Reflection type mask blank for EUV lithography, and substrate with conductive film

The EUV mask blank's conductive film, optimized for specific refractive and extinction coefficients, addresses inspection and deformation issues, ensuring effective defect detection and strong fixing force, thereby improving EUV mask blank performance.

JP2024167411AActive Publication Date: 2024-12-03AGC INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024155171
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-17
Filing Date
2024-09-09
Publication Date
2024-12-03
Estimated Expiration
2044-03-07

AI Technical Summary

Technical Problem

EUV mask blanks face challenges with conductive films that hinder defect inspection using Ar lasers due to high light transmittance in the 488 nm wavelength range and insufficient fixing force during exposure, while also experiencing deformation from internal stress in multilayer reflective and absorption layers.

Method used

A conductive film for EUV mask blanks is formulated with specific refractive indices and extinction coefficients for different wavelength ranges, allowing high transmittance in 1000 to 1100 nm and 600 to 700 nm, low transmittance in 400 to 500 nm, and low resistivity to ensure strong fixing force, composed of nitrogen (N) and boron (B), with optional inclusion of tantalum (Ta) and chromium (Cr), and a thickness of 20 to 350 nm.

Benefits of technology

The conductive film enables effective defect inspection with Ar lasers, suppresses deformation from internal stress, and provides excellent fixing strength during exposure, enhancing the performance of EUV mask blanks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167411000003
    Figure 2024167411000003
  • Figure 2024167411000001
    Figure 2024167411000001
  • Figure 2024167411000002
    Figure 2024167411000002
Patent Text Reader

Abstract

To provide an EUV mask blank that transmits light in the range of 1000 to 1100 nm and 600 to 700 nm when light is incident from the conductive film side, and suppresses the transmission of light in the range of 400 to 500 nm, and has excellent fixing force when fixed to an exposure device.SOLUTION: There is provided a reflection type mask blank for EUV lithography that has a substrate, a conductive film arranged on a rear side of the substrate, a reflective layer arranged on a front side of the substrate, and an absorption layer arranged on the reflective layer, wherein the conductive film contains at least one of nitrogen (N) and boron (B), the total content of N and B contained in the conductive film is more than 0 at% and 65 at% or less, and a refractive index and an extinction coefficient in the wavelengths of 1000 to 1100 nm, 600 to 700 nm, and 400 to 500 nm of the conductive film, as well as the thickness t and resistivity of the conductive film are within a specific range.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective mask blank for EUV (Extreme Ultra Violet) lithography (hereinafter referred to as "EUV mask blank" in this specification) used in semiconductor manufacturing and the like, and a substrate with a conductive film used in the manufacture of the EUV mask blank. [Background technology]

[0002] Conventionally, in the semiconductor industry, photolithography using visible light or ultraviolet light has been used as a transfer technology of fine patterns necessary for forming integrated circuits consisting of fine patterns on Si substrates and the like. However, while the miniaturization of semiconductor devices is accelerating, the limit of conventional photolithography is approaching. In the case of photolithography, the resolution limit of the pattern is about 1 / 2 of the exposure wavelength. Even if the immersion method is used, it is said to be about 1 / 4 of the exposure wavelength, and even if the immersion method of ArF laser (193 nm) is used, the limit is expected to be about 20 to 30 nm. Therefore, EUV lithography, an exposure technology using EUV light with an even shorter wavelength than ArF laser, is seen as promising as an exposure technology for 20 to 30 nm and beyond. In this specification, EUV light refers to light rays with a wavelength in the soft X-ray region or vacuum ultraviolet region. Specifically, it refers to light rays with a wavelength of about 10 to 20 nm, especially about 13.5 nm ± 0.3 nm.

[0003] EUV light is easily absorbed by all materials, and at this wavelength the refractive index of materials is close to 1. This means that refractive optics, as in conventional photolithography using visible or ultraviolet light, cannot be used, and so EUV lithography uses reflective optics, i.e., reflective photomasks and mirrors.

[0004] On the other hand, apart from shortening the wavelength of light, a resolution improvement technique using a phase shift mask has been proposed. A phase shift mask gives a phase difference of 180 degrees to the light transmitted through the transparent parts of a mask pattern by making the transparent parts of the mask pattern different in material or shape from the adjacent transparent parts. Therefore, in the region between the two transparent parts, the transmitted diffracted lights with a phase difference of 180 degrees cancel each other out, making the light intensity extremely small, improving the mask contrast, and as a result, the focal depth during transfer is expanded and the transfer accuracy is improved. In principle, a phase difference of 180 degrees is optimal, but a phase difference of about 175 to 185 degrees is sufficient to improve the resolution.

[0005] A mask blank is a pre-patterned laminate used in photomask manufacturing. An EUV mask blank has a structure in which a reflective layer that reflects EUV light and an absorbing layer that absorbs EUV light are formed in that order on a substrate made of glass or the like.

[0006] As the reflective layer, a multilayer reflective film is usually used, which is made by alternately laminating low refractive index layers that have a low refractive index to EUV light and high refractive index layers that have a high refractive index to EUV light, thereby increasing the light reflectance when the layer surface is irradiated with EUV light. As the low refractive index layer of the multilayer reflective film, a molybdenum (Mo) layer is usually used, and as the high refractive index layer, a silicon (Si) layer is usually used.

[0007] The absorption layer is made of a material having a high absorption coefficient for EUV light, specifically, for example, a material containing chromium (Cr) or tantalum (Ta) as a main component.

[0008] The multilayer reflective film and the absorbing layer are deposited on the optical surface of the glass substrate by ion beam sputtering or magnetron sputtering. When the multilayer reflective film and the absorbing layer are deposited, the glass substrate is held by a supporting means. The supporting means for the glass substrate includes a mechanical chuck and an electrostatic chuck, but an electrostatic chuck is preferably used due to the problem of dust generation. An electrostatic chuck is also used as a supporting means for the glass substrate during the mask patterning process or during mask handling during exposure.

[0009] Electrostatic chucks are a technology that has been used conventionally as a means of supporting silicon (Si) wafers in the manufacturing process of semiconductor devices. For this reason, in the case of substrates with low dielectric constants and electrical conductivity, such as glass substrates, a high voltage must be applied to obtain the same level of chucking force as that of Si wafers, which creates the risk of dielectric breakdown.

[0010] Therefore, in order to facilitate electrostatic chucking of the substrate, a conductive film is formed on the opposite side of the substrate from the multilayer reflective film.

[0011] In EUV masks and EUV mask blanks used therewith, deformation of the substrate caused by internal stress in the multilayer reflective film as a reflective layer or in the absorption layer can be problematic. A new technology is being introduced that improves substrate deformation caused by internal stress in the multilayer reflective film or absorption layer by locally irradiating a pulsed laser beam from the back side of the EUV mask or EUV mask blank to locally heat the glass substrate.

[0012] In order to apply the above technology, Patent Document 1 provides an EUV mask blank having a conductive film formed on the rear surface thereof, which has high transmittance for light having a wavelength of 400 to 800 nm. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] Japanese Patent Application Publication No. 2015-15420 Summary of the Invention [Problem to be solved by the invention]

[0014] On the other hand, an Ar laser with a wavelength of 488 nm is used for defect inspection after the conductive film is formed. If the conductive film has a high light transmittance in this wavelength range, defect inspection cannot be performed. Therefore, the conductive film is required to have a low light transmittance in this wavelength range.

[0015] When using an Ar laser with a wavelength of 488 nm for defect inspection after the formation of a conductive film, a Nd:YAG laser with a wavelength of 1064 nm or a He:Ne laser with a wavelength of 632 nm can be used to improve the deformation of the substrate caused by internal stress in the multilayer reflective film or absorption layer by locally irradiating the laser light. When using these lasers, the conductive film is required to have high light transmittance in these wavelength ranges.

[0016] In addition, the EUV mask blank is applied to an exposure tool after forming a pattern on the absorbing layer. At this time, the EUV mask blank on which the conductive film is formed may not be fixed to the exposure tool with sufficient fixing force. In order to prevent such insufficient fixing force, it is effective to reduce the resistivity of the conductive film.

[0017] In order to solve the above-mentioned problems of the conventional techniques, an object of the present invention is to provide an EUV mask blank which, when incident from the conductive film side, sufficiently transmits light in the wavelength range of 1000 to 1100 nm and light in the wavelength range of 600 to 700 nm and suppresses transmission of light in the wavelength range of 400 to 500 nm, and has excellent fixing strength when fixed to an exposure tool, and to provide a substrate with a conductive film for use in manufacturing the EUV mask blank. [Means for solving the problem]

[0018] The present inventors have found that the above problems can be solved by the following configuration. (1) a substrate; A conductive film disposed on the back side of the substrate; a reflective layer disposed on the front surface side of the substrate and reflecting EUV light; A reflective mask blank for EUV lithography having an absorption layer disposed on the reflective layer and absorbing EUV light, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B contained in the conductive film is more than 0 at% and 65 at% or less, The refractive index n of the conductive film at wavelengths of 1000 to 1100 nm λ1000-1100nmis 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, The refractive index n of the conductive film at wavelengths of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is less than or equal to 4.500, The refractive index n of the conductive film at wavelengths of 400 to 500 nm λ400-500nm is 2.500 or more, and the extinction coefficient k λ400-500nm is 0.440 or more, The thickness t of the conductive film is 20 to 350 nm, A reflective mask blank for EUV lithography with a conductive film resistivity of 3.5 mΩ·cm or less. (2) a substrate; A conductive film disposed on the back side of the substrate; a reflective layer disposed on the front surface side of the substrate and reflecting EUV light; A reflective mask blank for EUV lithography having an absorption layer disposed on the reflective layer and absorbing EUV light, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B in the conductive film is more than 0 at% and 65 at% or less, The refractive index n of the conductive film at wavelengths of 1000 to 1100 nm λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, Refractive index n of the conductive film at wavelengths of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is less than or equal to 4.500, The refractive index n of the conductive film at wavelengths of 480 to 500 nm λ480-500nm is 2.500 or more, and the extinction coefficient k λ480-500nm is 0.440 or more, The thickness t of the conductive film is 20 to 350 nm, A reflective mask blank for EUV lithography with a conductive film resistivity of 3.5 mΩ·cm or less. (3) A reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film contains at least one of tantalum (Ta) and chromium (Cr). (4) A reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film contains Ta and N. (5) A reflective mask blank for EUV lithography according to (4), wherein the conductive film contains N in an amount of more than 0 at % and not more than 65 at %. (6) A reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film contains Ta and B. (7) A reflective mask blank for EUV lithography according to (6), wherein the conductive film contains B in an amount of more than 0 at % and 35 at % or less. (8) A reflective mask blank for EUV lithography according to (1) or (2), wherein the resistivity of the conductive film is not less than 0.050 mΩ·cm and not more than 3.5 mΩ·cm. (9) The reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film contains Ta, and the half-width (FWHM) of a diffraction peak attributable to a bcc (110) plane of Ta, among diffraction peaks originating from the conductive film observed by an out of plane XRD method, is 1.5 to 4.0°. (10) The reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film has a light transmittance of 1.0% or more at a wavelength of 1000 to 1100 nm, a light transmittance of 1.0% or more at a wavelength of 600 to 700 nm, and a light transmittance of 1.0% or less at a wavelength of 400 to 500 nm. (11) A reflective mask blank for EUV lithography according to (1) or (2), wherein the sheet resistance of the conductive film is 250 Ω / □ or less. (12) A reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film has a surface hardness of 10.0 GPa or more. (13) an upper layer is provided on the conductive film; The reflective mask blank for EUV lithography according to (1) or (2), wherein the upper layer contains chromium (Cr) and at least one element selected from the group consisting of nitrogen (N) and oxygen (O). (14) The reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film has a surface roughness (Rq) of 0.600 nm or less. (15) A substrate having a conductive film thereon, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B contained in the conductive film is more than 0 at% and 65 at% or less, The refractive index n of the conductive film at a wavelength of 1000 to 1100 nm λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, The refractive index n of the conductive film at a wavelength of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is less than or equal to 4.500, The refractive index n of the conductive film at a wavelength of 400 to 500 nm λ400-500nm is 2.500 or more, and the extinction coefficient k λ400-500nm is 0.440 or more, The conductive film has a thickness t of 20 to 350 nm, A substrate with a conductive film, the resistivity of which is 3.5 mΩ·cm or less. (16) A substrate having a conductive film thereon, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B contained in the conductive film is more than 0 at% and 65 at% or less, The refractive index n of the conductive film at a wavelength of 1000 to 1100 nm λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, The refractive index n of the conductive film at a wavelength of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nmis less than or equal to 4.500, The refractive index n of the conductive film at a wavelength of 480 to 500 nm λ480-500nm is 2.500 or more, and the extinction coefficient k λ480-500nm is 0.440 or more, The conductive film has a thickness t of 20 to 350 nm, A substrate with a conductive film, the resistivity of which is 3.5 mΩ·cm or less. (17) The substrate with a conductive film according to (15) or (16), wherein the conductive film contains at least one of tantalum (Ta) and chromium (Cr). (18) The substrate with a conductive film according to (15) or (16), wherein the conductive film contains Ta and N. (19) The substrate with a conductive film according to (18), wherein the conductive film contains N in an amount of more than 0 at % and not more than 65 at %. (20) The substrate with a conductive film according to (15) or (16), wherein the conductive film contains Ta and B. (21) The substrate with a conductive film according to (20), wherein the conductive film contains B in an amount of more than 0 at % and 35 at % or less. (22) The substrate with a conductive film according to (15) or (16), wherein the conductive film has a resistivity of 0.050 mΩ·cm or more and 3.5 mΩ·cm or less. (23) The substrate with a conductive film according to (15) or (16), wherein the conductive film contains Ta, and among the diffraction peaks originating from the conductive film observed by an out of plane XRD method, the full width at half maximum (FWHM) of a diffraction peak assigned to a bcc (110) plane of Ta is 1.5 to 4.0°. (24) The substrate with a conductive film according to (15) or (16), wherein the conductive film has a light transmittance of 1.0% or more at a wavelength of 1000 to 1100 nm, a light transmittance of 1.0% or more at a wavelength of 600 to 700 nm, and a light transmittance of 1.0% or less at a wavelength of 400 to 500 nm. (25) The substrate with a conductive film according to (15) or (16), wherein the conductive film has a sheet resistance of 250 Ω / □ or less. (26) The substrate with a conductive film according to (15) or (16), wherein the conductive film has a surface hardness of 10.0 GPa or more. (27) An upper layer is further provided on the conductive film, The substrate with a conductive film according to (15) or (16), wherein the upper layer contains chromium (Cr) and at least one element selected from the group consisting of nitrogen (N) and oxygen (O). (28) The substrate with a conductive film according to (15) or (16), wherein the conductive film has a surface roughness (Rq) of 0.600 nm or less. Effect of the Invention

[0019] The EUV mask blank of the embodiment of the present invention (hereinafter also referred to as the EUV mask blank of the present embodiment) transmits light having a wavelength of 1000 to 1100 nm and light having a wavelength of 600 to 700 nm, and suppresses the transmission of light having a wavelength of 400 to 500 nm, when the light is incident from the conductive film side. In addition, since the resistivity of the conductive film is sufficiently low, excellent fixing force can be obtained when the mask blank is fixed to an exposure device. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of an EUV mask blank of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] A first aspect of the EUV mask blank of the present embodiment is a reflective mask blank for EUV lithography, comprising a substrate, a conductive film disposed on a rear surface side of the substrate, a reflective layer disposed on a front surface side of the substrate and reflecting EUV light, and an absorbing layer disposed on the reflective layer and absorbing EUV light, wherein the conductive film contains at least one of nitrogen (N) and boron (B), the total content of N and B contained in the conductive film is more than 0 at % and 65 at % or less, and the refractive index n λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is 5.200 or less, and the refractive index n λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nmis 4.500 or less, and the refractive index n λ400-500nm is 2.500 or more, and the extinction coefficient k λ400-500nm is 0.440 or more, the thickness t of the conductive film is 20 to 350 nm, and the resistivity of the conductive film is 3.5 mΩ·cm or less.

[0022] A second aspect of an EUV mask blank according to an embodiment of the present invention is a reflective mask blank for EUV lithography, comprising a substrate, a conductive film disposed on a rear surface side of the substrate, a reflective layer disposed on a front surface side of the substrate and reflecting EUV light, and an absorbing layer disposed on the reflective layer and absorbing EUV light, wherein the conductive film contains at least one of nitrogen (N) and boron (B), the total content of N and B contained in the conductive film is greater than 0 at % and is 65 at % or less, and the refractive index n λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is 5.200 or less, and the refractive index n λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is 4.500 or less, and the refractive index n λ480-500nm is 2.500 or more, and the extinction coefficient k λ480-500nm is 0.440 or more, the thickness t of the conductive film is 20 to 350 nm, and the resistivity of the conductive film is 3.5 mΩ·cm or less.

[0023] The EUV mask blank of this embodiment will be described below with reference to the drawings. Note that the following description of the EUV mask blank of this embodiment applies to both the first and second aspects of the EUV mask blank of this embodiment unless otherwise specified.

[0024] Fig. 1 is a schematic cross-sectional view showing one embodiment of an EUV mask blank of the present invention. In an EUV mask blank 10 shown in Fig. 1, a reflective layer 13 that reflects EUV light and an absorbing layer 14 that absorbs EUV light are formed in this order on one surface of a substrate 11 (the upper surface of the substrate 11 in the figure). A conductive film 12 is formed on the other surface of the substrate 11 (the lower surface of the substrate 11 in the figure). Hereinafter, in this specification, the surface of the substrate 11 on which the reflective layer 13 and the absorbing layer 14 are arranged is referred to as the front surface of the substrate 11, and the surface of the substrate 11 on which the conductive film 12 is arranged is referred to as the back surface of the substrate 11.

[0025] Hereinafter, the individual components of the EUV mask blank 10 of this embodiment will be described.

[0026] The substrate 11 satisfies the characteristics required for an EUV mask blank. Therefore, the substrate 11 has a low thermal expansion coefficient and is excellent in smoothness, flatness, and resistance to cleaning solutions used for cleaning the mask blank or the photomask after pattern formation. Here, the low thermal expansion coefficient is specifically a thermal expansion coefficient at 20° C. of 0±0.05×10 -7 / ℃ is preferred, 0±0.03×10 -7 / ° C. is more preferable. As the substrate 11, specifically, glass having a low thermal expansion coefficient, such as SiO2-TiO2 glass, is used, but the present invention is not limited thereto, and substrates such as crystallized glass in which a β-quartz solid solution is precipitated, quartz glass, silicon, and metal can also be used.

[0027] It is preferable that the substrate 11 has a smooth surface with a surface roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less, because this allows high reflectance and transfer accuracy to be obtained in the photomask after pattern formation.

[0028] The size and thickness of the substrate 11 are appropriately determined based on the design values ​​of the mask, etc. In the embodiment shown later, SiO2-TiO2 glass having an outer shape of 6 inches (152 mm) square and a thickness of 0.25 inches (6.3 mm) was used.

[0029] It is preferable that there are no defects on the surface of the substrate 11. However, even if defects are present, it is acceptable as long as no topological defects are caused by concave and / or convex defects. Specifically, it is preferable that the depth of the concave defect and the height of the convex defect are 2 nm or less, and the half-width of these concave and convex defects are 60 nm or less. The half-width of a concave defect refers to the width at a position half the depth of the concave defect. The half-width of a convex defect refers to the width at a position half the height of the convex defect.

[0030] The conductive film 12 has a refractive index n λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than 5.200.

[0031] Refractive index n λ1000-1100nm and the extinction coefficient k λ1000-1100nm When the thickness is within the above range, the conductive film 12 has a high transmittance for light having a wavelength of 1000 to 1100 nm, which is preferable when using an Nd:YAG laser having a wavelength of 1064 nm to improve deformation of the substrate.

[0032] The transmittance of the conductive film 12 for light having a wavelength of 1000 to 1100 nm is preferably 1.0% or more, more preferably 2.0% or more, and even more preferably 2.5% or more. The upper limit of the transmittance of the conductive film 12 for light having a wavelength of 1000 to 1100 nm is not particularly limited, but is, for example, 3.5% or less.

[0033] The refractive index n of the conductive film 12 λ1000-1100nm The refractive index n of the conductive film 12 is preferably 5.200 or less. λ1000-1100nm The lower limit is not particularly limited, but is, for example, 4,000 or more.

[0034] The extinction coefficient k of the conductive film 12 λ1000-1100nm The extinction coefficient k of the conductive film 12 is preferably 5.100 or less. λ1000-1100nm The lower limit is not particularly limited, but is, for example, 3,000 or more.

[0035] The conductive film 12 has a refractive index n λ600-700nm is 4.300 or less, and the extinction coefficient kλ600-700nm is less than 4.500.

[0036] Refractive index n λ600-700nm and the extinction coefficient k λ600-700nm When is in the above range, the conductive film 12 has high transmittance for light having a wavelength of 600 to 700 nm, which is preferable when a He:Ne laser having a wavelength of 632 nm is used to improve deformation of the substrate.

[0037] The transmittance of the conductive film 12 for light having a wavelength of 600 to 700 nm is preferably 1.0% or more, and more preferably 1.5% or more. The upper limit of the transmittance of the conductive film 12 for light having a wavelength of 600 to 700 nm is not particularly limited, but is, for example, 2.5% or less.

[0038] The refractive index n of the conductive film 12 λ600-700nm The refractive index n of the conductive film 12 is preferably 4.200 or less. λ600-700nm The lower limit of is not particularly limited, but is, for example, 3,100 or more.

[0039] The extinction coefficient k of the conductive film 12 λ600-700nm The extinction coefficient k of the conductive film 12 is preferably 4.400 or less. λ600-700nm There is no particular upper limit to the value, but it is, for example, 2,500 or more.

[0040] In a first aspect of the EUV mask blank of this embodiment, the conductive film 12 has a refractive index n λ400-500nm is 2.500 or more, and the extinction coefficient k λ400-500nm is 0.440 or more. In a second aspect of the EUV mask blank of this embodiment, the conductive film 12 has a refractive index n λ400-500nm is preferably 2.500 or more, and the extinction coefficient k λ400-500nm is preferably 0.440 or more.

[0041] Refractive index n λ400-500nm and the extinction coefficient k λ400-500nmWhen the thickness is within the above range, the conductive film 12 has a low transmittance for light having a wavelength of 400 to 500 nm, which is preferable when an Ar laser having a wavelength of 488 nm is used for defect inspection.

[0042] The transmittance of the conductive film 12 for light having a wavelength of 400 to 500 nm is preferably 1.0% or less, and more preferably less than 1.0%. The lower limit of the transmittance of the conductive film 12 for light having a wavelength of 400 to 500 nm is not particularly limited, but is, for example, 0.7% or more.

[0043] The refractive index n of the conductive film 12 λ400-500nm is preferably 2.600 or more, more preferably 2.650 or more, and even more preferably 2.700 or more. λ400-500nm There is no particular upper limit to the value, but it is, for example, 3,300 or less.

[0044] The extinction coefficient k of the conductive film 12 λ400-500nm is preferably 0.500 or more, more preferably 1.000 or more, further preferably 1.500 or more, and particularly preferably 1.800 or more. λ400-500nm There is no particular upper limit to the value, but it is, for example, 4,300 or less.

[0045] In a first aspect of the EUV mask blank of this embodiment, the conductive film 12 has a refractive index n λ480-500nm is preferably 2.500 or more, and the extinction coefficient k λ480-500nm is preferably 0.440 or more. In a second aspect of the EUV mask blank of this embodiment, the conductive film 12 has a refractive index n λ480-500nm is 2.500 or more, and the extinction coefficient k λ480-500nm is 0.440 or more.

[0046] The refractive index n of the conductive film 12 λ480-500nm is preferably 2.600 or more, more preferably 2.700 or more, and even more preferably 2.800 or more. λ480-500nm There is no particular upper limit to the value, but it is, for example, 3,300 or less.

[0047] The extinction coefficient k of the conductive film 12 λ480-500nm is preferably 0.500 or more, more preferably 1.000 or more, even more preferably 1.500 or more, particularly preferably 2.000 or more, and most preferably 2.200 or more. λ480-500nm There is no particular upper limit to the value, but it is, for example, 4,300 or less.

[0048] The conductive film 12 has a film thickness t of 20 to 350 nm. When the film thickness t is 20 nm or more, the transmittance of light having a wavelength of 400 to 500 nm can be sufficiently reduced. If the film thickness t exceeds 350 nm, the refractive index n λ1000-1100nm and the extinction coefficient k λ1000-1100nm Even if the refractive index n satisfies the above range, the light transmittance at wavelengths of 1000 to 1100 nm is not sufficiently high. λ600-700nm and the extinction coefficient k λ600-700nm Even if the above range is satisfied, the transmittance of light having a wavelength of 600 to 700 nm is not sufficiently high.

[0049] The thickness t of the conductive film 12 is preferably 20 nm or more, more preferably 25 nm or more, and even more preferably 30 nm or more. The thickness t of the conductive film 12 is preferably 300 nm or less, more preferably 200 nm or less, and even more preferably 100 nm or less.

[0050] Refractive index n λ1000-1100nm , refractive index n λ600-700nm and the refractive index n λ400-500nm satisfies the above range and the extinction coefficient k λ1000-1100nm , the extinction coefficient k λ600-700nm and the extinction coefficient k λ400-500nm The conductive film 12 that satisfies the above range contains at least one of nitrogen (N) and boron (B). Also, the refractive index n λ1000-1100nm , refractive index n λ600-700nm and the refractive index n λ480-500nm satisfies the above range and the extinction coefficient k λ1000-1100nm , the extinction coefficient k λ600-700nm and the extinction coefficient k λ480-500nmThe conductive film 12 that satisfies the above range contains at least one of nitrogen (N) and boron (B).

[0051] The conductive film 12 contains at least one of nitrogen (N) and boron (B). That is, the total content of N and B contained in the conductive film 12 exceeds 0 at%. This allows the conductive film 12 to be made amorphous. The total content of N and B is preferably 2 at% or more, more preferably 5 at% or more, and even more preferably 10 at% or more.

[0052] From the viewpoint of resistivity of the conductive film, the total content of N and B is 65 at% or less, preferably 60 at% or less, and more preferably 40 at% or less. That is, the total content of N and B is more than 0 at% and 65 at% or less.

[0053] From the same viewpoint as above, when the conductive film 12 contains N, the N content is preferably more than 0 at%, more preferably 2 at% or more, even more preferably 5 at% or more, and even more preferably 10 at% or more. When the conductive film 12 contains N, the N content is preferably 65 at% or less, more preferably 60 at% or less, and even more preferably 40 at% or less.

[0054] From the same viewpoint as above, when the conductive film 12 contains B, the content of B is preferably more than 0 at%, more preferably 5 at% or more, even more preferably 10 at% or more, and even more preferably 15 at% or more. When the conductive film 12 contains B, the content of B is preferably 65 at% or less, more preferably 50 at% or less, even more preferably 40 at% or less, particularly preferably 35 at% or less, and most preferably 30 at% or less.

[0055] The conductive film 12 preferably further contains at least one of tantalum (Ta) and chromium (Cr). Specific examples include a TaN film containing Ta and N, a TaB film containing Ta and B, a CrN film containing Cr and N, and a CrB film containing Cr and B. Among these, the TaN film is preferable because it has high film hardness and large film stress.

[0056] When a TaN film is used as the conductive film 12, the N content in the TaN film is preferably more than 0 at% since the hardness of the TaN film against the substrate 11 is improved, more preferably 2 at% or more, even more preferably 10 at% or more, and particularly preferably 15 at% or more. The N content in the TaN film is preferably 65 at% or less since the surface smoothness of the TaN film is improved and the sheet resistance value of the TaN film is reduced, more preferably 60 at% or less, and even more preferably 55 at% or less.

[0057] When a TaB film is used as the conductive film 12, the B content in the TaB film is preferably more than 0 at% because the film adhesion and surface smoothness are improved, more preferably 5 at% or more, even more preferably 10 at% or more, particularly preferably 15 at% or more, and most preferably 20 at% or more. The B content in the TaB film is preferably 35 at% or less because the hardness is improved, and more preferably 30 at% or less.

[0058] When a CrN film is used as the conductive film 12, the N content in the CrN film is preferably more than 0 at% since the hardness of the CrN film against the substrate 11 is improved, more preferably 1 at% or more, and even more preferably 2 at% or more. The N content in the CrN film is preferably 65 at% or less since the surface smoothness of the CrN film is improved and the sheet resistance value of the CrN film is reduced, more preferably 50 at% or less, even more preferably 30 at% or less, and particularly preferably 15 at% or less.

[0059] A laminated film of a TaN film and a CrN film may be used as the conductive film 12. The laminated film having the above configuration contains the TaN film, and therefore has high film hardness and large film stress.

[0060] When using a laminated film having the above configuration, it is preferable to use a laminated film in which a TaN film and a CrN film are laminated in this order from the substrate 11 side. When using a laminated film having the above configuration, the total thickness of the laminated film satisfies the above-mentioned thickness of the conductive film 12. In addition, the N content of the TaN film and the N content of the CrN film each satisfy the above-mentioned range.

[0061] Furthermore, an upper layer may be provided on the conductive film 12. The upper layer is preferably a film containing chromium (Cr) and at least one element selected from the group consisting of nitrogen (N) and oxygen (O). By providing an upper layer on the conductive film 12, it is possible to improve mechanical properties and suppress changes in optical properties due to the formation of a natural oxide film.

[0062] When a CrO film is used as the upper layer of the conductive film 12, the O content in the CrO film is preferably 5 at% or more since the hardness of the CrO film is improved, more preferably 8 at% or more, and even more preferably 10 at% or more. The O content in the CrO film is preferably 30 at% or less since the surface smoothness of the CrO film is improved and the sheet resistance of the CrO film is reduced, more preferably 25 at% or less, even more preferably 20 at% or less, and particularly preferably 15 at% or less.

[0063] The thickness t' of the upper layer of the conductive film 12 is preferably 5 nm or more, more preferably 10 nm or more, even more preferably 15 nm or more, and particularly preferably 20 nm or more. The thickness t' of the upper layer of the conductive film 12 is preferably 100 nm or less, more preferably 70 nm or less, and even more preferably 50 nm or less.

[0064] When the conductive film 12 contains Ta, the half-width FWHM of the diffraction peak attributable to the bcc (110) plane of Ta among the diffraction peaks attributable to the conductive film 12 observed by out of plane XRD is preferably 1.5 to 4.0°. When the half-width FWHM is 1.5° or more, crystallization of the conductive film is suppressed, and the surface of the conductive film 12 is smoother. The half-width FWHM is more preferably 2.0° or more, and further preferably 3.0° or more.

[0065] On the other hand, if the full width at half maximum (FWHM) is 4.0° or less, the crystallinity of the conductive film does not become too low, so the hardness of the film does not decrease, and therefore the film does not wear out due to repeated use, and the overlay accuracy does not decrease.

[0066] The resistivity of the conductive film 12 is 3.5 mΩ·cm or less. In general, the fixing force of the EUV mask to the exposure tool improves as the resistivity of the conductive film 12 decreases. In this embodiment, the resistivity of the conductive film 12 is sufficiently low at 3.5 mΩ·cm or less, so that excellent fixing force can be obtained when fixing the EUV mask to the exposure tool. The resistivity of the conductive film 12 is preferably 1.0 mΩ·cm or less, more preferably 0.320 mΩ·cm or less, even more preferably 0.300 mΩ·cm or less, and particularly preferably 0.250 mΩ·cm or less.

[0067] Furthermore, the lower limit of the resistivity of the conductive film 12 is not particularly limited, but is preferably 0.050 mΩ·cm or more, more preferably 0.060 mΩ·cm or more, and even more preferably 0.065 mΩ·cm or more.

[0068] The resistivity of the conductive film 12 is measured using a resistivity meter, and the detailed measurement conditions follow the measurement method described in the examples below.

[0069] In order to set the resistivity of the conductive film 12 within the above range, the nitrogen or boron content in the conductive film can be adjusted. Even if an upper layer is provided on the conductive film 12, the resistivity of the laminated film can be regarded as the resistivity of the conductive film as it is if the resistivity of the conductive film is sufficiently lower than that of the upper layer. An example of a combination of a conductive film and an upper layer that results in a conductive film with a resistivity sufficiently lower than that of the upper layer is a combination of a TaN film as the conductive film and a CrO film as the upper layer.

[0070] A low sheet resistance value of the conductive film 12 is preferable because it improves the chucking force of the electrostatic chuck. The sheet resistance value of the conductive film 12 is preferably 250 Ω / □ or less, more preferably 200 Ω / □ or less, even more preferably 150 Ω / □ or less, even more preferably 100 Ω / □ or less, and particularly preferably 80 Ω / □ or less.

[0071] The sheet resistance value of the conductive film 12 is preferably 0.1 Ω / □ or more, more preferably 0.5 Ω / □ or more, and even more preferably 1.0 Ω / □ or more.

[0072] The conductive film 12 is preferably small in surface roughness because it improves adhesion to the electrostatic chuck. The surface roughness of the conductive film 12 is preferably 0.600 nm or less in terms of Rq (root mean square height, JIS B0601:2013), more preferably 0.400 nm or less, even more preferably 0.200 nm or less, particularly preferably 0.150 nm or less, and most preferably 0.100 nm or less. The surface roughness of the conductive film 12 is preferably 0.030 nm or more in terms of Rq, more preferably 0.050 nm or more, and even more preferably 0.070 nm or more. When the gas pressure of the gas used during film formation is 0.3 Pa or more, the surface roughness of the conductive film tends to be high.

[0073] The conductive film 12 preferably has a high surface hardness because this suppresses the generation of particles due to friction with the electrostatic chuck. The surface hardness of the conductive film 12 is preferably 10.0 GPa or more.

[0074] The surface hardness of the conductive film 12 is preferably 16.0 GPa or less, more preferably 14.0 GPa or less, and even more preferably 12.0 GPa or less. There are no particular limitations on the method for measuring the surface hardness of the conductive film 12, and known methods, specifically, for example, a Vickers hardness test, a Rockwell hardness test, a Brinell hardness test, a nanoindentation test, etc., can be used. Among these, the nanoindentation test is widely used when measuring the surface hardness of a thin film.

[0075] If a TaN film, a CrN film, or a laminated film of a CrN film and a TaN film is used as the conductive film 12, the surface hardness of the conductive film 12 becomes high, and the surface hardness becomes 10.0 GPa or more.

[0076] 1, film stress is generated in the reflective layer 13 and the absorbing layer 14 formed on the front side of the substrate 11. Film stress is also generated in the conductive film 12 formed on the back side of the substrate 11. In the EUV mask blank, the stress generated on the front side of the substrate 11 and the stress generated on the back side of the substrate 11 cancel each other out, suppressing deformation of the substrate caused by the application of stress.

[0077] As an example of an EUV mask blank, when deformation of the substrate is suppressed in an EUV mask blank having the following configuration, the flatness of the conductive film-coated substrate having a conductive film 12 formed on the back surface side of a substrate 11 is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less.

[0078] (composition) Substrate: SiO2-TiO2 glass substrate (152mm square, 6.3mm thick) Reflective layer: Si / Mo multilayer reflective film (Si film (4.5 nm) and Mo film (2.3 nm) alternately stacked 40 times (total thickness 272 nm)) Absorption layer: TaNH film (thickness 60 nm)

[0079] If a TaN film, a TaB film, or a laminated film of a CrN film and a TaN film is used as the conductive film 12, the film stress of the conductive film 12 is large, and the flatness of the substrate with the conductive film becomes 500 nm or less.

[0080] When an EUV mask is produced from an EUV mask blank, a heat treatment may be performed as a pretreatment. This heat treatment reduces the film stress of the reflective layer 13 and the absorbing layer 14 formed on the front side of the substrate 11 due to the film stress relaxation. In addition, the film stress of the conductive film 12 formed on the back side of the substrate 11 is reduced due to the film stress relaxation. If the stress is reduced due to the film stress relaxation, it becomes impossible to suppress the deformation of the substrate 11, and there is a risk of misalignment occurring in the pattern formed on the EUV mask produced using the EUV mask blank.

[0081] It is preferable that the conductive film 12 is less relaxed in film stress due to heat treatment. The difference in flatness of the conductive film-attached substrate measured before and after heat treatment can be used as an index of the relaxation of film stress due to heat treatment. When a conductive film-attached substrate having a conductive film 12 formed on the back side of a substrate 11 is heat-treated at 136°C for 20 minutes, the thermal relaxation rate of the flatness (warpage) of the conductive film-attached substrate measured before and after heat treatment, calculated by the following formula, is preferably 15% or less, more preferably 12% or less, and even more preferably 10% or less. The lower limit of the thermal relaxation rate of the flatness (warpage) is not particularly limited, but is, for example, 1.0% or more. Thermal relaxation rate of flatness (%)={(flatness of substrate with TaN conductive film before heat treatment−flatness of substrate with TaN conductive film after heat treatment) / flatness of substrate with TaN conductive film before heat treatment}×100

[0082] The flatness is measured using a flatness measuring device manufactured by Fujinon Corporation.

[0083] The conductive film 12 can be formed by a known film forming method, for example, a sputtering method such as a magnetron sputtering method or an ion beam sputtering method.

[0084] When forming, for example, a TaN film as the conductive film 12 by a sputtering method, the sputtering method may be performed using a Ta target in an atmosphere containing nitrogen (N2) and an inert gas containing at least one of helium (He), argon (Ar), neon (Ne), krypton (Kr), and xenon (Xe). When using magnetron sputtering, the film formation may be performed under the following specific film formation conditions.

[0085] (Film formation conditions) Target: Ta target Sputtering gas: mixed gas of Ar and N2 (N2 gas concentration: preferably 2 to 50 vol%, more preferably 2 to 40 vol%, and further preferably 2 to 30 vol%. Gas pressure: preferably 1×10 -1 Pa~3×10 -1 Pa, more preferably 1×10 -1 Pa~2×10 -1 Pa, more preferably 1×10 -1 Pa~1.5×10 -1 Pa.) Input power: preferably 300 to 1500 W, more preferably 500 to 1000 W Film formation speed: preferably 0.010 to 0.200 nm / sec, more preferably 0.050 to 0.100 nm / sec

[0086] When forming, for example, a TaB film as the conductive film 12 by a sputtering method, the sputtering method may be performed using a Ta target and a B target, or a TaB compound target, in an atmosphere containing an inert gas containing at least one of helium (He), argon (Ar), neon (Ne), krypton (Kr), and xenon (Xe). When using magnetron sputtering, the film formation may be performed under the following specific film formation conditions.

[0087] (Film formation conditions) Target: Ta target and B target, or TaB compound target Sputtering gas: Ar gas (gas pressure: preferably 1.0 × 10-1 Pa~5.0×10 -1 Pa, more preferably 1.0×10 -1 Pa ~ 4.0 × 10 -1 Pa, and more preferably 1.0×10 -1 Pa~3.0×10 -1 Pa.) Input power: preferably 300 to 1500 W, more preferably 500 to 1000 W Film formation speed: preferably 0.010 to 0.200 nm / sec, more preferably 0.010 to 0.100 nm / sec

[0088] When forming a CrN film as the conductive film 12 by sputtering, for example, the sputtering may be performed using a Cr target in an atmosphere containing nitrogen (N2) and an inert gas containing at least one of helium (He), argon (Ar), neon (Ne), krypton (Kr), and xenon (Xe). When using magnetron sputtering, the film formation may be performed under the following specific film formation conditions.

[0089] (Film formation conditions) Target:Cr target Sputtering gas: mixed gas of Ar and N2 (N2 gas concentration: preferably 20 to 60 vol%, more preferably 30 to 60 vol%, and further preferably 40 to 60 vol%. Gas pressure: preferably 1×10 -1 Pa~3×10 -1 Pa, more preferably 1×10 -1 Pa~2×10 -1 Pa, more preferably 1×10 -1 Pa~1.5×10 -1 Pa.) Input power: preferably 300 to 2000 W, more preferably 500 to 2000 W Film formation speed: preferably 0.010 to 0.200 nm / sec, more preferably 0.050 to 0.200 nm / sec

[0090] When forming a CrO film as an upper layer on the conductive film 12 by a sputtering method, for example, the sputtering method may be performed using a Cr target in an atmosphere containing an inert gas containing at least one of helium (He), argon (Ar), neon (Ne), krypton (Kr), and xenon (Xe) and oxygen (O2). When using magnetron sputtering, the film formation conditions may be specifically as follows.

[0091] (Film formation conditions) Target:Cr target Sputtering gas: mixed gas of Ar and O2 (O2 gas concentration: preferably 10 to 40 vol%, more preferably 20 to 40 vol%, and further preferably 30 to 40 vol%. Gas pressure: preferably 1×10 -1 Pa~2.0×10 -1 Pa, more preferably 1×10 -1 Pa~1.8×10 -1 Pa, more preferably 1×10 -1 Pa~1.6×10 -1 Pa.) Input power: preferably 300 to 1000 W, more preferably 500 to 1000 W Film formation speed: preferably 0.010 to 0.200 nm / sec, more preferably 0.050 to 0.200 nm / sec

[0092] The reflective layer 13 is not particularly limited as long as it has the desired properties as a reflective layer of an EUV mask blank. Here, a property particularly required for the reflective layer 13 is high EUV light reflectance. Specifically, when a light beam in the wavelength region of EUV light is irradiated onto the surface of the reflective layer 13 at an incident angle of 6 degrees, the maximum value of the light reflectance at a wavelength of about 13.5 nm is preferably 60% or more, more preferably 65% ​​or more.

[0093] As the reflective layer 13, a multilayer reflective film in which high refractive index layers and low refractive index layers are alternately stacked multiple times is usually used because it can achieve a high EUV light reflectance. In the multilayer reflective film forming the reflective layer 13, Mo is widely used for the high refractive index layers, and Si is widely used for the low refractive index layers. That is, a Mo / Si multilayer reflective film is the most common. However, the multilayer reflective film is not limited to this, and Ru / Si multilayer reflective film, Mo / Be multilayer reflective film, Mo compound / Si compound multilayer reflective film, Si / Mo / Ru multilayer reflective film, Si / Mo / Ru / Mo multilayer reflective film, and Si / Ru / Mo / Ru multilayer reflective film can also be used.

[0094] The thickness of each layer constituting the multilayer reflective film constituting the reflective layer 13 and the number of repeating units of the layers can be appropriately selected according to the film material used and the EUV light reflectance required for the reflective layer. Taking a Mo / Si multilayer reflective film as an example, to obtain a reflective layer 13 with a maximum EUV light reflectance of 60% or more, the multilayer reflective film may be formed by laminating Mo layers with a thickness of 2.3±0.1 nm and Si layers with a thickness of 4.5±0.1 nm so that the number of repeating units is 30 to 60.

[0095] Each layer constituting the multilayer reflective film forming the reflective layer 13 may be deposited to a desired thickness using a known deposition method such as magnetron sputtering or ion beam sputtering. For example, when forming a Si / Mo multilayer reflective film using ion beam sputtering, a Si target is used as the target, and Ar gas (gas pressure 1.3×10) is used as the sputtering gas. -2 ~2.7×10 -2 A Si film was formed to a thickness of 4.5 nm using an ion accelerating voltage of 300 to 1500 V and a deposition rate of 0.030 to 0.300 nm / sec using a 1000 V sputtering gas (gas pressure 1.3 × 10 -2 ~2.7×10 -2 It is preferable to deposit the Mo film to a thickness of 2.3 nm using a vacuum chamber (100 Pa) at an ion acceleration voltage of 300 V to 1500 V and a deposition rate of 0.030 to 0.300 nm / sec. This counts as one cycle, and the Si film and Mo film are laminated 40 to 50 cycles to deposit the Si / Mo multilayer reflective film.

[0096] An extremely low EUV light reflectance is a characteristic particularly required for the absorbing layer 14. Specifically, when a light beam in the wavelength region of EUV light is irradiated onto the surface of the absorbing layer 14, the maximum light reflectance at a wavelength of about 13.5 nm is preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less.

[0097] In order to achieve the above characteristics, the absorbing layer 14 is made of a material with a high absorption coefficient for EUV light. As a material with a high absorption coefficient for EUV light, it is preferable to use a material mainly composed of tantalum (Ta). In this specification, a material mainly composed of tantalum (Ta) means a material containing 20 at% or more of Ta. The absorbing layer 14 preferably contains 30 at% or more of Ta, more preferably contains 35 at% or more, even more preferably contains 40 at% or more, particularly preferably contains 45 at% or more, and most preferably contains 50 at% or more.

[0098] The material containing Ta as a main component for use in the absorption layer 14 may further include hafnium (Hf), silicon (Si), zirconium (Zr), germanium (Ge), boron (B), palladium (Pd), tin (Sn), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), silver (Ag), cadmium (Cd), indium (In), antimony (Sb), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), and platinum. It is preferable that the ZnO alloy contains at least one of the following: platinum (Pt), gold (Au), thallium (Tl), lead (Pb), bismuth (Bi), carbon (C), titanium (Ti), zirconium (Zr), molybdenum (Mo), ruthenium (Ru), rhodium (Rh), palladium (Pd), calcium (Ca), magnesium (Mg), aluminum (Al), nickel (Ni), copper (Cu), zinc (Zn), gallium (Ga), arsenic (As), selenium (Se), tellurium (Te), hydrogen (H) and nitrogen (N).

[0099] Specific examples of materials containing the above elements other than Ta include TaN, TaNH, TaHf, TaHfN, TaBSi, TaBSiN, TaB, TaBN, TaSi, TaSiN, TaGe, TaGeN, TaZr, TaZrN, TaPd, TaSn, TaPdN, TaSn, TaCr, TaMn, TaFe, TaCo, TaAg, TaCd, TaIn, TaSb, TaW, etc.

[0100] The absorbing layer 14 having the above-mentioned configuration can be formed by using a film forming method such as a sputtering method, for example, a magnetron sputtering method or an ion beam sputtering method.

[0101] For example, when a TaNH film is formed as the absorbing layer 14 by magnetron sputtering, a Ta target is used as the target, and a mixed gas of Ar, N2, and H2 (H2 gas concentration: 1 to 30 vol%, N2 gas concentration: 5 to 75 vol%, Ar gas concentration: 10 to 94 vol%, gas pressure: 0.5 × 10 -1 It is preferable to deposit the film at a pressure of 300 to 2000 W, a deposition rate of 0.5 to 60 nm / min, and a thickness of 20 to 90 nm.

[0102] The EUV mask blank 10 of this embodiment may have a configuration other than the configuration shown in FIG. 1, that is, the substrate 11, the conductive film 12, the reflective layer 13, and the absorbing layer 14.

[0103] In the EUV mask blank of this embodiment, a protective layer may be formed between the reflective layer 13 and the absorbing layer 14. The protective layer is provided for the purpose of protecting the reflective layer 13 from damage during pattern formation on the absorbing layer 14 by an etching process, usually a dry etching process. Therefore, a material that is not easily affected by the etching process of the absorbing layer 14, that is, a material that has an etching rate slower than that of the absorbing layer 14 and is not easily damaged by the etching process, is selected as the material for the protective layer. In order to satisfy the above characteristics, the protective layer is preferably made of a material containing ruthenium (Ru). Specific examples of materials containing Ru include Ru and Ru compounds (RuB, RuSi, RuNb, RuTi, RuY, RuZr, RuLa, etc.). The material containing Ru is preferably a material containing 40.0 at% or more of Ru in the material, more preferably 50.0 at% or more, and even more preferably 55.0 at% or more.

[0104] When a protective layer is formed, its thickness is preferably from 1 to 20 nm, more preferably from 1 to 5 nm.

[0105] When forming a protective layer, a well-known film formation method such as magnetron sputtering or ion beam sputtering is used. When forming a Ru film by magnetron sputtering, a Ru target is used as the target, and Ar gas (gas pressure: 1.0×10 -2 ~10×10 -1 It is preferable to form a film to a thickness of 2 to 5 nm using a dielectric constant 100% (1 Pa) at an input voltage of 30 to 1500 V and a film formation rate of 0.020 to 1.000 nm / sec.

[0106] Even when a protective layer is provided on the reflective layer 13, the maximum reflectance of light at a wavelength of about 13.5 nm is preferably 60% or more, more preferably 63% or more, and even more preferably 65% ​​or more.

[0107] Furthermore, in the EUV mask blank of this embodiment, a low reflective layer for the inspection light used for inspecting the mask pattern may be formed on the absorber layer 14.

[0108] The low-reflection layer is composed of a film that has low reflection for the inspection light used to inspect the mask pattern. When manufacturing an EUV mask, a pattern is formed in the absorbing layer, and then the pattern is inspected to see if it has been formed as designed. Inspection of this mask pattern normally uses an inspection machine that uses light of about 257 nm as the inspection light. In other words, the inspection is performed based on the difference in reflectance of this light of about 257 nm, specifically, the difference in reflectance between the surface of the absorbing layer that is exposed after it has been removed by pattern formation, and the surface of the absorbing layer that remains without being removed by pattern formation.

[0109] Here, the former is the reflective layer surface or the protective layer surface, and is usually the protective layer surface. Therefore, if the difference in reflectance between the reflective layer surface or the protective layer surface and the absorbing layer surface with respect to the wavelength of the inspection light is small, the contrast during the inspection will be poor, and accurate inspection will not be possible. If the difference in reflectance between the reflective layer surface or the protective layer surface and the absorbing layer surface with respect to the wavelength of the inspection light is small, the formation of a low reflection layer will improve the contrast during the inspection. When a low reflection layer is formed on an absorbing layer, the low reflection layer has a maximum light reflectance of 15% or less at the wavelength of the inspection light when the low reflection layer surface is irradiated with light in the wavelength range of the inspection light, more preferably 10% or less, and even more preferably 5% or less.

[0110] In order to achieve the above characteristics, the low reflection layer is preferably made of a material whose refractive index at the wavelength of the inspection light is lower than that of the absorption layer.

[0111] A low-reflection layer that satisfies these characteristics includes at least one selected from the group consisting of tantalum (Ta), palladium (Pd), chromium (Cr), silicon (Si), and hafnium (Hf), and at least one selected from the group consisting of oxygen (O) and nitrogen (N). Suitable examples of such a low-reflection layer include a TaPdO layer, a TaPdON layer, a TaON layer, a CrO layer, a CrON layer, a SiON layer, a SiN layer, a HfO layer, and a HfON layer.

[0112] The total content of Ta, Pd, Cr, Si and Hf in the low reflective layer is preferably 10 to 55 at %, particularly 10 to 50 at %, because this allows control of the optical characteristics in the wavelength region of the pattern inspection light.

[0113] The total content of O and N in the low reflective layer is preferably 45 to 90 at%, particularly preferably 50 to 90 at%, because this allows control of the optical characteristics in the wavelength region of the pattern inspection light. The total content of Ta, Pd, Cr, Si, Hf, O and N in the low reflective layer is preferably 95 to 100 at%, more preferably 97 to 100 at%, and even more preferably 99 to 100 at%.

[0114] The low reflective layer having the above-mentioned structure can be formed by sputtering using a target containing at least one of Ta, Pd, Cr, Si, and Hf. The target can be any of the above-mentioned two or more kinds of metal targets and compound targets.

[0115] The use of two or more kinds of metal targets is convenient for adjusting the constituent components of the low reflection layer. When two or more kinds of metal targets are used, the constituent components of the absorption layer can be adjusted by adjusting the input power to the target. On the other hand, when a compound target is used, it is preferable to adjust the target composition in advance so that the low reflection layer to be formed has a desired composition.

[0116] The sputtering method using the above target can be carried out in an inert gas atmosphere, similar to the sputtering method for forming the absorber layer.

[0117] However, when the low reflective layer contains oxygen (O), the sputtering method is carried out in an inert gas atmosphere containing at least one of He, Ar, Ne, Kr, and Xe, and O2. When the low reflective layer contains N, the sputtering method is carried out in an inert gas atmosphere containing at least one of He, Ar, Ne, Kr, and Xe, and N2. When the low reflective layer contains O and N, the sputtering method is carried out in an inert gas atmosphere containing at least one of He, Ar, Ne, Kr, and Xe, and O2 and N2.

[0118] Specific conditions for carrying out the sputtering method vary depending on the target used and the composition of the inert gas atmosphere in which the sputtering method is carried out, but in any case, the sputtering method may be carried out under the following conditions. The conditions for forming the low reflective layer are shown below, taking as an example the case where the inert gas atmosphere is a mixed gas atmosphere of Ar and O2.

[0119] (Conditions for forming low reflection layer) Gas pressure: 1.0×10 -1 ~50×10 -1 Pa, preferably 1.0 x 10 -1 ~40×10 -1 Pa, more preferably 1.0×10 -1 ~30×10 -1 Pa. Sputtering gas: mixed gas of Ar and O2 (O2 gas concentration: 3 to 80 vol%, preferably 5 to 60 vol%, more preferably 10 to 40 vol%) Input power: 30 to 1000 W, preferably 50 to 750 W, more preferably 80 to 500 W Film formation rate: 0.01 to 60 nm / min, preferably 0.05 to 45 nm / min, more preferably 0.1 to 30 nm / min

[0120] When an inert gas other than Ar or multiple inert gases are used, the total concentration of the inert gases is set to the same concentration range as the Ar gas concentration described above. When the inert gas atmosphere contains N2, the N2 concentration is set to the same concentration range as the oxygen concentration described above. When the inert gas atmosphere contains N2 and O2, the total concentration is set to the same concentration range as the oxygen concentration described above.

[0121] In the EUV mask blank of this embodiment, it is preferable to form a low-reflection layer on the absorbing layer because the wavelength of the pattern inspection light is different from the wavelength of the EUV light. Therefore, when EUV light (around 13.5 nm) is used as the pattern inspection light, it is considered that it is not necessary to form a low-reflection layer on the absorbing layer. The wavelength of the inspection light tends to shift to the short wavelength side as the pattern dimensions become smaller, and it is considered that it may shift to 193 nm or even 13.5 nm in the future. When the wavelength of the inspection light is 13.5 nm, it is considered that it is not necessary to form a low-reflection layer on the absorbing layer.

[0122] In the EUV mask blank of this embodiment, a hard mask layer described in JP 2009-54899 A or JP 2009-21582 A, that is, a layer of a material having resistance to the etching conditions of the absorption layer (absorption layer and low reflection layer when a low reflection layer is formed on the absorption layer), may be formed on the absorption layer 14 (on the absorption layer when a low reflection layer is formed on the absorption layer). By forming such a hard mask layer, the etching selectivity of the absorption layer (absorption layer and low reflection layer when a low reflection layer is formed on the absorption layer) and the hard mask layer under the etching conditions of the absorption layer (absorption layer and low reflection layer when a low reflection layer is formed on the absorption layer), specifically, the ratio of the etching rate of the absorption layer (absorption layer and low reflection layer when a low reflection layer is formed on the absorption layer) under the etching conditions of the absorption layer (absorption layer and low reflection layer when a low reflection layer is formed on the absorption layer) to the etching rate of the hard mask layer, can be made thin.

[0123] Next, the substrate with a conductive film of this embodiment will be described. The substrate with a conductive film of this embodiment has a conductive film on a substrate. Here, the substrate and the conductive film are the same as the substrate and the conductive film in the EUV mask blank of this embodiment. That is, the EUV mask blank of this embodiment is formed by forming a reflective layer and an absorbing layer on the surface opposite to the surface on which the conductive film is provided of the substrate with a conductive film of this embodiment.

[0124] As described above, the present specification discloses the following configurations. (1) a substrate; A conductive film disposed on the back side of the substrate; a reflective layer disposed on the front surface side of the substrate and reflecting EUV light; A reflective mask blank for EUV lithography having an absorption layer disposed on the reflective layer and absorbing EUV light, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B contained in the conductive film is more than 0 at% and 65 at% or less, The refractive index n of the conductive film at wavelengths of 1000 to 1100 nm λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, Refractive index n of the conductive film at wavelengths of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is less than or equal to 4.500, The refractive index n of the conductive film at wavelengths of 400 to 500 nm λ400-500nm is 2.500 or more, and the extinction coefficient k λ400-500nm is 0.440 or more, The thickness t of the conductive film is 20 to 350 nm, A reflective mask blank for EUV lithography with a conductive film resistivity of 3.5 mΩ·cm or less. (2) a substrate; A conductive film disposed on the back side of the substrate; a reflective layer disposed on the front surface side of the substrate and reflecting EUV light; A reflective mask blank for EUV lithography having an absorption layer disposed on the reflective layer and absorbing EUV light, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B in the conductive film is more than 0 at% and 65 at% or less, The refractive index n of the conductive film at wavelengths of 1000 to 1100 nm λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, Refractive index n of the conductive film at wavelengths of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is less than or equal to 4.500, The refractive index n of the conductive film at wavelengths of 480 to 500 nm λ480-500nm is 2.500 or more, and the extinction coefficient k λ480-500nm is 0.440 or more, The thickness t of the conductive film is 20 to 350 nm, A reflective mask blank for EUV lithography with a conductive film resistivity of 3.5 mΩ·cm or less. (3) A reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film contains at least one of tantalum (Ta) and chromium (Cr). (4) A reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film contains Ta and N. (5) A reflective mask blank for EUV lithography according to (4), wherein the conductive film contains N in an amount of more than 0 at % and not more than 65 at %. (6) A reflective mask blank for EUV lithography according to (1) or (2), wherein the conductive film contains Ta and B. (7) A reflective mask blank for EUV lithography according to (6), wherein the conductive film contains B in an amount of more than 0 at % and 35 at % or less. (8) A reflective mask blank for EUV lithography according to (1) or (2), wherein the resistivity of the conductive film is not less than 0.050 mΩ·cm and not more than 3.5 mΩ·cm. (9) The reflective mask blank for EUV lithography according to (3) or (4), wherein the conductive film contains Ta, and the half-width (FWHM) of a diffraction peak assigned to the bcc (110) plane of Ta, among diffraction peaks originating from the conductive film observed by out of plane XRD, is 1.5 to 4.0°. (10) The reflective mask blank for EUV lithography according to any one of (1) to (4), wherein the conductive film has a light transmittance of 1.0% or more at a wavelength of 1000 to 1100 nm, a light transmittance of 1.0% or more at a wavelength of 600 to 700 nm, and a light transmittance of 1.0% or less at a wavelength of 400 to 500 nm. (11) A reflective mask blank for EUV lithography according to any one of (1) to (4), wherein the conductive film has a sheet resistance of 250 Ω / □ or less. (12) A reflective mask blank for EUV lithography according to any one of (1) to (4), wherein the conductive film has a surface hardness of 10.0 GPa or more. (13) an upper layer is provided on the conductive film; The reflective mask blank for EUV lithography according to any one of (1) to (4), wherein the upper layer contains chromium (Cr) and at least one element selected from the group consisting of nitrogen (N) and oxygen (O). (14) The reflective mask blank for EUV lithography according to any one of (1) to (4), wherein the conductive film has a surface roughness (Rq) of 0.600 nm or less. (15) A substrate having a conductive film thereon, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B contained in the conductive film is more than 0 at% and 65 at% or less, The refractive index n of the conductive film at a wavelength of 1000 to 1100 nm λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, The refractive index n of the conductive film at a wavelength of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is less than or equal to 4.500, The refractive index n of the conductive film at a wavelength of 400 to 500 nm λ400-500nm is 2.500 or more, and the extinction coefficient k λ400-500nm is 0.440 or more, The conductive film has a thickness t of 20 to 350 nm, A substrate with a conductive film, the resistivity of which is 3.5 mΩ·cm or less. (16) A substrate having a conductive film thereon, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B contained in the conductive film is more than 0 at% and 65 at% or less, The refractive index n of the conductive film at a wavelength of 1000 to 1100 nm λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, The refractive index n of the conductive film at a wavelength of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is less than or equal to 4.500, The refractive index n of the conductive film at a wavelength of 480 to 500 nm λ480-500nm is 2.500 or more, and the extinction coefficient k λ480-500nm is 0.440 or more, The conductive film has a thickness t of 20 to 350 nm, A substrate with a conductive film, the resistivity of which is 3.5 mΩ·cm or less. (17) The substrate with a conductive film according to (15) or (16), wherein the conductive film contains at least one of tantalum (Ta) and chromium (Cr). (18) The substrate with a conductive film according to (15) or (16), wherein the conductive film contains Ta and N. (19) The substrate with a conductive film according to (18), wherein the conductive film contains N in an amount of more than 0 at % and not more than 65 at %. (20) The substrate with a conductive film according to (15) or (16), wherein the conductive film contains Ta and B. (21) The substrate with a conductive film according to (20), wherein the conductive film contains B in an amount of more than 0 at % and 35 at % or less. (22) The substrate with a conductive film according to (15) or (16), wherein the conductive film has a resistivity of 0.050 mΩ·cm or more and 3.5 mΩ·cm or less. (23) The substrate with a conductive film according to (17) or (18), wherein the conductive film contains Ta, and among the diffraction peaks originating from the conductive film observed by an out of plane XRD method, the full width at half maximum (FWHM) of a diffraction peak assigned to a bcc (110) plane of Ta is 1.5 to 4.0°. (24) The substrate with a conductive film according to any one of (15) to (18), wherein the conductive film has a light transmittance of 1.0% or more for a wavelength of 1000 to 1100 nm, a light transmittance of 1.0% or more for a wavelength of 600 to 700 nm, and a light transmittance of 1.0% or less for a wavelength of 400 to 500 nm. (25) The substrate with a conductive film according to any one of (15) to (18), wherein the conductive film has a sheet resistance value of 250 Ω / □ or less. (26) The substrate with a conductive film according to any one of (15) to (18), wherein the conductive film has a surface hardness of 10.0 GPa or more. (27) An upper layer is further provided on the conductive film, The substrate with a conductive film according to any one of (15) to (18), wherein the upper layer contains chromium (Cr) and at least one element selected from the group consisting of nitrogen (N) and oxygen (O). (28) The substrate with a conductive film according to any one of (15) to (18), wherein the conductive film has a surface roughness (Rq) of 0.600 nm or less. EXAMPLES

[0125] The present invention will be described in more detail below with reference to Examples 1 to 10, but the present invention is not limited to these Examples 1 to 3, 5, and 10 are working examples, and Examples 4, and 6 to 9 are comparative examples.

[0126] <Example 1> In this example, a TaN film was formed as a conductive film on one surface of the substrate. A SiO2-TiO2 glass substrate (6-inch (152 mm) square, 6.3 mm thick) was used as the substrate for film formation. The thermal expansion coefficient of this glass substrate at 20°C is 0.02×10 -7 / ℃, Young's modulus is 67GPa, Poisson's ratio is 0.17, and specific rigidity is 3.07×10 7 m 2 / s 2 The glass substrate was polished to have a smooth surface with a surface roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less.

[0127] A TaN film was formed as a conductive film on one surface of the substrate by magnetron sputtering under the following conditions: (Film formation conditions) Target: Ta target Sputtering gas: Mixture of Ar and N2 (Ar: 90 vol%, N2: 10 vol%, gas pressure: 0.12 Pa) Input power: 1000W Deposition speed: 6nm / min Film thickness: 56 nm

[0128] (TaN film composition analysis) The composition of the TaN film was measured using a Rutherford Backscattering Spectrometry (RBS) X-ray photoelectron spectrometry. The N content of the TaN film was 21.0 at%.

[0129] (Refractive index n, extinction coefficient k) The refractive index n of the TaN film formed at wavelengths of 1000 to 1100 nm was λ1000-1100nm , and the extinction coefficient k λ1000-1100nm The refractive index n at wavelengths of 1000 to 1100 nm was measured using a spectroscopic ellipsometer (manufacturer: JA Woollam, model: M2000-DI). A light beam was incident on the surface on which the TaN film was formed, and the polarization state was measured and analyzed at room temperature. λ1000-1100nm , and the extinction coefficient k λ1000-1100nmThe refractive index n at wavelengths of 600 to 700 nm was calculated using the same procedure. λ600-700nm , and the extinction coefficient k λ600-700nm , the refractive index n at wavelengths of 400 to 500 nm λ400-500nm , and the extinction coefficient k λ400-500nm , and the refractive index n at wavelengths of 480 to 500 nm λ480-500nm , and the extinction coefficient k λ480-500nm The results are shown in Table 2.

[0130] (Light transmittance) For the substrate after the TaN film was formed, a light beam was applied perpendicularly to the surface on which the TaN film was formed, and the light transmittance was measured in the wavelength range of 175 to 2000 nm using a spectrophotometer (manufacturer: Hitachi High-Technologies Corporation, model: U-4100). The light transmittance at wavelengths of 1000 to 1100 nm, 600 to 700 nm, and 400 to 500 nm were obtained. If the light transmittance at wavelengths of 1000 to 1100 nm was 1.0% or more, the light transmittance at wavelengths of 1.0% or more, and the light transmittance at wavelengths of 400 to 500 nm were 1.0% or less, it was marked as ◯, and if any of these conditions were not met, it was marked as ×. The results are shown in Table 1.

[0131] (XRD half width FWHM) The TaN film was measured by the out of plane XRD method. The main peak of the diffraction peak attributed to the bcc (110) plane of Ta among the diffraction peaks from the TaN film was measured for the half-width (FWHM) in the diffraction angle range of 30 to 40 degrees. The results are shown in Table 1.

[0132] (Surface hardness) The surface hardness of the TaN film was measured by a nanoindentation test. A surface hardness of 10.0 GPa or more was marked as ◯, and a surface hardness of less than 10.0 GPa was marked as ×. The results are shown in Table 1.

[0133] (resistivity) The resistivity of the TaN film was calculated under the following conditions. Resistivity of 3.5 mΩ·cm or less was marked as ◯, and resistivity of over 3.5 mΩ·cm was marked as ×. If the resistivity is sufficiently low at 3.5 mΩ·cm or less, it can be considered that sufficient fixing force is obtained when fixing an EUV mask made from an EUV mask blank to an exposure tool. The resistivity was evaluated from the surface of the conductive film of the sample. Evaluation equipment: Nitto Seiko Analytech Loresta-GX Number of measurement points: 9 points Measurement range: 149mm x 149mm

[0134] (Surface roughness) The surface roughness (root-mean-square roughness RQ) was measured in an area of ​​2 μm × 2 μm using an atomic force microscope (AFM) manufactured by SII Corporation.

[0135] (Thermal relaxation rate of flatness) The flatness of the TaN film-coated substrate after the TaN film formation was measured using a flatness measuring device manufactured by Fujinon Co., Ltd. Next, the flatness of the TaN film-coated substrate after heat treatment at 136°C for 20 minutes was measured using a flatness measuring device manufactured by Fujinon Co., Ltd. Next, the thermal relaxation rate of the flatness was calculated using the following formula, and when the thermal relaxation rate of the flatness was 15% or less, it was marked as ◯, and when it was more than 15%, it was marked as ×. Thermal relaxation rate of flatness (%)={(flatness of TaN film-coated substrate before heat treatment−flatness of TaN film-coated substrate after heat treatment) / flatness of TaN film-coated substrate before heat treatment}×100

[0136] <Example 2> In this example, a laminated film of a TaN film and a CrN film was formed as a conductive film on one surface of the substrate by magnetron sputtering. The deposition conditions for the TaN film and the CrN film are as follows: (TaN film) Target: Ta target Sputtering gas: Ar and N2 mixed gas (Ar: 60 vol%, N2: 40 vol%, gas pressure: 0.11 Pa) Input power: 1000W Deposition speed: 3.9nm / min Film thickness: 23 nm (CrN film) Target:Cr target Sputtering gas: Ar and N2 mixed gas (Ar: 53 vol%, N2: 47 vol%, gas pressure: 0.10 Pa) Input power: 1700W Deposition speed: 11.4nm / min Film thickness: 26 nm

[0137] (Composition analysis of TaN and CrN films) The compositions of the TaN and CrN films were measured by RBS. The N content of the TaN film was 59.0 at% and the N content of the CrN film was 4.2 at%.

[0138] (Refractive index n, extinction coefficient k) The refractive index n and extinction coefficient k of the laminated film were measured in the same manner as in Example 1. The results are shown in Table 2. Note that the refractive index n and extinction coefficient k shown in Table 2 are the values ​​of the TaN film, and the refractive index n and extinction coefficient k of the CrN film were the same as those in Examples 3, 4 and 9.

[0139] (Light transmittance) The light transmittance of the laminated film was measured in the same manner as in Example 1. The results are shown in Table 1. (XRD half width FWHM) The TaN film was measured by the out of plane XRD method, and the half-width (FWHM) of the main peak of the diffraction peak attributed to the bcc (110) plane of Ta was measured in the diffraction angle range of 30 to 40°. The results are shown in Table 1.

[0140] (Surface hardness) The surface hardness of the laminated film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0141] (resistivity) The resistivity of the laminated film was measured by the same method as in Example 1. At this time, the resistivities of the TaN film and the CrN film were measured. The results are shown in Table 1.

[0142] (Surface roughness) The surface roughness of the laminated film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0143] (Thermal relaxation rate of flatness) The thermal relaxation rate of the flatness of the laminated film-coated substrate was measured in the same manner as in Example 1. The results are shown in Table 1.

[0144] <Example 3> In this example, a CrN film was formed as a conductive film on one surface of the substrate by magnetron sputtering. The deposition conditions for the CrN film are as follows: (Film formation conditions) Target:Cr target Sputtering gas: Ar and N2 mixed gas (Ar: 53 vol%, N2: 47 vol%, gas pressure: 0.10 Pa) Input power: 1700W Deposition speed: 11.4nm / min Film thickness: 40 nm

[0145] (CrN film composition analysis) The composition of the CrN film was measured by RBS, and the N content of the CrN film was 4.2 at%.

[0146] (Refractive index n, extinction coefficient k) The refractive index n and extinction coefficient k of the CrN film were measured in the same manner as in Example 1. The results are shown in Table 2.

[0147] (Light transmittance) The light transmittance of the CrN film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0148] (Surface hardness) The surface hardness of the CrN film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0149] (resistivity) The resistivity of the CrN film was measured using the same method as in Example 1. The results are shown in Table 1.

[0150] (Thermal relaxation rate of flatness) The thermal relaxation rate of the flatness of the CrN film-coated substrate was measured in the same manner as in Example 1. The results are shown in Table 1.

[0151] <Example 4> In this example, the same procedure as in Example 3 was carried out, except that the thickness of the CrN film was 360 nm.

[0152] (CrN film composition analysis) The composition of the CrN film was measured by RBS, and the N content of the CrN film was 4.2 at%.

[0153] (Refractive index n, extinction coefficient k) The refractive index n and extinction coefficient k of the CrN film were measured in the same manner as in Example 1. The results are shown in Table 2.

[0154] (Light transmittance) The light transmittance of the CrN film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0155] (Surface hardness) The surface hardness of the CrN film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0156] (resistivity) The resistivity of the CrN film was measured using the same method as in Example 1. The results are shown in Table 1.

[0157] (Thermal relaxation rate of flatness) The thermal relaxation rate of the flatness of the CrN film-coated substrate was measured in the same manner as in Example 1. The results are shown in Table 1.

[0158] <Example 5> In this example, a TaB film was formed as a conductive film on one surface of the substrate by magnetron sputtering. The deposition conditions for the TaB film are as follows. (Film formation conditions) Target: TaB compound target Sputtering gas: Ar gas (gas pressure: 0.205 Pa) Input power: 1000W Deposition speed: 1.67nm / min Film thickness: 56 nm

[0159] (TaB film composition analysis) The composition of the TaB film was measured by RBS and X-ray photoelectron spectroscopy (XPS). The N content of the TaB film was 0.0 at% and the B content was 28.0 at%.

[0160] (Refractive index n, extinction coefficient k) The refractive index n and extinction coefficient k of the TaB film were measured in the same manner as in Example 1. The results are shown in Table 2.

[0161] (Light transmittance) The light transmittance of the laminated film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0162] (XRD half width FWHM) The TaB film was measured by the out of plane XRD method, and the half-width (FWHM) of the main peak of the diffraction peak attributed to the bcc (110) plane of Ta was measured in the diffraction angle range of 30 to 40°. The results are shown in Table 1.

[0163] (Surface hardness) The surface hardness of the TaB film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0164] (resistivity) The resistivity of the TaB film was measured using the same method as in Example 1. The results are shown in Table 1.

[0165] (Surface roughness) The surface roughness of the TaB film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0166] (Thermal relaxation rate of flatness) The thermal relaxation rate of the flatness of the TaB film-coated substrate was measured in the same manner as in Example 1. The results are shown in Table 1.

[0167] <Example 6> In this example, a TaON film was formed as a conductive film on one surface of the substrate by magnetron sputtering. The deposition conditions for the TaON film are as follows: (Film formation conditions) Target: Ta target Sputtering gas: N2 and O2 mixed gas (N2: 88 vol%, O2: 12 vol%, gas pressure: 0.18 Pa) Input power: 1000W Deposition speed: 0.9nm / min Film thickness: 60nm

[0168] (TaON film composition analysis) The composition of the TaON film was measured by RBS, and the N content of the TaON film was 6.0 at% and the O content was 68.0 at%.

[0169] (Refractive index n, extinction coefficient k) The refractive index n and extinction coefficient k of the TaON film were measured in the same manner as in Example 1. The results are shown in Table 2.

[0170] (Light transmittance) The light transmittance of the TaON film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0171] (Resistance value) The resistivity of the TaON film was measured using the same method as in Example 1. The results are shown in Table 1.

[0172] <Example 7> In this example, a CrON film was formed as a conductive film on one surface of the substrate by magnetron sputtering. The deposition conditions for the CrON film are as follows: (Film formation conditions) Target:Cr target Sputtering gas: Mixture of Ar, N2 and O2 (Ar: 33 vol%, N2: 22 vol%, O2: 45 vol%, gas pressure: 0.09 Pa) Input power: 750W Deposition speed: 1.86nm / min Film thickness: 60nm

[0173] (Refractive index n, extinction coefficient k) The refractive index n and extinction coefficient k of the CrON film were measured in the same manner as in Example 1. The results are shown in Table 2.

[0174] (Light transmittance) The light transmittance of the CrON film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0175] <Example 8> In this example, the same procedure as in Example 1 was carried out, except that the thickness of the TaN film was set to 17 nm.

[0176] (TaN film composition analysis) The composition of the TaN film was measured by RBS, and the N content of the TaN film was 21.0 at%.

[0177] (Refractive index n, extinction coefficient k) The refractive index n and extinction coefficient k of the TaN film were measured in the same manner as in Example 1. The results are shown in Table 2.

[0178] (Light transmittance) The light transmittance of the TaN film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0179] (Thermal relaxation rate of flatness) The thermal relaxation rate of the flatness of the TaN film-coated substrate was measured in the same manner as in Example 1. The results are shown in Table 1.

[0180] <Example 9> In this example, the same procedure as in Example 3 was carried out, except that the thickness of the CrN film was set to 12 nm.

[0181] (CrN film composition analysis) The composition of the CrN film was measured by RBS, and the N content of the CrN film was 4.2 at%.

[0182] (Refractive index n, extinction coefficient k) The refractive index n and extinction coefficient k of the CrN film were measured in the same manner as in Example 1. The results are shown in Table 2.

[0183] (Light transmittance) The light transmittance of the CrN film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0184] (Thermal relaxation rate of flatness) The thermal relaxation rate of the flatness of the CrN film-coated substrate was measured in the same manner as in Example 1. The results are shown in Table 1.

[0185] <Example 10> In this example, a TaN film was formed as a conductive film on one side of the substrate by magnetron sputtering, and a CrO film was further formed as an upper layer. The TaN film was formed under the same film formation conditions as the TaN film in Example 2, except that the thickness was changed. The deposition conditions for the TaN film and the CrO film are as follows:

[0186] (TaN film) Target: Ta target Sputtering gas: Ar and N2 mixed gas (Ar: 60 vol%, N2: 40 vol%, gas pressure: 0.11 Pa) Input power: 1000W Deposition speed: 3.9nm / min Film thickness: 30 nm

[0187] (CrO film) Target:Cr target Sputtering gas: Ar and O2 mixed gas (Ar: 66 vol%, O2: 34 vol%, gas pressure: 0.16 Pa) Input power: 750W Deposition speed: 9.0nm / min Film thickness: 27 nm

[0188] (Composition analysis of TaN film and CrO film) The compositions of the TaN and CrO films were measured by RBS. The N content of the TaN film was 59.0 at% and the O content of the CrO film was 15.0 at%.

[0189] (Refractive index n, extinction coefficient k) The refractive index n and extinction coefficient k of the laminated film were measured in the same manner as in Example 1. The results are shown in Table 2. Note that the refractive index n and extinction coefficient k shown in Table 2 indicate the values ​​of the CrO film, and the refractive index n and extinction coefficient k of the TaN film were the same as those of the TaN film in Example 2.

[0190] (Light transmittance) The light transmittance of the laminated film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0191] (Surface hardness) The surface hardness of the laminated film was measured in the same manner as in Example 1. The results are shown in Table 1.

[0192] (resistivity) The resistivity of the TaN film was measured using the same method as in Example 1. The results are shown in Table 1.

[0193] (Surface roughness) The surface roughness of the laminate was measured in the same manner as in Example 1. The results are shown in Table 1.

[0194] (Thermal relaxation rate of flatness) The thermal relaxation rate of the flatness of the laminated film-coated substrate was measured in the same manner as in Example 1. The results are shown in Table 1.

[0195] [Table 1]

[0196] [Table 2]

[0197] Refractive index n λ1000-1100nm is 5.300 or less, extinction coefficient k λ1000-1100nm is 5.200 or less, refractive index n λ600-700nm is 4.300 or less, extinction coefficient k λ600-700nm is 4.500 or less, refractive index n λ400-500nmis 2.600 or more, extinction coefficient k λ400-500nm is 0.440 or more, and the refractive index n λ480-500nm is 2.500 or more, extinction coefficient k λ480-500nm In Examples 1, 2, 3, 5, and 10 in which the transmittance was 0.440 or more and the thickness t of the conductive film was 20 to 350 nm, the light transmittance was evaluated as ◯ and the resistivity of the conductive film was also evaluated as ◯.

[0198] In the case of Example 1 in which the conductive film 12 was a TaN film, Example 2 in which the conductive film 12 was a laminated film of a CrN film and a TaN film, Example 5 in which the conductive film 12 was a TaB film, and Example 10 in which a CrO film was provided as an upper layer on the TaN film, the thermal relaxation rate of the flatness of the conductive film-coated substrate was evaluated as ◯.

[0199] In Example 1 in which the conductive film 12 was a TaN film, Example 2 in which the conductive film 12 was a laminated film of a CrN film and a TaN film, and Example 3 in which the conductive film 12 was a CrN film, the surface hardness of the conductive film 12 was 10.0 GPa or more, and the surface hardness was ◯.

[0200] Refractive index n λ400-500nm is less than 2.500, extinction coefficient k λ400-500nm is less than 0.440, refractive index n λ480-500nm is less than 2.500, extinction coefficient k λ480-500nm In Examples 6 and 7, where the transmittance was less than 0.440, the light transmittance at wavelengths of 400 to 500 nm was high at more than 1.0%, and the light transmittance was evaluated as ×. In addition, in Comparative Example 6, the resistivity of the conductive film was evaluated as ×.

[0201] In Example 4, in which the thickness t of the conductive film was more than 350 nm, the light transmittance for wavelengths of 1000 to 1100 nm and the light transmittance for wavelengths of 600 to 700 nm were both 0.0%, and the light transmittance was evaluated as ×.

[0202] In Examples 8 and 9, in which the thickness t of the conductive film was less than 20 nm, the light transmittance at wavelengths of 400 to 500 nm was high at more than 1.0%, and the light transmittance was evaluated as ×.

[0203] Although various embodiments have been described above with reference to the drawings, it goes without saying that the present invention is not limited to such examples. It is clear that a person skilled in the art can come up with various modified or revised examples within the scope of the claims, and it is understood that these also naturally belong to the technical scope of the present invention. Furthermore, the components in the above-mentioned embodiments may be arbitrarily combined within the scope of the invention.

[0204] This application is based on a Japanese patent application (Patent Application No. 2023-043149) filed on March 17, 2023, the contents of which are incorporated by reference into this application. [Explanation of symbols]

[0205] 10: EUV mask blank 11: Substrate 12: Conductive film 13: Reflective layer (multilayer reflective film) 14: Absorption layer

Claims

1. A substrate; A conductive film disposed on a rear surface side of the substrate; a reflective layer disposed on a front surface side of the substrate and configured to reflect EUV light; A reflective mask blank for EUV lithography having an absorber layer disposed on the reflective layer and absorbing EUV light, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B contained in the conductive film is more than 0 at % and 65 at % or less, The refractive index n of the conductive film at wavelengths of 1000 to 1100 nm λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, The refractive index n of the conductive film at wavelengths of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is less than or equal to 4.500, The refractive index n of the conductive film at wavelengths of 480 to 500 nm λ480-500nm is 2.500 or more, and the extinction coefficient k λ480-500nm is 0.440 or more, The conductive film has a thickness t of 20 to 350 nm, The resistivity of the conductive film is 3.5 mΩ cm or less, The sheet resistance value of the conductive film is 0.1 Ω / □ or more and 250 Ω / □ or less. Reflective mask blank for EUV lithography.

2. 2. The reflective mask blank for EUV lithography according to claim 1, wherein the conductive film contains at least one of tantalum (Ta) and chromium (Cr).

3. The reflective mask blank for EUV lithography according to claim 1 , wherein the conductive film contains Ta and N.

4. The reflective mask blank for EUV lithography according to claim 3 , wherein the conductive film contains N in an amount of more than 0 at % and not more than 65 at %.

5. The reflective mask blank for EUV lithography according to claim 1 , wherein the conductive film contains Ta and B.

6. The reflective mask blank for EUV lithography according to claim 5 , wherein the conductive film contains B in an amount of more than 0 at % and 35 at % or less.

7. 3. The reflective mask blank for EUV lithography according to claim 1, wherein the conductive film has a resistivity of 0.050 mΩ·cm or more and 3.5 mΩ·cm or less.

8. 3. The reflective mask blank for EUV lithography according to claim 1, wherein the conductive film contains Ta, and a full width at half maximum (FWHM) of a diffraction peak assigned to a bcc(110) plane of Ta, among diffraction peaks originating from the conductive film observed by an out of plane XRD method, is 1.5 to 4.0°.

9. 3. The reflective mask blank for EUV lithography according to claim 1, wherein the conductive film has a light transmittance of 1.0% or more for a wavelength of 1000 to 1100 nm, a light transmittance of 1.0% or more for a wavelength of 600 to 700 nm, and a light transmittance of 1.0% or less for a wavelength of 400 to 500 nm.

10. 3. The reflective mask blank for EUV lithography according to claim 1, wherein the conductive film has a light transmittance of 1.0% or more for a wavelength of 1000 to 1100 nm, a light transmittance of 1.0% or more for a wavelength of 600 to 700 nm, and a light transmittance of less than 1.0% for a wavelength of 400 to 500 nm.

11. 3. The reflective mask blank for EUV lithography according to claim 1, wherein the conductive film has a surface hardness of 10.0 GPa or more.

12. An upper layer is further provided on the conductive film, 3. The reflective mask blank for EUV lithography according to claim 1, wherein the upper layer contains chromium (Cr) and at least one element selected from the group consisting of nitrogen (N) and oxygen (O).

13. 3. The reflective mask blank for EUV lithography according to claim 1, wherein the conductive film has a surface roughness (Rq) of 0.600 nm or less.

14. A substrate having a conductive film thereon, The conductive film contains at least one of nitrogen (N) and boron (B), The total content of N and B contained in the conductive film is more than 0 at % and 65 at % or less, The refractive index n of the conductive film at wavelengths of 1000 to 1100 nm λ1000-1100nm is 5.300 or less, and the extinction coefficient k λ1000-1100nm is less than or equal to 5.200, The refractive index n of the conductive film at wavelengths of 600 to 700 nm λ600-700nm is 4.300 or less, and the extinction coefficient k λ600-700nm is less than or equal to 4.500, The refractive index n of the conductive film at wavelengths of 480 to 500 nm λ480-500nm is 2.500 or more, and the extinction coefficient k λ480-500nm is 0.440 or more, The conductive film has a thickness t of 20 to 350 nm, The resistivity of the conductive film is 3.5 mΩ cm or less, The sheet resistance value of the conductive film is 0.1 Ω / □ or more and 250 Ω / □ or less. Substrate with conductive film.

15. 15. The substrate with a conductive film according to claim 14, wherein the conductive film contains at least one of tantalum (Ta) and chromium (Cr).

16. The substrate with a conductive film according to claim 14 , wherein the conductive film contains Ta and N.

17. The substrate with a conductive film according to claim 16 , wherein the conductive film contains N in an amount of more than 0 at % and not more than 65 at %.

18. The substrate with a conductive film according to claim 14 , wherein the conductive film contains Ta and B.

19. 20. The substrate with a conductive film according to claim 18, wherein the conductive film contains B in an amount of more than 0 at % and 35 at % or less.

20. 16. The substrate with a conductive film according to claim 14, wherein the resistivity of the conductive film is 0.050 mΩ·cm or more and 3.5 mΩ·cm or less.

21. The substrate with a conductive film according to claim 14 or 15, wherein the conductive film contains Ta, and a full width at half maximum (FWHM) of a diffraction peak attributable to a bcc (110) plane of Ta, among diffraction peaks attributable to the conductive film observed by an out of plane XRD method, is 1.5 to 4.0°.

22. 16. The substrate with a conductive film according to claim 14 or 15, wherein the conductive film has a light transmittance of 1.0% or more for a wavelength of 1000 to 1100 nm, a light transmittance of 1.0% or more for a wavelength of 600 to 700 nm, and a light transmittance of 1.0% or less for a wavelength of 400 to 500 nm.

23. 16. The substrate with a conductive film according to claim 14 or 15, wherein the conductive film has a light transmittance of 1.0% or more for a wavelength of 1000 to 1100 nm, a light transmittance of 1.0% or more for a wavelength of 600 to 700 nm, and a light transmittance of less than 1.0% for a wavelength of 400 to 500 nm.

24. 16. The substrate with a conductive film according to claim 14, wherein the conductive film has a surface hardness of 10.0 GPa or more.

25. An upper layer is further provided on the conductive film, 16. The substrate with a conductive film according to claim 14, wherein the upper layer contains chromium (Cr) and at least one element selected from the group consisting of nitrogen (N) and oxygen (O).

26. 16. The substrate with a conductive film according to claim 14, wherein the surface roughness (Rq) of the conductive film is 0.600 nm or less.

Citation Information

Patent Citations

  • Reflective mask blank for EUV lithography, substrate with functional film for mask blank

    JP2012049498A

  • Reflective mask blank for EUV lithography and substrate with functional film for mask blank

    JP2012178577A

  • Reflective mask blank for EUV lithography, and reflective mask for EUV lithography

    JP2015015420A

  • Reflection type mask blank for EUV lithography, and, reflection type mask for EUV lithography

    JP2018106183A

  • Reflection type mask blank and reflection type mask

    JP2019035848A