Concrete composition, concrete structure, and method for manufacturing concrete structure
A concrete composition with borate and a setting accelerator addresses the setting retardation issue, maintaining corrosion resistance and structural integrity by using a 1/5 to 1/4 mass ratio, enhancing the durability of reinforcing bars in concrete structures.
Patent Information
- Application Number
- JP2023083017
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
Smart Images

Figure 2024166717000001 
Figure 2024166717000002 
Figure 2024166717000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a concrete composition, a concrete structure, and a method for producing a concrete structure. [Background technology]
[0002] As a method for preventing corrosion of reinforcing bars in reinforced concrete (hereinafter referred to as "corrosion prevention method"), a method is known in which an anticorrosive agent is used to perform an anticorrosive treatment on the surface of existing concrete or on fresh concrete during production.
[0003] A method of applying tannic acid to the surface of existing concrete to perform anti-rust treatment is known (see, for example, Patent Document 1). The method described in Patent Document 1 is intended to prevent corrosion of reinforcing bars in existing hardened concrete. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-75775 Summary of the Invention [Problem to be solved by the invention]
[0005] Borates are known as materials used to prevent corrosion of metals. It is known that carbon steel is passivated in borate buffer solutions at pH 9 or higher. It is also known that the passive film of carbon steel can be maintained in borate buffer solutions at pH 9 or higher, even if the borate buffer solution contains a certain concentration of salt. This not only inhibits corrosion of reinforcing bars even when concrete is neutralized, but also improves the durability of reinforcing bars against salt damage.
[0006] However, adding borates to concrete significantly delays the setting of the concrete. In addition, if a large amount of borates is added to concrete, there is a concern that the strength of the concrete may decrease. For this reason, borates have not been used as a rust inhibitor for concrete.
[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a concrete composition, a concrete structure, and a method for manufacturing a concrete structure, which are capable of suppressing delay in setting when a borate is used as a rust inhibitor for reinforcing bars in reinforced concrete. [Means for solving the problem]
[0008] The present invention has the following aspects. [1] A concrete composition comprising a base concrete, a borate, and a set accelerator. [2] The concrete composition according to [1], wherein a mixing ratio of the borate to the setting accelerator is 1 / 5 to 1 / 4 by mass. [3] The concrete composition according to [1], wherein the set accelerator comprises an aluminum sulfonate. [4] The concrete composition according to [3], wherein the setting accelerator further comprises at least one selected from the group consisting of melamine-based compounds, oxycarboxylic acids, and salts of oxycarboxylic acids. [5] A concrete structure comprising a hardened concrete composition according to any one of [1] to [4]. [6] Adding a setting accelerator to the base concrete and mixing the mixture to prepare a mixture of the base concrete and the setting accelerator; Adding boric acid to the mixture to prepare a concrete composition; and pouring the concrete composition into a formwork containing reinforcing bars and compacting the composition. Effect of the Invention
[0009] According to the present invention, it is possible to provide a concrete composition, a concrete structure, and a method for manufacturing a concrete structure, which are capable of suppressing delay in setting when a borate is used as a rust inhibitor for reinforcing bars in reinforced concrete. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] BEST MODE FOR CARRYING OUT THE DISCLOSURE The concrete composition, concrete structure, and method for producing a concrete structure according to the present invention will be described below. It should be noted that the present embodiment is specifically described to allow a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified.
[0011] [Concrete composition] A concrete composition according to one embodiment of the present invention includes a base concrete, boric acid, and a set accelerator.
[0012] "Base concrete" The base concrete includes water, cement, fine aggregate, coarse aggregate, and chemical admixtures.
[0013] (water) The water is not particularly limited, and any water that complies with JIS A 5308:2019 "Ready Mixed Concrete" can be used.
[0014] (cement) The cement is not particularly limited as long as it is a powder that hardens by a chemical reaction with water and is made mainly of limestone, clay, silica stone, iron oxide raw materials, etc. Examples of the cement include portland cement (JIS R 5210:2009), blast furnace cement (JIS R 5211:2009), silica cement (JIS R 5212:2009), fly ash cement (JIS R 5213:2009), ecocement (JIS R 5214:2009), etc.
[0015] There are six types of Portland cement - normal, early strength, extra early strength, moderate heat, low heat and sulfate resistant - and their respective low alkali types, for a total of 12 types (JIS R 5210:2009).
[0016] Blast-furnace cement is classified into Type A, Type B, and Type C blast-furnace cement depending on the amount of blast-furnace slag mixed in (JIS R 5211:2009). Blast-furnace cement type A: Blast-furnace slag content: 5-30% by mass Blast-furnace cement type B: Blast-furnace slag content 10-60% by mass Blast-furnace cement type C: blast-furnace slag content 60-70% by mass
[0017] (fine aggregate) The fine aggregate is not particularly limited, and may be any aggregate for concrete as specified in JIS A 5005:2020 "Crushed stone and crushed sand for concrete" or the like.
[0018] (coarse aggregate) The coarse aggregate is not particularly limited, and may be any coarse aggregate for concrete as specified in JIS A 5005:2020 “Crushed stone and crushed sand for concrete” or the like.
[0019] (Chemical admixtures) The chemical admixture is not particularly limited, and any chemical admixture that is usually mixed with cement can be used.
[0020] (Borate) The content of borate in the concrete composition of this embodiment is determined according to the required corrosion resistance. The self-passivation behavior of carbon steel in an aqueous solution environment containing borate ions is known, and the passivation can be determined by the following formula (1). SPI = (0.5[SO4 2- ]+[Cl - ]) / ([HCO3 - ]+14[B(OH)4 - ] E ) (1) In the above formula (1), [Cl- ] is chloride, [B(OH)4 - ] corresponds to boric acid. Since concrete is inherently a highly alkaline environment, HCO3 - is 0. SO4 2- The source of is cement and the setting accelerator described below, but the SO4 2- Since the amount is very small, it is mostly determined by the setting accelerator. B(OH)4 - is determined by the borate added.
[0021] (setting accelerator) The setting accelerator preferably contains an aluminum sulfonate, more preferably consists of an aluminum sulfonate, and further preferably contains at least one selected from the group consisting of a melamine compound, an oxycarboxylic acid, and a salt of an oxycarboxylic acid.
[0022] Aluminum sulfonates include various aluminum sulfates. Aluminum sulfate is represented by the general formula Al2(SO4)3·nH2O, where n is in the range of 0 to 18. The aluminum sulfate may be either anhydrous aluminum sulfate or aluminum sulfate with various numbers of water of crystallization.
[0023] The average particle size of the aluminum sulfonate is not particularly limited, but is preferably 500 μm or less, and more preferably 325 μm or less. The average particle size of the aluminum sulfonate is a value measured by a laser diffraction / scattering type particle size distribution analyzer manufactured by Horiba, Ltd.
[0024] The melamine-based compound is preferably a powdered melamine-based compound, and examples of such compounds include methylol melamine condensates, melamine sulfonates, melamine sulfonate-formaldehyde condensates, etc. Specifically, products such as "Sikament FF" manufactured by Sika Japan Co., Ltd. can be used.
[0025] Examples of the oxycarboxylic acid include tartaric acid, citric acid, gluconic acid, etc. Examples of the salt of the oxycarboxylic acid include the salt of the above-mentioned oxycarboxylic acid, etc. These may be used alone or in combination of two or more.
[0026] In the concrete composition of this embodiment, the mixing ratio of the borate and the setting accelerator is preferably 1 / 5 to 1 / 4, more preferably 1 / 5, by mass ratio. When the mixing ratio is equal to or greater than the lower limit, the setting speed of the concrete composition containing boric acid can be made equal to that of the concrete composition using only the base concrete during the period until the setting begins. When the mixing ratio is equal to or less than the upper limit, the setting speed of the concrete composition can be made equal to that of the concrete composition using only the base concrete during the period until the setting ends.
[0027] (Other Ingredients) The concrete composition of the present embodiment may be mixed with other conventionally used components than those mentioned above, so long as the effects of the present invention are not impaired.
[0028] According to the concrete composition of the present embodiment, since the concrete composition contains base concrete, a borate, and a setting accelerator, even if the concrete composition contains a borate, the setting of the concrete composition can be prevented from being delayed. Furthermore, since the concrete composition of the present embodiment contains a borate, when a concrete structure containing a reinforcing bar is manufactured, the concrete composition of the present embodiment can prevent the corrosion of the reinforcing bar.
[0029] [Concrete structure] A concrete structure according to one embodiment of the present invention comprises a hardened product of the concrete composition according to one embodiment of the present invention.
[0030] According to the concrete structure of the present embodiment, since the concrete structure is made of the hardened product of the concrete composition of the above-mentioned embodiment, when the concrete structure contains reinforcing bars, corrosion of the reinforcing bars can be suppressed.
[0031] [Manufacturing method of concrete structures] A method for manufacturing a concrete structure according to one embodiment of the present invention includes the steps of adding a set accelerator to base concrete and mixing the base concrete to prepare a mixture of the base concrete and the set accelerator (hereinafter referred to as "step 1"); adding a borate to the mixture to prepare a concrete composition (hereinafter referred to as "step 2"); and pouring the concrete composition into a formwork containing reinforcing bars and compacting it (hereinafter referred to as "step 3").
[0032] The method for producing a concrete structure of the present embodiment may include, prior to step 1, a step of preparing base concrete. In the step of preparing the base concrete, first, the above-mentioned water, cement, fine aggregate, coarse aggregate, and chemical admixture are mixed in predetermined amounts to prepare the base concrete.
[0033] In step 1, a predetermined amount of the above-mentioned setting accelerator is added to the above-mentioned base concrete, and they are kneaded to prepare a mixture of the base concrete and the setting accelerator. The method for mixing the base concrete and the setting accelerator is not particularly limited, and may be, for example, in a mixer at a concrete production plant, or the base concrete may be produced in a mixer at a concrete production plant and then loaded into an agitator truck, and the setting accelerator may be loaded into the drum of the agitator truck and mixed therein.
[0034] In step 2, a predetermined amount of borate is added to the mixture obtained in step 1 to obtain the concrete composition of the above embodiment.
[0035] In step 3, the concrete composition is poured into a formwork containing reinforcing bars and compacted. Through the above steps, the concrete structure of the above embodiment is obtained.
[0036] According to the method for manufacturing a concrete structure of the present embodiment, a concrete structure is manufactured using the concrete composition of the above-mentioned embodiment, so that the concrete composition can be set without delaying setting to the same extent as in the case where only the base concrete is used.
[0037] According to the method for producing a concrete structure of this embodiment, the concrete composition of the above embodiment can be obtained by carrying out the above steps 1 and 2 in this order. If a borate is added to base concrete to prepare a mixture of base concrete and borate, and a set accelerator is mixed into the mixture, the set accelerator does not have a set acceleration effect, and a larger amount of set accelerator is required to obtain the concrete composition of the above embodiment. EXAMPLES
[0038] The present invention will be described in more detail below with reference to experimental examples, but the present invention is not limited to the following experimental examples.
[0039] [Preparation of base concrete] Tap water was used as the water (W). Ordinary Portland cement and blast-furnace slag cement type B were used as cement (C). Hard crushed sandstone was used as the fine aggregate (S). Hard crushed sandstone was used as the coarse aggregate (G). The chemical admixture (AE) used was a lignosulfonate AE water reducer. These materials were mixed as shown in Table 1 (mixture A), Table 2 (mixture B) and Table 3 (mixture C). Mixtures A and B have different water-cement ratios, but the other conditions are the same. Mixtures B and C have different types of cement, but the other conditions are the same.
[0040] [Table 1]
[0041] [Table 2]
[0042] [Table 3]
[0043] [Experimental Example 1] Only the base concrete of mix A above was used.
[0044] [Experimental Example 2] 1m of base concrete of above mix A 3 A borate was added in an amount of 0.5 mass % based on the mass of cement contained in the base concrete to prepare a concrete composition.
[0045] [Experimental Example 3] A concrete composition was prepared by adding a setting accelerator of 2.0 mass% of the mass of the borate contained in the concrete composition to the concrete composition of Experimental Example 2. The mixing ratio of the borate to the setting accelerator was 1 / 4 by mass ratio. As the setting accelerator, Denka ACF material (hereinafter simply referred to as "ACF material") manufactured by Denka Co., Ltd. was used.
[0046] [Experimental Example 4] Only the base concrete of mix B above was used.
[0047] [Experimental Example 5] 1m of base concrete of above mix B 3 A borate was added in an amount of 0.2 mass % based on the mass of cement contained in the base concrete to prepare a concrete composition.
[0048] [Experimental Example 6] 1m of base concrete of above mix B 3 A borate was added in an amount of 0.5 mass % based on the mass of cement contained in the base concrete to prepare a concrete composition.
[0049] [Experimental Example 7] A concrete composition was prepared by adding a setting accelerator in an amount of 0.5 mass% of the mass of the borate contained in the concrete composition to the concrete composition of Experimental Example 6. The mixing ratio of the borate to the setting accelerator was 1 / 1 in terms of mass ratio.
[0050] [Experimental Example 8] A concrete composition was prepared by adding a setting accelerator in an amount of 1.5 mass% of the mass of the borate contained in the concrete composition to the concrete composition of Experimental Example 6. The mixing ratio of the borate to the setting accelerator was 1 / 3 in terms of mass ratio.
[0051] [Experimental Example 9] A concrete composition was prepared by adding a setting accelerator in an amount of 2.0 mass% of the mass of the borate contained in the concrete composition to the concrete composition of Experimental Example 6. The mixing ratio of the borate to the setting accelerator was 1 / 4 in terms of mass ratio.
[0052] [Experimental Example 10] A concrete composition was prepared by adding a setting accelerator in an amount of 2.5 mass% of the mass of the borate contained in the concrete composition to the concrete composition of Experimental Example 6. The mixing ratio of the borate to the setting accelerator was 1 / 5 in terms of mass ratio.
[0053] [Experimental Example 11] 1m of base concrete of above mix B 3 A borate was added in an amount of 0.8 mass % based on the mass of cement contained in the base concrete to prepare a concrete composition.
[0054] [Experimental Example 12] A concrete composition was prepared by adding a setting accelerator in an amount of 2.0 mass% of the mass of the borate contained in the concrete composition to the concrete composition of Experimental Example 11. The mixing ratio of the borate to the setting accelerator was 2 / 5 by mass.
[0055] [Experimental Example 13] Only the base concrete of mix C above was used.
[0056] [Experimental Example 14] 1m of base concrete of the above mix C 3 A borate was added in an amount of 0.5 mass % based on the mass of cement contained in the base concrete to prepare a concrete composition.
[0057] [Experimental Example 15] A concrete composition was prepared by adding a setting accelerator in an amount of 2.0 mass% of the mass of the borate contained in the concrete composition to the concrete composition of Experimental Example 14. The mixing ratio of the borate to the setting accelerator was 1 / 4 in terms of mass ratio.
[0058] For the base concrete or concrete composition of Experimental Examples 1 to 15, tap water was poured in, and the concrete composition was measured from the start of pouring water until the hardened concrete composition started to harden (the strength of the hardened concrete composition was 3.5 N / mm2) in accordance with JIS A 1147:2019 "Test method for setting time of concrete". 2 The time required for the temperature to reach the above level was measured. The results are shown in Table 4.
[0059] [Table 4]
[0060] The results shown in Table 4 indicate that adding ACF material to a concrete composition containing borate shortens the time until the start of setting. In particular, when the mixing ratio of borate to ACF material is 1 / 5 to 1 / 4 by mass, as in Experimental Examples 3, 9, 10, and 15, it was found that the time until the start of setting is shortened to the same level as or shorter than when only base concrete is used.
Claims
1. A concrete composition comprising a base concrete, a borate, and a set accelerator.
2. The concrete composition according to claim 1, wherein a mixing ratio of the borate to the setting accelerator is 1 / 5 to 1 / 4 by mass ratio.
3. The concrete composition of claim 1 , wherein the set accelerator comprises an aluminum sulfonate.
4. The concrete composition according to claim 3 , wherein the set accelerator further comprises at least one selected from the group consisting of melamine-based compounds, oxycarboxylic acids, and salts of oxycarboxylic acids.
5. A concrete structure comprising a hardened concrete composition according to any one of claims 1 to 4.
6. A step of adding a setting accelerator to a base concrete and mixing the resulting mixture to prepare a mixture of the base concrete and the setting accelerator; Adding boric acid to the mixture to prepare a concrete composition; and pouring the concrete composition into a formwork containing reinforcing bars and compacting the composition.
Citation Information
Patent Citations
Manufacturing method of treatment agent performing Anti-corrosion treatment of internal steel material of concrete structure and deterioration prevention of concrete, and method of steel Anti-corrosion treatment and concrete deterioration prevention treatment