Method for manufacturing rolling slide member for evaluating peeling life and method for evaluating peeling life of rolling slide member

The method improves peeling life evaluation accuracy by replacing hydrogen with deuterium in rolling and sliding members through quenching, tempering, and rolling treatments, enabling precise measurement using temperature-programmed desorption.

JP2024167516AInactive Publication Date: 2024-12-04JTEKT CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023083637
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure 2024167516000001_ABST
    Figure 2024167516000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a rolling slide member, which improves accuracy of evaluation of a peeling life, and a method for evaluating the peeling life using the rolling slide member manufactured by the manufacturing method.SOLUTION: This method for manufacturing a rolling slide member comprises: a first step of obtaining a first member containing prescribed retained austenite and a contained hydrogen amount by at least hardening a steel material of the rolling slide member; a second step of obtaining a second member charged with heavy hydrogen; and a third step of obtaining a rolling slide member by processing the second member under a prescribed rolling condition and entering heavy hydrogen as non-diffusible hydrogen in the second member. A method for evaluating the peeling life uses this manufactured rolling slide member for evaluating the peeling life.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a manufacturing method of a rolling sliding member for evaluating a spalling life, and a method of evaluating the spalling life of a rolling sliding member, using a rolling sliding member manufactured by the manufacturing method. [Background technology]

[0002] It is known that hydrogen infiltrates into the steel material constituting a rolling bearing, causing white structure spalling and shortening the spalling life of the rolling bearing. An evaluation method is known in which the amount of hydrogen contained in a rolling bearing is measured using a temperature-programmed desorption method and correlated with the white structure spalling that occurs in the rolling bearing. For example, Patent Document 1 discloses a technique in which hydrogen is charged into a disk-shaped test piece of a thrust ball bearing to artificially infiltrate hydrogen, and then a rolling life test is performed to measure the amount of room-temperature non-diffusible hydrogen contained in the disk-shaped test piece, thereby predicting the possibility of white structure damage occurring depending on the amount of hydrogen. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6683301 Summary of the Invention [Problem to be solved by the invention]

[0004] In evaluating the spalling life of a rolling and sliding component by the thermal desorption method, when a rolling and sliding component in which hydrogen has been artificially charged into the steel material before the evaluation is used as an evaluation sample, it is difficult to distinguish between the hydrogen that has been charged into the steel material before the evaluation and the hydrogen that has entered the steel material during the evaluation.

[0005] In view of the above circumstances, the present invention aims to provide a method for manufacturing a rolling sliding member for evaluating a spalling life in order to improve the accuracy of the evaluation of the spalling life, and a method for evaluating a spalling life using a rolling sliding member manufactured by the manufacturing method. [Means for solving the problem]

[0006] Hereinafter, an outline of an embodiment of the present invention will be described.

[0007] (1) The manufacturing method of the rolling and sliding member for evaluating the spalling life of the present embodiment is as follows: a first step of at least quenching and tempering a steel material of a rolling and sliding member to obtain a first member having a retained austenite content of 60 vol% or less and a hydrogen content of 0.2 ppm or less of the steel material; a second step of charging the first component with deuterium to obtain a second component; The second member is subjected to a maximum contact pressure of 2 GPa to 5 GPa in a contact ellipse in a lubricating oil for 1000 min -1 More than 1500min -1 A third step of obtaining a rolling and sliding member for evaluating the above-mentioned spalling life by treating the rolling element under conditions of a rotational speed of 3×10^6 or more and 8×10^6 or less. Includes.

[0008] The measurement results of deuterium by thermal desorption of the rolling sliding member for evaluating the spalling life obtained by the manufacturing method (1) above (hereinafter sometimes simply referred to as the "evaluation rolling sliding member") show similar measurement results to the measurement results of hydrogen by thermal desorption of the initial rolling sliding member used in the manufacture. That is, according to this manufacturing method, it is possible to obtain an evaluation rolling sliding member in which the hydrogen contained in the initial rolling sliding member is appropriately replaced with deuterium. Therefore, according to this manufacturing method, it is possible to obtain an evaluation rolling sliding member that is suitable for evaluating the spalling life of a rolling sliding member by thermal desorption.

[0009] (2) In the manufacturing method of (1) above, the second step is a step of immersing the first component in a test solution in which 0.1 g to 10.0 g of ammonium thiocyanate is dissolved per L of a heavy water solution of sodium hydroxide having a concentration of 0.01 mol / L to 1.00 mol / L, and electrolyzing the test solution under conditions of 1 A / m2 to 100 A / m2 for 12 hours to 48 hours, thereby charging deuterium into the first component to obtain the second component.

[0010] According to the manufacturing method (2) above, the first member is suitably charged with deuterium.

[0011] (3) The method for evaluating the spalling life of the rolling sliding member of this embodiment is a method in which a first rolling sliding member manufactured by the manufacturing method of (1) or (2) above and a second rolling sliding member are brought into relative rolling and sliding contact, and then at least one of the hydrogen amount and the deuterium amount of the first rolling sliding member is measured.

[0012] The evaluation method (3) is a method for evaluating the spalling life by using the first rolling sliding member manufactured by the manufacturing method (1) or (2) above. Therefore, according to this evaluation method, the accuracy of the evaluation of the spalling life of the rolling sliding member is improved.

[0013] (4) In the evaluation method of (3) above, when the first rolling and sliding member and the second rolling and sliding member are brought into relative rolling and sliding contact, it is preferable to interpose an organic compound in which 99.9 mol % or more of the total of hydrogen and deuterium is hydrogen.

[0014] According to the evaluation method of (4) above, the influence of the intrusion of deuterium present in an organic compound intervening in the sliding contact between the first rolling sliding member and the second rolling sliding member into the first rolling sliding member is suppressed, and therefore, according to this evaluation method, the accuracy of the evaluation of the spalling life of the rolling sliding member is further improved.

[0015] (5) In the evaluation method of (3) or (4) above, when the first rolling and sliding member and the second rolling and sliding member are brought into relative rolling and sliding contact, it is preferable to interpose water which is 99.9 mol % or more hydrogen relative to the total of hydrogen and deuterium.

[0016] According to the evaluation method of (5) above, the influence of the intrusion of deuterium present in water, which is present in the sliding contact between the first rolling sliding member and the second rolling sliding member, into the first rolling sliding member is suppressed, and therefore, according to this evaluation method, the accuracy of the evaluation of the spalling life of the rolling sliding member is further improved. Effect of the Invention

[0017] According to the present invention, it is possible to provide a method for manufacturing an evaluation rolling and sliding member for improving the accuracy of evaluation of spallation life, and a method for evaluating spallation life using an evaluation rolling and sliding member. [Brief description of the drawings]

[0018] [Figure 1] 4 is a flowchart showing the steps of a manufacturing method for a rolling sliding member for evaluating a spalling life according to an embodiment. [Diagram 2] FIG. 2 is a schematic diagram of a hydrogen charging device used for cathodic hydrogen charging in the second step. [Diagram 3] FIG. 4 is a schematic diagram of a rolling device used in the rolling treatment of the third step. [Figure 4] 1 is a graph showing hydrogen release curves, measured by a temperature programmed desorption method, of a quenched and tempered member after hydrogen charging and a base member. [Diagram 5] 1 is a graph showing hydrogen release curves, measured by a thermal desorption method, of a deuterium-charged member and a base member after rolling treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0020] <Manufacturing method> 1 is a flow chart showing the steps of a method for manufacturing an evaluation rolling and sliding member according to an embodiment of the present invention, which includes a first step S1 of performing a quenching and tempering treatment, a second step S2 of performing a deuterium charging treatment, and a third step S3 of performing a rolling treatment.

[0021] [First step S1] The first step S1 is a step of performing at least quenching and tempering on a rolling sliding member (hereinafter sometimes simply referred to as a "base member") that is the basis of the evaluation rolling sliding member, to obtain a rolling sliding member (hereinafter sometimes simply referred to as a "first member") in which the residual austenite contained in the steel is 60 vol% or less and the hydrogen content is 0.2 ppm or less. The first step S1 may include treatments other than quenching and tempering as long as it is possible to obtain a first member in which the residual austenite and the hydrogen content are the above-mentioned predetermined contents. Annealing, normalizing, and cutting may be performed before quenching and tempering. Quenching may include subzero.

[0022] The quenching and tempering treatment in the first step S1 may be performed by a known method and is not particularly limited. For example, quenching and tempering treatment according to the Japanese Industrial Standard B6913:1999 may be performed. For example, when the base member is JIS SUJ2, the base member is treated at a temperature of 800°C to 900°C and for 1 hour to 3 hours, and then quenched by immediately immersing in quenching oil with an oil temperature of 80°C or less. After quenching, the base member is tempered at a temperature of 100°C to 220°C and for 0.5 hours to 2 hours. The base member becomes a first member in which the residual austenite contained in the steel material is 15 vol% or less and the hydrogen content is 0.2 ppm or less by quenching and tempering.

[0023] The amount of retained austenite contained in the first member is preferably 60 vol% or less, particularly 5 vol% or less. If the amount of retained austenite is 60 vol% or less, the structure of the steel material of the first member is stable. If the amount of retained austenite is 5 vol% or less, the structure of the steel material of the first member is even more stable. Furthermore, the preferred steel material is JIS SUJ2, and in this case, the preferred amount of retained austenite is 15 vol% or less.

[0024] The hydrogen content of the first member is preferably 0.2 ppm or less, particularly 0.1 ppm or less. If the hydrogen content of the first member is 0.2 ppm or less, the hydrogen contained in the steel material of the base member from the beginning (hereinafter, may be simply referred to as "initial hydrogen") is one-fifth or less of the deuterium diffused in the second step S2 described later. In other words, the initial hydrogen is sufficiently removed from the steel material of the evaluation rolling and sliding member obtained. This reduces the influence of the initial hydrogen in the evaluation of the spalling life using the evaluation rolling and sliding member. As a result, the accuracy of the evaluation result of the spalling life by the evaluation rolling and sliding member is improved. If the hydrogen content is 0.1 ppm or less, the initial hydrogen contained in the evaluation rolling and sliding member is further removed. This further improves the accuracy of the evaluation result of the spalling life by the evaluation rolling and sliding member.

[0025] The retained austenite in the first member can be measured using a known method. The retained austenite in the first member can be determined, for example, by calculating the ratio of α phase (martensite) to γ ​​phase (austenite) on the surface of the first member using an X-ray diffraction method. The hydrogen content in the first member can be measured using a known method. The hydrogen content in the first member can be determined, for example, by a temperature programmed desorption method, by heating the first member and measuring the hydrogen desorbed therefrom.

[0026] The conditions for quenching and tempering in the first step S1 include a plurality of different conditions for quenching and tempering the base member. The residual austenite and hydrogen content of the first member quenched and tempered under each of the conditions are measured in advance. The above-mentioned preliminary measurements are used to determine the quenching and tempering conditions under which the residual austenite is 60 vol% or less and the hydrogen content is 0.2 ppm or less, and these quenching and tempering conditions are set as the quenching and tempering conditions in the first step S1.

[0027] [Second process S2] The second step S2 is a step of obtaining a second member by charging the first member with deuterium through cathodic hydrogen charging. More specifically, the first member to be the cathode and the anode are immersed in a sodium hydroxide heavy water solution containing ammonium thiocyanate (hereinafter, sometimes simply referred to as a "test solution"), and the heavy water is electrolyzed. As a result, the first member is exposed to deuterium, and the first member is charged with deuterium.

[0028] FIG. 2 is a schematic diagram of a hydrogen charging device 10 used for cathodic hydrogen charging in the second step S2. The hydrogen charging device 10 has a power source 11, an anode 12, a test solution tank 13, a water tank 14, and a heater 15. A first member 20 is connected to the power source 11 as a cathode. The test solution tank 13 is a container that holds the test solution TS. The anode 12 and the first member 20 are immersed in the test solution TS held by the test solution tank 13. The water tank 14 has a size that can receive the test solution tank 13 therein. The heater 15 can heat the water WT in the water tank 14. The test solution TS in the test solution tank 13 is indirectly heated by heating the water WT in the water tank 14 by the heater 15.

[0029] The test solution TS is a solution in which 0.1 g to 10.0 g of ammonium thiocyanate is dissolved per 1 L of sodium hydroxide deuterium oxide solution of 0.01 mol / L to 1.00 mol / L. If the concentration of sodium hydroxide in deuterium oxide in the test solution TS is 0.01 mol / L or more, the first member is sufficiently exposed to deuterium by electrolysis of the test solution TS. This effectively charges the first member 20 with deuterium. If the concentration of sodium hydroxide in deuterium oxide is 1.00 mol / L or less, it is sufficient. If the amount of ammonium thiocyanate contained in 1 L of sodium hydroxide deuterium oxide solution is 0.1 g or more, charging of deuterium to the first member is promoted. This effectively charges the first member 20 with deuterium. If the amount of ammonium thiocyanate is 10.0 g or less, it is sufficient.

[0030] The electrolysis in the second step S2 is performed at 1 A / m 2 More than 100A / m 2 The electrolysis is performed under the following conditions for 12 hours to 48 hours. The electrolysis conditions can be set by adjusting the current and time flowing through the anode 12 immersed in the test solution TS and the first member 20, which is the cathode, using the power source 11. The current density of the electrolysis is 1 A / m 2 If the current density is 100 A / m or more, the first member 20 is sufficiently exposed to deuterium by electrolysis of the test solution TS. This allows the first member 20 to be effectively charged with deuterium. 2 If the electrolysis time is 12 hours or more, the first member 20 is sufficiently exposed to deuterium by electrolysis of the test solution TS, thereby effectively charging the first member 20 with deuterium. If the electrolysis time is 48 hours or less, the occurrence of the above-mentioned fracture is suppressed, and the productivity of the evaluation rolling and sliding member obtained in the third step S3 described below is improved.

[0031] [Third process S3] The third step S3 is a step of rolling the second member charged with deuterium to cause the deuterium to penetrate into the second member as non-diffusible hydrogen, and obtaining a rolling and sliding member for evaluation. More specifically, the second member is treated in a lubricant under conditions of a predetermined contact surface pressure, rotational speed, and rolling number to cause the deuterium to penetrate into the second member, and the rolling and sliding member for evaluation is obtained.

[0032] The lubricant used in the third step S3 may be a commercially available lubricant, and is not particularly limited. Examples of the lubricant include machine oil and spindle oil. The rolling process may be performed using a rolling bearing made using the second member. The rolling bearing made in the rolling process may be one to which the second member is applied, and is not particularly limited. Examples of the rolling bearing to which the second member is applied include ball bearings, roller bearings, and thrust bearings. The rolling element is a rolling element used in the rolling bearing to which the second member is applied, and examples of the rolling element include balls and rollers. The evaluation rolling sliding member obtained in the third step S3 is the rolling sliding member of the rolling bearing to which the second member is applied. For example, when the rolling bearing is a ball bearing or a roller bearing, the evaluation rolling sliding member is an inner ring or an outer ring. When the rolling bearing is a thrust bearing, the evaluation rolling sliding member is a raceway.

[0033] FIG. 3 is a schematic diagram of a rolling device 30 used in the rolling process of the third step S3. The rolling device 30 is used when the second member is a race of a thrust bearing. The rolling device 30 has a shaft 31, a mounting table 32, a housing 33, a load ball 34, and a load application unit 35. A thrust bearing 40 that is the target of the rolling process by the rolling device 30 has a first race (housing race) 41, a second race (shaft race) 42, balls 43, and a cage 44. In FIG. 3, the first race 41 is the second member (hereinafter, may be referred to as the "second member 41"). The balls 43 roll on a raceway surface OP of the second member 41. The second member 41 may be a flat plate instead of a housing race.

[0034] The mounting base 32 is disposed within the housing 33. The mounting base 32 has a fitting portion 32a into which the second member 41 is fitted. The shaft 31 has a press-fit portion into which the second race 42 is press-fitted (not shown). The second member 41 is fitted into the fitting portion 32a, whereby the second member 41, the balls 43, and the cage 44 are mounted on the mounting base 32. When the second member 41, the balls 43, and the cage 44 are placed on the mounting base 32, the housing 33 stores the lubricating oil SO in an amount such that at least the second member 41 is located in the lubricating oil SO.

[0035] A recess 33a is formed on the bottom surface of the housing 33 at a position intersecting the center line CL. The load ball 34 is fitted into the recess 33a. The load application part 35 applies a load in the direction of the center line CL to the housing 33 via the load ball 34. This causes the load to be applied to the thrust bearing 40. The load that the load application part 35 applies to the load ball 34 is adjusted by a weight (not shown).

[0036] The housing 33 is configured to be movable in the up-down direction indicated by the double-headed arrow in Fig. 3 by the load application unit 35. That is, the second member 41, the balls 43, and the retainer 44 placed on the mounting table 32 can be moved in the up-down direction by the load application unit 35. After the second member 41, the balls 43, and the retainer 44 are placed on the mounting table 32, the load application unit 35 is moved upward, whereby the second race 42 press-fitted onto the shaft 31 comes into contact with the balls 43 placed on the mounting table 32. This places the thrust bearing 40 between the shaft 31 and the mounting table 32.

[0037] The shaft 31 is rotated about a center line CL by a motor (not shown). The fitting portion 32a is formed on the mounting table 32 so that when the thrust bearing 40 is mounted on the mounting table 32, the first race 41 and the second member 41 of the thrust bearing 40 are positioned to rotate about the center line CL. Therefore, when the shaft 31 is rotated with the second race 42 and the shaft 31 in contact with each other, the second race 42 rotates. That is, when the shaft 31 rotates, the second race 42 and the second member (first race) 41 rotate relatively, and the second member 41 comes into rolling and sliding contact with the balls 43 relatively.

[0038] In the rolling process of the third step S3, the maximum contact surface pressure in the contact ellipse for the second member 41 is adjusted to be 2 GPa or more and 5 GPa or less. The maximum contact surface pressure in the contact ellipse is the maximum value of the surface pressure on the contact surface between the raceway surface OP of the second member 41 and the balls 43. Here, if the contact surface pressure is 2 GPa or more and 5 GPa or less, the deuterium of the second member 41 penetrates into the retained austenite. That is, the deuterium penetrates into the second member 41 as non-diffusible hydrogen.

[0039] In the rolling process of the third step S3, the rotation speed of the shaft 31 is 1000 min -1 More than 1500min -1 The rotation speed is adjusted to 1000 min -1 That's it, 1500min -1 If it is below this level, deuterium in the second member 41 penetrates into the retained austenite.

[0040] In the rolling process of the third step S3, the rolling number of the balls 43 is adjusted to be 3×10^6 or more and 8×10^6 or less. Here, if the rolling number is 3×10^6 or more and 8×10^6 or less, the deuterium of the second member 41 penetrates into the retained austenite.

[0041] <Evaluation method> In the evaluation rolling and sliding member obtained by the above-mentioned manufacturing method, hydrogen contained in the base member is appropriately replaced with deuterium. Therefore, the evaluation of the spalling life of the rolling and sliding member by the temperature-programmed desorption method using the evaluation rolling and sliding member is more accurate. In the evaluation method of the present embodiment of the evaluation of the spalling life of the rolling and sliding member by the temperature-programmed desorption method using the evaluation rolling and sliding member (hereinafter, sometimes simply referred to as "this evaluation method"), a known evaluation method of spalling life can be applied, except for using the evaluation rolling and sliding member.

[0042] This evaluation method uses a rolling bearing having an evaluation rolling sliding member manufactured by the above-mentioned manufacturing method. The rolling bearing after the above-mentioned third step S3 is used as an evaluation sample for evaluating the spalling life. Below, this evaluation method will be described in which the thrust bearing 40 after the above-mentioned third step S3 is used as the evaluation sample. Note that the first race 41 of the thrust bearing 40 after the above-mentioned third step S3 is the evaluation rolling sliding member.

[0043] As an evaluation device used in this evaluation method, for example, a rolling device 30 shown in FIG. 3 can be applied. When the rolling device 30 is applied as the evaluation device, the relative rolling and sliding contact conditions between the evaluation rolling and sliding member, which is the first race 41, and the balls 43 can be changed. Therefore, this evaluation method can be performed under various rolling and sliding contact conditions. For example, the effect of the load on the spalling life is evaluated by adjusting the load applied to the thrust bearing 40. In addition, the effect of the intervening components, such as water and organic compounds, on the spalling life is evaluated by storing the intervening components in the housing 33. In addition, the effect of the rotation speed of the rolling bearing and the rotation speed of the rolling elements is evaluated by adjusting the rotation conditions of the shaft 31.

[0044] The water or organic compound used in this evaluation method is preferably water or an organic compound in which hydrogen is 99.9 mol % or more of the total of hydrogen and deuterium. This suppresses the influence of deuterium from the water or organic compound, which is an intermediate component, penetrating into the evaluation rolling and sliding member. Therefore, the accuracy of the evaluation result of the spalling life obtained by this evaluation method is improved. In addition, examples of organic compounds include lubricants such as grease, and additives to the lubricants. EXAMPLES

[0045] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0046] <Base member> The housing race of the thrust bearing 51305 manufactured by JTEKT Corporation was used as the base material for the rolling and sliding member. The housing race was manufactured using JIS SUJ2.

[0047] <Temperature Programmed Desorption Method> The amounts of hydrogen and deuterium released at a heating temperature of 500° C. or less were measured using a thermal desorption analyzer (manufactured by Electro Scientific Co., Ltd., product name IH-TDS1700) according to the instruction manual.

[0048] <Quenching and tempering treatment> The base material was quenched and tempered in accordance with Japanese Industrial Standard B6913:1999. The quenching was performed by heating in a vacuum furnace at 830°C for 0.5 hours, followed by immediate immersion in quenching oil at 80°C. The tempering was performed at 180°C for 2 hours. It was confirmed that the member obtained by the quenching and tempering process (hereinafter sometimes simply referred to as the "quenched and tempered member") had a retained austenite content of 10 vol% and a hydrogen content of 0.03 ppm. The retained austenite was measured by X-ray diffraction. The hydrogen content was measured by thermal desorption.

[0049] <Hydrogen charging> Charging of hydrogen or deuterium into the quenched and tempered members was performed using the hydrogen charging device 10 shown in FIG. 2 with the quenched and tempered members as the cathode. The test solution TS for charging hydrogen was a solution in which 1 g of ammonium thiocyanate was dissolved per 1 L of 0.1 mol / L aqueous sodium hydroxide solution. The test solution TS for charging deuterium was a solution in which 1 g of ammonium thiocyanate was dissolved per 1 L of 0.1 mol / L aqueous sodium hydroxide solution. Electrolysis was performed at 10 A / m 2 It was held for 24 hours.

[0050] <Rolling process> A thrust bearing having a raceway made of a quenched and tempered member after deuterium charging (hereinafter sometimes simply referred to as a "deuterium-charged member") was subjected to rolling treatment under the following conditions using the rolling device 30 shown in Figure 3 described above. (Rolling treatment conditions) Maximum contact pressure in contact ellipse: 2.7GPa Rotation speed: 1200min -1 Number of revolutions of the rolling element: 3×10^6

[0051] <Measurement of hydrogen content by thermal desorption method for rolling and sliding components after hydrogen charging> FIG. 4 is a graph showing the hydrogen release curves of a quenched and tempered member after hydrogen charging (hereinafter, sometimes simply referred to as a "hydrogen-charged member") and a base member, measured by a temperature-programmed desorption method. The hydrogen content of the hydrogen-charged member was 1.40 ppm. The hydrogen content of the base member was 0.24 ppm. As shown in FIG. 4, the hydrogen release curve of the base member has one peak indicating the release of non-diffusible hydrogen. On the other hand, the hydrogen release curve of the hydrogen-charged member has two peaks indicating the release of diffusible hydrogen and non-diffusible hydrogen. Thus, it was revealed that the hydrogen-charged member and the base member have different hydrogen content and hydrogen release curves. This shows that the evaluation of the spalling life of a rolling and sliding member by a temperature-programmed desorption method using a hydrogen-charged member may be less accurate.

[0052] <Measurement of hydrogen content by thermal desorption method for rolling and sliding parts after rolling treatment> FIG. 5 is a graph showing the hydrogen release curves of the deuterium-charged member after rolling treatment (hereinafter, sometimes simply referred to as the "rolling treatment member") and the base member by the temperature-programmed desorption method. The amount of deuterium contained in the rolling treatment member was 0.21 ppm. The amount of hydrogen contained in the base member was 0.26 ppm. Also, as shown in FIG. 5, it can be seen that the hydrogen release curves of the rolling treatment member and the base member have approximately the same non-diffusible hydrogen peak. This shows that the evaluation of the spalling life of the rolling sliding member by the temperature-programmed desorption method using the rolling treatment member is improved in accuracy. The rolling treatment member is a member manufactured based on the manufacturing method of the present invention. Therefore, it was shown that the accurate evaluation of the spalling life by the temperature-programmed desorption method is possible by using the evaluation rolling sliding member manufactured by the manufacturing method of the present invention. [Explanation of symbols]

[0053] 10 Hydrogen charging device 11 Power supply 12 Anode 13 Test solution tank 14 Aquarium 15 Heater 20 First member 30 Rolling device 31 Axis 32 Placement table 32a Mating part 33 Housing 33a Recess 34 Load ball 35 Load application section 40 Thrust bearing 41 First race (second member) 42 Second raceway 43 balls 44 Cage

Claims

1. A first step of at least quenching and tempering a steel material of a rolling and sliding member to obtain a first member having a retained austenite content of 60 vol% or less and a hydrogen content of 0.2 ppm or less of the steel material; a second step of charging the first component with deuterium to obtain a second component; The second member is subjected to a maximum contact surface pressure in a contact ellipse of 2 GPa or more and 5 GPa or less in a lubricating oil for 1000 min. -1 More than 1500min -1 A third step of obtaining a rolling and sliding member by treating the rolling element under conditions in which the rolling element rolls at a rotation speed of 3×10^6 or more and 8×10^6 or less. The manufacturing method of a rolling sliding member for evaluating a spalling life, comprising:

2. 2. The manufacturing method according to claim 1, wherein the second step is a step of immersing the first member in a test solution in which 0.1 g to 10.0 g of ammonium thiocyanate is dissolved per 1 L of a deuterium oxide solution of 0.01 mol / L to 1.00 mol / L, and electrolyzing the test solution under conditions of 1 A / m2 to 100 A / m2 for 12 hours to 48 hours, thereby charging deuterium into the first member to obtain the second member.

3. 3. A method for evaluating the spalling life of a rolling and sliding member, comprising bringing a first rolling and sliding member manufactured by the manufacturing method according to claim 1 or 2 into relative rolling and sliding contact with a second rolling and sliding member, and then measuring at least one of the hydrogen amount and the deuterium amount of the first rolling and sliding member.

4. The evaluation method according to claim 3, wherein when the first rolling and sliding member and the second rolling and sliding member are brought into relative rolling and sliding contact with each other, an organic compound in which 99.9 mol % or more of hydrogen is present relative to the total of hydrogen and deuterium is present between them.

5. 4. The evaluation method according to claim 3, wherein when the first rolling and sliding member and the second rolling and sliding member are brought into relative rolling and sliding contact, water containing hydrogen at a content of 99.9 mol % or more of hydrogen relative to the total content of hydrogen and deuterium is present therebetween.

Citation Information

Patent Citations

  • Method for determining the degree of hydrogen environment and method for predicting the possibility of white structure damage

    JP6683301B1