Chemically strengthened glass and production method for chemically strengthened glass
A two-stage ion exchange process with heat treatment optimizes compressive stress in chemically strengthened glass, addressing insufficient set drop strength and explosive fragmentation issues, enhancing resistance to impact and deformation.
Patent Information
- Application Number
- JP2024073707
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-29
AI Technical Summary
Existing chemically strengthened glass technologies do not adequately increase the total amount of compressive stress, leading to insufficient set drop strength, particularly in mobile terminal applications, and can result in explosive fragmentation due to excessive tensile stress.
A two-stage ion exchange process with appropriate heat treatment after the first ion exchange and before the second, optimizing conditions to enhance the total amount of compressive stress and reduce tensile stress, resulting in a larger compressive stress at depth and improved set drop strength.
The method produces chemically strengthened glass with enhanced set drop strength, reducing the risk of explosive fragmentation and improving resistance to impact and deformation, while maintaining the compressive stress within safe limits.
Smart Images

Figure 2024167060000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to chemically strengthened glass and a method for producing chemically strengthened glass. [Background technology]
[0002] Chemically strengthened glass is used for cover glass of mobile terminals, etc. Chemically strengthened glass is made by contacting glass with a molten salt composition such as sodium nitrate to cause ion exchange between alkali metal ions contained in the glass and alkali metal ions with a larger ionic radius contained in the molten salt composition, thereby forming a compressive stress layer on the surface of the glass. The strength of chemically strengthened glass depends on the stress profile represented by the compressive stress value (hereinafter also abbreviated as CS), which is a variable of the depth from the glass surface.
[0003] The cover glass of a mobile device, etc., may break due to deformation when dropped, etc. In order to prevent such breakage, i.e., breakage due to bending, it is effective to increase the compressive stress on the glass surface. For this reason, it has become common to form a high surface compressive stress of 700 MPa or more in recent years.
[0004] On the other hand, the cover glass of a mobile device, etc., may be broken by impact with a protruding object when the device is dropped onto asphalt or sand. In order to prevent such damage, that is, damage caused by impact, it is effective to increase the depth of the compressive stress layer and form the compressive stress layer in a deeper part of the glass to improve the strength.
[0005] For example, Patent Document 1 discloses a stress value CS at a depth of 90 μm from the glass surface. 90 It is described that this value contributes to improving resistance to cracking due to impact when dropped.
[0006] On the other hand, when a compressive stress layer is formed on the surface of a glass article, a tensile stress (hereinafter abbreviated as CT) corresponding to the total amount of compressive stress is inevitably generated in the center of the glass article. If the CT value becomes too large, the glass article will break violently and fragments will scatter when it is broken. If the CT value exceeds the threshold value (hereinafter abbreviated as CT limit), the glass will break on its own and the number of fractures when damaged may increase explosively. The CT limit is a value specific to the glass composition.
[0007] Therefore, chemically strengthened glass increases the surface compressive stress and forms a compressive stress layer extending to a deeper portion, while the total amount of compressive stress in the surface layer is designed so as not to exceed the CT limit.
[0008] One of the indicators for evaluating the strength of glass-based materials used in smartphones is the "set drop strength test." The "set drop strength test" is a test in which a sample made by bonding a smartphone case or a mock board simulating a smartphone to a glass-based material is dropped, and the drop height at which cracks occur is used as an indicator of strength. The set drop strength is an indicator that can reflect the strength of a glass-based material when it is used as a product. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] International Publication No. 2022 / 181812 Summary of the Invention [Problem to be solved by the invention]
[0010] In Patent Document 1, the set drop strength is improved by performing chemical strengthening treatment in a predetermined manner that focuses on the CT limit. However, in the stress profile, 90 However, in terms of increasing the
[0011] Therefore, the present invention is a CS 90The present invention also aims to provide a chemically strengthened glass having a CS which is larger than the total amount of compressive stress and thus has excellent set drop strength. 90 The object of the present invention is to provide a method for producing chemically strengthened glass, which can increase the compressive stress relative to the total amount of compressive stress, thereby improving the set drop strength. [Means for solving the problem]
[0012] As a result of intensive research, the present inventors have found that, when producing chemically strengthened glass by two or more stages of ion exchange treatment, by carrying out an appropriate heat treatment after the first ion exchange treatment and before the second ion exchange treatment, the CS of the obtained chemically strengthened glass can be improved. 90 It has been found that the compressive stress can be increased relative to the total amount of compressive stress, and this has led to the completion of the present invention.
[0013] That is, the present invention relates to the following 1 to 13. 1. Chemically strengthened glass having a thickness t [mm], The compressive stress layer depth DOC [μm] is 160t [μm] or more, Compressive stress value CS at a depth of 90 μm from the surface 90 [MPa] divided by the integral value of tensile stress ICT [MPa μm] CS 90 / ICT[μm -1 ] is 0.0012μm -1 That's it, chemically strengthened glass. 2. Said CS 90 2. The chemically strengthened glass according to 1, wherein the compressive strength is 5+50t [MPa] or more. 3. The DOC is the compressive stress value CS at a depth of 50 μm from the surface. 50 [MPa] divided by DOC / CS 50 3. The chemically strengthened glass according to 1 or 2 above, wherein the glass modulus is 0.8 μm / MPa or more. 4. Said CS 90 is the compressive stress value CS at a depth of 50 μm from the surface 50 Value divided by [MPa]CS 90 / CS 50 3. The chemically strengthened glass according to 1 or 2 above, wherein 5. Stress value CS at a depth x [μm] from the glass surface measured with a scattered light photoelastic stress meter x In the profile of [MPa], CS x Stress CS in the range ≧0 x The first derivative value of CS x 3. The chemically strengthened glass according to 1 or 2, wherein ' is less than 2. 6. Stress value CS at a depth x [μm] from the glass surface measured with a scattered light photoelastic stress meter x In the profile of [MPa], CS x Stress CS in the range ≧0 x The second derivative of CS x 3. The chemically strengthened glass according to 1 or 2 above, wherein .lambda.'' is −0.02 to 0.06. 7. The surface compressive stress value CS0 measured by a glass surface stress meter is 750 MPa or more; 3. The chemically strengthened glass according to 1 or 2. 8. The chemically strengthened glass according to 1 or 2 above, having a set drop strength of 40.5 cm or more as measured by a sandpaper set drop strength test under the following conditions. Conditions: An electronic device with the chemically strengthened glass mounted on #80 sandpaper, or an electronic device simulation structure in which the chemically strengthened glass is integrated with a housing that holds the chemically strengthened glass, is dropped from a height of 30 cm. If the chemically strengthened glass does not break, the drop height is increased by 5 cm and dropped again. As long as the chemically strengthened glass does not break after the drop, The step of dropping from a height increased by 5 cm is repeated. The height at which the chemically strengthened glass first breaks is defined as the crack height. A drop test is performed using 10 samples, and the average crack height of the 10 samples is defined as the set drop strength. 9. Chemically strengthened glass having a thickness t [mm], The Na ion diffusion depth, as determined from the Na ion concentration profile in the thickness direction of the chemically strengthened glass measured by an electron beam microanalyzer, is 290t [μm] or more; Chemically strengthened glass, in which the ratio ΔNa90 / ΔNa50 of the difference ΔNa50 [mol%] between the Na2O concentration in the matrix composition of the chemically strengthened glass and the Na2O concentration at a depth of 50 μm from the surface to the difference ΔNa90 [mol%] between the Na2O concentration in the matrix composition of the chemically strengthened glass and the Na2O concentration at a depth of 90 μm from the surface is 0.55 or more. 10. The chemically strengthened glass according to 9 above, wherein the ratio of the ΔNa90 [mol%] to the Na2O concentration [mol%] in the matrix composition of the chemically strengthened glass is 1.26 or more. 11. A first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition; A method for producing chemically strengthened glass, comprising: a second ion exchange treatment in which, after the first ion exchange treatment, the glass for chemical strengthening is brought into contact with a second molten salt composition, heat-treating the material after the first ion-exchange treatment and before the second ion-exchange treatment; First ion exchange treatment temperature T CT [℃] and the first ion exchange time t CT [min] is in the range of 10600 or less for the strengthening index (H value) defined by the following formula, and A method for producing chemically strengthened glass, wherein the heat treatment has a heat treatment effect index value (I value) defined by the following formula of 220 or more in the heat treatment.
[0014]
number
[0015]
number
[0016] However, in the above formula, t CT is the treatment time of the first ion exchange treatment [min], T CT is the temperature of the ion exchange treatment [°C], Σ[Me2O] is the sum of the alkali metal ion oxide concentrations in the glass for chemical strengthening. [mol%], t d is the first ion exchange treatment temperature T CT The time [minutes] during which the glass for chemical strengthening is kept at a temperature of 80% or more of [℃], T d is the temperature of the heat treatment [°C]. 12. Temperature T of the heat treatment d [℃] is 360℃ or more, or the heat treatment time t d 12. The method for producing chemically strengthened glass according to claim 11, wherein [minutes] is 10 minutes or longer. 13. Regarding the above-mentioned glass for chemical strengthening, when the CTA value calculated by the following formula (1) is x [MPa], The first ion exchange treatment causes the CTave value of the glass for chemical strengthening calculated by the following formula (2) to exceed x [MPa]; 13. The method for producing chemically strengthened glass according to claim 11 or 12, wherein the CTave value of the glass for chemical strengthening is made less than x [MPa] by the second ion exchange treatment.
[0017]
number
[0018] t: Plate thickness [mm] K1c: Fracture toughness value [MPa m 1 / 2 ] CTave=ICT / LCT...Equation (2) ICT: Tensile stress integral value [MPa μm] LCT: Length of tensile stress region in the thickness direction [μm] Effect of the Invention
[0019] According to the present invention, CS 90 According to the present invention, by performing an appropriate heat treatment after the first ion exchange treatment and before the second ion exchange treatment, it is possible to provide a chemically strengthened glass having a CS 90The present invention provides a method for producing chemically strengthened glass that can increase the compressive stress relative to the total amount of compressive stress, thereby improving the drop strength of the glass. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a diagram showing an example of a stress profile of the chemically strengthened glass according to this embodiment, measured by SLP. [Diagram 2] FIG. 2 is a diagram showing an example of a Na ion concentration profile in the sheet thickness direction of the chemically strengthened glass according to this embodiment. [Diagram 3] FIG. 3 is a diagram illustrating a schematic example of the steps of the chemical strengthening treatment. [Figure 4] 4(a) and (b) are diagrams showing an example of a stress profile of the chemically strengthened glass according to the present embodiment. The stress profiles shown in FIG. 4(a) and (b) were created by combining the stress profile information of the glass surface layer measured by SLP and the stress profile information of the inside of the glass measured by FSM. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] In this specification, the use of "to" indicating a numerical range means that the numerical values before and after it are included as the lower and upper limits. In addition, in this specification, the composition of the glass (content of each component) is expressed in mole percentage based on oxides, and mole % is simply expressed as "%", unless otherwise specified. In addition, in this specification, "substantially free" means that the content is below the impurity level contained in raw materials, that is, that it is not intentionally added. Specifically, for example, it is less than 0.1%.
[0022] In this specification, "amorphous glass" refers to glass that does not show diffraction peaks indicating crystals by powder X-ray diffraction. "Crystallized glass" is obtained by heating "amorphous glass" to precipitate crystals, and contains crystals. In this specification, "amorphous glass" and "crystallized glass" are sometimes collectively referred to as "glass." In addition, amorphous glass that becomes crystallized glass by heat treatment is sometimes referred to as "mother glass of crystallized glass." In the following, "chemically strengthened glass" refers to glass after chemical strengthening treatment, and "glass for chemical strengthening" refers to glass before chemical strengthening treatment.
[0023] <Stress measurement method> In recent years, glass that has been chemically strengthened in two or more stages has become mainstream for use in cover glass for devices such as smartphones. In this process, the lithium ions inside the glass are first exchanged for sodium ions (Li-Na exchange), and then the sodium ions on the surface of the glass are further exchanged for potassium ions (Na-K exchange).
[0024] In order to obtain such a stress profile of chemically strengthened glass in a non-destructive manner, for example, a scattered light photoelastic stress meter (hereinafter also abbreviated as SLP) or a film stress measurement (hereinafter also abbreviated as FSM) can be used in combination.
[0025] The method using a scattered light photoelastic stress meter (SLP) can measure the compressive stress due to Li-Na exchange in the glass interior at a depth of several tens of micrometers from the glass surface.
[0026] On the other hand, a method using a glass surface stress meter (FSM) can measure the compressive stress resulting from Na-K exchange in the surface layer of the glass, within a few tens of μm from the glass surface (for example, WO 2018 / 056121, WO 2017 / 115811).
[0027] Therefore, in two-stage chemically strengthened glass, a combination of SLP and FSM information is sometimes used as the stress profile in the glass surface and interior.
[0028] In this specification, the compressive stresses CS0, CS1, and the depth of the surface compressive stress layer DOL-tail are values measured by a glass surface stress meter (FSM), and the compressive stress CS 50 , C.S. 90 The tensile stress CT and the compressive stress layer depth DOC are values measured by a scattered light photoelastic stress meter (SLP). The surface compressive stress layer depth DOL-tail is the maximum depth of the compressive stress layer that can be measured by FSM.
[0029] The scattered light photoelastic stress meter is a stress measuring device having a polarization phase difference variable member that varies the polarization phase difference of laser light by one or more wavelengths relative to the wavelength of the laser light, an imaging element that captures the scattered light emitted when the laser light with the varied polarization phase difference is incident on strengthened glass multiple times at a specified time interval to obtain multiple images, and a calculation unit that uses the multiple images to measure the periodic luminance change of the scattered light, calculates the phase change of the luminance change, and calculates the stress distribution in the depth direction from the surface of the strengthened glass based on the phase change.
[0030] A method for measuring a stress profile using a scattered light photoelastic stress meter includes the method described in International Publication No. 2018 / 056121. Examples of the scattered light photoelastic stress meter include SLP-1000 and SLP-2000 manufactured by Orihara Seisakusho. High-precision stress measurement is possible by combining these scattered light photoelastic stress meters with the attached software SlpIV_up3 (Ver.2019.01.10.001).
[0031] <ctave> "CTave" (MPa) in this specification is obtained by the following formula. CTave is a value corresponding to the average value of the tensile stress, which is the value obtained by integrating the stress values in the tensile stress region over the entire width of the plate thickness and dividing by the length of the tensile stress region. CTave = ICT / LCT ICT: Integrated value of tensile stress (MPa·μm) LCT: Length in the plate thickness direction of the tensile stress region (μm)
[0032] <CS x > "CS" in this specification x is the compressive stress value (MPa) at a depth x (μm) from the glass surface.
[0033] <Sodium ion concentration profile> In this specification, the sodium ion concentration at a depth x (μm) is measured by EPMA (Electron Probe Micro Analyzer) for the concentration in the cross-section in the plate thickness direction. The measurement by EPMA is specifically performed as follows, for example.
[0034] First, the glass sample is embedded in an epoxy resin, and a cross-section sample is prepared by mechanically polishing it perpendicular to the first main surface and the second main surface facing the first main surface. A C coat is applied to the polished cross-section, and measurement is performed using EPMA (manufactured by JEOL Ltd.: JXA - 8500F). The acceleration voltage is 15 kV, the probe current is 30 nA, and the integration time is 1000 msec. / point. A line profile of the X-ray intensity of the sodium ion concentration and the silicon ion concentration is obtained at 1-μm intervals. The obtained sodium ion concentration profile is normalized by dividing by the average count of the silicon ion concentration in the central part of the plate thickness (500×t) ± 25 μm (plate thickness t [mm]). The Na2O concentration at a specific depth is calculated by proportionally converting the count of the entire plate thickness to mol% of Na2O on the assumption that the average count in the central part of the plate thickness (500×t) ± 25 μm (plate thickness t [mm]) corresponds to the Na2O concentration in the parent composition of the chemically strengthened glass.
[0035] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following embodiments, and can be modified as desired without departing from the scope of the present invention. For example, among the embodiments exemplified in this specification, preferred aspects of each embodiment can be combined with each other, or a part of each embodiment can be replaced with a preferred aspect of another embodiment.
[0036] <Method of manufacturing chemically strengthened glass> A method for producing chemically strengthened glass according to an embodiment of the present invention (hereinafter also referred to as the present production method) includes a first ion exchange treatment in which a glass for chemical strengthening is brought into contact with a first molten salt composition, and a second ion exchange treatment in which the glass for chemical strengthening is brought into contact with a second molten salt composition after the first ion exchange treatment, wherein the ion exchange treatment has a strengthening index value (H value) defined by the following formula of 10600 or less. A method for producing chemically strengthened glass according to an embodiment of the present invention includes a heat treatment after the first ion exchange treatment and before the second ion exchange treatment, wherein the heat treatment has a heat treatment effect index value (I value) defined by the following formula of 220 or more.
[0037]
number
[0038]
number
[0039] However, in the above formula, t CT is the treatment time of the first ion exchange treatment [min], T CT is the temperature of the first ion exchange treatment [°C], Σ[MeO] is the sum [mol%] of the alkali metal ion oxide concentrations in the glass for chemical strengthening, t d is the first ion exchange treatment temperature T CT The time [minutes] during which the glass for chemical strengthening is kept at a temperature of 80% or more of [℃], T d is the temperature of the heat treatment [°C].
[0040] Chemical strengthening is a process in which glass is brought into contact with a metal salt, for example by immersing the glass in a molten liquid of a metal salt (e.g., potassium nitrate) containing a metal ion with a large ionic radius (typically, Na ion or K ion), thereby replacing the metal ion with a small ionic radius (typically, Na ion or Li ion) in the glass with a metal ion with a large ionic radius (typically, Na ion or K ion for Li ion, and K ion for Na ion).
[0041] In order to increase the speed of chemical strengthening, it is preferable to use "Li-Na exchange" in which Li ions in the glass are exchanged with Na ions. Also, in order to create a large compressive stress by ion exchange, it is preferable to use "Na-K exchange" in which Na ions in the glass are exchanged with K ions.
[0042] The present manufacturing method includes, as the chemical strengthening treatment, a first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition, and a second ion exchange treatment in which the glass for chemical strengthening is brought into contact with a second molten salt composition after the first ion exchange treatment. The chemical strengthening treatment may be a two-stage ion exchange treatment consisting of the first ion exchange treatment and the second ion exchange treatment, or may be a three-stage or more ion exchange treatment including a further ion exchange treatment.
[0043] In this manufacturing method, the first ion exchange treatment temperature T CT [℃] and the first ion exchange time t CT [min] includes a heat treatment performed after the first ion exchange treatment and before the second ion exchange treatment, and the strengthening index (H value) defined by the following formula is in the range of 10,600 or less, and the heat treatment effect index value (I value) defined by the following formula is 220 or more in such heat treatment.
[0044]
number
[0045]
number
[0046] However, in the above formula, t CT is the treatment time [min] of the first ion exchange treatment, T CT is the temperature of the first ion exchange treatment [°C], Σ[MeO] is the sum of the alkali metal ion oxide concentrations in the chemically strengthened glass [mol%], t d is the first ion exchange treatment temperature T CT The time [minutes] during which the glass for chemical strengthening is kept at a temperature of 80% or more of [℃], T d is the heat treatment temperature [℃].
[0047] The present inventors have discovered that, when producing chemically strengthened glass by two or more stages of ion exchange treatment, a suitable heat treatment is carried out in the first ion exchange treatment, and a suitable heat treatment is carried out after the first ion exchange treatment and before the second ion exchange treatment, thereby improving the CS of the obtained chemically strengthened glass. 90 In other words, by carrying out a heat treatment with a heat treatment effect index value (I value) of 220 or more after the first ion exchange treatment in which the H value defined by the above formula is in the range of 10600 or less and before the second ion exchange treatment, the CS of the obtained chemically strengthened glass can be increased. 90 It has been found that the compressive stress can be increased relative to the total amount of compressive stress, and this has led to the completion of the present invention.
[0048] FIG. 1 is a diagram showing an example of a stress profile of chemically strengthened glass obtained by the present manufacturing method, measured by SLP. The solid line in FIG. 1 is the stress profile of chemically strengthened glass obtained by the present manufacturing method (Example 3 in the Examples). The dashed line is the stress profile of chemically strengthened glass (Example 5 in the Examples) obtained by the same method as the chemically strengthened glass of the solid line, except that the heat treatment time and temperature were changed to a condition in which the heat treatment effect index value (I value) was below 220. Comparing the chemically strengthened glasses of Examples 5 and 3 from FIG. 1, in Example 3, CS 50 While maintaining the same level of CS 90 It can be seen that CS is larger. 90 In addition, as described in detail in the Examples, the chemically strengthened glass of Example 3 obtained by the present manufacturing method has a CS 90 The value of / ICT is larger than in Example 5. Here, CS 90 / ICT is the ratio of CS to the total amount of compressive stress introduced into chemically strengthened glass. 90 It is an index of the magnitude of the value, and details will be described later.
[0049] In this way, CS 90 The reason why the thermal treatment can improve the strength is believed to be that the alkali metal ions introduced in the first ion exchange treatment are diffused further toward the depth of the glass, thereby increasing the compressive stress in the deep part. FIG. 2 is a diagram showing the Na ion concentration profile in the sheet thickness direction of the chemically strengthened glass of Example 5 and Example 3 shown in FIG. 1, measured by an electron beam microanalyzer. The solid line shows the chemically strengthened glass of Example 3, and the dashed line shows the chemically strengthened glass of Example 5. When comparing the Na ion concentration profiles of the chemically strengthened glass of Example 5 and Example 3, it can be seen that the chemically strengthened glass of Example 3 has a higher Na ion concentration near a depth of 90 μm and a larger Na ion diffusion depth, as in the case of the stress profile.
[0050] To increase the effect of such heat treatment, for example, it is considered that increasing the temperature of the heat treatment can contribute to promoting the thermal motion of the alkali ions contained in the glass. Or, it is considered that increasing the time of the heat treatment can contribute to increasing the amount of heat applied in the heat treatment. In this regard, since the diffusion depth is proportional to the square root of the diffusion time according to the diffusion equation, it is considered that the heat treatment effect is also proportional to the square root of the heat treatment time. In addition, when the sum of the alkali metal ion concentrations in the glass for chemical strengthening is larger, it is considered that the glass is more susceptible to the influence of the heat treatment by increasing the total amount of alkali ions contained in the glass. In addition, when the treatment time of the first ion exchange treatment is longer, it is considered that the glass is more susceptible to the influence of the heat treatment by increasing the total amount of alkali ions contained in the glass after the application of chemical strengthening. The indices based on these findings are the strengthening index (H value) and the heat treatment effect index (I value) described above. By setting the strengthening index (H value) in the first ion exchange treatment to 10600 or less and performing heat treatment before the second ion exchange treatment under conditions where the heat treatment effect index (I value) is 220 or more, the CS 90 Thus, a chemically strengthened glass having improved properties can be obtained.
[0051] In the present manufacturing method, from the viewpoint of obtaining the above-mentioned effects, the heat treatment effect index value (I value) is 220 or more, preferably 230 or more, more preferably 240 or more, and even more preferably 250 or more. From the viewpoint of suppressing relaxation of generated stress, the heat treatment effect index value (I value) is preferably 300 or less, more preferably 280 or less, and even more preferably 270 or less.
[0052] As mentioned above, in order to make the heat treatment effect index value (I value) 220 or more, Σ[Me2O],t d , T d and t CT As described above, Σ[Me2O] is the sum of the alkali metal ion oxide concentrations [mol%] in the glass for chemical strengthening, and t d is the heat treatment time [min], T d is the temperature of the heat treatment [℃], and t CT is the treatment time [min] of the first ion exchange treatment.
[0053] For example, the temperature of the heat treatment T d [℃] is 360℃ or more, or the heat treatment time t d [minutes] is preferably 10 minutes or more, which makes it relatively easy to increase the heat treatment effect index value (I value).
[0054] From the viewpoint of increasing the heat treatment effect index value (I value), Σ[Me2O] is preferably 5 mol% or more, more preferably 6 mol% or more, even more preferably 7 mol% or more, particularly preferably 8 mol% or more, and most preferably 9 mol% or more. On the other hand, from the viewpoint of the moldability of the glass, Σ[Me2O] is preferably 35 mol% or less, more preferably 30 mol% or less, even more preferably 25 mol% or less, particularly preferably 20 mol% or less, and most preferably 18 mol% or less. Σ[Me2O] is the sum of the alkali metal ion concentrations in the chemically strengthened glass, specifically the sum [mol%] of the concentrations of Li2O, Na2O, and K2O expressed in mole percentage on an oxide basis.
[0055] Heat treatment temperature T d From the viewpoint of increasing the heat treatment effect index value (I value), the temperature [°C] is preferably 360°C or higher, more preferably 365°C or higher, even more preferably 370°C or higher, particularly preferably 375°C or higher, and most preferably 380°C or higher. d From the viewpoint of suppressing relaxation of generated stress, the temperature [°C] is preferably 500°C or less, more preferably 490°C or less, further preferably 480°C or less, particularly preferably 470°C or less, and most preferably 460°C or less.
[0056] Heat treatment time t d From the viewpoint of increasing the heat treatment effect index value (I value), [minutes] is preferably 10 minutes or more, more preferably 15 minutes or more, even more preferably 20 minutes or more, particularly preferably 25 minutes or more, and most preferably 30 minutes or more. d From the viewpoint of suppressing a decrease in productivity, [minutes] is preferably 120 minutes or less, more preferably 105 minutes or less, even more preferably 90 minutes or less, particularly preferably 75 minutes or less, and most preferably 70 minutes or less.
[0057] The treatment time [min] of the first ion exchange treatment is preferably 150 minutes or more, more preferably 180 minutes or more, even more preferably 200 minutes or more, and particularly preferably 220 minutes or more, from the viewpoint of sufficiently introducing stress energy that can be transferred to deep layers by heat treatment. On the other hand, the treatment time [min] of the first ion exchange treatment is preferably 360 minutes or less, more preferably 330 minutes or less, even more preferably 300 minutes or less, particularly preferably 270 minutes or less, and most preferably 250 minutes or less, from the viewpoint of suppressing a decrease in productivity.
[0058] The heat treatment may be performed after the first ion exchange treatment and before the second ion exchange treatment, and the specific method is not particularly limited. Note that "after the first ion exchange treatment" may be performed after the chemically strengthened glass is removed from the first molten salt composition in the first ion exchange treatment, and "before the second ion exchange treatment" may be performed before the chemically strengthened glass is immersed in the second molten salt composition in the second ion exchange treatment. Specific examples of the heat treatment include a "droplet process" for dropping the molten salt attached by the first ion exchange treatment, a "heating process" for heating the glass that has been subjected to the first ion exchange treatment and a "preheating process" for heating the glass that has been subjected to the first ion exchange treatment before the second ion exchange treatment.
[0059] The chemical strengthening treatment includes, for example, the following steps (a) to (d) in this order. In this manufacturing method, it is preferable to carry out a heat treatment in the droplet step (c) after the first ion exchange treatment ((b) strengthening step). This makes the process less complicated and allows the effects of the present invention to be obtained efficiently. (a) Preheating process (b) Strengthening process (ion exchange treatment) (c) Droplet process (d) Removal process
[0060] FIG. 3 is a diagram illustrating the above steps (a) to (d), and (a) to (d) in FIG. 3 correspond to the above steps (a) to (d), respectively. In the (a) preheating step, the glass 1 for chemical strengthening is heated in advance before being immersed in the molten salt composition 53. By carrying out the preheating step, it is possible to suppress glass cracking due to thermal shock when it is immersed in the molten salt. For example, it is preferable to heat the glass for chemical strengthening to a temperature range of −80° C. to +80° C. with respect to the temperature of the molten salt composition in the (b) strengthening step. The preheating step may be carried out by a known method, and for example, as shown in FIG. 3, the glass 1 for chemical strengthening can be heated using an atmosphere heater 25 provided on a molten salt bath 50. In FIG. 3, the molten salt bath 50 is provided with a molten salt heater 55, and the molten salt composition 53 is heated by the molten salt heater 55.
[0061] In the (b) strengthening step, an ion exchange treatment is performed by immersing the glass for chemical strengthening 1 in a molten salt composition 53. Preferable conditions for the ion exchange treatment will be described in detail later.
[0062] In the (c) droplet step, the glass 1 for chemical strengthening is taken out from the molten salt composition 53 and then left to stand for a predetermined time, thereby allowing the molten salt composition adhering to the glass 1 for chemical strengthening to fall naturally and be removed. In the (c) droplet step, in order to maintain the molten state of the molten salt composition adhering to the glass 1 for chemical strengthening, the glass 1 for chemical strengthening is heated using an atmosphere heater 25 as shown in FIG. 3 or the like. Here, the heat treatment of the present manufacturing method can be carried out in the droplet step by setting the heating conditions to the above-mentioned preferred heat treatment conditions and setting the heat treatment effect index value (I value) to 220 or more. By carrying out the heat treatment of the present manufacturing method in this manner in the droplet step, the CS of the chemically strengthened glass can be obtained without complicating the process. 90 This is preferable because it allows the steel to have a larger CT limit and makes it less likely to exceed the CT limit when removed from the tempering furnace.
[0063] In the (d) removal step, the chemically strengthened glass (glass for chemical strengthening) is removed from the chemical strengthening treatment apparatus. The removed chemically strengthened glass (glass for chemical strengthening) may be subjected to, for example, a cleaning step, a decorating step, or the like. If it is necessary to perform the next stage of ion exchange treatment, the steps (a) to (d) may be performed again. Since the present manufacturing method includes two stages of ion exchange treatment, specifically, for example, the first step (a), the first step (b) which is the first ion exchange treatment, the first step (c) which performs the heat treatment of the present manufacturing method, the first step (d), the second step (a), the second step (b) which is the second ion exchange treatment, the second step (c), and the second step (d) may be included in this order. In the present manufacturing method, when a total of two or more heating steps are included between the first ion exchange treatment and the second ion exchange treatment, it is preferable that the sum of the heat treatment effect index values in each heating is 220 or more.
[0064] Although the above describes an example in which the heat treatment of the present manufacturing method is performed in the droplet process, the heat treatment of the present manufacturing method may be performed outside the droplet process. For example, the heat treatment of the present manufacturing method may be performed in the second step (a), or after the first step (d), the heat treatment of the present manufacturing method may be performed using a separately prepared heating device or the like.
[0065] In the droplet process, the molten salt composition adheres to the surface of the glass for chemical strengthening, but the amount is small compared to when the glass for chemical strengthening is immersed in the molten salt composition. Therefore, even if the heat treatment of the present manufacturing method is performed in the droplet process, it is considered that ion exchange or the like that would affect the obtained chemically strengthened glass does not occur. In addition, the diffusion of alkali metal ions toward the depths of the glass due to the heat treatment of the present manufacturing method is a phenomenon that occurs inside the glass. For these reasons, it is considered that the CS is similarly improved even if the heat treatment of the present manufacturing method is performed outside the droplet process. 90 This can have the effect of improving the following:
[0066] A preferred embodiment of the ion exchange treatment in the present production method will now be described in detail.
[0067] As described above, the present production method includes the first ion exchange treatment and the second ion exchange treatment. The first molten salt composition used in the first ion exchange treatment and the second molten salt composition used in the second ion exchange treatment usually have different compositions. From the viewpoint of easily obtaining a suitable stress profile, it is preferable that the first ion exchange treatment is a treatment that mainly utilizes "Li-Na exchange", and it is preferable that the second ion exchange treatment is a treatment that mainly utilizes "Na-K exchange".
[0068] (First ion exchange treatment) The first ion exchange treatment is preferably a treatment mainly using "Li-Na exchange". In this case, it is preferable to perform the first ion exchange treatment by immersing the glass for chemical strengthening in a first molten salt composition containing sodium ions. Although the details of the glass for chemical strengthening will be described later, in order to perform the Li-Na exchange, it is preferable to use a lithium-containing glass as the glass for chemical strengthening.
[0069] According to the first ion exchange treatment, which mainly utilizes "Li-Na exchange," lithium ions in the glass are exchanged for sodium ions in the molten salt, whereby sodium is introduced deep into the glass, forming a deep compressive stress layer.
[0070] Examples of molten salts for performing chemical strengthening treatment include nitrates, sulfates, carbonates, and chlorides. Examples of nitrates include lithium nitrate, sodium nitrate, potassium nitrate, cesium nitrate, and silver nitrate. Examples of sulfates include lithium sulfate, sodium sulfate, potassium sulfate, cesium sulfate, and silver sulfate. Examples of carbonates include lithium carbonate, sodium carbonate, and potassium carbonate. Examples of chlorides include lithium chloride, sodium chloride, potassium chloride, cesium chloride, and silver chloride. These molten salts may be used alone or in combination.
[0071] The molten salt composition is preferably one containing a nitrate as a main component, more preferably one containing sodium nitrate or potassium nitrate as a main component. Here, "containing" as a main component means that the content of the nitrate in the molten salt composition is 80 mass% or more.
[0072] The content of sodium nitrate in the first molten salt composition is preferably more than 40% by mass. In the first embodiment, the content of sodium nitrate in the first molten salt composition may be 65% by mass or more, 75% by mass or more, 85% by mass or more, or 95% by mass or more. When the sodium nitrate content is within the above range, the amount of sodium that enters the deep layer of the glass increases due to "Li-Na exchange" in the first ion exchange, and the CS 90 This has the effect of raising
[0073] On the other hand, when potassium nitrate is added to the first molten salt composition, the content may be 65 mass % or less, 45 mass % or less, 25 mass % or less, or 15 mass % or less. When the potassium nitrate content is within the above range, "Li-Na exchange" functions more predominantly than "Na-K exchange", so that sodium ions can be sufficiently introduced into the deep layer of the glass.
[0074] In the first ion exchange treatment, it is preferable to immerse the glass for chemical strengthening in the first molten salt composition at a temperature of 360°C or higher. When the temperature of the first molten salt composition is 360°C or higher, the ion exchange is likely to proceed, and compressive stress can be introduced to a range exceeding the CT limit. The temperature is more preferably 380°C or higher, and even more preferably 400°C or higher. In addition, the temperature of the first molten salt composition is usually 450°C or lower in view of the risk of evaporation and the change in the composition of the molten salt.
[0075] In the first ion exchange treatment, the time for immersing the glass for chemical strengthening in the first molten salt composition is preferably 30 minutes or more since the surface compressive stress increases. The immersion time is more preferably 60 minutes or more. If the immersion time is too long, not only the productivity decreases, but the compressive stress may decrease due to a relaxation phenomenon. Therefore, the immersion time is usually 360 minutes or less. The time for the first ion exchange treatment is the above-mentioned t CT This value may also affect the heat treatment effect index value (I value). Therefore, the time of the first ion exchange treatment may be adjusted in order to set the heat treatment effect index value (I value) to a suitable value.
[0076] (Second ion exchange treatment) The second ion exchange treatment is preferably a treatment mainly using "Na-K exchange". In this case, it is preferable to perform the second ion exchange treatment by immersing the glass for chemical strengthening in a second molten salt composition containing potassium ions. In the second ion exchange treatment mainly using "Na-K exchange", the sodium ions in the glass are exchanged with potassium ions, and potassium ions are introduced into a region of the glass surface layer of 10 μm or less. In addition, when the second molten salt composition contains a small amount of lithium ions, the sodium ions in the glass surface layer are simultaneously reduced by "Na-Li exchange", thereby relaxing the compressive stress caused by sodium. Note that the stress profile measured by SLP does not reflect the influence of the stress of the glass surface layer into which potassium ions have been introduced. Therefore, the stress profile measured by SLP can be used to confirm the reduction in tensile stress due to the reduction in sodium ions.
[0077] The potassium nitrate concentration in the second molten salt composition is preferably 85 mass % or more, more preferably 90 mass % or more, and further preferably 95 mass % or more. There is no particular upper limit, but it is usually 99.95 mass % or less.
[0078] When the second molten salt composition contains lithium ions, the second molten salt composition preferably contains 0.05% by mass or more and 10% by mass or less of lithium nitrate. By containing lithium nitrate in the above range in the second molten salt composition, the exchange between the sodium ions introduced near the glass surface in the first ion exchange treatment and the lithium ions in the second molten salt composition occurs in parallel with the exchange between the sodium ions and the potassium ions in the second molten salt composition, thereby reducing the stress on the glass surface. The content of lithium nitrate in the second molten salt composition is more preferably 0.3% by mass or more and 5% by mass or less.
[0079] The second molten salt composition may contain sodium nitrate. When it contains sodium nitrate, the sodium nitrate concentration is preferably more than 0.1 mass%, more preferably 0.5 mass% or more. When the sodium nitrate content is within the above range, the period during which the effect of the present invention can be exhibited without replacing the second molten salt composition can be extended, and the amount of glass processed can be increased. When the sodium nitrate concentration of the second molten salt composition is preferably 5 mass% or less, more preferably 3 mass% or less, even more preferably 2 mass% or less, and most preferably 1 mass% or less, the tensile stress of the chemically strengthened glass after the second ion exchange treatment is easily suppressed to less than the CT limit value.
[0080] In the second ion exchange treatment, it is preferable to immerse the glass for chemical strengthening in the second molten salt composition at a temperature of 360°C or higher. When the temperature of the second molten salt composition is 360°C or higher, the ion exchange is likely to proceed. It is more preferably 380°C or higher, and even more preferably 400°C or higher. In addition, the temperature of the second molten salt composition is usually 450°C or lower from the viewpoint of the risk of evaporation and the change in the composition of the molten salt, and more preferably 440°C or lower from the viewpoint of preventing an excessive decrease in stress due to "Na-Li exchange".
[0081] In the second ion exchange treatment, if the time for immersing the glass for chemical strengthening in the second molten salt composition is 5 minutes or more, the sodium ions introduced near the glass surface in the first ion exchange treatment and the lithium ions in the second molten salt composition are sufficiently exchanged, and the stress on the glass surface is easily weakened. The immersion time is more preferably 30 minutes or more, and even more preferably 45 minutes or more. From the viewpoint of preventing an excessive reduction in stress due to heat input to the substrate, the immersion time is preferably 120 minutes or less.
[0082] In this manufacturing method, it is preferable to impart a tensile stress exceeding the CT limit value to the glass for chemical strengthening by the first ion exchange treatment, and then to make the tensile stress less than the CT limit value by the subsequent second ion exchange treatment. This makes it possible to increase the compressive stress in a region relatively deep from the surface while preventing the tensile stress from exceeding the CT limit, thereby contributing to further increasing the drop strength of the chemically strengthened glass.
[0083] That is, for chemically strengthened glass, using the CTA value [MPa] calculated by the following formula (1), the first ion exchange treatment is performed to make the CTave value of the chemically strengthened glass calculated by the following formula (2) exceed the CTA value [MPa], and the second ion exchange treatment is performed to make the CTave value of the chemically strengthened glass less than the CTA value [MPa].
[0084]
number
[0085] t: Plate thickness [mm] K1c: Fracture toughness value [MPa m 1 / 2 ] CTave=ICT / LCT...Equation (2) ICT: Tensile stress integral value [MPa μm] LCT: Length of tensile stress region in the thickness direction [μm]
[0086] Here, the "fracture toughness value K1c" is a value obtained by the IF method defined in JIS R1607: 2015. The value of K1c depends on the glass composition and can be adjusted by the glass composition. The CTA value is a value corresponding to the CT limit. Setting the CTave value to more than x [MPa] corresponds to setting the tensile stress to more than the CT limit value, and setting the CTave value to less than x [MPa] corresponds to setting the tensile stress to less than the CT limit value. As a method for setting the CTave value of the glass for chemical strengthening calculated by the following formula (2) to more than x [MPa] by the first ion exchange treatment and the CTave value of the glass for chemical strengthening to less than x [MPa] by the second ion exchange treatment, for example, 1) a method of appropriately optimizing the treatment conditions in the heat treatment between the first ion exchange treatment and the second ion exchange treatment in this manufacturing method, and 2) a method of ion exchange treatment described in International Publication No. 2022 / 181812 can be mentioned.
[0087] <Glass for chemical strengthening> In this manufacturing method, chemically strengthened glass is obtained by chemically strengthening a chemically strengthened glass. The chemically strengthened glass in this manufacturing method is preferably a lithium-containing glass, and is preferably a lithium aluminosilicate glass. The chemically strengthened glass in this manufacturing method may be crystallized glass or amorphous glass. The matrix composition of the chemically strengthened glass according to the embodiment of the present invention is the same as the composition of the chemically strengthened glass before chemical strengthening, and when the chemically strengthened glass is crystallized glass, the chemically strengthened glass also becomes crystallized glass.
[0088] In one embodiment, the matrix composition of the chemically strengthened glass (the composition of the glass for chemical strengthening) is, more specifically, for example, the following glass composition Xa, glass composition Xb, and glass composition Xc. When the chemically strengthened glass is a crystallized glass, the matrix composition is preferably glass composition Xc. Glass composition Xa: A composition containing, in mole percent based on oxides, 54-77% SiO2, 9-21% Al2O3, and 5-16% Li2O. Glass composition Xb: A composition containing, in mole percent based on oxides, 52-75% SiO2, 8-20% Al2O3, and 5-16% Li2O. Glass composition Xc: A composition containing, in mole percent based on oxides, 40-70% SiO2, 10-35% Li2O, and 1-15% Al2O3.
[0089] One aspect of the glass composition Xc is, in mole percent on an oxide basis, SiO2 40-70%, Li2O 10~35%, Al2O3 1-15%, P2O5 0.5-5%, ZrO2 0.5-5%, B2O3 0-10%, Na2O 0-3%, K2O 0-1%, Examples of compositions include those containing 0 to 4% SnO2.
[0090] Another aspect of the glass composition Xc is, in mole percent on an oxide basis, SiO2 50-70%, Li2O 15~30%, Al2O3 1-10%, P2O5 0.5-5%, ZrO2 0.5-8%, MgO 0.1-10%, Y2O3 0-5% B2O3 0-10%, Na2O 0-3%, K2O 0-1%, Examples include compositions containing 0 to 2% SnO2.
[0091] A preferred glass composition will now be described.
[0092] In the chemically strengthened glass of the present embodiment, SiO2 is a component that forms a network structure of the glass and also increases the chemical durability. In the glass composition Xa, the SiO2 content is preferably 54% or more. The SiO2 content is more preferably 56% or more, even more preferably 60% or more, particularly preferably 64% or more, and extremely preferably 68% or more. On the other hand, in the glass composition Xa, in order to improve the melting property, the SiO2 content is preferably 77% or less, more preferably 75% or less, even more preferably 73% or less, and particularly preferably 71% or less. In the glass composition Xb, the SiO2 content is preferably 52% or more. The SiO2 content is more preferably 56% or more, even more preferably 60% or more, particularly preferably 64% or more, and extremely preferably 68% or more. On the other hand, in the glass composition Xb, in order to improve the melting property, the SiO2 content is preferably 75% or less, more preferably 73% or less, even more preferably 71% or less, and particularly preferably 69% or less. In the glass composition Xc, the SiO2 content is preferably 45% or more. The SiO2 content is more preferably 48% or more, even more preferably 50% or more, particularly preferably 52% or more, and extremely preferably 54% or more. On the other hand, in order to improve the melting property, the SiO2 content is preferably 70% or less, more preferably 68% or less, even more preferably 66% or less, and particularly preferably 64% or less.
[0093] Al2O3 is an essential component that increases the surface compressive stress due to chemical strengthening. In glass composition Xa, the content of Al2O3 is preferably 9% or more, more preferably 10% or more, 11% or more, 12% or more, 13% or more, further preferably 14% or more, and particularly preferably 15% or more. On the other hand, in glass composition Xa, the content of Al2O3 is preferably 21% or less, more preferably 18% or less, further preferably 17% or less, 16% or less, and most preferably 15% or less, in order to prevent the devitrification temperature of the glass from becoming too high. In glass composition Xb, the content of Al2O3 is preferably 8% or more, more preferably 10% or more, 11% or more, 12% or more, 13% or more, further preferably 14% or more, and particularly preferably 15% or more. On the other hand, in glass composition Xb, the content of Al2O3 is preferably 20% or less, more preferably 18% or less, further preferably 17% or less, 16% or less, and most preferably 15% or less, in order to prevent the devitrification temperature of the glass from becoming too high. In glass composition Xc, the content of Al2O3 is preferably 1% or more, more preferably 2% or more, further preferably 3% or more, 5% or more, 5.5% or more, 6% or more, particularly preferably 6.5% or more, and most preferably 7% or more. On the other hand, the content of Al2O3 is preferably 15% or less, more preferably 12% or less, further preferably 10% or less, particularly preferably 9% or less, and most preferably 8% or less, so that the devitrification temperature of the glass does not become too high.
[0094] Li2O is a component that forms compressive stress through ion exchange and is essential since it is a constituent of the main crystal. In the glass composition Xa, the content of Li2O is preferably 5% or more, more preferably 7% or more, and even more preferably 10% or more. On the other hand, in order to stabilize the glass in the glass composition Xa, the content of Li2O is preferably 16% or less, more preferably 15% or less, even more preferably 14% or less, and most preferably 12% or less. In glass composition Xb, the content of Li2O is preferably 5% or more, more preferably 7% or more, and even more preferably 10% or more. On the other hand, in order to stabilize the glass in glass composition Xb, the content of Li2O is preferably 16% or less, more preferably 15% or less, even more preferably 14% or less, and most preferably 12% or less. In the glass composition Xc, the content of Li2O is preferably 10% or more, more preferably 14% or more, more preferably 15% or more, even more preferably 18% or more, particularly preferably 20% or more, and most preferably 22% or more. On the other hand, in order to stabilize the glass, the content of Li2O is preferably 35% or less, more preferably 32% or less, even more preferably 30% or less, particularly preferably 28% or less, and most preferably 26% or less.
[0095] Na2O is a component that improves the meltability of glass. In the glass composition Xa, Na2O is not essential, but when it is contained, it is preferably 0.5% or more, more preferably 0.8% or more, and particularly preferably 1% or more. If the Na2O content is too high, crystals become difficult to precipitate or the chemical strengthening properties decrease, so the Na2O content is preferably 10% or less, more preferably 8% or less, and particularly preferably 6% or less. In the glass composition Xb, Na2O is not essential, but when it is contained, it is preferably 1% or more, more preferably 2% or more, and particularly preferably 5% or more. If the Na2O content is too high, crystals become difficult to precipitate or the chemical strengthening properties decrease, so the Na2O content is preferably 15% or less, more preferably 12% or less, and particularly preferably 10% or less. In the glass composition Xc, Na2O is not essential, but when it is contained, it is preferably 0.5% or more, more preferably 1% or more, and particularly preferably 2% or more. If there is too much Na2O, it becomes difficult to precipitate crystals such as Li3PO4, which is the main crystal, or the chemical strengthening properties are reduced, so the Na2O content is preferably 10% or less, more preferably 9% or less, even more preferably 8% or less, and particularly preferably 7% or less.
[0096] Like Na2O, K2O is a component that lowers the melting temperature of glass and may be contained. In the glass composition Xa, when K2O is contained, the content is preferably 0.5% or more, more preferably 0.8% or more, and even more preferably 1% or more. If the amount of K2O is too much, the chemical strengthening property or chemical durability decreases, so that the content is preferably 5% or less, more preferably 4% or less, even more preferably 3% or less, particularly preferably 2.5% or less, and most preferably 2% or less. In the glass composition Xb, when K2O is contained, the content is preferably 0.5% or more, more preferably 0.8% or more, and further preferably 1% or more. If the amount of K2O is too much, the chemical strengthening property or chemical durability decreases, so that the content is preferably 10% or less, more preferably 8% or less, further preferably 6% or less, particularly preferably 4% or less, and most preferably 2% or less. In the glass composition Xc, when K2O is contained, the content is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. If the amount of K2O is too much, the chemical strengthening property or chemical durability decreases, so the content is preferably 5% or less, more preferably 4% or less, even more preferably 3% or less, particularly preferably 2% or less, and most preferably 1% or less.
[0097] In the glass composition Xa, the total content of Na2O and K2O (Na2O+K2O) is preferably 2% or more, more preferably 3% or more, in order to improve the melting property of the glass raw material. In addition, the ratio of the K2O content to the total content of Li2O, Na2O and K2O (hereinafter referred to as R2O) is preferably 0.2 or less, since this enhances the chemical strengthening properties and chemical durability. K2O / R2O is more preferably 0.17 or less, and even more preferably 0.15 or less. In addition, R2O is preferably 10% or more, more preferably 12% or more, and even more preferably 14% or more. In addition, R2O is preferably 20% or less, and more preferably 18% or less.
[0098] In the glass composition Xb, the total content of Na2O and K2O (Na2O+K2O) is preferably 3% or more, more preferably 5% or more, in order to improve the melting property of the glass raw material. In addition, the ratio of the K2O content to the total content of Li2O, Na2O and K2O (hereinafter referred to as R2O) is preferably 0.2 or less, since this enhances the chemical strengthening properties and chemical durability. K2O / R2O is more preferably 0.15 or less, and even more preferably 0.10 or less. In addition, R2O is preferably 10% or more, more preferably 12% or more, and even more preferably 15% or more. In addition, R2O is preferably 20% or less, and more preferably 18% or less.
[0099] In the glass composition Xc, the total content of Na2O and K2O (Na2O+K2O) is preferably 1% or more, more preferably 2% or more, in order to improve the melting property of the glass raw material. In addition, the ratio of the K2O content to the total content of Li2O, Na2O and K2O (hereinafter referred to as R2O) is preferably 0.2 or less, since this enhances the chemical strengthening properties and chemical durability. K2O / R2O is more preferably 0.15 or less, and even more preferably 0.10 or less. In addition, R2O is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more. In addition, R2O is preferably 29% or less, and more preferably 26% or less.
[0100] In the glass compositions Xa and Xb, P2O5 is a component that deepens the compressive stress layer due to chemical strengthening, and may be contained. In order to deepen the compressive stress layer, the content of P2O5 is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, particularly preferably 2% or more, and extremely preferably 2.5% or more. On the other hand, if the P2O5 content is too high, phase separation occurs easily when melted and acid resistance is significantly reduced, so the P2O5 content is preferably 5% or less, more preferably 4.8% or less, even more preferably 4.5% or less, and particularly preferably 4.2% or less.
[0101] In the glass composition Xc, P2O5 is a component of Li3PO4 crystal and is essential. The content of P2O5 is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, particularly preferably 2% or more, and extremely preferably 2.5% or more in order to promote crystallization. On the other hand, if the content of P2O5 is too high, phase separation occurs easily during melting and acid resistance is significantly reduced, so the content of P2O5 is preferably 5% or less, more preferably 4.8% or less, even more preferably 4.5% or less, and particularly preferably 4.2% or less.
[0102] SiO2, Al2O3, P2O5 and B2O3 are glass network forming components (hereinafter also referred to as NWF), and the strength of the crystallized glass increases when the total amount of NWF is large. This improves the fracture toughness value of the crystallized glass. From this viewpoint, in the glass composition Xc, the total amount of NWF is preferably 60% or more, more preferably 63% or more, and particularly preferably 65% or more. However, glass with too much NWF has a high melting temperature and is difficult to manufacture, so it is preferably 85% or less, more preferably 80% or less, and more preferably 75% or less.
[0103] In the glass composition Xc, the ratio of the total amount of Li2O, Na2O and K2O to the total amount of NWF, i.e., SiO2, Al2O3, P2O5 and B2O3, is preferably 0.20 to 0.60. Li2O, Na2O and K2O are network modifiers, and decreasing the ratio to NWF increases the gaps in the network, improving impact resistance. Therefore, the ratio to NWF is preferably 0.60 or less, more preferably 0.55 or less, and particularly preferably 0.50 or less. On the other hand, since these are components necessary for chemical strengthening, in order to improve the chemical strengthening properties, the ratio of the total amount of Li2O, Na2O and K2O to NWF is preferably 0.20 or more, more preferably 0.25 or more, and particularly preferably 0.30 or more.
[0104] ZrO2 is a component that enhances mechanical strength and chemical durability, and is preferably contained since it significantly improves CS. The content of ZrO2 is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, particularly preferably 2% or more, and most preferably 2.5% or more. On the other hand, in order to suppress devitrification during melting, ZrO2 is preferably 8% or less, more preferably 7.5% or less, even more preferably 7% or less, and particularly preferably 6% or less. If the ZrO2 content is too high, the viscosity decreases due to an increase in the devitrification temperature. In order to suppress deterioration of formability due to such a decrease in viscosity, when the forming viscosity is low, the ZrO2 content is preferably 5% or less, more preferably 4.5% or less, and even more preferably 3.5% or less.
[0105] In order to enhance chemical durability, ZrO2 / R2O is preferably 0.02 or more, more preferably 0.04 or more, even more preferably 0.06 or more, particularly preferably 0.08 or more, and most preferably 0.1 or more. In order to enhance transparency after crystallization, ZrO2 / R2O is preferably 0.2 or less, more preferably 0.18 or less, even more preferably 0.16 or less, and particularly preferably 0.14 or less.
[0106] Since MgO is a component that stabilizes glass and also enhances mechanical strength and chemical resistance, it is preferable to contain MgO when the Al2O3 content is relatively low, etc. The MgO content is preferably 1% or more, more preferably 2% or more, even more preferably 3% or more, and particularly preferably 4% or more. On the other hand, if too much MgO is added, the viscosity of the glass decreases and devitrification or phase separation tends to occur. The content of MgO is preferably 20% or less, more preferably 19% or less, further preferably 18% or less, and particularly preferably 17% or less.
[0107] TiO2 is a component that can promote crystallization and may be contained. TiO2 is not essential, but if it is contained, it is preferably 0.05% or more, more preferably 0.1% or more. On the other hand, in order to suppress devitrification during melting, the content of TiO2 is preferably 1% or less, more preferably 0.5% or less, and even more preferably 0.3% or less.
[0108] SnO2 has the effect of promoting the formation of crystal nuclei and may be contained. SnO2 is not essential, but when it is contained, it is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. On the other hand, in order to suppress devitrification during melting, the content of SnO2 is preferably 4% or less, more preferably 3.5% or less, even more preferably 3% or less, and particularly preferably 2.5% or less.
[0109] Y2O3 is a component that has the effect of preventing fragments from scattering when the chemically strengthened glass is broken, and may be contained. The content of Y2O3 is preferably 0.2% or more, more preferably 0.5% or more, even more preferably 1% or more, particularly preferably 2% or more, and extremely preferably 3% or more. On the other hand, in order to suppress devitrification during melting, the content of Y2O3 is preferably 5% or less, more preferably 4% or less.
[0110] B2O3 is a component that improves the chipping resistance of the chemically strengthened glass or the chemically strengthened glass and improves the meltability, and may be contained. When B2O3 is contained, the content is preferably 0.5% or more, more preferably 1% or more, and even more preferably 2% or more in order to improve the meltability. On the other hand, if the content of B2O3 is too high, striae may occur during melting, or phase separation may occur easily, which may lead to a deterioration in the quality of the chemically strengthened glass, so that the content is preferably 10% or less. The content of B2O3 is more preferably 8% or less, even more preferably 6% or less, and particularly preferably 4% or less.
[0111] BaO, SrO, MgO, CaO and ZnO are all components that improve the meltability of glass and may be contained.
[0112] Among these, BaO, SrO, and ZnO may be contained in the glass composition Xc to improve the refractive index of the residual glass and bring it closer to the precipitated crystal phase, thereby improving the light transmittance of the crystallized glass and reducing the haze value. In this case, the total content of BaO, SrO, and ZnO (hereinafter, BaO+SrO+ZnO) is preferably 0.3% or more, more preferably 0.5% or more, even more preferably 0.7% or more, and particularly preferably 1% or more. On the other hand, these components may reduce the ion exchange rate. In order to improve the chemical strengthening properties, BaO+SrO+ZnO is preferably 2.5% or less, more preferably 2% or less, even more preferably 1.7% or less, and particularly preferably 1.5% or less.
[0113] La2O3, Nb2O5 and Ta2O5 are all components that make it difficult for chemically strengthened glass to scatter fragments when broken, and may be contained to increase the refractive index. When these are contained, the total content of La2O3, Nb2O5 and Ta2O5 (hereinafter, La2O3+Nb2O5+Ta2O5) is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. In addition, in order to make the glass less susceptible to devitrification during melting, La2O3+Nb2O5+Ta2O5 is preferably 4% or less, more preferably 3% or less, even more preferably 2% or less, and particularly preferably 1% or less.
[0114] CeO2 may also be contained. CeO2 may suppress coloring by oxidizing the glass. When CeO2 is contained, the content is preferably 0.03% or more, more preferably 0.05% or more, and even more preferably 0.07% or more. In order to increase transparency, the content of CeO2 is preferably 1.5% or less, and more preferably 1.0% or less.
[0115] When chemically strengthened glass is used after coloring, coloring components may be added to the extent that the desired chemical strengthening characteristics are not hindered. Examples of coloring components include Co3O4, MnO2, Fe2O3, NiO, CuO, Cr2O3, V2O5, Bi2O3, SeO2, Er2O3, and Nd2O3.
[0116] The total content of coloring components is preferably within the range of 1% or less. If it is desired to increase the visible light transmittance of the glass, it is preferable that these components are substantially not contained.
[0117] In order to improve weather resistance against ultraviolet light irradiation, HfO2, Nb2O5, and Ti2O3 may be added. When added for the purpose of improving weather resistance against ultraviolet light irradiation, the total content of HfO2, Nb2O5, and Ti2O3 is preferably 1% or less, more preferably 0.5% or less, and even more preferably 0.1% or less, in order to suppress the influence on other properties.
[0118] In addition, SO3, chlorides, and fluorides may be appropriately contained as clarifiers for melting glass. The total content of components functioning as clarifiers is preferably 2% or less, more preferably 1% or less, and even more preferably 0.5% or less, expressed as mass% on an oxide basis, since adding too much of them affects the strengthening characteristics and crystallization behavior. The lower limit is not particularly limited, but typically, the total content is preferably 0.05% or more, expressed as mass% on an oxide basis.
[0119] When SO3 is used as a fining agent, the content of SO3 is preferably 0.01% or more, more preferably 0.05% or more, and even more preferably 0.1% or more, expressed as mass% on the oxide basis, since the effect is not observed if the content is too small. Also, when SO3 is used as a fining agent, the content of SO3 is preferably 1% or less, more preferably 0.8% or less, and even more preferably 0.6% or less, expressed as mass% on the oxide basis.
[0120] When Cl is used as a fining agent, if too much is added, it affects physical properties such as strengthening characteristics, so the Cl content is preferably 1% or less, more preferably 0.8% or less, and even more preferably 0.6% or less, expressed as mass % on the oxide basis. Also, if Cl is used as a fining agent, if the Cl content is too low, no effect is observed, so the Cl content is preferably 0.05% or more, more preferably 0.1% or more, and even more preferably 0.2% or more, expressed as mass % on the oxide basis.
[0121] When SnO2 is used as a clarifier, the content of SnO2 is preferably 1% or less, more preferably 0.5% or less, and even more preferably 0.3% or less, expressed as mass% on the oxide basis, since too little SnO2 content affects crystallization behavior. Also, when SnO2 is used as a clarifier, the content of SnO2 is not effective if it is too little, so it is preferably 0.02% or more, more preferably 0.05% or more, and even more preferably 0.1% or more, expressed as mass% on the oxide basis.
[0122] It is preferable that As2O3 is not contained. When As2O3 is contained, the content is preferably 0.3% or less, more preferably 0.1% or less, and most preferably, As2O3 is not contained.
[0123] The composition of the chemically strengthened glass used in the chemical strengthening of the present invention has the above composition. The glass raw materials are appropriately mixed so as to obtain the glass of the above composition, and are heated and melted in a glass melting furnace. The glass is then homogenized by bubbling, stirring, adding a clarifier, etc., formed into a glass plate of a predetermined thickness, and slowly cooled. Alternatively, the glass may be formed into a plate shape by forming it into a block shape, slowly cooling it, and then cutting it.
[0124] Examples of methods for forming into a plate include the float method, the press method, the fusion method, and the down-draw method. In particular, when producing a large glass plate, the float method is preferred. In addition, continuous forming methods other than the float method, such as the fusion method and the down-draw method, are also preferred.
[0125] The chemically strengthened glass may be crystallized glass. In the case of crystallized glass, it is preferable that the crystallized glass contains one or more crystals selected from the group consisting of lithium silicate crystals, lithium aluminosilicate crystals, and lithium phosphate crystals. As the lithium silicate crystals, lithium metasilicate crystals, lithium disilicate crystals, etc. are preferable. As the lithium phosphate crystals, lithium orthophosphate crystals, etc. are preferable. As the lithium aluminosilicate crystals, β-spodumene crystals, petalite crystals, etc. are preferable.
[0126] The crystallization rate of the crystallized glass is preferably 10% or more in order to increase the mechanical strength, more preferably 15% or more, even more preferably 20% or more, and particularly preferably 25% or more. In order to increase the transparency, it is preferably 70% or less, more preferably 60% or less, and particularly preferably 50% or less. A small crystallization rate is also excellent in that it is easy to heat and bend. The crystallization rate can be calculated from the X-ray diffraction intensity by the Rietveld method. The Rietveld method is described in "Crystal Analysis Handbook" edited by the editorial committee of the Japanese Crystallographic Society (Kyoritsu Shuppan, 1999, p492-499).
[0127] The average particle size of the precipitated crystals of the crystallized glass is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, and particularly preferably 100 nm or less, in order to increase transparency. The average particle size of the precipitated crystals can be obtained from a transmission electron microscope (TEM) image. It can also be estimated from a scanning electron microscope (SEM) image.
[0128] <Chemically strengthened glass> The chemically strengthened glass according to the embodiment of the present invention (hereinafter also referred to as the present chemically strengthened glass) is obtained by the above-mentioned present manufacturing method. That is, the present chemically strengthened glass has a compressive stress of CS 90 This gives the chemically strengthened glass excellent set drop strength. Here, in the set drop strength test, it is known that the stress at a certain depth from the glass surface is effective, especially for evaluation surfaces with large surface roughness such as sandpaper. Specifically, when the evaluation surface is sandpaper with grits of 60 to 100, the set drop strength is positively correlated with the stress at a depth of 90 μm from the surface. When the evaluation surface is sandpaper with grits of 100 to 140, the set drop strength is positively correlated with the stress at a depth of 70 μm from the surface. When the evaluation surface is sandpaper with grits of 160 to 200, the set drop strength is positively correlated with the stress at a depth of 50 μm from the surface.
[0129] That is, C.S. 90 A large value of contributes to improving the set drop strength, especially the "SP#80 drop strength." Therefore, this chemically strengthened glass is particularly excellent in "SP#80 drop strength."
[0130] (First embodiment) The chemically strengthened glass according to the first embodiment of the present invention is a chemically strengthened glass having a thickness t [mm], a compressive stress layer depth DOC [μm] of 160t [μm] or more, and a compressive stress value CS at a depth of 90 μm from the surface 90 [MPa] divided by the integral value of tensile stress ICT [MPa μm] CS 90 / ICT[μm -1 ] is 0.0012μm -1 That's all.
[0131] CS 90 The relatively large value of / ICT indicates that the CS 90 This means that the value of CS is relatively large. 90 The larger the value of / ICT, the greater the CS when the same level of compressive stress is introduced. 90 The chemically strengthened glass has improved strength and drop strength.
[0132] In addition, the glass obtained by the present manufacturing method has a relatively large DOC. As a result, the present chemically strengthened glass has compressive stress introduced to a deeper portion, and has excellent drop strength. Specifically, in this embodiment, the DOC is 160t [μm] or more.
[0133] CS 90 / ICT[μm -1 ] is 0.0012μm -1 More than 0.0013μm -1 More than 0.0014μm is preferable. -1 More preferably, 0.0015 μm or more -1 More preferably, 0.0016 μm or more. -1 The above is particularly preferable. On the other hand, from the viewpoint of balance with strengths other than the set drop strength, CS 90 / ICT[μm -1 ] is 0.0050μm -1 Less than 0.0048μm is preferable. -1 Less than 0.0045m is preferable. -1 More preferably, 0.0042 μm or less -1 Particularly preferred is 0.0040 μm -1 The following are most preferred:
[0134] The DOC is 160t [μm] or more, preferably 165t [μm] or more, more preferably 170t [μm] or more, even more preferably 180t [μm] or more, and most preferably 190t [μm] or more, where t [mm] is the thickness of the chemically strengthened glass. On the other hand, from the viewpoint of a decrease in productivity due to an increase in processing time, the DOC is preferably 350t [μm] or less, more preferably 300t [μm] or less, even more preferably 280t [μm] or less, particularly preferably 250t [μm] or less, and most preferably 240t [μm] or less.
[0135] CS 90 From the viewpoint of increasing the drop strength, it is preferable that CS is large, but the preferable value varies depending on the plate thickness t [mm]. 90 is preferably 5+50t [MPa] or more, more preferably 7+50t [MPa] or more, even more preferably 8+50t [MPa] or more, and particularly preferably 9+50t [MPa] or more. 90 From the viewpoint of balance with strengths other than the set drop strength, it is preferably -85+250t[MPa] or less, more preferably -83+250t[MPa] or less, even more preferably -84+250t[MPa] or less, and particularly preferably -83+250t[MPa] or less.
[0136] DOC is the compressive stress value at a depth of 50 μm from the surface, CS 50 [MPa] divided by DOC / CS 50 is preferably 0.8 μm / MPa or more, more preferably 0.83 μm / MPa or more, even more preferably 0.85 μm / MPa or more, particularly preferably 0.87 μm / MPa or more, and most preferably 0.9 μm / MPa or more. 50 The relatively large value of CS 50 This means that the DOC is larger than the DOC when compared with the case where the stress is the same. This is preferable because it allows stress to be introduced deeper into the soil and a high set drop strength can be obtained. On the other hand, from the viewpoint of the balance between deep layer stress and surface layer stress, the DOC / CS 50 is preferably 2.0 μm / MPa or less, more preferably 1.8 μm / MPa or less, even more preferably 1.6 μm / MPa or less, particularly preferably 1.5 μm / MPa or less, and most preferably 1.4 μm / MPa or less.
[0137] CS 90 is the compressive stress value CS at a depth of 50 μm from the surface 50 Value divided by [MPa]CS 90 / CS 50 is preferably 0.30 or more, more preferably 0.31 or more, even more preferably 0.32 or more, particularly preferably 0.35 or more, and most preferably 0.40 or more. 90 / CS 50 The relatively large value of CS 50 In the comparison of cases where CS 90 This is preferable because it can increase the drop strength of SP#80 in particular. On the other hand, from the viewpoint of the balance with the drop strength of SP#180, CS 90 / CS 50 is preferably 2.0 or less, more preferably 1.8 or less, even more preferably 1.6 or less, particularly preferably 1.5 or less, and most preferably 1.2 or less.
[0138] Stress value CS at depth x [μm] from the glass surface measured with a scattered light photoelastic stress meter x In the profile of [MPa], CS x Stress CS in the range ≧0 x The absolute value of the first derivative of |CS x is preferably less than 4, more preferably 3.5 or less, even more preferably 3.0 or less, particularly preferably 2.8 or less, and most preferably 2.6 or less. x The relatively small '| means that the profile shape is gentle and the stress value is stable throughout the deep layers. x It is preferable that |CS ' is in the above range because it is possible to obtain high set drop strength with high stress on the deep layer side. On the other hand, from the viewpoint of the balance between compressive stress and tensile stress, x is preferably 0.05 or more, more preferably 0.1 or more, even more preferably 0.2 or more, particularly preferably 0.3 or more, and most preferably 0.5 or more.
[0139] Stress value CS at depth x [μm] from the glass surface measured with a scattered light photoelastic stress meter x In the profile of [MPa], CS x Stress CS in the range ≧0 x The second derivative of CS x It is preferable that CS '' is -0.02 to 0.06. x is preferably 0.06 or less, more preferably 0.057 or less, even more preferably 0.055 or less, particularly preferably 0.052 or less, and most preferably 0.050 or less. x is preferably -0.02 or more, more preferably 0.000 or more, even more preferably 0.010 or more, particularly preferably 0.015 or more, and most preferably 0.020 or more. x The closer the value of '' is to 0 (the smaller the absolute value), the more linear the stress profile becomes, and the stress value CS at a depth of 90 μm 90 It can effectively improve CS x '' may be 0, that is, the stress profile may have an inflection point. A stress profile having an inflection point in a deep layer is preferable from the viewpoint that the tensile stress CT can be particularly small and therefore CT can be easily made less than the CT limit value. On the other hand, CS x '' takes a positive value, and the stress profile does not have to have an inflection point. A profile without an inflection point is preferable in that it has no local stress drop and can prevent the propagation of cracks generated from the surface layer of the glass.
[0140] In the present invention, the differentiation method of the stress profile is expressed by the following formula: CS x In the profile, CS when the change in x is 0.5 μm x The rate of change of CS x ' is used as the value of CS when the change in x is 0.5 μm. x ', the rate of change of CS x '' is used as the value. CS x '=(CS x+0.5 -CS x ) / 0.5 CS x ''=(CS x+0.5 '-CS x ') / 0.5
[0141] The surface compressive stress value CS0 measured by a glass surface stress meter is preferably 750 MPa or more, more preferably 780 MPa or more, even more preferably 800 MPa or more, particularly preferably 850 MPa or more, and most preferably 900 MPa or more, from the viewpoint of increasing the compressive stress of the surface layer and improving the strength against deformation such as bending. On the other hand, from the viewpoint of suppressing the occurrence of severe shattering in the event of cracking, CS0 is preferably 2500 MPa or less, more preferably 2000 MPa or less, even more preferably 1800 MPa or less, particularly preferably 1600 MPa or less, and most preferably 1400 MPa or less.
[0142] The compressive stress value CS1 [MPa] at a depth of 1 μm from the glass surface measured by a glass surface stress meter is preferably 550 MPa or more, more preferably 560 MPa or more, even more preferably 580 MPa or more, particularly preferably 600 MPa or more, and most preferably 650 MPa or more, from the viewpoint of suppressing further opening of the tips of fine scratches present on the glass surface. On the other hand, CS1 is preferably 1000 MPa or less, more preferably 950 MPa or less, even more preferably 900 MPa or less, particularly preferably 850 MPa or less, and most preferably 800 MPa or less, from the viewpoint of suppressing scattering of fine fragments in the event of breakage.
[0143] The surface compressive stress layer depth DOL-tail [μm] measured by a glass surface stress meter is preferably 2.8 μm or more, more preferably 3.0 μm or more, even more preferably 3.1 μm or more, particularly preferably 3.3 μm or more, and most preferably 3.5 μm or more, from the viewpoint of preventing cracks due to collision. On the other hand, in order to balance the total amount of compressive stress and tensile stress over the entire thickness direction of the glass, DOL-tail [μm] is preferably 10.0 μm or less, more preferably 9.0 μm or less, even more preferably 8.5 μm or less, particularly preferably 8.0 μm or less, and most preferably 7.5 μm or less.
[0144] Compressive stress value CS at a depth of 50 μm from the glass surface 50 From the viewpoint of improving the drop strength, [MPa] is preferably 90 MPa or more, more preferably 95 MPa or more, even more preferably 100 MPa or more, particularly preferably 105 MPa or more, and most preferably 110 MPa or more. 50 From the viewpoint of suppressing scattering of fine fragments during crushing due to the introduction of excessive energy by stress, the CS is preferably 300 MPa or less, more preferably 250 MPa or less, even more preferably 200 MPa or less, particularly preferably 180 MPa or less, and most preferably 160 MPa or less. 50 A large value contributes to improving the set drop strength, especially the "SP#180 drop strength."
[0145] Compressive stress value CS at a depth of 50 μm from the surface 50 [MPa] divided by the integral value of tensile stress ICT [MPa μm] CS 50 / ICT[μm -1 ] is 0.0037μm from the viewpoint of improving drop strength. -1 More than 0.0039 μm is preferable. -1 More preferably, 0.0040 μm or more -1 More preferably, 0.0042 μm or more -1 More preferably, 0.0043 μm or more. -1 The above is the most preferable. On the other hand, from the viewpoint of balance with strength other than drop strength, CS 50 / ICT[μm -1 ] is 0.0100μm -1 Less than 0.0090μm is preferable. -1 Less than 0.0080μm is more preferable. -1 More preferably, 0.0060 μm or less -1 Particularly preferred is 0.0050 μm -1 The following are most preferred:
[0146] CT-Max [MPa] represents the maximum tensile stress value in the stress profile. From the viewpoint of realizing excellent set drop strength, CT-Max is preferably 170-150t [MPa] or more, more preferably 172-150t [MPa] or more, even more preferably 175-150t [MPa] or more, and particularly preferably 180-150t [MPa] or more, in the case of thickness t [mm]. On the other hand, CT-Max is preferably 157.5-75t [MPa] or less, more preferably 152.5-75t [MPa] or less, even more preferably 150-75t [MPa] or less, particularly preferably 148-75t [MPa] or less, and most preferably 146-75t [MPa] or less, from the viewpoint of suppressing scattering of fine fragments when crushed due to excessive introduction of stress energy.
[0147] CTave [MPa] is a value equivalent to the average value of the tensile stress obtained by the above-mentioned method. From the viewpoint of realizing excellent set drop strength, CTave is preferably 107.5-75t [MPa] or more for thickness t [mm], more preferably 110-75t [MPa] or more, even more preferably 112.5-75t [MPa] or more, and particularly preferably 115-75t [MPa] or more. On the other hand, CTave is preferably 127.5-75t [MPa] or less, more preferably 125-75t [MPa] or less, particularly preferably 122.5-75t [MPa] or less, and most preferably 120-75t [MPa] or less, from the viewpoint of suppressing scattering of fine fragments when crushed due to excessive introduction of stress energy.
[0148] ICT [MPa·μm] represents the integral value of the tensile stress up to half the plate thickness. From the viewpoint of realizing excellent set drop strength, ICT is preferably 250+17500t [MPa·μm] or more for thickness t [mm], more preferably 300+17500t [MPa·μm] or more, even more preferably 350+17500t [MPa·μm] or more, and particularly preferably 400+17500t [MPa·μm] or more. On the other hand, from the viewpoint of preventing the scattering of fine fragments during crushing due to the introduction of excessive stress energy, ICT is preferably 4000+20000t[MPa·μm] or less, more preferably 3950+20000t[MPa·μm] or less, even more preferably 3900+20000t[MPa·μm] or less, particularly preferably 3850+20000[MPa·μm] or less, and most preferably 3800+20000t[MPa·μm] or less.
[0149] Second embodiment The chemically strengthened glass according to the second embodiment of the present invention is a chemically strengthened glass having a thickness t [mm], and the diffusion depth of Na ions, as determined from a Na ion concentration profile in the sheet thickness direction of the chemically strengthened glass measured by an electron beam microanalyzer, is 290t [μm] or more, and the ratio ΔNa90 / ΔNa50 of the difference ΔNa90 [mol%] between the Na2O concentration in the matrix composition of the chemically strengthened glass and the Na2O concentration at a depth of 90 μm from the surface to the difference ΔNa50 [mol%] between the Na2O concentration in the matrix composition of the chemically strengthened glass and the Na2O concentration at a depth of 50 μm from the surface is 0.55 or more. As described above with reference to FIGS. 1 and 2, the glass obtained by this manufacturing method is CS 90 and DOC are relatively large, and correspondingly, the diffusion depth of Na ions and the Na2O concentration at a depth of 90 μm from the surface are also relatively large. The chemically strengthened glass according to the second embodiment of the present invention has a diffusion depth of Na ions of 290t [μm] or more and a ΔNa90 / ΔNa50 of 0.55 or more, and is therefore excellent in set drop strength, particularly SP#80 drop strength.
[0150] The method for measuring the Na ion concentration profile in the sheet thickness direction of the chemically strengthened glass using an electron beam microanalyzer is as described above. The Na ion diffusion depth is the value at the position closest to the substrate surface where the count number is μ+3σ or more, calculated by calculating the average value μ and standard deviation σ of the count number in the range of ±50 μm from the center of the sheet thickness in the obtained Na ion profile in the sheet thickness direction.
[0151] From the viewpoint of introducing compressive stress to the deep layer and improving the drop strength, the Na ion diffusion depth [μm] is preferably 290t [μm] or more, more preferably 330t [μm] or more, even more preferably 360t [μm] or more, particularly preferably 400t [μm] or more, and most preferably 430t [μm] or more, where t [mm] is the thickness of the chemically strengthened glass. On the other hand, from the viewpoint of suppressing deterioration of the molten salt due to a large amount of ion exchange, the Na ion diffusion depth is preferably 500t [μm] or less, more preferably 480t [μm] or less, even more preferably 470t [μm] or less, particularly preferably 460t [μm] or less, and most preferably 450t [μm] or less.
[0152] The ratio ΔNa90 / ΔNa50 of the difference ΔNa50 [mol%] between the Na2O concentration in the matrix composition of the chemically strengthened glass and the Na2O concentration at a depth of 50 μm from the surface to the difference ΔNa90 [mol%] between the Na2O concentration in the matrix composition of the chemically strengthened glass and the Na2O concentration at a depth of 90 μm from the surface is preferably 0.55 or more, more preferably 0.60 or more, even more preferably 0.70 or more, particularly preferably 0.80 or more, and most preferably 0.90 or more, from the viewpoint of improving the drop strength. On the other hand, from the viewpoint of the balance with the surface layer stress, ΔNa90 / ΔNa50 is preferably 2.0 or less, more preferably 1.5 or less, even more preferably 1.3 or less, particularly preferably 1.2 or less, and most preferably 1.0 or less.
[0153] The ratio of ΔNa90 [mol%] to the Na2O concentration [mol%] in the matrix composition of the chemically strengthened glass is preferably 1.26 or more, more preferably 1.27 or more, even more preferably 1.28 or more, particularly preferably 1.29 or more, and most preferably 1.30 or more from the viewpoint of improving the drop strength. On the other hand, from the viewpoint of the balance with the surface stress, such a ratio is preferably 2.0 or less, more preferably 1.8 or less, even more preferably 1.7 or less, particularly preferably 1.6 or less, and most preferably 1.5 or less.
[0154] The chemically strengthened glass of the present invention may be the chemically strengthened glass according to the first embodiment and also the chemically strengthened glass according to the second embodiment. That is, a more preferred aspect of the chemically strengthened glass according to the second embodiment is similar to the preferred aspect of the chemically strengthened glass according to the first embodiment. In addition, the glass according to the first embodiment may have a preferred aspect of the chemically strengthened glass according to the second embodiment.
[0155] Hereinafter, preferred aspects common to the chemically strengthened glasses according to the first and second embodiments will be further described.
[0156] The chemically strengthened glass preferably has a set drop strength (SP#180 drop strength) of 60 cm or more, more preferably 65 cm or more, even more preferably 70 cm or more, and most preferably 75 cm or more, measured by a sandpaper set drop strength test under the following conditions. The set drop strength of 60 cm or more provides excellent strength when the glass is used as a product. Conditions: An electronic device with the chemically strengthened glass mounted on #180 sandpaper, or an electronic device simulation structure in which the chemically strengthened glass is integrated with a housing that holds the chemically strengthened glass, is dropped from a height of 30 cm. If the chemically strengthened glass does not break, the drop height is increased by 5 cm and dropped again. As long as the chemically strengthened glass does not break after being dropped, the process of dropping from a height increased by 5 cm is repeated. The height at which the chemically strengthened glass first breaks is defined as the break height. A drop test is performed using 10 samples, and the average break height of the 10 samples is defined as the set drop strength.
[0157] The chemically strengthened glass preferably has a set drop strength (SP#80 drop strength) of 40.5 cm or more, more preferably 41.0 cm or more, even more preferably 42.0 cm or more, and most preferably 45.0 cm or more, measured by a sandpaper set drop strength test under the following conditions. The set drop strength of 40.5 cm or more ensures that the glass exhibits excellent strength when used as a product. In addition, the chemically strengthened glass has a CS 90 A large / ICT tends to increase the set drop strength under the following conditions. Conditions: An electronic device with the chemically strengthened glass mounted on #80 sandpaper, or an electronic device simulation structure in which the chemically strengthened glass is integrated with a housing that holds the chemically strengthened glass, is dropped from a height of 30 cm. If the chemically strengthened glass does not break, the drop height is increased by 5 cm and dropped again. As long as the chemically strengthened glass does not break after being dropped, the process of dropping from a height increased by 5 cm is repeated. The height at which the chemically strengthened glass first breaks is defined as the break height. A drop test is performed using 10 samples, and the average break height of the 10 samples is defined as the set drop strength.
[0158] The present chemically strengthened glass preferably has a four-point bending strength of 650 MPa or more, more preferably 675 MPa or more, further preferably 700 MPa or more, and particularly preferably 750 MPa or more.
[0159] The shape of the chemically strengthened glass is not particularly limited, but is typically a plate shape, and may be flat or curved. Also, the glass may have portions with different thicknesses.
[0160] When the chemically strengthened glass is in the form of a plate, its thickness (t) is preferably 3.0 mm or less, more preferably 2.0 mm or less, 1.6 mm or less, 1.5 mm or less, 1.1 mm or less, 0.9 mm or less, 0.80 mm or less, and 0.70 mm or less in the following stepwise manner. In addition, the thickness (t) is preferably 0.30 mm or more, more preferably 0.40 mm or more, and even more preferably 0.50 mm or more in order to obtain sufficient strength by the chemical strengthening treatment.
[0161] The chemically strengthened glass is particularly useful as a cover glass for electronic devices such as mobile devices such as mobile phones and smartphones. It is also useful as a cover glass for electronic devices such as televisions, personal computers, and touch panels that are not intended to be portable, as elevator walls, and as walls (full-surface displays) of buildings such as houses and buildings. It is also useful as building materials such as window glass, table tops, interiors of automobiles and airplanes, and cover glass for these, and for curved housings. EXAMPLES
[0162] The present invention will be described below with reference to examples, but the present invention is not limited thereto. <Preparation of glass for chemical strengthening> The glass raw materials were mixed to obtain the following composition expressed in mole percentage based on oxides, and weighed out to obtain 400 g of glass. The mixed raw materials were then placed in a platinum crucible and placed in an electric furnace at 1500 to 1700°C to melt for about 3 hours, degassed, and homogenized. Glass material A: SiO2 68%, Al2O3 12%, Y2O3 1.4%, Li2O 10.7%, Na2O 1.6%, K2O 1.8%, MgO 3.5%, other components 1%. Glass material B: SiO2 66.2%, Al2O3 11.2%, Y2O3 0.5%, Li2O 10.4%, Na2O 5.6%, K2O 1.5%, MgO 3.1%, other components 1.5%.
[0163] The obtained molten glass was poured into a metal mold, held at a temperature about 50°C higher than the glass transition point for 1 hour, and then cooled to room temperature at a rate of 0.5°C / min to obtain a glass block. The obtained molten glass was poured into a mold, held at a temperature near the glass transition point (714°C) for about 1 hour, and then cooled to room temperature at a rate of 0.5°C / min to obtain a glass block.
[0164] The obtained glass block was cut, ground, and finally mirror-polished on both sides to obtain glass plates (glass for chemical strengthening) of 120 mm x 60 mm and thicknesses of 0.70 mm and 0.50 mm.
[0165] <Evaluation of chemical strengthening treatment and chemically strengthened glass> The glass plate obtained above was immersed in a molten salt composition under the conditions shown in Tables 1 to 3 to perform the first ion exchange treatment and the second ion exchange treatment, thereby obtaining chemically strengthened glass of Examples 1 to 16. However, in the droplet step (first droplet step) after the strengthening step as the first ion exchange treatment, heat treatment was performed under the conditions shown in Tables 1 to 3. "Droplet temperature" indicates the temperature of the heat treatment, and "Droplet time" indicates the time of the heat treatment. Examples 3, 4, 7, 9 to 16, 20, 21, and 25 are working examples, and Examples 1, 2, 5, 6, 8, 17 to 19, and 22 to 24 are comparative examples. The obtained chemically strengthened glass was evaluated by the following method. The results are shown in Tables 1 to 3.
[0166] [Stress measurement using a scattered light photoelastic stress meter] The stress of the chemically strengthened glass was measured by the method described in International Publication No. 2018 / 056121 using a scattered light photoelastic stress meter (SLP-2000 manufactured by Orihara Seisakusho). In addition, the stress profile was calculated using the attached software [SlpV (Ver. 2019.11.07.001)] of the scattered light photoelastic stress meter (SLP-2000 manufactured by Orihara Seisakusho).
[0167] The function used to obtain the stress profile is σ(x) = [a1 × erfc(a2 × x) + a3 × erfc(a4 × x) + a5]. i ( i = 1 to 5) are fitting parameters, and erfc is the complementary error function. The complementary error function is defined by the following equation.
[0168]
number
[0169] In the evaluation in this specification, the fitting parameters were optimized by minimizing the residual sum of squares between the obtained raw data and the above function. The measurement processing conditions were single shot, and the measurement area processing adjustment items were selected as follows: edge method on the surface, 6.0 μm for the inner surface end, automatic for the inner left and right ends, automatic (center of the sample thickness) for the inner deep end, and the extension of the phase curve to the center of the sample thickness was selected as a fitting curve.
[0170] The stress in the glass surface layer within a distance of several tens of μm from the glass surface was measured using a glass surface stress meter (FSM6000-UV manufactured by Orihara Seisakusho) according to the methods described in WO 2018 / 056121 and WO 2017 / 115811.
[0171] At the same time, the concentration distribution of alkali metal ions (sodium ions and potassium ions) in the cross-sectional direction was measured using an EPMA (Electron Probe Micro Analyzer) and it was confirmed that there was no inconsistency with the obtained stress profile.
[0172] In addition, from the above measurement results and the obtained stress profile, CS0, CS1, CS3, DOL-tail, CS x ', C.S. x '', C.S. 50 , C.S. 90 The values of DOC, ICT, CT-Max, and CTave were obtained. x ', C.S. x The maximum and minimum values of each are shown in Tables 1 to 3.
[0173] [Na ion concentration profile] The Na ion concentration at a depth x (μm) was measured in a cross section in the plate thickness direction by an EPMA (Electron Probe Micro Analyzer). The EPMA measurement was specifically performed as follows. First, the glass sample was embedded in epoxy resin, and mechanically polished in a direction perpendicular to the first main surface and the second main surface opposite the first main surface to prepare a cross-sectional sample. The polished cross section was coated with C-coat and measured using an EPMA (JEOL: JXA-8500F). The acceleration voltage was 15 kV, the probe current was 30 nA, and the integration time was 1000 msec. / point to obtain line profiles of X-ray intensity of Na ion concentration and Si ion concentration at 1 μm intervals. The obtained Na ion concentration profile was normalized by dividing by the average count of Si ion concentration at the center of the plate thickness (500 × t) ± 25 μm (plate thickness t [mm]). The Na2O concentration at a specific depth was calculated by converting the average count in the center of the sheet thickness (500 × t) ± 25 μm (sheet thickness t [mm]) proportionally to the Na2O concentration in the matrix composition of the chemically strengthened glass, and then converting the count for the entire sheet thickness proportionally to the molar percentage of Na2O concentration.
[0174] [Set Drop Strength Test] For the drop strength test, glass samples of 120 x 60 x 0.7 mm, 0.6 mm, and 0.5 mm were fitted into a structure whose mass and rigidity were adjusted to match the size of smartphones commonly used at the time of filing, a pseudo smartphone housing was prepared, and a marble was placed horizontally on the floor. Either #180 SiC sandpaper or #80 SiC sandpaper was laid parallel to the marble and fixed in place, and the pseudo smartphone housing was allowed to freely fall onto the #180 SiC sandpaper or #80 SiC sandpaper while held horizontal to the sandpaper. The drop height was started from 30cm, and if the sample did not break, it was dropped from a height of 5cm higher and dropped again, and this process was repeated until the sample broke. The height at which the sample first broke was recorded as the drop height. The average break height obtained when ten samples were dropped for each example is shown in Tables 1 to 3 as "SP#180 drop strength" or "SP#80 drop strength."
[0175] [4PB strength (4-point bending strength)] The chemically strengthened glass was processed into a strip of 120 mm x 60 mm, and a four-point bending test was performed under the conditions of a distance between the outer supports of the support of 30 mm, a distance between the inner supports of 10 mm, and a crosshead speed of 5.0 mm / min, to measure the four-point bending strength. The number of test pieces was 10. The chemically strengthened glass was processed into a strip, and then automatically chamfered (C chamfered) using a grinding wheel of No. 1000 (manufactured by Tokyo Diamond Tool Manufacturing Co., Ltd.), and the end faces were mirror-finished using a 0.1 mm diameter nylon brush and Showlox NZ abrasive grains (manufactured by Showa Denko Co., Ltd.) to obtain a 120 x 60 x 0.7 mm thick specimen.
[0176] [Table 1]
[0177] [Table 2]
[0178] [Table 3]
[0179] 1 shows stress profiles measured by SLP for the chemically strengthened glasses of Examples 5 and 3. FIG. 2 shows Na ion concentration profiles for the chemically strengthened glasses of Examples 5 and 3. Figure 4(a) shows the stress profile of the chemically strengthened glass of Example 4, and Figure 4(b) shows the stress profile of the chemically strengthened glass of Example 5. The stress profiles shown in Figures 4(a) and (b) were created by combining the stress profile information of the glass surface measured by SLP and the stress profile information inside the glass measured by FSM. The stress profiles were synthesized using "PMC", a software made by Orihara Seisakusho. From the results shown in Table 1 and Figures 1, 2 and 4, the chemically strengthened glass of the example, which was heat-treated under conditions where the heat treatment effect index value was 220 or more after the first ion exchange treatment and before the second ion exchange treatment, had a CS 90 / ICT and DOC are relatively large, and the CS 90 The values of were relatively large. In addition, the chemically strengthened glass of the examples also tended to have relatively large ΔNa90 / ΔNa50 and Na ion diffusion depth. The chemically strengthened glass of the examples was particularly excellent in terms of strength, particularly in SP#80 drop strength. For example, when Examples 1 to 5, 6 to 16, 17 to 21, and 22 to 25, which have the same plate thickness and composition of the chemically strengthened glass, were compared with each other, the chemically strengthened glass of the examples all had a superior SP#80 drop strength to the chemically strengthened glass of the comparative example.
[0180] As described above, the present specification discloses the following: 1. Chemically strengthened glass having a thickness t [mm], The compressive stress layer depth DOC [μm] is 160t [μm] or more, Compressive stress value CS at a depth of 90 μm from the surface 90 [MPa] divided by the integral value of tensile stress ICT [MPa μm] CS 90 / ICT[μm -1 ] is 0.0012μm -1 That's it, chemically strengthened glass. 2. Said CS 90 2. The chemically strengthened glass according to 1, wherein the compressive strength is 5+50t [MPa] or more. 3. The DOC is the compressive stress value CS at a depth of 50 μm from the surface. 50 [MPa] divided by DOC / CS 50 3. The chemically strengthened glass according to 1 or 2 above, wherein the glass modulus is 0.8 μm / MPa or more. 4. Said CS 90 is the compressive stress value CS at a depth of 50 μm from the surface 50 Value divided by [MPa]CS 90 / CS 50 4. The chemically strengthened glass according to any one of 1 to 3 above, wherein the value is 0.30 or more. 5. Stress value CS at a depth x [μm] from the glass surface measured with a scattered light photoelastic stress meter x In the profile of [MPa], CS x Stress CS in the range ≧0 x The first derivative value of CS x 5. The chemically strengthened glass according to any one of 1 to 4 above, wherein ' is less than 2. 6. Stress value CS at a depth x [μm] from the glass surface measured with a scattered light photoelastic stress meter x In the profile of [MPa], CS x Stress CS in the range ≧0 x The second derivative of CS x 6. The chemically strengthened glass according to any one of 1 to 5 above, wherein .lambda.'' is −0.02 to 0.06. 7. The surface compressive stress value CS0 measured by a glass surface stress meter is 750 MPa or more; 7. The chemically strengthened glass according to any one of 1 to 6 above. 8. The chemically strengthened glass according to any one of 1 to 7 above, which has a set drop strength of 40.5 cm or more as measured by a sandpaper set drop strength test under the following conditions: Conditions: An electronic device with the chemically strengthened glass mounted on #80 sandpaper, or an electronic device simulation structure in which the chemically strengthened glass is integrated with a housing that holds the chemically strengthened glass, is dropped from a height of 30 cm. If the chemically strengthened glass does not break, the drop height is increased by 5 cm and dropped again. As long as the chemically strengthened glass does not break after the drop, The step of dropping from a height increased by 5 cm is repeated. The height at which the chemically strengthened glass first breaks is defined as the crack height. A drop test is performed using 10 samples, and the average crack height of the 10 samples is defined as the set drop strength. 9. Chemically strengthened glass having a thickness t [mm], The Na ion diffusion depth, as determined from the Na ion concentration profile in the thickness direction of the chemically strengthened glass measured by an electron beam microanalyzer, is 290t [μm] or more; Chemically strengthened glass, in which the ratio ΔNa90 / ΔNa50 of the difference ΔNa50 [mol%] between the Na2O concentration in the matrix composition of the chemically strengthened glass and the Na2O concentration at a depth of 50 μm from the surface to the difference ΔNa90 [mol%] between the Na2O concentration in the matrix composition of the chemically strengthened glass and the Na2O concentration at a depth of 90 μm from the surface is 0.55 or more. 10. The chemically strengthened glass according to 9 above, wherein the ratio of the ΔNa90 [mol%] to the Na2O concentration [mol%] in the matrix composition of the chemically strengthened glass is 1.26 or more. 11. A first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition; A method for producing chemically strengthened glass, comprising: a second ion exchange treatment in which, after the first ion exchange treatment, the glass for chemical strengthening is brought into contact with a second molten salt composition, heat-treating the material after the first ion-exchange treatment and before the second ion-exchange treatment; First ion exchange treatment temperature T CT [℃] and the first ion exchange time t CT [min] is in the range of 10600 or less for the strengthening index (H value) defined by the following formula, and A method for producing chemically strengthened glass, wherein the heat treatment has a heat treatment effect index value (I value) defined by the following formula of 220 or more in the heat treatment.
[0181]
number
[0182]
number
[0183] However, in the above formula, t CT is the treatment time of the first ion exchange treatment [min], T CT is the temperature of the ion exchange treatment [°C], Σ[Me2O] is the sum of the alkali metal ion oxide concentrations in the glass for chemical strengthening. [mol%], t d is the first ion exchange treatment temperature T CT The time [minutes] during which the glass for chemical strengthening is kept at a temperature of 80% or more of [℃], T d is the temperature of the heat treatment [°C]. 12. Temperature T of the heat treatment d [℃] is 360℃ or more, or the heat treatment time t d 12. The method for producing chemically strengthened glass according to claim 11, wherein [minutes] is 10 minutes or longer. 13. Regarding the above-mentioned glass for chemical strengthening, when the CTA value calculated by the following formula (1) is x [MPa], The first ion exchange treatment causes the CTave value of the glass for chemical strengthening calculated by the following formula (2) to exceed x [MPa]; 13. The method for producing chemically strengthened glass according to claim 11 or 12, wherein the CTave value of the glass for chemical strengthening is made less than x [MPa] by the second ion exchange treatment.
[0184]
number
[0185] t: Plate thickness [mm] K1c: Fracture toughness value [MPa m 1 / 2 ] CTave=ICT / LCT...Equation (2) ICT: Tensile stress integral value [MPa μm] LCT: Length of tensile stress region in the thickness direction [μm]
[0186] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various modifications and changes can be made therein without departing from the spirit and scope of the invention. [Explanation of symbols]
[0187] 1. Chemically strengthened glass 25 Atmosphere Heater 50 Molten Salt Bath 55 Molten Salt Heater 53 Molten salt composition< / ctave>
Claims
1. A chemically strengthened glass having a thickness t [mm], The compressive stress layer depth DOC [μm] is 160t [μm] or more, Compressive stress value CS at a depth of 90 μm from the surface 90 [MPa] divided by the integral value of the tensile stress ICT [MPa μm] 90 / ICT [μm -1 ] is 0.0012 μm -1 That's it, chemically strengthened glass.
2. Said CS 90 The chemically strengthened glass according to claim 1, wherein the strain is 5 + 50t [MPa] or more.
3. The DOC is the compressive stress value CS at a depth of 50 μm from the surface. 50 Value divided by [MPa] DOC / CS 50 The chemically strengthened glass according to claim 1 or 2, wherein the chemical strengthening strength is 0.8 μm / MPa or more.
4. Said CS 90 The compressive stress value CS at a depth of 50 μm from the surface 50 Value divided by [MPa] CS 90 / CS 50 The chemically strengthened glass according to claim 1 or 2, wherein the chemical strengthening coefficient is 0.30 or more.
5. The stress value CS at a depth x [μm] from the glass surface is measured using a scattered light photoelastic stress meter. x In the profile of [MPa], CS x Stress CS in the range of ≧0 x The first derivative value CS x The chemically strengthened glass according to claim 1 or 2, wherein ' is less than 2.
6. The stress value CS at a depth x [μm] from the glass surface is measured using a scattered light photoelastic stress meter. x In the profile of [MPa], CS x Stress CS in the range of ≧0 x The second derivative value CS x The chemically strengthened glass according to claim 1 or 2, wherein '' is −0.02 to 0.
06.
7. Surface compressive stress value CS measured by a glass surface stress meter 0 The chemically strengthened glass according to claim 1 or 2, wherein the strength of the glass is 750 MPa or more.
8. The chemically strengthened glass according to claim 1 or 2, having a set drop strength of 40.5 cm or more measured by a sandpaper set drop strength test under the following conditions. Conditions: An electronic device with the chemically strengthened glass mounted on #80 sandpaper, or an electronic device simulation structure in which the chemically strengthened glass and a housing holding the chemically strengthened glass are integrated, is dropped from a height of 30 cm. If the chemically strengthened glass does not break, the drop height is increased by 5 cm and dropped again. As long as the chemically strengthened glass does not break after dropping, the process of dropping from a height increased by 5 cm is repeated. The height at which the chemically strengthened glass first breaks is defined as the crack height. A drop test is performed using 10 samples, and the average crack height of the 10 samples is defined as the set drop strength.
9. A chemically strengthened glass having a thickness t [mm], The Na ion diffusion depth obtained from the Na ion concentration profile in the plate thickness direction of the chemically strengthened glass measured by an electron beam microanalyzer is 290t [μm] or more, and Na in the matrix composition of the chemically strengthened glass 2 O concentration and Na concentration at a depth of 50 μm from the surface 2 Na in the parent composition of chemically strengthened glass relative to the difference ΔNa 50 [mol%] from the O concentration 2 O concentration and Na concentration at a depth of 90 μm from the surface 2 Chemically strengthened glass, wherein the ratio ΔNa90 / ΔNa50 of the difference ΔNa90 [mol%] from the O concentration is 0.55 or more.
10. Na in the matrix composition of chemically strengthened glass 2 The chemically strengthened glass according to claim 9, wherein a ratio of the ΔNa90 [mol%] to the O concentration [mol%] is 1.26 or more.
11. A first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition; A method for producing chemically strengthened glass, comprising: a second ion exchange treatment in which the glass for chemical strengthening is contacted with a second molten salt composition after the first ion exchange treatment; heat treating after the first ion exchange treatment and before the second ion exchange treatment; First ion exchange treatment temperature T CT [°C] and the first ion exchange time t CT [min] is in the range of 10600 or less of the strengthening index (H value) defined by the following formula, The method for producing chemically strengthened glass, wherein in the heat treatment, a heat treatment effect index value (I value) defined by the following formula is 220 or more. [0010] [0025] However, in the above formula, t CT is the treatment time [min] of the first ion exchange treatment, T CT is the temperature of the first ion exchange treatment [°C], Σ[Me 2 O] is the sum [mol%] of the alkali metal ion oxide concentrations in the chemically strengthened glass, t d is the first ion exchange treatment temperature T CT The time [min] for which the glass for chemical strengthening is left standing at a temperature of 80% or more [°C], T d is the temperature of the heat treatment [°C].
12. The temperature T of the heat treatment d [°C] is 360°C or more, or the heat treatment time t d The method for producing chemically strengthened glass according to claim 11, wherein [minutes] is 10 minutes or more.
13. For the glass for chemical strengthening, when the CTA value calculated by the following formula (1) is x [MPa], The first ion exchange treatment causes the CTave value of the glass for chemical strengthening calculated by the following formula (2) to exceed x [MPa], The method for producing chemically strengthened glass according to claim 11 or 12, wherein the CTave value of the chemically strengthened glass is less than x [MPa] by the second ion exchange treatment. [0030] t: Plate thickness [mm] K1c: Fracture toughness value [MPa m 1/2 ] CTave=ICT / LCT...Formula (2) ICT: integral value of tensile stress [MPa μm] LCT: Length of tensile stress region in the plate thickness direction [μm]
Citation Information
Patent Citations
Chemically strengthened glass production method and chemically strengthened glass
WO2022181812A1