Solid-state electrolyte and all-solid-state lithium ion battery

Surface treatment of LISICON-type oxide-based solid electrolytes with a silane coupling agent improves moisture resistance, maintaining ionic conductivity and preventing impurity formation in all-solid-state lithium-ion batteries.

JP2024166919AInactive Publication Date: 2024-11-29JX NIPPON MINING & METALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023083351
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

LISICON-type oxide-based solid electrolytes used in all-solid-state lithium-ion batteries are prone to purity loss due to moisture exposure, leading to decreased ionic conductivity from impurity phase formation.

Method used

Surface treatment of solid electrolyte particles with a silane coupling agent having an alkoxy group and an alkyl group with 3 or more carbon atoms, such as hexyltrimethoxysilane, to enhance moisture resistance by preventing water vapor adsorption.

Benefits of technology

The treated solid electrolytes exhibit improved moisture resistance, maintaining high ionic conductivity and preventing impurity phase formation, thereby enhancing the performance of all-solid-state lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166919000001_ABST
    Figure 2024166919000001_ABST
Patent Text Reader

Abstract

To provide a solid-state electrolyte and an all-solid-state lithium ion battery having an excellent resistance to moisture.SOLUTION: The solid electrolyte has solid electrolyte particles expressed by a composition formula 1: LiαAxMyO4 (A denotes one of Ge, Si, and Ti, M denotes one of V, P, and As, 3.25≤α≤3.75, 0.30≤x≤0.75, and 0.25≤y≤0.70 are satisfied in the composition formula 1), and the solid electrolyte particles have a surface surface-processed by a silane coupling agent having an alkoxy group and an alkyl group with at least 3 carbons.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid electrolyte and an all-solid-state lithium-ion battery. [Background technology]

[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries to be used as power sources for these devices has become important. Among these batteries, lithium-ion batteries have attracted attention from the viewpoint of their high energy density. In addition, there is a demand for improvements in the energy density and battery characteristics of lithium-ion secondary batteries for large-scale applications such as vehicle-mounted power sources and load leveling.

[0003] LISICON-type oxide-based solid electrolytes are expected to be the next-generation solid electrolyte for all-solid-state batteries as solid materials that conduct Li ions. In addition, it is possible to introduce Li deficiency or excess Li by replacing it with ions of different valence, and it has the advantage that materials can be prepared by combining various elements.

[0004] In Non-Patent Document 1, a LISICON-type oxide-based solid electrolyte, Li 3.5 Ge 0.5 V 0.5 They disclose that they combined O4 with NCM111 (a positive electrode active material containing Ni, Co and Mn in a 1:1:1 composition ratio), a Ni-Co-Mn ternary positive electrode active material, and co-sintered it using spark plasma sintering to create a cell, resulting in the production of a sintered body for a cell that exhibits stable charge / discharge behavior. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Toyoki Okumura, Tomonari Takeuchi, and Hironori Kobayashi, All-Solid-State Batteries with LiCoO2-Type Electrodes: Realization of an Impurity-Free Interface by Utilizing a Cosinterable Li3.5Ge0.5V0.5O4 Electrolyte, ACS Appl. Energy Mater. (2021), 4, 1, 30-34. [Non-Patent Document 2] M. Bose, A. Basu, D. Mazumdar, DN Bose, Solid solutions of Li3VO4 Li4GeO4 as solid electrolytes: NMR and related studies, Solid State Ionics, Volume 15, Issue 2, (1985), 101-107. Summary of the Invention [Problem to be solved by the invention]

[0006] All-solid-state lithium-ion batteries using non-flammable oxide-based solid electrolytes are attracting attention as next-generation batteries that are much safer and more reliable than conventional lithium-ion batteries. The material used as the solid electrolyte in these batteries is Li 3.5 Ge 0.5 V 0.5 O4 belongs to a group of materials known as LISICON-type structures. It has a relatively high ionic conductivity approaching 0.1 mS / cm for an oxide-based solid electrolyte, can be sintered at around 700°C, and is characterized by its ease of forming an interface with the positive electrode active material.

[0007] However, Li 3.5 Ge 0.5 V 0.5When many LISICON-type structural materials, including O4, are exposed to an atmosphere containing water vapor, the impurity phase Li2CO3 gradually precipitates via LiOH, causing a decrease in purity. For example, NMR and electrical conductivity studies of Li3VO4·Li4GeO4 solid solutions have shown that the activation energy is not affected by changes in composition over a wide range, but is very sensitive to moisture (Non-Patent Document 2). The decrease in purity of the solid electrolyte due to the formation of this impurity phase causes a problem of decreased ionic conductivity.

[0008] The present invention has been made in order to solve the above-mentioned problems, and has an object to provide a solid electrolyte and an all-solid-state lithium ion battery having good moisture resistance. [Means for solving the problem]

[0009] The present invention, which has been completed based on the above findings, is defined by the following (1) to (4). (1) Composition formula 1: Li α A x M y O4 (In the composition formula 1, A is Ge, Si or Ti, M is V, P or As, 3.25≦α≦3.75, 0.30≦x≦0.75, and 0.25≦y≦0.70.) The solid electrolyte particles are represented by The solid electrolyte particles have surfaces that are surface-treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms. (2) The solid electrolyte according to (1), wherein the alkyl group of the silane coupling agent is a linear alkyl group. (3) The solid electrolyte according to (1) or (2), wherein the silane coupling agent is hexyltrimethoxysilane, hexyltriethoxysilane, isobutyltrimethoxysilane, or isobutyltriethoxysilane. (4) An all-solid-state lithium ion battery comprising a solid electrolyte layer containing the solid electrolyte according to any one of (1) to (3), a positive electrode layer, and a negative electrode layer. Effect of the Invention

[0010] According to the present invention, it is possible to provide a solid electrolyte and an all-solid-state lithium ion battery having good moisture resistance. [Brief description of the drawings]

[0011] [Figure 1] 3 is a schematic diagram showing a bonding state due to a dehydration condensation reaction of hexyltrimethoxysilane, a silane coupling agent, on the surface of a solid electrolyte particle according to the present embodiment. FIG. [Diagram 2] FIG. 1 is a schematic diagram of an all-solid-state lithium-ion battery according to an embodiment of the present invention. [Diagram 3] 1 is an X-ray diffraction pattern according to Example 1. [Figure 4] 1 is an X-ray diffraction pattern according to Example 2. [Diagram 5] 1 is an X-ray diffraction pattern according to Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Next, the embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0013] <Solid electrolyte> The solid electrolyte of this embodiment is represented by the composition formula 1: Li α A x M y The solid electrolyte particles have a surface that has been surface-treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms.

[0014] The solid electrolyte particles of this embodiment are Li, which is a LISICON type solid electrolyte. α Gex V y The composition is a base material of O4, or a base material substituted with Si, Ti, P, or As. With such a composition, the solid electrolyte is a LISICON type having a large number of elements, so that the activation energy is reduced and a solid electrolyte with good ion conductivity is obtained. As a result, the capacity of the all-solid-state lithium-ion battery is increased. In the present invention, the solid electrolyte refers to a solid electrolyte having, in its skeleton, an oxo acid ion in which an oxygen atom is coordinately bonded to a central element, as a counter anion to a lithium ion.

[0015] In the solid electrolyte particles of this embodiment, if α is less than 3.25 in the above composition formula 1, the carrier concentration is low, so that the ion conductivity may be reduced. Also, if α is more than 3.75, the single-phase synthesis may be difficult. In the solid electrolyte particles of this embodiment, it is preferable that 3.4≦α≦3.7 in the above composition formula 1.

[0016] In the solid electrolyte particles of this embodiment, if x is less than 0.30 in the above composition formula 1, a phase with low ion conductivity such as Li4GeO4 phase may be generated. If x is more than 0.75, the crystal lattice becomes large, the distance between Li sites becomes long, and the ion conductivity may decrease. In the solid electrolyte particles of this embodiment, it is preferable that 0.4≦x≦0.6 in the above composition formula 1.

[0017] In the solid electrolyte particles of this embodiment, in the above composition formula 1, if y is less than 0.25, the effect of reducing activation energy by element substitution is weak, so the effect of improving ion conductivity may be small. In addition, if y is more than 0.70, impurity phases such as Li4VO4 may be generated, and ion conductivity may decrease. In the solid electrolyte particles of this embodiment, in the above composition formula 1, it is preferable that 0.3≦y≦0.6.

[0018] In the solid electrolyte of this embodiment, the solid electrolyte particles have a surface treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms. The silane coupling agent of this embodiment is a compound containing Si (silicon, silane) that has both a site that reacts with an organic compound or a site with high affinity with an organic compound (alkyl group having 3 or more carbon atoms) and a site that reacts with an inorganic compound (alkoxy group). The surface of the solid electrolyte particles that has been surface treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms is arranged so that the alkoxy group is located on the solid electrolyte particle side and the alkyl group is located on the opposite side of the solid electrolyte particle, and the alkoxy group is bonded to the surface of the solid electrolyte particle by a dehydration condensation reaction. FIG. 1 shows a schematic diagram showing a bonded state by a dehydration condensation reaction of hexyltrimethoxysilane of the silane coupling agent on the surface of the solid electrolyte particle according to this embodiment.

[0019] In this way, when the solid electrolyte particles have a surface treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms, when the solid electrolyte is exposed to an atmosphere containing water vapor, the silane coupling agent treated on the surface of the solid electrolyte particles suppresses the adsorption of water vapor to the surface of the solid electrolyte particles. It is presumed that one of the reasons for this is that the "alkyl group having 3 or more carbon atoms" has hydrophobicity. Therefore, the moisture resistance of the solid electrolyte of this embodiment is improved.

[0020] When the carbon number of the alkyl group of the silane coupling agent is 3 or more, the carbon group present on the surface of the solid electrolyte particle increases, and the adsorption of water vapor can be suppressed well. The upper limit of the carbon number of the alkyl group of the silane coupling agent is not particularly limited, but it is preferable that it is to the extent that does not hinder the performance of the solid electrolyte. From this viewpoint, the carbon number of the alkyl group of the silane coupling agent is preferably 3 to 16, more preferably 3 to 12, and even more preferably 3 to 8.

[0021] Although the alkyl group of the silane coupling agent can improve moisture resistance even if it is a branched alkyl group, it is more preferable that the alkyl group is a straight chain alkyl group. When the alkyl group of the silane coupling agent is a straight chain alkyl group, as shown in FIG. 1, the alkyl group of the silane coupling agent extends linearly to the opposite side of the solid electrolyte particle, so that the water vapor approaching the surface of the solid electrolyte particle can be expelled farther with a smaller number of carbon atoms. Therefore, the moisture resistance can be improved while maintaining the performance of the solid electrolyte.

[0022] When at least a portion of the surface of the solid electrolyte particle is surface-treated with the silane coupling agent, the moisture resistance is improved accordingly. However, from the viewpoint of maximally improving the moisture resistance, it is preferable that the entire surface of the solid electrolyte particle is surface-treated with the silane coupling agent.

[0023] Specific examples of the silane coupling agent include hexyltrimethoxysilane, hexyltriethoxysilane, isobutyltrimethoxysilane, and isobutyltriethoxysilane. These silane coupling agents have a linear or branched alkyl group having 4 to 6 carbon atoms, and since the number of carbon atoms is not too large, the performance of the solid electrolyte can be maintained. In addition, since they have a linear or one-branched alkyl group, they are particularly preferred silane coupling agents from the viewpoint of further improving moisture resistance.

[0024] The solid electrolyte of this embodiment may have an average particle size D50 (50% cumulative volume particle size D50) of 0.01 to 100 μm, 0.1 to 100 μm, or 0.1 to 50 μm. The smaller the average particle size D50 of the solid electrolyte, the larger the surface area per unit mass of the solid electrolyte. Therefore, the amount of the silane coupling agent attached to the surface per unit mass of the solid electrolyte increases, and the moisture resistance is further improved. From this viewpoint, the average particle size D50 of the solid electrolyte of this embodiment is preferably 0.1 to 10 μm, more preferably 0.1 to 4 μm, and even more preferably 0.1 to 2 μm.

[0025] The solid electrolyte of this embodiment can be produced as follows. First, the raw materials for the solid electrolyte particles are weighed out to obtain a predetermined composition in a glove box with an inert gas atmosphere such as argon gas or nitrogen gas. Examples of the raw materials used here include LiOH·H2O, GeO2, V2O5, SiO2, TiO2, H3PO4, and H3AsO3.

[0026] Next, the mixture is mixed for 5 to 30 minutes in a mortar or the like to produce a mixed powder. At this time, it is preferable to mix for such a time that the average particle size D50 (50% cumulative volume particle size D50) of the mixed powder becomes 5 to 40 μm.

[0027] Next, the mixed powder is placed in an alumina sagger and sintered at 600 to 1000°C for 1 to 20 hours to obtain a powder of the composition formula 1: Li α A x M y O4 (in composition formula 1, A is Ge, Si or Ti, M is V, P or As, 3.25≦α≦3.75, 0.30≦x≦0.75, and 0.25≦y≦0.70), it is possible to produce solid electrolyte particles of the present embodiment.

[0028] Next, a solution of a silane coupling agent adjusted to 4% by mass in absolute ethanol is prepared as a coating liquid. Next, the solid electrolyte particles and the coating liquid are placed in an Erlenmeyer flask so that the amount of the silane coupling agent is 0.05 g to 0.1 g per 1 g of solid electrolyte particles, and pure water is further added in an amount of 5 mass% of the coating liquid. The mixture is dispersed with a stirrer at room temperature for 30 minutes to prepare a slurry. Next, the slurry of the solid electrolyte particles and the coating liquid is centrifuged for solid-liquid separation, the supernatant liquid is removed, and the recovered solid is vacuum-dried at 60° C. for 12 hours using a tubular furnace. In this manner, the solid electrolyte according to this embodiment can be produced.

[0029] <All-solid-state lithium-ion battery> The all-solid-state lithium-ion battery according to the embodiment of the present invention includes a solid electrolyte layer, a positive electrode layer, and a negative electrode layer. The all-solid-state lithium-ion battery according to the embodiment of the present invention can be configured as shown in FIG. 2 using the solid electrolyte layer, the positive electrode layer, and the negative electrode layer.

[0030] (Solid electrolyte layer) The solid electrolyte layer of this embodiment is formed by the solid electrolyte of this embodiment. The average thickness of the solid electrolyte layer is not particularly limited and can be appropriately designed according to the purpose. The average thickness of the solid electrolyte layer of this embodiment may be, for example, 50 μm to 500 μm, or 50 μm to 100 μm.

[0031] The method for forming the solid electrolyte layer of the present embodiment is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method for forming the solid electrolyte layer of the present embodiment include sputtering using the target material of the solid electrolyte of the present embodiment described above, and compression molding of the solid electrolyte of the present embodiment described above.

[0032] (Positive electrode layer) The positive electrode layer of the present embodiment is a layer of a positive electrode mixture obtained by mixing a known positive electrode active material for lithium ion batteries with the above-mentioned solid electrolyte of the present embodiment or another solid electrolyte. The content of the positive electrode active material in the positive electrode layer is, for example, preferably 50% by mass or more and 99% by mass or less, and more preferably 60% by mass or more and 90% by mass or less.

[0033] Known positive electrode active materials for lithium ion batteries include, for example, those represented by the formula 2: Li a Ni b Co c Mn dO2 (in composition formula 2, 1.00≦a≦1.08, 0.60≦b≦0.90, and b+c+d=1.0). When the positive electrode active material of this embodiment is a high nickel NCM positive electrode active material having a high Ni ratio of 0.60 to 0.90 as shown in composition formula 2, the capacity of the all-solid-state lithium ion battery generally becomes high. From this viewpoint, it is more preferable that in composition formula 2, 0.80≦b≦0.90.

[0034] The positive electrode mixture may further include a conductive assistant. As the conductive assistant, a carbon material, a metal material, or a mixture thereof may be used. The conductive assistant may include at least one element selected from the group consisting of, for example, carbon, nickel, copper, aluminum, indium, silver, cobalt, magnesium, lithium, chromium, gold, ruthenium, platinum, beryllium, iridium, molybdenum, niobium, osmium, rhodium, tungsten, and zinc. The conductive assistant is preferably a highly conductive carbon element, carbon, or a metal element containing nickel, copper, silver, cobalt, magnesium, lithium, ruthenium, gold, platinum, niobium, osmium, or rhodium, or a mixture or compound thereof. As the carbon material, for example, carbon black such as Ketjen Black, acetylene black, denka black, thermal black, channel black, graphite, carbon fiber, activated carbon, etc. may be used.

[0035] The average thickness of the positive electrode layer of the all-solid-state lithium ion battery is not particularly limited and can be appropriately designed according to the purpose. The average thickness of the positive electrode layer of the all-solid-state lithium ion battery may be, for example, 1 μm to 100 μm, or 1 μm to 10 μm.

[0036] The method for forming the positive electrode layer of the all-solid-state lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. For example, the method for forming the positive electrode layer of the all-solid-state lithium ion battery includes a method of compression molding the positive electrode active material for the all-solid-state lithium ion battery.

[0037] (Negative electrode layer) The negative electrode layer of the all-solid-state lithium ion battery may be a layer of a known negative electrode active material for all-solid-state lithium ion batteries. The negative electrode layer may be a layer of a negative electrode mixture obtained by mixing a known negative electrode active material for all-solid-state lithium ion batteries with a solid electrolyte. The content of the negative electrode active material in the negative electrode layer is, for example, preferably 10% by mass or more and 99% by mass or less, and more preferably 20% by mass or more and 90% by mass or less.

[0038] The negative electrode layer may contain a conductive assistant, as in the positive electrode layer. The conductive assistant may be the same material as that described in the positive electrode layer. As the negative electrode active material, for example, a carbon material, specifically, artificial graphite, graphite carbon fiber, resin-calcined carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-calcined carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, non-graphitizable carbon, or a mixture thereof may be used. As the negative electrode material, for example, a metal itself, such as metallic lithium, metallic indium, metallic aluminum, or metallic silicon, or an alloy in combination with other elements or compounds may be used.

[0039] The average thickness of the negative electrode layer of the all-solid-state lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. The average thickness of the negative electrode layer of the all-solid-state lithium ion battery may be, for example, 1 μm to 100 μm, or 1 μm to 10 μm.

[0040] The method for forming the negative electrode layer of the all-solid-state lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method for forming the negative electrode layer of the all-solid-state lithium ion battery include a method of compression molding a negative electrode active material and a method of vapor-depositing a negative electrode active material.

[0041] Other members constituting the lithium ion battery are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include a positive electrode collector, a negative electrode collector, and a battery case.

[0042] The size and structure of the positive electrode current collector are not particularly limited and can be appropriately selected depending on the purpose. Examples of the material for the positive electrode current collector include die steel, stainless steel, aluminum, aluminum alloys, titanium alloys, copper, gold, and nickel. The positive electrode current collector may be in the form of, for example, a foil, a plate, or a mesh. The average thickness of the positive electrode current collector may be, for example, 10 μm to 500 μm, or 50 μm to 100 μm.

[0043] The size and structure of the negative electrode current collector are not particularly limited and can be appropriately selected depending on the purpose. Examples of the material for the negative electrode current collector include die steel, gold, indium, nickel, copper, and stainless steel. The negative electrode current collector may be in the form of, for example, a foil, a plate, or a mesh. The average thickness of the negative electrode current collector may be, for example, 10 μm to 500 μm, or 50 μm to 100 μm.

[0044] The battery case is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include known laminate films that can be used in conventional all-solid-state batteries, etc. Examples of the laminate film include a resin laminate film and a film in which a metal is vapor-deposited on a resin laminate film. The shape of the battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the shape of the battery include cylindrical, square, button, coin, and flat types.

[0045] <Moisture resistance> Li 3.5 Ge 0.5 V 0.5When many LISICON-type structural materials, including O4, are exposed to an atmosphere containing water vapor, Li2CO3, an impurity phase, is gradually precipitated via LiOH, causing a decrease in purity. In this embodiment, the moisture resistance of the solid electrolyte is evaluated by using the height of the Li2CO3 peak (2θ=31.65°-31.90°) obtained by powder X-ray diffraction method: XRD (θ / 2θ method) as an index of how much moisture the solid electrolyte contains. Then, to evaluate the moisture resistance of the solid electrolyte, an air exposure test is performed on the solid electrolyte, and XRD analysis is performed before and after the air exposure. Then, the maximum value of the height of the Li2CO3 peak (2θ=31.65°-31.90°) in the XRD results before air exposure (I a ) and the maximum value after exposure to air (I b ) compared to:I b / I a When the value is 2.0 or less, the film is evaluated as having good moisture resistance.

[0046] The above-mentioned XRD can be analyzed under the following conditions. X-ray diffraction equipment: Rigaku SmartLab ·Light source: CuKα line Voltage: 40kV ·Current: 30mA Scan speed: 2θ=7.5° / min EXAMPLES

[0047] The following examples are provided to provide a better understanding of the present invention and its advantages, but the present invention is not limited to these examples.

[0048] <1. Preparation of solid electrolyte> Example 1 In a glove box with an argon atmosphere, the raw materials were weighed so that the raw material composition was the stoichiometric composition of the target compound, and mixed in a mortar for 15 minutes to produce a mixed powder. Next, about 2 g of the mixed powder was placed in an alumina boat and calcined at 600 °C for 12 hours, and then crushed by hand in the mortar to obtain a calcined powder. After that, about 1 g of the calcined powder was placed again in the alumina boat and calcined at 700 °C for 12 hours to obtain Li 3.5 Ge 0.5 V 0.5 Solid electrolyte particles having a composition of O4 were obtained. Next, the obtained solid electrolyte particles were treated with a jet mill to obtain solid electrolyte particles having an average particle size D50 of 3.7 μm. Next, hexyltrimethoxysilane was dissolved in absolute ethanol to prepare a 4 mass % hexyltrimethoxysilane solution in absolute ethanol as a coating liquid. Next, the solid electrolyte particles and the coating liquid were placed in an Erlenmeyer flask so that 0.08 g of hexyltrimethoxysilane was used per 1 g of solid electrolyte particles, and approximately 1 mL of pure water was added thereto and dispersed with a stirrer at room temperature for 30 minutes to prepare a slurry. Next, the slurry of the solid electrolyte particles and the coating liquid was centrifuged for solid-liquid separation, the supernatant liquid was removed, and the recovered solid was vacuum-dried at 60° C. for 12 hours using a tubular furnace. After drying, the powder was lightly crushed with a pestle and mortar. In this way, Li coated with hexyltrimethoxysilane 3.5 Ge 0.5 V 0.5 O4 powder was obtained.

[0049] Example 2 The solid electrolyte particles used were synthesized Li 3.5 Ge 0.5 V 0.5 The same procedure as in Example 1 was carried out, except that solid electrolyte particles having an average particle size D50 of 0.4 μm were produced from O4 by planetary ball milling and jet milling.

[0050] Comparative Example 1 The same procedure as in Example 1 was carried out, except that the solid electrolyte particles were not subjected to a coating treatment.

[0051] 2. Evaluation of the composition of solid electrolyte particles 0.5 g of each sample of the solid electrolyte particles obtained in Examples 1 and 2 and Comparative Example 1 is weighed out and dissolved in various acids, and then the composition is analyzed using an inductively coupled plasma optical emission spectrometer (ICP-OES) "PS7800" manufactured by Hitachi High-Tech Corporation.

[0052] <3. Average particle size of solid electrolyte particles> For each of the solid electrolyte particle samples obtained in Examples 1 and 2 and Comparative Example 1, the average particle size D50 was measured as follows. 100 mg of each of the obtained solid electrolyte particles was dispersed by irradiating 40 W ultrasonic waves for 60 seconds at 50% flow rate using a Microtrac laser diffraction type particle size distribution measuring device "MT3300EXII", and then the particle size distribution was measured to obtain a cumulative particle size distribution curve based on volume. In the obtained cumulative particle size distribution curve, the volume particle size at 50% accumulation was taken as the 50% cumulative volume particle size D50 (average particle size D50) of the solid electrolyte particles. In addition, the water-soluble solvent used in the measurement was passed through a 0.02 μm filter, the solvent refractive index was 1.333, the particle permeability conditions were permeable, the particle refractive index was 1.81, the shape was non-spherical, the measurement range was 0.021 to 2000 μm, and the measurement time was 30 seconds.

[0053] <4. XRD evaluation of solid electrolyte (evaluation of moisture resistance)> The solid electrolyte samples obtained in Examples 1 and 2 (samples in which the surfaces of the solid electrolyte particles were surface-treated with a silane coupling agent) and the solid electrolyte sample obtained in Comparative Example 1 were exposed to the atmosphere under the following conditions. Approximately 0.5 g of each solid electrolyte sample was gently placed on an alumina boat, and the alumina boat was placed in a thermohygrostat (ADVANTEC, THR050FB) set at 60°C and 40% relative humidity for 15 hours. After placement, each sample was lightly crushed in a mortar and pestle to obtain an air-exposed sample. For each of the solid electrolyte samples obtained in Examples 1 and 2 (samples in which the surfaces of the solid electrolyte particles were surface-treated with a silane coupling agent) and the solid electrolyte sample obtained in Comparative Example 1, XRD evaluation was performed under the conditions shown below for the samples after the above-mentioned exposure to the atmosphere and the samples before and after the exposure to the atmosphere. X-ray diffraction equipment: Rigaku SmartLab ·Light source: CuKα line Voltage: 40kV ·Current: 30mA Scan speed: 2θ=7.5° / min The X-ray diffraction patterns obtained here according to Examples 1 and 2 and Comparative Example 1 before and after exposure to the atmosphere are shown in FIGS. 3 to 5, respectively. Regarding the maximum height of the Li2CO3 peak (2θ = 31.65° to 31.90°) in the XRD results, the maximum value (I a ) and the maximum value after exposure to air (I b ) compared to:I b / I a was calculated. The above manufacturing conditions and test results are shown in Table 1.

[0054] [Table 1]

[0055] (Evaluation Results) The solid electrolytes according to Examples 1 and 2 were all represented by the composition formula 1: Li α A x M y The solid electrolyte particles have a surface that has been surface-treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms. Therefore, the maximum value of the height of the Li2CO3 peak (2θ=31.65° to 31.90°) in the XRD result is the maximum value (I a ) and the maximum value after exposure to air (Ib ) compared to:I b / I a was 2.0 or less. Therefore, it is understood that the solid electrolytes according to Examples 1 and 2 all had good moisture resistance. On the other hand, in Comparative Example 1, the solid electrolyte particles did not have a surface treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms, and the maximum value (I a ) and the maximum value after exposure to air (I b ) compared to:I b / I a was greater than 2.0. This shows that the solid electrolyte according to Comparative Example 1 had poor moisture resistance. The solid electrolytes according to Examples 1 and 2 were composed of the composition formula 1: Li α A x M y In the composition of O4, A is Ge and M is V. Here, even if A is Si or Ti or M is P or As, the solid electrolyte particles have a surface treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms, so that the silane coupling agent acts as a physical barrier, and the alkyl group having 3 or more carbon atoms has a certain degree of hydrophobicity, so that it is considered that the effect of suppressing water vapor from being adsorbed on the solid electrolyte surface is generated. Therefore, even if A is Si or Ti or M is P or As in the composition formula 1 of the solid electrolyte, a solid electrolyte having a surface treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms is considered to have good moisture resistance compared to a solid electrolyte not having a surface treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms.

Claims

1. Composition formula 1: Li α A x M y O 4 (In the composition formula 1, A is Ge, Si or Ti, M is V, P or As, 3.25≦α≦3.75, 0.30≦x≦0.75, and 0.25≦y≦0.70.) The solid electrolyte particles are represented by The solid electrolyte particles have surfaces that are surface-treated with a silane coupling agent having an alkoxy group and an alkyl group having 3 or more carbon atoms.

2. The solid electrolyte according to claim 1 , wherein the alkyl group of the silane coupling agent is a straight-chain alkyl group.

3. 2. The solid electrolyte of claim 1, wherein the silane coupling agent is hexyltrimethoxysilane, hexyltriethoxysilane, isobutyltrimethoxysilane, or isobutyltriethoxysilane.

4. An all-solid-state lithium ion battery comprising a solid electrolyte layer comprising the solid electrolyte according to any one of claims 1 to 3, a positive electrode layer, and a negative electrode layer.