Method for manufacturing positive electrode active material
The described method enhances the rate characteristics of O2 type positive electrode active materials by controlling stirring power and dropping rates during coprecipitation, maintaining spherical particle shape, and ion-exchanging Na to Li, resulting in improved performance in secondary batteries.
Patent Information
- Application Number
- JP2023083145
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-19
AI Technical Summary
Positive electrode active materials with an O2 type structure have room for improvement in terms of rate characteristics.
A method involving coprecipitation to produce a precursor, followed by reaction with a Na source to form a P2-type structure, and then ion-exchanging Na to Li, with specific stirring power and dropping rate controls to achieve a spherical particle shape, and finally coating with a Na source to maintain the spherical form during firing.
The method produces a positive electrode active material with an O2 type structure that exhibits excellent rate characteristics, including improved reaction resistance and diffusion resistance, leading to enhanced performance in secondary batteries.
Smart Images

Figure 2024166799000001_ABST
Abstract
Description
[Technical field]
[0001] The present application discloses a method for producing a positive electrode active material. [Background technology]
[0002] Positive electrode active materials having an O2 type structure are known. As disclosed in Patent Document 1, a positive electrode active material having an O2 type structure is obtained by ion-exchanging at least a part of Na in a Na-containing oxide having a P2 type structure with Li. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-186937 A Summary of the Invention [Problem to be solved by the invention]
[0004] There is room for improvement in the rate characteristics of positive electrode active materials having an O2 structure. [Means for solving the problem]
[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A method for producing a positive electrode active material having an O2 type structure, comprising the steps of: Obtaining the precursor by coprecipitation; reacting the precursor with a Na source to obtain a Na-containing oxide having a P2 type structure; and At least a part of the Na in the Na-containing oxide is ion-exchanged with Li to obtain a Li-containing oxide having an O2 type structure; Including, The stirring power required during coprecipitation is 0.020 W or more and 0.200 W or less. Manufacturing method. <Aspect 2> The method for producing aspect 1, The dripping speed during coprecipitation is 4 ml / min or more and 20 ml / min or less. Manufacturing method. <Aspect 3> The method for producing aspect 1 or 2, The precursor comprises at least one element of Mn, Ni, and Co; Manufacturing method. <Aspect 4> In any one of the production methods of the first to third aspects, using an ion source capable of forming a precipitate in an aqueous solution together with transition metal ions, and a transition metal compound containing at least one element selected from Mn, Ni, and Co, to obtain a precipitate as the precursor by the coprecipitation method. Manufacturing method. <Aspect 5> The production method according to any one of aspects 1 to 4, Coating the surface of the precursor with a Na source to obtain a composite; and calcining the composite to obtain the Na-containing oxide; Including, The precursor is a spherical particle, The composite is obtained by covering 40% or more by area of the surface of the precursor with the Na source; and The Na-containing oxide is a spherical particle. Manufacturing method. Effect of the Invention
[0006] According to the method of the present disclosure, it is possible to produce a positive electrode active material having an O2 type structure and having excellent rate characteristics. [Brief description of the drawings]
[0007] [Figure 1] 1 shows an example of a process for producing a Na-containing oxide having an O2 type structure. [Diagram 2] 2 shows SEM photographs of the appearance of each precursor of Examples 1 and 2 and Comparative Examples 1 to 3. [Diagram 3]1 shows the relationship between the circularity of the precursor and the stirring power required during coprecipitation. [Figure 4] 2 shows SEM photographs of the appearance of the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] 1, a method for producing a positive electrode active material having an O2 type structure according to one embodiment includes obtaining a precursor by coprecipitation (S1), reacting the precursor with a Na source to obtain a Na-containing oxide having a P2 type structure (S2), and ion-exchanging at least a part of Na in the Na-containing oxide with Li to obtain a Li-containing oxide having an O2 type structure (S3). Here, the stirring power required during the coprecipitation is 0.020 W or more and 0.200 W or less.
[0009] 1.S1 In S1, a precursor is obtained by a coprecipitation method. The chemical composition of the precursor is not particularly limited, and depends on the chemical composition of the Na-containing oxide or Li-containing oxide described later. The precursor may contain at least one element of Mn, Ni, and Co, may contain at least Mn and one or both of Ni and Co, or may contain at least Mn, Ni, and Co. The precursor may be a salt containing at least one element of Mn, Ni, and Co. For example, the precursor may be at least one of carbonates, sulfates, nitrates, and acetates. Alternatively, the precursor may be a compound other than a salt. For example, the precursor may be a hydroxide. The precursor may be a hydrate. The precursor may be a combination of multiple types of compounds. The precursor may be, for example, particulate, or may be spherical particles as described later. The particle size of the particles made of the precursor is not particularly limited.
[0010] In S1, a precipitate as the precursor may be obtained by coprecipitation using an ion source capable of forming a precipitate in an aqueous solution with transition metal ions and a transition metal compound containing at least one element selected from Mn, Ni, and Co. This makes it easier to obtain spherical particles as the precursor. The "ion source capable of forming a precipitate in an aqueous solution with transition metal ions" may be at least one selected from sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, and sodium oxide. The transition metal compound may be the above salt or hydroxide containing at least one element selected from Mn, Ni, and Co. Specifically, in S1, the ion source and the transition metal compound may be prepared as solutions, and then the solutions may be dropped and mixed to obtain a precipitate as the precursor. In this case, for example, water is used as the solvent. In this case, various sodium compounds may be used as the base, and an aqueous ammonia solution or the like may be added to adjust the basicity. In S1, for example, an aqueous solution of a transition metal compound containing at least one element selected from Mn, Ni, and Co, and an aqueous solution of sodium carbonate are prepared, and each aqueous solution is dropped and mixed to obtain a precipitate as a precursor by a coprecipitation method.
[0011] According to the findings of the present inventors, when a precursor is obtained by a coprecipitation method, spherical particles as a precursor can be obtained more efficiently by controlling the dropping speed of the above aqueous solution and appropriately controlling the pH, etc. In this regard, in S1, it is preferable that the dropping speed during coprecipitation is 4 ml / min or more and 20 ml / min or less.
[0012] As described above, the precursor may be a spherical particle. In the present application, the term "spherical particle" refers to a particle having a circularity of 0.80 or more. The circularity of the particle may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the particle is 4πS / L 2Here, S is the orthogonal projected area of the particle, and L is the perimeter of the orthogonal projected image of the particle. The circularity of a particle can be determined by observing the appearance of the particle with a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope. When a particle is composed of more than 100 particles, the circularity is measured, for example, as an average value as follows.
[0013] (1) First, the particle size distribution of the particles is measured. Specifically, the particle size at 10% cumulative value (D10) and the particle size at 90% cumulative value (D90) in the volume-based particle size distribution are determined by a laser diffraction / scattering method. (2) Regarding the appearance of the particles whose particle size distribution has been measured, images are observed using a SEM, TEM, or optical microscope, and from the particles contained in the images, 100 particles having a circle equivalent diameter (the diameter of a circle having the same area as the orthogonal projected area of the particle) equal to or greater than D10 and equal to or less than D90 as determined in (1) are randomly selected. (3) The circularity of each of the 100 extracted particles is determined by image processing, and the average value is regarded as the "circularity of the particle."
[0014] In S1, the precursor may contain element M. Element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. These elements M have, for example, a function of stabilizing the P2 type structure. The method of obtaining a precursor containing element M is not particularly limited. When the precursor is obtained by coprecipitation in S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni, and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and each aqueous solution is dropped and mixed to obtain a precursor containing element M together with at least one element of Mn, Ni, and Co. Alternatively, in the manufacturing method of the present disclosure, element M may not be added in S1, and element M may be doped when Na-doping baking is performed in S2 and S3 described later.
[0015] In S1, it is important that the stirring power required during the coprecipitation (the stirring power required during the drop of the solution) is 0.020 W or more and 0.200 W or less. By having the stirring power required during the coprecipitation within a predetermined range, it becomes easier to obtain a precursor having an appropriate size and a spherical shape. The stirring power required may be 0.030 W or more, 0.040 W or more, or 0.050 W or more, or 0.180 W or less, 0.160 W or less, 0.140 W or less, 0.120 W or less, or 0.100 W or less.
[0016] "Required mixing power (hereinafter, P)" is the work done by the mixing blade on the solution per unit time (power: P (W)). The relationship for calculating the power is publicly known (power = force x speed), and the required mixing power P is similarly calculated as "required mixing power P = force applied to the mixer x rotation speed of the mixer." For example, the required mixing power P can be calculated from the following formula (I) described in Non-Patent Document 1 (Noboru Kamei, Setsuro Hiraoka, Yoshito Kato, Yutaka Tada, Yuki Shida, Young-se Lee, Takao Yamaguchi, Seung-tae Ko; Collection of Chemical Engineering Papers, 21, 41-48 (1995)). P=N p ρn 3 d 5 (I)
[0017] The above formula (I) can be interpreted as follows. Mixing power required P = force applied to mixer × rotation speed of mixer v Force acting on the stirrer = density of solution ρ × cross-sectional area of stirrer A × (rotation speed of stirrer v) 2 Cross-sectional area of the agitator A ∝ (blade diameter d) 2 Rotational speed of the agitator v = blade diameter d × rotational speed n Combining these, Mixing power required P ∝ ρd 2 (n.d.) 2 (nd)=ρn 3 d 5 (I') The above formula (I') is multiplied by the power number Np as a proportionality constant to obtain the above formula (I). The mixing power P is well known in the art, and the formula and each factor used to calculate the mixing power P are also well known. For each factor (e.g., power number Np) used to calculate the mixing power P, reference can be made to, for example, Non-Patent Document 2 (Edited by the Society of Chemical Engineers; Fundamentals and Applications of the Latest Mixing Technology (Advances in Chemical Engineering 42), Sankeisha (2008), 1. Basics), Non-Patent Document 3 (Edited by the Society of Chemical Engineers; Chemical Engineering Handbook Revised Seventh Edition, Maruzen (2011), I-6 Mixing and Mixing), and Non-Patent Document 4 (Yoshito Kato; Calculation and Experimental Methods for the Operation and Design of Mixing Vessels Revised and Supplemented Edition, Information Organization (2015), Chapter 5 Power Characteristics). For example, it is as follows.
[0018]
number
[0019]
number
[0020] In the above formula, n p : Number of blades (pieces), D: Reactor diameter (m), d: Blade diameter (m), b: Agitator blade width (m), θ: Agitator blade inclination angle (deg.), H: Liquid surface height (m), ρ: Liquid density (kg / m 3 ), n: Blade rotation speed (1 / s), μ: Liquid viscosity (Pa s), π: Pi, B w :Baffle plate width (m), n B : Number of baffle plates (pieces).
[0021] 2.S2 In S2, the precursor obtained in S1 is reacted with a Na source to obtain a Na-containing oxide having a P2 type structure. In one embodiment, S2 may include: coating a surface of the precursor with a Na source to obtain a composite (S2-1); and calcining the composite to obtain the Na-containing oxide (S2-2).
[0022] 2.1 S2-1 In S2-1, the surface of the precursor is coated with a Na source to obtain a composite. The Na source may be a salt containing Na, such as carbonate or nitrate, or a compound other than a salt, such as sodium oxide or sodium hydroxide. In S2-1, the amount of the Na source coated on the surface of the precursor may be determined taking into account the amount of Na lost during the subsequent calcination.
[0023] In S2-1, the coverage of the Na source on the surface of the precursor is not particularly limited. For example, in S2, the above-mentioned composite may be obtained by covering 40 area% or more, 50 area% or more, 60 area% or more, or 70 area% or more of the surface of the above-mentioned precursor with the Na source. Here, when the precursor obtained by S1 is a spherical particle, and the composite obtained by S2-1 is obtained by covering 40 area% or more of the surface of the precursor with the Na source, the Na-containing oxide having the P2 type structure is likely to become a spherical particle in S2-2 described later. If the coverage of the Na source is small, when the composite is fired, the P2 type crystal is likely to grow abnormally on the surface of the composite, and the Na-containing oxide is likely to become a plate-like. If the coverage of the Na source is large, when the composite is fired, the crystallites of the P2 type crystal are likely to become small, and the Na-containing oxide is likely to become a spherical particle corresponding to the shape of the precursor.
[0024] In S2-1, the method for coating the surface of the precursor with the Na source is not particularly limited. As described above, when 40% or more of the area of the surface of the precursor is coated with the Na source, various methods can be used. For example, a tumbling fluidized coating method and a spray drying method can be used. That is, a coating solution in which a Na source is dissolved is prepared, and the coating solution is brought into contact with the surface of the precursor, and dried at the same time or after the contact. By adjusting the coating conditions (temperature, time, number of times, etc.), 40% or more of the area of the surface of the precursor can be coated with the Na source.
[0025] In S2-1, the precursor may be coated with an M source together with a Na source. For example, in S2-1, the precursor obtained in S1, a Na source, and an M source containing at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W may be mixed to obtain a composite. The M source may be, for example, a salt containing the element M, such as a carbonate or sulfate, or a compound other than a salt, such as an oxide or hydroxide. The amount of the M source relative to the precursor may be determined according to the chemical composition of the Na-containing oxide after firing.
[0026] 2.2 S2-2 In S2-2, the composite obtained in S2-1 is fired to obtain a Na-containing oxide having a P2 type structure. In S2-2, the composite may be optionally molded, optionally pre-fired, and then finally fired.
[0027] The pre-firing of the composite may be performed at a temperature equal to or lower than that of the main firing. For example, the pre-firing may be performed at a temperature lower than 700°C. The pre-firing time is not particularly limited. The pre-firing atmosphere is also not particularly limited. The pre-firing atmosphere may be the same as or different from the main firing atmosphere.
[0028] The sintering of the composite may be carried out at a temperature of, for example, 700° C. or more and 1100° C. or less. It is preferably 800° C. or more and 1000° C. or less. If the sintering temperature is too low, Na doping is not performed, and if the sintering temperature is too high, phases other than the P2 phase are likely to be formed. The temperature rise conditions from the preliminary sintering temperature to the sintering temperature are not particularly limited.
[0029] The firing time is not particularly limited, and may be, for example, 30 minutes or more and 48 hours or less. However, the shape of the Na-containing oxide can be controlled by the firing time. As described above, in the method of the present disclosure, when the coverage rate of the Na source in the composite is 40 area % or more, when the composite is fired, a P2 type crystal with small crystallites is easily formed on the surface. In this embodiment, the shape of the Na-containing oxide corresponds to the shape of the precursor by growing the P2 type crystal along the surface of the particle so that one P2 type crystallite and another P2 type crystallite are connected to each other. For example, when the precursor is a spherical particle, the Na-containing oxide can also be a spherical particle. If the firing time is too short, Na doping is not performed and the desired P2 type structure is not obtained. On the other hand, if the firing time is too long, the P2 type structure grows excessively, resulting in plate-like particles rather than spherical ones. As far as the present inventors have confirmed, if the firing time is 30 minutes or more and 3 hours or less, spherical particles of the Na-containing oxide are easily obtained. The Na-containing oxide obtained after the main firing may have a structure in which a plurality of crystallites are present on the surface and the crystallites are connected to each other.
[0030] The firing atmosphere is not particularly limited, and may be, for example, an oxygen-containing atmosphere such as air atmosphere, or an inert gas atmosphere.
[0031] 3.S3 In S3, at least a part of Na in the Na-containing oxide obtained in S2 is ion-exchanged with Li to obtain a Li-containing oxide having an O2 type structure. In S3, Na in the Na-containing oxide particles can be ion-exchanged with Li by contacting the Na-containing oxide with an ion exchange material.
[0032] Examples of the ion exchange material include a mixture (e.g., a molten salt) of a lithium halide and another lithium salt. The lithium halide constituting the molten salt is preferably at least one of lithium chloride, lithium bromide, and lithium iodide. The other lithium salt constituting the molten salt is preferably lithium nitrate. By using a molten salt, the melting point becomes lower than when a lithium halide or another lithium salt is used alone, and ion exchange can be performed at a lower temperature. The temperature in the ion exchange is from the melting point of the ion exchange material to 300°C. If the ion exchange temperature is too high, the stable phase O3 type structure is likely to be formed instead of the O2 type structure. On the other hand, from the viewpoint of shortening the ion exchange time, the ion exchange temperature is preferably as high as possible. The ion exchange time is 30 minutes or more and less than 3 hours. If the ion exchange time is too short, the amount of remaining Na in the Li-containing oxide particles increases. On the other hand, if the ion exchange time is too long, the O3 type structure and the like are likely to be formed together with the O2 type structure.
[0033] 4. Positive electrode active material with O2 structure By the above steps S1 to S3, a Li-containing oxide having an O2 type structure can be produced as a positive electrode active material. Hereinafter, a Li-containing oxide according to one embodiment will be described.
[0034] 4.1 Crystal structure The Li-containing oxide according to an embodiment has at least an O2-type structure (belonging to space group P63mc) as a crystal structure. The Li-containing oxide according to an embodiment has an O2-type structure and may have a crystal structure other than the O2-type structure. Examples of crystal structures other than the O2-type structure include a T♯2-type structure (belonging to space group Cmca) and an O6-type structure (belonging to space group R-3m, with a c-axis length of 2.5 nm to 3.5 nm, typically 2.9 nm to 3.0 nm, and different from the O3-type structure also belonging to space group R-3m) formed when Li is deintercalated from the O2-type structure. The Li-containing oxide according to an embodiment may have an O2-type structure as a main phase, or may have a structure other than the O2-type structure as a main phase. The Li-containing oxide according to an embodiment may have one or both of a T♯2-type structure and an O6-type structure together with the O2-type structure. The crystal structure of the Li-containing oxide as a main phase may change depending on the charge / discharge state.
[0035] The Li-containing oxide according to an embodiment may be polycrystalline having a plurality of crystallites. For example, the Li-containing oxide according to an embodiment may have a surface formed of a plurality of crystallites. In other words, the Li-containing oxide may have a structure in which a plurality of crystallites are connected to each other on the surface. When the surface of the Li-containing oxide is formed of a plurality of crystallites, a crystal grain boundary is present on the surface. Here, the crystal grain boundary may be an inlet and an outlet of intercalation. That is, when the Li-containing oxide is polycrystalline having a plurality of crystallites, the effect of increasing the number of inlets and outlets of intercalation and decreasing the reaction resistance, the effect of shortening the distance of movement of lithium ions and decreasing the diffusion resistance, the effect of reducing the absolute amount of expansion and contraction during charging and discharging and making it difficult for cracks to occur, and the like can be expected. The size of the crystallites may be large or small, but it is considered that the smaller the size of the crystallites, the more the crystal grain boundaries will be, and the more likely the above-mentioned advantageous effects will be exhibited. For example, when the diameter of the crystallites constituting the Li-containing oxide is less than 1 μm, higher performance is likely to be obtained. The "crystallite" and "diameter of the crystallite" can be determined by observing the surface of the Li-containing oxide with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, when the surface of the Li-containing oxide is observed and a closed region surrounded by a grain boundary is observed, the region is regarded as a "crystallite". The maximum Feret diameter of the crystallite is determined and regarded as the "diameter of the crystallite". If the Li-containing oxide is composed of a single crystal, the particle itself can be said to be a single crystallite, and the maximum Feret diameter of the particle is the "diameter of the crystallite". Alternatively, the diameter of the crystallite can be determined by EBSD or XRD. For example, the diameter of the crystallite can be determined based on the Scherrer formula from the half-width of the diffraction line of the XRD pattern. If the diameter of the crystallite of the Li-containing oxide specified by any method is less than 1 μm, the performance of the Li-containing oxide is likely to be higher.
[0036] 4.2 Chemical composition The Li-containing oxide according to one embodiment may contain, as constituent elements, at least one element selected from Mn, Ni, and Co, Li, and O. In particular, when the constituent elements contain at least Li, Mn, one or both of Ni and Co, and O, and especially when the constituent elements contain at least Li, Mn, Ni, Co, and O, higher performance is likely to be obtained. The Li-containing oxide according to one embodiment may contain Li. a Na b Mn x-p Ni y-q Co z-r M p+q+rIt may have a chemical composition represented by O2 (where 0 < a ≤ 1.00, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). When the Li-containing oxide has such a chemical composition, the O2-type structure is likely to be maintained. In the above chemical composition, a is greater than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, or 0.70 or less. In the above chemical composition, b is 0 or more, and may be 0.01 or more, 0.02 or more, or 0.03 or more, and is at most 0.20, and may be 0.15 or less, or 0.10 or less. Also, x is 0 or more, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y is 0 or more, and may be 0.10 or more, or 0.20 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Also, z is 0 or more, and may be 0.10 or more, or 0.20 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The element M has a small contribution to charge and discharge. In this regard, in the above chemical composition, when p + q + r is less than 0.17, a high charge and discharge capacity is likely to be ensured. p + q + r may be 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. On the other hand, when the element M is included, the O2-type structure is likely to be stabilized. In the above chemical composition, p + q + r is 0 or more, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more.The composition of O is approximately 2, but is not necessarily exactly 2.0 and is variable.
[0037] 4.3 Shape The P2 type structure before ion exchange is a hexagonal system, has a large diffusion coefficient of Na ions, and is likely to grow crystals in a specific direction. In particular, when at least one of Mn, Ni, and Co is included as a transition metal element constituting the P2 type structure, the crystals are likely to grow in a plate-like shape in a specific direction. Therefore, the Na-containing oxide having the P2 type structure usually becomes a plate-like particle with a large aspect ratio in which the crystal growth direction is biased in a specific direction, and when ion exchange is performed using such a plate-like particle, the Li-containing oxide having the O2 type structure also becomes plate-like. In contrast, the Na-containing oxide according to one embodiment may be a spherical particle as described above, and the Li-containing oxide after ion exchange may also be a spherical particle. When the Li-containing oxide is a spherical particle, the reaction resistance decreases due to the reduction in crystallite size, and the diffusion resistance inside the particle is likely to decrease. Furthermore, when applied to a secondary battery or the like, it is considered that the degree of bending is reduced by spheroidization, and the lithium ion conduction resistance is reduced. As a result, for example, the rate characteristic is improved and the reversible capacity is likely to increase. The Li-containing oxide according to an embodiment may be a solid particle, a hollow particle, or a particle having a void. The size of the Li-containing oxide particles is not particularly limited, but it is considered that a smaller size is more advantageous. For example, the average particle diameter (D50) of the Li-containing oxide particles may be 0.1 μm or more and 10 μm or less, 1.0 μm or more and 8.0 μm or less, or 2.0 μm or more and 6.0 μm or less. The average particle diameter (D50) is a particle diameter (D50, median diameter) at an integrated value of 50% in a volume-based particle size distribution by a laser diffraction / scattering method. EXAMPLES
[0038] As described above, one embodiment of the manufacturing method of the positive electrode active material (Li-containing oxide) having an O2 type structure has been described, but the manufacturing method of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the present disclosure. Below, the technology of the present disclosure will be described in more detail while showing examples, but the technology of the present disclosure is not limited to the following examples.
[0039] 1. Preparation of Positive Electrode Active Material 1.1 Preparation of precursor (1) MnSO4·5H2O, NiSO4·6H2O, and CoSO4·7H2O were weighed out to obtain the desired composition ratio, and dissolved in distilled water to obtain the desired concentration to obtain solution 1. In a separate container, Na2CO3 was dissolved in distilled water to obtain the desired concentration to obtain solution 2. (1-1) In Example 1 and Comparative Examples 1 to 3, the concentrations of the first and second solutions were both set to 1.2 mol / L. (1-2) In Example 2, the concentrations of the first solution and the second solution were both set to 2.0 mol / L. (2) Pure water was placed in a reaction vessel, and the first solution and the second solution were added dropwise thereto at a predetermined rate. (2-1) In Example 1 and Comparative Examples 1 to 3, 1000 mL of pure water was placed in a 4 L reaction vessel, and 500 mL of the first solution and 500 mL of the second solution were dropped into the vessel at a rate of 4.17 mL / min. The design of the stirring blades in the reaction vessel and the stirring speed were changed to change the stirring power required during the dropping. Specifically, the stirring power required in Example 1 was 0.086 W, the stirring power required in Comparative Example 1 was 0.015 W, the stirring power required in Comparative Example 2 was 0.203 W, and the stirring power required in Comparative Example 3 was 0.685 W. (2-2) In Example 2, 2500 mL of pure water was placed in a 9 L reaction vessel, and 2250 mL of the first solution and 2250 mL of the second solution were dropped into the vessel at a rate of 18.75 mL / min. The design of the stirring blades in the reaction vessel and the stirring speed were adjusted so that the stirring power required during the dropping was 0.054 W. (3) After the dropwise addition was completed, the mixture was stirred at room temperature at a stirring speed of 150 rpm for 1 hour to obtain a product. (4) The product was washed with pure water, subjected to solid-liquid separation using a centrifuge, and the precipitate was collected. (5) The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and then the fine particles were removed by air classification to obtain a precursor.
[0040] 1.2 Appearance observation by SEM FIG. 2 shows SEM photographs of the appearance of the precursors of Examples 1 and 2 and Comparative Examples 1 to 3. FIG. 3 shows the relationship between the circularity of the precursor and the required stirring power. As shown in FIGS. 2 and 3, in Examples 1 and 2, spherical precursors with a circularity of 0.80 or more were obtained, whereas in Comparative Examples 1 to 3, non-spherical precursors with a small particle size and a circularity of 0.60 or less were obtained. In Comparative Example 1, the required stirring power in the liquid phase synthesis of the precursor was too small, which is considered to have caused insufficient stirring and inhibited the particle growth of the precursor. In Comparative Examples 2 and 3, the required stirring power in the liquid phase synthesis of the precursor was too large, which is considered to have caused excessive stirring and collapsed the particles of the precursor.
[0041] 1.3 Preparation of the complex (1) Na2CO3 as a Na source and the above precursor are mixed, and the composition after calcination described below is Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 It was weighed to be O2. (2) The weighed Na source and precursor were mixed by spray drying. Specifically, the weighed Na source and precursor were added to a solvent, and the dispersion solution in which the Na source was dissolved and the precursor was dispersed was spray dried. The spray drying temperature was 200°C, and the spray pressure was 0.3 MPa. A composite in which 75% or more of the surface area of the precursor was covered with the Na source was obtained by spray drying.
[0042] 1.4 Firing of the composite The composite was placed in an alumina crucible and sintered in an air atmosphere under the following conditions (1) to (5). (1) The alumina crucible containing the above composite is placed in a heating furnace. (2) The temperature inside the heating furnace is increased from room temperature to 600°C. (3) The temperature in the heating furnace is kept at 600°C for six hours to perform pre-firing (preliminary firing). (4) The temperature inside the heating furnace is increased from 600°C to 900°C. (5) The temperature in the heating furnace is kept at 900°C for one hour to carry out the main firing. (6) After the main firing, the temperature inside the heating furnace is lowered from 900°C to 250°C over a period of 2 hours and 20 minutes. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool in the air.
[0043] The fired product after cooling in the air was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles having a P2 type structure. 0.7 Mn 0.5 Ni 0.2 Co 0.3 It had a chemical composition indicated as O2.
[0044] 1.5 Ion exchange (1) LiNO3 and LiCl were weighed out to have a molar ratio of 50:50, and mixed with the above-mentioned Na-containing oxide particles in a molar ratio that was 10 times the minimum Li amount required for ion exchange to obtain a mixture. (2) Using an alumina crucible, ion exchange was carried out at 280°C for 1 hour in an air atmosphere to obtain a product containing Li-containing oxide particles. (3) The salt remaining in the product was washed with pure water, and solid-liquid separation was performed by vacuum filtration to obtain a precipitate. (4) The obtained precipitate was dried overnight at 120° C. to obtain a positive electrode active material.
[0045] 2. Evaluation of positive electrode active material 2.1 Identification of crystal structure by X-ray diffraction measurement For each of the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 to 3, X-ray diffraction measurements were performed using CuKα as a radiation source to obtain X-ray diffraction patterns and identify the crystal structures. As a result, each of the positive electrode active materials had an O2 type crystal structure.
[0046] 2.2 Appearance observation by SEM FIG. 4 shows SEM photographs of the appearance of the positive electrode active materials according to each of Examples 1 and 2 and Comparative Examples 1 to 3. From FIG. 4, it can be seen that the positive electrode active materials according to Examples 1 and 2 are spherical particles having a circularity of 0.80 or more, while the positive electrode active materials according to Comparative Examples 1 to 3 are non-spherical particles. It can also be seen that the surface of the positive electrode active materials according to Examples 1 and 2 is composed of a plurality of crystallites, and the diameter of the crystallites is less than 1 μm. On the other hand, it can be seen that the positive electrode active materials according to Comparative Examples 1 to 3 have a structure in which plate-like single crystals are aggregated and turned into secondary particles, or a structure in which spherical particles are bonded to each other and turned into secondary particles. As described above, in Comparative Examples 1 to 3, since the Na-containing oxide was synthesized using a precursor having a small particle diameter and a non-spherical shape, the Na-containing oxide was also non-spherical, and as a result, it is considered that the positive electrode active material was also non-spherical. It is to be noted that, in Comparative Example 1, a large amount of plate-like primary particles were aggregated, and the circularity could not be measured.
[0047] 3. Preparation of evaluation cells Coin cells were produced using the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 to 3. The coin cells were produced as follows. (1) The positive electrode active material, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder were weighed out so that the mass ratio of the positive electrode active material:AB:PVdF=85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode mixture slurry. The positive electrode mixture slurry was applied onto an aluminum foil and vacuum dried overnight at 120°C to obtain a positive electrode, which is a laminate of a positive electrode active material layer and a positive electrode current collector. (2) TDDK-217 (manufactured by Daikin Industries, Ltd.) was prepared as the electrolyte. (3) Metallic lithium foil was prepared as the negative electrode. (4) A coin cell (CR2032) was prepared using the positive electrode, electrolyte, and negative electrode.
[0048] 4.Charge / Discharge Characteristics Evaluation Each coin cell was charged and discharged at 0.1C (1C=220mA / g) in a voltage range of 2.0-4.8V in a thermostatic chamber maintained at 25°C, and the discharge capacity was measured. Each coin cell was also charged at 0.1C in a voltage range of 2.0-4.8V in a thermostatic chamber maintained at 5°C, and discharged at 0.5C, 1C, or 3C, and the discharge capacity at each rate was measured. The ratio of the discharge capacity at each rate to the discharge capacity at 0.1C was calculated to evaluate the rate characteristics. The results are shown in Table 1 below.
[0049] [Table 1]
[0050] As shown in Table 1, the coin cells of Examples 1 and 2 have a larger discharge capacity than the coin cells of Comparative Examples 1 to 3, and the difference between the capacity during low-rate discharge and the capacity during high-rate discharge is small, meaning that a large capacity can be maintained even during high-rate discharge.
[0051] 4. Supplementary Information In the above examples, the surface of the precursor is coated with a Na source by spray drying to obtain a composite, but the composite can be obtained by other methods. In the above examples, the Na-containing oxide having a P2 type structure and the positive electrode active material having an O type structure are exemplified as having a predetermined chemical composition, but the chemical composition is not limited thereto, and various chemical compositions can be adopted. In addition, the positive electrode active material may be doped with an element M other than Mn, Ni, and Co. The element M is as described in the embodiment.
[0052] 5. Summary As described above, according to the method for producing a positive electrode active material having an O2 type structure, which includes the following S1 to S3, a positive electrode active material having excellent rate characteristics can be produced. S1: Obtaining a precursor by a coprecipitation method, where the stirring power required during coprecipitation is 0.020 W or more and 0.200 W or less. S2: Reacting the precursor with a Na source to obtain a Na-containing oxide having a P2 type structure. S3: At least a part of the Na in the Na-containing oxide is ion-exchanged with Li to obtain a Li-containing oxide having an O2 type structure.
Claims
1. A method for producing a positive electrode active material having an O2 type structure, comprising the steps of: Obtaining the precursor by coprecipitation; reacting the precursor with a Na source to obtain a Na-containing oxide having a P2 type structure; and At least a part of the Na in the Na-containing oxide is ion-exchanged with Li to obtain a Li-containing oxide having an O2 type structure; Including, The stirring power required during coprecipitation is 0.020 W or more and 0.200 W or less. Manufacturing method.
2. The method according to claim 1, The dropping speed during coprecipitation is 4 ml / min or more and 20 ml / min or less. Manufacturing method.
3. The method according to claim 1, The precursor comprises at least one element of Mn, Ni, and Co; Manufacturing method.
4. The method according to claim 1, obtaining a precipitate as the precursor by the coprecipitation method using an ion source capable of forming a precipitate in an aqueous solution together with transition metal ions and a transition metal compound containing at least one element selected from Mn, Ni, and Co. Manufacturing method.
5. The method according to any one of claims 1 to 4, Coating the surface of the precursor with a Na source to obtain a composite; and calcining the composite to obtain the Na-containing oxide; Including, The precursor is a spherical particle, The composite is obtained by covering 40% by area or more of the surface of the precursor with the Na source; and The Na-containing oxide is a spherical particle. Manufacturing method.
Citation Information
Patent Citations
Positive electrode active material for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery arranged by use thereof
JP2014186937A
Cathode active material and producing method thereof, and lithium secondary battery including the same
JP2021177491A
Method for producing positive electrode active material
JP2022097885A
Rechargeable battery with nonaqueous electrolyte, method for producing rechargeable battery with nonaqueous electrolyte, and method for using rechargeable battery with nonaqueous electrolyte
WO2020090678A1
Cited By
Positive electrode material, electrochemical device, and electronic device
WO2026207674A1