Polyamide-based film, manufacturing method therefor, and cover window and display device each comprising the same

A polyamide film with tailored XRD and IR peak characteristics addresses the trade-off in mechanical and optical properties, offering improved modulus, scratch resistance, and reduced haze for display applications.

JP2024167300AActive Publication Date: 2024-12-03マイクロワークス ソリューションズ 株式会社
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024145022
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-29
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2041-09-08

AI Technical Summary

Technical Problem

There is a need for polyamide films with improved mechanical and optical properties, particularly for applications in foldable and flexible displays, where there is often a trade-off between mechanical strength and optical clarity.

Method used

A polyamide-based film with specific XRD and IR peak characteristics is developed, featuring a first XRD peak with a 2θ value between 10° and 20° and a half-width of 6° or less, and a ratio of IR peak areas of 1.4 or less, achieved through polymerization and heat-treatment of diamine and dicarbonyl compounds.

Benefits of technology

The film exhibits enhanced mechanical properties such as modulus and scratch resistance, along with improved optical properties like low haze and yellowness, making it suitable for display devices, especially in large or flexible formats.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167300000001_ABST
    Figure 2024167300000001_ABST
Patent Text Reader

Abstract

To provide a polyamide-based film excellent in optical characteristics and mechanical characteristics, and a manufacturing method therefor.SOLUTION: The polyamide-based film comprises a polyamide-based polymer and has a first IR peak having a maximum value in a section where the wavenumber is 2,950 cm-1 to 2,900 cm-1 and a second IR peak having a maximum value in a section where the wavenumber is 2,875 cm-1 to 2,825 cm-1, on an IR spectrum, wherein the area of the first IR peak may be 1.4 times or less relative to the area of the second IR peak.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The realization relates to a polyamide-based film having excellent optical and mechanical properties, a method for producing the same, and a cover window and a display device including the same. [Background technology]

[0002] Polyamide polymers have excellent resistance to friction, heat, and chemicals and are used in primary electrical insulation materials, coating agents, adhesives, extrusion resins, heat-resistant paints, heat-resistant plates, heat-resistant adhesives, heat-resistant fibers, and heat-resistant films.

[0003] Polyamides are used in a variety of fields. For example, polyamides are made into powder form and used as coatings for metals or magnet wires, and are mixed with other additives depending on the application. Polyamides are also used as decorative and corrosion-resistant paints together with fluoropolymers, and serve to adhere the fluoropolymers to metal substrates. Polyamides are also used to coat kitchen utensils, and are used as membranes for gas separation, due to their heat and chemical resistance, and are also used in devices that filter contaminants such as carbon dioxide, hydrogen sulfide, and impurities in natural gas wells.

[0004] Recently, polyamide-based films have been developed that are cheaper and have excellent optical, mechanical, and thermal properties by forming polyamide into films. Such polyamide-based films can be applied to display materials such as organic light-emitting diodes (OLEDs) or liquid crystal displays (LCDs), and can be used as anti-reflection films, compensation films, or retardation films when retardation properties are realized.

[0005] When such polyamide-based films are applied to foldable displays, flexible displays, etc., optical properties such as transparency and colorlessness, and mechanical properties such as flexibility and hardness are required. However, optical properties and mechanical properties are generally in a trade-off relationship, and improving mechanical properties may result in a decrease in optical properties.

[0006] Therefore, there is a continuing need for research into polyamide-based films with improved mechanical and optical properties. Summary of the Invention [Problem to be solved by the invention]

[0007] The implementation seeks to provide a polyamide-based film having excellent optical and mechanical properties, a method for producing the same, and a cover window and a display device including the same. [Means for solving the problem]

[0008] According to one embodiment, the polyamide-based film includes a polyamide-based polymer, and includes a first X-ray diffraction (XRD) peak having a maximum value in a range of 2θ values ​​of 10° or more and less than 20° on an XRD graph, and the half-width of the first XRD peak may be 6° or less.

[0009] According to one embodiment, a cover window for a display device includes a polyamide-based film and a functional layer, and the polyamide-based film includes a first XRD peak having a maximum value in a range of 2θ value of 10° or more and less than 20° on an XRD graph, and the half width of the first XRD peak may be 6° or less.

[0010] According to one embodiment, a display device includes a display unit and a cover window disposed on the display unit, the cover window includes a polyamide-based film and a functional layer, the polyamide-based film includes a first XRD peak having a maximum value in a range of 2θ values ​​of 10° or more and less than 20° on an XRD graph, and the half-width of the first XRD peak may be 6° or less.

[0011] A method for producing a polyamide-based film according to one embodiment includes the steps of: polymerizing a diamine compound and a dicarbonyl compound in an organic solvent to prepare a polymer solution containing a polyamide-based polymer; casting the polymer solution to produce a gel sheet; and heat-treating the gel sheet.

[0012] According to one embodiment, the polyamide-based film includes a polyamide-based polymer and has an IR spectrum of 2950 cm -1 ~2900cm -1 The first IR peak with a maximum value in the range and a wavenumber of 2875 cm -1 ~2825cm -1 The area of ​​the first IR peak may be 1.4 times or less than the area of ​​the second IR peak, the second IR peak having a maximum value in the interval.

[0013] According to one embodiment, a cover window for a display device includes a polyamide-based film and a functional layer, the polyamide-based film having a wavelength of 2950 cm in the IR spectrum. -1 ~2900cm -1 The first IR peak with a maximum value in the range and a wavenumber of 2875 cm -1 ~2825cm -1 and a second IR peak having a maximum value in the range, and the area of ​​the first IR peak may be 1.4 times or less than the area of ​​the second IR peak.

[0014] A display device according to one embodiment includes a display unit and a cover window disposed on the display unit, the cover window including a polyamide-based film and a functional layer, the polyamide-based film having a wavelength of 2950 cm in the IR spectrum.-1 ~2900cm -1 The first IR peak with a maximum value in the range and a wavenumber of 2875 cm -1 cm -1 ~2825cm -1 and a second IR peak having a maximum value in the range, and the area of ​​the first IR peak may be 1.4 times or less than the area of ​​the second IR peak.

[0015] A method for producing a polyamide-based film according to one embodiment includes the steps of: polymerizing a diamine compound and a dicarbonyl compound in an organic solvent to prepare a polymer solution containing a polyamide-based polymer; casting the polymer solution to produce a gel sheet; and heat-treating the gel sheet. Effect of the Invention

[0016] In one embodiment of the polyamide-based film, when separating XRD peaks in an XRD graph, the half-width of a first XRD peak located in the 2θ value range of 10° to less than 20° is 6° or less, and the spacing between the crystal planes of the crystalline component corresponding to the first XRD peak is relatively uniform, so that the polyamide-based film has excellent optical properties (low yellowness and haze, and high light transmittance) while also having improved mechanical properties (modulus, scratch resistance, etc.).

[0017] For example, the percentage of the half-width of the first XRD peak relative to the sum of the half-width of the first XRD peak and the half-width of the second XRD peak is 40% or less, and the spacing between the crystal planes of the wide-spacing crystal form is relatively uniform, thereby improving the modulus, transmittance, and scratch resistance of the polyamide-based film and reducing haze and yellowness.

[0018] In one embodiment, the polyamide-based film has an IR spectrum with a wave number of 2950 cm -1 ~2900cm -1 The area of ​​the first IR peak located in the section with a wavenumber of 2875 cm -1 ~2825cm -1The second IR peak is located in the interval of 1.4 times or less, and the film can have excellent modulus, transmittance, and low haze and yellowness.

[0019] In some embodiments of the polyamide-based film, the ratio of the area of ​​the first IR peak to the area of ​​the second IR peak is 0.6 or more, and the difference between the area of ​​the first IR peak and the area of ​​the second IR peak is small. Therefore, the chemical bonds corresponding to the first IR peak and the chemical bonds corresponding to the second IR peak are present in a ratio that does not differ significantly, and properties such as modulus, transmittance, haze, and yellowness can all be improved.

[0020] In addition, the polyamide-based film according to the embodiment has excellent mechanical and optical properties, and therefore can be usefully applied to cover windows for display devices and foldable / flexible display devices. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 shows a cross-sectional view of a display device according to one implementation. [Diagram 2] FIG. 2 shows a schematic flow chart of a method for producing a polyamide-based film according to one embodiment. [Diagram 3] FIG. 3 is a schematic flow chart illustrating steps for preparing a polyamide-based polymer solution according to some implementations. [Figure 4] FIG. 4 is an XRD analysis graph (diffractogram) for the polyamide film of Example 1. [Diagram 5] FIG. 5 shows FT-IR analysis spectra for the polyamide films of the examples and comparative examples. [Figure 6] FIG. 6 is an FT-IR analysis spectrum for the polyamide film of Example 7. [Figure 7] FIG. 7 is an FT-IR analysis spectrum for the polyamide film of Comparative Example 5. [Figure 8]FIG. 8 is an FT-IR analysis spectrum for the polyamide film of Comparative Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention will be described in detail below with reference to the accompanying drawings so that those skilled in the art can easily carry out the present invention. However, the present invention may be realized in various different forms and is not limited to the embodiments described herein.

[0023] In this specification, when it is described that each film, window, panel, or layer is formed "on" or "under" each film, window, panel, or layer, "on" and "under" include those formed "directly" or "indirectly through other components. In addition, the reference to the top / bottom of each component is described based on the drawings. Note that the size of each component in the drawings may be exaggerated for the purpose of explanation and does not represent the size actually applied. In addition, the same reference numerals refer to the same components throughout the specification.

[0024] In this specification, when a part is said to "comprise" a certain component, unless specifically stated to the contrary, it does not mean that it excludes other components, but that it may further include other components.

[0025] In this specification, the singular expressions are to be construed as including the singular or plural as the context requires, unless otherwise specified.

[0026] Also, all numbers and expressions expressing quantities of components, reaction conditions, and the like described herein should be understood to be modified in all instances by the term "about," unless otherwise specified.

[0027] In this specification, the terms "first", "second", etc. are used to describe various components, and the components should not be limited by the terms. The terms are used only to distinguish one component from another.

[0028] In addition, unless otherwise specified, the term "substituted" in this specification means substituted with one or more substituents selected from the group consisting of deuterium, -F, -Cl, -Br, -I, a hydroxyl group, a cyano group, a nitro group, an amino group, an amidino group, a hydrazine group, a hydrazone group, an ester group, a ketone group, a carboxyl group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted alkynyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted alicyclic organic group, a substituted or unsubstituted heterocyclic group, a substituted or unsubstituted aryl group, and a substituted or unsubstituted heteroaryl group, and the substituents listed above may be bonded to each other to form a ring.

[0029] [Polyamide film] One implementation provides polyamide-based films that have excellent optical properties such as high transmission, low haze, low yellowness, as well as excellent scratch resistance and / or modulus.

[0030] The polyamide-based film according to one implementation includes a polyamide-based polymer.

[0031] The polyamide-based film may include an XRD peak corresponding to a crystalline phase component on an XRD graph. The XRD peak may be a single XRD peak or a combined XRD peak including a plurality of single XRD peaks, and the plurality of XRD peaks included in the combined XRD peak may be separated into each single XRD peak by an XRD analysis method and program. In some implementations, the single XRD peak and the combined XRD peak may include a first XRD peak having a maximum value in a range of 2θ values ​​from 10° to less than 20°.

[0032] For example, the maximum or highest point of the first XRD peak may be located in a range of 2θ values ​​from 10° to less than 20°.

[0033] In some implementations, the combined XRD peak can further include a second XRD peak. In some implementations, the combined XRD peak can consist of the sum of the first XRD peak and the second XRD peak.

[0034] For example, the second XRD peak may have a maximum value in the 2θ range of 20° to 25°. The maximum value or highest point of the second XRD peak may be located in the 2θ range of 20° to 25°.

[0035] The first XRD peak and the second XRD peak may be summed to form a summed XRD peak, which may be located in a 2θ value range of 2° to 40°, preferably 5° to 35°, in some implementations.

[0036] As used herein, the term "XRD peak" may refer to an XRD pattern or its shape that deviates from a specific regression that can be expressed, for example, by a function, when the XRD pattern outside the section in which the XRD peak is located on the XRD graph has the specific regression.

[0037] The function is, for example, y=ae x +b, where a and b may be constants.

[0038] The particular regression may be defined as a baseline on the XRD graph. For example, the baseline may correspond to an XRD pattern of a non-crystalline component in the polyamide-based polymer or film, and the XRD peaks may correspond to an XRD pattern of a crystalline component.

[0039] In this case, the XRD peak may be defined as the portion whose intensity value is greater than (above) the baseline, which may be provided as the base of the XRD peak.

[0040] In some implementations, the half-width of the XRD peak may be measured. For example, the half-width may be defined as the width in a direction parallel to a tangent line from a point on the baseline to a maximum distance (maximum height) of the XRD pattern of the XRD peak in a direction perpendicular to the tangent line.

[0041] Among the crystal forms having various interplanar spacings that appear in the XRD pattern, a crystal form having a relatively wide interplanar spacing can be defined as a wide spacing crystal form, and a crystal form having a relatively narrow interplanar spacing can be defined as a narrow spacing crystal form.

[0042] In some implementations, the crystalline component corresponding to the first XRD peak may include a high proportion of a wide spacing crystalline form having a relatively wide spacing between crystal planes, and the crystalline component corresponding to the second XRD peak may include a high proportion of a narrow spacing crystalline form having a relatively narrow spacing between crystal planes.

[0043] The half-width of the first XRD peak may be 6° or less. In this case, the variation in the spacing between crystal planes of the crystalline component corresponding to the first XRD peak may be small. For example, the uniformity of the spacing between crystal planes of the wide spacing crystal form increases, and the mechanical properties such as scratch resistance and modulus of the polyamide-based film and the optical properties such as transmittance, haze, and yellowness may be improved. Preferably, the half-width of the first XRD peak may be 5.8° or less or 5.6° or less. Also, the half-width of the first XRD peak may be 5.0° or more, 5.2° or more, 5.4° or more, or 5.5° or more.

[0044] In some implementations, the percentage of the half-width of the first XRD peak to the sum of the half-width of the second XRD peak and the half-width of the first XRD peak may be 40% or less. In this case, for example, the uniformity between the crystal planes of the wide-spacing crystal form may be higher than the uniformity between the crystal planes of the narrow-spacing crystal form. In this case, the wide-spacing crystal form may have a relatively uniform crystal plane spacing. Therefore, mechanical properties such as scratch resistance and modulus and optical properties such as transmittance, haze, and yellowness of the polyamide-based film may both be improved. Preferably, the percentage of the half-width of the first XRD peak may be 38% or less or 36% or less.

[0045] Some examples of polyamide-based films have wavelengths of 3000 cm in the IR spectrum. -1 ~2800cm -1 The interval may include a first IR peak and a second IR peak.

[0046] In some implementations, the first IR peak has a wavenumber of 2950 cm -1 ~2900cm -1 For example, the maximum point of the first IR peak may be at wavenumber 2950 cm -1 ~2900cm -1 It may be located in the interval.

[0047] The second IR peak has a wave number of 2875 cm -1 ~2825cm -1 For example, the maximum point of the second IR peak may be at wavenumber 2875 cm -1 ~2825cm -1 It may be located in the interval.

[0048] In some implementations, the first IR peak has a wavenumber of about 2960 cm -1 ~2895cm -1 The second IR peak appears in the wavenumber range of about 2890 cm -1 ~2820cm -1 It can appear in the interval.

[0049] When the polyamide polymer has a sufficient length, the amide group (-C(=O)NH-) can form a hydrogen bond with an adjacent amide group (another amide group in the molecule) that is close to the polymer due to bending of the polymer. The hydrogen bond is formed between the oxygen and hydrogen of the amide group, and can also be formed between the nitrogen and hydrogen.

[0050] Alternatively, amide groups contained in different polyamide polymers may form hydrogen bonds (intermolecular hydrogen bonds) with each other. Therefore, at least four types of hydrogen bonds may be formed, including intramolecular oxygen-hydrogen bonds, intramolecular nitrogen-hydrogen bonds, intermolecular oxygen-hydrogen bonds, and intermolecular nitrogen-hydrogen bonds.

[0051] In an embodiment, the first IR peak and the second IR peak may be due to the hydrogen bonds. For example, among the four types of hydrogen bonds, a part (hereinafter, the first hydrogen bond group) may correspond to the first IR peak, and the rest (hereinafter, the second hydrogen bond group) may correspond to the second IR peak.

[0052] For example, one of the intramolecular hydrogen bonds and the intermolecular hydrogen bonds may correspond to the first IR peak and the other may correspond to the second IR peak, or one of the oxygen-hydrogen bonds and the nitrogen-hydrogen bonds may correspond to the first IR peak and the other may correspond to the second IR peak.

[0053] In some implementations, the polyamide polymer is sp3 It does not contain -H bonds. Therefore, the IR spectrum has a wave number of 3000 cm -1 ~2800cm -1 In the section, C sp3 May not include IR peaks due to -H, wavenumber 3000 cm -1 ~2800cm -1 In this section, IR peaks due to the hydrogen bonds may appear.

[0054] The area of ​​the first IR peak may be 1.4 times or less than the area of ​​the second IR peak. In this case, since the difference between the ratio of the first hydrogen bonding group and the second hydrogen bonding group is not large, the optical properties such as light transmittance, haze, yellowness index, etc. and the mechanical properties such as modulus of the polyamide film may be improved. Preferably, the area of ​​the first IR peak may be 1.3 times or less, 1.2 times or less, or 1.1 times or less than the area of ​​the second IR peak.

[0055] In some implementations, the area of ​​the first IR peak can be 0.6 times or more, 0.7 times or more, 0.8 times or more, or 0.9 times or more relative to the area of ​​the second IR peak.

[0056] In some implementations, the area of ​​the first IR peak may be 0.8 times or more and 1.2 times or less than the area of ​​the second IR peak. In this case, the first hydrogen bonding group and the second hydrogen bonding group are present in substantially equal amounts, and the optical and mechanical properties of the polyamide-based film may be improved. Preferably, the area of ​​the first IR peak may be 0.9 times or more and 1.1 times or less than the area of ​​the second IR peak.

[0057] The area of ​​an IR peak can be obtained by subtracting the area of ​​noise from the total area of ​​the section in which the IR peak appears on the IR spectrum. For example, a straight line connecting the start point and end point of the IR peak is defined as a baseline, and the area below the baseline (an area with low absorbance) can correspond to noise.

[0058] The refractive index in the x direction (n x ) may be 1.60 to 1.70, 1.61 to 1.69, 1.62 to 1.68, 1.64 to 1.68, 1.64 to 1.66, or 1.64 to 1.65.

[0059] In addition, the refractive index in the y direction of the polyamide film (n y) may be 1.60 to 1.70, 1.61 to 1.69, 1.62 to 1.68, 1.63 to 1.68, 1.63 to 1.66, or 1.63 to 1.64.

[0060] Furthermore, the z-direction refractive index (n z ) may be 1.50 to 1.60, 1.51 to 1.59, 1.52 to 1.58, 1.53 to 1.58, 1.54 to 1.58, or 1.54 to 1.56.

[0061] When the values ​​of the x-direction refractive index, y-direction refractive index, and z-direction refractive index of the polyamide-based film are within the above ranges, when the film is applied to a display device, excellent visibility can be achieved not only when viewed from the front but also from the side, and a wide viewing angle can be achieved.

[0062] In-plane retardation (R o ) may be 800 nm or less. Specifically, the in-plane retardation (R o ) can be 700 nm or less, 600 nm or less, 550 nm or less, 100 nm to 800 nm, 200 nm to 800 nm, 200 nm to 700 nm, 300 nm to 700 nm, 300 nm to 600 nm, or 300 nm to 540 nm.

[0063] In addition, the thickness direction retardation (R th ) may be 5000 nm or less. Specifically, the thickness direction retardation (R th ) can be 4800 nm or less, 4700 nm or less, 4650 nm or less, 1000 nm to 5000 nm, 1500 nm to 5000 nm, 2000 nm to 5000 nm, 2500 nm to 5000 nm, 3000 nm to 5000 nm, 3500 nm to 5000 nm, 4000 nm to 5000 nm, 3000 nm to 4800 nm, 3000 nm to 4700 nm, 4000 nm to 4700, or 4200 nm to 4650 nm.

[0064] Here, the in-plane retardation (Ro ) is the anisotropy of the refractive index along two perpendicular axes in the plane of the film (△n xy =|n x -n y |) and the film thickness (d) (△n xy × d) is a measure of optical isotropy or anisotropy.

[0065] In addition, the thickness direction retardation (R th ) are the two birefringences Δn xz (=|n x -n z |) and △n yz (=|n y -n z This parameter is defined as the average of the phase difference obtained by multiplying the phase difference (f,g) and the film thickness (d).

[0066] When the in-plane retardation and thickness direction retardation of the polyamide-based film are within the above ranges, optical distortion and color distortion can be minimized when the film is applied to a display device, and the light leakage phenomenon in which light leaks from the side can also be minimized.

[0067] The polyamide film may further include a filler in addition to the polyamide polymer.

[0068] The average particle size of the filler may be 60 nm to 180 nm. Specifically, the average particle size of the filler may be, but is not limited to, 80 nm to 180 nm, 100 nm to 180 nm, 110 nm to 160 nm, 120 nm to 160 nm, or 130 nm to 150 nm.

[0069] When the average particle size of the filler is within the above range, the optical properties do not deteriorate even if a relatively large amount is added, as compared with other inorganic fillers.

[0070] The refractive index of the filler may be 1.55 to 1.75. Specifically, the refractive index of the filler may be, but is not limited to, 1.60 to 1.75, 1.60 to 1.70, 1.60 to 1.68, or 1.62 to 1.65.

[0071] When the refractive index of the filler satisfies the above range, n x , n y , n z By appropriately adjusting the birefringence values ​​associated with the .lambda., the brightness at various angles of the film can be improved.

[0072] On the other hand, if the refractive index of the filler is outside the above range, the presence of the filler may be visible to the naked eye on the film, or the filler may cause problems such as an increase in haze.

[0073] The content of the filler may be 100 ppm to 3000 ppm based on the total weight of the polyamide-based polymer solid content, specifically, the content of the filler may be, but is not limited to, 100 ppm to 2500 ppm, 100 ppm to 2200 ppm, 200 ppm to 2500 ppm, 200 ppm to 2200 ppm, 250 ppm to 2100 ppm, or 300 ppm to 2000 ppm based on the total weight of the polyamide-based polymer solid content.

[0074] If the filler content is outside the above range, the haze of the film will increase rapidly, and the fillers will aggregate on the film surface, causing a visually noticeable foreign body sensation, problems with running during the production process, and reduced winding properties.

[0075] The fillers may include, for example, but are not limited to, silica and barium sulfate.

[0076] The filler may be included in a particulate form, and may be uniformly dispersed throughout the film without any special surface coating treatment.

[0077] By including the filler in the polyamide-based film, the film can ensure a wide viewing angle without deteriorating the optical properties.

[0078] The residual solvent content in the polyamide film may be 1500 ppm or less. For example, the residual solvent content may be, but is not limited to, 1200 ppm or less, 1000 ppm or less, 800 ppm or less, or 500 ppm or less.

[0079] The residual solvent means the amount of solvent that is not evaporated during the film production and remains in the final film.

[0080] If the content of the residual solvent in the polyamide film exceeds the above range, the durability of the film may decrease and the brightness may also be affected.

[0081] According to an embodiment, when a polyamide-based film having a thickness of 50 μm is folded to a curvature radius of 3 mm, the film can be folded more than 200,000 times before breaking.

[0082] The number of folding cycles is defined as one cycle of bending the film to a curvature radius of 3 mm and then unfolding it.

[0083] Since the polyamide-based film satisfies the folding number within the above range, it can be usefully applied to a foldable display device or a flexible display device.

[0084] According to an embodiment, the surface roughness of the polyamide-based film may be 0.01 μm to 0.07 μm. Specifically, the surface roughness may be 0.01 μm to 0.07 μm or 0.01 μm to 0.06 μm, but is not limited thereto.

[0085] When the surface roughness of the polyamide film satisfies the above range, it is advantageous to realize high brightness even when the angle from the normal direction of the surface light source is large.

[0086] According to one embodiment, the polyamide-based film includes a polyamide-based polymer, which includes amide repeat units and may optionally include imide repeat units.

[0087] In some implementations, the polyamide-based polymer may not include the imide repeat unit and may include only the amide repeat unit, which may increase the modulus of the polyamide-based film and allow it to be effectively applied to foldable / flexible display devices, and may improve transmittance and reduce yellowness and haze.

[0088] The polyamide-based film includes a polyamide-based polymer, which may be formed by simultaneously or sequentially reacting reactants including a diamine compound and a dicarbonyl compound, and more specifically, the polyamide-based polymer may be formed by polymerizing a diamine compound and a dicarbonyl compound.

[0089] Alternatively, the polyamide-based polymer may be formed by polymerizing a diamine compound, a dianhydride compound, and a dicarbonyl compound, and may include an imide repeating unit derived from the polymerization of the diamine compound and the dianhydride compound, and an amide repeating unit derived from the polymerization of the diamine compound and the dicarbonyl compound.

[0090] In some implementations, the polyamide-based polymer may be polymerized without the dianhydride compound, in which case the polyamide-based polymer may not include imide repeat units.

[0091] According to an embodiment, the polyamide-based film may include a polyamide-based polymer formed by polymerizing a diamine compound and a dicarbonyl compound to form an amide bond, and the polyamide-based polymer may optionally include a polyamide-imide-based polymer formed by further polymerizing a dianhydride compound to form an imide bond.

[0092] In some implementations, the polyamide-based polymer may not include the polyamide-imide-based polymer, in which case the modulus of the polyamide-based film may be increased, making it more effective for use in foldable / flexible display devices, and the transmittance may be improved and yellowness and haze may be reduced.

[0093] The diamine compound is a compound that forms an imide bond with the dianhydride compound and an amide bond with the dicarbonyl compound to form a copolymer.

[0094] The diamine compound is not particularly limited, and may be, for example, an aromatic diamine compound having an aromatic structure. For example, the diamine compound may be a compound represented by the following Formula 1: [C1] JPEG2024167300000002.jpg863

[0095] In the above formula 1, E is a substituted or unsubstituted divalent C6-C 30 Alicyclic radicals, substituted or unsubstituted divalent C4-C 30 Heteroalicyclic groups, substituted or unsubstituted divalent C6-C 30 Aromatic ring groups, substituted or unsubstituted divalent C4-C 30 Aromatic heterocyclic groups, substituted or unsubstituted C1-C 30 Alkylene groups, substituted or unsubstituted C2-C 30 Alkenylene groups, substituted or unsubstituted C2-C 30 Alkynylene groups may be selected from among -O-, -S-, -C(=O)-, -CH(OH)-, -S(=O)2-, -Si(CH3)2-, -C(CH3)2-, and -C(CF3)2-.

[0096] e is selected from integers of 1 to 5, and when e is 2 or more, E may be the same or different.

[0097] (E) of Chemical Formula 1 ecan be selected from groups represented by the following chemical formulas 1-1a to 1-14a, but is not limited thereto. JPEG2024167300000003.jpg89141

[0098] Specifically, (E) of the above Chemical Formula 1 e can be selected from groups represented by the following chemical formulas 1-1b to 1-13b, but is not limited thereto. JPEG2024167300000004.jpg88131

[0099] More specifically, (E) of the above Chemical Formula 1 e may be a group represented by the above chemical formula 1-6b or a group represented by the above chemical formula 1-9b.

[0100] In one implementation, the diamine compound may include a compound having a fluorine-containing substituent or a compound having an ether group (-O-).

[0101] The diamine compound may be a compound having a fluorine-containing substituent, where the fluorine-containing substituent is a fluorinated hydrocarbon group, specifically, a trifluoromethyl group, but is not limited thereto.

[0102] In another embodiment, the diamine compound may be one type of diamine compound, i.e., the diamine compound may consist of a single component.

[0103] For example, the diamine compound may include, but is not limited to, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl (TFMB) having the following structure: JPEG2024167300000005.jpg66117

[0104] The dicarbonyl compound is not particularly limited, and may be, for example, a compound represented by the following formula 3. [C3] JPEG2024167300000006.jpg2657

[0105] In the above formula 3, J is a substituted or unsubstituted divalent C6-C 30 Alicyclic radicals, substituted or unsubstituted divalent C4-C 30 Heteroalicyclic groups, substituted or unsubstituted divalent C6-C 30 Aromatic ring groups, substituted or unsubstituted divalent C4-C 30 Aromatic heterocyclic groups, substituted or unsubstituted C1-C 30 Alkylene groups, substituted or unsubstituted C2-C 30 Alkenylene groups, substituted or unsubstituted C2-C 30 Alkynylene groups may be selected from among -O-, -S-, -C(=O)-, -CH(OH)-, -S(=O)2-, -Si(CH3)2-, -C(CH3)2-, and -C(CF3)2-.

[0106] j is selected from integers of 1 to 5, and when j is 2 or more, J may be the same or different. X is a halogen atom. Specifically, X can be F, Cl, Br, I, etc. More specifically, X can be Cl, but is not limited thereto.

[0107] JPEG2024167300000007.jpg96144 (J) of the above chemical formula 3 j can be selected from groups represented by the following chemical formulas 3-1a to 3-14a, but is not limited thereto.

[0108] Specifically, (J) of the above Chemical Formula 3 j can be selected from groups represented by the following chemical formulas 3-1b to 3-8b, but is not limited thereto. JPEG2024167300000008.jpg74150

[0109] More specifically, (J) of the above Chemical Formula 3 jmay be a group represented by the above chemical formula 3-1b, a group represented by the above chemical formula 3-2b, a group represented by the above chemical formula 3-3b, or a group represented by the above chemical formula 3-8b.

[0110] In one embodiment, the dicarbonyl compound may be a mixture of at least two different dicarbonyl compounds. When two or more dicarbonyl compounds are used, the dicarbonyl compound may be (J) in Formula 3. j may be used two or more selected from the groups represented by the chemical formulas 3-1b to 3-8b.

[0111] In another implementation, the dicarbonyl compound can be an aromatic dicarbonyl compound that includes an aromatic structure.

[0112] The dicarbonyl compound may include, but is not limited to, terephthaloyl chloride (TPC), 1,1'-biphenyl-4,4'-dicarbonyl dichloride (BPDC), isophthaloyl chloride (IPC), or a combination thereof, having the following structure: JPEG2024167300000009.jpg2657JPEG2024167300000010.jpg2874JPEG2024167300000011.jpg3446

[0113] In one embodiment, the polyamide polymer may include two or more types of amide repeat units.

[0114] For example, the two or more kinds of amide repeating units may include a first amide repeating unit and a second amide repeating unit, the first amide repeating unit being formed by a reaction between a first dicarbonyl compound and the diamine compound, and the second amide repeating unit being formed by a reaction between a second dicarbonyl compound and the diamine compound.

[0115] The first dicarbonyl compound and the second dicarbonyl compound may be different compounds.

[0116] The first dicarbonyl compound and the second dicarbonyl compound may each include two carbonyl groups, and the angle between the two carbonyl groups included in the first dicarbonyl compound may be greater than the angle between the two carbonyl groups included in the second dicarbonyl compound.

[0117] In an exemplary embodiment, the first dicarbonyl compound and the second dicarbonyl compound may be structural isomers. By using two dicarbonyl compounds having a structural isomer relationship, a polyamide-based polymer satisfying the above-mentioned crystal plane spacing can be formed, and thus the optical properties and mechanical properties of the polyamide-based polymer can be improved.

[0118] The first dicarbonyl compound and the second dicarbonyl compound can each be an aromatic dicarbonyl compound.

[0119] For example, the first dicarbonyl compound and the second dicarbonyl compound may be different aromatic dicarbonyl compounds, but are not limited thereto.

[0120] When the first dicarbonyl compound and the second dicarbonyl compound are each an aromatic dicarbonyl compound, they contain a benzene ring, which can contribute to improving mechanical properties such as surface hardness and tensile strength of a film containing the produced polyamide-based polymer.

[0121] For example, the angle between the two carbonyl groups contained in the first dicarbonyl compound may be 160° to 180°, and the angle between the two carbonyl groups contained in the second dicarbonyl compound may be 80° to 140°.

[0122] For example, the dicarbonyl compound can include a first dicarbonyl compound and / or the second dicarbonyl compound.

[0123] For example, the first dicarbonyl compound may include TPC and the second dicarbonyl compound may include IPC, but is not limited thereto.

[0124] When TPC is used as the first dicarbonyl compound and IPC is used as the second dicarbonyl compound in an appropriate combination, the film containing the prepared polyamide-based polymer may have high oxidation resistance, productivity, light transmittance, transparency, modulus, etc., and may have low haze.

[0125] The diamine compound and the dicarbonyl compound can be polymerized to form a repeating unit represented by the following chemical formula B. [Case B] JPEG2024167300000012.jpg3679In the chemical formula B, the explanations for E, J, e, and j are as described above.

[0126] For example, the diamine compound and the dicarbonyl compound can be polymerized to form amide repeat units represented by formulas B-1 and B-2.

[0127] [Case B-1] JPEG2024167300000013.jpg38128 In the chemical formula B-1, y is an integer of 1 to 400.

[0128] [Case B-2] JPEG2024167300000014.jpg40128 In the chemical formula B-2, y is an integer of 1 to 400.

[0129] In some embodiments, the molar ratio of the first amide repeating unit to the second amide repeating unit may be 10:90 to 90:10. By setting the molar ratio of the first and second amide repeating units within the above range, the crystal plane spacing of the polyamide polymer may be adjusted to the above range. Therefore, physical properties such as haze, light transmittance, yellowness, and modulus of the polyamide film may be improved. Preferably, the molar ratio of the first amide repeating unit to the second amide repeating unit may be 25:75 to 80:20, 40:60 to 80:20, or 50:50 to 75:25.

[0130] In some implementations, the polyamide-based film may have a thickness deviation of 4 μm or less based on a thickness of 50 μm. The thickness deviation may refer to the deviation between the maximum or minimum value from the average thickness measured at 10 random positions on the film. In this case, the polyamide-based film has a uniform thickness, so that the optical and mechanical properties at each point may be uniform.

[0131] The haze of the polyamide film may be 1% or less. For example, the haze may be 0.5% or less or 0.4% or less, but is not limited thereto.

[0132] The polyamide film may have a transmittance of 80% or more. For example, the transmittance may be 82% or more, 85% or more, 88% or more, 89% or more, 80% to 99%, 88% to 99%, or 89% to 99%, but is not limited thereto.

[0133] The polyamide film may have a yellow index of 3.5 or less. For example, the yellow index may be 3 or less, 2.5 or less, or 2 or less, but is not limited thereto.

[0134] The polyamide-based film may have a modulus of 5 GPa or more. Specifically, the modulus may be 5.5 GPa or more, or 6.0 GPa or more, but is not limited thereto.

[0135] The polyamide film may have a compressive strength of 0.4 kgf / μm or more. Specifically, the compressive strength may be 0.45 kgf / μm or more or 0.46 kgf / μm or more, but is not limited thereto.

[0136] When the polyamide film is perforated in UTM compression mode using a 2.5 mm spherical tip at a speed of 10 mm / min, the maximum diameter (mm) of the perforation including cracks is 60 mm or less. Specifically, the maximum diameter of the perforation may be, but is not limited to, 5 mm to 60 mm, 10 mm to 60 mm, 15 mm to 60 mm, 20 mm to 60 mm, 25 mm to 60 mm, or 25 mm to 58 mm.

[0137] The polyamide-based film may have a surface pencil hardness of HB or more. Specifically, the surface pencil hardness may be H or more or 2H or more, but is not limited thereto.

[0138] The polyamide film has a tensile strength of 15 kgf / mm 2 Specifically, the tensile strength may be 18 kgf / mm 2 Above 20kgf / mm 2 Above, 21kgf / mm 2 or more than 22kgf / mm 2 It may be more than this, but is not limited to this.

[0139] The polyamide film may have an elongation percentage of 15% or more. Specifically, the elongation percentage may be, but is not limited to, 16% or more, 17% or more, or 17.5% or more.

[0140] The polyamide-based film according to the embodiment has excellent optical properties such as low haze, low yellowness, and high transmittance, as well as excellent scratch resistance and / or modulus, and therefore can be effectively applied to, for example, flexible / foldable display devices.

[0141] The above-mentioned physical properties of the polyamide film are based on a thickness of 40 μm to 60 μm, for example, based on a thickness of 50 μm.

[0142] The aforementioned features regarding the components and physical properties of the polyamide-based film may be combined with each other.

[0143] For example, the polyamide-based film may include a polyamide-based polymer and have a transmittance of 80% or more, a haze of 1% or less, and a yellowness index of 3.5 or less, or 3 or less.

[0144] In addition, the above-mentioned XRD pattern and IR spectral characteristics and physical properties of the polyamide-based film may be the result of combining the process conditions of each step in the method for producing the polyamide-based film described below, together with the chemical and physical properties of the components constituting the polyamide-based film.

[0145] For example, the composition and contents of the components constituting the polyamide film, the polymerization conditions and heat treatment conditions in the film manufacturing process, etc., can all be combined to realize the desired characteristics in the XRD and IR patterns.

[0146] In some implementations, the molecular structure of the polyamide polymer may be changed depending on the amounts of the first dicarbonyl compound and the second dicarbonyl compound used, polymerization conditions, etc. In this case, the ratio of the first hydrogen bond group to the second hydrogen bond group may be changed, and thus the ratio of the area of ​​the first IR peak to the area of ​​the second IR peak may be adjusted.

[0147] [Cover window for display device] A cover window for a display device according to one implementation includes a polyamide-based film and a functional layer.

[0148] According to some embodiments, the polyamide-based film includes a polyamide-based polymer, and includes a first XRD peak having a maximum value in the range of 2θ value of 10° or more and less than 20° on an XRD graph, and the half width of the first XRD peak may be 6° or less.

[0149] The polyamide film is as described above. The cover window for a display device can be usefully applied to a display device.

[0150] The polyamide film has the above-mentioned characteristics of the peak position and half width in the XRD analysis pattern, and therefore can have excellent optical properties and mechanical properties.

[0151] The polyamide-based film according to some implementations includes a polyamide-based polymer and has an IR spectrum of 2950 cm -1 ~2900cm -1 The first IR peak with a maximum value in the range and a wavenumber of 2875 cm -1 cm -1 ~2825cm -1 and a second IR peak having a maximum value in the range, and the area of ​​the first IR peak may be 1.4 times or less than the area of ​​the second IR peak.

[0152] The polyamide-based film has an IR spectrum wave number of 3000 cm -1 ~2800cm -1 When the area ratio of the peaks located in the section has the above-mentioned characteristics, the film can have excellent optical properties and mechanical properties.

[0153] [Display device] A display device according to one implementation includes a display portion and a cover window disposed on the display portion, the cover window including a polyamide-based film and a functional layer.

[0154] According to some embodiments, the polyamide-based film includes a polyamide-based polymer and includes a first XRD peak having a maximum value in a range of 2θ values ​​of 10° or more and less than 20° on an XRD graph, and the half-width of the first XRD peak may be 6° or less.

[0155] The polyamide-based film according to some implementations includes a polyamide-based polymer and has an IR spectrum of 2950 cm -1 ~2900cm -1 The first IR peak with a maximum value in the range and a wavenumber of 2875 cm -1 cm -1 ~2825cm -1 and a second IR peak having a maximum value in the range, and the area of ​​the first IR peak may be 1.4 times or less than the area of ​​the second IR peak.

[0156] The polyamide film and the cover window are described above in detail.

[0157] FIG. 1 shows a cross-sectional view of a display device according to one implementation.

[0158] Specifically, Figure 1 illustrates a display device in which a display unit 400 is disposed on the display unit 400, and a cover window 300 including a polyamide-based film 100 having a first surface 101 and a second surface 102 and a functional layer 200, and an adhesive layer 500 is disposed between the display unit 400 and the cover window 300.

[0159] The display unit 400 can display an image and can have a flexible characteristic.

[0160] The display unit 400 may be a display panel for displaying an image, such as a liquid crystal display panel or an organic electroluminescence display panel. The organic electroluminescence display panel may include a front polarizer and an organic EL panel.

[0161] The front polarizer may be disposed on a front surface of the organic electroluminescence panel. Specifically, the front polarizer may be attached to a surface of the organic electroluminescence panel on which an image is displayed.

[0162] The organic EL panel may display an image by self-luminescence in pixel units. The organic EL panel may include an organic EL substrate and a driving substrate. The organic EL substrate may include a plurality of organic electroluminescent units each corresponding to a pixel. Specifically, each may include a cathode, an electron transport layer, a light-emitting layer, a hole transport layer, and an anode. The driving substrate may be drivingly connected to the organic EL substrate. That is, the driving substrate may be connected to the organic EL substrate so as to apply a driving signal such as a driving current to the organic EL substrate, thereby applying a current to each of the organic electroluminescent units to drive the organic EL substrate.

[0163] Also, an adhesive layer 500 may be included between the display unit 400 and the cover window 300. The adhesive layer may be an optically transparent adhesive layer, and is not particularly limited.

[0164] The cover window 300 may be disposed on the display unit 400. The cover window may be located at the outermost periphery of a display device according to an embodiment, and may protect the display unit.

[0165] The cover window 300 may include a polyamide-based film and a functional layer. The functional layer may be at least one selected from the group consisting of a hard coating layer, a reflectance reducing layer, an antifouling layer, and an antiglare layer. The functional layer may be coated on at least one surface of the polyamide-based film.

[0166] In the case of the polyamide-based film according to the embodiment, it can be easily applied in the form of a film to the outside of a display device without changing the display driving method, color filter inside the panel, lamination structure, etc., and can provide a display device with excellent scratch resistance, light transmittance, transparency and / or low haze. In addition, since excessive process changes and cost increases are not required, it is possible to reduce production costs.

[0167] Polyamide-based films according to implementations may have excellent optical properties such as high transmittance, low haze, low yellowness, as well as excellent scratch resistance and / or modulus.

[0168] In addition, the polyamide-based film according to the embodiment has an in-plane retardation and a thickness direction retardation below a specific level, thereby minimizing optical distortion and reducing the light leakage phenomenon in which light leaks from the sides.

[0169] In particular, as the screen size of a display device increases or a flexible cover window is required for a flexible / foldable display, excellent mechanical properties such as surface strength are required, and the polyamide-based film according to the embodiment has excellent scratch resistance, modulus and / or optical properties, and can therefore be effectively applied to large-area or foldable / flexible display devices.

[0170] [Method of manufacturing polyamide film] One implementation provides a method for producing a polyamide-based film.

[0171] A method for producing a polyamide-based film according to one embodiment includes the steps of polymerizing a diamine compound and a dicarbonyl compound to prepare a polymer solution containing a polyamide-based polymer in an organic solvent, casting the polymer solution to produce a gel sheet, and heat-treating the gel sheet.

[0172] Referring to FIG. 2, a method for producing a polyamide-based film according to one embodiment includes a step of polymerizing a diamine compound and a dicarbonyl compound in an organic solvent to prepare a polymer solution containing a polyamide-based polymer (S100), a step of casting the polymer solution to produce a gel sheet (S200), and a step of heat-treating the gel sheet (S300).

[0173] The polyamide-based film is a film mainly composed of a polyamide-based polymer, which is a resin containing an amide repeating unit as a structural unit. Optionally, the polyamide-based polymer may contain an imide repeating unit.

[0174] In the method for producing the polyamide-based film, the polymer solution for preparing the polyamide-based polymer may be prepared by simultaneously or sequentially mixing a diamine compound and a dicarbonyl compound in an organic solvent in a reactor and reacting the mixture (S100).

[0175] In one embodiment, the polymer solution can be prepared by simultaneously adding and reacting a diamine compound and a dicarbonyl compound in an organic solvent.

[0176] In another implementation, the step of preparing the polymer solution may include mixing and reacting the diamine compound and the dicarbonyl compound in a solvent to prepare a polyamide (PA) solution, the polyamide solution being a polymer solution having amide repeat units.

[0177] In one embodiment, the step of preparing the polymer solution may be performed using two different dicarbonyl compounds as the dicarbonyl compounds. In this case, the two dicarbonyl compounds may be mixed and reacted simultaneously or sequentially. Preferably, a first dicarbonyl compound may react with the diamine compound to form a prepolymer, and the prepolymer may react with a second dicarbonyl compound to form the polyamide polymer. In this case, a polyamide polymer and a polyamide film may be effectively produced in which the peak of the XRD pattern has the above-mentioned position and half-width, or the peak of a specific section of the IR pattern has the above-mentioned area ratio.

[0178] 3 is a schematic flow chart illustrating the steps of preparing a polyamide-based polymer solution according to some embodiments. Referring to FIG. 3, the dicarbonyl compound may be added in at least four steps (e.g., S120 to S150).

[0179] The step of preparing the polymer solution (S100) may include a step of dissolving a diamine compound in an organic solvent (S110), a step of adding a first dicarbonyl compound and stirring to react (S120), a step of adding a second dicarbonyl compound and stirring to prepare a first polymer solution after step S120 (S130), a step of further adding the first dicarbonyl compound or the second dicarbonyl compound and stirring to prepare a second polymer solution (S140), and a step of further adding the first dicarbonyl compound or the second dicarbonyl compound a second time and stirring to prepare a third polymer solution (S150).

[0180] For example, the general molecular structure and / or molecular weight of the polyamide-based polymer are realized through steps S110 to S130, and the viscosity of the polyamide-based polymer solution is adjusted through steps S140 and S150, and the position and half-width of the peak in the XRD pattern and / or the wave number of 3000 cm of the IR spectrum are adjusted. -1 ~2800cm -1The area ratio of the peaks located in the sections can be precisely adjusted, thereby forming a polyamide-based film having desired optical and mechanical properties.

[0181] In one embodiment, the viscosity of the polymer solution can be adjusted to 200,000 cps to 350,000 cps at room temperature, thereby improving the film formability of the polyamide film, thereby improving the thickness uniformity and / or scratch resistance.

[0182] In some implementations, different dicarbonyl compounds may be used in the step of preparing the second polymer solution (S140) and the step of preparing the third polymer solution (S150). For example, when a first dicarbonyl compound is used in the step of preparing the second polymer solution (S140), a second dicarbonyl compound may be used in the step of preparing the third polymer solution (S150). When a second dicarbonyl compound is used in the step of preparing the second polymer solution (S140), a first dicarbonyl compound may be used in the step of preparing the third polymer solution (S150). Preferably, after the reactant in step S120 reacts with the second dicarbonyl compound, the first dicarbonyl compound is used in step S130 to adjust the XRD and / or IR pattern characteristics of the polyamide-based polymer to the aforementioned range.

[0183] In the steps of preparing the first polymer solution, preparing the second polymer solution, and preparing the third polymer solution, the viscosities of the prepared polymer solutions may be different, for example, the viscosity of the second polymer solution may be higher than that of the first polymer solution, and the viscosity of the third polymer solution may be higher than that of the second polymer solution.

[0184] The stirring speed when preparing the first polymer solution, the stirring speed when preparing the second polymer solution, and the stirring speed when preparing the third polymer solution may be different from each other. For example, the stirring speed when preparing the first polymer solution may be faster than the stirring speed when preparing the second polymer solution and / or the third polymer solution.

[0185] The polymer contained in the polymer solution contains an amide repeating unit derived from the polymerization of the diamine compound and the dicarbonyl compound.

[0186] Alternatively, the polymer contained in the polymer solution may contain imide repeating units derived from the polymerization of the diamine compound and the dianhydride compound, and amide repeating units derived from the polymerization of the diamine compound and the dicarbonyl compound.

[0187] In one embodiment, the step of preparing a polymer solution containing the polyamide-based polymer may be performed at a temperature of −10° C. to 25° C. For example, the mixing and reaction of the solvent, the diamine compound, and the dicarbonyl compound may be performed at a temperature of −10° C. to 25° C. Outside this temperature range, the position and half width of the peak on the XRD pattern may deviate from the aforementioned range.

[0188] In one embodiment, the step of preparing the polymer solution containing the polyamide-based polymer may be performed at a temperature of −20° C. to 25° C. For example, the mixing and reaction of the solvent, the diamine compound, and the dicarbonyl compound may be performed at a temperature of −20° C. to 25° C. Outside this temperature range, the IR spectrum wavenumber of 3000 cm -1 ~2800cm -1 The area ratio of the peaks located in the interval may deviate from the above-mentioned range. Therefore, the properties such as modulus and yellowness of the polyamide-based film may be reduced. In addition, the viscosity of the polymer solution does not reach the predetermined range, so that the variation in thickness of the formed film may increase. Preferably, the step of preparing the polymer solution containing the polyamide-based polymer may be performed under the temperature conditions of -20°C to 20°C, -20°C to 15°C, -20°C to 10°C, -15°C to 20°C, -15°C to 15°C, -15°C to 10°C, -10°C to 20°C, -10°C to 15°C, -10°C to 10°C, -8°C to 20°C, -8°C to 15°C, -8°C to 10°C, -5°C to 20°C, -5°C to 15°C, or -5°C to 10°C.

[0189] The solid content of the polymer solution may be 10% by weight to 30% by weight, but is not limited thereto.

[0190] When the solid content of the polymer solution is within the above range, a polyamide-based film can be effectively produced in the extrusion and casting processes, and the produced polyamide-based film can have improved mechanical properties such as modulus and optical properties such as low yellowness.

[0191] In another embodiment, the step of preparing the polymer solution may further include a step of adjusting the pH of the polymer solution, in which the pH of the polymer solution is adjusted to 4 to 7, for example, 4.5 to 7.

[0192] The pH of the polymer solution is adjusted by adding a pH adjuster, which is not particularly limited and may include, for example, an amine-based compound such as an alkoxyamine, an alkylamine, or an alkanolamine.

[0193] By adjusting the pH of the polymer solution within the above range, it is possible to prevent the occurrence of defects in the film produced from the polymer solution and to achieve the desired optical and mechanical properties in terms of yellowness index and modulus.

[0194] The pH adjuster may be added in an amount of 0.1 mol % to 10 mol % based on the total moles of monomers in the polymer solution.

[0195] In some implementations, the molar ratio of the first dicarbonyl compound to the second dicarbonyl compound used to prepare the polymer solution may be 10:90 to 90:10. Preferably, it may be 25:75 to 80:20, 40:60 to 80:20, or 50:50 to 75:25. For example, when the first dicarbonyl compound and the second dicarbonyl compound are charged in four or more stages, the molar ratio may be determined based on the total number of moles of the first and second dicarbonyl compounds charged in each stage.

[0196] In some implementations, the molar ratio of the first dicarbonyl compound to the second dicarbonyl compound used to prepare the polymer solution may be 10:90 to 79:21. Preferably, it may be 30:70 to 79:21, 40:60 to 79:21, or 50:50 to 75:25. For example, when the first dicarbonyl compound and the second dicarbonyl compound are charged in four or more stages, the molar ratio may be determined based on the total number of moles of the first and second dicarbonyl compounds charged in each stage.

[0197] In some implementations, the content of the first dicarbonyl compound or the second dicarbonyl compound added in the step of preparing the second polymer solution (S140) may be 0.5 mol% to 15 mol% based on the total number of moles of the dicarbonyl compounds. In this case, the position and half width of the peak on the XRD pattern and / or the area ratio of the peak on the IR pattern of the polyamide-based polymer may be precisely adjusted to a desired range. Preferably, the amount of the dicarbonyl compound added in the step of preparing the second polymer solution (S140) may be 0.5 mol% to 10 mol%, 0.5 mol% to 5 mol%, 1 mol% to 3 mol%, or 0.5 mol% to 3 mol%.

[0198] In some implementations, the content of the first dicarbonyl compound or the second dicarbonyl compound added in the step of preparing the third polymer solution (S150) may be 0.5 mol% to 15 mol% based on the total number of moles of the dicarbonyl compounds. In this case, the position and half width of the peak on the XRD pattern and / or the area ratio of the peak on the IR pattern of the polyamide-based polymer may be precisely adjusted to a desired range. Preferably, the amount of the dicarbonyl compound added in the step of preparing the third polymer solution (S150) may be 0.5 mol% to 10 mol%, 0.5 mol% to 5 mol%, 1 mol% to 3 mol%, or 0.5 mol% to 3 mol%.

[0199] By using the first dicarbonyl compound and the second dicarbonyl compound in such a ratio, it is possible to produce a polyamide-based polymer and film having the above-mentioned characteristics in the XRD pattern and / or IR spectrum, and the scratch resistance, modulus, haze, transmittance, yellowness index, etc. of the polyamide-based film can be improved.

[0200] Outside the above ranges, optical properties such as brightness and haze, and mechanical properties such as scratch resistance and modulus may decrease.

[0201] The diamine compound and the dicarbonyl compound are as described above.

[0202] In one embodiment, the organic solvent may be one or more selected from the group consisting of dimethylformamide (DMF), dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), m-cresol, tetrahydrofuran (THF), and chloroform. The organic solvent used in the polymer solution may be, but is not limited to, dimethylacetamide (DMAc).

[0203] The polymer solution may be stored at -20°C to 20°C, -20°C to 10°C, -20°C to 5°C, -20°C to 0°C, or 0°C to 10°C.

[0204] Storage at this temperature can prevent deterioration of the polymer solution and reduce the moisture content, thereby preventing defects in the produced film.

[0205] In one embodiment, the polyamide-based polymer solution may be degassed, which can remove water and reduce impurities in the polymer solution, thereby increasing the reaction yield and achieving a final film with excellent surface appearance and mechanical properties.

[0206] The degassing may include vacuum degassing or inert gas purging. The vacuum degassing may be carried out for 30 minutes to 3 hours after reducing the pressure of the reactor containing the polymer solution to 0.1 bar to 0.7 bar. By carrying out the vacuum degassing under such conditions, it is possible to reduce the number of bubbles in the polymer solution, and as a result, it is possible to prevent surface defects in the film produced therefrom and realize excellent optical properties such as haze.

[0207] Specifically, the purging can be performed by a method of purging the tank with an internal pressure of 1 to 2 atmospheres using an inert gas. By performing the purging under such conditions, the water content in the polymer solution can be removed and impurities can be reduced, thereby increasing the reaction yield and achieving excellent optical properties such as haze and mechanical properties.

[0208] The inert gas may be one or more selected from the group consisting of nitrogen, helium (He), neon (Ne), argon (Ar), krypton (Kr), xenon (Xe), and radon (Rn), but is not limited thereto. Specifically, the inert gas may be nitrogen.

[0209] The vacuum degassing and the inert gas purging may be performed in separate steps. For example, a vacuum degassing step may be performed, followed by a purging step with an inert gas, but this is not limiting.

[0210] By carrying out the vacuum degassing and / or the inert gas purging, the physical properties of the surface of the produced polyamide-based film can be improved.

[0211] As described above, a polymer solution containing a polyamide-based polymer may be prepared in an organic solvent, and then a filler may be added to the solution.

[0212] The filler has an average particle size of 60 nm to 180 nm, a refractive index of 1.55 to 1.75, and a content of 100 ppm to 3000 ppm based on the total weight of the polyamide polymer solid content. The filler may be silica or barium sulfate. The filler has been described in more detail above.

[0213] The polymer solution may be cast to produce a gel sheet (S200). For example, the polymer solution may be extruded, coated and / or dried onto a substrate to form a gel sheet.

[0214] In addition, the casting thickness of the polymer solution may be 200 μm to 700 μm. By casting the polymer solution in this thickness range, it is possible to ensure an appropriate thickness and thickness uniformity when the polymer solution is manufactured into a final film through drying and heat treatment.

[0215] The viscosity of the polymer solution may be 200,000 cps to 350,000 cps at room temperature as described above. By satisfying this viscosity range, the polymer solution can be cast to a uniform thickness without defects, and a polyamide film of substantially uniform thickness can be formed without local / partial thickness changes during the drying process.

[0216] After casting the polymer solution, a gel sheet can be produced by drying for 5 to 60 minutes at a temperature of 60° C. to 150° C. Specifically, a gel sheet can be produced by drying the polymer solution for 15 to 40 minutes at a temperature of 70° C. to 90° C.

[0217] During the drying, the solvent of the polymer solution may be partially or completely evaporated to produce the gel sheet.

[0218] The dried gel sheet may be heat treated to form a polyamide-based film (S300).

[0219] The heat treatment of the gel sheet can be carried out, for example, by a heat curing device. The heat curing device can heat treat the gel sheet with hot air.

[0220] When heat treatment is performed with hot air, the heat can be applied evenly. If the heat is not distributed evenly, a satisfactory surface roughness cannot be achieved, and the surface tension may increase or decrease too much.

[0221] The heat treatment of the gel sheet may be performed for 5 to 200 minutes at a temperature range of 60° C. to 500° C. Specifically, the heat treatment of the gel sheet may be performed for 10 to 150 minutes at a temperature increase rate of 1.5° C. / min to 20° C. / min at a temperature range of 80° C. to 300° C.

[0222] In this case, the heat treatment of the gel sheet may start at a temperature of 60° C. or more. Specifically, the heat treatment of the gel sheet may start at a temperature of 80° C. to 180° C.

[0223] The maximum temperature during the heat treatment may be 300° C. to 500° C. For example, the maximum temperature during the heat treatment may be 350° C. to 500° C., 380° C. to 500° C., 400° C. to 500° C., 410° C. to 480° C., 410° C. to 470° C., or 410° C. to 450° C.

[0224] According to one implementation, the heat treatment of the gel sheet can be carried out in two or more stages. Specifically, the heat treatment may include a first hot air treatment step performed at a temperature range of 60°C to 120°C for 5 minutes to 30 minutes, and a second hot air treatment step performed at a temperature range of 120°C to 350°C for 10 minutes to 120 minutes.

[0225] By performing the heat treatment under such conditions, the gel sheet is cured to have an appropriate surface hardness and modulus, and the cured film can simultaneously have high light transmittance, low haze, and an appropriate level of gloss.

[0226] According to one embodiment, the heat treatment may include passing the substrate through an IR heater. The heat treatment using the IR heater may be performed at a temperature range of 300° C. or more for 1 to 30 minutes. Specifically, the heat treatment using the IR heater may be performed at a temperature range of 300° C. to 500° C. for 1 to 20 minutes.

[0227] The polyamide-based film produced by the above-mentioned production method can exhibit excellent optical and mechanical properties. Such polyamide-based films can be applied to various applications requiring flexibility, transparency, and a specific level of brightness. For example, the polyamide-based films can be applied to solar cells, displays, semiconductor devices, sensors, etc.

[0228] In particular, the polyamide-based film has excellent modulus, scratch resistance and / or optical properties, and is therefore usefully applied to cover windows for display devices and display devices, and has excellent folding properties, and is therefore usefully applied to foldable display devices and flexible display devices.

[0229] The polyamide film produced by the above-mentioned production method is as described above.

[0230] (Example) The above contents will be explained in more detail with reference to the following examples. Note that the following examples are merely illustrative of the present invention, and the scope of the examples is not limited to these examples.

[0231] Example 1 A temperature-controllable double-jacketed 1 L glass reactor was filled with 567 g of dimethylacetamide (DMAc), an organic solvent, under a nitrogen atmosphere at 10°C, and then 64.0 g (0.200 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), an aromatic diamine, was gradually added and dissolved.

[0232] Next, terephthaloyl chloride (TPC) as the first dicarbonyl compound was slowly added in an amount of 48.5 mol% based on the total number of moles of the dicarbonyl compounds used in the polymerization, and the mixture was stirred for 1 hour. After that, isophthaloyl chloride (IPC) as the second dicarbonyl compound was slowly added in an amount of 48.5 mol% based on the total number of moles of the dicarbonyl compounds, and the mixture was stirred for 1 hour to prepare a first polymer solution.

[0233] A 10 wt % solution of TPC and IPC was prepared in DMAc organic solvent.

[0234] The process of adding 1 mL of the TPC solution to the first polymer solution and stirring for 30 minutes was repeated to prepare a second polymer solution by reacting 1.5 mol % of TPC based on the total moles of the dicarbonyl compound.

[0235] The process of adding 1 mL of the IPC solution to the second polymer solution and then stirring for 30 minutes was repeated to react 1.5 mol % of IPC based on the total moles of dicarbonyl compounds to prepare a third polymer solution. At this time, the reaction temperature (temperature during polymerization) of the first, second and third polymer solutions was adjusted to about 10° C., and the reaction was terminated when the viscosity of the third polymer solution reached about 200,000 cps.

[0236] Viscosity was measured using a Toki Sangyo Co., Ltd. BH-II model viscometer while maintaining the temperature of the polymer solution (Varnish) at 10° C. The RPM was set at 4 and a No. 7 spindle was used to confirm that the target viscosity was achieved.

[0237] The third polymer solution was applied to a glass plate and dried. The dried polyamide polymer was peeled off from the glass plate and then heat-treated to obtain a polyamide film having a thickness of 50 μm.

[0238] Regarding the contents of the diamine compound (TFMB) and the dicarbonyl compounds (IPC, TPC), the number of moles of the dicarbonyl compounds and the order of addition based on 100 moles of the diamine compound are shown in Table 1 below.

[0239] In the case of a dicarbonyl compound, the step of adding and stirring was carried out in the order (from top to bottom) shown in Table 1 below. For example, in the case of Example 1, after the step of adding and dissolving a diamine compound in an organic solvent, the steps of adding and stirring 48.5 mol % of TPC, adding and stirring 48.5 mol % of IPC, adding and stirring 1.5 mol % of TPC, and adding and stirring 1.5 mol % of IPC were carried out in this order.

[0240] (Examples 2 and 3 and Comparative Examples 1 to 3) As shown in Table 1 below, the film was produced in the same manner as in Example 1, except that the content of each reactant and the order and amount of the dicarbonyl compound were changed.

[0241] [Table 1]

[0242] <Evaluation example> The physical properties of the films prepared in the above examples and comparative examples were measured and evaluated as follows, and the results are shown in Table 2 below.

[0243] (Evaluation example 1: Film thickness measurement) A digital micrometer 547-401 manufactured by Mitutoyo Corporation, Japan was used to measure the thickness at 10 random positions, and the average thickness was used to determine the thickness.

[0244] (Evaluation example 2: Modulus measurement) Using an Instron universal testing machine UTM5566A, the sample was cut at 10 cm or more in the direction perpendicular to the main shrinkage direction and at 10 mm in the main shrinkage direction, and attached to clips spaced 10 cm apart. The sample was then stretched at a rate of 12.5 mm / min until breakage occurred at room temperature to obtain a stress-strain curve. In the stress-strain curve, the slope of the load relative to the initial deformation was taken as the modulus (GPa). The modulus was measured at room temperature (approximately 20°C to 25°C).

[0245] (Evaluation Example 3: Transmittance and Haze Measurement) The light transmittance and haze were measured using a haze meter NDH-5000W manufactured by Nippon Denshoku Industries Co., Ltd., based on the JIS K 7105, JIS K 7136 and JIS K 7161 standards.

[0246] (Evaluation Example 4: Yellowness Measurement) Yellowness index (YI) was measured by a spectrophotometer (UltraScan PRO, Hunter Associates Laboratory) at d65 and 10° according to the ASTM-E313 standard.

[0247] (Evaluation example 5: XRD (X-ray diffraction crystallography) analysis) The polyamide films of the examples and comparative examples were subjected to XRD analysis using Rigaku's Ultima IV under the following analytical conditions: -Scan source: Cu (40kV, 30mA) -Scan range (2θ): 5°~45° -Scan size: 0.02° -Scan speed: 0.24° / sec

[0248] FIG. 4 is an XRD analysis graph (diffractogram) for the polyamide film of Example 2. Referring to FIG. 4, a combined XRD peak 10, which is the combination of two XRD peaks, was observed in the 2θ value range of about 5° to 35°.

[0249] The combined XRD peak 10 was separated into a first XRD peak 11 and a second XRD peak 12, with the first XRD peak 11 being located in a section (first section) with a maximum value of 2θ values ​​of 10° or more and less than 20°, and the second XRD peak 12 being located in a section (second section) with a maximum value of 2θ values ​​of 20° to 25°. The combined XRD peak 10 was separated such that the first XRD peak 11 and the second XRD peak 12 had a Gaussian distribution shape with respect to a baseline 18.

[0250] The start point (14; a point with a 2θ value of about 5°) and the end point (15; a point with a 2θ value of about 35°) of the combined XRD peak 10 are plotted using an exponential function (e.g., y=ae x +b; a and b are constants), and a baseline 18 was set by connecting the XRD pattern in the section excluding the combined XRD peak.

[0251] In the first XRD peak 11 and the second XRD peak 12, the full width at half maximum (FWHM) of the portion having an intensity value greater than the baseline 18 was analyzed by an analysis program.

[0252] Table 2 below shows the percentage of the half width of the first XRD peak 11 to the sum of the half width of the first XRD peak 11 and the half width of the second XRD peak 12.

[0253] (Evaluation Example 6: Scratch Resistance Evaluation) A KIPAE E&T Pencil Hardness Tester and a Mitsubishi Pressure-Proofed Hi-Density Lead Pencil from Japan were used. A pencil with hardness H was placed so that the contact angle with the film was approximately 45°, and a load of 750g was applied while rubbing the film five times over a measurement area of ​​40mm at a speed of 300mm per minute to evaluate the film surface. The film surface was evaluated as "good" when no scratches were observed, and as "poor" when scratches were observed on the film surface.

[0254] [Table 2]

[0255] As can be seen from Table 2, in the case of the Examples in which the half width of the first XRD peak in the XRD graph is 6° or less, it was confirmed that the Examples have superior properties such as modulus, transmittance, haze, and yellowness index compared to the Comparative Examples.

[0256] Meanwhile, in the case of the comparative example in which the half width of the first XRD peak on the XRD graph is more than 6°, it was confirmed that the properties such as yellowness index, modulus, transmittance, and haze were deteriorated.

[0257] Specifically, in the case of Comparative Example 1 in which the IPC was reacted with the diamine compound prior to the TPC, the half width of the first XRD peak was 6.2°, and the haze and yellowness were relatively increased.

[0258] In the case of Comparative Example 2 in which TPC was used in a relatively excessive amount of 95 mol % based on the total moles of the dicarbonyl compound, the half width of the first XRD peak was 6.2°, the yellowness and haze were significantly increased, and the transmittance was decreased.

[0259] In addition, in the case of Comparative Example 3 in which TPC was used in a relatively small amount of 5 mol % based on the total moles of the dicarbonyl compound, the half-width of the first XRD peak was 6.1°, the modulus was decreased, the yellowness index was increased, and in particular, scratches were observed in the scratch resistance evaluation.

[0260] Example 4 A temperature-controllable double-jacketed 1 L glass reactor was filled with 567 g of dimethylacetamide (DMAc), an organic solvent, under a nitrogen atmosphere at 10°C, and then 64.0 g (0.200 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), an aromatic diamine, was gradually added and dissolved.

[0261] Next, terephthaloyl chloride (TPC) as the first dicarbonyl compound was slowly added in an amount of 38.8 mol% based on the total number of moles of the dicarbonyl compounds used in the polymerization, and the mixture was stirred for 1 hour. After that, isophthaloyl chloride (IPC) as the second dicarbonyl compound was slowly added in an amount of 58.2 mol% based on the total number of moles of the dicarbonyl compounds, and the mixture was stirred for 1 hour to prepare a first polymer solution.

[0262] A 10 wt % solution of TPC and IPC was prepared in DMAc organic solvent.

[0263] The process of adding 1 mL of the TPC solution to the first polymer solution and stirring for 30 minutes was repeated to react 1.2 mol % of TPC based on the total moles of the dicarbonyl compound, thereby preparing a second polymer solution.

[0264] The process of adding 1 mL of the IPC solution to the second polymer solution and then stirring for 30 minutes was repeated to react 1.8 mol % of IPC based on the total moles of dicarbonyl compounds to prepare a third polymer solution. At this time, the reaction temperature (temperature during polymerization) of the first, second and third polymer solutions was adjusted to about 10° C., and the reaction was terminated when the viscosity of the third polymer solution reached about 250,000 cps.

[0265] Viscosity was measured using a Toki Sangyo Co., Ltd. BH-II model viscometer while maintaining the temperature of the polymer solution at 10° C. The RPM was set at 4 and a No. 7 spindle was used to check whether the target viscosity was achieved.

[0266] The third polymer solution was applied to a glass plate and dried for 30 minutes with hot air at 100° C. The dried polyamide polymer was peeled off from the glass plate, fixed to a pin frame, and heated at a rate of 2° C. / min in the temperature range of 80° C. to 300° C. to obtain a polyamide film having a thickness of 50 μm.

[0267] Regarding the contents of the diamine compound (TFMB) and the dicarbonyl compounds (IPC, TPC), the number of moles of the dicarbonyl compounds and the order of addition are shown in Table 3 based on 100 moles of the diamine compound.

[0268] In the case of a dicarbonyl compound, the step of adding and stirring was performed in the order (from top to bottom) shown in Table 3. For example, in the case of Example 4, after the step of adding and dissolving a diamine compound in an organic solvent, the steps of adding and stirring 38.8 mol % of TPC, adding and stirring 58.2 mol % of IPC, adding and stirring 1.2 mol % of TPC, and adding and stirring 1.8 mol % of IPC were sequentially performed.

[0269] (Examples 5 to 8 and Comparative Examples 4 to 6) As shown in Table 3 below, films were produced in the same manner as in Example 4, except that the content of each reactant was changed.

[0270] Comparative Example 7 In Example 4, the first polymer solution was prepared by adding 70 mol % of TPC and 30 mol % of IPC based on the total dicarbonyl compounds. The steps of preparing the second polymer solution and the third polymer solution were omitted, and the first polymer solution was applied to a glass plate, dried and heat-treated to produce a polyamide film.

[0271] Comparative Example 8 A polyamide film was produced in the same manner as in Comparative Example 7, except that the first polymer solution was prepared by adding TPC in an amount of 75 mol % based on the total dicarbonyl compounds and IPC in an amount of 25 mol %.

[0272] The films produced in Examples 4 to 8 and Comparative Examples 4 to 6 were measured and evaluated for the above-mentioned physical properties, and further subjected to the following FT-IR analysis.

[0273] (Evaluation Example 7: FT-IR (Fourier-Transform Infrared spectroscopy) analysis) The polyamide films of the examples and comparative examples were subjected to FT-IR analysis using an FT-IR spectrometer manufactured by Thermo Fisher Scientific under the following analytical conditions: -Detector: MIR TGA -Scan range: 4000cm -1 ~650cm -1 -Resolution: 4 -Scan count: 16

[0274] Fig. 5 shows FT-IR analysis spectra for the polyamide films of the examples and comparative examples, and Figs. 6 to 8 show FT-IR analysis spectra for the polyamide films of Example 7, and Comparative Examples 5 and 6, respectively.

[0275] The spectra in Figures 5 to 8 are from 4000 cm -1 ~650cm -1 In the spectrum against wavenumber, the wavenumber is about 3800 cm -1 ~2500cm -1 The section has been expanded.

[0276] The spectra in Figures 6 to 8 are at a wavenumber of approximately 3800 cm -1 ~2500cm -1 The largest IR peak in the section is at wavenumber 1415 cm -1 The IR peak heights were normalized to obtain the spectrum shown in Figure 5.

[0277] 5 to 7, the wave number is about 2960 cm -1 ~2895cm -1 The first IR peak was observed in the range of 2890 cm -1 1~2820cm -1 A second IR peak was observed in the section, and the highest point of the first IR peak was at a wavenumber of approximately 2924.43 cm -1 The maximum of the second IR peak is located at a wavenumber of approximately 2853.72 cm -1 was located at.

[0278] For the first and second IR peaks, the onset of the peaks (2960 cm -1 and 2890 cm -1 ) and the end point (2895 cm -1 and 2820 cm -1 ) was connected with a straight line to set the baseline of the IR peak. The area of ​​each IR peak was calculated by integrating the portion of the IR peak with an intensity value greater than the baseline.

[0279] Then, the ratio of the area of ​​the first IR peak to the area of ​​the second IR peak (area ratio) was calculated and shown in Table 3 below.

[0280] [Table 3]

[0281] Referring to Table 3, it was confirmed that the examples having an area ratio of 1.4 or less had improved modulus, light transmittance, haze, and yellowness compared to the comparative examples.

[0282] For example, in the comparative examples, the ratio of TPC to IPC used in the polymerization was 5:95, 80:20, or 95:5, and the area of ​​the first IR peak in the IR spectrum was 1.5 times or more that of the second IR peak, which resulted in deterioration of the modulus, light transmittance, haze, and / or yellowness.

[0283] In addition, in the case of Comparative Example 7 and Comparative Example 8, the viscosity of the first polymer solution was significantly below 250,000 cps, and it was difficult to produce a polyamide-based film of a grade that could be used as an optical film. The polyamide-based film produced in this way had a significantly non-uniform thickness, and the properties such as modulus, light transmittance, haze, and yellowness index varied greatly in each region on the polyamide-based film, significantly reducing its suitability as a cover window for a display device. [Explanation of symbols]

[0284] 100: Polyamide film 101: 1st page 102:Second side 200: Functional layer 300: Cover window 400: Display section 500: Adhesive layer

Claims

1. Contains a polyamide polymer, Wave number on the IR spectrum: 2950 cm -1 ~2900cm -1 The first IR peak having a maximum value in the range and a wave number of 2875 cm -1 ~2825cm -1 a second IR peak having a maximum value in the interval; A polyamide-based film, wherein the area of ​​the first IR peak is 1.4 times or less the area of ​​the second IR peak.

2. The polyamide film according to claim 1 , wherein the area of ​​the first IR peak is 0.6 times or more as large as the area of ​​the second IR peak.

3. The polyamide film according to claim 1, wherein the area of ​​the first IR peak is 0.8 to 1.2 times the area of ​​the second IR peak.

4. The polyamide film according to claim 1 , wherein the polyamide polymer contains two or more kinds of amide repeating units.

5. the two or more kinds of amide repeating units include a first amide repeating unit derived from a first dicarbonyl compound and a second amide repeating unit derived from a second dicarbonyl compound, the angle between the two carbonyl groups in the first dicarbonyl compound is 160° to 180°; The polyamide-based film according to claim 4, wherein the angle between the two carbonyl groups in the second dicarbonyl compound is 80° to 140°.

6. Based on a film thickness of 50 μm, The modulus is 5 GPa or more, Transmittance is 80% or more, Haze is less than 1%. The polyamide film according to claim 1 , having a yellowness index of 3.5 or less.

7. A cover window for a display device, comprising the polyamide film according to claim 1 and a functional layer.

8. A display unit; a cover window disposed on the display portion, A display device, wherein the cover window comprises the polyamide-based film according to claim 1 and a functional layer.

9. A step of polymerizing a diamine compound and a dicarbonyl compound in an organic solvent to prepare a polymer solution containing a polyamide-based polymer; Casting the polymer solution to prepare a gel sheet; and heat-treating the gel sheet.

10. the dicarbonyl compound includes a first dicarbonyl compound and a second dicarbonyl compound having a smaller angle between two carbonyl groups than that of the first dicarbonyl compound; The step of preparing a polymer solution containing a polyamide-based polymer includes: adding and dissolving a diamine compound in an organic solvent; preparing a first polymer solution by adding and stirring a first dicarbonyl compound, and then adding and stirring a second dicarbonyl compound; preparing a second polymer solution by adding and stirring a first dicarbonyl compound or a second dicarbonyl compound; and (b) adding and stirring the first dicarbonyl compound or the second dicarbonyl compound to prepare a third polymer solution.

11. The method for producing a polyamide film according to claim 10, wherein the first dicarbonyl compound is added in the step of preparing the second polymer solution, and the second dicarbonyl compound is added in the step of preparing the third polymer solution.

12. The content of the first dicarbonyl compound or the second dicarbonyl compound added in the step of preparing the second polymer solution is 0.5 mol % to 15 mol % based on the total moles of the dicarbonyl compounds; The method for producing a polyamide film according to claim 10, wherein the content of the first dicarbonyl compound or the second dicarbonyl compound added in the step of preparing the third polymer solution is 0.5 mol % to 15 mol % based on the total moles of the dicarbonyl compounds.

Citation Information

Patent Citations

  • Aromatic polyamide film and laminate

    JP2015120886A

  • Polyamide solution

    JP2016098260A

  • Film, method for producing film and laminate

    JP2016108482A

  • Aromatic Polyamide Solution for the Production of Display Elements, Optical Elements or Lighting Elements

    JP2016500128A

  • Polyamide-imide film and method for producing the same

    JP2020505486A