Toner, toner storage unit, image forming apparatus, and image forming method

The toner with controlled circularity and specific external additives addresses irregular shape issues in conventional toners, ensuring stable charging and improved image quality and cleaning performance.

JP2024167688APending Publication Date: 2024-12-04RICOH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023083928
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

Conventional toners with irregularly shaped particles of low circularity lead to image quality deterioration due to charge fluctuation and cleaning performance issues, resulting in background smudge and poor transferability.

Method used

A toner formulation with toner base particles having an average circularity of 0.850 to 0.950, combined with external additives like barium sulfate, magnesium hydroxide, or magnesium oxide particles of 350 to 1000 nm, ensuring stable charging performance over time.

Benefits of technology

The toner maintains high-quality image formation over a long period with minimal charge fluctuation and improved cleaning performance, reducing background smudge and transfer defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167688000005
    Figure 2024167688000005
  • Figure 2024167688000006
    Figure 2024167688000006
  • Figure 2024167688000007
    Figure 2024167688000007
Patent Text Reader

Abstract

To provide a toner that has less variations in electrification over time, and can form high-quality images for a long period.SOLUTION: A toner includes a toner base particle including a binder resin, a mold release agent, and an electrification control agent, and an external additive. The toner base particles has an average circularity of 0.850 or more and 0.950 or less. The external additive includes inorganic particles of at least one selected from the group consisting of barium sulfate, magnesium hydroxide, and magnesium oxide having an average particle diameter of 350 nm or more and 1000 nm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner, a toner storage unit, an image forming apparatus, and an image forming method. [Background technology]

[0002] Conventionally, in electrophotographic toner, fine particles with an average primary particle size of several nm to several tens of nm are used as external additives to obtain fluidity and charging characteristics. In recent years, toner particles have been made smaller and more spherical in size in response to the diversification, speedup, and higher image quality of the image forming apparatuses. The smaller particle size of the toner improves the reproducibility of a section (dot) of the formed image, and the spherical shape of the toner improves the developability and transferability.

[0003] It is required to uniformly disperse colorants, charge control agents, release agents, etc. in thermoplastic resins. If dispersion is insufficient, the colorants, charge control agents, release agents, etc. added to the toner will become cracked interfaces during the grinding process, and irregularly shaped toner particles with low average circularity will be generated in the ultra-fine powder region with a particle size of 3 μm or less. In addition, problems such as variations in the raw material content contained in the toner particles and an increase in the surface exposure amount of the raw materials will occur when viewed at the level of a single particle. Therefore, the non-uniformity of the toner particles will cause problems such as poor toner charging, poor transport, and even reduced image quality due to background scumming.

[0004] To address the above-mentioned issues, technologies have been proposed to specify the proportion of toner with low average circularity or the abundance ratio of toner particles with different circularity within a certain range, to keep the abundance of toner particles with a diameter of 4 μm or less below a certain value, and to control the toner shape within that particle diameter range (see Patent Documents 1 and 2). Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above-mentioned conventional techniques have the problem that the presence of irregular toner with low circularity reduces image quality (background scumming), and there is also the problem that cleaning properties deteriorate when an attempt is made to increase the level of circularity.

[0006] An object of the present invention is to provide a toner that is less susceptible to charge fluctuation over time and is capable of forming high-quality images over a long period of time. [Means for solving the problem]

[0007] The toner of the present invention as a means for solving the above-mentioned problems is a toner comprising toner base particles including a binder resin, a release agent, and a charge control agent, and an external additive, wherein the average circularity of the toner base particles is 0.850 or more and 0.950 or less, and the external additive comprises at least one type of inorganic particle selected from the group consisting of barium sulfate, magnesium hydroxide, and magnesium oxide, having an average particle diameter of 350 nm or more and 1000 nm or less. Effect of the Invention

[0008] According to the present invention, it is possible to provide a toner which is less susceptible to charge fluctuation over time and is capable of forming high quality images over a long period of time. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram showing an example of a tandem type image forming apparatus of the present invention. [Diagram 2] FIG. 2 is a partially enlarged view of FIG. [Diagram 3] FIG. 3 is a diagram showing an example of a process cartridge as a toner storage unit of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (toner) The toner of the present invention contains toner base particles including a binder resin, a release agent, and a charge control agent, and an external additive, and further contains other components as required. The toner base particles have an average circularity of 0.850 or more and 0.950 or less, and the external additive contains at least one type of inorganic particle selected from barium sulfate, magnesium hydroxide, and magnesium oxide having a size of 350 nm or more and 1000 nm or less. The toner may be referred to as "toner for electrophotography."

[0011] The conventional technology has problems such as a decrease in image quality due to the presence of irregular toner with low circularity (background scumming) and a decrease in cleaning ability when an attempt is made to increase the level of circularity. SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a toner which can ensure sufficient cleaning properties and can provide good image quality with little background scumming.

[0012] The present inventors conducted intensive research to solve the problems of the conventional techniques, and as a result, discovered that a toner can be provided that exhibits sufficient charging performance from the initial stage through aging and is capable of forming high-quality images over a long period of time, by providing a toner that includes toner base particles containing a binder resin, a release agent, and a charge control agent, and an external additive, wherein the average circularity of the toner base particles is 0.850 or more and 0.950 or less, and the external additive includes at least one type of inorganic particle selected from barium sulfate, magnesium hydroxide, and magnesium oxide having a size of 350 nm or more and 1000 nm or less, and thus provides a toner that exhibits sufficient charging performance from the initial stage through aging and is capable of forming high-quality images over a long period of time, and thus completed the present invention.

[0013] <Toner base particles> The toner base particles (hereinafter, sometimes referred to as "toner base") contain a binder resin, a release agent, and a charge control agent, and preferably contain a colorant, and further contain other components as necessary.

[0014] [Average circularity of toner base particles] The average circularity of the toner base particles is from 0.850 to 0.950, and preferably from 0.890 to 0.945. When the average circularity of the toner base particles is 0.950 or less, in a system using blade cleaning or the like, the problem of poor cleaning of the photoconductor and transfer belt, etc., causing stains on the image can be prevented. For example, in development and transfer with a low image area ratio, there is little residual toner after transfer, so poor cleaning does not become a problem, but when the image area ratio is high, such as in a color photo image, or when an untransferred image is formed due to poor paper feed, the toner may be generated as residual toner on the charged body such as the photoconductor, and if accumulated, it may cause background staining of the image. In addition, the charging roller that contacts and charges the charged body such as the photoconductor may be contaminated, and the original charging ability may not be exhibited. When the average circularity of the toner base particles is 0.950 or less, such a problem can be prevented. Furthermore, if the average circularity of the toner base particles is less than 0.850, the transferability deteriorates. This is unlikely to be a problem when the image area ratio is low, but when the image area ratio is high, the transferability deteriorates, causing a large amount of residual toner on the photoreceptor, and the amount of recovered toner increases, resulting in early toner end.

[0015] The average circularity of the toner base particles can be measured, for example, by using a flow particle image analyzer FPIA-3000 (manufactured by Sysmex Corporation). In a specific measurement method, 0.1 to 0.5 mL of a surfactant, preferably an alkylbenzene sulfonate, is added as a dispersant to 100 to 150 mL of water from which solid impurities have been removed in advance in a container, and 0.1 to 0.5 g of toner base particles are further added as a measurement sample. The suspension in which the toner base particles are dispersed is subjected to a dispersion treatment for 1 to 3 minutes with an ultrasonic disperser, and the shape of the toner base particles is measured with the above device with a dispersion concentration of 3,000 particles / μL to 10,000 particles / μL to determine the average circularity.

[0016] <<Binding resin>> The binder resin is not particularly limited and can be appropriately selected from known resins depending on the purpose, and examples thereof include styrene-based resins (homopolymers or copolymers containing styrene or styrene substitutes) such as styrene, poly-α-styrenestyrene, styrene-chlorostyrene copolymer, styrene-propylene copolymer, styrene-butadiene copolymer, styrene-vinyl chloride copolymer, styrene-vinyl acetate copolymer, styrene-maleic acid copolymer, styrene-acrylic acid ester copolymer, styrene-methacrylic acid ester copolymer, styrene-α-methyl chloroacrylate copolymer, and styrene-acrylonitrile-acrylic acid ester copolymer, epoxy resins, vinyl chloride resins, rosin-modified maleic acid resins, phenolic resins, polyethylene resins, polypropylene resins, petroleum resins, polyurethane resins, ketone resins, ethylene-ethyl acrylate copolymers, xylene resins, and polyvinyl butyrate resins. These may be used alone or in combination of two or more. Among these, polyester resins are preferred because they are capable of low-temperature fixing while maintaining high-temperature and high-humidity storage stability.

[0017] The method for producing the binder resin is not particularly limited and may be appropriately selected depending on the purpose. Examples of the method include bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization.

[0018] <<<Polyester resin>>> The polyester resin is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include amorphous polyester resins, modified polyester resins, crystalline polyester resins, etc. These may be used alone or in combination of two or more. Among these, a non-crystalline polyester resin obtained by reacting a polyol with a polycarboxylic acid is preferable.

[0019] Examples of the polyol include diols and trihydric or higher polyols. Examples of the diol include glycols such as ethylene glycol, diene glycol, triethylene glycol, and propylene glycol; etherified bisphenols such as 1,4-bis(hydroxymeta)cyclohexane and bisphenol A; alkylene (carbon number 2-3) oxide (average added mole number 1-10) adducts of bisphenol A such as polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane and polyoxyethylene(2.2)-2,2-bis(4-hydroxyphenyl)propane; hydrogenated bisphenol A, and alkylene (carbon number 2-3) oxide (average added mole number 1-10) adducts of hydrogenated bisphenol A. Examples of the trihydric or higher alcohol include glycerin, pentaerythritol, and trimethylolpropane. These may be used alone or in combination of two or more.

[0020] Examples of the polycarboxylic acid include dicarboxylic acids and tri- or higher carboxylic acids. Examples of the dicarboxylic acid include adipic acid, phthalic acid, isophthalic acid, terephthalic acid, fumaric acid, maleic acid, succinic acid, malonic acid, dodecenylsuccinic acid, octylsuccinic acid, and other alkyl groups having 1 to 20 carbon atoms; succinic acid substituted with an alkenyl group having 2 to 20 carbon atoms; and the like.

[0021] Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 1,2,5-benzenetricarboxylic acid, 1,2,4-cyclohexanetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methylenecarboxypropane, 1,2,7,8-octanetetracarboxylic acid, and acid anhydrides thereof. These may be used alone or in combination of two or more.

[0022] The molecular weight of the polyester resin is not particularly limited and may be appropriately selected depending on the purpose, but is preferably within the following range. The weight average molecular weight (Mw) of the polyester resin is preferably from 10,000 to 100,000, and more preferably from 30,000 to 50,000. The peak top molecular weight of the polyester resin is preferably from 10,000 to 60,000, and more preferably from 10,000 to 16,000. The molecular weight can be measured by GPC (gel permeation chromatography).

[0023] The glass transition point (Tg) of the polyester resin is preferably 50° C. or higher and 75° C. or lower, and more preferably 60° C. or higher and 72° C. or lower. When the Tg is 50° C. or higher, the toner has improved heat-resistant storage stability and durability against stress such as stirring in a developing machine, while when the Tg is 75° C. or lower, deformation due to heating and pressure during fixing of the toner is improved, and low-temperature fixing property is improved.

[0024] The content of the polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50 parts by mass or more and 95 parts by mass or less, and more preferably 60 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the toner base particles. When the content is 50 parts by mass or more, the dispersibility of the colorant and the release agent in the toner can be obtained, and fogging and distortion of the image can be suppressed. When the content is 95 parts by mass or less, it is advantageous in terms of high image quality and excellent low-temperature fixing property.

[0025] <<Release agent>> The release agent (wax) is not particularly limited and can be appropriately selected from known ones depending on the purpose, and examples thereof include natural waxes, synthetic waxes, etc. These may be used alone or in combination of two or more kinds.

[0026] Examples of the natural waxes include vegetable waxes such as carnauba wax, cotton wax, and wood wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusin; and petroleum waxes such as paraffin, microcrystalline, and petrolatum.

[0027] Examples of the synthetic wax include synthetic hydrocarbon waxes such as Fischer-Tropsch wax, polyethylene, and polypropylene; fatty acid amide compounds such as esters, ketones, ethers, 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride imide, and chlorinated hydrocarbons; low molecular weight crystalline polymer resins, such as polyacrylate homopolymers and copolymers (e.g., n-stearyl acrylate-ethyl methacrylate copolymers); and crystalline polymers having long alkyl groups in their side chains. Of these, carnauba wax, montan wax and oxidized rice wax are preferred.

[0028] These may be used alone or in combination of two or more. The carnauba wax is preferably microcrystalline, has an acid value of 5 or less, and has a particle size of 1 μm or less when dispersed in a binder resin. The montan wax generally refers to a montan wax refined from minerals, and is preferably microcrystalline and has an acid value of 5 mgKOH / g or more and 14 mgKOH / g or less. The oxidized rice wax is obtained by oxidizing rice bran wax with air, and its acid value is preferably 10-30.

[0029] The content of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 part by mass or more and 20 parts by mass or less, and more preferably 2 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the toner. When the content is 1 part by mass or more, problems such as poor high-temperature offset resistance and poor low-temperature fixability during fixing can be prevented, and when the content is 20 parts by mass or less, problems such as reduced heat-resistant storage stability and image fogging can be prevented.

[0030] <<Charge control agent>> The charge control agent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include nigrosine dyes, metal complex dyes (metal azo dyes), salicylic acid metal complexes, etc. These may be used alone or in combination of two or more. Among these, metal complexes having a trivalent or higher metal capable of forming a 6-coordinate structure are preferred. Examples of the metal include Al, Fe, Cr, and Zr. Among these, metal complexes having non-toxic Fe as the central metal are preferred. Specifically, an azo iron dye represented by the following structural formula (1) is preferred. [ka] In structural formula (1), A + represents an ammonium ion. The azo iron dye represented by structural formula (1) may be a commercially available product, and is available as T-77 (manufactured by Hodogaya Chemical Co., Ltd.).

[0031] The content of the charge control agent is preferably 0.5 parts by mass or more and 3.0 parts by mass or less, and more preferably 0.5 parts by mass or more and 2.0 parts by mass or less, relative to 100 parts by mass of the binder resin. When the content is 0.5 parts by mass or more, the function as a charge control agent is obtained, and when it is 3.0 parts by mass or less, cracking and chipping of the toner can be suppressed, and the occurrence of blade adhesion and photoreceptor filming can be suppressed, and degradation of image quality such as poor charging, poor supply, and background scumming can be suppressed.

[0032] <<Coloring agent>> The colorant is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include carbon black, lamp black, iron black, aniline blue, phthalocyanine blue, phthalocyanine green, Hansa Yellow G, rhodamine 6C lake, chalco oil blue, chrome yellow, quinacridone, benzidine yellow, rose bengal, triarylmethane dyes, etc. These may be used alone or in combination of two or more. By using the above colorant, the toner of the present invention can be used as both a black toner and a full-color toner.

[0033] The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 part by mass or more and 35 parts by mass or less, and more preferably 3 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the toner.

[0034] <External additives> The external additive contains inorganic particles having a size of 350 nm or more and 1000 nm or less selected from barium sulfate, magnesium hydroxide, and magnesium oxide, and further contains other external additives as necessary.

[0035] <<Inorganic particles>> The inorganic particles are selected from barium sulfate, magnesium hydroxide, and magnesium oxide. All of these materials have positive charging properties, and among them, barium sulfate has the highest charging ability, including resistance to environmental changes.

[0036] The average particle size of the inorganic particles is from 350 nm to 1000 nm, and preferably from 500 nm to 800 nm. If the average particle size is smaller than 350 nm, the barium sulfate particles are embedded in the toner surface, and lose the opportunity to acquire charge when the barium sulfate is released from the toner base particle surface over time, resulting in a decrease in charge. If the average particle size is more than 1000 nm, the toner base particles lose the opportunity to be triboelectrically charged with each other, leading to a decrease in charge.

[0037] The average particle size of the inorganic particles can be measured by a known method. Specifically, a scanning electron microscope SU8200 series (Hitachi High-Technologies Corporation) is used to measure inorganic particles or toner to which the inorganic particles are added. The obtained image is processed by image processing software A-zo-kun (Asahi Kasei Engineering Co., Ltd.) to recognize the additive particles by binarization or the like, and the circularity, circle-equivalent diameter, and particle area are calculated. The circle-equivalent diameter is calculated by assuming that the value obtained above is based on the circular area, and is converted to a diameter value. In the case of inorganic particles, the substrate on which the particles are dispersed is measured, and in the case of toner measurements, if the toner surface is measured, there is no designated area for observation, but three or more arbitrary points in the field of view are confirmed, and the circle-equivalent diameters of about 100 particles are calculated, and the average value is determined as the average particle diameter.

[0038] <<Hydrophobic treated polymethylsilsesquioxane particles>> Polymethylsilsesquioxane is a polymer of methyltrimethoxysilane. The polymethylsilsesquioxane is a silicone resin in which methyltrimethoxysilane is crosslinked and polymerized in a three-dimensional network structure, and is a spherical fine particle. Therefore, it is called "polymethylsilsesquioxane particles". The hydrophobized polymethylsilsesquioxane particles can be obtained by subjecting polymethylsilsesquioxane particles to a hydrophobization treatment.

[0039] The average particle size of the polymethylsilsesquioxane particles is from 0.050 μm to 0.150 μm, and preferably from 0.100 μm to 0.135 μm. If the average particle size is larger than 0.150 μm, the adhesion to the toner surface is weak, so that the toner rolls on the toner surface and falls off. The average particle size of the polymethylsilsesquioxane particles can be measured by a known method. Specifically, a scanning electron microscope SU8200 series (Hitachi High-Technologies Corporation) is used to measure polymethylsilsesquioxane particles or toner to which the polymethylsilsesquioxane particles are added. The obtained image is processed by image processing software A-zo-kun (Asahi Kasei Engineering Co., Ltd.) to recognize the additive particles by binarization or the like, and the circularity, circle-equivalent diameter, and particle area are calculated. The circle-equivalent diameter is calculated based on the circle area and converted to a diameter value. In the case of measuring polymethylsilsesquioxane particles, the substrate on which the particles are dispersed is measured, and in the case of measuring toner, if the toner surface is measured, there is no designated area for observation, but three or more arbitrary points in the field of view are confirmed, and the circle-equivalent diameters of about 100 particles are calculated, and the average value is obtained as the average particle diameter.

[0040] [Method of producing polymethylsilsesquioxane particles] The polymethylsilsesquioxane particles can be produced by mixing a hydrolysis solution containing a hydrolysis product of methyltrimethoxysilane and an anionic surfactant with a deposition solution containing water, a base catalyst, and an anionic surfactant, followed by condensation.

[0041] Examples of the anionic surfactant include carboxylate-type anionic surfactants such as aliphatic monocarboxylates, polyoxyethylene alkyl ether carboxylates, and fatty acid oils; sulfonate-type anionic surfactants such as dialkyl sulfosuccinates, polyoxyethylene alkyl sulfosuccinates, alkanesulfonates, linear alkylbenzene sulfonates, branched alkylbenzene sulfonates, naphthalenesulfonate-formaldehyde condensates, and alkylnaphthalenesulfonates; sulfate-type anionic surfactants such as alkyl sulfates, polyoxyalkylene alkyl ether sulfates, and oil and fat sulfates; and phosphate-type anionic surfactants such as alkyl phosphates, alkyl phosphates, polyoxyethylene alkyl ether phosphates, and polyoxyethylene alkylaryl ether phosphates. Among these, sulfonate-type anionic surfactants, sulfate-type anionic surfactants, and sulfate-type anionic surfactants are preferred.

[0042] The hydrolysis liquid preferably further contains an acid catalyst such as an organic acid or an inorganic acid. Examples of the organic acid include formic acid, acetic acid, propionic acid, oxalic acid, citric acid, etc. Examples of the inorganic acid include hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, etc.

[0043] By mixing the hydrolysis liquid with the deposition liquid, a condensation reaction of the silanol groups proceeds, producing polymethylsilsesquioxane particles. Polymethylsilsesquioxane particles can be obtained from the polymethylsilsesquioxane particle dispersion obtained by the above reaction by methods such as membrane separation, centrifugation, etc. Surface treatment with HMDS or the like can be performed in the liquid before separation to impart hydrophobicity.

[0044] The hydrophobized polymethylsilsesquioxane particles can be obtained by subjecting the surfaces of polymethylsilsesquioxane particles to a hydrophobization treatment with a hydrophobization agent. Examples of the hydrophobic treatment agent include known organosilicon compounds having an alkyl group (e.g., a methyl group, an ethyl group, a propyl group, a butyl group, etc.), and specific examples include silazane compounds (e.g., silane compounds such as methyltrimethoxysilane, dimethyldimethoxysilane, trimethylchlorosilane, trimethylmethoxysilane, hexamethyldisilazane, tetramethyldisilazane, etc.) etc. These may be used alone or in combination of two or more.

[0045] Among these, trimethyl group-containing organosilicon compounds such as trimethylmethoxysilane and hexamethyldisilazane are preferred. Other examples include silicone oil treatment. By carrying out hydrophobic treatment, it is possible to suppress the aggregation of particles and improve the dispersibility in the toner matrix. It also suppresses environmental fluctuations such as high temperature and high humidity / low temperature and low humidity, resulting in stable, high image quality.

[0046] The content of the polymethylsilsesquioxane particles is preferably 0.05 parts by mass or more and 3 parts by mass or less relative to 100 parts by mass of the toner. When the content is 3 parts by mass or less, the occurrence of filming can be prevented, and when the content is 0.05 parts by mass or more, it is advantageous in that fluctuations in fluidity and chargeability over a long period of time can be suppressed, and high image quality can be obtained.

[0047] <<Other external additives>> The toner of the present invention contains inorganic particles selected from at least barium sulfate, magnesium hydroxide, and magnesium oxide, and may be combined with other external additives, and two or more kinds of them may be used in combination.

[0048] Examples of other external additives include flow improvers and hydrophobic treatment agents. Examples of the flow improver include silicon oxide, titanium oxide, silicon carbide, aluminum oxide, barium titanate, etc. Among these, hydrophobic silica that has been subjected to a hydrophobic treatment is particularly preferred.

[0049] [Toner manufacturing method] The toner can be produced by a known method including a melt-kneading process of melting and kneading toner materials, a pulverizing process of pulverizing the resulting molten and kneaded material, a classification process of classifying the pulverized material obtained by the pulverization, and an external addition process of externally adding an external additive to the resulting toner base particles.

[0050] In the melt-kneading step, the toner materials are mixed, and the mixture obtained is charged into a melt-kneader and melt-kneaded. As the melt-kneader, for example, a single-screw or twin-screw continuous kneader or a batch-type kneader using a roll mill can be used, and for example, a KTK twin-screw extruder manufactured by Kobe Steel, Ltd., a TEM extruder manufactured by Toshiba Machine Co., Ltd., a twin-screw extruder manufactured by KCK Corporation, a PCM twin-screw extruder manufactured by Ikegai Corporation, a co-kneader manufactured by Buss Co., Ltd., etc. are preferably used. The melt-kneading is preferably carried out under appropriate conditions so as not to cut the molecular chains of the binder resin. Specifically, the melt-kneading temperature is preferably set with reference to the softening point of the binder resin. If the temperature is too high above the softening point, severe cutting may occur, and if the temperature is too low, dispersion may not proceed.

[0051] In the pulverization step, the kneaded product obtained in the melt-kneading step is pulverized. In this pulverization, it is preferable to first coarsely pulverize the kneaded product and then finely pulverize it. Suitable examples of the pulverization method include a method of pulverizing the product by colliding it with a collision plate in a jet stream, a method of pulverizing the product by colliding particles with each other in a jet stream, and a method of pulverizing the product in a narrow gap between a mechanically rotating rotor and a stator.

[0052] In the classification step, the pulverized material obtained in the pulverization step is classified to adjust the particles to a predetermined particle size. Examples of the classification method include a method of removing fine particles using a cyclone, a decanter, a centrifuge, etc. After the pulverization step and the classification step are completed, the pulverized material is classified in an air stream by centrifugal force, etc., to produce toner base particles of a predetermined particle size.

[0053] In the external addition step, an external additive is added to the toner base particles obtained in the classification step. The toner base particles and the external additive are mixed and stirred using a mixer, so that the external additive is coated on the surfaces of the toner base particles while being crushed.

[0054] (Developer) The developer contains at least the toner, and further contains other components such as a carrier, which are appropriately selected as necessary. When the toner of the present invention is used as a developer, it may be used as a one-component developer composed of only the toner, or may be mixed with a carrier to use as a two-component developer, and there is no particular limitation thereon. However, when used in high-speed printers and the like that correspond to the recent improvements in information processing speed, a two-component developer is preferred from the viewpoint of improving the life, etc.

[0055] When the developer is a two-component developer containing the toner of the present invention and a carrier, the carrier may be a magnetic carrier or a non-magnetic carrier depending on the two-component development method.

[0056] Examples of the magnetic carrier include magnetite, spinel ferrites such as gamma iron oxide, spinel ferrites containing one or more metals other than iron (Mn, Ni, Zn, Mg, Cu, etc.), magnetoplumbite-type ferrites such as barium ferrite, and particles of iron or alloys having an oxide layer on the surface.

[0057] The shape of the magnetic carrier may be any of granular, spherical and needle-like. Among these, when particularly high magnetization is required, it is preferable to use ferromagnetic fine particles such as iron, and from the standpoint of chemical stability, magnetite, spinel ferrite containing gamma iron oxide, and magnetoplumbite-type ferrite such as barium ferrite are preferred. Specific preferred examples of the magnetoplumbite ferrite include MFL-35S and MFL-35HS (manufactured by Powder Tech Co., Ltd.); DFC-400M, DFC-410M, and SM-350NV (manufactured by DOWA IP Creation Co., Ltd.).

[0058] As the magnetic carrier, a resin carrier containing magnetic fine particles such as ferromagnetic fine particles and having a desired magnetization by selecting the type and content of the fine particles can also be used. The magnetic properties of the resin carrier are preferably 30 emu / g to 150 emu / g in terms of magnetization strength at 1,000 oersted.

[0059] Examples of the method for producing the resin carrier include a method for producing the resin carrier by spraying a molten mixture of magnetic fine particles and an insulating binder resin with a spray dryer; a method for producing a resin carrier in which magnetic fine particles are dispersed in a condensation type binder resin by reacting and curing a monomer or prepolymer in an aqueous medium in the presence of magnetic fine particles; a method for producing a resin carrier by fixing positively or negatively charged fine particles or conductive fine particles to the surface of the magnetic carrier, coating the surface of the magnetic carrier with a resin, or coating the surface of the magnetic carrier with a resin containing positively or negatively charged fine particles or conductive fine particles; etc. By these methods, the chargeability can be appropriately controlled. Examples of the resin for coating include silicone resin, acrylic resin, epoxy resin, fluorine-based resin, etc. Among these, silicone resin and acrylic resin are preferable.

[0060] The carrier content in the two-component developer is preferably 85% by mass or more and less than 98% by mass. When the content is 85% by mass or more, the occurrence of defective images due to the tendency of toner scattering from the developing device can be suppressed. When the content is less than 98% by mass, the charge amount of the electrophotographic toner can be suppressed from increasing excessively and the supply amount of the electrophotographic toner can be suppressed from being insufficient, and a decrease in image density and the occurrence of defective images can be effectively prevented.

[0061] (Toner storage unit) The toner storage unit in the present invention refers to a unit having a function of storing toner, which stores the above-mentioned toner of the present invention. Examples of the toner storage unit include a toner storage container, a developing device, and a process cartridge. The toner storage container refers to a container that stores the toner. The developing device has a means for containing the toner and performing development. The process cartridge is a cartridge which integrates at least an image carrier and a developing unit, contains the toner, and is detachably mountable to an image forming apparatus. The process cartridge may further include at least one selected from a charging unit, an exposure unit, and a cleaning unit. The toner storage unit of the present invention stores the toner of the present invention. By mounting the toner storage unit of the present invention in an image forming apparatus and forming an image, an image is formed using the toner of the present invention, and therefore an excellent image having excellent low-temperature fixability and heat-resistant storage stability can be obtained.

[0062] (Image forming apparatus and image forming method) The image forming apparatus of the present invention has at least an electrostatic latent image carrier, an electrostatic latent image forming means, a developing means, a transfer means, and a fixing means, and further has other means appropriately selected as necessary, such as a discharging means, a cleaning means, a recycling means, a control means, etc. The image forming method of the present invention includes at least an electrostatic latent image forming step, a developing step, a transfer step, and a fixing step, and further includes other steps appropriately selected as necessary, such as a discharging step, a cleaning step, a recycling step, and a control step.

[0063] The image forming method of the present invention can be suitably carried out by the image forming apparatus of the present invention, and the electrostatic latent image forming step can be performed by the electrostatic latent image forming means, the developing step can be performed by the developing means, the transfer step can be performed by the transfer means, the fixing step can be performed by the fixing means, and the other steps can be performed by the other means.

[0064] <Electrostatic latent image forming process and electrostatic latent image forming means> The electrostatic latent image forming step is a step of forming an electrostatic latent image on an electrostatic latent image bearing member. The electrostatic latent image forming unit is a unit for forming an electrostatic latent image on an electrostatic latent image carrier. The electrostatic latent image carrier (sometimes referred to as a "photoconductive insulator," "electrophotographic photoreceptor," or "photoreceptor") is not particularly limited in terms of its material, shape, structure, size, and the like, and may be appropriately selected from known ones. A preferred shape is a drum shape, and examples of its material include inorganic photoreceptors such as amorphous silicon and selenium, and organic photoreceptors such as polysilane and phthalopolymethine. Examples of the organic photoreceptor include a laminated type photoreceptor having a laminated structure in which a layer (charge generation layer) in which a charge generation material such as metal-free phthalocyanine or titanyl phthalocyanine is dispersed in a binder resin and a layer (charge transport layer) in which a charge transport material is dispersed in a binder resin are stacked on a support such as an aluminum drum, and a single-layer type photoreceptor having a single-layer photosensitive layer on a support in which both a charge generation material and a charge transport material are dispersed in a binder resin. In the case of a single-layer type photoreceptor, a hole transport material and an electron transport material can be added as charge transport materials to the photosensitive layer. An undercoat layer may be provided between the support and the multi-layer charge generating layer or the single-layer photosensitive layer.

[0065] The electrostatic latent image can be formed, for example, by uniformly charging the surface of the electrostatic latent image bearing member and then exposing it imagewise, and can be formed by the electrostatic latent image forming unit. The electrostatic latent image forming unit includes, for example, at least a charger that uniformly charges the surface of the electrostatic latent image carrier, and an exposure device that imagewise exposes the surface of the electrostatic latent image carrier.

[0066] The charging can be carried out, for example, by applying a voltage to the surface of the electrostatic latent image bearing member using the charger. The charger is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charger include a contact charger known per se having a conductive or semiconductive roller, brush, film, rubber blade, or the like, and a non-contact charger utilizing corona discharge such as a corotron or scorotron.

[0067] The charger is preferably disposed in contact or non-contact with the electrostatic latent image carrier, and charges the surface of the electrostatic latent image carrier by applying a superimposed DC voltage and an AC voltage to the charger. The charger is preferably a charging roller disposed in close proximity to the photoconductor in a non-contact manner via a gap tape, and charges the surface of the photoconductor by applying a superimposed DC voltage and an AC voltage to the charging roller.

[0068] The exposure can be carried out, for example, by exposing the surface of the electrostatic latent image bearing member imagewise using the exposure unit. The exposure device is not particularly limited as long as it can perform image-wise exposure on the surface of the photoconductor charged by the charger, and can be appropriately selected depending on the purpose, and examples thereof include a copying optical system, a rod lens array system, a laser optical system, a liquid crystal shutter optical system, etc. Note that a light back system in which image-wise exposure is performed from the back side of the photoconductor may be adopted.

[0069] <Developing step and developing means> The developing step is a step of developing the electrostatic latent image with the toner or developer of the present invention to form a visible image. The developing means is a means for developing the electrostatic latent image with the toner or the developer of the present invention to form a visible image. The visible image can be formed, for example, by developing the electrostatic latent image with the toner or the developer of the present invention, and can be formed by the developing unit. The developing means is not particularly limited as long as it can develop using the toner or the developer of the present invention, and can be appropriately selected from known ones. For example, a developing means that contains the toner or the developer of the present invention and has at least a developing unit that can apply the toner or the developer to the electrostatic latent image in a contact or non-contact manner is preferable, and a developing unit that is detachably provided with the toner container of the present invention is more preferable.

[0070] The developing device may be of a dry developing type or a wet developing type, and may be a single-color developing device or a multi-color developing device. For example, a suitable example is one having an agitator that frictionally stirs and charges the toner or developer, and a rotatable magnetic roller.

[0071] In the developing device, for example, the toner and the carrier are mixed and stirred, and the toner is charged by friction during this process and held in a bristled state on the surface of a rotating magnet roller to form a magnetic brush. Since the magnet roller is disposed in the vicinity of the electrostatic latent image carrier, a part of the toner constituting the magnetic brush formed on the surface of the magnet roller moves to the surface of the electrostatic latent image carrier by electrical attraction. As a result, the electrostatic latent image is developed by the toner, and a visible image of the toner is formed on the surface of the electrostatic latent image carrier. It is preferable to apply an alternating electric field when moving the toner to the surface of the electrostatic latent image carrier.

[0072] <Transfer process and transfer means> The transfer step is a step of transferring the visible image onto a recording medium. The transfer means is a means for transferring the visible image onto a recording medium. The transfer step preferably uses an intermediate transfer body, and after a visible image is primarily transferred onto the intermediate transfer body, the visible image is secondarily transferred onto the recording medium. It is more preferable that the toner used is a toner of two or more colors, preferably a full-color toner, and includes a primary transfer step of transferring the visible image onto the intermediate transfer body to form a composite transfer image, and a secondary transfer step of transferring the composite transfer image onto the recording medium.

[0073] The transfer of the visible image can be performed, for example, by charging the electrostatic latent image carrier using a transfer charger, and can be performed by the transfer means. The transfer means preferably has a first transfer means for transferring the visible image onto an intermediate transfer body to form a composite transfer image, and a second transfer means for transferring the composite transfer image onto a recording medium.

[0074] The transfer means (primary transfer means, secondary transfer means) preferably has at least a transfer device that peels and charges the visible image formed on the electrostatic latent image carrier to the transferee side. The number of transfer devices may be one or more. Examples of the transfer device include a corona transfer device that uses corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, and an adhesive transfer device. The intermediate transfer body is not particularly limited and can be appropriately selected from known transfer bodies depending on the purpose. Suitable examples include a transfer belt. The transfer medium is not particularly limited and can be appropriately selected from known recording media (recording paper).

[0075] <Fixing process and fixing means> The fixing step is a step of fixing the visible image transferred onto the recording medium. The fixing means is a means for fixing the visible image transferred onto the recording medium. The fixing step may be carried out for each color toner each time it is transferred onto the recording medium, or may be carried out simultaneously for each color toner in a laminated state.

[0076] The fixing means is not particularly limited and can be appropriately selected according to the purpose, but known heating and pressurizing means are suitable. Examples of the fixing means include a combination of a heating roller and a pressure roller; a combination of a heating roller, a pressure roller and an endless belt; a means having a heating body with a heating element, a film in contact with the heating body, and a pressure member in pressure contact with the heating body through the film, and passing a transfer body on which an unfixed image has been formed between the film and the pressure member to heat and pressurize the image; and the like.

[0077] The heating temperature in the fixing means is usually preferably 80°C to 200°C. In the present invention, depending on the purpose, for example, a known optical fixing device may be used together with or instead of the fixing step and fixing means.

[0078] <Other steps and other means> The charge removing step is a step of removing electricity by applying a charge removing bias to the electrostatic latent image bearing member, and can be suitably performed by a charge removing unit. The charge removing means is not particularly limited as long as it can apply a charge removing bias to the electrostatic latent image bearing member, and can be appropriately selected from known charge removers. For example, a charge removing lamp is preferably used.

[0079] The cleaning step is a step of removing the electrophotographic toner remaining on the electrostatic latent image bearing member, and can be suitably carried out by a cleaning means. The cleaning means is not particularly limited as long as it can remove the electrophotographic toner remaining on the electrostatic latent image carrier, and can be appropriately selected from among known cleaners. Suitable examples of the cleaning means include magnetic brush cleaners, electrostatic brush cleaners, magnetic roller cleaners, blade cleaners, brush cleaners, and web cleaners.

[0080] The recycling step is a step of recycling the electrophotographic toner removed in the cleaning step to the developing means, and can be suitably carried out by a recycling means. The recycling means is not particularly limited, and examples thereof include known transport means.

[0081] The control step is a step of controlling each of the steps, and can be suitably performed by a control means. The control means is not particularly limited as long as it can control the movement of each of the means, and can be appropriately selected depending on the purpose. For example, the control means includes devices such as a sequencer and a computer.

[0082] Next, another embodiment of the image forming method of the present invention will be described with reference to FIG. 1 is a tandem type color image forming apparatus, which includes a copying machine main body 150, a paper feed table 200, a scanner 300, and an automatic document feeder (ADF) 400. An endless belt-like intermediate transfer member 50 is provided in the center of a copying machine main body 150 . The intermediate transfer body 50 is stretched around support rollers 14, 15, and 16, and can rotate clockwise in FIG. 2. An intermediate transfer body cleaning device 17 for removing residual toner on the intermediate transfer body 50 is disposed near the support roller 15. An image forming unit 120 is disposed on the intermediate transfer body 50 stretched around the support rollers 14 and 15 along the conveying direction of the intermediate transfer body 50, in which four image forming means 18 for yellow, cyan, magenta, and black are arranged in a row facing each other. An exposure device 21 is disposed near the image forming unit 120. A secondary transfer device 22 is disposed on the side of the intermediate transfer body 50 opposite to the side where the image forming unit 120 is disposed. In the secondary transfer device 22, a secondary transfer belt 24, which is an endless belt, is stretched around a pair of rollers 23, and the transfer paper conveyed on the secondary transfer belt 24 and the intermediate transfer body 50 can come into contact with each other. A fixing device 25 is disposed near the secondary transfer device 22. The fixing device 25 includes a fixing belt 26, which is an endless belt, and a pressure roller 27 arranged to be pressed against the fixing belt 26. In the tandem image forming apparatus, a sheet inverting device 28 is disposed near the secondary transfer device 22 and the fixing device 25 for inverting the transfer paper so that images can be formed on both sides of the transfer paper.

[0083] Next, a description will be given of the formation of a full-color image (color copy) using the image forming unit 120. That is, first, an original is set on the original table 130 of the automatic document feeder (ADF) 400, or the automatic document feeder 400 is opened and an original is set on the contact glass 32 of the scanner 300, and the automatic document feeder 400 is closed.

[0084] When a start switch (not shown) is pressed, after the document is transported and moved onto the contact glass 32 when the document is set on the automatic document feeder 400, the scanner 300 is driven and the first travelling body 33 and the second travelling body 34 travel, while immediately after the document is set on the contact glass 32. At this time, light from a light source is irradiated by the first travelling body 33, and the reflected light from the document surface is reflected by a mirror in the second travelling body 34, and is received by the reading sensor 36 through the imaging lens 35 to read the color document (color image), which is converted into image information of black, yellow, magenta and cyan. Next, each image information is transmitted to each image forming unit 18 in the image forming unit 120, and a visible image of each color of black, yellow, magenta and cyan is formed.

[0085] Then, the black, yellow, magenta, and cyan image information is transmitted to each image forming means 18 (black image forming means, yellow image forming means, magenta image forming means, and cyan image forming means) in the tandem image forming unit 120, and black, yellow, magenta, and cyan toner images are formed in each image forming means. That is, as shown in FIG. 2, each of the image forming means 18 of each color (image forming means for black, image forming means for yellow, image forming means for magenta, and image forming means for cyan) in the image forming unit 120 includes an electrostatic latent image carrier 10, a charging device 160 for uniformly charging the electrostatic latent image carrier 10, an exposure device for exposing the electrostatic latent image carrier to light (L in FIG. 2) in the form of an image corresponding to each color image based on each color image information, and forming an electrostatic latent image corresponding to each color image on the electrostatic latent image carrier, a developing device 61 for developing the electrostatic latent image with each color toner (black toner, yellow toner, magenta toner, and cyan toner) to form a toner image with each color toner, a transfer charger 62 for transferring the toner image onto the intermediate transfer body 50, a cleaning device 63, and a static eliminator 64, and each monochrome image (black image, yellow image, magenta image, and cyan image) can be formed based on the image information of each color. The black image formed on the black electrostatic latent image carrier 10K, the yellow image formed on the yellow electrostatic latent image carrier 10Y, the magenta image formed on the magenta electrostatic latent image carrier 10M, and the cyan image formed on the cyan electrostatic latent image carrier 10C are sequentially transferred (primary transfer) onto the intermediate transfer body 50 which is rotated by the support rollers 14, 15, and 16. Then, the black image, the yellow image, the magenta image, and the cyan image formed on the cyan electrostatic latent image carrier 10C are superimposed on the intermediate transfer body 50 to form a composite color image (color transfer image).

[0086] On the other hand, in the paper feed table 200, one of the paper feed rollers 142 is selectively rotated to feed a sheet (recording paper) from one of the paper feed cassettes 144 provided in multiple stages in the paper bank 143, and the sheet is separated one by one by the separation roller 145 and sent to the paper feed path 146, and is conveyed by the conveyance roller 147 to be guided to the paper feed path 148 in the copying machine main body 150, and is stopped by hitting the registration roller 49. Alternatively, the paper feed roller 142 is rotated to feed a sheet (recording paper) on the manual feed tray 54, and the sheet is separated one by one by the separation roller 145 and placed in the manual feed path 53, and is also stopped by hitting the registration roller 49. The registration roller 49 is generally used while being grounded, but may be used with a bias applied to remove paper dust from the sheet. Then, the registration rollers 49 are rotated in synchronization with the composite color image (color transfer image) composited on the intermediate transfer body 50, a sheet (recording paper) is sent between the intermediate transfer body 50 and the secondary transfer device 22, and the composite color image (color transfer image) is transferred (secondary transfer) onto the sheet (recording paper) by the secondary transfer device 22, thereby transferring and forming a color image onto the sheet (recording paper). Note that residual toner on the intermediate transfer body 50 after the image transfer is cleaned by the intermediate transfer body cleaning device 17.

[0087] The sheet (recording paper) on which the color image has been transferred and formed is transported by the secondary transfer device 22 and sent to the fixing device 25, where the composite color image (color transfer image) is fixed onto the sheet (recording paper) by heat and pressure. Thereafter, the sheet (recording paper) is switched by the switching claw 55 and discharged by the discharge rollers 56 and stacked on the paper discharge tray 57, or is switched by the switching claw 55 and inverted by the sheet inverting device 28 and guided to the transfer position again, an image is recorded on the back side as well, and then the sheet is discharged by the discharge rollers 56 and stacked on the paper discharge tray 57.

[0088] Next, one embodiment of the process cartridge is shown in Fig. 3. As shown in Fig. 3, the process cartridge 110 of this embodiment has an electrostatic latent image carrier 10 built-in, includes a charger 58 as a charging means, a developing device 40 as a developing means, and a cleaning device 90 as a cleaning means, and further includes other means as necessary. In Fig. 3, the symbol L indicates exposure from an exposure means (not shown), and the symbol 95 indicates recording paper. The electrostatic latent image carrier 10 may be the same as the electrostatic latent image carrier in the image forming apparatus. The charger 58 may be any charging member.

[0089] In the image forming process by the process cartridge shown in FIG. 3, while the electrostatic latent image carrier 10 rotates in the direction of the arrow, an electrostatic latent image corresponding to the exposed image is formed on its surface by charging with the charger 58 and exposing with light L by the exposure means. This electrostatic latent image is developed with toner by the developing device 40, and the toner development is transferred to recording paper 95 by the transfer roller 80 and printed out. Next, the surface of the electrostatic latent image carrier 10 after the image transfer is cleaned by the cleaning device 90, and further discharged by a discharging means (not shown), and the above operations are repeated again. According to the image forming apparatus and image forming method of the present invention, the toner of the present invention, which has little charge fluctuation over time and can form high-quality images over a long period of time, is used, so that high-quality images can be provided over a long period of time.

[0090] According to the image forming apparatus and image forming method of the present invention, the toner of the present invention, which exhibits sufficient charging performance from the initial stage to the lapse of time, is used, and therefore high quality images can be provided for a long period of time. EXAMPLES

[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. In addition, the term "parts" refers to parts by mass unless otherwise specified.

[0092] <Production Example of Polyester Resin 1> The acid components and alcohol components shown in Table 1 were placed in a 1 L four-neck round-bottom flask equipped with a thermometer, a stirrer, a condenser, and a nitrogen gas inlet tube. The flask was then attached to a mantle heater, and nitrogen gas was introduced through the nitrogen gas inlet tube to raise the temperature while maintaining the inside of the flask under an inert atmosphere. Next, 0.05 g of dibutyltin oxide was added and the reaction was carried out while maintaining the temperature at 200° C., thereby obtaining Polyester Resin 1.

[0093] Various physical properties of the polyester resin 1 are also shown in Table 1. In the table, the polycarboxylic acid component and the polyol component are expressed in "parts by mass", "Mw" is the weight average molecular weight, and the value of "peak top molecular weight" is the molecular weight of the main peak value.

[0094] <Production Example of Polyester Resin 2> Polyester resin 2 was obtained in the same manner as in Production Example of Polyester resin 1, except that the types and parts by mass of the polycarboxylic acid component and the polyol component in Production Example of Polyester resin 1 were changed as shown in Table 1. Various physical properties of polyester resin 2 are also shown in Table 1.

[0095] [Table 1]

[0096] Example 1 <Production of toner base A> A mixture of the following composition was stirred and mixed in a Henschel mixer (FM20B, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) at a rotation speed of 3,000 rpm for 5 minutes, and then melt-kneaded in a twin-screw extrusion kneader (TEM-18SS, manufactured by Toshiba Machine Co., Ltd.) at a rotation speed of 600 rpm and a barrel temperature of 100° C. to 160° C. The resulting kneaded product was rolled to an average thickness of 1.7 mm with a roller, cooled to room temperature, and then pulverized and classified with a jet mill (IDS-2, manufactured by Nippon New Match Kogyo Co., Ltd.) and a rotor classifier (100TTSP, manufactured by Hosokawa Micron Corporation) to obtain [toner base A] with a volume average particle size of 7.5 μm and an average circularity of 0.935.

[0097] -composition- 150 parts polyester resin Polyester resin 2 50 parts 3 parts Carnauba wax (WA05TS, manufactured by Toa Kasei Co., Ltd.) Carbon black (MOGUL L, manufactured by Cabot Corporation) 10 parts ·Metal azo dye (T-77, manufactured by Hodogaya Chemical Industry Co., Ltd.) 1.8 parts

[0098] <Measurement of average circularity of toner base particles> The average circularity of the toner matrix was measured as follows. Specifically, 0.1 mL of alkylbenzene sulfonate was added as a dispersant to 100 mL of water from which solid impurities had been removed in advance in a container, and 0.08 g of toner base particles were further added as a measurement sample. The suspension in which the toner base particles were dispersed was subjected to dispersion treatment twice for 1 minute using an ultrasonic disperser, and the shape of the toner base particles was measured by the above-mentioned measurement method with the dispersion concentration set to 3,000 particles / μL to 10,000 particles / μL to determine the circularity.

[0099] <Toner manufacturing> To 100 parts of [toner base A], 1 part of hexamethyldisilazane-treated (HMDS-treated) hydrophobic silica (RX200, manufactured by Nippon Aerosil Co., Ltd.) having an average particle size of 12 nm, 1 part of silicone oil-treated hydrophobic silica (NY50L, manufactured by Nippon Aerosil Co., Ltd.) having an average particle size of 30 nm, 1 part of barium sulfate (Variace B-55, manufactured by Sakai Chemical Co., Ltd.) having an average particle size of 600 nm, and 0.5 parts of hydrophobized polymethylsilsesquioxane particles (Sunsil MP-01, manufactured by Tokuyama Corporation) having an average particle size of 0.05 μm were added, and the mixture was stirred and mixed in a Henschel mixer to obtain [toner 1] of Example 1.

[0100] <Manufacture of Carrier 1> A mixture of the following composition was dispersed in a homomixer for 10 minutes to prepare a resin liquid for forming a resin layer. -composition- Silicone resin solution 2,100 parts Toluene 6,100 parts Aminosilane 30 parts Carbon black 30 parts

[0101] Ferrite particles (DFC-400M, manufactured by DOWA IP Creation Co., Ltd.) having a weight average particle size of 35 μm were used as the carrier core material. The above resin liquid was applied to the surface of the core material to a thickness of 0.50 μm using a fluidized bed coating device in an atmosphere of 60°C, and then dried. The obtained carrier was left to stand in an electric furnace at 180° C. for 2 hours for firing, and after cooling, was crushed using a sieve with 100 μm openings to obtain [carrier 1].

[0102] <Preparation of two-component developer> The above obtained [Toner 1] and [Carrier 1] were uniformly mixed and charged for 5 minutes using a Turbula Mixer (manufactured by WAB) at 48 rpm to prepare [Developer 1] of Example 1 as a two-component developer. The mixture ratio of the toner and the carrier was adjusted to match the toner concentration of 4% by mass in the initial developer of the evaluation machine.

[0103] Example 2 [Toner 2] and [Developer 2] of Example 2 were obtained in the same manner as in Example 1, except that in Example 1, the hydrophobized polymethylsilsesquioxane particles having an average particle size of 0.05 μm were replaced with 1.5 parts of polymethylsilsesquioxane particles having an average particle size of 0.12 μm (Sunsil MP-01, manufactured by Tokuyama Corporation).

[0104] Example 3 [Toner 3] and [Developer 3] of Example 3 were obtained in the same manner as in Example 2, except that the amount of barium sulfate in Example 2 was changed from 1 part to 3 parts.

[0105] Example 4 [Toner 4] and [Developer 4] of Example 4 were obtained in the same manner as in Example 1, except that the polymethylsilsesquioxane particles were not added.

[0106] Example 5 [Toner 5] and [Developer 5] of Example 5 were obtained in the same manner as in Example 1, except that in Example 1, the hydrophobized polymethylsilsesquioxane particles having an average particle size of 0.05 μm were replaced with 1.5 parts of polymethylsilsesquioxane particles having an average particle size of 0.20 μm (Sunsil MP-01, manufactured by Tokuyama Corporation).

[0107] Example 6 [Toner 6] and [Developer 6] of Example 6 were obtained in the same manner as in Example 2, except that the barium sulfate in Example 2 was changed to 1.5 parts of magnesium hydroxide (manufactured by Sakai Chemical Industry Co., Ltd.) having an average particle size of 700 nm.

[0108] Example 7 [Toner 7] and [Developer 7] of Example 7 were obtained in the same manner as in Example 2, except that in Example 2, barium sulfate was changed to 1.5 parts of magnesium oxide (CF6, manufactured by Tateho Chemical Industries Co., Ltd.) having an average particle size of 600 nm.

[0109] Example 8 [Toner 8] and [Developer 8] of Example 8 were obtained in the same manner as in Example 2, except that [Toner Base A] in Example 2 was changed to [Toner Base B] produced as follows.

[0110] <Production of toner base B> [Toner base B] having an average circularity of 0.920 was obtained in the same manner as [Toner base A], except that in the production of [Toner base A], carnauba wax was replaced with rice wax (TOWAX-3F16, manufactured by Toa Chemical Industry Co., Ltd.).

[0111] Comparative Example 1 [Toner 9] and [Developer 9] of Comparative Example 1 were obtained in the same manner as in Example 2, except that barium sulfate was not added.

[0112] Comparative Example 2 In Example 2, except that the barium sulfate having an average particle size of 600 nm was replaced with 0.3 parts of barium sulfate having an average particle size of 100 nm (Varifine BF-1L, manufactured by Sakai Chemical Industry Co., Ltd.), [Toner 10] and [Developer 10] of Comparative Example 2 were obtained in the same manner as in Example 2.

[0113] Comparative Example 3 [Toner 11] and [Developer 11] of Comparative Example 3 were obtained in the same manner as in Example 2, except that in Example 2, barium sulfate having an average particle size of 600 nm was replaced with 1 part of alumina fine particles having an average particle size of 600 nm.

[0114] Comparative Example 4 [Toner 12] and [Developer 12] of Comparative Example 4 were obtained in the same manner as in Example 2, except that [Toner Base A] in Example 2 was changed to [Toner Base C] produced as follows.

[0115] <Production of toner base C> [Toner Base C] having an average circularity of 0.955 was obtained in the same manner as [Toner Base A], except that the jet mill in [Toner Base A] was changed to a turbo mill (T250, Matsubo Corporation). Table 2 shows the combinations of the toner base and the external additives of the toners obtained in Examples 1 to 8 and Comparative Examples 1 to 4.

[0116] (evaluation) The following evaluations were carried out for the toners and developers of Examples 1 to 8 and Comparative Examples 1 to 4. The evaluation results are shown in Table 3.

[0117] <Charge stability> To evaluate the charge stability, the developer was stirred again in a ball mill for 1 minute, and the charge amount was measured using a blow-off charge amount measuring device (TB-200 model, manufactured by Toshiba Chemical Corporation) to obtain the charge amount Q(1). After that, the charge amount Q(60) was also measured for the developer that had been stirred in a ball mill for 60 minutes in the same manner. The charge amount after stirring for 1 minute was defined as the initial charge amount, and the charge amount after stirring for 60 minutes was defined as the charge amount over time. The stability of the charge amount was evaluated using the numerical value (Qst) calculated by the following formula as an index of stability of the charge amount. [Formula]: |1-(Q(60) / Q(1))|×100=Qst ◎: Qst is less than 15 〇: Qst is 15 or more and less than 20 △: Qst is 20 or more and less than 40 ×: Qst is 40 or more

[0118] <Skin Cover> The developer obtained above was placed in a commercially available image forming device (manufactured by Ricoh Co., Ltd.) and conditioned overnight in a high temperature and high humidity environment of 27°C and 80%. Scotch tape was applied to the entire exposed part of the photoconductor that had stopped printing on a blank sheet, and the peeled Scotch tape was applied to a Ricoh Type 6000T paper and stored. The tape was then scanned with an X-rite (manufactured by Videojet X-Rite) to obtain a 100% L. * The evaluation criteria were as follows: [Evaluation Criteria] ◎:L * is 92.0 or higher ○:L * is 91.0 or more and less than 92.0 △:L * is 90.0 or more and less than 91.0 ×:L * is less than 90.0

[0119] <Image quality> The image quality was evaluated comprehensively based on the deterioration of the image quality after paper passing (specifically, the occurrence of transfer failure and photoconductor cleaning failure). The transfer failure was evaluated by using each developer in a commercially available image forming apparatus (manufactured by Ricoh Co., Ltd.) to print 1,000 sheets of A4 landscape, 2 cm wide vertical stripe images as output images, and then printing a full black solid image. The level of transfer failure of the image was visually ranked and the transfer failure was evaluated.

[0120] For photoconductor cleaning defects, 1,000 sheets of 2cm-wide vertical stripe images were printed on A4 paper, then development of the solid black stripe image was stopped, and the toner on the photoconductor after cleaning by the cleaning unit was transferred to a tape using Scotch tape, attached to a white paper, and measured with a spectrophotometer (X-Rite938). On the other hand, Scotch tape alone was attached to the same white paper and measured with a spectrophotometer, and the reflection density (ID) of the Scotch tape and the white paper combined was subtracted from the reflection density (ID) of the toner, tape, and white paper combined to obtain the difference value, and the photoconductor cleaning defects were evaluated. The smaller the difference value, the better the cleaning performance. The image quality was evaluated based on the following criteria.

[0121] [Evaluation Criteria] ○: No abnormal images △: A slight decrease in image density due to a minor transfer failure and a slight image stain due to a minor cleaning failure are observed, but are within the range of practical use. ×: Image density reduction or defects due to transfer failure, and image stains due to cleaning failure are observed.

[0122] [Table 2]

[0123] [Table 3]

[0124] From the above, it has become clear that the toner of the present invention can exhibit sufficient charging performance from the initial stage to the lapse of time by adding inorganic particles selected from barium sulfate, magnesium hydroxide, and magnesium oxide having a size of 350 nm or more, and can form high-quality images over the long term.

[0125] For example, aspects of the present invention are as follows. (1) A toner comprising toner base particles including a binder resin, a release agent, and a charge control agent, and an external additive, the toner base particles have an average circularity of 0.850 or more and 0.950 or less; The toner, wherein the external additive contains at least one type of inorganic particle selected from the group consisting of barium sulfate, magnesium hydroxide, and magnesium oxide, the average particle size of which is 350 nm or more and 1000 nm or less. (2) The toner according to the above (1), wherein the content of the inorganic particles is from 0.1 parts by mass to 2.0 parts by mass per 100 parts by mass of the toner. (3) The toner according to (1) or (2) above, further comprising hydrophobically treated polymethylsilsesquioxane particles as the external additive. (4) The toner according to the above (3), wherein the average particle size of the hydrophobically treated polymethylsilsesquioxane particles is from 0.050 μm to 0.150 μm. (5) The toner according to the above (3), wherein the content of the hydrophobized polymethylsilsesquioxane particles is from 0.05 parts by mass to 3 parts by mass based on 100 parts by mass of the toner. (6) A toner storage unit, characterized in that it stores the toner according to any one of (1) to (5) above. (7) an electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; a developing unit for developing the electrostatic latent image formed on the electrostatic latent image carrier with the toner according to any one of (1) to (5) above to form a visible image; a transfer means for transferring the visible image onto a transfer material; and a fixing means for fixing the visible image transferred onto the transfer material. (8) forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with the toner according to any one of (1) to (5) above to form a visible image; a transfer step of transferring the visible image onto a transfer material; and a fixing step of fixing the visible image transferred onto the transfer material.

[0126] The toner described in any one of (1) to (5), the toner storage unit described in (6), the image forming apparatus described in (7), and the image forming method described in (8) can solve the conventional problems and achieve the object of the present invention. [Explanation of symbols]

[0127] (Fig. 1, Fig. 2) 10, 10K, 10Y, 10M, 10C Electrostatic latent image carrier 14, 15, 16 Support rollers 17 Intermediate transfer body cleaning device 18 Image forming means 21 Exposure equipment 22 Secondary transfer device 23 Support roller 24 Secondary transfer belt 25 Fixing device 26 Fixing belt 27 Pressure roller 28 Sheet reversing device 32 Contact Glass 33 First Running Body 34 Second Running Body 35 Imaging Lens 36 Reading sensor 40 Developer 49 Registration roller 50 Intermediate transfer body 52 Separation roller 53 Manual feed path 54 Manual feed tray 55 Switching claw 56 Discharge roller 57 Output tray 61 Developing device 62 Transfer charger 63 Cleaning Equipment 64 Static eliminator 80 Transfer roller 120 Image forming unit 130 Manuscript stand 142 Paper feed roller 143 Paper Bank 144 Paper feed cassette 145 Separation roller 146 Paper feed path 147 Transport roller 148 Paper feed path 150 Copying device body 160 Charging device 200 Paper feed table 300 Scanner 400 Automatic Document Feeder (ADF) L exposure

[0128] (Figure 3) 10 Electrostatic latent image carrier 40 Developer 58 Charger 80 Transfer roller 90 Cleaning Equipment 95 Recording Paper 110 Process cartridge L exposure [Prior art documents] [Patent documents]

[0129] [Patent Document 1] JP 2005-107517 A [Patent Document 2] JP 2009-103767 A

Claims

1. A toner comprising toner base particles including a binder resin, a release agent, and a charge control agent, and an external additive, the toner base particles have an average circularity of 0.850 or more and 0.950 or less; The toner, wherein the external additive contains at least one type of inorganic particle selected from the group consisting of barium sulfate, magnesium hydroxide, and magnesium oxide, the average particle size of which is 350 nm or more and 1000 nm or less.

2. The toner according to claim 1 , wherein the content of the inorganic particles is from 0.1 parts by mass to 2.0 parts by mass with respect to 100 parts by mass of the toner.

3. The toner according to claim 1 or 2, further comprising hydrophobically treated polymethylsilsesquioxane particles as the external additive.

4. 4. The toner according to claim 3, wherein the average particle size of the hydrophobically treated polymethylsilsesquioxane particles is from 0.050 μm to 0.150 μm.

5. 4. The toner according to claim 3, wherein the content of the hydrophobically treated polymethylsilsesquioxane particles is from 0.05 parts by mass to 3 parts by mass based on 100 parts by mass of the toner.

6. A toner storage unit, comprising the toner according to claim 1 or 2 stored therein.

7. An electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; a developing unit for developing the electrostatic latent image formed on the electrostatic latent image carrier with the toner according to claim 1 or 2 to form a visible image; a transfer means for transferring the visible image onto a transfer material; and a fixing means for fixing the visible image transferred onto the transfer material.

8. an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with the toner according to claim 1 or 2 to form a visible image; a transfer step of transferring the visible image onto a transfer material; and a fixing step of fixing the visible image transferred onto the transfer material.

Citation Information

Patent Citations

  • Color toner and full-color image forming method using the color toner

    JP2005107517A

  • Toner, developer, developing device and image forming apparatus

    JP2009103767A