Aqueous lithium and silicon-containing solution, production method thereof, and production method of active material for lithium secondary battery having coating layer containing lithium orthosilicate

An aqueous solution with controlled lithium and silicon content forms a uniform lithium orthosilicate coating on positive electrode active materials, addressing coating issues in lithium ion batteries and enhancing battery performance by improving Li ion conductivity and reducing resistance.

JP2024166591APending Publication Date: 2024-11-29DOWA HOLDINGS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023082780
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing methods for coating positive electrode active materials in lithium ion secondary batteries with lithium silicate face issues such as limited versatility, low productivity, non-uniform coating, high manufacturing costs, and the formation of high-resistance regions, leading to deteriorated battery performance.

Method used

An aqueous solution containing lithium and silicon with a specific molar ratio and controlled absorbance is used to coat the positive electrode active material, forming a lithium orthosilicate layer, which is then heat-treated to achieve a uniform and conductive coating.

Benefits of technology

The method enhances Li ion conductivity and improves the performance of all-solid-state lithium ion secondary batteries by ensuring a uniform and effective coating layer of lithium orthosilicate, reducing interfacial resistance and maintaining battery capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166591000001_ABST
    Figure 2024166591000001_ABST
Patent Text Reader

Abstract

To provide an aqueous lithium and silicon-containing solution having a low absorbance, for coating a surface of a positive pole active material particle of a lithium ion secondary battery with Li4SiO4 (lithium orthosilicate) having good Li ionic conductivity; a production method thereof; and a production method of a positive pole active material for lithium secondary battery having a coating layer containing lithium orthosilicate by using the aqueous solution.SOLUTION: An aqueous lithium and silicon-containing solution includes 0.1 mass% or more and 3.0 mass% or less of lithium and 0.1 mass% or more and 3.0 mass% or less of silicon. In the aqueous solution, the molar ratio Li / Si of lithium to silicon is 3.70 or more and 5.20 or less and the absorbance at a wavelength of 660 nm is 0.10 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous solution containing lithium and silicon for coating the surfaces of positive electrode active material particles of a lithium ion secondary battery with lithium orthosilicate as a solid electrolyte, and a production method thereof, as well as a production method for an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate. [Background technology]

[0002] The positive electrode active material of lithium-ion secondary batteries has generally been composed of a composite oxide of lithium and a transition metal. Among them, lithium cobalt oxide (LiCoO2), a composite oxide containing Co, is widely used. Recently, lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), or ternary oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2) and their combinations are also on the rise.

[0003] The electrolyte for lithium ion secondary batteries is mainly made by dissolving lithium salts such as electrolyte LiPF6 and LiBF4 in a mixed solvent of cyclic carbonate esters such as PC (propylene carbonate) and EC (ethylene carbonate) and chain esters such as DMC (dimethyl carbonate), EMC (ethyl methyl carbonate), and DEC (diethyl carbonate). Such organic solvents are weak in an oxidizing atmosphere, and are prone to oxidative decomposition reactions when they come into contact with transition metals such as Co, Ni, and Mn, especially on the surface of the positive electrode. Possible causes of this include the high potential of the positive electrode surface and the catalytic action of transition metals in a highly oxidized state. Therefore, it is effective to prevent contact between the electrolyte and the transition metals (e.g., one or more of Co, Ni, and Mn) that constitute the positive electrode active material as much as possible in order to maintain the performance of the electrolyte.

[0004] As a method for fundamentally solving the problems associated with the organic solvent-based electrolyte, an all-solid-state lithium ion secondary battery has been proposed in which the electrolyte is replaced with a non-flammable solid electrolyte. In general, the electrode reaction of a battery occurs at the interface between the electrode active material and the electrolyte. When a liquid electrolyte is used, the electrolyte penetrates the surface of the electrode active material present on the electrode, forming a reaction interface for charge transfer. In the case of an all-solid-state battery, a solid electrolyte having ion conductivity plays the role of the electrolyte, but since the solid electrolyte itself does not have the fluidity of a liquid, it is necessary to mix the powder that will become the electrode active material with the solid electrolyte or to coat the powder that will become the electrode active material with the solid electrolyte before constructing the secondary battery.

[0005] However, in the case of all-solid-state lithium-ion secondary batteries, there is a problem that the resistance (hereinafter, sometimes referred to as "interface resistance") that occurs when lithium ions move across the interface between the positive electrode active material and the solid electrolyte increases, and the performance of the all-solid-state lithium-ion secondary battery, such as the battery capacity, is likely to decrease. The increase in the interface resistance is believed to be caused by the reaction between the positive electrode active material and the solid electrolyte, resulting in the formation of high-resistance sites on the surface of the positive electrode active material, and it is known that the interface resistance can be reduced by coating the surface of lithium cobalt oxide, which is the positive electrode active material, with lithium silicate.

[0006] For example, Non-Patent Document 1 discloses a thin-film lithium battery in which Li4SiO4 (lithium orthosilicate) or Li2SiO3 (lithium metasilicate) is deposited as a solid electrolyte on a LiCoO2 positive electrode deposited on a metal substrate by using a pulsed laser deposition method. Non-Patent Document 1 also discloses that the Li ion conductivity of Li4SiO4 is one order of magnitude higher than that of Li2SiO3. As an example of a technique for coating the surface of a positive electrode active material with lithium silicate as a solid electrolyte using a highly productive wet method, Patent Document 1 discloses a powder of a positive electrode active material whose surface is coated with vitreous lithium silicate.

[0007] Non-Patent Document 2 discloses a positive electrode active material powder coated with Li4SiO4. The technology disclosed in Non-Patent Document 2 involves forming a SiO2 coating on a positive electrode active material powder using an aqueous solution of sodium metasilicate (Na2SiO3), and then reacting the coating layer with lithium acetate powder in the solid phase to form Li4SiO4. Non-Patent Document 3 discloses a technique for coating the surface of a positive electrode active material with Li4SiO4 by a wet method. Patent Document 2 discloses a technique for obtaining lithium orthosilicate by mixing an aqueous solution of lithium metasilicate and a lithium compound as a precursor solution of Li4SiO4 without using TEOS to prepare a reaction precursor. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 2014-513392 [Patent Document 2] Patent Publication No. 2021-075406 [Non-patent literature]

[0009] [Non-Patent Document 1] Atsuo Nakagawa et al., Abstracts of the 35th Solid State Ionics Symposium, p.82, 2009 [Non-Patent Document 2] S. Yang et al., Front. Energy, 2017, 11(3) p.374-382 [Non-Patent Document 3] Y. Xu et al., J. Materiomics, 2 (2016) p.265-272 Summary of the Invention [Problem to be solved by the invention]

[0010] The pulsed laser deposition method of Non-Patent Document 1 has limitations on the materials to be treated, and has problems such as lack of versatility and poor productivity. 11 (lithium polysilicate) or Li2SiO3, and these lithium silicates have a problem of lower Li-ion conductivity compared to Li4SiO4, and the output characteristics of the battery during operation are reduced. In Non-Patent Document 2, the coating is likely to become non-uniform because a solid-phase reaction is ultimately used, and high-resistance parts are formed from parts where Li4SiO4 formation is insufficient, resulting in a decrease in battery characteristics. In the technology disclosed in Non-Patent Document 3, the starting materials for the coating solution are alcohol solutions using lithium acetate and tetraethoxysilane (TEOS), which increases the manufacturing cost. In addition, since TEOS absorbs moisture from the air and is easily hydrolyzed, there is a problem that it is difficult to handle as a coating solution, and therefore a coating solution that does not use TEOS has been desired. In the case of the technology disclosed in Patent Document 2, it was found that when the molar ratio of lithium to silicon approaches that of Li4SiO4 and the molar ratio of lithium to silicon Li / Si becomes 3.7 or more, fine particles are generated in the aqueous solution. When such an aqueous solution is used to form a coating on the surface of an electrode active material, the coating tends to become non-uniform, and high-resistance areas are formed where the Li4SiO4 formation is insufficient, resulting in a decrease in battery characteristics.

[0011] In view of the above problems, the present invention aims to provide an aqueous solution containing lithium and silicon and having low absorbance, for coating the surfaces of positive electrode active material particles of a lithium ion secondary battery with Li4SiO4 (lithium orthosilicate) having good Li ion conductivity, a method for producing the aqueous solution, and a method for producing a positive electrode active material for a lithium secondary battery having a coating layer containing lithium orthosilicate using the aqueous solution. [Means for solving the problem]

[0012] [1] In order to achieve the above object, the present invention provides an aqueous solution containing lithium and silicon, the aqueous solution containing lithium at 0.1% by mass or more and 3.0% by mass or less, silicon at 0.1% by mass or more and 3.0% by mass or less, a molar ratio of lithium to silicon Li / Si of 3.70 or more and 5.20 or less, and an absorbance at a wavelength of 660 nm of 0.10 or less. [2] The aqueous solution containing lithium and silicon according to the above item [1] is preferably dried and then heat-treated in an air atmosphere at 750°C for 5 hours to obtain a sintered powder that is mainly composed of lithium orthosilicate (Li4SiO4) crystals. [3] The aqueous solution containing lithium and silicon according to the above item [1] preferably has a lithium content of 0.5% by mass or more and 2.0% by mass or less. [4] The aqueous solution containing lithium and silicon according to the above item [1] preferably has a silicon content of 0.5% by mass or more and 2.0% by mass or less. [5] The aqueous solution containing lithium and silicon according to the above item [1] preferably has a molar ratio of lithium to silicon in the aqueous solution, Li / Si, of 3.70 or more and 5.00 or less. [6] The aqueous solution containing lithium and silicon according to the above item [1] preferably has an absorbance of 0.07 or less at a wavelength of 660 nm. [7] The present invention also provides a method for producing an aqueous solution containing lithium and silicon according to the above item [1], comprising the steps of: mixing an aqueous solution containing a silicon compound with an aqueous solution containing a lithium compound to obtain an aqueous solution having a lithium to silicon molar ratio Li / Si of 3.70 or more and 5.20 or less; and maintaining the aqueous solution containing lithium and silicon at 45° C. or more and 60° C. or less. [8] The present invention further provides a method for producing an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate, the method comprising the steps of: coating a surface of a positive electrode active material for a lithium secondary battery with the aqueous solution containing lithium and silicon obtained by the production method described in the above item [7]; drying the positive electrode active material for a lithium secondary battery coated with the aqueous solution containing lithium and silicon to form a coating layer containing lithium and silicon; and a heat treatment step of subjecting the positive electrode active material for a lithium secondary battery having a coating layer containing lithium and silicon to a heat treatment. [9] The present invention further provides a method for producing an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate, the method comprising the steps of: coating a surface of a positive electrode active material for a lithium secondary battery with the aqueous solution containing lithium and silicon described in the above item [1]; drying the positive electrode active material for a lithium secondary battery coated with the aqueous solution containing lithium and silicon to form a coating layer containing lithium and silicon; and a heat treatment step of subjecting the positive electrode active material for a lithium secondary battery having a coating layer containing lithium and silicon to a heat treatment. Effect of the Invention

[0013] When the aqueous solution containing lithium and silicon obtained by the manufacturing method of the present invention is used, it becomes possible to coat the surface of the electrode active material with a layer mainly composed of Li4SiO4 (lithium orthosilicate) crystals even if the molar ratio of lithium to silicon in the aqueous solution is Li / Si 3.70 or more. Therefore, the present invention can contribute to improving the performance of all-solid-state lithium ion secondary batteries. [Brief description of the drawings]

[0014] [Figure 1] 1 shows an X-ray diffraction pattern of a powder obtained by drying and calcining the aqueous solution obtained in Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] [Cathode active material] Examples of the cathode active material coated with the aqueous solution containing lithium and silicon of the present invention include the following. The cathode active material is composed of a composite oxide of Li and transition metal M, and is a material conventionally used in lithium ion secondary batteries, such as lithium cobalt oxide (Li 1+X CoO2, -0.1 ≦ X ≦ 0.3), Li 1+X NiO2, Li 1+X Mn2O4, Li 1+X Ni 1 / 2 Mn 1 / 2 O2, Li 1+X Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (all -0.1 ≦ X ≦ 0.3), Li 1+X [Ni Y Li 1 / 3-2Y / 3 Mn 2 / 3-Y / 3 O2 (0 ≦ X ≦ 1, 0 < Y < 1 / 2), etc., lithium transition metal oxides in which part of these Li or transition metal elements are substituted with Al or other elements, Li 1+X FePO4, Li 1+X MnPO4 (both -0.1 ≦ X ≦ 0.3), etc., phosphates having an olivine structure, and lithium manganate (LiMnO4) as a spinel-type compound and those in which part of Mn is substituted with Al, Ti, Cr, Fe, Zr, Y, W, Ta, Nb, Ni, Co, Fe, etc. (LiAl 0.1 Mn 0.9 O4, LiNi 0.5 Mn 1.5 O4, etc.).

[0016] [Li source] In the aqueous solution containing lithium and silicon of the present invention, water-soluble lithium hydroxide (LiOH), lithium chloride (LiCl), lithium sulfate, lithium nitrate, etc. can be used as the Li source. As the Li source, it is preferable to use LiOH which is difficult to leave impurities when finally forming a coating layer containing lithium orthosilicate on the surface of the cathode active material. LiOH may be anhydrous or hydrated. The LiOH added to the aqueous solution is Li + and OH -and exhibits strong alkalinity. Strong alkalinity is preferred because the aqueous solution is stable and the generation of fine particles in the aqueous solution is suppressed. In this specification, an aqueous solution in which an additional Li source such as LiOH is dissolved is referred to as solution A. In the present invention, an aqueous solution containing lithium and silicon is prepared by adding solution A containing additional Li to solution B described below, and the lithium concentration in the aqueous solution after preparation is 0.1 mass % or more and 3.0 mass % or less in terms of Li. When the lithium concentration is 0.1% by mass or more, the concentration of the coating layer components in the aqueous solution becomes large, and the coating becomes more uniform in the coating layer forming process. When the Li concentration is 3.0% by mass or less, the generation of a large amount of fine particles in the aqueous solution is suppressed, and the coating becomes more uniform in the coating layer forming process. The lithium concentration is preferably 0.5% by mass or more and 2.0% by mass or less.

[0017] [Si source] In the aqueous solution containing lithium and silicon of the present invention, the starting material of Si is not particularly limited as long as it is soluble in water, but it is preferable to use an aqueous solution containing lithium and silicon that also serves as a Li source. For example, Li2Si5O 11 Aqueous solution, Li2Si 14 O 29 Aqueous solution, Li2Si 18 O 37 It is preferable to use an aqueous solution of lithium polysilicate in which the molar ratio of lithium to silicon (Li / Si) in the aqueous solution is 0.1 or more. Although it is possible to solubilize Si on the acidic side by using fluoride ions or the like, this is not preferable because the coated positive electrode active material dissolves on the acidic side. In this specification, Li2Si5O 11 The aqueous solution in which the above is dissolved is referred to as Solution B. In the present invention, the above-mentioned Solution A containing Li is added to Solution B to prepare an aqueous solution containing lithium and silicon, and the silicon concentration in the aqueous solution after the preparation is 0.1% by mass or more and 3.0% by mass or less in terms of Si. When the silicon concentration is 0.1% by mass or more, the concentration of the coating layer components in the aqueous solution becomes large, and the coating becomes more uniform in the coating layer forming process. When the silicon concentration is 3.0% by mass or less, the generation of a large amount of fine particles in the aqueous solution is suppressed, and the coating becomes more uniform in the coating layer forming process. The silicon concentration is preferably 0.5% by mass or more and 2.0% by mass or less.

[0018] In the aqueous solution containing lithium and silicon of the present invention, the molar ratio Li / Si of lithium to silicon in the aqueous solution is 3.70 or more and 5.20 or less. By setting the Li / Si value to 3.70 or more and 5.20 or less, Li4SiO4 with high Li ion conductivity is easily obtained. Furthermore, if the Li / Si molar ratio exceeds 5.20, fine particles are likely to be generated in an amount exceeding the soluble concentration. The value of the lithium to silicon molar ratio Li / Si is preferably 3.70 or more and 5.00 or less. The aqueous solution containing lithium and silicon may contain an organic solvent such as alcohol within a range that does not impair the effect.

[0019] [Absorbance] The absorbance value of the aqueous solution containing lithium and silicon according to the present invention at a wavelength of 660 nm is preferably 0.1 or less. Here, the absorbance of the aqueous solution at a wavelength of 660 nm is an index showing the intensity of scattered light by fine particles present in the aqueous solution, and a high absorbance at that wavelength means a high concentration of fine particles present in the aqueous solution. When the aqueous solution with a high concentration of fine particles is applied to the electrode active material, the fine particles adhere to the surface of the electrode active material, making the coating layer uneven, and the thickness of the coating layer is likely to become uneven. If the thickness of the coating layer becomes uneven, a thin film part with an insufficient thickness of the coating layer or even an uncoated part may occur, resulting in a decrease in the coverage rate. According to the study by the present inventors, if the absorbance value of the aqueous solution at a wavelength of 660 nm is 0.10 or less, the amount of fine particles in the aqueous solution is sufficiently small, and adverse effects on the uniformity of the coating layer thickness and the coverage rate are suppressed. The absorbance value is preferably 0.07 or less. The absorbance value was measured using an ultraviolet-visible spectrophotometer at a temperature of 25°C and the absorbance at a wavelength of 660 nm. In this case, the lower limit of absorbance is 0.000. However, the detection limit of the UV-visible spectrophotometer used for the absorbance measurement is 0.001.

[0020] [Carbon content] If the aqueous solution containing lithium and silicon of the present invention contains carbon, it may remain as an impurity when a coating layer containing lithium orthosilicate is finally formed on the surface of the positive electrode active material, which may cause a decrease in battery performance. Therefore, it is preferable that the aqueous solution containing lithium and silicon of the present invention contains a small amount of organic matter that does not volatilize even when fired. The carbon content in the aqueous solution can be 5 mg / L or less in terms of total organic carbon (TOC). If a reagent containing 1000 ppm or less of unavoidable impurities excluding Li, Si, and water is used as the Si source and Li source of the aqueous solution containing lithium and silicon of the present invention, the TOC can be 5 mg / L or less. The carbon content in the aqueous solution can be 3 mg / L or less, more preferably 2 mg / L or less.

[0021] [Manufacturing method] In the method for producing an aqueous solution containing lithium and silicon according to the present invention, as described above, a mixed solution containing lithium and silicon is prepared by adding a solution A containing Li to a solution B containing Si. This mixed solution generates fine particles and becomes cloudy. 11 If an aqueous solution of lithium polysilicate (LiSi) is used as solution A and an aqueous solution of lithium hydroxide (LiOH) is used as solution B, the mixed solution will essentially contain only lithium ions, silicate ions, and unavoidable impurities. Note that solution B may also be added to solution A. Subsequently, the temperature of the aqueous solution is maintained at 45° C. or higher and 60° C. or lower while stirring the mixture using a known mechanical stirring means, whereby the fine particles are dissolved to obtain an aqueous solution containing lithium and silicon.

[0022] By setting the holding temperature for dissolving the fine particles at 45° C. or higher and 60° C. or lower, the fine particles are dissolved, and the absorbance value of the resulting aqueous solution at a wavelength of 660 nm can be made to be 0.10 or lower. It is preferable to maintain the temperature of the aqueous solution at 45°C or higher and 60°C or lower while stirring the mixture using a known mechanical stirring means, since this can prevent a local temperature drop due to the addition of Liquid A and shorten the time required for dissolving the fine particles.

[0023] In the present invention, the retention time for dissolving the fine particles is not particularly specified, but from the viewpoint of economy, it is preferable to set it to 3 hours or less. The retention time can be, for example, 15 minutes or more. The time point at which the dissolution of the fine particles is completed is the time point at which the absorbance of the aqueous solution obtained in the above step becomes 0.10 or less.

[0024] In the method for producing an aqueous solution containing lithium and silicon according to the present invention, a step of filtering the aqueous solution containing lithium and silicon using a known filtering means may be provided after the step of dissolving the fine particles. The mixed solution may be kept at 45°C or more and 60°C or less by heating the solution obtained by mixing the aqueous solution A containing lithium and the aqueous solution B containing silicon at less than 45°C and keeping it at 45°C or more and 60°C or less. Alternatively, the aqueous solution A containing lithium and the aqueous solution B containing silicon may be mixed at a liquid temperature of 45°C or more and 60°C or less, and the temperature may be adjusted to keep it at 45°C or more and 60°C or less. The molar ratio Li / Si of lithium to silicon in the aqueous solution containing lithium and silicon obtained by dissolving the fine particles is set to 3.70 to 5.20. The silicon concentration in the aqueous solution after the adjustment is preferably 0.1% by mass to 3.0% by mass in terms of Si, and the lithium concentration is preferably 0.1% by mass to 3.0% by mass in terms of Li.

[0025] In the method for producing an aqueous solution containing lithium and silicon according to the present invention, a step of filtering the obtained aqueous solution containing lithium and silicon using a known filtering means may be provided after the step of dissolving the fine particles.

[0026] The aqueous solution containing lithium and silicon of the present invention is dried and then heat-treated in an air atmosphere at 750°C for 5 hours to obtain a sintered powder, which is mainly composed of lithium orthosilicate (Li4SiO4) crystals, i.e., has the crystals as the main phase. The term "having Li4SiO4 crystals as the main phase" means that the ion conductor has a diffraction peak intensity ratio I1 / I0 of I1 / I0<1.0, where I0 is the highest peak intensity among the diffraction peaks identified as Li4SiO4 crystals in the X-ray diffraction pattern obtained by X-ray diffraction measurement of the sintered powder, and I1 is the highest peak intensity among the diffraction peaks of the different phases (peaks that could not be identified as the Li4SiO4 crystal phase). Here, if no different phase is detected, I1=0, and the above-mentioned relationship of I1 / I0<1.0 is satisfied. Although the presence of different phases is permitted within a range that does not impair the effects of the present invention, it is preferable that the amount of different phases is small. For example, I1 / I0≦0.50 is more preferable, and I1 / I0≦0.15 is even more preferable. For example, a spray drying method or the like is used as a method for drying the aqueous solution.

[0027] [Coating treatment] The following is an embodiment of the coating treatment for a positive electrode active material for a lithium ion secondary battery using the aqueous solution containing lithium and silicon according to the present invention. The positive electrode active material to be coated must have a specific surface area of ​​0.1 to 2 m 2 Since the specific surface area of ​​the positive electrode active material is inversely proportional to the particle size, the specific surface area of ​​the positive electrode active material is appropriately selected depending on the application of the lithium ion secondary battery. The thickness of the coating layer that coats the positive electrode active material is preferably 3 to 20 nm, and more preferably 5 to 15 nm. For the coating treatment, a known method such as a tumbling fluidized bed coating method or a high-velocity air current collision shear method can be used, and the positive electrode active material is brought into contact with the aqueous solution of the present invention, dried, and then heat-treated, to obtain a positive electrode active material having a coating layer containing lithium orthosilicate. EXAMPLES

[0028] [Measurement of lithium and silicon content] 15mL of pure water and 5mL of hydrochloric acid were added to a 0.1g sample of the solution, and then 2mL of hydrogen peroxide was added to dissolve lithium and silicon. The volume of the solution was measured using a measuring flask, and then diluted as necessary. The lithium and silicon concentrations in the diluted solution were measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES, Agilent Technologies CP-720) to calculate the lithium and silicon contents in the solution sample.

[0029] [Measurement of absorbance] The amount of insoluble fine particles in the aqueous solution was qualitatively evaluated by measuring the absorbance at a wavelength of 660 nm using an ultraviolet-visible spectrophotometer (UV-1800, manufactured by SHIMADZU CORPORATION). The absorbance was measured at 25°C using pure water (ion-exchanged water) as a reference sample in a quartz cell (10 mm x 10 mm x 45 mm). [X-ray diffraction measurement] The powder sample obtained by spray drying the aqueous solution was heat-treated at 750°C and then subjected to X-ray diffraction measurement under the following measurement conditions. Tube: Cu, tube voltage: 40 kV, tube current: 30 mA, divergence slit: 1.0°, scattering slit: 1.0°, receiving slit: 0.3 mm, scan speed: 2.0° / min, step width: 0.02. The peak search was performed using Shimadzu XRD-6100 software under the following conditions: Smoothing process: Automatic Background processing: Automatic Ka1-a2 ratio: 50 Peak search: Automatic

[0030] [Carbon content measurement] The amount of carbon in the aqueous solution was measured by the TC-IC method. The TC-IC method is a method in which the total carbon (TC) and inorganic carbon (IC) in a sample are measured separately, and the total organic carbon (TOC) is calculated from the difference. A total organic carbon meter (Shimadzu Corporation, TOC-LCHS) was used for the measurement. TC measurement: The sample is injected into a combustion tube (680°C) filled with an oxidation catalyst, and the carbon dioxide (CO2) produced by combustion or decomposition is detected in the analysis section. IC measurement: The sample is made acidic (pH 3 or less) and aerated to release CO2 from carbonates, etc., which is then detected in the analysis section.

[0031] [Example 1] 5.99 g of LiOH·H2O (lithium hydroxide monohydrate, Fujifilm Wako Pure Chemical Industries, Ltd.) and 59.94 g of ion-exchanged water were added to a 100 mL beaker and stirred at room temperature for 10 minutes to dissolve. This was used as solution A. 11 11.02 g of an aqueous solution (Sigma-Aldrich Corporation, concentration 20 mass%) and 34.04 g of ion-exchanged water were added and kept at 50°C with stirring, and this was designated as Liquid B. Liquid A was added to Liquid B at a rate of 5 g / min while stirring and kept at 50°C, and white fine particles were generated in the mixed solution after the addition. The mixed solution was then kept at 50°C and stirred for 120 minutes, at which point the fine particles dissolved to give a transparent aqueous solution.

[0032] The amounts of lithium and silicon contained in the resulting solution were measured by ICP-AES, and the absorbance of the resulting solution at a wavelength of 660 nm was also measured. The lithium and silicon contents were almost equal to the amounts charged as raw materials, and the Li / Si molar ratio was 4.70. The absorbance was 0.03, and the TOC was 1 mg / L.

[0033] The aqueous solution obtained in this example was spray-dried using a spray dryer (Tokyo Rikakikai Co., Ltd. SD-1000) to obtain a white dry powder. The conditions for spray drying were an inlet temperature of 180°C, an outlet temperature of 90°C, and a solution addition rate of 10g / min. The dried powder was heat-treated for 5 hours in an air atmosphere at 750°C and then crushed in a mortar to obtain a 750°C fired powder. When the 750°C fired powder was subjected to X-ray diffraction measurement, a diffraction peak derived from Li4SiO4 (lithium orthosilicate) crystals was observed. The diffraction peak intensity I0 derived from Li4SiO4 (lithium orthosilicate) crystals was the diffraction peak with the highest peak intensity in the obtained X-ray diffraction pattern. In addition, since no heterogeneous phase was detected, the diffraction peak intensity I1 with the highest peak intensity among the diffraction peaks of the heterogeneous phase (peaks that could not be identified as the Li4SiO4 crystal phase) was 0. Since the relationship I1 / I0<1.0 holds, it was found that the obtained sintered powder has lithium orthosilicate (Li4SiO4) crystals as the main phase. Therefore, the aqueous solution containing lithium and silicon obtained in this example is a precursor of lithium orthosilicate, and the aqueous solution is coated on a positive electrode active material, dried, and heat-treated at 750°C to obtain a positive electrode active material for lithium secondary batteries having a coating layer containing lithium orthosilicate.

[0034] The preparation conditions of the aqueous solution in this example are shown in Table 1, and the composition of the resulting aqueous solution and the results of X-ray diffraction measurement of the powder calcined at 750° C. are shown in Table 2.

[0035] [Examples 2 to 5] In Examples 2 and 3, the amounts of LiOH·H2O and ion-exchanged water used to obtain solution A and the amount of ion-exchanged water used to obtain solution B were changed to obtain transparent aqueous solutions in which fine particles were dissolved, with a different Li / Si molar ratio from that in Example 1. The preparation conditions for the aqueous solutions in these Examples are shown in Table 1, and the compositions of the aqueous solutions obtained and the results of X-ray diffraction measurements of the powders calcined at 750°C are shown in Table 2. In both cases, diffraction peaks derived from Li4SiO4 (lithium orthosilicate) crystals were observed in the X-ray diffraction measurements of the powders calcined at 750°C obtained from the aqueous solutions of Examples 2 and 3. The diffraction peak intensity I0 derived from the Li4SiO4 (lithium orthosilicate) crystals was the diffraction peak with the highest peak intensity in the obtained X-ray diffraction patterns. Therefore, when the diffraction peak intensity with the highest peak intensity among the diffraction peaks of Li4SiO4 crystal is I0 and the diffraction peak intensity with the highest peak intensity among the diffraction peaks of the different phase is I1, the diffraction peak intensity ratio I1 / I0 has a relationship of I1 / I0<1.0, so it was found that the obtained sintered powder has lithium orthosilicate (Li4SiO4) crystal as the main phase. In Example 2, a different phase was detected, and the diffraction peak intensity ratio was I1 / I0=0.09. In Example 3, no different phase was detected.

[0036] In Examples 4 and 5, the amount of LiOH·H2O and ion-exchanged water used to obtain the A solution and the amount of ion-exchanged water used to obtain the B solution were changed, the Li / Si molar ratio was changed from that in Example 1, and the holding temperature in the fine particle dissolving step was changed to obtain transparent aqueous solutions in which fine particles according to Examples 4 and 5 were dissolved. The preparation conditions of the aqueous solutions in these Examples are shown in Table 1, and the composition of the obtained aqueous solutions and the results of X-ray diffraction measurement of the powders calcined at 750°C are shown in Table 2. In both of the X-ray diffraction measurement results of the powders calcined at 750°C obtained from the aqueous solutions according to Examples 4 and 5, a diffraction peak derived from Li4SiO4 (lithium orthosilicate) crystals was observed. Figure 1 shows the X-ray diffraction pattern obtained by X-ray diffraction measurement of the powder obtained by drying and calcining the aqueous solution obtained in Example 5 using the method described above. In Figure 1, a peak derived from Li4SiO4 (lithium orthosilicate) is observed. The diffraction peak intensity I0 derived from the Li4SiO4 (lithium orthosilicate) crystals was the diffraction peak with the highest peak intensity in the obtained X-ray diffraction pattern. Therefore, when the diffraction peak intensity with the highest peak intensity among the diffraction peaks of Li4SiO4 crystal is I0 and the diffraction peak intensity with the highest peak intensity among the diffraction peaks of the different phase is I1, the diffraction peak intensity ratio I1 / I0 has a relationship of I1 / I0<1.0, so it was found that the obtained sintered powder has lithium orthosilicate (Li4SiO4) crystal as the main phase. In Example 4, a different phase was detected, and the diffraction peak intensity ratio was I1 / I0=0.03. In Example 5, a different phase was detected, and the diffraction peak intensity ratio was I1 / I0=0.09.

[0037] [Comparative Example 1] 8.76 g of LiOH·H2O (lithium hydroxide monohydrate, Fujifilm Wako Pure Chemical Industries, Ltd.) and 87.59 g of ion-exchanged water were added to a 100 mL beaker and stirred at room temperature for 10 minutes to dissolve. This was used as solution A. 1111.02 g of an aqueous solution (Sigma-Aldrich Corporation, concentration 20 mass%) and 3.63 g of ion-exchanged water were added and kept at 50°C while stirring, and this was designated as Liquid B. Liquid A was added to Liquid B while stirring and kept at 50°C at an addition rate of 5 g / min, and white fine particles were generated in the mixed solution after the addition. In this case, the molar ratio of Li / Si was 5.98. The mixed solution containing the fine particles was then kept at 50°C and stirred for 120 minutes, but the fine particles did not dissolve and the absorbance became 1.00. In this case, it is believed that the fine particles did not completely dissolve because the amount of fine particles generated exceeded the soluble concentration. Since the fine particles did not dissolve, a powder calcined at 750°C was not prepared.

[0038] [Comparative Examples 2 and 3] The amounts of LiOH·H2O and ion-exchanged water used to obtain solution A from Example 1 and the amount of ion-exchanged water used to obtain solution B were changed to change the molar ratio of Li / Si, and the holding temperature in the microparticle dissolving step was also changed to obtain aqueous solutions of Comparative Examples 2 and 3. In these cases, the Li / Si was within the range of the present invention, but the generated microparticles did not dissolve. In this case, it is believed that the holding temperature was not appropriate, so the microparticles did not dissolve. Since the microparticles did not dissolve, no powder was produced by firing at 750°C. The preparation conditions for the aqueous solutions of these Comparative Examples are shown in Table 1, and the compositions of the obtained aqueous solutions are shown in Table 2.

[0039] [Comparative Example 4] 45.40g of LiOH·H2O (lithium hydroxide monohydrate, Fujifilm Wako Pure Chemical Industries, Ltd.) and 272.43g of ion-exchanged water were added to a 500mL beaker and stirred for 10 minutes at room temperature to dissolve. This was designated as Liquid A. 95.95g of lithium silicate solution (Nihon Kagaku Kogyo Co., Ltd., lithium silicate 35, SiO2: 20.9% by mass, LiO2: 2.9% by mass, molar ratio: 3.55) was added to a 500mL beaker and kept at 40°C while stirring, which was designated as Liquid B. Liquid A was added to Liquid B at a rate of 5g / min while stirring and kept at 40°C, and white fine particles were generated in the mixed solution after the addition. In this case, the Li content was 2.13% by mass, the Si content was 2.27% by mass, and the Li / Si molar ratio was 3.80. The mixed solution was then kept at 40°C and stirred for 70 minutes, but the fine particles did not dissolve. Since the fine particles did not dissolve, no powder was prepared by calcining at 750° C. Table 1 shows the preparation conditions of the aqueous solution in Comparative Example 4, and Table 2 shows the composition of the aqueous solution obtained.

[0040] From the above results, it is seen that by using the production method of the present invention, an aqueous solution containing lithium and silicon can be obtained that can be used as a precursor for forming a coating layer containing lithium orthosilicate on the surface of a positive electrode active material for a lithium secondary battery.

[0041] [Table 1]

[0042] [Table 2]

Claims

1. An aqueous solution containing lithium and silicon, the aqueous solution containing lithium from 0.1% by mass to 3.0% by mass and silicon from 0.1% by mass to 3.0% by mass, a molar ratio of lithium to silicon Li / Si of 3.70 to 5.20, and an absorbance at a wavelength of 660 nm of 0.10 or less.

2. The aqueous solution was dried and then heat-treated at 750° C. for 5 hours in an air atmosphere to obtain a calcined powder, which was mainly composed of lithium orthosilicate (Li 4 SiO 4 2. The aqueous solution containing lithium and silicon according to claim 1, wherein the aqueous solution is composed of crystals of the formula (I).

3. 2. The aqueous solution containing lithium and silicon according to claim 1, wherein the lithium content in the aqueous solution is 0.5% by mass or more and 2.0% by mass or less.

4. 2. The aqueous solution containing lithium and silicon according to claim 1, wherein the aqueous solution has a silicon content of 0.5% by mass or more and 2.0% by mass or less.

5. 2. The aqueous solution containing lithium and silicon according to claim 1, wherein the molar ratio Li / Si of lithium to silicon in said aqueous solution is 3.70 or more and 5.00 or less.

6. 2. The aqueous solution containing lithium and silicon according to claim 1, wherein the aqueous solution has an absorbance of 0.07 or less at a wavelength of 660 nm.

7. mixing an aqueous solution containing a silicon compound with an aqueous solution containing a lithium compound to obtain an aqueous solution having a lithium to silicon molar ratio Li / Si of 3.70 or more and 5.20 or less; The method for producing the aqueous solution containing lithium and silicon according to claim 1, further comprising the step of: maintaining the aqueous solution containing lithium and silicon at a temperature of 45° C. or higher and 60° C. or lower.

8. An aqueous solution coating step of coating the surface of the positive electrode active material for a lithium secondary battery with an aqueous solution containing lithium and silicon obtained according to claim 7; a coating layer forming step of drying the lithium secondary battery positive electrode active material coated with the aqueous solution containing lithium and silicon to form a coating layer containing lithium and silicon; a heat treatment step of subjecting the lithium secondary battery positive electrode active material having the coating layer containing lithium and silicon to a heat treatment; The present invention relates to a method for producing an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate,

9. An aqueous solution coating step of coating a surface of a positive electrode active material for a lithium secondary battery with the aqueous solution containing lithium and silicon according to claim 1; a coating layer forming step of drying the lithium secondary battery positive electrode active material coated with the aqueous solution containing lithium and silicon to form a coating layer containing lithium and silicon; a heat treatment step of subjecting the lithium secondary battery positive electrode active material having the coating layer containing lithium and silicon to a heat treatment; The present invention relates to a method for producing an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate,

Citation Information

Patent Citations

  • Glass-coated cathode powder for rechargeable batteries

    JP2014513392A

  • Method of producing ortho lithium silicate, method of producing meta lithium silicate, and method of producing carbon-dioxide absorbing material