Polymerizable composition, ion exchange resin, ion exchange film, membrane electrode assembly, and hydrogen production device
A polymerizable composition with enhanced compatibility components addresses the challenge of producing efficient ion exchange resins and membranes for hydrogen production devices, ensuring high performance and stability in water electrolysis systems.
Patent Information
- Application Number
- JP2023083625
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
AI Technical Summary
Existing water electrolysis methods for producing hydrogen face challenges in efficiently producing a cured ion exchange resin and membrane for anion exchange membranes, which are crucial for hydrogen production devices, due to compatibility issues between quaternary ammonium salts and polymerizable monomers, leading to phase separation and reduced performance.
A polymerizable composition comprising a quaternary ammonium salt, a polymerizable monomer, a linear or branched alkylene glycol, and a nitrogen-containing compound is used to enhance compatibility, allowing for efficient production of a cured ion exchange resin and membrane without phase separation, even with low-compatibility photopolymerization initiators.
The composition enables the production of an ion exchange resin with high ion exchange performance and durability, facilitating efficient hydrogen production through improved compatibility and stability, suitable for use in hydrogen production devices.
Smart Images

Figure 2024167509000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymerizable composition, an ion exchange resin, an ion exchange membrane, a membrane electrode assembly, and a hydrogen production device. [Background technology]
[0002] Water electrolysis, in which water is electrolyzed to produce hydrogen gas and oxygen gas, is being researched as a method of producing hydrogen. Hydrogen produced using energy obtained by a method that suppresses the generation of carbon dioxide as electricity is called CO2-free hydrogen, or green hydrogen, and is expected to be a next-generation clean energy source that can replace fossil fuels.
[0003] Among water electrolysis methods, AEM-type water electrolysis using an anion exchange membrane (AEM) is attracting attention because it does not require the use of expensive precious metals as a catalyst. An AEM-type water electrolysis device includes, for example, an AEM, and an anode chamber and a cathode chamber separated by the AEM and each equipped with an anode and a cathode. The AEM is obtained, for example, by filling a porous substrate with an ion exchange resin. It is known to use a resin having a quaternary ammonium group as the ion exchange resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2022-502522 [Patent Document 2] International Publication No. 2016 / 027595 [Patent Document 3] International Publication No. 2011 / 125717 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a polymerizable composition that can efficiently produce a cured product, and an ion exchange resin, an ion exchange membrane, a membrane electrode assembly, and a hydrogen production device, each of which contains a cured product of the polymerizable composition. [Means for solving the problem]
[0006] According to one aspect, there is provided a polymerizable composition comprising a quaternary ammonium salt represented by the following formula (I), a polymerizable monomer, a linear or branched alkylene glycol having 1 to 4 carbon atoms, and a nitrogen-containing compound represented by the following formula (II):
[0007] [ka]
[0008] In the above formula (I), R 1 R is an alkenyl group having 2 to 5 carbon atoms. 2 R is an alkylene group having 1 to 10 carbon atoms. 3 , R 4 , and R 5 are each independently a linear or branched alkyl group having 1 to 4 carbon atoms, or a linear or branched alkoxy group having 1 to 4 carbon atoms. - is an anion.
[0009] [ka]
[0010] In the above formula (II), R 10 is an alkyl group having 1 to 4 carbon atoms. 11 is an alkyl group having 1 to 4 carbon atoms. 12 R is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a secondary amino group having an alkyl group having 1 to 3 carbon atoms as a substituent, or a tertiary amino group having an alkyl group having 1 to 3 carbon atoms as a substituent. 11 and R 12may be bonded to each other to form a heterocycle. 10 , R 11 , and R 12 The total number of carbon atoms is 3 or more and 7 or less.
[0011] According to one aspect, there is provided an ion exchange resin comprising at least one of a cured product of the polymerizable composition according to the embodiment and an ion exchanger of an anion of the cured product.
[0012] According to one aspect, an ion exchange membrane is provided, the ion exchange membrane including an ion exchange resin according to an embodiment and a substrate.
[0013] According to one aspect, a membrane electrode assembly is provided, the membrane electrode assembly including an ion exchange membrane according to an embodiment and an electrode.
[0014] According to one aspect, a hydrogen production device is provided, the hydrogen production device including an ion exchange membrane according to an embodiment. Effect of the Invention
[0015] According to the present invention, there are provided a polymerizable composition that can efficiently produce a cured product, and an ion exchange resin, an ion exchange membrane, a membrane electrode assembly, and a hydrogen production device, each of which includes a cured product of the polymerizable composition. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a hydrogen production device according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The polymerizable composition according to the embodiment contains a quaternary ammonium salt represented by the above formula (I), a polymerizable monomer, a linear or branched alkylene glycol having 1 to 4 carbon atoms, and a nitrogen-containing compound represented by the above formula (II).
[0018] When such a polymerizable composition is used, a cured product can be efficiently produced. The reason is considered to be as follows. That is, the compatibility of the quaternary ammonium salt having a polymerizable group shown in formula (I) with the polymerizable monomer tends to be lower than that of the primary ammonium salt having a polymerizable group. As a result of intensive research by the present inventors, it was found that a polymerizable composition in which the quaternary ammonium salt having a polymerizable group shown in formula (I) and the polymerizable monomer are unlikely to separate can be obtained by using a linear or branched alkylene glycol having 1 to 4 carbon atoms and a nitrogen-containing compound shown in formula (II) as a co-solvent. The reason for this is unclear, but it is considered to be because the compatibility of the nitrogen-containing compound is excellent with both the quaternary ammonium salt and the polymerizable monomer, or the nitrogen-containing compound exerts a surfactant effect. When such a polymerizable composition having excellent compatibility and unlikely to cause phase separation is used, a cured product can be continuously produced without stirring the polymerizable composition. In addition, the polymerizable composition according to the embodiment can achieve excellent compatibility even when a photopolymerization initiator having low compatibility with a quaternary ammonium salt or a polymerizable monomer is added, and therefore the polymerizable composition is suitably used as a polymerizable composition for photocuring.
[0019] [Polymerizable composition] The polymerizable composition according to the embodiment is typically liquid at room temperature and pressure. Here, room temperature means a temperature of 20° C. or higher and 40° C. or lower, and normal pressure means 1 atmosphere. The viscosity of the polymerizable composition at 25° C., as measured by a tuning fork vibration viscometer, is, in one example, 300 mPa·s or lower, and in another example, 100 mPa·s or lower. By using the liquid polymerizable composition, an ion exchange resin with high ion exchange performance can be realized.
[0020] The polymerizable composition according to the embodiment contains a quaternary ammonium salt represented by the following formula (I), a polymerizable monomer, a linear or branched alkylene glycol having 1 to 4 carbon atoms, and a nitrogen-containing compound represented by the formula (II).
[0021] [ka]
[0022] In the above formula (I), R 1 R is an alkenyl group having 2 to 5 carbon atoms. 1 is preferably a vinyl group or an allyl group, and more preferably a vinyl group.
[0023] R 2 R is an alkylene group having 1 to 10 carbon atoms. 2 is preferably an alkylene group having 1 to 5 carbon atoms, more preferably a methylene group or an ethylene group, and even more preferably a methylene group.
[0024] R 3 , R 4 , and R 5 are each independently a linear or branched alkyl group having 1 to 4 carbon atoms, or a linear or branched alkoxy group having 1 to 4 carbon atoms. 3 , R 4 , and R 5 are each independently preferably a linear alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group or an ethyl group.
[0025] X - X may be a monovalent anion or a divalent anion. - is, for example, a halide ion, a tetrafluoroborate ion, a bicarbonate ion, a hydroxide ion, a triflate, or a bistrifluoromethanesulfonimide ion. A halide ion is, for example, a fluoride ion, a chloride ion, or a bromide ion. X - is preferably a chloride ion, a triflate, or a bistrifluoromethanesulfonimide ion. - When X is a chloride ion, an ion exchange resin having a large amount of ion exchange groups per unit mass can be obtained. -When the quaternary ammonium salt is a triflate or bistrifluoromethanesulfonimide, the solubility of the composition increases, and the concentration of the quaternary ammonium salt in the polymerizable composition tends to be easily increased.
[0026] Specific examples of quaternary ammonium salts include (vinylbenzyl)trialkylammonium salts, 4-ethenyl-N,N-dimethylbenzeneethanaminium salts, and 4-ethenyl-N,N-dimethylbenzenepropanaminium salts.
[0027] Specific examples of (vinylbenzyl)trialkylammonium salts include (vinylbenzyl)trimethylammonium chloride, (vinylbenzyl)trimethylammonium triflate, (vinylbenzyl)trimethylammonium bistrifluoromethanesulfonimide, (vinylbenzyl)dimethylethylammonium chloride, (vinylbenzyl)dimethylethylammonium triflate, (vinylbenzyl)dimethylethylammonium bistrifluoromethanesulfonimide, (vinylbenzyl)trimethylammonium tetrafluoroborate, (vinylbenzyl)trimethylammonium bicarbonate, and (vinylbenzyl)trimethylammonium hydroxide.
[0028] Other specific examples of quaternary ammonium salts include 4-ethenyl-N,N-dimethylbenzeneethanaminium chloride, 4-ethenyl-N,N-dimethylbenzeneethanaminium triflate, 4-ethenyl-N,N-dimethylbenzeneethanaminium bistrifluoromethansulfonium, 4-ethenyl-N,N-dimethylbenzeneethanaminium hydroxide, 4-ethenyl-N,N-dimethylbenzenepropanaminium chloride, 4-ethenyl-N,N-dimethylbenzenepropanaminium triflate, 4-ethenyl-N,N-dimethylbenzenepropanaminium bistrifluoromethansulfonium, 4-ethenyl-N,N-dimethylbenzenepropanaminium hydroxide, and the like.
[0029] As the quaternary ammonium salt, it is preferable to use a (vinylbenzyl)trialkylammonium salt, and it is more preferable to use at least one salt selected from the group consisting of (vinylbenzyl)trimethylammonium chloride, (vinylbenzyl)trimethylammonium triflate, and (vinylbenzyl)trimethylammonium bistrifluoromethanesulfonylimide.
[0030] In the polymerizable composition, the proportion of the quaternary ammonium salt is, for example, 5% by mass or more and 95% by mass or less. This proportion is preferably 50% by mass or more, preferably 60% by mass or more, and more preferably 65% by mass or more. When this proportion is high, an ion exchange resin having a large amount of ion exchange groups per unit mass tends to be obtained. This proportion may be 92% by mass or less, 85% by mass or less, or 80% by mass or less.
[0031] The proportion of the quaternary ammonium salt in the polymerizable composition can be measured, for example, by subtracting the weight of the quaternary ammonium salt remaining unreacted after the polymerization reaction from the total mass of the quaternary ammonium salts used as raw materials.
[0032] In the polymerizable composition, the ratio of the quaternary ammonium salt may vary depending on the type. The concentration of vinylbenzyltrimethylammonium chloride is, for example, 60% by mass or more and 70% by mass or less. The concentration of vinylbenzyltrimethylammonium triflate is, for example, 75% by mass or more and 85% by mass or less. The concentration of vinylbenzyltrimethylammonium bistrifluoromethanesulfonimide is, for example, 85% by mass or more and 95% by mass or less.
[0033] The polymerizable monomer may be a comonomer that polymerizes with the quaternary ammonium salt. The polymerizable monomer may crosslink the quaternary ammonium salts together, thereby increasing the durability of the cured product.
[0034] The polymerizable monomer may have one radical polymerizable group in one molecule, or may have two or more radical polymerizable groups in one molecule. Examples of the radical polymerizable group include a vinyl group, an allyl group, an acryloyl group, and a methacryloyl group, and it is preferable to use a vinyl group.
[0035] As the polymerizable monomer, for example, at least one selected from the group consisting of a vinyl compound having one vinyl group, a divinyl compound having two vinyl groups, an allyl compound having one allyl group, a diallyl compound having two allyl groups, and a diene is used. The polymerizable monomer preferably has two polymerizable groups, and is more preferably a divinyl compound.
[0036] Specific examples of the polymerizable monomer include divinylbenzene, divinylbenzene derivatives, divinyl sulfone, butadiene, chloroprene, divinylphenyl, trivinylbenzenes, divinylnaphthalene, allylamine, diallylamine, divinylpyridine, styrene, acrylonitrile, methylstyrene, acrolein, methyl vinyl ketone, vinyl biphenyl, diallyl isocyanurate, 1,2-bis(4-vinylphenyl)ethane, trivinylbenzene, 1,6-bis(4-vinylbenzyloxy)hexane, and N,N-dimethyl-N-(4-vinylbenzyl)-4-(4-vinylphenyl)butane-1-ammonium chloride.
[0037] As the radical polymerizable monomer, it is preferable to use at least one styrene derivative selected from the group consisting of divinylbenzene, 1,2-bis(4-vinylphenyl)ethane, trivinylbenzene, 1,6-bis(4-vinylbenzyloxy)hexane, and N,N-dimethyl-N-(4-vinylbenzyl)-4-(4-vinylphenyl)butane-1-ammonium chloride.
[0038] In the polymerizable composition, the proportion of the polymerizable monomer is, for example, 0.1% by mass or more and 50% by mass or less, preferably 1% by mass or more and 20% by mass or less, and more preferably 2% by mass or more and 10% by mass or less. If this proportion is high, the durability of the cured body tends to be increased. If this proportion is excessively high, the performance of the ion exchange resin may be reduced. This proportion can be measured, for example, by subtracting the weight of the polymerizable composition remaining unreacted after the polymerization reaction from the total mass of the polymerizable composition used as a raw material.
[0039] The ratio M3 / M4 of the mass M3 of the quaternary ammonium salt to the mass M4 of the polymerizable monomer is, for example, 1 or more and 100 or less, preferably 3 or more and 50 or less, and more preferably 5 or more and 25 or less. When this ratio is high, the performance of the ion exchange resin tends to be improved. When this ratio is low, the durability of the cured body tends to be improved.
[0040] A linear or branched alkylene glycol having 1 to 4 carbon atoms can function as an organic solvent. The alkylene glycol preferably has 1 to 3 carbon atoms, more preferably 2 carbon atoms.
[0041] The boiling point of the alkylene glycol is preferably 110° C. or higher, and more preferably 120° C. or higher. There is no particular upper limit to this boiling point, but according to one example, it is 300° C. or lower.
[0042] The flash point of the alkylene glycol is preferably 90° C. or higher, and more preferably 110° C. or higher. There is no particular lower limit for this flash point, but according to one example, it is 200° C. or higher.
[0043] Specific examples of the alkylene glycol include methylene glycol, ethylene glycol, propylene glycol, trimethylene glycol, 1,3-butylene glycol, tetramethylene glycol, etc. As the alkylene glycol, it is preferable to use ethylene glycol.
[0044] In the polymerizable composition, the proportion of alkylene glycol is, for example, 1% by mass or more and 50% by mass or less, preferably 5% by mass or more and 40% by mass or less, and more preferably 10% by mass or more and 35% by mass or less. If this proportion is high, the compatibility of the polymerizable composition tends to increase. If this proportion is excessively high, the performance of the ion exchange resin may decrease. This proportion can be measured, for example, by subtracting the weight of the polymerizable composition remaining unreacted after the polymerization reaction from the total mass of the polymerizable composition used as a raw material.
[0045] The ratio M3 / M2 of the mass M3 of the quaternary ammonium salt to the mass M2 of the alkylene glycol is, for example, 0.01 or more and 95 or less, preferably 1 or more and 50 or less, and more preferably 1.8 or more and 10 or less. When this ratio is high, the performance of the ion exchange resin tends to be improved. When this ratio is low, the compatibility of the polymerizable composition tends to be improved.
[0046] The ratio M4 / M2 of the mass M4 of the polymerizable monomer to the mass M2 of the alkylene glycol is, for example, 0.02 or more and 1 or less, preferably 0.05 or more and 0.5 or less, and more preferably 0.10 or more and 0.25 or less. When this ratio is high, the durability of the cured body tends to be increased. When this ratio is low, the compatibility of the polymerizable composition tends to be increased.
[0047] The nitrogen-containing compound is represented by the following formula (II): The nitrogen-containing compound may function as a stabilizer that inhibits separation of the polymerizable composition.
[0048] [ka]
[0049] In the above formula (II), R 10 is an alkyl group having 1 to 4 carbon atoms. 10 is an alkyl group having 1 to 4 carbon atoms. 11 is preferably a methyl group or an ethyl group.
[0050] R11 is an alkyl group having 1 to 4 carbon atoms. 11 is preferably a methyl group or an ethyl group.
[0051] R 12 R is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a secondary amino group having an alkyl group having 1 to 3 carbon atoms as a substituent, or a tertiary amino group having an alkyl group having 1 to 3 carbon atoms as a substituent. 12 is preferably a hydrogen atom, a methyl group, an ethyl group, a dimethylamino group, or a diethylamino group.
[0052] R 11 and R 12 may be bonded to each other to form a heterocycle. The number of ring carbon atoms in this heterocycle may be, for example, 2 or more and 6 or less, or 3 or more and 5 or less. The number of ring nitrogen atoms in this heterocycle is 1 or 2. This heterocycle may have, for example, an alkyl group having 1 to 3 carbon atoms as a substituent.
[0053] R 10 , R 11 , and R 12 The total number of carbon atoms is 3 or more and 7 or less. The total number of carbon atoms may be 4 or more, 5 or more, or 6 or more.
[0054] The nitrogen-containing compound may be in a liquid state or a solid state under normal temperature and pressure, but is preferably in a liquid state.
[0055] The boiling point of the nitrogen-containing compound is preferably 100° C. or higher, and more preferably 140° C. or higher. There is no particular upper limit to this boiling point, but according to one example, it is 300° C. or lower.
[0056] The flash point of the nitrogen-containing compound is preferably 60° C. or higher, more preferably 70° C. or higher, and more preferably 80° C. or higher. There is no particular upper limit to this flash point, but according to one example, it is 200° C. or lower.
[0057] The molar mass of the nitrogen-containing compound is, for example, 70 g / mol or more and 200 g / mol or less, and preferably 80 g / mol or more and 130 g / mol or less.
[0058] Examples of the nitrogen-containing compound include at least one compound selected from the group consisting of N,N-dimethylpropylene urea, 1-methyl-2-pyrrolidone, N-methyl-2-piperidone, 1,3-dimethyl-2-imidazolidinone, N,N-dimethylacetamide, N,N-diethylformamide, N,N-diethylacetamide, and tetramethylurea. As the nitrogen-containing compound, it is preferable to use at least one compound selected from the group consisting of N,N-dimethylpropylene urea, 1-methyl-2-pyrrolidone, N-methyl-2-piperidone, and 1,3-dimethyl-2-imidazolidinone. When these compounds are used, the polymerizability of the polymerizable composition tends to increase.
[0059] In the polymerizable composition, the proportion of the nitrogen-containing compound is, for example, 1% by mass or more and 10% by mass or less, preferably 1% by mass or more and 5% by mass or less, and more preferably 2.0% by mass or more and 4.0% by mass or less. If this proportion is high, the compatibility of the polymerizable composition tends to increase. If this proportion is excessively high, the performance of the ion exchange resin may decrease. This proportion can be measured, for example, by subtracting the weight of the polymerizable composition remaining unreacted after the polymerization reaction from the total mass of the polymerizable composition used as a raw material.
[0060] In the polymerizable composition, the amount of the nitrogen-containing compound may be, for example, 0.01 to 0.5 molar equivalents relative to the quaternary ammonium salt, preferably 0.03 to 0.4 molar equivalents, more preferably 0.1 to 0.3 molar equivalents.
[0061] The ratio M3 / M1 of the mass M3 of the quaternary ammonium salt to the mass M1 of the nitrogen-containing compound is, for example, 5 or more and 95 or less, preferably 7 or more and 50 or less, and more preferably 10 or more and 30 or less. When this ratio is high, the performance of the ion exchange resin tends to be improved. When this ratio is low, the compatibility of the polymerizable composition tends to be improved.
[0062] The ratio M4 / M1 of the mass M4 of the polymerizable monomer to the mass M1 of the nitrogen-containing compound is, for example, 0.01 or more and 50 or less, preferably 0.1 or more and 25 or less, and more preferably 0.5 or more and 5 or less. When this ratio is high, the durability of the cured body tends to be increased. When this ratio is low, the compatibility of the polymerizable composition tends to be increased.
[0063] The ratio M1 / M2 of the mass M1 of the nitrogen-containing compound to the mass M2 of the alkylene glycol is, for example, 0.03 or more and 10 or less, preferably 0.03 or more and 3 or less, and more preferably 0.05 or more and 0.3 or less. When this ratio is within this range, the compatibility of the polymerizable composition tends to be increased.
[0064] The polymerizable composition according to the embodiment may contain a polymerization initiator, an organic solvent, other additives, and the like.
[0065] As the polymerization initiator, at least one of a thermal polymerization initiator and a photopolymerization initiator is used. Examples of the thermal polymerization initiator include benzoyl peroxide, p-chlorobenzoyl peroxide, decanoyl peroxide, lauroyl peroxide, acetyl peroxide, tert-butyl (2-ethylhexanoyl) peroxide hexanoate, and tert-butyl peroxy octoate. Examples of the photopolymerization initiator include 1-phenyl-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-benzyl-2-(N,N-dimethylamino)-1-(4-morpholinophenyl)butan-1-one, and 2-methyl-1-[4-(methylthio)phenyl]-2-2morpholinopropan-1-one.
[0066] The proportion of the polymerization initiator in the polymerizable composition is, for example, 0.1% by mass to 10% by mass, preferably 1% by mass to 5% by mass, which can be measured, for example, by subtracting the weight of the polymerizable composition remaining unreacted after the polymerization reaction from the total weight of the polymerizable composition used as a raw material.
[0067] As the organic solvent other than the alkylene glycol and the nitrogen-containing compound, for example, at least one selected from the group consisting of methanol, ethanol, 1-propanol, isopropanol, dialkylene glycol, dimethyl sulfoxide (DMSO), 1-butanol, 1-pentanol, 1-hexanol, 1-heptanol, 1-octanol, 1-nonanol, 1-decanol, isodecanol, tridecanol, 1-undecanol, 1-dodecanol, 2-butanol, 3-pentanol, 3-hexanol, 3-heptanol, 2-undecanol, 2-dodecanol, cyclopentanol, cyclohexanol, cyclooctanol, 1,2-hexanediol, 1,2-octanediol, and 1,2-decanediol is used.
[0068] The polymerizable composition preferably does not contain at least one selected from the group consisting of methanol, ethanol, 1-propanol, isopropanol, dialkylene glycol, and trihydric alcohol. The polymerizable composition preferably does not contain alcohol having 1 to 3 carbon atoms. If these compounds are contained, the compatibility of the polymerizable composition may decrease. The content of these compounds is preferably 5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.1% by mass or less. The lower limit of the content of these compounds is, for example, 0% by mass, and in another example, 100 ppm or more. This ratio can be measured, for example, by NMR or liquid chromatography.
[0069] The polymerizable composition preferably does not contain water. When the polymerizable composition contains water, components constituting the composition, such as a polymerizable monomer and a polymerization initiator, may precipitate. The concentration of water in the polymerizable composition is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less. In one example, the lower limit of the water concentration is 0% by mass, and in another example, 100 ppm. This concentration can be measured, for example, by Karl Fischer water content measurement or gas chromatography.
[0070] As other additives, known additives such as antioxidants, polymerization inhibitors, plasticizers, and surfactants may be used.
[0071] As the polymerization inhibitor, for example, at least one selected from the group consisting of 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4-OH-TEMPO), 4-tert-butylcatechol (TBC), cupferron, and benzoquinone is used.
[0072] The proportion of the polymerization inhibitor in the polymerizable composition is, for example, 0.0001% by mass or more and 2% by mass or less, preferably 0.001% by mass or more and 1.0% by mass or less, and more preferably 0.005% by mass or more and 0.1% by mass or less. This proportion can be measured, for example, by gas chromatography.
[0073] [Ion exchange resin] The ion exchange resin according to the embodiment includes a cured product of the polymerizable composition according to the embodiment. The ion exchange resin may be a copolymer of a quaternary ammonium salt and a polymerizable monomer. The ion exchange resin may be an ion exchanger of the anion of the cured product. The ion exchanger of the anion of the cured product means a resin in which the anion of the quaternary ammonium group of the cured product is replaced with another type of anion.
[0074] The ion exchange resin may be suitably used as an anion exchange resin.
[0075] The ion exchange resin contains a quaternary ammonium group as an ion exchange group. The anion of the quaternary ammonium group is, for example, a halide ion, a triflate, a bistrifluoromethanesulfonimide, a hydroxide ion, a carbonate ion, or a bicarbonate ion. The counter ion is preferably a hydroxide ion, a carbonate ion, a bicarbonate ion, or a halide ion. Ion exchange resins having these ions are suitable as anion exchange resins.
[0076] The weight average molecular weight of the ion exchange resin is, for example, not less than 1,000, and preferably not less than 5,000. The average molecular weight of the ion exchange resin can be measured, for example, by gel permeation chromatography or a limiting viscosity method.
[0077] The ion exchange resin has a structure in which, for example, a main chain made of a hydrocarbon is bonded to a plurality of side chains each containing a quaternary ammonium group. The plurality of main chains may be bonded via a crosslinking agent which is a radical polymerizable monomer.
[0078] The ion exchange resin according to the embodiment has, for example, a structure represented by the following formula (IV): The ion exchange resin having the structure represented by formula (IV) is obtained by curing a polymerizable composition containing divinylbenzene as a radical polymerizable monomer.
[0079] [ka]
[0080] In formula (IV), R 1a is an alkylene group having 1 to 4 carbon atoms. 2 , R 3 , R 4 , and R 5 Each of X1 independently has the same meaning as in formula (I). - X1 is a halide ion, a triflate, a bistrifluoromethanesulfonimide, a hydroxide ion, a carbonate ion, a bicarbonate ion, or a tetrafluoroborate. - is preferably a hydroxide ion, a carbonate ion, or a bicarbonate ion.
[0081] The ion exchange resin can be obtained, for example, by thermally polymerizing or photopolymerizing the polymerizable composition according to the embodiment.
[0082] [Ion exchange membrane] The ion exchange membrane according to the embodiment includes the ion exchange resin according to the embodiment and a substrate. The ion exchange resin can be supported on the substrate. The ion exchange membrane according to the embodiment can be suitably used as an anion exchange membrane (AEM).
[0083] The ion exchange membrane according to the embodiment can be used in a hydrogen production apparatus, a water electrolysis apparatus, a fuel cell, an electrodialysis apparatus, a diffusion dialysis apparatus, a pure water production apparatus, an ion-exchanged water production apparatus, etc. The ion exchange membrane according to the embodiment can be suitably used as an anion exchange membrane for an AEM hydrogen production apparatus, an AEM water electrolysis apparatus, or a fuel cell.
[0084] The thickness of the ion exchange membrane is, for example, 1 μm or more and 500 μm or less. When a thick ion exchange membrane is used, the membrane resistance tends to increase. When a thin ion exchange membrane is used, the membrane resistance tends to decrease. The thickness of the ion exchange membrane is preferably 10 μm or more and 200 μm or less, more preferably 20 μm or more and 100 μm or less. The method for measuring the thickness of the ion exchange membrane will be described later in the examples.
[0085] The ion exchange capacity of the ion exchange membrane according to the embodiment is, for example, 1.0 mmol / g or more, in another example, 2.0 mmol / g or more, and in yet another example, 2.5 mmol / g or more. The ion exchange membrane according to the embodiment can realize a high ion exchange capacity because a polymerizable composition having a high concentration of a quaternary ammonium salt can be used. There is no particular upper limit to the ion exchange capacity, but in one example, it is 4.0 mmol / g or less, and in another example, it is 3.0 mmol / g or less. The method for measuring the ion exchange capacity will be described later in the examples.
[0086] The membrane resistance of the ion exchange membrane according to the embodiment is, for example, 2.0 Ω cm 2 or less, and according to other examples, 1.0 Ω cm 2 There is no particular lower limit for the membrane resistance, but one example is 0.1 Ω cm 2 or more, and according to other examples, 0.2 Ω cm 2 The method for measuring the membrane resistance will be described later in the Examples.
[0087] The water content of the ion exchange membrane according to the embodiment is, for example, 20% or more, in another example, 30% or more, and in yet another example, 40% or more. When the water content of the ion exchange membrane is high, the ionic conductivity of water tends to increase, and it is considered that the conductivity is improved. From the viewpoint of increasing the mechanical strength of the membrane, the water content of the ion exchange membrane is preferably 120% or less, and more preferably 100% or less. The method for measuring the water content will be described later in the examples.
[0088] The substrate functions as a support for the ion exchange resin. The substrate is preferably a porous membrane. For example, a porous film, a woven fabric, a nonwoven fabric, a sponge, a film, etc. can be used as the substrate. When a porous membrane is used as the substrate, it is preferable that the pores of the substrate are filled with the ion exchange resin.
[0089] The substrate is, for example, a polyolefin resin, a fluorine-based resin, polyacrylonitrile, polyvinyl chloride, polyester, polyamide, polysulfone, polyethersulfone, polyphenylenesulfone, polyphenylenesulfide, polyimide, polyethermide, polyamideimide, polycarbonate, polyacrylate, cellulose acetate, polyetheretherketone, or a copolymer thereof. The polyolefin resin includes polyethylene, polypropylene, polybutadiene, polymethylpentene, polybutene, polypentene, polyhexene, polymethylheptene, and a copolymer thereof. The fluorine-based resin includes polytetrafluoroethylene, poly(tetrafluoroethylene-hexafluoropropylene), polyvinylidene fluoride, polyvinylidene fluoride, polyhexafluoropropylene, polychlorotrifluoroethylene, and a copolymer thereof. The substrate preferably includes a polyolefin resin, and more preferably includes at least one of polyethylene and polypropylene.
[0090] The film thickness of the substrate is, for example, 1 μm or more and 500 μm or less, preferably 5 μm or more and 200 μm or less, more preferably 10 μm or more and 150 μm or less, and further preferably 20 μm or more and 100 μm or less.
[0091] The porosity of the substrate is, for example, 25% or more and 60% or less, preferably 30% or more and 50% or less, and more preferably 35% or more and 45% or less.
[0092] [Method of manufacturing ion exchange membrane] The method for producing an ion exchange membrane according to the embodiment includes contacting the polymerizable composition according to the embodiment with a substrate to obtain a first structure, and irradiating the first structure with ultraviolet light to obtain a second structure.
[0093] In this manufacturing method, since a polymerizable composition containing a quaternary ammonium salt is used, the step of introducing an ion exchange group into the resin obtained by polymerization can be omitted, compared with the case where a polymerizable composition consisting of only a compound having no ion exchange group is used. In addition, since a part or the whole of the polymerizable composition is polymerized by ultraviolet irradiation, the ion exchange membrane can be manufactured in a short time, compared with the case where a thermal polymerization method is used.
[0094] The manufacturing method will be described in detail below.
[0095] The method of contacting the polymerizable composition according to the embodiment with the substrate is not particularly limited. The polymerizable composition may be applied to the substrate, sprayed, or dropped. The substrate may be immersed in the polymerizable composition. The amount of the polymerizable composition per 1 g of substrate is, for example, 0.2 g or more and 2.0 g or less. The substrate may be subjected to a surface treatment such as a corona treatment, a glow discharge treatment, or an alkali treatment in order to enhance adhesion to the polymerizable composition.
[0096] In the first structure, the polymerizable composition is supported on the substrate. At least one of the main surfaces of the substrate of the first structure is preferably covered with a resin film, and both surfaces are more preferably covered with a resin film. By covering with a resin film, the composition change of the polymerizable composition supported on the first structure can be suppressed. That is, when the polymerizable composition contains an organic solvent, the composition of the polymerizable composition may change due to the volatilization of the organic solvent. By covering with a resin film, the volatilization of the organic solvent can be suppressed. In addition, by covering with a resin film, the smoothness of the surface of the ion exchange membrane is increased, and an ion exchange membrane with a uniform thickness can be obtained. As the resin of the resin film, for example, polyethylene terephthalate, polyester, perfluoroethylene propene copolymer, tetrafluoroethylene-hexaethylene propylene copolymer, etc. are used.
[0097] The first structure is irradiated with ultraviolet light to obtain a second structure in which the polymerizable composition is polymerized, that is, an ion exchange membrane. The wavelength of the ultraviolet light to be irradiated is, for example, 300 nm or more and 400 nm or less, and preferably, 330 nm or more and 380 nm or less. The ultraviolet light intensity is, for example, 1 mW / cm. 2 More than 10000mW / cm 2 Less than or equal to 50 mW / cm 2 More than 8000mW / cm 2 The irradiation time is, for example, from 0.5 seconds to 3 hours, and preferably from 1 second to 1 hour. As the irradiation source, for example, an ultraviolet light-emitting diode (LED), a halogen lamp, a xenon lamp, a tungsten lamp, a mercury lamp, or the like is used. From the viewpoints of ease of control of the irradiation wavelength and low heat generation, it is preferable to use an LED.
[0098] As described above, when the polymerizable composition contains an organic solvent, the composition of the polymerizable composition may change due to the volatilization of the organic solvent, so it is preferable to irradiate with ultraviolet rays immediately after obtaining the first structure. Specifically, after the production of the first structure, the ultraviolet rays are irradiated preferably within 0.5 hours, more preferably within 0.1 hours. Note that the organic solvent volatilizes during the ultraviolet irradiation or the heat treatment described below, so it does not remain in the ion exchange membrane.
[0099] After the first structure is irradiated with ultraviolet light to obtain the second structure, the second structure may be heat-treated to obtain the third structure, i.e., the ion exchange membrane. That is, after a part of the polymerizable composition is polymerized by ultraviolet light irradiation, the polymerizable composition may be completely polymerized by thermal polymerization. In the heat treatment, the heating temperature is, for example, 50°C or more and 150°C or less, preferably 80°C or more and 130°C or less. The heating time is, for example, 1 minute or more and 3 hours or less, preferably 3 minutes or more and 1 hour or less. The heating method may be a hot plate, an oven, an infrared heater, a heating furnace, or the like.
[0100] It is also possible to omit the ultraviolet irradiation and carry out only the heat treatment, or to carry out the ultraviolet irradiation after the heat treatment.
[0101] The structure obtained after light irradiation, heating, or both light irradiation and heating may be washed with water, an organic solvent (ethanol, acetone, chloroform, dichloromethane, etc.), or a mixed solvent thereof to wash off ethylene glycol and the like contained in the polymerizable composition. When water is used, an anion substitution treatment described below may be performed in combination.
[0102] The ion exchange membrane obtained by the above method may be subjected to a drying treatment. In the drying treatment, the drying temperature is, for example, from 40° C. to 90° C., and the drying time is, for example, from 3 hours to 24 hours.
[0103] The ion exchange membrane obtained by the above method may be subjected to an anion substitution treatment. This allows the anion of the quaternary ammonium group of the ion exchange resin to be substituted with another type of anion. When the anion of the quaternary ammonium group is triflate or bistrifluoromethanesulfonimide, the anion can be substituted with a halide ion by immersing the ion exchange membrane in an aqueous solution containing a halogen compound such as a hydrogen chloride solution or a hydrogen bromide solution for a certain period of time. When the anion of the quaternary ammonium group is a halide ion, the anion can be substituted with a hydroxide ion by immersing the ion exchange membrane in an alkali metal hydroxide solution such as a sodium hydroxide solution for a certain period of time. When the anion of the quaternary ammonium group is a hydroxide ion, the anion can be substituted with a carbonate ion or a bicarbonate ion by immersing the ion exchange membrane in a carbonate solution such as a potassium carbonate solution or a sodium bicarbonate solution for a certain period of time. Alternatively, the anion can be substituted with a carbonate ion or a bicarbonate ion by exposing an ion exchange membrane in which the anion of the quaternary ammonium group is a hydroxide ion to the atmosphere for a certain period of time.
[0104] [Membrane electrode assembly] The membrane electrode assembly according to the embodiment includes an ion exchange membrane according to the embodiment and an electrode. In the membrane electrode assembly (MEA), the ion exchange membrane and the electrode are integrated. The electrode may include a first electrode that is a cathode and a second electrode that is an anode. The membrane electrode assembly may have an ion exchange membrane interposed between the first electrode and the second electrode.
[0105] The membrane electrode assembly according to the embodiment can be used for hydrogen production devices, water electrolysis devices, fuel cells, and the like.
[0106] The electrode may include a metal catalyst and, optionally, an ion conductive agent, a conductive agent, and a binder. The proportions of the metal catalyst, the ion conductive agent, the conductive agent, and the binder in the electrode are, for example, 50% by mass or more and 99% by mass or less, 0.1% by mass or more and 30% by mass or less, 0.1% by mass or more and 30% by mass or less, and 0.1% by mass or more and 30% by mass or less, respectively.
[0107] The metal catalyst promotes the oxidation or reduction reaction. The metal catalyst is typically in the form of particles. Examples of the metal catalyst include platinum, gold, silver, palladium, iridium, rhodium, ruthenium, tin, iron, cobalt, nickel, manganese, molybdenum, tungsten, vanadium, chromium, tantalum, zirconium, aluminum, zinc, oxides or hydroxides thereof, or alloys thereof. The metal catalyst for the anode preferably includes nickel. The metal catalyst for the cathode preferably includes platinum, gold, silver, palladium, iridium, rhodium, ruthenium, tin, iron, cobalt, nickel, manganese, or alloys thereof.
[0108] The ion conductive agent enhances the ion conductivity of the electrode. Examples of the ion conductive agent include perfluorocarbon polymers, aromatic polyether ether ketones, and polysulfones having basic functional groups. An ion exchange resin may be used as the ion conductive agent. The ion exchange resin may be the ion exchange resin according to the embodiment, or another ion exchange resin may be used. As the other ion exchange resin, for example, an ion exchange resin having an imidazole group is used.
[0109] The conductive agent enhances the electronic conductivity of the electrode. The conductive agent may be used as a support for a metal catalyst. Examples of the conductive agent include carbon black, activated carbon, graphite, fullerene, carbon nanotubes, and mixtures thereof.
[0110] The binder increases the rigidity of the electrode. Examples of the binder that can be used include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, and mixtures thereof.
[0111] The membrane electrode assembly is produced, for example, by the following method.
[0112] First, the ion exchange membrane according to the embodiment is prepared by the method described above. The ion exchange membrane may be in a wet state, but is preferably in a dry state.
[0113] Next, the metal catalyst is mixed with, optionally, an ion conductive agent, a conductive agent, a binder, and an organic solvent to prepare a composition for forming a first electrode. This composition for forming a first electrode is applied, for example, onto a release paper to obtain a first coating film. This first coating film is dried. The dried first coating film is peeled off from the release paper and laminated on one of the main surfaces of the ion exchange membrane. An ion conductive agent may be applied onto one of the main surfaces of the ion exchange membrane. The composition for forming a first electrode may be directly applied onto one of the main surfaces of the ion exchange membrane to form the first coating film.
[0114] Next, the metal catalyst is mixed with, optionally, an ion conductive agent, a conductive agent, a binder, and an organic solvent to prepare a composition for forming a second electrode. This composition for forming a second electrode is applied, for example, onto a release paper to obtain a second coating film. This second coating film is dried. The dried second coating film is peeled off from the release paper and laminated on the other main surface of the ion exchange membrane. An ion conductive agent may be applied to the other main surface of the ion exchange membrane. The composition for forming a first electrode may be directly applied onto the other main surface of the ion exchange membrane to form a second coating film. Alternatively, the first coating film may be formed after the formation of the second coating film.
[0115] The obtained laminate is subjected to heating, pressure, or both to integrate the first coating film and the second coating film with the ion exchange membrane. In this manner, a membrane electrode assembly is obtained in which the first electrode, the ion exchange membrane, and the second electrode are laminated in this order. Note that the first electrode or the second electrode may be omitted.
[0116] [Hydrogen production equipment] The hydrogen production device according to the embodiment includes the ion exchange membrane according to the embodiment. The hydrogen production device may include the membrane electrode assembly according to the embodiment.
[0117] The hydrogen production device according to the embodiment includes the ion exchange membrane according to the embodiment, and therefore can efficiently split water.
[0118] Hereinafter, a hydrogen production device including a membrane electrode assembly according to an embodiment will be described in detail with reference to FIG.
[0119] Fig. 1 is a cross-sectional view showing an example of a hydrogen production device according to an embodiment. The hydrogen production device 1 shown in Fig. 1 includes a membrane electrode assembly 4, and a first electrode chamber 2 and a second electrode chamber 3 separated by the membrane electrode assembly 4.
[0120] The membrane electrode assembly 4 includes an anion exchange membrane 5, a first electrode 6 supported on one main surface of the anion exchange membrane 5, and a second electrode 7 supported on the other main surface of the anion exchange membrane. The first electrode 6 and the second electrode 7 are connected to a power source via a conductor (not shown). A gas diffusion layer may be provided on the surface of the first electrode and the second electrode. As the gas diffusion layer, for example, carbon paper, carbon cloth, nickel foam, titanium foam, porous graphite, etc. are used.
[0121] The first electrode chamber 2 is provided with a first electrode 6, and is connected to a hydrogen exhaust pipe 8. The hydrogen exhaust pipe 8 is connected to a hydrogen tank (not shown). The first electrode chamber 2 may be provided with a first partition wall (not shown). The first partition wall is provided with a plurality of grooves connecting to the first electrode chamber 2, and a hydrogen exhaust passage connected to these grooves and the hydrogen exhaust pipe 8. The first partition wall is preferably made of an electronically conductive material. For example, a metal plate is used for the first partition wall. The first partition wall may be in contact with the gas diffusion layer described above.
[0122] The second electrode chamber 3 is provided with a second electrode 7, and is connected to an oxygen exhaust pipe 9 and a water supply pipe 10. The oxygen exhaust pipe 9 is connected to an oxygen tank (not shown). The water supply pipe 10 is connected to a water supply device (not shown). The second electrode chamber 3 may be provided with a second partition wall (not shown). The second partition wall is provided with a plurality of grooves connecting to the second electrode chamber 3, and oxygen exhaust channels connected to these grooves, the oxygen exhaust pipe 9, and the water supply pipe 10. The second partition wall is preferably made of an electronically conductive material. For example, a metal plate is used for the second partition wall. The second partition wall may be in contact with the above-mentioned gas diffusion layer.
[0123] Next, a hydrogen production method using the hydrogen production device according to the embodiment will be described in detail with reference to FIG.
[0124] First, the liquid to be treated is supplied to the second electrode chamber 3 via the water supply pipe 10. The liquid to be treated may be water or an alkaline aqueous solution. The alkaline aqueous solution is, for example, an aqueous solution of an alkali metal hydroxide, carbonate, or bicarbonate. The pH of the alkaline aqueous solution is, for example, 10 or more and 14 or less. The concentration of the alkaline aqueous solution is, for example, 0.1 mass % or more and 30 mass % or less.
[0125] The liquid to be treated that has come into contact with the membrane electrode assembly 4 is held in the anion exchange membrane 5. That is, the liquid to be treated is supplied to the first electrode chamber 2 via the anion exchange membrane 5.
[0126] Next, power is supplied from a power source (not shown) to the first electrode 6 and the second electrode 7. As a result, water (H2O) is decomposed at the first electrode 6 to hydrogen (H2) and hydroxide ions (OH - The generated hydroxide ions are supplied to the second electrode 7 through the anion exchange membrane 5. The supplied hydroxide ions are decomposed and synthesized into oxygen (O2) and water (HO) at the second electrode 7, as shown in the following formula (B).
[0127] 2H2O+2e - → H2+2OH - (A) 2OH - → 1 / 2O2+H2O+2e - (B) The hydrogen gas produced in the first electrode chamber 2 is supplied to a hydrogen tank via a hydrogen discharge pipe 8. The oxygen gas produced in the second electrode chamber 3 is supplied to an oxygen tank via an oxygen discharge pipe 9. EXAMPLES
[0128] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0129] <Preparation of Polymerizable Composition> Example 1 A polymerizable composition was obtained by mixing 6 g of vinylbenzyltrimethylammonium chloride, 0.37 g of a polymerizable monomer, 3.15 g of an organic solvent, 0.2 equivalents of a nitrogen-containing compound, 0.09 g of a photopolymerization initiator, 0.05 g of a thermal polymerization initiator, and 0.0015 g of a polymerization inhibitor at room temperature and normal pressure. Divinylbenzene was used as the polymerizable monomer. Ethylene glycol was used as the organic solvent. 0.36 g of N,N-dimethylpropyleneurea (DMPU) was used as the nitrogen-containing compound. 1-phenyl-2-hydroxy-2-methylpropan-1-one was used as the photopolymerization initiator. tert-butyl peroxyoctoate was used as the thermal polymerization initiator. 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl was used as the polymerization inhibitor.
[0130] (Examples 2 to 8, Comparative Examples 1 to 19) As shown in Table 1, polymerizable compositions were prepared in the same manner as in Example 1, except that the types of additives were changed.
[0131] <Evaluation test> (phase separation) The polymerizable compositions obtained in the Examples and Comparative Examples were visually observed for phase separation. Specifically, 10 g of the polymerizable composition in a screw tube was stirred for 300 seconds, and then, if phase separation was observed visually after 10 minutes, it was marked as "present," and if no phase separation was observed, it was marked as "absent."
[0132] (Polymerizable) The polymerizability of the polymerizable compositions obtained in the examples and comparative examples was confirmed. Specifically, when an ion exchange membrane was produced by the method of Example 9, the polymerizability was judged to be "good" when the membrane surface was uniformly transparent. On the other hand, the polymerizability was judged to be "poor" when part of the membrane surface was cloudy.
[0133] [Table 1]
[0134] [Table 2]
[0135] <Ion exchange membrane manufacturing> Example 9 First, a substrate was prepared. A polyethylene film having a thickness of 25 μm and a porosity of 42% was used as the substrate.
[0136] This substrate was immersed in the polymerizable composition of Example 1, and then pulled out from the polymerizable composition. In this way, a first structure in which the polymerizable composition was supported on the substrate was obtained. Both main surfaces of this first structure were covered with PET films. One of the main surfaces of the first structure was irradiated with ultraviolet light using an LED to obtain a second structure. The irradiation wavelength was 365 nm, and the irradiation intensity was 100 mW / cm. 2 The irradiation time was 1 min.
[0137] Next, the second structure was placed in a heat dryer and subjected to a heat treatment. The heating temperature was set to 120°C so that the surface temperature of the membrane was about 110°C, and the heating time was set to 15 minutes. The PET film was peeled off from the second structure after heating to obtain an ion exchange membrane.
[0138] (Examples 10 to 13) An ion exchange membrane was produced in the same manner as in Example 9, except that the polymerizable composition shown in Table 3 was used.
[0139] <Performance evaluation> (film thickness measurement) The thickness of the ion exchange membranes obtained in the examples and comparative examples was measured. Specifically, the measurement was performed using ID-H0530 manufactured by Mitutoyo Corporation.
[0140] (Measurement of ion exchange capacity and water content) The anion exchange capacity (IEC) and water content of the ion exchange membranes obtained in the examples and comparative examples were measured.
[0141] Specifically, first, the ion exchange membrane was immersed in a 0.2 mol / L NaNO3 aqueous solution for 10 hours or more to replace the counter ion from chloride ion to nitrate ion. Note that, for the ion exchange membranes according to Examples 19 to 22, the counter ion was replaced with chloride ion prior to the conversion to nitrate ion. The replacement with chloride ion was performed by immersing the ion exchange membrane in a 0.5 mol / L HCl aqueous solution for 10 hours or more.
[0142] The amount of chloride ions liberated during the replacement with nitrate ions was measured using a potentiometric titrator with an aqueous silver nitrate solution. The value obtained was designated as A (mol). The potentiometric titrator used was a COMTITE-900 made by Hiranuma Sangyo Co., Ltd.
[0143] Next, the ion exchange membrane was immersed in a 1 mol / L HCl aqueous solution for 4 hours or more. After the immersion, the ion exchange membrane was thoroughly washed with ion exchange water, the moisture on the surface was wiped off, and the weight of the ion exchange membrane was measured. The obtained value was designated as W (g). This ion exchange membrane was dried under reduced pressure at 60°C for 5 hours, and the weight after drying was measured. The obtained value was designated as D (g). Based on the amount of liberated chloride ions (A) and the weight of the ion exchange membrane after drying (D), the anion exchange capacity of the ion exchange membrane was calculated by the following formula.
[0144] Anion exchange capacity [mmol / g-dry weight] = A x 1000 / D In addition, based on the weight (W) of the ion exchange membrane when wet and the weight (D) of the ion exchange membrane after drying, the water content of the ion exchange membrane was calculated by the following formula. Moisture content [%]=(WD) / D×100.
[0145] (Membrane resistance measurement) The membrane resistance of the ion exchange membranes obtained in the examples and comparative examples was measured, and the results are shown in Table 2. Specifically, first, the ion exchange membrane was immersed in a 0.5 mol / L NaCl aqueous solution for 30 minutes or more. The ion exchange membrane after immersion was placed in the center of a two-chamber cell equipped with platinum electrodes. Both sides of the ion exchange membrane were filled with a 0.5 mol / L NaCl aqueous solution, and the resistance value between the electrodes at 25°C was measured using an AC bridge (frequency 1000 cycles / second). Next, the resistance value between the electrodes without the ion exchange membrane was measured. The resistance value between the electrodes without the ion exchange membrane was subtracted from the resistance value between the electrodes after the ion exchange membrane was installed. The obtained value was taken as the membrane resistance.
[0146] [Table 3]
[0147] Preferred embodiments are described below. [1] A quaternary ammonium salt represented by the following formula (I), A polymerizable monomer, a linear or branched alkylene glycol having 1 to 4 carbon atoms; A nitrogen-containing compound represented by the following formula (II): A polymerizable composition comprising:
[0148] [ka]
[0149] In the above formula (I), R 1 is an alkenyl group having 2 to 5 carbon atoms, R 2 is an alkylene group having 1 to 10 carbon atoms, R 3 , R 4 , and R 5 each independently represents a linear or branched alkyl group having from 1 to 4 carbon atoms, or a linear or branched alkoxy group having from 1 to 4 carbon atoms, X - is an anion,
[0150] [ka]
[0151] In the above formula (II), R 10 is an alkyl group having 1 to 4 carbon atoms, R 11 is an alkyl group having 1 to 4 carbon atoms, R 12 represents a hydrogen atom, an alkyl group having from 1 to 4 carbon atoms, a secondary amino group having as a substituent an alkyl group having from 1 to 3 carbon atoms, or a tertiary amino group having as a substituent an alkyl group having from 1 to 3 carbon atoms, R 11 and R 12 may be bonded to each other to form a heterocycle, R 10 , R 11 , and R 12 The total number of carbon atoms is 3 or more and 7 or less. [2] The polymerizable composition according to [1], wherein the concentration of the quaternary ammonium salt represented by the formula (I) is 5% by mass or more and 95% by mass or less. [3] The polymerizable composition according to [1] or [2], wherein the concentration of the nitrogen-containing compound represented by the formula (II) is 1% by mass or more and 10% by mass or less. [4] The polymerizable composition according to any one of [1] to [3], wherein a concentration of the alkylene glycol is 1% by mass or more and 50% by mass or less. [5] The polymerizable composition according to any one of [1] to [4], wherein a concentration of the polymerizable monomer is 1% by mass or more and 50% by mass or less. [6] The polymerizable composition according to any one of [1] to [5], wherein the quaternary ammonium salt includes at least one salt selected from the group consisting of (vinylbenzyl)trimethylammonium chloride, (vinylbenzyl)trimethylammonium triflate, and (vinylbenzyl)trimethylammonium bistrifluoromethanesulfonylimide. [7] The polymerizable composition according to any one of [1] to [6], wherein the nitrogen-containing compound represented by formula (II) includes at least one compound selected from the group consisting of N,N-dimethylpropyleneurea, 1-methyl-2-pyrrolidone, N-methyl-2-piperidone, 1,3-dimethyl-2-imidazolidinone, N,N-dimethylacetamide, N,N-diethylformamide, N,N-diethylacetamide, and tetramethylurea. [8] The polymerizable composition according to any one of [1] to [7], wherein the nitrogen-containing compound represented by formula (II) has a flash point of 60° C. or higher. [9] The polymerizable composition according to any one of [1] to [8], wherein the polymerizable monomer includes at least one compound selected from the group consisting of divinylbenzene, 1,2-bis(4-vinylphenylethane, trivinylbenzene, 1,6-bis(4-vinylbenzyloxy)hexane, and N,N-dimethyl-N-(4-vinylbenzyl)-4-(4-vinylphenyl)butane-1-ammonium chloride.
[10] The polymerizable composition according to any one of [1] to [9], wherein a ratio M1 / M2 of a mass M1 of the nitrogen-containing compound represented by the formula (II) to a mass M2 of the alkylene glycol is 0.03 or more and 10 or less.
[11] The polymerizable composition according to any one of [1] to
[10] , further comprising a polymerization initiator.
[12] The polymerizable composition according to
[11] , wherein the polymerization initiator comprises at least one compound selected from the group consisting of benzoyl peroxide, p-chlorobenzoyl peroxide, decanoyl peroxide, lauroyl peroxide, acetyl peroxide, tert-butyl peroxyoctoate, 1-phenyl-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-benzyl-2-(N,N-dimethylamino)-1-(4-morpholinophenyl)butan-1-one, and 2-methyl-1-[4-(methylthio)phenyl]-2-2morpholinopropan-1-one.
[13] An ion exchange resin comprising a cured product of the polymerizable composition according to any one of [1] to
[12] .
[14] An ion exchange membrane comprising the ion exchange resin according to
[13] and a substrate.
[15] A membrane electrode assembly comprising the ion exchange membrane according to
[14] and an electrode.
[16] A hydrogen production device comprising the ion exchange membrane according to
[14] . [Explanation of symbols]
[0152] Reference Signs List 1: hydrogen production device, 2: first electrode chamber, 3: second electrode chamber, 4: membrane electrode assembly, 5: anion exchange membrane 5, 6: first electrode, 7: second electrode, 8: hydrogen exhaust pipe, 9: oxygen exhaust pipe, 10: water supply pipe 10.
Claims
1. A quaternary ammonium salt represented by the following formula (I), A polymerizable monomer, a linear or branched alkylene glycol having 1 to 4 carbon atoms; A nitrogen-containing compound represented by the following formula (II): A polymerizable composition comprising: 【Chemistry 1】 In the above formula (I), R 1 is an alkenyl group having from 2 to 5 carbon atoms, R 2 is an alkylene group having 1 to 10 carbon atoms, R 3 , R 4 , and R 5 each independently represents a linear or branched alkyl group having from 1 to 4 carbon atoms, or a linear or branched alkoxy group having from 1 to 4 carbon atoms, X - is an anion, 【Chemistry 2】 In the above formula (II), R 10 is an alkyl group having 1 to 4 carbon atoms, R 11 is an alkyl group having 1 to 4 carbon atoms, R 12 represents a hydrogen atom, an alkyl group having from 1 to 4 carbon atoms, a secondary amino group having as a substituent an alkyl group having from 1 to 3 carbon atoms, or a tertiary amino group having as a substituent an alkyl group having from 1 to 3 carbon atoms, R 11 and R 12 may be bonded to each other to form a heterocycle, R 10 , R 11 , and R 12 The total number of carbon atoms is 3 or more and 7 or less.
2. The polymerizable composition according to claim 1 , wherein the concentration of the quaternary ammonium salt represented by formula (I) is 5% by mass or more and 95% by mass or less.
3. The polymerizable composition according to claim 1 , wherein the concentration of the nitrogen-containing compound represented by formula (II) is 1% by mass or more and 10% by mass or less.
4. The polymerizable composition according to claim 1 , wherein a concentration of the alkylene glycol is 1% by mass or more and 50% by mass or less.
5. The polymerizable composition according to claim 1 , wherein the concentration of the polymerizable monomer is 1% by mass or more and 50% by mass or less.
6. 2. The polymerizable composition according to claim 1, wherein the quaternary ammonium salt comprises at least one salt selected from the group consisting of (vinylbenzyl)trimethylammonium chloride, (vinylbenzyl)trimethylammonium triflate, and (vinylbenzyl)trimethylammonium bistrifluoromethanesulfonylimide.
7. The polymerizable composition according to claim 1, wherein the nitrogen-containing compound represented by formula (II) comprises at least one compound selected from the group consisting of N,N-dimethylpropyleneurea, 1-methyl-2-pyrrolidone, N-methyl-2-piperidone, 1,3-dimethyl-2-imidazolidinone, N,N-dimethylacetamide, N,N-diethylformamide, N,N-diethylacetamide, and tetramethylurea.
8. The polymerizable composition according to claim 1 , wherein the nitrogen-containing compound represented by formula (II) has a flash point of 60° C. or higher.
9. The polymerizable composition according to claim 1, wherein the polymerizable monomer comprises at least one compound selected from the group consisting of divinylbenzene, 1,2-bis(4-vinylphenylethane, trivinylbenzene, 1,6-bis(4-vinylbenzyloxy)hexane, and N,N-dimethyl-N-(4-vinylbenzyl)-4-(4-vinylphenyl)butane-1-ammonium chloride.
10. 2. The polymerizable composition according to claim 1, wherein a ratio M1 / M2 of a mass M1 of the nitrogen-containing compound represented by the formula (II) to a mass M2 of the alkylene glycol is 0.03 or more and 10 or less.
11. The polymerizable composition of claim 1 further comprising a polymerization initiator.
12. The polymerization initiator comprises at least one compound selected from the group consisting of benzoyl peroxide, p-chlorobenzoyl peroxide, decanoyl peroxide, lauroyl peroxide, acetyl peroxide, tert-butyl peroxyoctoate, 1-phenyl-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-benzyl-2-(N,N-dimethylamino)-1-(4-morpholinophenyl)butan-1-one, and 2-methyl-1-[4-(methylthio)phenyl]-2-2morpholinopropan-1-one. The polymerizable composition according to claim 11.
13. An ion exchange resin comprising a cured product of the polymerizable composition according to claim 1.
14. An ion exchange membrane comprising the ion exchange resin according to claim 13 and a substrate.
15. A membrane electrode assembly comprising the ion exchange membrane according to claim 14 and an electrode.
16. A hydrogen production device comprising the ion exchange membrane according to claim 14.
Citation Information
Patent Citations
UV-initiated polymerization of ion-exchange membranes.
JP2022502522A
Method for producing diaphragm for solid polymer fuel cell
WO2011125717A1
Composition for forming polymeric membrane, process for producing same, polymeric membrane, separation membrane module, and ion exchange device
WO2016027595A1
Cited By
Ion exchange membrane, method for manufacturing an ion exchange membrane, membrane electrode assembly, and hydrogen production apparatus
JP7850875B1
Ion exchange membrane, method for producing ion exchange membrane, membrane electrode assembly, and hydrogen production device
WO2026028988A1