Paper barrier material

A paper barrier material with polyurethane and swellable mica in the water vapor layer, and polyvinyl alcohol in the gas barrier layer, addresses the need for effective gas and water vapor barriers in flexible packaging, maintaining performance under bending and being eco-friendly.

JP2024166759APending Publication Date: 2024-11-29NIPPON PAPER IND CO LTD

Patent Information

Application Number
JP2023083080
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

Smart Images

  • Figure 2024166759000001
    Figure 2024166759000001
Patent Text Reader

Abstract

To provide a novel paper barrier material.SOLUTION: There is provided a paper barrier material that comprises a water vapor barrier layer on a paper base material. The water vapor barrier layer contains a polyurethane-based resin and swellable mica, and the polyurethane-based resin is contained in the amount of 65 pts.wt. or more and 88 pts.wt. or less based on 100 pts.wt. of the total amount of the water vapor barrier layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a paper barrier material. [Background technology]

[0002] 2. Description of the Related Art It is important to impart gas barrier properties (particularly oxygen barrier properties) to paper materials, particularly paper packaging materials, in order to protect various packaged products from deterioration due to gas, for example oxidation due to oxygen. Conventionally, the main method for imparting gas barrier properties to paper packaging materials has been to extrusion laminate or attach a gas barrier layer to a paper base material, such as a metal foil or metal vapor-deposited film made of a metal such as aluminum, a resin film such as polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinylidene chloride, or polyacrylonitrile, or a film coated with these resins, or a ceramic vapor-deposited film on which an inorganic oxide such as silicon oxide or aluminum oxide is vapor-deposited. It is also important to impart water resistance (particularly water vapor barrier properties) to paper packaging materials in order to protect various packaged products from deterioration due to water vapor.

[0003] The present applicant has proposed a paper barrier packaging material with both gas barrier properties and water vapor barrier properties, which has a water vapor barrier layer containing a water vapor barrier resin and a pigment, and a gas barrier layer containing a polyvinyl alcohol-based resin and a pigment, on a paper base material (Patent Document 1). Furthermore, among such paper barrier packaging materials, there are known those that enable heat sealing processing by providing a sealant layer on at least one of the outermost layers. For example, Patent Document 2 proposes providing a laminate layer (corresponding to a sealant layer) by melt extrusion lamination, dry lamination, or direct melt coating. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2013 / 069788 [Patent Document 2] International Publication No. 2017 / 170462 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a novel paper barrier material. [Means for solving the problem]

[0006] The means for solving the problems of the present invention are as follows. 1. A water vapor barrier layer is provided on a paper substrate. the water vapor barrier layer contains a polyurethane resin and a swellable mica, A paper barrier material comprising 65 to 88 parts by weight of the polyurethane resin per 100 parts by weight of the total amount of the water vapor barrier layer. 2. The paper barrier material according to 1, characterized in that the glass transition temperature of the polyurethane resin is -20°C or higher and 150°C or lower. 3. The paper barrier material according to 1 or 2, characterized in that the aspect ratio of the swellable mica is 300 or more. 4. The paper barrier material according to any one of 1. to 3., characterized in that the 50% volume average particle size of the swellable mica is 10 μm or more and 25 μm or less. 5. The paper barrier material according to any one of 1. to 4., characterized in that the water vapor barrier layer contains 5 parts by weight or more and 35 parts by weight or less of the swellable mica per 100 parts by weight of the total amount of the water vapor barrier layer. 6. The paper barrier material according to any one of 1. to 5., characterized in that it has a gas barrier layer on the water vapor barrier layer. 7. The paper barrier material according to 6., wherein the gas barrier layer contains a water-soluble polymer. 8. The coating amount (dry weight) of the water vapor barrier layer is 3 g / m 2 More than 8g / m 2The coating amount (dry weight) of the gas barrier layer is 4 g / m 2 More than 10g / m 2 8. The paper barrier material according to 6. or 7., characterized in that: 9. The water vapor transmission rate of the paper barrier material at 40°C and 90% RH is 0.1 g / m 2 ·day or more 15g / m 2 9. The paper barrier material according to any one of 1. to 8., characterized in that the heat resistance is 50% or less. Effect of the Invention

[0007] The present invention provides a novel paper barrier material. The paper barrier material of the present invention has excellent water vapor barrier properties. The paper barrier material of the present invention, which is provided with a gas barrier layer, also has excellent gas barrier properties. The paper barrier material of the present invention has excellent flex resistance and exhibits little deterioration in barrier properties when bent. Therefore, the paper barrier material of the present invention can be suitably used for flexible packaging bags which are prone to bending. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] "Paper barrier material" The paper barrier material of the present invention has a paper substrate and a water vapor barrier layer on the paper substrate, The water vapor barrier layer contains a polyurethane resin and swellable mica, and contains 65 parts by weight or more and 88 parts by weight or less of the polyurethane resin per 100 parts by weight of the total amount of the water vapor barrier layer.

[0009] (Paper base material) In the present invention, the paper base material is a sheet made of pulp, filler, and various auxiliary agents. The pulp may be chemical pulp such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), unbleached softwood kraft pulp (NUKP), sulfite pulp, etc., mechanical pulp such as stone grind pulp and thermomechanical pulp, wood fibers such as deinked pulp and waste paper pulp, non-wood fibers obtained from kenaf, bamboo, hemp, etc., and one or more of these may be used in combination. Among these, it is preferable to use chemical pulp of wood fiber or mechanical pulp of wood fiber, and it is more preferable to use chemical pulp of wood fiber, for reasons such as the fact that foreign matter is unlikely to be mixed into the paper base material, that discoloration is unlikely to occur over time when recycled as waste paper raw material after use, that the surface texture is good when printed due to high whiteness, and that the value of use is high especially when used as a packaging material.

[0010] As the filler, known fillers such as white carbon, talc, kaolin, clay, heavy calcium carbonate, light calcium carbonate, titanium oxide, zeolite, and synthetic resin fillers can be used as necessary. In addition, aluminum sulfate and various anionic, cationic, nonionic or amphoteric retention aids, drainage aids, paper strength agents, internal sizing agents, etc. may be used as necessary. Furthermore, dyes, fluorescent whitening agents, pH adjusters, defoamers, pitch control agents, slime control agents, etc. may also be added as necessary.

[0011] The method for producing the paper base material (papermaking) is not particularly limited, and the paper base material can be produced by acidic papermaking, neutral papermaking, or alkaline papermaking using a known Fourdrinier former, on-top hybrid former, gap former machine, etc. The paper base material may be one layer, or may be composed of two or more layers. Furthermore, the surface of the paper substrate can be treated with various chemicals. Examples of chemicals that can be used include oxidized starch, hydroxyethyl etherified starch, enzyme-modified starch, polyacrylamide, polyvinyl alcohol, surface sizing agents, water-resistant agents, water retention agents, thickeners, and lubricants, and these can be used alone or in combination of two or more. Furthermore, these various chemicals can be used in combination with pigments. Examples of pigments include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white, and organic pigments such as solid, hollow, or core-shell types can be used alone or in combination of two or more.

[0012] The method for treating the surface of the paper substrate is not particularly limited, but known coating devices such as a rod metering size press, a pond type size press, a gate roll coater, a spray coater, a blade coater, and a curtain coater can be used. Examples of the paper base material obtained in this manner include various known types of paper, such as fine paper, medium quality paper, coated paper, one-sided glossy paper, kraft paper, one-sided glossy kraft paper, bleached kraft paper, glassine paper, paperboard, white paperboard, and liner.

[0013] The basis weight of the paper substrate can be appropriately selected depending on the desired qualities and handling properties of the paper barrier material, but is usually 20 g / m 2 More than 500g / m 2 For paper barrier materials used for packaging applications such as food packaging, containers, and cups, a maximum of 25 g / m2 is preferable. 2 More than 400g / m 2 The following is more preferable, and in particular for paper barrier materials used for flexible packaging bags described below, the following is 30 g / m 2 More than 110g / m 2 The following is more preferred: The thickness of the paper substrate can be appropriately selected depending on the various qualities and handleability desired for the paper barrier material, but it is preferably from 30 μm to 600 μm, and more preferably from 45 μm to 125 μm.

[0014] (Water vapor barrier layer) The water vapor barrier layer contains a polyurethane resin and swellable mica, and contains 65 parts by weight or more and 88 parts by weight or less of the polyurethane resin relative to 100 parts by weight of the total amount of the water vapor barrier layer.

[0015] [Polyurethane resin] The polyurethane resin can be obtained by reacting a polyol with a polyisocyanate and, if necessary, a chain extender. The polyurethane resin of the present invention may be a polyurethane urea having a urea bond. As the polyol, those used as raw materials for polyurethane, such as polyether polyol, polyester polyol, and polycarbonate polyol, can be used without any particular limitation. In addition, the polyisocyanate is also not particularly limited, and those used as raw materials for polyurethane, such as aliphatic isocyanate, alicyclic isocyanate, and aromatic isocyanate, can be used without any particular limitation, but from the viewpoint of water vapor barrier properties, cyclic isocyanate is preferred, and specific examples thereof include MDI, hydrogenated MDI, XDI, and hydrogenated XDI. In the present invention, one or more types of polyurethane resins can be used in combination.

[0016] The polyurethane resin preferably has a glass transition temperature of -20° C. or more and 150° C. or less, more preferably -10° C. or more and 140° C. or less, and even more preferably 0° C. or more and 135° C. or less. The glass transition temperature is measured in accordance with JIS K 7122:2012. As the polyurethane resin, commercially available products can be used, such as "Takelac W series," "Takelac WPB series," and "Takelac WS series" manufactured by Mitsui Chemicals, Inc., and specifically, Takelac WPB-341 (product name) can be mentioned. The water vapor barrier layer contains 65 to 88 parts by weight of polyurethane resin per 100 parts by weight of the total amount of the water vapor barrier layer. If the content of the polyurethane resin is within this range, the water vapor barrier properties are excellent and it is easy to adjust the viscosity to a suitable level for application. The water vapor barrier layer preferably contains 70 parts by weight or more of polyurethane resin per 100 parts by weight of the total amount of the water vapor barrier layer, and preferably contains 85 parts by weight or less.

[0017] [Swellable mica] Mica is a mineral whose main components are SiO2, Al2O3, K2O, and crystal water, and has excellent heat resistance, electrical insulation, water resistance, etc. There are various types of mica, such as muscovite, phlogopite, and biotite, as well as margarite, taeniolite, and synthetic mica. Since mica has a high aspect ratio and improves water vapor barrier properties, the present invention uses swelling mica, which is a type of synthetic mica, as the mica, and two or more types of swelling mica can also be mixed and used. Synthetic mica is artificially synthesized mica, and is also called synthetic fluorine phlogopite because its composition formula is similar to that of phlogopite.

[0018] The 50% volume average particle size (D50, median size) (hereinafter also referred to as "average particle size") of the swellable mica used in the present invention is preferably 1 μm or more and 100 μm or less, more preferably 5 μm or more, even more preferably 10 μm or more, more preferably 50 μm or less, and even more preferably 25 μm or less. The aspect ratio of the swellable mica is preferably 300 or more, more preferably 400 or more, and even more preferably 450 or more. Here, the aspect ratio is a value calculated from a microscopic enlarged photograph of the cross section of the coating layer, and is the average value of the average particle size of the mica divided by the thickness. The larger the aspect ratio, the more improved the water vapor barrier property. There is no particular upper limit to the aspect ratio of the swellable mica used in the present invention, but it is, for example, 1600 or less. Specific examples of the swelling mica include synthetic mica manufactured by Topy Industries Ltd. (product name: NTS-10) and synthetic mica manufactured by Katakura Co-op Agri Co., Ltd. (product name: ME300B-4T). From the viewpoint of improving the water vapor barrier property, the content of the swellable mica in the water vapor barrier layer is preferably from 5 to 35 parts by weight, relative to 100 parts by weight of the total amount of the water vapor barrier layer, more preferably 10 parts by weight or more, and even more preferably 15 parts by weight or more.

[0019]

[0043] In addition to the above-mentioned polyurethane resin and swellable mica, the water vapor barrier layer can contain various commonly used auxiliary agents such as water vapor barrier resins, water-soluble polymers, pigments, crosslinking agents, water repellents, dispersants, thickeners, water retention agents, defoamers, water resistance agents, dyes, and fluorescent dyes.

[0020] (Gas barrier layer) The paper barrier material of the present invention preferably has a gas barrier layer on the water vapor barrier layer. The gas barrier layer contains at least a gas barrier resin. As the gas barrier resin, a water-soluble resin or a water-suspendable resin can be used, and a water-soluble resin is preferred. As the gas barrier resin, for example, polyvinyl alcohol resins such as fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, and ethylene copolymerized polyvinyl alcohol, proteins such as casein, soybean protein, and synthetic protein, starches such as oxidized starch, cationic starch, urea phosphate esterified starch, and hydroxyethyl etherified starch, cellulose derivatives such as carboxymethyl cellulose, hydroxymethyl cellulose, and hydroxyethyl cellulose, polyurethane resins, polyvinylpyrrolidone, and sodium alginate can be exemplified, and these can be used alone or in a mixture of two or more kinds. Among these, from the viewpoint of gas barrier properties, polyvinyl alcohol resins and cellulose derivatives are preferred, polyvinyl alcohol resins are more preferred, polyvinyl alcohol resins having a degree of polymerization of 400 to 1700 are even more preferred, and polyvinyl alcohol resins having a degree of polymerization of 800 to 1400 are even more preferred. The saponification degree of the polyvinyl alcohol resin is preferably 95.0 or more, more preferably 97.0 or more, and even more preferably 99.0 or more.

[0021] The gas barrier layer may contain a pigment. Examples of the pigment include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white, and organic pigments such as solid, hollow, and core-shell types, which may be used alone or in combination of two or more. Among these, the pigment is preferably a flat pigment having an average particle size of 3 μm or more and an aspect ratio of 10 or more, and more preferably a flat pigment having an average particle size of 5 μm or more and an aspect ratio of 30 or more.

[0022] When a gas barrier layer contains a pigment, particularly a flat pigment, gases such as oxygen travel a longer distance to bypass the pigment, and therefore the gas barrier layer containing the pigment has superior gas barrier properties compared to a gas barrier layer not containing a pigment, and exhibits superior gas barrier properties especially under high humidity conditions. The blending amount of the pigment in the gas barrier layer is preferably 90 parts by weight or less of the pigment per 100 parts by weight of the gas barrier resin, in terms of dry weight. Note that the pigment is an optional component of the gas barrier layer, and it is also possible to not include it (0 parts by weight). By setting the blending amount of the pigment in the gas barrier layer within this range, excellent flex resistance can be exhibited. Furthermore, by containing a pigment in the gas barrier layer, the adhesion between the gas barrier layer and the layer in contact with it is improved. If the blending amount of the pigment is reduced, the flex resistance is improved, but the gas barrier properties are reduced. Therefore, the blending amount of the pigment can be adjusted according to the balance between the gas barrier properties and flex resistance required for the paper barrier material, and can be, for example, 5 parts by weight or more and 80 parts by weight or less per 100 parts by weight of the gas barrier resin. In addition to the above-mentioned water-soluble resins and pigments, the gas barrier layer may contain various commonly used auxiliary agents such as dispersants, thickeners, water retention agents, defoamers, water-resistant agents, dyes, and fluorescent dyes.

[0023] A crosslinking agent, such as a polyvalent metal salt, can be added to the gas barrier layer. The crosslinking agent causes a crosslinking reaction with the water-soluble polymer contained in the gas barrier layer, increasing the number of bonds (crosslinking points) in the gas barrier layer. In other words, the gas barrier layer has a dense structure and can exhibit good gas barrier properties. The type of crosslinking agent is not particularly limited, and can be appropriately selected and used according to the type of water-soluble polymer contained in the gas barrier layer, such as polyvalent metal salts (compounds in which polyvalent metals such as copper, zinc, silver, iron, potassium, sodium, zirconium, aluminum, calcium, barium, magnesium, titanium, etc. are bonded to ionic substances such as carbonate ions, sulfate ions, nitrate ions, phosphate ions, silicate ions, nitrogen oxides, boron oxides, etc.), amine compounds, amide compounds, aldehyde compounds, hydroxy acids, etc. From the viewpoint of the expression of the crosslinking effect, it is preferable to use polyvalent metal salts, and it is more preferable to use potassium alum. The amount of the crosslinking agent is not particularly limited as long as it is within the range of the paint concentration and viscosity that can be applied, but it is preferably 1 part by weight to 10 parts by weight, more preferably 3 parts by weight to 5 parts by weight, per 100 parts by weight of the pigment. If it is less than 1 part by weight, the effect of adding the crosslinking agent may not be fully obtained. If it is more than 10 parts by weight, the viscosity of the paint may increase significantly, making application difficult.

[0024] It is preferable that the gas barrier layer contains a surfactant, since the adhesion between the gas barrier layer and the water vapor barrier layer is improved, and the barrier property is improved. The ionicity of the surfactant is not limited, and any of anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants may be used alone or in combination of two or more. Examples of surfactants include silicone surfactants, fluorine surfactants, alcohol surfactants, acetylene surfactants having an acetylene group, acetylene diol surfactants having an acetylene group and two hydroxyl groups, alkylsulfonic acid surfactants having an alkyl group and sulfonic acid, ester surfactants, amide surfactants, amine surfactants, alkyl ether surfactants, phenyl ether surfactants, sulfate ester surfactants, and phenol surfactants. Among these, it is preferable to use an acetylene diol surfactant, which has a large effect of improving the leveling property of the paint. In addition, when the leveling property of the paint is improved, the uniformity of the gas barrier layer is improved, and the gas barrier property is improved. When a gas barrier layer is provided on a water vapor barrier layer, from the viewpoint of adhesion to the water vapor barrier layer, the surface tension of the paint for the gas barrier layer is preferably adjusted to 10 mN / m or more and 60 mN / m or less, and more preferably 15 mN / m or more and 50 mN / m or less. In addition, from the viewpoint of adhesion between the water vapor barrier layer and the gas barrier layer, it is preferable to adjust the surface tension of the paint for the gas barrier layer to ±20 mN / m with respect to the wetting tension of the water vapor barrier layer surface.

[0025] (Water vapor barrier layer, gas barrier layer coating) In the present invention, the water vapor barrier layer and the gas barrier layer are coated layers, and can be formed by applying a paint for forming a barrier coating layer using various coating devices and drying it. Whether or not a layer is a coated layer can be determined by cutting the paper barrier material and observing the cross section of the layer under a microscope or the like. The method of applying the coating material for forming the water vapor barrier layer and the gas barrier layer to the paper substrate is not particularly limited, and the coating can be performed using a known coating device and coating system. Examples of the coating device include a blade coater, a bar coater, a roll coater, an air knife coater, a reverse roll coater, a curtain coater, a spray coater, a size press coater, and a gate roll coater. Examples of the coating system include water-based coating using a solvent such as water, and solvent-based coating using a solvent such as an organic solvent, with water-based coating being preferred. As a method for drying the water vapor barrier layer and the gas barrier layer, for example, a usual method such as using a steam heater, a gas heater, an infrared heater, an electric heater, a hot air heater, a microwave, or a cylinder dryer is used.

[0026] In the present invention, the coating amount of the water vapor barrier layer is 2 g / m2 in terms of dry weight. 2 More than 50g / m 2 The coating weight of the water vapor barrier layer is preferably 2 g / m or less. 2 If the coating weight is less than 50 g / m2, it may be difficult to completely cover the paper substrate with the paint, resulting in insufficient water vapor barrier properties, or when a coating layer is formed on top of it, the paint may penetrate into the paper substrate, making it difficult to form a uniform coating layer. 2 If the amount is more than this, the drying load during coating will be large. The coating amount of the water vapor barrier layer is 3g / m2 in dry weight. 2 More preferably, 40 g / m 2 Less than 30 g / m is more preferable. 2 More preferably, 20 g / m 2 Even more preferably, 10 g / m 2 Even more preferably, 8 g / m 2 Even more preferred is the following: The water vapor barrier layer may be one layer, or may be configured as two or more layers. When the water vapor barrier layer is configured as two or more layers, the total coating amount of all the water vapor barrier layers is preferably within the above range.

[0027] In the present invention, the coating amount of the gas barrier layer is 0.2 g / m2 in terms of dry weight. 2 More than 20g / m 2 The coating weight of the gas barrier layer is preferably 0.2 g / m or less. 2 If the thickness is less than 20 g / m, it is difficult to form a uniform gas barrier layer, and sufficient gas barrier properties may not be obtained. 2 If the amount is more than this, the drying load during coating will be large. The coating amount of the gas barrier layer is 0.5 g / m2 in dry weight. 2 More preferably, 1 g / m 2 More preferably, 2 g / m 2 More preferably, 4 g / m 2 More preferably, 15 g / m 2 Less than 10 g / m is more preferable. 2 The following is even more preferred: The gas barrier layer may be one layer or may be configured as two or more layers. When the gas barrier layer is configured as two or more layers, it is preferable that the total coating amount of all the gas barrier layers is within the above range.

[0028] (protective layer) The paper barrier material of the present invention can have a protective layer on at least one side. When a protective layer is provided on only one side, it is preferably provided on the side of the paper substrate that has the water vapor barrier layer. The protective layer can also be provided on both sides of the paper barrier material. The protective layer prevents deterioration of the water vapor barrier layer and gas barrier layer due to moisture in the air, etc., and can also impart additional water vapor barrier properties and gas barrier properties to the paper barrier material, or can impart oil resistance, solvent resistance, heat resistance, abrasion resistance, impact resistance, light resistance, etc. Furthermore, when the protective layer is a resin layer, it can also impart heat sealability. Examples of the protective layer include a resin layer, a paper layer, and a metal foil, and among these, a resin layer is preferred.

[0029] (Resin layer) Resins for the resin layer may include polyester resins (polyethylene terephthalate, polyethylene succinate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyvinyl alcohol resins, ethylene-vinyl acetate resins, polyolefin resins (polyethylenes such as LDPE and LLDPE, polypropylene, etc.), polystyrene resins, styrene-acrylate copolymer resins, (meth)acrylic resins, ethylene-acrylic resins, resins derived from fossil resources such as polyvinyl chloride, acrylonitrile-butadiene-styrene, acrylonitrile-styrene, polyvinylidene chloride, polyamide (nylon), polyacetal, and polycarbonate, as well as biological resins such as polylactic acid (PLA), esterified starch, cellulose acetate, polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), biopolyethylene, biopolyethylene terephthalate, and biopolyurethane. Among these, polyolefin resins, ethylene-vinyl acetate resins, styrene-acrylic acid ester copolymer resins, acrylic resins, and ethylene-acrylic resins are preferred from the viewpoint of heat seal strength. Also, biodegradable resins such as polyvinyl alcohol, polylactic acid, and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBH) are preferred from the viewpoint of reducing the environmental load when they are discharged as waste. Note that the term "biodegradable resin" refers to a polymer material with a number average molecular weight (Mn) of 1,000 or more, which is obtained by chemical or biological synthesis using renewable organic resource-derived substances as raw materials. Also, the term "biodegradable resin" refers to a resin that is decomposed to the molecular level by the action of microorganisms, and ultimately circulates into the natural world as carbon dioxide and water.

[0030] In the present invention, the resin layer is preferably a resin laminate layer. Examples of the resin laminate layer include an extrusion laminate layer and a film attachment layer such as a barrier film or a vapor deposition film. When the resin laminate layer is an extrusion laminate layer, the above-mentioned various resins are laminated as a resin laminate layer on at least one surface of the paper barrier material by an extrusion lamination method. When the resin laminate layer is a film attachment layer, the above-mentioned various resin films are attached as a resin laminate layer on at least one surface of the paper barrier material by a dry lamination method, a sand lamination method, or the like.

[0031] In the present invention, the film used for the film attachment layer may be any of the above-mentioned various resin films. Among these films, preferred are barrier films such as films mainly composed of resins such as polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinylidene chloride, polyacrylonitrile, etc., films made of the above-mentioned various resins coated with resins such as polyvinyl alcohol, films made of the above-mentioned various resins and laminated with metal foils made of various metals such as aluminum, and vapor deposition films made of the above-mentioned various resins and vapor-deposited with various metals such as aluminum or inorganic oxides such as silicon oxide and aluminum oxide, and more preferred are vapor deposition films. Depending on the purpose, one or more of these films may be laminated and used.

[0032] When the resin laminate layer is bonded by the dry lamination method, the adhesive can be any adhesive used in dry lamination without any particular restrictions, and for example, polyurethane-based (polyether-based polyol, polyester-based polyol, etc.), polyacrylic-based, polyester-based, epoxy-based, polyvinyl acetate-based, cellulose-based, etc. adhesives can be used, with polyurethane-based adhesives being preferred in terms of adhesive strength. In addition to the adhesive, a hardener, a solvent, etc. can also be blended into the adhesive layer. Among these, those that use water as a solvent are preferred in terms of reducing the emission of volatile organic compounds into the atmosphere and improving the hygienic working environment. The coating amount (solid content) of the adhesive layer is not particularly limited, but is preferably 2.0 g / m 2 More than 4.5g / m 2 The coating weight (solid content) of the adhesive layer is preferably 2.0 g / m or less.2 If the coating weight (solid content) of the adhesive layer is less than 4.5 g / m, the adhesion may be insufficient and gaps may occur. 2 If the coating rate exceeds this range, problems such as a decrease in the coating speed and drying speed, resulting in a decrease in productivity, a large amount of residual solvent causing odor, and an increase in the amount of material used, resulting in high costs, are likely to occur.

[0033] The paper barrier material of the present invention has a water vapor transmission rate of 0.1 g / m under conditions of 40°C and 90% RH. 2 ·day or more 15g / m 2 ·day or less. This water vapor permeability is preferably 14g / m 2 ·day or less is preferable, 13g / m 2 ·day or less is more preferable, and 12g / m 2 ・day or less is more preferable, 11g / m 2 ·day or less is even more preferable. In addition, the paper barrier material of the present invention having a gas barrier layer has an oxygen permeability of 0.1 cc / m under conditions of 23°C and 0% RH. 2 ·day · atm or more 15cc / m 2 The oxygen permeability is preferably 14cc / m 2 ·day·atm or less is preferable, 13cc / m 2 ·day·atm or less is even more preferable, 12cc / m 2 ·day·atm or less is even more preferable.

[0034] The paper barrier material of the present invention can be used as it is, or laminated with various resins, etc., or pasted with various general-purpose films, barrier films, aluminum foil, etc., to form paper packaging materials used for packaging applications such as packaging materials for food, containers, cups, etc., or packaging laminates used for industrial materials, etc. Among these, the paper barrier material of the present invention can be suitably used as paper packaging materials used for packaging applications such as packaging materials for food, containers, cups, etc., and can be particularly suitably used as soft packaging bags for food, etc. Note that a soft packaging bag is a packaging material composed of a material with high flexibility, and generally refers to a packaging material composed of thin, flexible materials such as paper, film, aluminum foil, etc., either alone or pasted together. The shape of the soft packaging bag is not particularly limited, and examples thereof include vertical pillow packaging bags, horizontal pillow packaging bags, side seal bags, two-sided seal bags, three-sided seal bags, four-sided seal bags, gusset bags, bottom gusset bags, and stand-up bags.

[0035] When the paper barrier material of the present invention is used as a packaging material for food and the like, in particular as a soft packaging bag, by laminating a resin having heat sealability as a protective layer, it is possible to improve the airtightness of the packaging material, protect the contents from oxidation by oxygen and deterioration due to moisture, etc., and extend the storage period. Furthermore, since soft packaging materials are thin and flexible, they are prone to bending during production, transportation, storage, sales, etc., but the paper barrier material of the present invention has excellent bending resistance and suppresses deterioration of the barrier properties even when bending occurs, so it is possible to prevent the quality of the contents from being damaged by unexpected bending. Furthermore, when used as a laminate for industrial materials, etc., it is possible to prevent putrefaction and deterioration by suppressing the intrusion of oxygen and moisture, and it is also expected to have effects such as flavor barrier properties that prevent the odor of solvents from leaking out. EXAMPLES

[0036] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, parts and % are by weight, respectively, unless otherwise specified. The obtained paper substrate, barrier base paper, and paper barrier material were tested according to the evaluation methods shown below. The results are shown in Table 1.

[0037] Pigments Expandable mica 1 Topy Industries, Ltd., NTS-10, average particle size 17μm, aspect ratio 1500 Expandable mica 2 Katakura Coop Agri Co., Ltd., ME300B-4T, average particle size 15 μm, aspect ratio 500 Montmorillonite Kunimine Industries Co., Ltd., Kunipia-F, average particle size 0.4 μm, aspect ratio 300 Non-swelling mica Kinsei Matec Co., Ltd., GP-1, average particle size 30μm, aspect ratio 40, natural mica

[0038] Polyvinyl alcohol PVA1 Manufactured by Japan Vinyl Acetate & Poval Co., Ltd., VC-10, polymerization degree 1000, saponification degree 99.3 or higher PVA2 Kuraray Co., Ltd., Kuraray Poval PVA117, polymerization degree 1700, saponification degree 98.0-99.0

[0039] Evaluation method <Water vapor permeability (water vapor barrier properties)> Measurements were performed using a PERMATRAN W3 / 34 manufactured by MOCON under conditions of 40°C and 90% RH. <Oxygen permeability (gas barrier properties)> Measurements were performed using OX-TRAN2 / 21 manufactured by MOCON under conditions of 23°C and 0% RH. The water vapor permeability and oxygen permeability were measured on the sheet sample as is (no creases) and on a sheet sample folded with the barrier layer side facing outwards to create a cross crease (creased) by rolling an approximately 400g rubber roller back and forth five times. For the folded sample, the measurement was performed so that the cross was positioned in the centre of the jig.

[0040] [Example 1] (Preparation of Paper Base 1) The raw material pulp was prepared by blending hardwood bleached kraft pulp (LBKP) with a Canadian standard freeness (CSF) of 500 ml and softwood bleached kraft pulp (NBKP) with a CSF of 530 ml in a weight ratio of 80 / 20. The raw pulp was mixed with 0.1% of polyacrylamide (PAM) with a molecular weight of 2.5 million as a dry strength agent, 0.35% of alkyl ketene dimer (AKD) as a sizing agent, 0.15% of polyamide epichlorohydrin (PAEH) resin as a wet strength agent, and 0.08% of polyacrylamide (PAM) with a molecular weight of 10 million as a retention agent, and then pulp was mixed with 0.1% of polyacrylamide (PAM) with a molecular weight of 2.5 million as a dry strength agent, based on the absolute dry pulp weight. The mixture was then spun at a speed of 300 m / min on a Fourdrinier papermaking machine (manufactured by Suzuki Seikisho Co., Ltd.) equipped with a Yankee dryer to produce a paper with a basis weight of 50 g / m. 2 Thus, a paper base material 1 was obtained.

[0041] (Preparation of coating solution for water vapor barrier layer) A polyurethane resin emulsion (Mitsui Chemicals, Inc., WPB-341, Tg 130°C) was blended into a slurry of swelling mica 1 so that the total amount of the water vapor barrier layer was 100 parts by weight, with 20 parts by weight of pigment and 80 parts by weight of polyurethane resin, to obtain a coating liquid for the water vapor barrier layer with a solids concentration of 22%. (Preparation of Coating Solution for Gas Barrier Layer) An aqueous solution of polyvinyl alcohol 1 with a solid content concentration of 12% was prepared and used as a coating liquid for the gas barrier layer.

[0042] (Preparation of paper barrier material 1) The coating solution for the water vapor barrier layer was applied to the surface of the obtained paper substrate that had come into contact with the mirror surface of the Yankee dryer (glossy surface) in a dry weight amount of 5.0 g / m 2 After coating and drying, a coating solution for the gas barrier layer was applied on top of the single-sided coating solution so that the dry weight was 4.0 g / m. 2 The paper barrier base paper was obtained by coating on one side so as to obtain the above. Furthermore, a film (Futamura Chemical Co., Ltd., LLDPE, thickness 30 μm) was applied onto the gas barrier layer of the obtained paper barrier base paper, and an adhesive (two-component curing polyurethane adhesive, curing agent: polyisocyanate, solvent: ethyl acetate) was applied in an amount (solid content) of 4.0 g / m 2 The sheets were laminated by dry lamination so as to obtain a paper barrier material.

[0043] [Example 2] (Preparation of paper barrier material 2) The coating amount of the water vapor barrier layer coating solution was 4.0 g / m 2 A paper barrier material 2 was obtained in the same manner as in Example 1, except for the above. [Example 3] (Preparation of paper barrier material 3) The coating amount of the coating solution for the water vapor barrier layer is 7.5 g / m 2 A paper barrier material 3 was obtained in the same manner as in Example 1, except for the above. [Example 4] (Preparation of paper barrier material 4) The coating amount of the gas barrier layer coating solution is 7.0 g / m 2 A paper barrier material 4 was obtained in the same manner as in Example 1, except for the above. [Example 5] (Preparation of Paper Barrier Material 5) A paper barrier material 5 was obtained in the same manner as in Example 1, except that 15 parts by weight of the pigment and 85 parts by weight of the polyurethane-based resin were mixed relative to 100 parts by weight of the total amount of the water vapor barrier layer. [Example 6] (Preparation of Paper Barrier Material 6) A paper barrier material 6 was obtained in the same manner as in Example 1, except that 30 parts by weight of the pigment and 70 parts by weight of the polyurethane-based resin were mixed relative to 100 parts by weight of the total amount of the water vapor barrier layer. [Example 7] (Preparation of Paper Barrier Material 7) Paper barrier material 7 was obtained in the same manner as in Example 1, except that PVA2 was used as the polyvinyl alcohol in the coating solution for the gas barrier layer. [Example 8] (Preparation of Paper Barrier Material 8) A paper barrier material 8 was obtained in the same manner as in Example 1, except that Swellable Mica 2 was used instead of Swellable Mica 1. [Example 9] (Preparation of Paper Barrier Material 9) A paper barrier material 9 was obtained in the same manner as in Example 1, except that the gas barrier layer coating liquid was not applied.

[0044] [Comparative Example 1] (Preparation of Paper Barrier Material 10) A paper barrier material 10 was obtained in the same manner as in Example 1, except that montmorillonite was used instead of the swelling mica 1. [Comparative Example 2] (Preparation of Paper Barrier Material 11) A paper barrier material 11 was obtained in the same manner as in Example 1, except that non-swelling mica was used instead of the swelling mica 1. [Comparative Example 3] (Preparation of Paper Barrier Material 12) A paper barrier material 12 was obtained in the same manner as in Example 1, except that 50 parts by weight of the pigment and 50 parts by weight of the polyurethane resin were mixed for a total of 100 parts by weight of the water vapor barrier layer. [Comparative Example 4] (Preparation of Paper Barrier Material 13) A paper barrier material 13 was obtained in the same manner as in Example 1, except that the coating liquid for the water vapor barrier layer was not applied. [Comparative Example 5] (Preparation of Paper Barrier Material 14) A paper barrier material 14 was obtained in the same manner as in Example 1, except that 40 parts by weight of the pigment and 60 parts by weight of the polyurethane resin were mixed relative to 100 parts by weight of the total amount of the water vapor barrier layer.

[0045] [Table 1]

[0046] The paper barrier materials obtained in Examples 1 to 9 had excellent water vapor barrier properties. Furthermore, the paper barrier materials obtained in Examples 1 to 8, which had a gas barrier layer, also had excellent gas barrier properties. In contrast, the paper barrier materials obtained in Comparative Examples 1 to 5 had high water vapor permeability values ​​and poor water vapor barrier properties. The paper barrier materials obtained in Comparative Examples 1 to 3 and 5 had water vapor permeability values ​​equivalent to the paper barrier material obtained in Comparative Example 4, which did not have a water vapor barrier layer, and from this it is presumed that the water vapor barrier properties of the paper barrier materials obtained in Comparative Examples 1 to 5 are derived from the LLDPE laminated thereto.

Claims

1. A water vapor barrier layer is provided on a paper substrate. the water vapor barrier layer contains a polyurethane resin and a swellable mica, 1. A paper barrier material comprising 65 parts by weight or more and 88 parts by weight or less of the polyurethane-based resin per 100 parts by weight of the total amount of the water vapor barrier layer.

2. The paper barrier material according to claim 1, characterized in that the polyurethane resin has a glass transition temperature of -20°C or higher and 150°C or lower.

3. 3. The paper barrier material according to claim 1 or 2, characterized in that the aspect ratio of the swellable mica is 300 or more.

4. 3. The paper barrier material according to claim 1 or 2, characterized in that the 50% volume average particle size of the swellable mica is 10 μm or more and 25 μm or less.

5. 3. The paper barrier material according to claim 1 or 2, characterized in that the water vapor barrier layer contains 5 parts by weight or more and 35 parts by weight or less of the swellable mica relative to 100 parts by weight of a total amount of the water vapor barrier layer.

6. The paper barrier material according to claim 1 or 2, characterized in that it has a gas barrier layer on the water vapor barrier layer.

7. The paper barrier material according to claim 6, characterized in that the gas barrier layer contains a water-soluble polymer.

8. The coating amount (dry weight) of the water vapor barrier layer is 3 g / m 2 8g / m or more 2 The coating amount (dry weight) of the gas barrier layer is 4 g / m 2 10g / m or more 2 7. The paper barrier material according to claim 6, characterized in that:

9. The water vapor transmission rate of the paper barrier material under conditions of 40°C and 90% RH is 0.1 g / m 2 ・15g / m for more than 1 day 2 3. The paper barrier material according to claim 1, wherein the resistance to moisture is less than or equal to 100 MPa.

Citation Information

Patent Citations

  • Barrier paper packaging material

    WO2013069788A1

  • Paper-made barrier material

    WO2017170462A1

Cited By

  • Laminated film and packaging film comprising the same

    JP2025174306A

  • Laminated film and packaging film comprising the same

    JP7836852B2

  • Laminated film and packaging film provided with same

    WO2025239057A1