Chemically strengthened glass, production method therefor, and glass

A two-stage ion exchange process for chemically strengthened glass optimizes stress profiles to enhance set drop strength and impact resistance by reducing tensile stress below the CT limit, addressing the limitations of conventional technologies.

JP2024166883AInactive Publication Date: 2024-11-29AGC INC

Patent Information

Application Number
JP2023083281
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional chemically strengthened glass technologies face limitations in achieving high set drop strength while avoiding the CT limit, leading to potential explosive fractures and increased fragmentation upon impact.

Method used

A two-stage ion exchange process is employed, where chemically strengthened glass is first treated with a first molten salt composition to introduce alkali metal ions, followed by a second treatment with a different molten salt composition to enhance compressive stress and reduce tensile stress, resulting in specific stress profiles that maximize set drop strength without exceeding the CT limit.

Benefits of technology

The method produces glass with enhanced set drop strength, reduced surface layer compressive stress, and suppressed internal tensile stress, achieving superior impact resistance and fracture resistance compared to conventional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166883000011
    Figure 2024166883000011
  • Figure 2024166883000012
    Figure 2024166883000012
  • Figure 2024166883000013
    Figure 2024166883000013
Patent Text Reader

Abstract

To provide a chemically strengthened glass, a production method therefor, and a glass in which CS90 is maximized and excellent set drop strength is achieved.SOLUTION: The present invention relates to: a chemically strengthened glass having a sheet thickness t (mm), a compressive stress layer depth DOC of 180×t (μm) or more, CS30-50 which is a compressive stress integrated value at a depth of 30 μm to 50 μm from a surface of the chemically strengthened glass of 12000 Pa m or less, and CS90 which is a compressive stress value at a depth of 90 μm from the surface of 175×t-88 (MPa) or more; a chemically strengthened glass having a surface resistivity logρ of 10 logΩ / sq or less, and a Young's modulus of 80 GPa or more; and a chemically strengthened glass having a value obtained by dividing an Na2O concentration at a depth of 30 μm from a surface of the chemically strengthened glass by an Na2O concentration at a depth of 90 μm from the surface of 1.30 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a chemically strengthened glass, a method for producing the same, and the glass. [Background technology]

[0002] Chemically strengthened glass is used for cover glass of electronic device terminals such as computers, smartphones, and tablets. Chemically strengthened glass is formed by forming a compressive stress layer on the surface of the glass by an ion exchange treatment in which the glass is brought into contact with a molten salt composition such as sodium nitrate or potassium nitrate. In the ion exchange treatment, ion exchange occurs between the alkali metal ions contained in the glass and the alkali metal ions having a larger ionic radius than those contained in the molten salt composition, and a compressive stress layer is formed on the surface of the glass.

[0003] The strength of chemically strengthened glass depends on the stress profile, which is expressed by compressive stress (hereinafter also abbreviated as CS), with the depth from the glass surface as a variable. When ion exchange treatment is performed in two or more stages, the compressive stress layer is formed of a "surface compressive stress layer" formed mainly by the introduction of potassium ions and the like into the glass, and a "deep compressive stress layer" formed mainly by the introduction of sodium ions and the like into the glass.

[0004] On the other hand, when a compressive stress layer is formed on the surface of glass, a tensile stress (hereinafter abbreviated as CT) corresponding to the total amount of compressive stress is inevitably generated in the center of the glass. If the CT value becomes too large, the glass product will break violently and fragments will scatter when broken. If the CT value exceeds the threshold value (hereinafter abbreviated as CT limit), the glass will break on its own and the number of fractures when damaged may increase explosively. The CT limit is a value specific to the glass composition.

[0005] Therefore, in chemically strengthened glass, the surface compressive stress is increased and a compressive stress layer is formed in a deeper portion, while the total amount of compressive stress in the surface layer is designed so as not to exceed the CT limit. For example, Patent Document 1 discloses chemically strengthened glass in which the CT is controlled within a specific range. Patent Document 2 discloses chemically strengthened glass having specific ranges of CS and DOC. Patent Document 3 discloses chemically strengthened glass in which the total amount of compressive stress is equal to or less than a certain value.

[0006] The sandpaper set drop strength test is one of the indices for evaluating the strength of glass-based materials used in smartphones. In the sandpaper set drop strength test, a sample made by bonding a smartphone case or a mock board simulating a smartphone to a glass-based material is dropped onto sandpaper of #60 to #200, and the drop height at which cracks occur (hereinafter abbreviated as "crack height" or "set drop strength") is used as an index of strength. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] U.S. Patent No. 9,359,251 [Patent Document 2] U.S. Pat. No. 10,150,698 [Patent Document 3] International Publication No. 2018 / 186402 Summary of the Invention [Problem to be solved by the invention]

[0008] CS, the compressive stress value at a depth of 90 μm 90 If CS is increased, a stress profile will be created in which a large compressive stress is formed at a depth of, for example, 90 μm, and it will be possible to prevent fracture due to impact with a relatively large protrusion. 90 As shown in Figure 1, CS shows a high correlation with the set drop strength. Therefore, in order to develop glasses with higher set drop strength, 90It is necessary to increase the value of

[0009] For example, U.S. Patent No. 10,730,791 discloses that deep layer stress can be improved by diffusing Na ions as deep as possible near the center of the plate thickness and increasing CT. However, as mentioned above, increasing CT causes the glass to self-destruct and the number of fractures when damaged increases explosively, so there is a CT limit. Therefore, the set drop strength is insufficient with conventional technology, and in order to further improve the set drop strength, a higher CS 90 There is a demand for chemically strengthened glass having the above properties.

[0010] Therefore, the present invention provides a method for producing a CS 90 An object of the present invention is to provide a chemically strengthened glass in which the strength is maximized and excellent set drop strength is achieved, a manufacturing method thereof, and the glass. [Means for solving the problem]

[0011] When ion exchange treatment is performed in two or more stages in the manufacturing process of chemically strengthened glass, in the first stage ion exchange (hereinafter also abbreviated as "first ion exchange"), glass is brought into contact with a first molten salt composition for ion exchange, whereby a "first alkali metal ion" in the glass is exchanged with a "second alkali metal ion having an ionic radius larger than that of the first alkali metal ion" in the first molten salt composition, and the second alkali metal ion in the first molten salt composition is introduced into the glass. Furthermore, in the second stage ion exchange (hereinafter also abbreviated as "second ion exchange") after the first ion exchange, the glass for chemical strengthening that has undergone the first ion exchange is brought into contact with a second molten salt composition for ion exchange.

[0012] In the second ion exchange and subsequent steps, simultaneously with the exchange of ions in the molten salt composition (e.g., a third alkali metal ion having an ionic radius larger than that of the second alkali metal ion) with ions in the glass (e.g., the second alkali metal ion), the second alkali metal ion introduced into the glass from the first molten salt composition in the first ion exchange diffuses into the glass.

[0013] The present inventors have found that in the first ion exchange, a composition containing a first alkali metal ion (e.g., Li ion, etc.) is used as the first molten salt composition, and ion exchange (hereinafter also abbreviated as reverse ion exchange) between a second alkali metal ion (e.g., Na ion, etc.) in the glass and the first alkali metal ion in the first molten salt composition is carried out in parallel with the above-mentioned exchange between the first alkali metal ion in the glass and the second alkali metal ion in the first molten salt composition, thereby obtaining CS 90 The present invention was completed based on this finding.

[0014] The present invention provides a chemically strengthened glass having the following configuration, a manufacturing method thereof, and a glass. 1. The plate thickness is t (mm), and the compressive stress layer depth DOC is 180×t (μm) or more. The integral value of compressive stress from the surface to a depth of 30 to 50 μm, CS 30-50 is 12000 Pa m or less, and Compressive stress value CS at a depth of 90 μm from the surface 90 Chemically strengthened glass having a strength of 175×t-88 (MPa) or more. 2. The chemically strengthened glass according to 1 above, having a Young's modulus of 80 GPa or more. 3. Stress value CS at a depth x [μm] from the glass surface measured with a scattered light photoelastic stress meter x In the profile of [MPa], the stress value CS x The second derivative of CS x '' but C.S. x 3. The chemically strengthened glass according to 1 or 2 above, which satisfies the following formula in the range of ≧0. -0.03≦CS x ''≦0.013 4. The chemically strengthened glass according to any one of 1 to 3 above, having a surface compressive stress value FSM-CS0 of 800 MPa or more. 5. Surface resistivity is 10 log Ω / sq or less; Chemically strengthened glass with a Young's modulus of 80 GPa or more. 6. Chemically strengthened glass, in which the Na2O concentration at a depth of 30 μm from the surface divided by the Na2O concentration at a depth of 90 μm from the surface is 1.30 or less. 7. The chemically strengthened glass according to 6 above, wherein a value obtained by dividing the Na2O concentration at a depth of 50 μm from the surface by the Na2O concentration at the center of the sheet thickness is 2 or more and 4 or less. 8. The chemically strengthened glass according to 6 or 7 above, wherein a value obtained by dividing the Na2O concentration at a depth of 90 μm from the surface by the Na2O concentration at the center of the plate thickness is 2.4 or more. 9. The parent composition is expressed in mole percent based on oxides. SiO2 55-75%, Li2O 3~15%, 9. The chemically strengthened glass according to any one of 1 to 8 above, which contains 8 to 25% of Al2O3. 10. A first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition; A method for producing chemically strengthened glass, comprising at least a second ion exchange treatment in which the glass for chemical strengthening is contacted with a second molten salt composition after the first ion exchange treatment, In the first ion exchange treatment, the glass for chemical strengthening is contacted with the first molten salt composition at 350 to 450° C. for 150 minutes or more, The glass for chemical strengthening has, in mole percent based on oxides, SiO2 55-75%, Li2O 3~15%, A method for producing chemically strengthened glass containing 8-25% Al2O3. 11. The method for producing chemically strengthened glass according to 10 above, wherein the first molten salt composition contains 0.01 to 1 mass % of lithium ions. 12. A first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition; A method for producing chemically strengthened glass, comprising at least a second ion exchange treatment in which the glass for chemical strengthening is contacted with a second molten salt composition after the first ion exchange treatment, the first ion exchange treatment is performed at 350 to 450° C. for 150 minutes or longer, and the first molten salt composition contains lithium ions; The glass for chemical strengthening has, in mole percent based on oxides, SiO2 55-75%, Li2O 3~15%, A method for producing chemically strengthened glass containing 8-25% Al2O3. 13. The method for producing chemically strengthened glass according to 12 above, wherein the second molten salt composition contains 0 to 5 mass % of lithium nitrate. 14. A third ion exchange treatment is included in which the glass for chemical strengthening is contacted with a third molten salt composition after the second ion exchange treatment, 14. The method for producing chemically strengthened glass according to 12 or 13 above, wherein the third molten salt composition contains 98 mass % or more of potassium nitrate. 15. The method for producing chemically strengthened glass according to any one of 11 to 13 above, wherein the CTave of the glass for chemical strengthening is made less than the CTA by the second ion exchange treatment or subsequent ion exchange treatments, wherein the CTA is calculated by the following formula (1) and the CTave is calculated by the following formula (2):

[0015]

number

[0016] t: Plate thickness (μm) K1c: Fracture toughness value (MPa m 1 / 2 ) CTave=ICT / LCT...Equation (2) ICT: Integrated value of tensile stress (Pa m) LCT: Length of tensile stress area in the thickness direction (μm) 16. In mole percent based on oxide, SiO2 55-75%, Al2O3 8-25%, Li2O 3~15%, Na2O 1-5%, K2O 0-3%, MgO 0-10%, CaO 0-10%, SrO 0-5%, ZnO 0-5%, TiO2 0-3%, ZrO2 0-3%, SnO2 0-1%, P2O5 0-1%, B2O3 0-10%, Y2O3 0-3%, Fe2O3 content is 0-0.1%. Li2O / [Li2O+Na2O+K2O], which is the ratio of the Li2O content to the total content of Li2O, Na2O and K2O, is 0.5 to 0.9; The ratio of the Li2O content to the Na2O content, Li2O / Na2O, is 1.5 to 10, and Young's modulus is 80 GPa or more Glass. 17. The glass according to 16, wherein the ratio of the B2O3 content to the P2O5 content, B2O3 / P2O5, is 2.5 to 500. 18. When a compressive stress layer is formed by ion exchange treatment at 380°C for 4 hours using a molten salt of sodium nitrate, what is the compressive stress value CS at a depth of 30 μm from the surface of the compressive stress layer? 30 18. The glass according to 16 or 17, wherein the compressive strength is 150 MPa or more. Effect of the Invention

[0017] The chemically strengthened glass according to the first embodiment of the present invention has stress characteristics in a specific range. In particular, the integrated value CS of the compressive stress at a depth of 30 to 50 μm from the surface 30-50 By keeping the surface compressive stress at 12000 Pa m or less, the internal tensile stress can be suppressed and the CS 90 However, it has a high deep compressive stress of 175 x t-88 (MPa) or more, where t is the plate thickness (mm). This makes it possible to avoid the CT limit and achieve excellent set drop strength that could not be achieved with conventional technology.

[0018] The chemically strengthened glass according to the second embodiment of the present invention has a surface resistivity and Young's modulus within a specific range, which can suppress peeling of the coating and can achieve a deep layer compressive stress higher than that of the conventional glass while maintaining a high surface compressive stress.

[0019] The chemically strengthened glass according to the third embodiment of the present invention has a DOC of 180t or more, where t (mm) is the plate thickness, and the value obtained by dividing the Na2O concentration at a depth of 30 μm from the surface by the Na2O concentration at a depth of 90 μm from the surface is 1.30 or less. In general chemically strengthened glass, the Na concentration increases from the center of the glass to the glass surface, but by setting the value to 1.30 or less, the profile of the sodium concentration in the glass becomes flat, the surface compressive stress can be reduced, the internal tensile stress can be suppressed, and a high deep compressive stress can be realized. In addition, compared to the conventional glass, the increase in surface resistivity can be effectively suppressed, and peeling of the coating can be suppressed.

[0020] A method for producing chemically strengthened glass according to a fourth embodiment of the present invention includes at least a first ion exchange treatment in which a glass for chemical strengthening having a composition in a specific range is contacted with a first molten salt composition at 350 to 450°C for 150 minutes or more, and a second ion exchange treatment in which the glass for chemical strengthening is contacted with a second molten salt composition after the first ion exchange treatment. 90 By maximizing this, it is possible to produce chemically strengthened glass that exhibits excellent set drop strength that was not possible with conventional technology.

[0021] A method for producing chemically strengthened glass according to a fifth embodiment of the present invention includes at least a first ion exchange treatment in which a glass for chemical strengthening having a composition within a specific range is brought into contact with a first molten salt composition containing lithium ions at 350 to 450°C for 150 minutes or more, and a second ion exchange treatment in which the glass for chemical strengthening is brought into contact with a second molten salt composition after the first ion exchange treatment. This reduces the surface compressive stress and reduces the internal tensile stress through processes such as thermal structural relaxation and reverse ion exchange in the surface layer in the first ion exchange treatment, thereby improving the CS while avoiding the CT limit. 90By maximizing this, it is possible to produce chemically strengthened glass that exhibits excellent set drop strength that was not possible with conventional technology.

[0022] The glass of the sixth embodiment of the present invention has a composition and Young's modulus within specific ranges, and by chemically strengthening it is possible to obtain a chemically strengthened glass that has a high deep layer compressive stress compared to conventional glass while maintaining a high surface compressive stress. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a graph showing the correlation between CS90 and drop strength using #80 sandpaper set. [Diagram 2] 2(a) and (b) are schematic diagrams for explaining ion exchange in one embodiment of the present invention, where (a) in Fig. 2 shows a first ion exchange treatment, and (b) in Fig. 2 shows a second ion exchange treatment. [Diagram 3] FIG. 3 is a diagram showing the stress characteristics of glass after one-stage chemical strengthening. [Figure 4] FIG. 4 is a diagram showing the results of measuring CS for chemically strengthened glass. [Diagram 5] FIG. 5 is a diagram showing the correlation between CTave and CS90 for chemically strengthened glass. [Figure 6] 6(a) and (b) are diagrams showing stress profiles of chemically strengthened glass. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] In this specification, "chemically strengthened glass" refers to glass after chemical strengthening treatment, and "glass for chemical strengthening" refers to glass before chemical strengthening treatment.

[0025] In this specification, glass compositions are expressed in mol % based on oxides unless otherwise specified, and mol % is simply represented as "%".

[0026] In addition, in this specification, "substantially free" means that the content is below the impurity level contained in raw materials, that is, that it is not intentionally added. Specifically, for example, it is less than 0.1%.

[0027] In this specification, the term "stress profile" refers to a representation of compressive stress values ​​with the depth from the glass surface as a variable. In the stress profile, tensile stress may be represented as negative compressive stress. In this specification, tensile stress is represented as an absolute value.

[0028] The "compressive stress value (CS)" can be measured by cutting a cross section of glass into thin slices and analyzing the sliced ​​samples with a birefringence imaging system. A birefringence imaging system stress meter is a device that measures the magnitude of retardation caused by stress using a polarizing microscope and a liquid crystal compensator, etc., and one example is the birefringence imaging system Abrio-IM manufactured by CRi.

[0029] Measurements can also be made using scattered light photoelasticity. With this method, light is incident on the glass surface, and the polarization of the scattered light is analyzed to measure CS. An example of a stress measuring device that uses scattered light photoelasticity is the SLP-2000 scattered light photoelasticity meter manufactured by Orihara Seisakusho.

[0030] In this specification, the "depth of compressive stress layer (DOC)" is the depth at which the compressive stress value becomes zero. In the following, the surface compressive stress value measured by the scattered light photoelastic stress meter is referred to as CS0, and the compressive stress value at a depth of 50 μm from the surface is referred to as CS 50 The compressive stress at a depth of 90 μm from the surface is calculated as CS 90 In addition, "internal tensile stress (CT)" refers to the absolute value of the tensile stress at a depth of 1 / 2 the plate thickness t, and in this specification, "CS t / 2 " is equivalent to "

[0031] In this specification, "Young's modulus" is measured by ultrasonic methods.

[0032] In this specification, the "fracture toughness value K1c" is the value determined by the IF method specified in JIS R1607:2015. The value of K1c depends on the glass composition and can be adjusted according to the glass composition.

[0033] In this specification, the "surface resistivity" is measured using a contact conductivity meter. The surface resistivity has a positive correlation with the volume resistivity.

[0034] <set drop strength> In this specification, the "#80 drop strength" is measured by the following method. A glass sample of 120 mm × 60 mm × 0.7 mm is fitted into a structure whose mass and rigidity have been adjusted to the size of a currently used general smartphone to prepare a pseudo-smartphone, and then freely dropped onto #80 SiC sandpaper. If it does not break when dropped from a height of 5 cm, the height is increased by 5 cm and the dropping operation is repeated until it breaks, and the height at which it first breaks is taken as the dropping height. The result of the average break height when 20 sheets of each glass sample are subjected to the dropping test is defined as the "#80 sandpaper average set drop strength".

[0035] <4PB strength (4-point bending strength)> In this specification, the 4PB strength is measured by the following method. The chemically strengthened glass is processed into a strip shape of 120 mm × 60 mm, and a 4-point bending test is performed under the conditions that the external fulcrum distance of the support is 30 mm, the internal fulcrum distance is 10 mm, and the crosshead speed is 5.0 mm / min to measure the 4-point bending strength. The number of test pieces is 10. Note that the chemically strengthened glass is, after being processed into a strip shape, automatically chamfered (C chamfering) using a 1000-grit grinding wheel (manufactured by Tokyo Diamond Tool Works), and the end face is mirror-finished using a 0.1 mm diameter nylon brush and SHOUROX NZ abrasive grains (manufactured by Showa Denko KK), and the one with a thickness of 120 × 60 × 0.7 mm is measured.

[0036] <Na concentration> In this specification, the Na2O concentration at a depth x [μm] is measured at a cross section in the plate thickness direction by an EPMA (Electron Probe Micro Analyzer). Specifically, the measurement by EPMA is performed as follows, for example. First, a glass sample is embedded in epoxy resin, and mechanically polished in a direction perpendicular to the first main surface and the second main surface opposite the first main surface to prepare a cross-sectional sample. The polished cross-section is coated with C-coat and measured using an EPMA (JEOL: JXA-8500F). The acceleration voltage is 15 kV, the probe current is 30 nA, and the integration time is 1000 msec. / point to obtain a line profile of the X-ray intensity of Na at 1 μm intervals. For the obtained Na2O concentration profile, the average count at the center of the plate thickness (0.5 × t) ± 25 μm (plate thickness is t μm) is taken as the bulk composition, and the count for the entire plate thickness is proportionally converted to mole %.

[0037] <Stress measurement method> In recent years, glass that has been subjected to a two-stage chemical strengthening process in which the lithium ions inside the glass are exchanged for sodium ions (Li-Na exchange), and then the sodium ions inside the glass are further exchanged for potassium ions on the surface of the glass (Na-K exchange) has become mainstream for cover glass for devices such as smartphones.

[0038] In order to obtain the stress profile of such two-stage chemically strengthened glass in a non-destructive manner, for example, a scattered light photoelastic stress meter (hereinafter also abbreviated as SLP) or a film stress measurement (hereinafter also abbreviated as FSM) can be used in combination.

[0039] The method using a scattered light photoelastic stress meter (SLP) can measure the compressive stress resulting from Li-Na exchange in the glass interior at a depth of several tens of μm or more from the glass surface. On the other hand, the method using a glass surface stress meter (FSM) can measure the compressive stress resulting from Na-K exchange in the glass surface layer at a depth of several tens of μm or less from the glass surface (for example, International Publication No. 2018 / 056121, International Publication No. 2017 / 115811). Therefore, a combination of SLP and FSM information is sometimes used as the stress profile in the glass surface and interior in two-stage chemically strengthened glass.

[0040] In the present invention, the stress profile measured mainly by a scattered light photoelastic stress meter (SLP) is used. In this specification, the compressive stress CS, the tensile stress CT, the compressive stress layer depth DOC, etc. refer to the values ​​in the SLP stress profile.

[0041] The scattered light photoelastic stress meter is a stress measuring device having a polarization phase difference variable member that varies the polarization phase difference of laser light by one or more wavelengths relative to the wavelength of the laser light, an imaging element that captures the scattered light emitted when the laser light with the varied polarization phase difference is incident on strengthened glass multiple times at a specified time interval to obtain multiple images, and a calculation unit that uses the multiple images to measure the periodic luminance change of the scattered light, calculates the phase change of the luminance change, and calculates the stress distribution in the depth direction from the surface of the strengthened glass based on the phase change.

[0042] A method for measuring a stress profile using a scattered light photoelastic stress meter includes the method described in International Publication No. 2018 / 056121. Examples of the scattered light photoelastic stress meter include SLP-1000 and SLP-2000 manufactured by Orihara Seisakusho. High-precision stress measurement is possible by combining these scattered light photoelastic stress meters with the attached software SlpIV_up3 (Ver.2019.01.10.001).

[0043] <cta> The CT limit corresponds to the CTA calculated by the following formula (1), and is a value determined by the composition of the glass for chemical strengthening.

[0044]

number

[0045] t: Plate thickness (mm) K1c: Fracture toughness value (MPa m 1 / 2 )

[0046] <ctave> In this specification, "CTave" is calculated by the following formula (2). CTave is a value equivalent to the average value of tensile stress, and is calculated by integrating the stress value in the tensile stress region in the plate thickness direction in the tensile stress region and dividing the result by the length of the tensile stress region. CTave=ICT / LCT...Equation (2) ICT: Integrated value of tensile stress (Pa m) LCT: Length of tensile stress area in the thickness direction (μm)

[0047] <Chemically strengthened glass: 1st to 3rd embodiments> Hereinafter, first to third embodiments of the chemically strengthened glass according to the present invention will be described. In this specification, the chemically strengthened glass according to the present invention including the first to third embodiments is also abbreviated as "the present chemically strengthened glass".

[0048] [Chemically strengthened glass of the first embodiment] The chemically strengthened glass according to the first embodiment has a sheet thickness of t (mm), a compressive stress layer depth DOC of 180×t (μm) or more, and an integral value CS of the compressive stress at a depth of 30 to 50 μm from the surface. 30-50 is 12000 Pa m or less and the compressive stress value CS at a depth of 90 μm from the surface 90 is 175×t-88 (MPa) or more.

[0049] The chemically strengthened glass according to the first embodiment has a compressive stress layer depth DOC of 180×t (μm) or more, preferably 182.5×t (μm) or more, more preferably 185×t (μm) or more, even more preferably 187.5×t (μm) or more, and particularly preferably 190×t (μm) or more. By forming a compressive stress layer in a deep part of the glass with a DOC of 190×t (μm) or more, the effect of being less likely to break even when subjected to a large impact is obtained. The upper limit of DOC is not particularly limited, but in order to keep the integrated value of the compressive stress value low, it is, for example, 300×t (μm) or less, preferably 280×t (μm) or less, more preferably 260×t (μm) or less, and particularly preferably 250×t (μm) or less.

[0050] The chemically strengthened glass according to the first embodiment has an integral value CS of compressive stress at a depth of 30 to 50 μm from the surface. 30-50 is 12000 Pa m or less. CS 30-50 By keeping the surface compressive stress at 12,000 Pa·m or less, the internal tensile stress can be suppressed by reducing the surface compressive stress. 30-50 The lower limit is not particularly limited, but is usually 7500 Pa·m or more, preferably 8000 Pa·m or more, more preferably 8250 Pa·m or more, and even more preferably 8500 Pa·m or more.

[0051] The chemically strengthened glass according to the first embodiment has a compressive stress value CS 90 is 175×t-88 (MPa) or more, preferably 175×t-86 (MPa) or more, more preferably 175×t-83 (MPa) or more, even more preferably 175×t-81 (MPa) or more, and particularly preferably 175×t-78 (MPa) or more. 90 By making the CS greater than or equal to 175×t-88 (MPa), the set drop strength (for example, the #80 sandpaper set drop strength) can be increased compared to the conventional case. 90 Although there is no particular upper limit, in order to keep the integrated value of the compressive stress low, it is, for example, 175×t-40 (MPa) or less, preferably 175×t-42.5 (MPa) or less, more preferably 175×t-45 (MPa) or less, and particularly preferably 175×t-50 (MPa) or less.

[0052] The chemically strengthened glass according to the first embodiment has a Young's modulus of preferably 80 GPa or more, more preferably 82 GPa or more, further preferably 84 GPa or more, and particularly preferably 85 GPa or more. By having a Young's modulus of 80 GPa or more, a higher CTA can be realized and deep layer stress can be improved.

[0053] Young's modulus is correlated with the diffusivity of sodium ions, and the higher the Young's modulus, the less likely Na ions are to diffuse. If the Young's modulus is 80 GPa or more, Na ions are less likely to diffuse, and it is easy to introduce high surface compressive stress by ion exchange, and even if the surface compressive stress is reduced by reverse ion exchange, it is possible to maintain a high deep compressive stress while maintaining a high surface compressive stress. The upper limit of the Young's modulus is not particularly limited, but from the viewpoint of the bending process, it is usually 100 GPa or less, preferably 95 GPa or less, and more preferably 90 GPa or less.

[0054] As described above, the chemically strengthened glass of the first embodiment is measured with a scattered light photoelastic stress meter, and the stress value CS at a depth x [μm] from the glass surface is x In the profile of [MPa], the stress value CS x The second derivative of CS x '' but C.S. x In the range of 0, the formula -0.03 ≤ CS x It is preferable that CS ''≦0.013 is satisfied. x When CS '' is more preferably 0.010 or less, further preferably 0.008 or less, and particularly preferably 0.006 or less, a more linear shape is obtained, and the stress value CS 90 It can effectively improve CS x is more preferably equal to or greater than −0.028, and further preferably equal to or greater than −0.024.

[0055] CS x Stress value CS in the range of ≧0 x The first derivative value of CS x The first derivative value CS ' is preferably -3.0 or more, more preferably -2.8 or more, and further preferably -2.6 or more. x When ' is in the above range, CS x The change in stress value CS x The profile of CS0 is linear. x 'By making the CS 90 This has the effect of keeping the CS high. x ' is typically less than or equal to -0.8.

[0056] In the present invention, the differentiation method of the stress profile is expressed by the following formula: CS x In the profile, CS when the change in x is 0.5 μm x The rate of change of CS x ' is used as the value of CS when the change in x is 0.5 μm. x ', the rate of change of CS x '' is used as the value. CS x '=(CS x+0.5 -CS x ) / 0.5 CS x ''=(CS x+0.5 '-CS x ') / 0.5

[0057] In the chemically strengthened glass of the first embodiment, the surface compressive stress value FSM-CS0 measured by FSM is preferably 800 MPa or more, since the set drop strength is further improved and the glass is less likely to break due to deformation such as bending. FSM-CS0 is more preferably 900 MPa or more, further preferably 950 MPa or more, and particularly preferably 1000 MPa or more. There is no particular upper limit for FSM-CS0, but from the viewpoint of keeping the integrated value of the compressive stress value low, it is usually preferably 1500 MPa or less. FSM-CS0: Compressive stress value at a depth of 0 μm measured by FSM CS x : Compressive stress value at depth x [μm] measured by SLP

[0058] In the chemically strengthened glass of the first embodiment, the surface compressive stress layer depth DOL-tail is preferably 2.8 μm or more, more preferably 2.9 μm or more, even more preferably 3.0 μm or more, and particularly preferably 3.3 μm or more. By having a DOL-tail of 2.8 μm or more, the four-point bending strength can be improved. The upper limit of the DOL-tail is not particularly limited, but from the viewpoint of the balance with the deep layer stress, it is preferably, for example, 8.0 μm or less, more preferably 7.0 μm or less. In this specification, the surface compressive stress layer depth DOL-tail refers to the maximum depth of the compressive stress layer that can be measured by FSM.

[0059] The chemically strengthened glass according to the first embodiment has a surface resistivity of preferably 10 log Ω / sq or less, more preferably 9.5 log Ω / sq or less, even more preferably 9.0 log Ω / sq or less, and particularly preferably 8.5 log Ω / sq or less. By having a surface resistivity of 10 log Ω / sq or less, peeling of the coating can be suppressed. The lower limit of the surface resistivity is not particularly limited, but it is usually preferably 7.0 log Ω / sq or more.

[0060] In the first embodiment, the plate thickness t (mm) of the chemically strengthened glass is preferably 0.8 mm or less, more preferably 0.7 mm or less, further preferably 0.65 mm or less, and particularly preferably 0.6 mm or less, from the viewpoint of improving strength. The smaller t is, the greater the effect of improving strength according to the present invention. t is typically 0.02 mm or more.

[0061] The stress characteristics and ion profile of the chemically strengthened glass of the first embodiment can be adjusted by its matrix composition and the conditions of the ion exchange treatment. The glass composition of the chemically strengthened glass of the first embodiment will be described later in the section "Matrix composition of chemically strengthened glass."

[0062] [Chemically strengthened glass according to the second embodiment] The chemically strengthened glass according to the second embodiment is characterized in that it has a surface resistivity of 10 log Ω / sq or less and a Young's modulus of 80 GPa or more.

[0063] The chemically strengthened glass according to the second embodiment has a surface resistivity of 10 log Ω / sq or less, preferably 9.5 log Ω / sq or less, more preferably 9.0 log Ω / sq or less, even more preferably 8.5 log Ω / sq or less, and particularly preferably 8.0 log Ω / sq or less.

[0064] The higher the surface resistivity of chemically strengthened glass, the more likely the coating is to peel off (WO 2021 / 010376). In addition, the content ratio of alkali metal oxides affects the surface resistivity (WO 2021 / 010376). For example, glass containing three types of alkali metal oxides, Li2O, Na2O, and K2O, has a higher surface resistivity due to the so-called mixed alkali effect compared to glass containing only one or two types of alkali metal oxides, even if it contains the same amount of alkali metal oxide.

[0065] Therefore, when glass is chemically strengthened by two or more stages of ion exchange, the resulting chemically strengthened glass contains the three elements Li2O, Na2O, and K2O, and the coating tends to peel off. On the other hand, if the glass composition before strengthening or the chemical strengthening treatment conditions are adjusted in order to suppress coating peeling after chemical strengthening, a problem occurs in which it becomes difficult to obtain sufficient strength by chemical strengthening.

[0066] The chemically strengthened glass of the second embodiment has a surface resistivity of 10 log Ω / sq or less, which can suppress charging between the coating surface and the glass surface and can suppress peeling of the coating. The lower limit of the surface resistivity is not particularly limited, but is usually preferably 7.0 log Ω / sq or more.

[0067] The chemically strengthened glass according to the second embodiment has a Young's modulus of 80 GPa or more, preferably 82 GPa or more, more preferably 84 GPa or more, even more preferably 85 GPa or more, and particularly preferably 85.5 GPa or more. If the Young's modulus is 80 GPa or more, Na ions are less likely to diffuse, and it is easy to introduce a high surface compressive stress by ion exchange. Even if the surface compressive stress is reduced by reverse ion exchange, the deep compressive stress can be maintained higher while maintaining a high surface compressive stress.

[0068] The chemically strengthened glass of the second embodiment preferably has similar properties to those of the chemically strengthened glass of the first embodiment, other than the surface resistivity and Young's modulus.

[0069] [Chemically strengthened glass according to the third embodiment] The chemically strengthened glass of the third embodiment is characterized in that the value obtained by dividing the Na2O concentration at a depth of 30 μm from the surface by the Na2O concentration at a depth of 90 μm from the surface is 1.30 or less. In the chemically strengthened glass of the third embodiment, the value obtained by dividing the Na2O concentration at a depth of 30 μm from the surface by the Na2O concentration at a depth of 90 μm from the surface is preferably 1.25 or less, more preferably 1.2 or less, even more preferably 1.15 or less, even more preferably 1.1 or less, and particularly preferably 1 or less. By the value being 1.30 or less, the profile of the sodium concentration in the glass becomes flat, the surface layer compressive stress can be reduced, the internal tensile stress can be suppressed, and a high deep layer compressive stress can be realized. In addition, compared to the conventional case, the increase in the surface resistivity can be effectively suppressed, and peeling of the coating can be suppressed.

[0070] In the chemically strengthened glass of the third embodiment, the lower limit of the value obtained by dividing the Na2O concentration at a depth of 30 μm from the surface by the Na2O concentration at a depth of 90 μm from the surface is not particularly limited.

[0071] In the chemically strengthened glass of the third embodiment, the value obtained by dividing the Na2O concentration at a depth of 50 μm from the surface by the Na2O concentration at the center of the plate thickness is preferably from 2 to 4. By making the value from 2 to 4, the surface layer compressive stress can be further reduced to suppress the internal tensile stress, and the deep layer compressive stress can be further increased.

[0072] In the chemically strengthened glass of the third embodiment, the value obtained by dividing the Na2O concentration at a depth of 50 μm from the surface by the Na2O concentration at the center of the sheet thickness is preferably 2 or more, more preferably 2.5 or more, even more preferably 2.7 or more, still more preferably 2.8 or more, and particularly preferably 2.9 or more. In addition, the value is preferably 4 or less, more preferably 3.5 or less, even more preferably 3.3 or less, still more preferably 3.2 or less, and particularly preferably 3.1 or less.

[0073] In the chemically strengthened glass of the third embodiment, the value obtained by dividing the Na2O concentration at a depth of 90 μm from the surface by the Na2O concentration at the center of the plate thickness is preferably 2.4 or more. More preferably, it is 2.5 or more, even more preferably 2.7 or more, and particularly preferably 3.0 or more. By having the value of 2.4 or more, it is possible to efficiently increase the deep layer stress that is effective for the drop strength against #80 sandpaper, and to realize a high deep layer compressive stress.

[0074] In the chemically strengthened glass of the third embodiment, the upper limit of the value obtained by dividing the Na2O concentration at a depth of 90 μm from the surface by the Na2O concentration at the center of the sheet thickness is not particularly limited, but is usually preferably 6.0 or less.

[0075] The chemically strengthened glass of the third embodiment preferably has similar characteristics to those of the chemically strengthened glass of the first embodiment, except for the Na2O concentration profile.

[0076] <<Applications of chemically strengthened glass>> The chemically strengthened glass is also useful as a cover glass for electronic devices such as mobile devices such as mobile phones and smartphones. It is also useful as a cover glass for electronic devices such as televisions, personal computers, and touch panels that are not intended to be portable, as elevator walls, and as walls (full-surface displays) of buildings such as houses and buildings. It is also useful as building materials such as window glass, table tops, interiors of automobiles and airplanes, and cover glass for these, and for curved housings.

[0077] <<Mother composition of chemically strengthened glass>> In this specification, the "base composition of chemically strengthened glass" refers to the composition of glass before chemical strengthening. This composition will be described later. The composition of this chemically strengthened glass has a composition similar to that of the glass before strengthening as a whole, except when extreme ion exchange treatment is performed, and the composition of the glass before strengthening is usually equivalent to the composition of the center of the plate thickness in the chemically strengthened glass. In particular, the composition of the deepest part from the glass surface is the same as the composition of the glass before strengthening, except when extreme ion exchange treatment is performed. The base composition of the present chemically strengthened glass preferably contains SiO2, Li2O, and Al2O3.

[0078] As an embodiment of the base composition of the chemically strengthened glass, it is preferable that the glass contains, in mole percent based on oxides, 52 to 75% SiO2, 3 to 15% Li2O, and 8 to 25% Al2O3. Hereinafter, glass having such a composition is referred to as glass. X1 Let us assume that.

[0079] Glass X1 As for the composition, SiO2 is 55-75%, Li2O 3~15%, Al2O3 8-25%, Na2O 1-5%, K2O 0-3%, MgO 0-10%, CaO 0-10%, SrO 0-5%, ZnO 0-5%, TiO2 0-3%, ZrO2 0-3%, SnO2 0-1%, P2O5 0-1%, B2O3 0-10%, Y2O3 0-3%, It is more preferable that Fe2O3 is contained in an amount of 0 to 0.1%.

[0080] Another embodiment of the base composition of the chemically strengthened glass preferably contains, in mole percent on an oxide basis, 40 to 70% SiO2, 10 to 35% Li2O, and 1 to 15% Al2O3. Hereinafter, glass having such a composition is referred to as glass. X2 When the chemically strengthened glass is a crystallized glass, the base composition is glass. X2 The composition is preferably:

[0081] Glass X2 As one embodiment, expressed in mole percent based on oxide, SiO2 40-70%, Li2O 10~35%, Al2O3 1-15%, P2O5 0.5-5%, ZrO2 0.5-5%, B2O3 0-10%, Na2O 0-3%, K2O 0-1%, It is preferable that the content of SnO2 is 0 to 4%.

[0082] Glass X2 In another embodiment, the oxide-based mole percent is: SiO2 50-70%, Li2O 15~30%, Al2O3 1-10%, P2O5 0.5-5%, ZrO2 0.5-8%, MgO 0.1-10%, Y2O3 0-5% B2O3 0-10%, Na2O 0-3%, K2O 0-1%, It is preferable that the content of SnO2 is 0 to 2%.

[0083] The glass composition will be described below.

[0084] SiO2 is a component that constitutes the skeleton of glass. It also increases chemical durability and reduces the occurrence of cracks when the glass surface is scratched. Glass X1 In the above, the SiO2 content is 55% or more, preferably 60% or more, more preferably 61% or more, even more preferably 62% or more, and particularly preferably 65% ​​or more. On the other hand, from the viewpoint of improving melting property, the SiO2 content is 75% or less, preferably 72% or less, more preferably 70% or less, even more preferably 67% or less, and particularly preferably 67.5% or less. Glass X2 In the above, the SiO2 content is preferably 45% or more. The SiO2 content is more preferably 48% or more, even more preferably 50% or more, particularly preferably 52% or more, and extremely preferably 54% or more. On the other hand, in order to improve the melting property, the SiO2 content is preferably 70% or less, more preferably 68% or less, even more preferably 66% or less, and particularly preferably 64% or less.

[0085] Al2O3 is an effective component from the viewpoints of improving the ion exchange performance during chemical strengthening and increasing the surface compressive stress after strengthening. Glass X1 In the glass, the content of Al2O3 is 8% or more, preferably 9% or more, more preferably 10% or more, even more preferably 11% or more, and particularly preferably 12% or more. On the other hand, if the content of Al2O3 is too high, crystals tend to grow during melting, and the yield is likely to decrease due to devitrification defects. In addition, the viscosity of the glass increases and the melting property decreases. The content of Al2O3 is 25% or less, preferably 22% or less, more preferably 20% or less, even more preferably 18% or less, and particularly preferably 16% or less. Glass X2 In the above, the content of Al2O3 is preferably 1% or more, more preferably 2% or more, further preferably 3% or more, 5% or more, 5.5% or more, 6% or more, particularly preferably 6.5% or more, and most preferably 7% or more. On the other hand, the content of Al2O3 is preferably 15% or less, more preferably 12% or less, further preferably 10% or less, particularly preferably 9% or less, and most preferably 8% or less, so that the devitrification temperature of the glass does not become too high.

[0086] Glass X1 In the above, SiO2 and Al2O3 are both components that stabilize the glass structure, and in order to reduce brittleness, the total content is preferably 65% ​​or more, more preferably 70% or more, and even more preferably 75% or more.

[0087] Li2O is a component that forms surface compressive stress through ion exchange and improves the melting property of glass. By including Li2O in chemically strengthened glass, lithium ions on the glass surface are ion-exchanged with sodium ions, and the sodium ions are further ion-exchanged with potassium ions, resulting in a large stress profile for both the surface compressive stress and the compressive stress layer.

[0088] Glass X1 In order to easily obtain a preferred stress profile, the Li2O content is 3% or more, preferably 5% or more, more preferably 7% or more, even more preferably 9% or more, particularly preferably 10% or more, and most preferably 11% or more. On the other hand, if the Li2O content is too high, the crystal growth rate during glass molding increases, and the problem of reduced yield due to devitrification defects becomes greater. The Li2O content is 15% or less, preferably 14% or less, more preferably 13% or less, and particularly preferably 12% or less.

[0089] Glass X2 In the glass, the Li2O content is preferably 10% or more, more preferably 14% or more, more preferably 15% or more, even more preferably 18% or more, particularly preferably 20% or more, and most preferably 22% or more. On the other hand, in order to stabilize the glass, the Li2O content is preferably 35% or less, more preferably 32% or less, even more preferably 30% or less, particularly preferably 28% or less, and most preferably 26% or less.

[0090] Although neither Na2O nor K2O is essential, they are components that improve the meltability of glass and reduce the crystal growth rate of glass. X1 In order to improve the ion exchange performance, the total content of Na2O and K2O (Na2O+K2O) is preferably 2% or more. Also, Na2O+K2O is preferably 10% or less, preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, and particularly preferably 5% or less.

[0091] Na2O is a component that forms a surface compressive stress layer in a chemical strengthening treatment using a potassium salt, and is also a component that can improve the meltability of glass. Glass X1 In order to obtain this effect, the Na2O content is 1% or more, preferably 2% or more, more preferably 3% or more, and further preferably 4% or more. On the other hand, from the viewpoint of avoiding a decrease in surface compressive stress (FSM-CS0) in the strengthening treatment using sodium salts, and from the viewpoint of preventing a decrease in CS 90 From the viewpoint of realizing a high profile, the thickness is 5% or less, preferably 4% or less, more preferably 3.5% or less, and even more preferably 3% or less. Glass composition X2 In the above, Na2O is not essential, but when it is contained, it is preferably 0.5% or more, more preferably 1% or more, and particularly preferably 2% or more. If there is too much Na2O, it becomes difficult to precipitate crystals such as Li3PO4, which is the main crystal, or the chemical strengthening properties are reduced, so the Na2O content is preferably 10% or less, more preferably 9% or less, even more preferably 8% or less, and particularly preferably 7% or less.

[0092] K2O may be contained for the purpose of improving ion exchange performance. Glass X1 In the case where K2O is contained, the content is preferably 0.1% or more, more preferably 0.15% or more, and particularly preferably 0.2% or more. In order to further prevent devitrification, the content is preferably 0.5% or more, and more preferably 1.2% or more. On the other hand, since a large amount of K is a factor of brittleness and a decrease in surface layer stress due to back exchange during strengthening, the content is 3% or less, preferably 2% or less, and more preferably 1% or less. Glass composition X2 In the case where K2O is contained, the content is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. If the amount of K2O is too much, the chemical strengthening properties or chemical durability decreases, so the content is preferably 5% or less, more preferably 4% or less, even more preferably 3% or less, particularly preferably 2% or less, and most preferably 1% or less.

[0093] The balance of Li2O, Na2O, and K2O affects the ion exchange performance. X1 In the above, the ratio of Li2O in the composition divided by the total content of Li2O, Na2O and K2O, i.e., Li2O / [Li2O+Na2O+K2O], is 0.5 or more and 0.9 or less. When the value is 0.5 or more, Li ions in the glass and Na ions in the molten salt composition are efficiently exchanged. When the value is 0.9 or less, the resistance of the glass can be reduced. Li2O / [Li2O+Na2O+K2O] is preferably 0.55 or more, more preferably 0.60 or more, and even more preferably 0.65 or more, and is preferably 0.85 or less, more preferably 0.80 or less, and even more preferably 0.75 or less.

[0094] Glass X1 In the glass, Li2O / Na2O, which is the ratio of the Li2O content to the Na2O content, is 1.5 or more and 10 or less. When Li2O / Na2O is 1.5 or more, Li ions in the glass and Na ions in the molten salt composition are efficiently exchanged. When Li2O / Na2O is 10 or less, the resistance of the glass can be reduced. Li2O / Na2O is preferably 2 or more, more preferably 4 or more, and even more preferably 6 or more, and is preferably 9 or less, more preferably 8 or less, and even more preferably 7 or less.

[0095] Glass X2 In order to improve the meltability of the glass raw material, the total content of Na2O and K2O (Na2O+K2O) is preferably 1% or more, more preferably 2% or more. X2 In the above, the ratio of the K2O content to the total content of Li2O, Na2O and K2O (hereinafter referred to as R2O), K2O / R2O, is preferably 0.2 or less, since this improves the chemical strengthening properties and chemical durability. K2O / R2O is more preferably 0.15 or less, and even more preferably 0.10 or less. R2O is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more. R2O is preferably 29% or less, and more preferably 26% or less.

[0096] MgO may be contained to reduce the viscosity during melting. When MgO is contained, the content is preferably 1% or more, more preferably 2% or more, and even more preferably 3% or more. On the other hand, if the content of MgO is too high, it becomes difficult to increase the compressive stress layer during chemical strengthening treatment, and the resistance of the glass increases. The content of MgO is 10% or less, preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, and particularly preferably 6% or less.

[0097] CaO may be contained to reduce the viscosity during melting. When CaO is contained, its content is preferably 1% or more, more preferably 2% or more, and even more preferably 3% or more. On the other hand, if the CaO content is too high, the resistance of the glass increases. The CaO content is 10% or less, preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, and particularly preferably 6% or less.

[0098] SrO may be contained to reduce the viscosity during melting. When SrO is contained, the content is preferably 0.5% or more, more preferably 1% or more, and even more preferably 2% or more. On the other hand, if the content of SrO is too high, the resistance of the glass increases. The content of SrO is 5% or less, preferably 4.5% or less, more preferably 4% or less, even more preferably 3.5% or less, and particularly preferably 3% or less.

[0099] When ZnO is contained, its content is preferably 0.5% or more, more preferably 1% or more, and even more preferably 2% or more. On the other hand, if the ZnO content is too high, the thermal expansion coefficient becomes small. The ZnO content is 5% or less, preferably 4.5% or less, more preferably 4% or less, even more preferably 3.5% or less, and particularly preferably 3% or less.

[0100] When TiO2 is contained, its content is preferably 0.05% or more, more preferably 0.1% or more, and even more preferably 0.2% or more. On the other hand, if the TiO2 content is too high, devitrification occurs during glass melting. The TiO2 content is 3% or less, preferably 2.5% or less, more preferably 2% or less, even more preferably 1.7% or less, and particularly preferably 1.4% or less.

[0101] Although ZrO2 does not have to be contained, it is preferable to contain it from the viewpoint of increasing the surface compressive stress of the chemically strengthened glass. When ZrO2 is contained, its content is preferably 0.1% or more, more preferably 0.15% or more, even more preferably 0.2% or more, particularly preferably 0.25% or more, typically 0.3% or more. On the other hand, if the content of ZrO2 is too high, devitrification defects are likely to occur, making it difficult to increase the compressive stress value during chemical strengthening treatment. The content of ZrO2 is 3% or less, preferably 2% or less, more preferably 1.5% or less, even more preferably 1% or less, and particularly preferably 0.8% or less.

[0102] SnO2 may be contained as a clarifier during glass production. When SnO2 is contained, its content is preferably 0.02% or more, more preferably 0.05% or more, and even more preferably 0.1% or more. On the other hand, if the SnO2 content is too high, it may affect the color. The SnO2 content is 1% or less, preferably 0.5% or less, more preferably 0.3% or less, even more preferably 0.2% or less, and particularly preferably 0.1% or less.

[0103] Glass X1 In the above, P2O5 may be contained to increase the compressive stress layer due to chemical strengthening. When P2O5 is contained, its content is preferably 0.1% or more, more preferably 0.2% or more, and even more preferably 0.3% or more. On the other hand, if the content of P2O5 is too high, the durability against acids and bases decreases. The content of P2O5 is 1% or less, preferably 0.8% or less, more preferably 0.7% or less, even more preferably 0.6% or less, and particularly preferably 0.5% or less.

[0104] Glass X2 In the above, P2O5 is a component of Li3PO4 crystal and is essential. The content of P2O5 is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, particularly preferably 2% or more, and extremely preferably 2.5% or more in order to promote crystallization. On the other hand, if the content of P2O5 is too high, phase separation occurs easily during melting and acid resistance is significantly reduced, so the content of P2O5 is preferably 5% or less, more preferably 4.8% or less, even more preferably 4.5% or less, and particularly preferably 4.2% or less.

[0105] Glass X2 In the above, SiO2, Al2O3, P2O5 and B2O3 are glass network formers (hereinafter also referred to as NWFs), and the strength of the glass-ceramics increases when the total amount of NWFs is large. This improves the fracture toughness of the glass-ceramics. From this viewpoint, glass X2 In the above, the total amount of NWF is preferably 60% or more, more preferably 63% or more, and particularly preferably 65% ​​or more. However, since glass with too much NWF has a high melting temperature and is difficult to manufacture, the total amount is preferably 85% or less, more preferably 80% or less, and still more preferably 75% or less.

[0106] Glass X2 In the above, the ratio of the total amount of Li2O, Na2O and K2O to the NWF, i.e., the total amount of SiO2, Al2O3, P2O5 and B2O3, is preferably 0.20 to 0.60. Li2O, Na2O and K2O are network modifiers, and decreasing the ratio to the NWF increases the gaps in the network, improving impact resistance. Therefore, the NWF is preferably 0.60 or less, more preferably 0.55 or less, and particularly preferably 0.50 or less. On the other hand, since these are components necessary for chemical strengthening, in order to enhance the chemical strengthening properties, the NWF is preferably 0.20 or more, more preferably 0.25 or more, and particularly preferably 0.30 or more.

[0107] B2O3 may be contained to improve the scratch resistance of glass. When B2O3 is contained, its content is preferably 1% or more, more preferably 3% or more, and even more preferably 5% or more. On the other hand, if the content of B2O3 is too high, striae may be generated during melting, or phase separation may occur easily, which may lead to a deterioration in the quality of the glass for chemical strengthening. The content of B2O3 is 10% or less, preferably 9.5% or less, more preferably 9% or less, even more preferably 8.5% or less, and particularly preferably 8% or less.

[0108] Glass X1 In the present invention, the B2O3 / P2O5 ratio is preferably 2.5 or more and 500 or less. By having the B2O3 / P2O5 ratio of 2.5 or more, the occurrence of striae during melting of the glass can be prevented, and stable production can be achieved. The B2O3 / P2O5 ratio is more preferably 5 or more, even more preferably 10 or more, and particularly preferably 50 or more. By having the B2O3 / P2O5 ratio of 500 or less, the glass becomes easy to ion exchange and is less susceptible to scratches. The B2O3 / P2O5 ratio is more preferably 450 or less, even more preferably 400 or less, particularly preferably 300 or less, and most preferably 250 or less.

[0109] Y2O3 may be contained to improve the fracture toughness value of the glass. When Y2O3 is contained, its content is preferably 0.1% or more, more preferably 0.2% or more, even more preferably 0.5% or more, and particularly preferably 1% or more. On the other hand, if it is too much, it becomes difficult to increase the compressive stress layer during chemical strengthening treatment. The content of Y2O3 is 3% or less, preferably 2.5% or less, more preferably 2% or less, and even more preferably 1.5% or less.

[0110] Fe2O3 may be contained to reduce the resistance of the glass. When Fe2O3 is contained, its content is preferably 0.01% or more, more preferably 0.02% or more, and even more preferably 0.04% or more. On the other hand, if the content of Fe2O3 is too high, the glass becomes colored, and its marketability as a cover glass for electronic devices is impaired. The content of Fe2O3 is 0.1% or less, preferably 0.09% or less, more preferably 0.08% or less, even more preferably 0.07% or less, and particularly preferably 0.06% or less.

[0111] BaO, SrO, MgO, CaO and ZnO are all components that improve the meltability of glass and may be contained.

[0112] Of these, BaO, SrO, and ZnO are glass X2 In the present invention, BaO may be added to improve the refractive index of the residual glass and bring it closer to the precipitated crystal phase, thereby improving the light transmittance of the crystallized glass and reducing the haze value. In this case, the total content of BaO, SrO and ZnO (hereinafter, BaO+SrO+ZnO) is preferably 0.3% or more, more preferably 0.5% or more, even more preferably 0.7% or more, and particularly preferably 1% or more. On the other hand, these components may reduce the ion exchange rate. In order to improve the chemical strengthening properties, BaO+SrO+ZnO is preferably 2.5% or less, more preferably 2% or less, even more preferably 1.7% or less, and particularly preferably 1.5% or less.

[0113] La2O3, Nb2O5 and Ta2O5 are all components that make it difficult for chemically strengthened glass to scatter fragments when broken, and may be contained to increase the refractive index. When these are contained, the total content of La2O3, Nb2O5 and Ta2O5 (hereinafter, La2O3+Nb2O5+Ta2O5) is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. In addition, in order to make the glass less susceptible to devitrification during melting, La2O3+Nb2O5+Ta2O5 is preferably 4% or less, more preferably 3% or less, even more preferably 2% or less, and particularly preferably 1% or less.

[0114] CeO2 may also be contained. CeO2 may suppress coloring by oxidizing the glass. When CeO2 is contained, the content is preferably 0.03% or more, more preferably 0.05% or more, and even more preferably 0.07% or more. In order to increase transparency, the content of CeO2 is preferably 1.5% or less, and more preferably 1.0% or less.

[0115] When chemically strengthened glass is used after coloring, coloring components may be added to the extent that the desired chemical strengthening characteristics are not hindered. Examples of coloring components include Co3O4, MnO2, Fe2O3, NiO, CuO, Cr2O3, V2O5, Bi2O3, SeO2, Er2O3, and Nd2O3.

[0116] The total content of coloring components is preferably within the range of 1% or less. If it is desired to increase the visible light transmittance of the glass, it is preferable that these components are substantially not contained.

[0117] In order to improve weather resistance against ultraviolet light irradiation, HfO2, Nb2O5, and Ti2O3 may be added. When added for the purpose of improving weather resistance against ultraviolet light irradiation, the total content of HfO2, Nb2O5, and Ti2O3 is preferably 1% or less, more preferably 0.5% or less, and even more preferably 0.1% or less, in order to suppress the influence on other properties.

[0118] In addition, SO3, chlorides, and fluorides may be appropriately contained as clarifiers for melting glass. The total content of components functioning as clarifiers is preferably 2% or less, more preferably 1% or less, and even more preferably 0.5% or less, expressed as mass% on an oxide basis, since adding too much of them affects the strengthening characteristics and crystallization behavior. The lower limit is not particularly limited, but typically, the total content is preferably 0.05% or more, expressed as mass% on an oxide basis.

[0119] When SO3 is used as a fining agent, the content of SO3 is preferably 0.01% or more, more preferably 0.05% or more, and even more preferably 0.1% or more, expressed as mass% on the oxide basis, since the effect is not observed if the content is too small. Also, when SO3 is used as a fining agent, the content of SO3 is preferably 1% or less, more preferably 0.8% or less, and even more preferably 0.6% or less, expressed as mass% on the oxide basis.

[0120] When Cl is used as a fining agent, if too much is added, it affects physical properties such as strengthening characteristics, so the Cl content is preferably 1% or less, more preferably 0.8% or less, and even more preferably 0.6% or less, expressed as mass % on the oxide basis. Also, if Cl is used as a fining agent, if the Cl content is too low, no effect is observed, so the Cl content is preferably 0.05% or more, more preferably 0.1% or more, and even more preferably 0.2% or more, expressed as mass % on the oxide basis.

[0121] When SnO2 is used as a clarifier, the content of SnO2 is preferably 1% or less, more preferably 0.5% or less, and even more preferably 0.3% or less, expressed as mass% on the oxide basis, since too little SnO2 content affects crystallization behavior. Also, when SnO2 is used as a clarifier, the content of SnO2 is not effective if it is too little, so it is preferably 0.02% or more, more preferably 0.05% or more, and even more preferably 0.1% or more, expressed as mass% on the oxide basis.

[0122] It is preferably free of As2O3. It may contain impurities such as Sb2O3 as trace components. When containing Sb2O3, it is preferably 0.3% or less, more preferably 0.1% or less, and most preferably not contain it.

[0123] Specifically, as the base composition of this chemically strengthened glass, for example, glasses having the following compositions (i) to (iii) are preferable. (i) A glass containing 66% of SiO2, 11% of Li2O, 11% of Al2O3, 5.5% of Na2O, 1.5% of K2O, 1.3% of ZrO2, 3% of MgO, 0.5% of Y2O3, and 0.3% of other components. (ii) A glass containing 68% of SiO2, 11% of Li2O, 12% of Al2O3, 1.6% of Na2O, 1.6% of K2O, 0.6% of ZrO2, 1.4% of Y2O3, 3.5% of MgO, and 0.3% of other components. (iii) A glass containing 57% of SiO2, 11% of Li2O, 18% of Al2O3, 3% of Na2O, 0.5% of K2O, 0.5% of P2O5, 6% of B2O3, and 4.5% of MgO.

[0124] It is more preferable that the base composition of this chemically strengthened glass including the first to third embodiments is the same as the composition described later in the section <Glass: Sixth Embodiment>.

[0125] <<Set Drop Strength>> The chemically strengthened glass of this embodiment preferably has a #80 drop strength of 40 cm or more, more preferably 42 cm or more, still more preferably 43 cm or more, and particularly preferably 45 cm or more.

[0126] <<Four-Point Bending Strength>> The chemically strengthened glass of this embodiment preferably has a four-point bending strength of 550 MPa or more, more preferably 600 MPa or more, still more preferably 700 MPa or more, and particularly preferably 750 MPa or more.

[0127] <Manufacturing Method of Chemically Strengthened Glass: Fourth and Fifth Embodiments> Hereinafter, as specific embodiments of the method for producing chemically strengthened glass according to the present invention, a fourth embodiment and a fifth embodiment will be described. In this specification, the method for producing chemically strengthened glass according to the present invention including the fourth embodiment and the fifth embodiment will also be abbreviated as "this production method".

[0128] [Method for producing chemically strengthened glass according to the fourth embodiment] A method for producing chemically strengthened glass according to a fourth embodiment of the present invention is a method for producing chemically strengthened glass, comprising at least a first ion exchange treatment in which a glass for chemical strengthening is brought into contact with a first molten salt composition, and a second ion exchange treatment in which, after the first ion exchange treatment, the glass for chemical strengthening is brought into contact with a second molten salt composition at 350 to 450° C. for 150 minutes or more, and the glass for chemical strengthening has, in mole % on an oxide basis, SiO2 55-75%, Li2O 3~15%, Al2O3 8~25% It is characterized by containing

[0129] [Method for producing chemically strengthened glass according to the fifth embodiment] A method for producing chemically strengthened glass according to a fifth embodiment of the present invention is a method for producing chemically strengthened glass, comprising at least a first ion exchange treatment in which a glass for chemical strengthening is brought into contact with a first molten salt composition, and a second ion exchange treatment in which, after the first ion exchange treatment, the glass for chemical strengthening is brought into contact with a second molten salt composition, wherein the first ion exchange treatment is performed at 350 to 450° C. for 150 minutes or longer, the first molten salt composition contains Li ions, and the glass for chemical strengthening has, in mole % on an oxide basis, SiO2 55-75%, Li2O 3~15%, It is characterized by containing 8 to 25% Al2O3.

[0130] <<Glass for chemical strengthening>> One aspect of the chemically strengthened glass of this embodiment contains, in mole % on an oxide basis, 55 to 75% SiO2, 3 to 15% Li2O, and 8 to 25% Al2O3. Another aspect of the chemically strengthened glass of this embodiment contains, in mole % on an oxide basis, 40 to 70% SiO2, 10 to 35% Li2O, and 1 to 15% Al2O3. The chemically strengthened glass preferably has the composition described above in the section <<Base composition of chemically strengthened glass>>, and more preferably has the composition described below in the section <<Glass: Sixth embodiment>>. To obtain glass of the above composition, glass raw materials are appropriately mixed and heated and melted in a glass melting furnace. The glass is then homogenized by bubbling, stirring, adding a clarifier, etc., formed into a glass plate of a predetermined thickness, and slowly cooled. Alternatively, the glass may be formed into a plate by forming it into a block shape, slowly cooling it, and then cutting it.

[0131] Examples of methods for forming into a plate include the float method, the press method, the fusion method, and the down-draw method. In particular, when producing a large glass plate, the float method is preferred. In addition, continuous forming methods other than the float method, such as the fusion method and the down-draw method, are also preferred.

[0132] The chemically strengthened glass may be crystallized glass. In the case of crystallized glass, it is preferable that the crystallized glass contains one or more crystals selected from the group consisting of lithium silicate crystals, lithium aluminosilicate crystals, and lithium phosphate crystals. As the lithium silicate crystals, lithium metasilicate crystals, lithium disilicate crystals, etc. are preferable. As the lithium phosphate crystals, lithium orthophosphate crystals, etc. are preferable. As the lithium aluminosilicate crystals, β-spodumene crystals, petalite crystals, etc. are preferable.

[0133] The crystallization rate of the crystallized glass is preferably 10% or more in order to increase the mechanical strength, more preferably 15% or more, even more preferably 20% or more, and particularly preferably 25% or more. In order to increase the transparency, it is preferably 70% or less, more preferably 60% or less, and particularly preferably 50% or less. A small crystallization rate is also excellent in that it is easy to heat and bend. The crystallization rate can be calculated from the X-ray diffraction intensity by the Rietveld method. The Rietveld method is described in "Crystal Analysis Handbook" edited by the editorial committee of the Japanese Crystallographic Society (Kyoritsu Shuppan, 1999, p492-499).

[0134] The average particle size of the precipitated crystals of the crystallized glass is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, and particularly preferably 100 nm or less, in order to increase transparency. The average particle size of the precipitated crystals can be obtained from a transmission electron microscope (TEM) image. It can also be estimated from a scanning electron microscope (SEM) image.

[0135] <<Chemical strengthening treatment>> Chemical strengthening is a process in which glass is brought into contact with a metal salt, such as by immersing the glass in a molten liquid of a metal salt (e.g., potassium nitrate) containing a metal ion with a large ionic radius (typically Na ion or K ion), thereby replacing the metal ion with a small ionic radius (typically Na ion or Li ion) in the glass with a metal ion with a large ionic radius (typically Na ion or K ion for Li ion, and K ion for Na ion).

[0136] Examples of molten salts for performing chemical strengthening treatment include nitrates, sulfates, carbonates, and chlorides. Examples of nitrates include lithium nitrate, sodium nitrate, potassium nitrate, cesium nitrate, and silver nitrate. Examples of sulfates include lithium sulfate, sodium sulfate, potassium sulfate, cesium sulfate, and silver sulfate. Examples of carbonates include lithium carbonate, sodium carbonate, and potassium carbonate. Examples of chlorides include lithium chloride, sodium chloride, potassium chloride, cesium chloride, and silver chloride. These molten salts may be used alone or in combination.

[0137] The molten salt composition is preferably one containing a nitrate as a main component, more preferably one containing sodium nitrate or potassium nitrate as a main component. Here, "containing" as a main component means that the content of the molten salt composition is 80 mass%.

[0138] The present production method is characterized by including the following first ion exchange treatment and second ion exchange treatment in this order. (First ion exchange treatment) A step of contacting glass for chemical strengthening with a first molten salt composition. (Second ion exchange treatment) A step of contacting the glass for chemical strengthening with a second molten salt composition after the first ion exchange treatment.

[0139] In one embodiment of the present manufacturing method, in the first ion exchange treatment, the glass for chemical strengthening preferably contains a first alkali metal ion, and the first molten salt composition preferably contains a second alkali metal ion having a larger ionic radius than the first alkali metal ion. In the second ion exchange treatment, the second molten salt composition preferably contains a third alkali metal ion having a larger ionic radius than the second alkali metal ion. More preferably, the second molten salt composition further contains the first alkali metal ion.

[0140] In the present embodiment, the first ion exchange treatment exchanges the first alkali metal ions in the glass for chemical strengthening with the second alkali metal ions in the first molten salt composition. In the second ion exchange treatment, the second alkali metal ions in the glass for chemical strengthening are exchanged with the third alkali metal ions in the second molten salt composition.

[0141] 2(a) and (b) are schematic diagrams illustrating ion exchange in this embodiment. In this embodiment, the first alkali metal ion is a lithium (Li) ion, the second alkali metal ion is a sodium (Na) ion, and the third alkali metal ion is a potassium (K) ion.

[0142] FIG. 2(a) shows the first ion exchange treatment, and FIG. 2(b) shows the second ion exchange treatment. In the first ion exchange process, the following ion movements occur: 1-1) The second alkali metal ion is introduced into the glass by ion exchange between the first alkali metal ion in the glass for chemical strengthening and the second alkali metal ion in the first molten salt composition. 1-2) The second alkali metal ions introduced into the glass for chemical strengthening by the ion exchange of 1-1) above are released from the glass by ion exchange [reverse ion exchange, A in (a) of FIG. 2] between the second alkali metal ions in the first molten salt composition, thereby reducing excess second alkali metal ions in the surface layer of the glass and controlling the tensile stress below the CT limit value. 1-3) The second alkali metal ions are diffused from the glass surface to a depth of preferably about 18% of the plate thickness [B in FIG. 2(a)]. This results in the formation of CS 90 can be improved.

[0143] In the second ion exchange process, the following ion movements occur: 2-1) The third alkali metal ion in the second molten salt composition is exchanged with the second alkali metal ion in the glass for chemical strengthening, thereby introducing the third alkali metal ion into the surface layer of the glass, thereby improving the surface compressive stress of the glass [C in (b) of FIG. 2]. 2-2) The second alkali metal ions diffused into the glass in the above 1-3) are further diffused to the deeper layers of the glass. This allows the CS 90 can be improved. Due to the movement of the ions, as shown in FIG. 2(b), for example, the second alkali metal ions can be reduced in the region from a depth of about 3.3 μm from the surface to a depth of about 80 to 90 μm from the surface to reduce the compressive stress, and by maintaining the Cs high in the region deeper than 90 μm from the surface, a stress profile with high surface compressive stress can be formed.

[0144] Each ion exchange treatment in this production method will be described in detail below. <<First ion exchange treatment>> The first ion exchange treatment is a step of contacting the glass for chemical strengthening with a first molten salt composition. In this embodiment, the temperature and time in the first ion exchange treatment are preferably set by observing the saturation behavior of the compressive stress layer depth DOC with the progress of the first ion exchange time. Specifically, for example, in the first ion exchange treatment, when the plate thickness is t (mm), the temperature and time are preferably set so that the compressive stress layer depth DOC exceeds 180×t (μm). By making the DOC exceed 180×t, the CS 90 can be further improved.

[0145] In one embodiment, the temperature at which the first molten salt composition is brought into contact with the glass for chemical strengthening in the first ion exchange treatment is preferably 350° C. or higher, more preferably 360° C. or higher, and even more preferably 380° C. or higher. When the temperature of the first molten salt composition is 350° C. or higher, reverse ion exchange occurs sufficiently, which reduces the stress in the surface layer of the glass and facilitates the introduction of a compressive stress layer to a depth of about 18% of the plate thickness, thereby improving the CS 90 Moreover, the temperature of the first molten salt composition is usually 450° C. or lower, from the viewpoints of the risk of evaporation and changes in the composition of the molten salt.

[0146] In the first ion exchange treatment, when the time for contacting the first molten salt composition with the glass for chemical strengthening is 150 minutes or longer, reverse ion exchange occurs sufficiently, the stress in the surface layer of the glass is weakened, and a compressive stress layer is easily introduced to a depth of about 18% of the plate thickness, and CS 90 The heating time is more preferably 180 minutes or more, and further preferably 210 minutes or more.

[0147] Specifically, for example, when the temperature of the first molten salt composition with which the glass for chemical strengthening is brought into contact is 420° C., the contact time is preferably 360 minutes or more and 660 minutes or less. When the temperature of the first molten salt composition with which the glass for chemical strengthening is brought into contact is higher than 420° C., the contact time is preferably 600 minutes or less.

[0148] In one embodiment, in the first ion exchange treatment, it is preferable that the time t1 (minutes) for immersing the glass for chemical strengthening in the first molten salt composition with respect to the temperature T (°C) of the first molten salt composition satisfies the following formula. 90 can be maximized. -7.5T+3400 <t1<-7.5T+3850

[0149] t1 (min) is preferably greater than (-7.5T+3400), more preferably greater than (-7.5T+3500), and even more preferably greater than (-7.5T+3550). Also, t1 (min) is preferably less than (-7.5T+3850), more preferably less than (-7.5T+3800), and even more preferably less than (-7.5T+3700).

[0150] In the fourth embodiment, the first molten salt composition preferably contains lithium ions. In the fifth embodiment, the first molten salt composition contains lithium ions. The content of lithium ions in the first molten salt composition can be set, for example, as follows. When determining the temperature and time from the saturation behavior of DOC accompanying the progress of the first ion exchange, a lithium ion concentration that can make the number of fragments at the time of scratching equal to or less than the CT limit is simulated. The lithium ion concentration to be contained in the first molten salt composition can be set from the concentration.

[0151] In one embodiment, the lithium content in the first molten salt composition is preferably 0.010% by mass or more, more preferably 0.060% by mass or more, and even more preferably 0.15% by mass or more. When the lithium ion content in the first molten salt composition is 0.010% by mass or more, reverse ion exchange is sufficiently promoted, the surface compressive stress is reduced, and the internal tensile stress can be further suppressed, and the number of fractures at the time of scratching is easily kept below the CT limit. Since the lithium ions in the molten salt composition and SiO2 in the glass component are bonded to each other, which may cause a crystallinity defect in appearance, the lithium content in the first molten salt composition is preferably 1.0% by mass or less, more preferably 0.80% by mass or less, and even more preferably 0.60% by mass or less.

[0152] In one embodiment, the content of sodium nitrate in the first molten salt composition is preferably 92 mass% or more, more preferably 92.5 mass% or more, 93.0 mass% or more, 93.5 mass% or more, and further preferably 94 mass% or more, in the following order. When the content of sodium nitrate is within the above range, the amount of sodium introduced into the deep layer of the glass is increased, and the CS 90 can be further improved.

[0153] In one embodiment, when potassium nitrate is added to the first molten salt composition, the content thereof is preferably 35 mass% or less, and more preferably 25 mass% or less, 15 mass% or less, and 5 mass% or less, in that order. When the content of potassium nitrate is within the above range, sodium ions are easily introduced sufficiently into the deep layer of the glass.

[0154] <<Second ion exchange treatment>> This is a step of contacting the glass for chemical strengthening with a second molten salt composition after the first ion exchange treatment. In this embodiment, it is preferable to measure the surface ion concentration of the glass for chemical strengthening after the first ion exchange treatment to obtain the Na / Li ratio, and to determine the Na / Li ratio in the second molten salt composition based on the Na / Li ratio.

[0155] In one embodiment, the temperature and time of the second ion exchange treatment are preferably set so that the surface compressive stress layer depth DOL-tail value is 3.3 μm or more. By setting the DOL-tail to 3.3 μm or more, the bending strength can be further improved and mass production is facilitated.

[0156] In one embodiment, the glass for chemical strengthening is preferably immersed in the second molten salt composition at a temperature of 420° C. or higher. The temperature of the second molten salt composition is more preferably 422° C. or higher, and further preferably 425° C. or higher. The temperature of the second molten salt composition is usually 450° C. or lower from the viewpoints of the risk of evaporation and the composition change of the molten salt, and is more preferably 435° C. or lower from the viewpoint of preventing an excessive reduction in stress.

[0157] In one embodiment, the time for contacting the second molten salt composition with the glass for chemical strengthening is preferably 0.5 hours or more, more preferably 0.75 hours or more, and even more preferably 1 hour or more. By making the time 1.25 hours or more, the compressive stress can be further reduced in a region from the surface to a depth of about 80 to 90 μm, and the CS can be maintained higher in a region deeper than 90 μm from the surface. On the other hand, if the contact time is too long, the CS 50 Therefore, it is usually preferable that the time is 4 hours or less.

[0158] Specifically, for example, when the temperature of the second molten salt composition with which the glass for chemical strengthening is brought into contact is 420°C, the contact time is preferably 0.5 hours or more and 2 hours or less, more preferably 0.5 hours or more and 1.75 hours or less, and even more preferably 0.5 hours or more and 1.5 hours or less.

[0159] In one embodiment, in the second ion exchange treatment, it is preferable that the time t2 (minutes) for immersing the glass for chemical strengthening in the second molten salt composition with respect to the temperature T (°C) of the second molten salt composition satisfies the following formula, which makes it easy to make the value of the surface compressive stress layer depth DOL-tail 3.3 μm or more. -1×T+450 <t2<-4×T+1740

[0160] t2 (min) is preferably greater than (-1 x T + 450), more preferably greater than (-1 x T + 455), and even more preferably greater than (-1 x T + 460). Also, t2 (min) is preferably less than (-4 x T + 1740), more preferably less than (-4 x T + 1735), and even more preferably less than (-4 x T + 1730).

[0161] In the present embodiment, the second molten salt composition preferably contains lithium nitrate in an amount of 0% by mass or more and 5% by mass or less. By setting the lithium nitrate content in the second molten salt composition to 0% by mass or more and 5% by mass or less, the stress due to potassium can be sufficiently introduced into the surface layer, the surface layer compressive stress can be increased, and the bending strength can be further improved.

[0162] In one embodiment, the content of potassium nitrate in the second molten salt composition is preferably 90 mass% or more, more preferably 92 mass% or more, and further preferably 95 mass% or more. The upper limit is not particularly limited, but is usually 99.9 mass% or less.

[0163] The second molten salt composition may contain sodium nitrate. When the second molten salt composition contains sodium nitrate, the content of sodium nitrate is preferably 0.1 mass% or more, and more preferably 0.3 mass% or more. When the content of sodium nitrate is within the above range, CS 90 The effect of raising the

[0164] The second molten salt composition may further contain an additive other than the nitrate. Examples of the additive include silicic acid and specific inorganic salts. When the second molten salt composition contains the additive, the FSM-CS0 can be increased. The second molten salt composition may contain silicic acid as an additive. Silicic acid refers to a compound consisting of silicon, hydrogen, and oxygen, represented by the chemical formula nSiO2·xH2O, where n and x are natural numbers. Examples of such silicic acid include metasilicic acid (SiO2·H2O), metadisilicic acid (2SiO2·H2O), orthosilicic acid (SiO2·2H2O), pyrosiliic acid (2SiO2·3H2O), and silica gel [SiO2·mH2O (m is a real number from 0.1 to 1)].

[0165] By including silicic acid, the silicic acid adsorbs lithium ions and potassium ions can easily enter the glass, so that the stress of the surface layer of several μm can be increased while suppressing the CT. The amount of silicic acid added is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, and most preferably 0.5 mass% or more. The amount of silicic acid added is preferably 3 mass% or less, more preferably 2 mass% or less, and most preferably 1 mass% or less.

[0166] The silicic acid is preferably silica gel [SiO2·mH2O (m is a real number between 0.1 and 1)]. Silica gel has the advantage that it is easy to settle in the molten salt and easy to add and recover because the secondary particles of silica gel are relatively large. In addition, there is no risk of dust flying around, ensuring the safety of workers. Furthermore, it is a porous body, and the molten salt is easily supplied to the surfaces of the primary particles, so it has excellent reactivity and is effective in adsorbing lithium ions.

[0167] The second molten salt composition may contain a specific inorganic salt (hereinafter referred to as a flux) as an additive. As the flux, carbonates, bicarbonates, phosphates, sulfates, hydroxides, and chlorides are preferable, and it is preferable to contain at least one salt selected from the group consisting of K2CO3, Na2CO3, KHCO3, NaHCO3, K3PO4, Na3PO4, K2SO4, Na2SO4, KOH, NaOH, KCl, and NaCl. Particularly, it is more preferable to contain at least one salt selected from the group consisting of K2CO3 and Na2CO3, and even more preferable to be K2CO3.

[0168] The chemical strengthening treatment may be performed by an ion exchange treatment in two or more steps. When performing a three-step ion exchange treatment in the present embodiment, in the third ion exchange treatment, it is preferable to set the conditions of the ion exchange treatment (for example, the composition, temperature, and time of the molten salt composition) so that the surface compressive stress exceeds 1000 MPa.

[0169] When performing a third ion exchange treatment in which the chemically strengthened glass is brought into contact with the third molten salt composition after the second ion exchange treatment, the third molten salt composition preferably contains 98% by mass or more of potassium nitrate, more preferably 98.5% by mass or more, and even more preferably 99% by mass or more. By setting the content of potassium nitrate in the third molten salt composition to 98% by mass or more, CS 90 can be increased more.

[0170] In the present embodiment, when performing ion exchange in two or more steps, the chemically strengthened glass after the first ion exchange treatment preferably has CTave larger than CTA, and by the ion exchange treatment after the second ion exchange treatment, CTave is preferably made less than CTA.

[0171] The CT limit is obtained by the following formula (1). CTA corresponds to the CT limit and is a value determined by the composition of the chemically strengthened glass. Further, CTave corresponds to the average value of the tensile stress, and CTave is obtained by the following formula (2). If CTave < CTA, it is below the CT limit, and an explosive increase in the number of fractures during scratching can be suppressed.

[0172]

number

[0173] t: Plate thickness (mm) K1c: Fracture toughness value (MPa m 1 / 2 ) CTave=ICT / LCT...Equation (2) ICT: Integrated value of tensile stress (Pa m) LCT: Length of tensile stress area in the thickness direction (μm)

[0174] When a compressive stress layer is formed on the surface portion of a glass article by chemical strengthening treatment, a tensile stress corresponding to the total amount of compressive stress on the surface is inevitably generated in the center of the glass article. If this tensile stress value becomes too large, the glass article will break violently and fragments will scatter when it is broken. If the CT exceeds its threshold value, the CT limit, the number of fractures during damage will increase explosively. In this embodiment, when two or more stages of ion exchange are performed, it is preferable that the maximum tensile stress value of the stress profile formed inside the glass by the first ion exchange treatment (first ion exchange treatment) is greater than the CT limit. Since the maximum tensile stress value after the first ion exchange treatment is greater than the CT limit, compressive stress is sufficiently introduced by the first ion exchange treatment, and even after the stress value of the glass surface layer is reduced in the subsequent second ion exchange treatment, the CS 90 can be maintained high.

[0175] <Glass: Sixth embodiment> The glass according to the sixth embodiment of the present invention has the following properties: SiO2 55-75% Al2O3 8~25% Li2O 3~15% Na2O 1-5% K2O 0~3% MgO 0-10% CaO 0-10% SrO 0-5% ZnO 0-5% TiO2 0-3% ZrO2 0-3% SnO2 0-1% P2O5 0-1% B2O3 0-10% Y2O3 0-3% Fe2O3 content is 0-0.1%. Li2O / [Li2O+Na2O+K2O], which is the ratio of the Li2O content to the total content of Li2O, Na2O and K2O, is 0.5 to 0.9; The ratio of the Li2O content to the Na2O content, Li2O / Na2O, is 1.5 to 10, and It is characterized by having a Young's modulus of 80 GPa or more. Each composition is similar to that described in the section <<Base composition of chemically strengthened glass>> of the third embodiment.

[0176] The glass of this embodiment has the above composition. To obtain glass of the above composition, glass raw materials are appropriately mixed and heated and melted in a glass melting furnace. The glass is then homogenized by bubbling, stirring, adding a clarifier, etc., formed into a glass plate of a predetermined thickness, and slowly cooled. Alternatively, the glass may be formed into a plate by forming it into a block shape, slowly cooling it, and then cutting it.

[0177] Examples of methods for forming into a plate include the float method, the press method, the fusion method, and the down-draw method. In particular, when producing a large glass plate, the float method is preferred. In addition, continuous forming methods other than the float method, such as the fusion method and the down-draw method, are also preferred.

[0178] The glass of the present embodiment may be crystallized glass. The crystallized glass is the same as that described above in the section <<Glass for chemical strengthening>>.

[0179] The glass of this embodiment preferably has a Young's modulus of 80 GPa or more, more preferably 82 GPa or more, even more preferably 84 GPa or more, and particularly preferably 85 GPa or more. By having a Young's modulus of 80 GPa or more, a higher CTA can be achieved when chemically strengthened, and deep layer stress can be improved. The upper limit of the Young's modulus is not particularly limited, but from the viewpoint of the processability of the glass, it is usually 100 GPa or less, preferably 95 GPa or less, more preferably 90 GPa or less.

[0180] In the glass of the present embodiment, when a compressive stress layer is formed by ion exchange treatment at 380° C. for 4 hours using a molten salt of sodium nitrate, the compressive stress value CS at a depth of 30 μm from the surface of the compressive stress layer is 30 However, the CS is preferably 150 MPa or more. 30 Since the tensile strength is 150 MPa or more, the CTA can be easily increased by ion exchange treatment, and the deep compressive stress can be further increased by reducing the surface compressive stress and suppressing the internal tensile stress. 30 is preferably 160 MPa or more, more preferably 170 MPa or more, and further preferably 180 MPa or more. EXAMPLES

[0181] The present invention will be described below with reference to examples, but the present invention is not limited thereto.

[0182] <Evaluation of amorphous glass> (Young's modulus E) Measured by ultrasonic method.

[0183] (Fracture toughness value K1c) Fracture toughness value K1c (unit: MPa m 1 / 2 ) was measured using the IF method in accordance with JIS R1607:2015.

[0184] [CTA value] The CTA value was calculated from the following formula (1).

[0185]

number

[0186] t: Plate thickness (mm)

[0187] Table 1 shows the compositions of the glasses used in the test examples described later and the evaluation results.

[0188] [Table 1]

[0189] <Evaluation of chemically strengthened glass> The evaluation method of chemically strengthened glass will be described below. (EPMA) Measurements using EPMA were performed as follows. First, a glass sample was embedded in epoxy resin and mechanically polished in a direction perpendicular to the first main surface and the second main surface opposite the first main surface to prepare a cross-sectional sample. The polished cross-section was coated with C-coat and measured using an EPMA (JEOL: JXA-8500F). The acceleration voltage was 15 kV, the probe current was 30 nA, and the integration time was 1000 msec. / point, and a line profile of the Na X-ray intensity was obtained at 1 μm intervals.

[0190] (Stress Profile) The stress profile was measured using a scattered light photoelastic stress meter SLP-2000 and a glass surface stress meter FSM manufactured by Orihara Seisakusho.

[0191] (Surface resistivity) (1) Sample preparation and film formation process The glass sample used was a 120 x 60 x 0.7 mm glass sample. Before measuring the surface resistivity, a film was formed using the following procedure. A film was formed on a 120 x 60 x 0.7 mm glass sample using a sputtering device. A platinum film was formed on the glass surface. When forming the film, patterning based on JIS R3256:1998 was performed. (2)Surface resistivity measurement The surface resistivity was measured by the following method. The measurement device used was an ultra-microcurrent meter 5450. The glass sample used was 120×60×0.7 mm. The measurements were performed according to JIS C2141:1992 and JIS R3256:1998 using a three-terminal method. The applied voltage was 100 V, and the value was measured 180 seconds after the voltage application. The discharge time was 3 seconds.

[0192] (Drop test) For the drop strength test, the obtained 120 x 60 x 0.7 mm glass sample was fitted into a structure whose mass and rigidity were adjusted to match the size of a typical smartphone currently in use, and then a mock smartphone was prepared and allowed to freely drop onto #80 SiC sandpaper. The drop height was 5 cm. If the sample did not break, it was dropped from a height of 5 cm and then dropped again, and this process was repeated until the sample broke. The height at which the sample first broke was recorded as the drop height. The average break height obtained when 20 samples were dropped for each example was recorded as the "average set drop strength for #80 sandpaper."

[0193] (4PB strength) The chemically strengthened glass was processed into a strip of 120 mm x 60 mm, and a four-point bending test was performed under the conditions of a distance between the outer supports of the support of 30 mm, a distance between the inner supports of 10 mm, and a crosshead speed of 5.0 mm / min, to measure the four-point bending strength. The number of test pieces was 10. The chemically strengthened glass was processed into a strip, and then automatically chamfered (C chamfered) using a grinding wheel of No. 1000 (manufactured by Tokyo Diamond Tool Manufacturing Co., Ltd.), and the end faces were mirror-finished using a 0.1 mm diameter nylon brush and Showlox NZ abrasive grains (manufactured by Showa Denko Co., Ltd.) to obtain a 120 x 60 x 0.7 mm thick specimen.

[0194] [Test Example 1] Glass raw materials were mixed to obtain the composition of Glass A shown in Table 1 in mole percent based on oxides, and weighed out to obtain 800 g of glass. The mixed glass raw materials were then placed in a platinum crucible and placed in an electric furnace at 1600°C to melt for about 5 hours, degassed, and homogenized.

[0195] The molten glass was poured into a mold and held at the glass transition temperature for 1 hour, then cooled to room temperature at a rate of 0.5°C / min to obtain a glass block. The glass block was cut, ground, and finally mirror-polished on both sides to produce a glass plate with a size of 120 mm x 60 mm and a thickness of 0.7 mm.

[0196] The glass plate prepared by the above procedure was subjected to ion exchange under the conditions shown in Table 2 to obtain chemically strengthened glass. The obtained chemically strengthened glass was subjected to CTave and CS 90 The results of the measurement are shown in Figure 3. In Figure 3, each of Groups 1 to 3 shows the results of using a molten salt composition of the same components within the same group, at the same temperature, and with the ion exchange time being changed, as shown in Table 1.

[0197] [Table 2]

[0198] As shown in Figure 3, when ion exchange treatment was performed with a molten salt composition with a high sodium ion content, CT increased and CTave exceeded the CT limit. On the other hand, when an attempt was made to reduce CT in an ion exchange treatment using the same molten salt composition, deep layer stress tended to decrease. From this result, it was found that in the method for producing chemically strengthened glass of this embodiment, by increasing the amount of lithium ions contained in the molten salt composition, it is possible to realize high deep layer stress while keeping CTave below the CT limit.

[0199] [Test Example 2] A glass plate made of glass A was prepared in the same manner as in Test Example 1, and the glass plate was subjected to ion exchange under the conditions shown in Table 3 to obtain chemically strengthened glass. The CS of the obtained chemically strengthened glass was measured, and the results are shown in FIG.

[0200] [Table 3]

[0201] As shown in Figure 4, by including lithium ions in the molten salt composition, the compressive stress in the surface layer (0 to 80 μm) decreased, and the compressive stress in the surface layer decreased as the lithium ion content increased. This reduced the internal tensile stress in the deep layer below the CT limit, and it was found that the compressive stress in the deep layer could be increased while avoiding the CT limit.

[0202] [Test Example 3] Using the same procedure as in Test Example 1, a glass plate made of the above-mentioned glass A, and glass plates made of glass B and glass C having the glass compositions shown in Table 1 in terms of oxide-based mole percent were prepared. Each of the obtained glass plates was subjected to ion exchange under the conditions shown in Table 4 to obtain chemically strengthened glass. For the obtained chemically strengthened glass, the amount of sodium ions and the amount of lithium ions in the molten salt composition as well as the temperature and time of the ion exchange treatment were changed as shown in Table 4, and CS 90 The results of plotting and CTave are shown in Figure 5.

[0203] [Table 4]

[0204] As shown in Figure 5, glass C has a low possible CTave value and therefore a low possible CS 90 In contrast, glass A is a glass material that can have a high CTave due to ion exchange treatment compared to glass C. Therefore, it was found that the manufacturing method of chemically strengthened glass of this embodiment can further increase deep layer compressive stress by reducing surface compressive stress and suppressing internal tensile stress, particularly in glass materials that can have a high CTave due to ion exchange treatment such as glass A.

[0205] [Test Example 4] A glass plate made of Glass A was prepared in the same manner as in Test Example 1, and the glass plate was subjected to ion exchange under the conditions shown in Table 5 to obtain chemically strengthened glass. The results of evaluation of the glass plate and the chemically strengthened glass are shown in Table 5. Examples 1 to 7 in Table 5 are working examples, and Examples 8 to 10 are comparative examples. Blank spaces (horizontal lines) indicate no evaluation. The stress profile of Example 1 is shown in FIG. 6(a), and the stress profile of Example 8 is shown in FIG. 6(b).

[0206] In Table 5, the following notations apply: Na2O@center: Na2O concentration at the center depth of the plate thickness, expressed as mole percentage based on oxide (%) Na2O@30μm / Na2O@90μm: The Na2O concentration (%) at a depth of 30μm from the surface divided by the Na2O concentration (%) at a depth of 90μm from the surface, expressed as mole percentage based on oxide. Na2O@50μm / Na2O@center: The Na2O concentration (%) at a depth of 50μm from the surface divided by the Na2O concentration (%) at the center depth of the plate thickness, expressed as mole percentage based on oxide. FSM-CS0: Compressive stress value (MPa) on glass surface measured by FSM CS 30 : Compressive stress value at a depth of 30 μm from the glass surface (MPa) CS 50 : Compressive stress value at a depth of 50 μm from the glass surface (MPa) CS 30-50 :Integral value of compressive stress CS from the surface to a depth of 30 to 50 μm (Pa m) CS 90 : Compressive stress value at a depth of 90 μm from the glass surface (MPa) DOC: Depth of compressive stress layer (μm) CTave=ICT / LCT ICT: Integrated value of tensile stress (Pa m) LCT: Length of tensile stress area in the thickness direction (μm) K1c: Fracture toughness value (MPa m 1 / 2 ) DOL-tail: Surface compressive stress layer depth (μm) CS x '': Second derivative of compressive stress measured by SLP

[0207] [Table 5]

[0208] As shown in Table 5, Examples 1 to 4, which are examples, are compared with Examples 8 and 9, which are comparative examples, and Examples 5 and 6, which are examples, are compared with Examples 10 and 11, which are comparative examples, in terms of CS that contributes to the #80set drop strength. 90 It can be seen that the set drop strength was improved. Examples 1 to 4, which are examples, had higher bending strength than Comparative Examples 8 and 9, and Examples 5 to 7 had higher bending strength than Comparative Examples 10 and 11. The surface resistivities of Examples 1 to 7 were lower than Comparative Examples 8 to 11, being 10 log Ω / sq or less.< / ctave> < / cta>

Claims

1. The plate thickness is t (mm), and the compressive stress layer depth DOC is 180×t (μm) or more; The integral value of compressive stress from the surface to a depth of 30 to 50 μm, CS 30-50 is 12000 Pa m or less, and Compressive stress value CS at a depth of 90 μm from the surface 90 Chemically strengthened glass, wherein the strength is 175 × t-88 (MPa) or more.

2. The chemically strengthened glass according to claim 1, having a Young's modulus of 80 GPa or more.

3. Stress value CS at a depth x [μm] from the glass surface measured with a scattered light photoelastic stress meter x In the profile of [MPa], the stress value CS x The second derivative value CS x '' but C.S. x The chemically strengthened glass according to claim 1, which satisfies the following formula in the range of ≧0. -0.03≦CS x ''≦0.013

4. Surface compressive stress value FSM-CS 0 The chemically strengthened glass according to claim 1, wherein the strength of the glass is 800 MPa or more.

5. The surface resistivity is 10 log Ω / sq or less, Chemically strengthened glass having a Young's modulus of 80 GPa or more.

6. Na at a depth of 30 μm from the surface 2 The O concentration at a depth of 90 μm from the surface is 2 Chemically strengthened glass having a value divided by O concentration of 1.30 or less.

7. Na at a depth of 50 μm from the surface 2 The O concentration at the center of the plate thickness is 2 The chemically strengthened glass according to claim 6, wherein the value divided by the O concentration is 2 to 4.

8. Na at a depth of 90 μm from the surface 2 The O concentration at the center of the plate thickness is 2 The chemically strengthened glass according to claim 6, wherein the value divided by the O concentration is 2.4 or more.

9. The matrix composition is expressed as mole percent on an oxide basis. SiO 2 55 to 75% Li 2 O 3-15%, A 2 O 3 The chemically strengthened glass according to claim 1, 5 or 6, containing 8 to 25% by weight.

10. A first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition; A method for producing chemically strengthened glass, comprising at least a second ion exchange treatment in which the glass for chemical strengthening is contacted with a second molten salt composition after the first ion exchange treatment, In the first ion exchange treatment, the glass for chemical strengthening is contacted with the first molten salt composition at 350 to 450° C. for 150 minutes or more, The glass for chemical strengthening is, in terms of mole percent based on oxides, SiO 2 55 to 75% Li 2 O 3-15%, A 2 O 3 A method for producing chemically strengthened glass, comprising:

11. The method for producing chemically strengthened glass according to claim 10, wherein the first molten salt composition contains 0.01 to 1 mass% of lithium ions.

12. A first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition; A method for producing chemically strengthened glass, comprising at least a second ion exchange treatment in which the glass for chemical strengthening is contacted with a second molten salt composition after the first ion exchange treatment, the first ion exchange treatment is performed at 350 to 450° C. for 150 minutes or longer, and the first molten salt composition contains lithium ions; The glass for chemical strengthening is, in terms of mole percent based on oxides, SiO 2 55 to 75% Li 2 O 3-15%, A 2 O 3 A method for producing chemically strengthened glass, comprising:

13. The method for producing chemically strengthened glass according to claim 12, wherein the second molten salt composition contains 0 to 5 mass% of lithium nitrate.

14. A third ion exchange treatment is included in which the glass for chemical strengthening is contacted with a third molten salt composition after the second ion exchange treatment, The method for producing chemically strengthened glass according to claim 12, wherein the third molten salt composition contains 98 mass% or more of potassium nitrate.

15. The method for producing chemically strengthened glass according to any one of claims 10 to 14, wherein the CTave of the glass for chemical strengthening is made less than the CTA by the ion exchange treatment after the second ion exchange treatment. Here, CTA is calculated by the following formula (1), and CTave is calculated by the following formula (2). [0010] t: plate thickness (μm) K1c: Fracture toughness value (MPa m 1/2 ) CTave=ICT / LCT...Formula (2) ICT: integral value of tensile stress (Pa·m) LCT: Length of tensile stress area in the thickness direction (μm)

16. In mole percent based on oxide, SiO 2 55 to 75% A 2 O 3 8 to 25%, Li 2O 3-15%, Na 2 O 1-5%, K 2 O 0 to 3%, MgO 0 to 10%, CaO 0 to 10%, SrO 0 to 5%, ZnO 0 to 5%, TiO 2 0 to 3%, ZrO 2 0 to 3%, SnO 2 0 to 1%, P 2 O 5 0 to 1%, B 2 O 3 0 to 10%, Y 2 O 3 0 to 3%, Fe 2 O 3 Contains 0 to 0.1% Li 2 O, Na 2 O and K 2 Li relative to the total content of O 2 The ratio of the content of Li 2 O / [Li 2 O+Na 2 O+K 2 O] is 0.5 to 0.9, Na 2 Li relative to O content 2 The ratio of the content of Li 2 O / Na 2 O is 1.5 to 10, and Young's modulus is 80 GPa or more Glass.

17. P 2 O 5 B relative to the content of 2 O 3 The ratio of the content of B 2 O 3 / P 2 O 5The glass of claim 16, wherein the Mn is 2.5 to 500.

18. When a compressive stress layer is formed by ion exchange treatment at 380° C. for 4 hours using a molten salt of sodium nitrate, the compressive stress value CS at a depth of 30 μm from the surface of the compressive stress layer is 30 The glass according to claim 16 or 17, wherein the modulus of elasticity is 150 MPa or more.

Citation Information

Patent Citations

  • Strengthened glass with ultra deep depth of compression

    US10150698B2

  • Ion exchanged glasses via non-error function compressive stress profiles

    US9359251B2

  • Chemically toughened glass

    WO2018186402A1

Cited By

  • High-aluminum glass and preparation method thereof

    CN120965098A