Quantitative determination method of corrosion product

Neutron transmittance spectroscopy allows for the precise quantification of corrosion products on reinforcing bars by deriving and analyzing neutron spectra, addressing the limitations of narrow analysis ranges in existing methods and achieving comprehensive thickness measurements.

JP2024166771APending Publication Date: 2024-11-29SHIMIZU CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023083105
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing methods for quantifying corrosion products on reinforcing bars in concrete are limited to narrow analysis ranges and cannot accurately measure the depth of corrosion over a wide area.

Method used

A method utilizing neutron transmittance spectroscopy to derive and analyze the neutron transmittance spectrum of corrosion products, employing a corrosion product reagent to estimate the thickness of corrosion over a 100 μm range by raising the neutron transmittance spectrum to the nth power and fitting it to the spectral difference, incorporating regression analysis and the neutron Bragg edge analysis code RITS to calculate the thickness of iron and corrosion products.

Benefits of technology

Enables the quantification of corrosion products over a wide range on the reinforcing steel surface with a single measurement, providing accurate thickness measurements of both iron and corrosion products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166771000002
    Figure 2024166771000002
  • Figure 2024166771000003
    Figure 2024166771000003
  • Figure 2024166771000004
    Figure 2024166771000004
Patent Text Reader

Abstract

To provide a quantitative determination method for a corrosion product capable of quantifying the corrosion product on the surface of reinforcing steel over a wide range in a single measurement.SOLUTION: A method for quantifying a corrosion product of reinforcing steel in concrete comprises quantifying an amount of the corrosion product formed in the reinforcing steel by using neutron transmission spectra of the reinforcing steel and neutron transmission spectra of a substance identical to the corrosion product.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for quantifying corrosion products formed on reinforcing bars in concrete. [Background technology]

[0002] The quantitative determination of corrosion products occurring on reinforcing bars inside concrete is one of the typical deterioration phenomena of reinforced concrete. Research on reinforcing bar corrosion has been conducted for a long time. The amount of corrosion of reinforcing bars was usually measured by visually checking the corroded area on the reinforcing bar surface and measuring the mass change before and after removing the corroded area.

[0003] Conventionally, research on the mechanism of crack generation due to corrosion expansion of reinforcing bars has been known (see, for example, Non-Patent Document 1). Also, a method is known for clarifying the state of corrosion of reinforcing bars in mortar due to carbonation (see, for example, Non-Patent Document 2). Also, it is known to conduct microstructural and micromechanical investigations of reinforcing bar corrosion products by combining a scanning electron microscope, Raman spectroscopy, and nanoindentation (see, for example, Non-Patent Document 3). Furthermore, a method is known for estimating the amount of corrosion of reinforcing bars in concrete from crack width (see, for example, Non-Patent Document 4).

[0004] Thus, corrosion of reinforcing bars in concrete has been studied for many years using various approaches. However, there has been no research that has investigated corrosion products or corroded reinforcing bars using neutron transmittance spectra obtained by irradiating a sample with pulsed neutrons and the change in transmittance spectrum caused by polycrystalline diffraction of neutrons, known as the "Bragg edge" (see, for example, Non-Patent Document 5). [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Masayuki Morikawa et al.: Fundamental Study on the Mechanism of Crack Initiation Caused by Corrosion Expansion of Steel Bars, Journal of the Japan Society of Civil Engineers, Vol. 378 / V-6, pp. 97-105, February 1987. [Non-Patent Document 2] Tatsuhiko Saeki et al.: Quantitative evaluation of corrosion of rebar in mortar due to carbonation, Journal of Japan Society of Civil Engineers, No. 532 / V-30, pp. 55-66, February 1996. [Non-Patent Document 3] Baozhen Jianga et.al.: Micromechanical properties of steel corrosion products in concrete studied by nano-indentation technique, Corrosion Science 163 (2020), 108304. [Non-Patent Document 4] Yasuhiro Michimasa et al.: Study on Estimation of Rebar Corrosion from Rebar Corrosion Crack Width, Annual Papers of the Concrete Institute, vol.36, No.1, pp.1180-1185, 2014. [Non-Patent Document 5] Hirotaka Sato: Imaging of metal structure information by neutron transmission Bragg edge method, Materia, Vol. 55, No. 11, pp. 532-536, 2016. Summary of the Invention [Problem to be solved by the invention]

[0006] Although there are known methods for non-destructively analyzing localized corrosion products (e.g., microscopic Raman analysis), the analytical range is very narrow and it is not possible to quantify the depth of corrosion. Furthermore, with conventional methods for measuring the extent of corrosion in rebar, the range that can be measured at one time is very narrow, at around 1 μm.

[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for quantifying corrosion products that can quantify corrosion products over a wide range on the surface of reinforcing bars with a single measurement. [Means for solving the problem]

[0008] The present invention has the following aspects. [1] A method for quantifying corrosion products of reinforcing steel in concrete, comprising the steps of: A method for quantifying corrosion products, comprising quantifying the amount of corrosion products formed in the reinforcing bar using a neutron transmittance spectrum of the reinforcing bar and a neutron transmittance spectrum of a substance of the same quality as the corrosion products. [2] A step of deriving a neutron transmittance spectrum of a corrosion product equivalent to a thickness of 100 μm using a corrosion product reagent; Measuring the neutron transmittance spectrum of a reference reinforcing bar of the same quality as the reinforcing bar; Measuring the neutron transmittance spectrum of the reinforcing bar; Obtaining a difference between the neutron transmittance spectrum of the reference rebar and the neutron transmittance spectrum of the rebar; The method for quantifying corrosion products described in [1], further comprising a step of raising the neutron transmittance spectrum of the corrosion product to the nth power and fitting the result to the difference to estimate the thickness of the corrosion product on the surface of the reinforcing bar. [3] The method for quantifying corrosion products according to [2], wherein the corrosion product reagent is α-ferric oxidehydroxide or γ-ferric oxidehydroxide. [4] A method for quantifying corrosion products described in [1], comprising the steps of: performing regression analysis on the linear attenuation coefficient spectrum of the corrosion products to calculate functional data of the corrosion products; incorporating the functional data into the neutron Bragg edge analysis code RITS to analyze the neutron transmittance spectrum of the reinforcing bar; and deriving the thickness of the iron in the reinforcing bar and the thickness of the corrosion products, respectively. Effect of the Invention

[0009] According to the present invention, a method for quantifying corrosion products can be provided that can quantify corrosion products over a wide range on the surface of a reinforcing bar with a single measurement. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a diagram showing a neutron transmittance spectrum of α-ferric oxyhydroxide measured in an example. [Diagram 2]FIG. 1 is a diagram showing neutron transmittance spectra of a reinforcing bar and a reference reinforcing bar after electrolytic corrosion measured in an embodiment. [Diagram 3] FIG. 13 is a diagram showing the estimated thickness of corrosion products on the surface of a reinforcing bar in an embodiment. [Figure 4] FIG. 2 is a diagram showing the results of regression analysis of the linear attenuation coefficient spectrum of a corrosion product (iron hydroxide) in an example and calculation of function data of the corrosion product. [Diagram 5] FIG. 1 is a diagram showing the results of visualizing the thickness of corrosion products in reinforcing bars in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] An embodiment of a method for quantifying corrosion products according to one embodiment of the present invention will be described. It should be noted that the present embodiment is specifically described to allow a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified.

[0012] [Quantitative method for corrosion products] The method for quantifying corrosion products of this embodiment is a method for quantifying corrosion products of reinforcing bars inside concrete, and quantifies the amount of corrosion products produced in the reinforcing bars using a neutron transmittance spectrum of the reinforcing bars and a neutron transmittance spectrum of a material of the same nature as the corrosion products.

[0013] The method for quantifying corrosion products in this embodiment preferably includes the steps of: using a corrosion product reagent to derive a neutron transmittance spectrum of a corrosion product equivalent to a thickness of 100 μm (hereinafter referred to as the "first step"); measuring the neutron transmittance spectrum of a reference rebar of the same quality as the rebar (hereinafter referred to as the "second step"); measuring the neutron transmittance spectrum of the rebar (hereinafter referred to as the "third step"); determining the difference between the neutron transmittance spectrum of the reference rebar and the neutron transmittance spectrum of the rebar (hereinafter referred to as the "fourth step"); and raising the neutron transmittance spectrum of the corrosion product to the nth power and fitting to the difference to estimate the thickness of the corrosion product on the surface of the rebar (hereinafter referred to as the "fifth step").

[0014] "First step" In the first step, a neutron transmittance spectrum of corrosion products equivalent to a thickness of 100 μm in the reinforcing bar inside the concrete is derived using a corrosion product reagent. That is, the neutron transmittance spectrum of the corrosion product reagent is measured, and the neutron transmittance spectrum is regarded as equivalent to the neutron transmittance spectrum of corrosion products equivalent to a thickness of 100 μm in the reinforcing bar inside the concrete.

[0015] The corrosion product reagent used is α-ferric oxide hydroxide or γ-ferric oxide hydroxide, which correspond to the corrosion products generated by the corrosion of reinforcing bars. α-ferric oxide hydroxide is in the form of a fine powder with a purity of 99% and a density of 4.26 g / cm 3 The γ-ferric oxide hydroxide is in powder form, has a purity of 99%, and a density of 4.26 g / cm. 3 , with a formula mass of 88.9 is used.

[0016] An aluminum holder is filled with the corrosion product reagent, and a neutron irradiation device is used to measure the neutron transmittance spectrum of the corrosion product reagent. Specifically, the reagent is irradiated with white neutrons emitted from an accelerator-driven pulsed neutron source, and the neutron transmittance is calculated by subtracting the neutron count when there is no reagent from the count of neutrons that have passed through the reagent, and the neutron transmittance spectrum of the corrosion product reagent is measured by performing neutron wavelength analysis using the time-of-flight method. The negative natural logarithm of this is calculated, and multiplied by 100 / effective thickness (unit: μm). The neutron transmittance spectrum of the corrosion product reagent is calculated by calculating the negative exponential function of this.

[0017] In the measurement of the neutron transmittance spectrum, the electron energy is preferably 30 MeV or more. In measuring the neutron transmittance spectrum, the electron beam output is preferably 1 kW or more. In measuring the neutron transmittance spectrum, the electron beam pulse width is preferably 5 μs or less. In the measurement of the neutron transmittance spectrum, the neutron flight distance is preferably 5 m or more. In the measurement of the neutron transmittance spectrum, the direct beam measurement time is preferably one hour or more. In measuring the neutron transmittance spectrum, the sample measurement time is preferably 1 hour or more. In measuring the neutron transmittance spectrum, the distance between the sample and the detector is preferably 200 mm or less. The detector is preferably a pulsed neutron time-of-flight imaging detector.

[0018] "Second step" In the second step, a neutron irradiation device is used to measure the neutron transmittance spectrum of a reference rebar of the same quality as the rebar. Specifically, the reference rebar is irradiated with white neutrons emitted from an accelerator-driven pulsed neutron source, and the neutron transmittance is calculated by subtracting the neutron count without the reagent from the count of neutrons that have passed through the reference rebar. The neutron transmittance spectrum of the reference rebar is measured by performing neutron wavelength analysis using the time-of-flight method.

[0019] In the measurement of the neutron transmittance spectrum, the electron energy is preferably 30 MeV or more. In measuring the neutron transmittance spectrum, the electron beam output is preferably 1 kW or more. In measuring the neutron transmittance spectrum, the electron beam pulse width is preferably 5 μs or less. In the measurement of the neutron transmittance spectrum, the neutron flight distance is preferably 5 m or more. In the measurement of the neutron transmittance spectrum, the direct beam measurement time is preferably one hour or more. In measuring the neutron transmittance spectrum, the sample measurement time is preferably 1 hour or more. In measuring the neutron transmittance spectrum, the distance between the sample and the detector is preferably 200 mm or less. The detector is preferably a pulsed neutron time-of-flight imaging detector.

[0020] "The third step" In the third step, a neutron irradiation device is used to measure the neutron transmittance spectrum of the reinforcing bar. Specifically, the reinforcing bar is irradiated with white neutrons emitted from an accelerator-driven pulsed neutron source, and the neutron transmittance is calculated by subtracting the neutron count without the reagent from the count of neutrons that have passed through the reinforcing bar, and the neutron transmittance spectrum of the reinforcing bar is measured by performing neutron wavelength analysis using the time-of-flight method.

[0021] In the measurement of the neutron transmittance spectrum, the electron energy is preferably 30 MeV or more. In measuring the neutron transmittance spectrum, the electron beam output is preferably 1 kW or more. In measuring the neutron transmittance spectrum, the electron beam pulse width is preferably 5 μs or less. In the measurement of the neutron transmittance spectrum, the neutron flight distance is preferably 5 m or more. In the measurement of the neutron transmittance spectrum, the direct beam measurement time is preferably one hour or more. In measuring the neutron transmittance spectrum, the sample measurement time is preferably 1 hour or more. In measuring the neutron transmittance spectrum, the distance between the sample and the detector is preferably 200 mm or less. The detector is preferably a pulsed neutron time-of-flight imaging detector.

[0022] "The fourth step" In the fourth step, the difference between the neutron transmittance spectrum of the reference rebar obtained in the second step and the neutron transmittance spectrum of the rebar obtained in the third step is obtained. Specifically, the neutron transmittance spectrum of the reference rebar is subtracted from the neutron transmittance spectrum of the rebar to obtain the difference (hereinafter referred to as the "spectral difference") between the neutron transmittance spectrum of the reference rebar and the neutron transmittance spectrum of the rebar.

[0023] "The fifth step" In the fifth step, the neutron transmittance spectrum of the corrosion product is raised to the nth power and fitted to the spectral difference to estimate the thickness of the corrosion product on the surface of the rebar. Specifically, the thickness of the corrosion products on the surface of the reinforcing bar is estimated as follows. The neutron transmittance spectrum (T(λ)) is expressed by the following formula (1) using Lambert's law. T(λ)=exp(-σ(λ)nt) (1) In the above formula (1), T(λ) is the neutron transmission rate per neutron wavelength λ, and σ(λ) is the microscopic neutron total cross section (cm 2 ), n is the atomic density (cm -3 ), t is the thickness (cm). Moreover, the above formula (1) can be written as the following formula (2). T(λ)=exp(-Σ(λ)t) (2) In the above equation (2), Σ(λ) is the macroscopic neutron total cross section (cm -1 ), also known as the linear attenuation coefficient. From the above formula (2), it can be seen that raising the neutron transmittance spectrum (T(λ)) to the nth power is equivalent to multiplying the thickness t by n, as shown in the following formula (3). T(λ) n =exp(-Σ(λ)nt) (3) From this, the thickness of the corrosion product on the surface of the reinforcing bar can be estimated by raising the neutron transmittance spectrum of the corrosion product to the nth power and fitting it to the spectral difference. Specifically, n is determined manually or by computer so that the sum of the squares of the differences for each wavelength between the neutron transmittance spectrum of the corrosion product and the spectral difference is minimized.

[0024] "Other processes" In the method for quantifying corrosion products of this embodiment, the linear attenuation coefficient spectrum of the corrosion products is regression-analyzed to calculate the function data of the corrosion products, and the function data is incorporated into the neutron Bragg edge analysis code RITS to analyze the neutron transmittance spectrum of the reinforcing bar, and the thickness of the iron in the reinforcing bar and the thickness of the corrosion products are derived. In the neutron Bragg edge analysis code RITS, the neutron transmittance Bragg edge spectrum of iron is calculated from structural parameters such as the crystal structure, texture structure, and crystallite structure of iron and the thickness of the iron, and the neutron transmittance spectrum of the corrosion products can be calculated from the function and the parameters of the thickness of the corrosion products. The multiplication value of these two spectra is fitted to the neutron transmittance spectrum of the reinforcing bar by least squares fitting using a computer, and the structural parameters, the thickness of the iron, and the thickness of the corrosion products can be determined simultaneously. By performing this analysis on all pixels of the pulsed neutron time-of-flight analysis imaging detector, the structural parameters, the thickness of the iron, and the thickness of the corrosion products can be visualized. This makes it possible to visualize the thickness of the corrosion products.

[0025] According to the method for quantifying corrosion products of this embodiment, the neutron transmittance spectrum of the reinforcing bar and the neutron transmittance spectrum of a substance of the same nature as the corrosion products are used to quantify the amount of corrosion products produced in the reinforcing bar, so that the corrosion products on the surface of the reinforcing bar can be quantified over a wide range with a single measurement. EXAMPLES

[0026] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0027] [Example] "Derivation of neutron transmittance spectrum of corrosion products equivalent to a thickness of 100 μm" As a corrosion product reagent, α-ferric oxidehydroxide (fine powder, purity 99%, density 4.26 g / cm 3 The neutron transmittance spectrum of the corrosion products equivalent to a thickness of 100 μm in the reinforcing steel inside the concrete was derived using a neutron spectrometer (equivalently, formula weight 88.9, manufactured by Nilaco Corporation). The corrosion product reagent was filled into an aluminum holder, and the neutron transmittance spectrum of the corrosion product reagent was measured using a neutron irradiation device. In measuring the neutron transmittance spectrum, the electron energy was 32.4 MeV, the electron beam power was 2.3 kW, the electron beam pulse width was 4 μs, the neutron flight distance was 6.24 m, the direct beam measurement time was 2 hours, the sample measurement time was 2 hours, and the sample-to-detector distance was 8.6 mm. The detector used was a GEM type pulsed neutron time-of-flight imaging detector. The neutron transmission spectrum of α-ferric oxide hydroxide is shown in Figure 1.

[0028] "Preparation of electrolytic corrosion rebar" Mortar was prepared based on the mix shown in Table 1. In order to homogenize the effects of variations due to the type of aggregate, glass beads for sandblasting (particle size 1.5 mm) were used as the aggregate. The mortar was then poured into a steel formwork measuring 100 mm length x 200 mm width x 100 mm height, in which D6 deformed reinforcing bars were arranged, and the specimen was cured underwater for 28 days. The obtained specimen was subjected to electrochemical corrosion in accordance with a non-patent document (Tetsu Takatani et al.: Formation process and electrochemical characteristics of corrosion products of rebar in concrete, Journal of the Japan Society of Civil Engineers, Vol. 71, No. 3, pp. 235-247, 2015). The electrochemical corrosion density was 1.32 mA / cm 2 The elapsed time was set to three levels: 24 hours, 72 hours, and 120 hours.

[0029] [Table 1]

[0030] "Measurement of neutron transmittance spectra of reinforcing bars and reference bars" Using a neutron irradiation device, the neutron transmittance spectra of the above reinforcing bars and a reference reinforcing bar (a reinforcing bar that was not electrolytically corroded) of the same quality as the above reinforcing bars were measured. In measuring the neutron transmittance spectrum, the electron energy was 32.4 MeV, the electron beam power was 2.3 kW, the electron beam pulse width was 4 μs, the neutron flight distance was 5.92 m, the direct beam measurement time was 18.44 hours, the sample measurement time was 11.00 hours, and the sample-to-detector distance was 89 mm. The detector used was a GEM type pulsed neutron time-of-flight imaging detector. Figure 2 shows the neutron transmittance spectra of the reinforcing bar after electrical corrosion and the reference reinforcing bar.

[0031] "Estimation of thickness of corrosion products on the surface of reinforcing bars" First, the difference (spectral difference) between the neutron transmittance spectrum of the reference rebar obtained as described above and the neutron transmittance spectrum of the rebar after electrolytic corrosion was determined. Next, the neutron transmittance spectrum of the corrosion product (iron hydroxide) was raised to the nth power and fitted to the spectral difference to estimate the thickness of the corrosion product on the surface of the rebar. The results are shown in Figure 3. As shown in Figure 3, it is estimated that the thickness of the corrosion product is 1 μm when the electrolytic corrosion time is 24 hours, 150 μm when the electrolytic corrosion time is 72 hours, and 220 μm when the electrolytic corrosion time is 120 hours.

[0032] "Regression analysis of linear attenuation coefficient spectra of corrosion products" The linear attenuation coefficient spectrum of the corrosion product (iron hydroxide) was subjected to regression analysis to calculate the functional data of the corrosion product. The results are shown in Figure 4.

[0033] "Visualization of steel thickness and corrosion product thickness in reinforcing bars" The above-mentioned functional data of the corrosion products was incorporated into the neutron Bragg edge analysis code RITS to analyze the neutron transmittance spectrum of the rebar after electrolytic corrosion, and the thickness of the iron in the rebar after electrolytic corrosion and the thickness of the corrosion products were derived. The thickness of the corrosion products was visualized by analyzing the thickness of the iron in the rebar after electrolytic corrosion and the thickness of the corrosion products at all pixels. The results are shown in Figure 5. As shown in Figure 5, the thickness of the corrosion products can be visualized.

Claims

1. A method for quantifying corrosion products of reinforcing steel in concrete, comprising the steps of: A method for quantifying corrosion products, comprising quantifying the amount of corrosion products formed in the reinforcing bar using a neutron transmittance spectrum of the reinforcing bar and a neutron transmittance spectrum of a substance of the same quality as the corrosion products.

2. deriving a neutron transmittance spectrum of a corrosion product equivalent to a thickness of 100 μm using a corrosion product reagent; Measuring the neutron transmittance spectrum of a reference reinforcing bar of the same quality as the reinforcing bar; Measuring the neutron transmittance spectrum of the reinforcing bar; Obtaining a difference between the neutron transmittance spectrum of the reference rebar and the neutron transmittance spectrum of the rebar; The method for quantifying corrosion products according to claim 1, further comprising the step of raising the neutron transmittance spectrum of the corrosion products to the nth power and fitting the difference to estimate the thickness of the corrosion products on the surface of the reinforcing bar.

3. 3. The method for quantifying corrosion products according to claim 2, wherein the corrosion product reagent is α-ferric oxyhydroxide or γ-ferric oxyhydroxide.

4. 2. The method for quantifying corrosion products according to claim 1, further comprising the steps of: performing regression analysis on the linear attenuation coefficient spectrum of the corrosion products to calculate function data of the corrosion products; incorporating the function data into a neutron Bragg edge analysis code RITS to analyze the neutron transmittance spectrum of the reinforcing steel; and deriving the thickness of the iron in the reinforcing steel and the thickness of the corrosion products, respectively.