being heated at 120°C.

[0090] The resulting polyethylene fiber had a fiber diameter of 126 μm, and a tensile test revealed that the tensile modulus, tensile strength and tensile breaking stress were 8.2 GPa and 434 MPa, respectively.

[0091] Example 6 A composition (E-3) was prepared using 100 g of the ethylene resin (E-2) obtained in Production Example 2 and 900 g of polyethylene (NH5110). A polyethylene fiber was obtained in the same manner as in Example 4, except that the composition (E-3) was stretched 8 times between two driving rolls while being heated at 120°C.

[0092] The resulting polyethylene fiber had a fiber diameter of 94 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 5.3 GPa and 323 MPa, respectively.

[0093] Example 7 A polyethylene fiber was obtained in the same manner as in Example 4, except that 500 g of the ethylene resin (III-3) obtained in Production Example 3 was used to prepare a composition (III-4), and the composition was stretched 9 times between two driving rolls while being heated at 120°C.

[0094] The resulting polyethylene fiber had a fiber diameter of 111 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 6.0 GPa and 369 MPa, respectively.

[0095] Example 8 A composition (E-5) was prepared using 40 g of the ethylene resin (E-4) obtained in Production Example 4 and 960 g of polyethylene (NH5110). A polyethylene fiber was obtained in the same manner as in Example 4, except that the composition (E-5) was stretched 5 times between two driving rolls while being heated at 120°C.

[0096] The resulting polyethylene fiber had a fiber diameter of 71 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 4.1 GPa and 314 MPa, respectively.

[0097] Example 9 500 g of the ethylene-based resin (H-2) obtained in Production Example 2, polyethylene (manufactured by Tosoh Corporation, (product name) Nipolon Hard 06S81A (MFR = 1.0 g / 10 min, density = 952 kg / m 3A composition (E-6) was prepared by using 500 g of NH06S81A (hereinafter sometimes referred to as NH06S81A), and the composition was stretched 11 times between two driven rolls while heating at 125°C, to obtain a polyethylene fiber in the same manner as in Example 4.

[0098] The resulting polyethylene fiber had a fiber diameter of 137 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 4.4 GPa and 329 MPa, respectively.

[0099] Example 10 A composition (E-7) was prepared using 500 g of the ethylene resin (E-5) obtained in Production Example 5 and 500 g of the polyethylene obtained in Production Example 6, and polyethylene fibers were obtained in the same manner as in Example 4, except that the composition (E-7) was stretched to 11 times its original size between two driving rolls while being heated at 125°C.

[0100] The resulting polyethylene fiber had a fiber diameter of 146 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 4.5 GPa and 363 MPa, respectively.

[0101] [Table 2]

[0102] [Table 3]

[0103] Comparative Example 1 Fibers were obtained in the same manner as in Example 4, except that 1000 g of polyethylene (NH5110) and 2 g of an antioxidant (BASF, (trade name) Irganox B225) were used and stretched 4 times between two driven rolls while being heated at 120°C.

[0104] The obtained fiber had a fiber diameter of 117 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 4.0 GPa and 284 MPa, respectively.

[0105] Comparative Example 2 An attempt was made to produce fibers in the same manner as in Example 4, except that 40 g of ultra-high molecular weight polyethylene (product name Million 030S, manufactured by Mitsui Chemicals, Inc.) and 960 g of polyethylene (NH5110) were used and stretched 3 times between two driven rolls while heating at 120°C. However, it was difficult to extrude a uniform filament from the extruder, and breakage occurred during stretching, making it impossible to produce fibers.

[0106] Comparative Example 3 Fibers were obtained in the same manner as in Example 4, except that 1000 g of polyethylene (NH06S81A) was stretched 3 times between two driven rolls while being heated at 125°C.

[0107] The obtained fiber had a fiber diameter of 114 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 2.6 GPa and 239 MPa, respectively.

[0108] Comparative Example 4 Fibers were obtained in the same manner as in Example 4, except that 1000 g of the polyethylene obtained in Production Example 6 was stretched 4 times between two driven rolls while being heated at 125°C.

[0109] The obtained fiber had a fiber diameter of 143 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 3.2 GPa and 288 MPa, respectively.

[0110] Comparative Example 5 Polyethylene (manufactured by Tosoh Corporation, product name Nipolon Hard 8D01A (MFR = 0.05 g / 10 min, density = 957 kg / m 3 A fiber was obtained in the same manner as in Example 4, except that 1000 g of NH8D01A (hereinafter sometimes referred to as NH8D01A) was used and stretched 11 times between two driven rolls while being heated at 120°C.

[0111] The obtained fiber had a fiber diameter of 111 μm, and a tensile test revealed that the tensile modulus and tensile breaking stress were 5.4 GPa and 286 MPa, respectively.

[0112] Comparative Example 6 500 g of the ethylene resin (H-1) obtained in Production Example 1 and polyethylene (manufactured by Tosoh Corporation, (product name) Nipolon Hard 2000 (MFR = 15 g / 10 min, density = 960 kg / m 3 An attempt was made to produce fibers in the same manner as in Example 4, except that 500 g of NH2000 (hereinafter sometimes referred to as NH2000) was used and stretched 3 times between two driven rolls while heated at 120°C. However, it was difficult to extrude a uniform filament from the extruder, and breakage occurred during stretching, making it impossible to produce fibers.

[0113] Comparative Example 7 500 g of the ethylene resin (H-1) obtained in Production Example 1 and polyethylene (manufactured by Tosoh Corporation, (trade name) Petrothene 176 (MFR = 1.0 g / 10 min, density = 924 kg / m 3 An attempt was made to produce fibers in the same manner as in Example 4, except that 500 g of P2000 (hereinafter sometimes referred to as P2000) was used and stretched 3 times between two driven rolls while heated at 120°C. However, it was difficult to extrude a uniform filament from the extruder, and breakage occurred during stretching, making it impossible to produce fibers.

[0114] [Table 4] [Industrial Applicability]

[0115] The polyethylene fiber of the present invention is excellent in processability and in mechanical strength of the molded product, and can be used in various applications where thinning and long life are required.

Claims

1. (1) A polyethylene fiber, comprising an ethylene-based resin having a melt flow rate (HLMFR) of 0.01 to 100 g / 10 min at a temperature of 190° C. and a load of 21.6 kg, and a bimodal elution curve as measured by gel permeation chromatography in accordance with JIS 6922-2:1997.

2. Furthermore, the melt flow rate (MFR) is 0.01 to 10 g / 10 min at a temperature of 190° C. and a load of 2.16 kg according to JIS 6922-2:1997, and the density measured according to JIS K6922-1 (1997) is 930 to 980 kg / m 3 2. The polyethylene fiber according to claim 1, characterized in that it is made of a composition comprising a polyethylene of

3. 3. The polyethylene fiber according to claim 1, wherein the ethylene resin satisfies the following characteristic (2): (2) The elution curve measured by gel permeation chromatography has two peaks, and when the elution curve is expressed as a differential molecular weight distribution (x-axis: Log [M], y-axis: differential distribution value) and the peak is divided into two normal distributions according to the following formula (i), the following (2-1) to (2-3) are satisfied: f(x)=a×(1 / (2π(σ 2 )) (1/2) ) x 2 ) / (2(s 2 ))) formula (i) (Here, a is the peak intensity, σ is the standard deviation, x is the variable, and μ is the average.) (2-1): The weight average molecular weight, calculated as linear polyethylene, based on the peak on the high molecular weight side is 900,000 to 5,000,000, and the molecular weight distribution, expressed as weight average molecular weight / number average molecular weight, is 2.0 to 5.

0. (2-2): The weight average molecular weight, calculated based on the peak on the low molecular weight side, is 10,000 to 500,000 in terms of linear polyethylene, and the molecular weight distribution is 2.0 to 5.

0. (2-3): The weight ratio of the high molecular weight peak to the weight ratio of the low molecular weight peak is greater than 5 / 95 and smaller than 80 / 20.

4. 3. The polyethylene fiber according to claim 1, wherein the ethylene resin also satisfies the following characteristic (3): (3) The molecular weight distribution, calculated as standard polyethylene, measured by gel permeation chromatography is 4.0 or more and less than 50.

5. 3. The polyethylene fiber according to claim 1 or 2, characterized in that the ethylene-based resin also satisfies the following characteristic (4). (4): The crystal melting peak (Tm) in the first scan measured using a differential scanning calorimeter by heating from 0° C. to 230° C. at a heating rate of 10° C. / min (1st scan) is single-peaked.

6. 3. The polyethylene fiber according to claim 1, wherein the fiber has a tensile modulus of elasticity of 4.0 GPa or more and a tensile breaking strength of 300 MPa or more, measured at 23°C.

7. 3. The polyethylene fiber according to claim 1, wherein the ethylene-based resin is an ethylene homopolymer.

Citation Information

Patent Citations

  • JP1973068853A

  • Thermal transfer type sheet

    JP1989005888A

  • Modifier for polyethylene resin, manufacturing method of polyethylene resin composition using the same and manufacturing method of molded body

    JP2017179304A

  • Polyethylene fibers

    JP2021070902A