Photovoltaic packaging adhesive, preparation method thereof and photovoltaic module
By using POE film layer and transparent inorganic particles in photovoltaic packaging adhesive, the problems of aging and strong fluidity of photovoltaic packaging film materials are solved, and higher heat resistance and light utilization are achieved, reducing the film The layer is separated from risk.
Patent Information
- Application Number
- CN202411217919.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
AI Technical Summary
The existing photovoltaic packaging film materials are prone to PID after aging, and the molecular weight distribution of POE materials is narrow and the fluidity is strong, resulting in a decrease in component yield. In addition, the interlayer force of traditional photovoltaic packaging glue is large when used, which can easily lead to the film layer. detachment and lobes.
Photovoltaic encapsulation glue consisting of a POE film layer and two layers of transparent inorganic particles. The thermal conductivity coefficient of transparent inorganic particles is greater than or equal to 3.9W/(m·K), and the particle size is 5-30μm, passing through the layer Pressure composite and UV curing treatment form a film layer structure with uniform thickness, reducing fluidity and enhancing binding force.
It effectively reduces the thermal conductivity of the photovoltaic packaging film, improves the heat resistance, reduces the risk of film layer detachment and lobes, and improves the service life and light utilization rate of photovoltaic modules.
Smart Images

Figure CN119060650A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the photovoltaic field, and specifically to a photovoltaic encapsulation adhesive and a preparation method thereof, and a photovoltaic module. Background Art
[0002] Photovoltaic modules are devices that use the photoelectric effect of batteries to directly convert sunlight into electrical energy. In order to ensure that photovoltaic modules also extend their service life, a packaging film will be attached to the surface of the cell array in the photovoltaic module; conventional packaging films usually include two materials: EVA and POE. EVA material is a copolymer of ethylene and vinyl acetate, which has good processing characteristics and adhesion, but due to its molecular characteristics, it is very easy to decompose acetic acid after aging, causing PID phenomenon; POE material is a copolymer of ethylene and α-olefin, which does not contain acetic acid in its molecular structure and has the advantages of low water permeability and high body resistance, which makes the double-sided modules have a longer-lasting anti-PID performance, but POE has a narrow molecular weight distribution and strong fluidity. After lamination, it is easy to produce bubbles and cracks, which leads to a decrease in the yield rate of the module.
[0003] Therefore, there is an urgent need to develop a type of photovoltaic encapsulation adhesive that not only has high light transmittance at the gap between the battery cells, but also has excellent stability in terms of packaging performance, heat resistance and insulation properties. Summary of the invention
[0004] The embodiments of the present application provide a photovoltaic encapsulation adhesive and a preparation method thereof, and a photovoltaic module. On the one hand, the light utilization rate of the traditional photovoltaic encapsulation adhesive is improved, the interlayer force of the photovoltaic encapsulation film during use is reduced, and the risk of the film layer detaching and cracking is effectively avoided. On the other hand, the thermal conductivity of the photovoltaic encapsulation adhesive is effectively reduced, the heat resistance of the light film encapsulation adhesive is improved, and the scope of use of the photovoltaic encapsulation adhesive is expanded.
[0005] The embodiment of the present application provides a photovoltaic encapsulation adhesive, comprising: a first adhesive film layer, a POE adhesive film layer, and a second adhesive film layer stacked in sequence;
[0006] The POE film layer is filled with a number of transparent inorganic particles, the thickness of the first film layer is greater than the thickness of the second film layer, so that the neutral layer of the photovoltaic encapsulation glue is close to the interface between the first film layer and the POE film layer, and the thickness of the POE film layer is less than the thickness of the second film layer;
[0007] The thermal conductivity of the transparent inorganic particles is greater than or equal to 3.9 W / (m·K), and the particle size of the transparent inorganic particles is in the range of 5-30 μm.
[0008] Preferably, the transparent inorganic particles include one or more combinations of TiO2 and silicon nitride, and the doping amount of the transparent inorganic particles in the POE adhesive film layer is 10-20wt%.
[0009] Preferably, the transparent inorganic particles are modified TiO2, and the modified TiO2 is TiO2 modified with an organic group, and the organic group includes a silane coupling group.
[0010] Preferably, the transparent inorganic particles include a mixture of first inorganic particles and second inorganic particles, the particle size of the first inorganic particles is 5-10um, the particle size of the second inorganic particles is 20-30um, and the mass ratio of the first inorganic particles to the second inorganic particles is 1:(1-3).
[0011] Preferably, the first adhesive film layer and the second inorganic adhesive film layer are made of the same material, and both include transparent EVA resin, a cross-linking agent, a UV absorber, and an antioxidant.
[0012] Preferably, the first adhesive film layer is filled with a plurality of transparent inorganic particles.
[0013] Preferably, the photovoltaic encapsulation adhesive has a thickness of about 200-500 μm, the first adhesive film layer and the second adhesive film layer have thicknesses of 50-100 μm and 30-90 μm respectively, and the POE adhesive film layer has a thickness of 20-80 μm.
[0014] Preferably, the POE adhesive film layer further includes a cross-linking agent, a UV absorber, and an antioxidant.
[0015] A method for preparing a photovoltaic encapsulation adhesive, comprising:
[0016] Step 1: Prepare POE film layer: POE material and transparent inorganic particles are blended and then extruded into granules to obtain POE masterbatch;
[0017] Step 2: Three-layer lamination, the raw material of the first film, the POE masterbatch and the raw material of the second film are compounded by melt lamination;
[0018] Step 3: Curing treatment: subjecting the three-layer film compounded in step 2 to UV curing and curing treatment to obtain a photovoltaic module encapsulation film.
[0019] The present invention provides a photovoltaic module, comprising a front transparent packaging layer, a first photovoltaic packaging adhesive layer, a battery cell array, a second photovoltaic packaging adhesive layer and a back packaging layer, the first photovoltaic packaging adhesive layer and the second photovoltaic packaging adhesive layer are the photovoltaic packaging adhesive layers described in any of the above embodiments, and in the first photovoltaic packaging adhesive layer and / or the second photovoltaic packaging adhesive layer, the first adhesive film layer is arranged on the side of the POE adhesive film layer away from the battery cell array.
[0020] Beneficial Effects
[0021] The present invention provides a photovoltaic encapsulation adhesive. By filling a plurality of transparent inorganic particles into a POE adhesive film layer, the fluidity of the POE adhesive film layer can be reduced, so that when the first adhesive film layer, the POE adhesive film layer and the second adhesive film layer are co-extruded, the obtained film layer structure is uniform, with fewer bubbles and strong bonding force between the film layers. The filled plurality of transparent inorganic particles have different light refraction surfaces, which can further improve the refraction rate of light between the battery plate and improve the light efficiency.
[0022] By controlling the thickness of the first adhesive film layer to be greater than the thickness of the second adhesive film layer, so that the neutral layer of the photovoltaic encapsulation adhesive is close to the interface junction of the first adhesive film layer and the POE adhesive film layer, when the photovoltaic module is squeezed and bent after encapsulation, the force at the interface of the photovoltaic encapsulation film layer is smaller, thereby reducing the risk of cracks or film separation.
[0023] Abstract of the drawings
[0024] Figure 1 This is a diagram showing the structure of a photovoltaic encapsulation film layer according to an embodiment of the present application;
[0025] Figure 2 This is a structural diagram of a photovoltaic encapsulation film layer shown in another embodiment of the present application;
[0026] Figure 3 This is a structural diagram of a photovoltaic encapsulation film layer shown in another embodiment of the present application;
[0027] Figure 4 This is a structural diagram of a photovoltaic encapsulation film layer shown in another embodiment of the present application;
[0028] Figure 5 This is a diagram of the film structure of the photovoltaic module of this application. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.
[0030] The embodiments of the present application provide a photovoltaic encapsulation adhesive and a preparation method thereof, and a photovoltaic module. The following are described in detail. It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels, and no numerical requirements or order are imposed. Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and simplicity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which are applicable regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any quoted numbers (fractions or integers) within the indicated range.
[0031] The present application provides a photovoltaic encapsulation adhesive, such as Figure 1 As shown, it comprises: a first adhesive film layer 101, a POE adhesive film layer 201 and a second adhesive film layer 102 stacked in sequence;
[0032] The POE film layer 201 is filled with a plurality of transparent inorganic particles 202, the thickness of the first film layer 101 is greater than the thickness of the second film layer 102, so that the neutral layer of the photovoltaic encapsulation adhesive is close to the interface between the first film layer 101 and the POE film layer 201, and the thickness of the POE film layer 201 is less than the thickness of the second film layer 102;
[0033] The thermal conductivity of the transparent inorganic particles 202 is greater than or equal to 3.9 W / (m·K), and the particle size of the transparent inorganic particles 202 is in the range of 5-30 μm.
[0034] Specifically, the material of the first adhesive film layer 101 and the second adhesive film layer 102 can be EVA resin, EPE resin or POE resin.
[0035] The materials of the first adhesive film layer 101 and the second adhesive film layer 102 can be the same or different, and can be adjusted according to actual conditions.
[0036] Specifically, the first adhesive film layer 101 and the second adhesive film layer 102 further include a cross-linking agent, a UV absorber and an antioxidant;
[0037] Wherein, the crosslinking agent includes at least one of dipentaerythritol hexaacrylate, diethylene glycol diacrylate phthalate, 1,6-hexanediol dimethacrylate, TAIC (triallyl isocyanurate), and PL-400;
[0038] Wherein, the UV absorber includes at least one of UV531, UV328, UV400, UV-P, and UV-1;
[0039] The antioxidant is one or both of phenols and phosphites. The phenol antioxidant may be antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, etc., preferably antioxidant 1010. The phosphite antioxidant may be antioxidant 168, antioxidant 242, antioxidant TPP, etc., preferably antioxidant 168.
[0040] In the following examples of the present invention, the antioxidants are antioxidant 1010 and antioxidant 168 added in a mass ratio of 1:2.
[0041] Specifically, the POE film layer 201 further includes a cross-linking agent, a UV absorber, and an antioxidant.
[0042] Wherein, the crosslinking agent is a mixture of one or more of dicumyl peroxide, pentaerythritol tetraacrylate and tert-butyl peroxide 2-ethylhexanoate.
[0043] Wherein, the UV absorber is a mixture of one or more of UV-531, UV-328 and UV-234.
[0044] Specifically, the antioxidant is a mixture of one or more of antioxidant 168 , antioxidant 264 and antioxidant 1076 .
[0045] The present application provides a photovoltaic encapsulation adhesive, which can reduce the fluidity of the POE adhesive film layer 201 by filling a plurality of transparent inorganic particles 202 into the POE adhesive film layer 201, so that when the first adhesive film layer 101, the POE adhesive film layer 201 and the second adhesive film layer 102 are co-extruded, the obtained film layer structure is uniform, with fewer bubbles and strong bonding force in the middle of the film layer. At the same time, the plurality of transparent inorganic particles 202 filled have different light refraction surfaces, further improving the refraction rate of light between array cells and improving light efficiency;
[0046] By controlling the thickness of the first adhesive film layer 101 to be greater than the thickness of the second adhesive film layer 102, the neutral layer of the photovoltaic encapsulation adhesive is close to the interface junction between the first adhesive film layer 101 and the POE adhesive film layer 201, so that when the photovoltaic module is squeezed and bent after encapsulation, the force at the interface of the photovoltaic encapsulation film layer is smaller, thereby reducing the risk of cracks or film separation.
[0047] It should be noted that the light utilization rate of the cell is related to the conversion efficiency of the cell itself, as well as the optical properties of the glass and film at the front of the cell. It is necessary to adjust the scattering properties of the film to improve the light utilization rate. However, the higher the light transmittance of the film, the higher the light utilization rate of the cell after encapsulation. The higher the haze of the film, the better the light trapping effect of the film. This application adds transparent inorganic particles to balance the light transmittance and haze of the film, thereby maximizing the light utilization rate of the encapsulated cell.
[0048] In one embodiment, the transparent inorganic particles 202 include one or more combinations of TiO 2 and silicon nitride, and the doping amount of the transparent inorganic particles in the POE film layer is 10-20 wt %.
[0049] Specifically, the TiO2 and the silicon nitride can be regular spheres or amorphous particles, that is, irregular particles, such as Figure 4 shown.
[0050] This embodiment uses one or more combinations of TiO2 and silicon nitride as doped particles and limits the doping amount of transparent inorganic particles, which can effectively reduce the fluidity of the POE film layer 201. At the same time, TiO2 and silicon nitride both have good thermal conductivity and can promptly conduct the heat generated by the photovoltaic module to the outside of the module, thereby effectively ensuring the service life of the photovoltaic module.
[0051] In another embodiment, referring to Figure 3 The transparent inorganic particles 202 include a mixture of first inorganic particles 202b and second inorganic particles 202a, the particle size of the first inorganic particles 202b is 5-10um, the particle size of the second inorganic particles 202a is 20-30um, and the mass ratio of the first inorganic particles 202b to the second inorganic particles 202a is 1:(1~3).
[0052] Specifically, the materials of the first inorganic particles 202b and the second inorganic particles 202a may be the same or different. For example, the materials of the first inorganic particles 202b and the second inorganic particles 202a may both be TiO2, or the material of the first inorganic particles 202b may be TiO2, and the material of the second inorganic particles 202a may be silicon nitride.
[0053] Specifically, the particle size of the first inorganic particles 202b includes but is not limited to any one of 5um, 6um, 7um, 8um, 9um, and 10um; the particle size of the second inorganic particles 202a includes but is not limited to any one of 20um, 21um, 22um, 23um, 24um, 25um, 26um, 27um, 28um, 29um, and 30um;
[0054] Specifically, the first inorganic particles 202 b and the second inorganic particles 202 a may include modified TiO 2 .
[0055] In this embodiment, by configuring two transparent inorganic particles 202 with different particle sizes, on the one hand, the fluidity of the POE film layer 201 can be finely controlled to reduce the generation of bubbles during the lamination process and prevent cracking; on the other hand, more light refraction / reflection surfaces are provided to adjust the light path of the light in the gap between the battery cells and improve the light utilization rate of the battery cells.
[0056] In another embodiment, the transparent inorganic particles 202 are modified TiO2, and the modified TiO2 is TiO2 modified with an organic group, and the organic group includes a silane coupling group.
[0057] Specifically, the preparation method of TiO2 modified by silane coupling agent includes:
[0058] Triethoxysilane, petroleum ether and solid acid were uniformly mixed in a mass ratio of 1:10:0.02 to prepare a triethoxysilane mixed solution;
[0059] 3-methacryloxypropyltriethoxysilane and 95% ethanol were mixed and stirred at a mass ratio of 1:9 to prepare a silane hydrolyzate;
[0060] Titanium dioxide and silane hydrolyzate were mixed evenly in a weight ratio of 1:13, immersed for 30 minutes, and dried at low temperature. The titanium dioxide after the reaction was mixed with triethoxysilane mixed solution in a weight ratio of 1:12, refluxed for 3.5 hours under a nitrogen atmosphere, washed and dried at low temperature to obtain modified titanium dioxide;
[0061] In this embodiment, titanium dioxide is modified by doping and the surface of titanium dioxide is modified with siloxane organic groups, which can prevent titanium dioxide from agglomerating. The organic groups modified on the surface of titanium dioxide can effectively adsorb free acetate ions and reduce the impact of PID.
[0062] In another embodiment, the first adhesive film layer 101 is filled with a plurality of transparent inorganic particles 202 .
[0063] Specifically, Figure 2 As shown, the plurality of transparent inorganic particles 202 filled in the first adhesive film layer 101 include titanium dioxide or silicon nitride, and specific reference may be made to the transparent inorganic particles 202 doped in POE;
[0064] In this embodiment, because the first film layer 101 is relatively thicker than the thinner second film layer 102, the first film layer 101 and the POE film layer 201 are more likely to delaminate and split. By filling a plurality of transparent inorganic particles 202 into the first film layer 101, the contact area between the first film layer 101 and the POE layer can be further increased, thereby improving the adhesion between the film layers and preventing delamination between the film layers.
[0065] In another embodiment, the photovoltaic encapsulation adhesive has a thickness of about 200-500 μm, the first adhesive film layer 101 and the second adhesive film layer 102 have thicknesses of 50-100 μm and 30-90 μm, respectively, and the POE adhesive film layer 201 has a thickness of 20-80 μm.
[0066] Specifically, the thickness of the first adhesive film layer 101 is greater than the thickness of the second adhesive film layer 102 , and the thickness of the POE adhesive film layer 201 is less than the thickness of the second adhesive film layer 102 .
[0067] A method for preparing a photovoltaic encapsulation adhesive, comprising:
[0068] Step 1: preparing the POE adhesive film layer 201: blending the POE material and the transparent inorganic particles in a weight ratio of 8:(0.89-2) and then extruding and granulating to obtain a POE masterbatch;
[0069] Step 2: Three-layer lamination, the raw material of the first film, the POE masterbatch and the raw material of the second film are compounded by melt lamination;
[0070] Step 3: Curing treatment: subjecting the three-layer film compounded in step 2 to UV curing and curing treatment to obtain a photovoltaic module encapsulation film.
[0071] Specifically, in the step 1, the POE film layer includes 100 parts of POE resin, 0.1-2 parts of a cross-linking agent, 0-3 parts of a UV absorber, and 0-4 parts of an antioxidant.
[0072] Specifically, the first adhesive film and the second adhesive film include 100 parts of EVA resin; 0.8-1.2 parts of cross-linking agent, 0-3 parts of UV absorber, and 0.1-0.2 parts of antioxidant;
[0073] Furthermore, the first adhesive film and the second adhesive film may further include 1.0-1.5 parts of a cross-linking aid; the cross-linking aid includes but is not limited to at least one or more combinations of triallyl isocyanurate, trimethylolpropane trimethacrylate, propoxylated trimethylolpropane triacrylate and pentaerythritol triacrylate.
[0074] Specifically, the steps of mixing the raw materials of each layer may be:
[0075] The raw materials of each layer were mixed and configured according to the formula in a mixer, and mixed and stirred at a temperature of 40° C. and a rotation speed of 80 rpm for 2 h to obtain a mixed raw material;
[0076] Specifically, in the step 2, the POE film layer raw material is placed in a twin-screw extruder, and melt blended at a temperature of 85° C., 90° C., 95° C., and 100° C. in each zone and a rotation speed of 60 rpm;
[0077] The raw materials of the two EVA layers were placed in a twin-screw extruder respectively, and the temperatures of each zone were 80°C, 95°C, 90°C, and 95°C respectively. The raw materials were melt-blended at a rotation speed of 50 rpm, and discharged through a co-extrusion cast film die, pulled, stretched, and formed into a film.
[0078] The first adhesive film layer 101 has a thickness of 50-100 μm, the second adhesive film layer 102 has a thickness of 30-90 μm, and the POE adhesive film layer 201 has a thickness of 20-80 μm. The thickness of the first adhesive film layer 101 is greater than the thickness of the second adhesive film layer 102, and the thickness of the POE adhesive film layer is less than the thickness of the second adhesive film layer 102.
[0079] Specifically, in step three, the film is irradiated with a mercury or halogen light source with a UV wavelength of 300-400nm, and the stretched film is cooled, pulled, and rolled up to obtain a photovoltaic encapsulation film.
[0080] A photovoltaic module, such as Figure 5 As shown, it includes a front transparent packaging layer 30, a first photovoltaic packaging adhesive layer 10, a battery cell array 20, a second photovoltaic packaging adhesive layer 40 and a back packaging layer, the first photovoltaic packaging adhesive layer 10 and the second photovoltaic packaging adhesive layer 40 are the photovoltaic packaging adhesive layers described in any of the above embodiments, and in the first photovoltaic packaging adhesive layer 10 and / or the second photovoltaic packaging adhesive layer 40, the first adhesive film layer 101 is arranged on the side of the POE adhesive film layer 201 away from the battery cell array 20.
[0081] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with specific implementation methods.
[0082] Example 1
[0083] The embodiment of the present application provides a photovoltaic encapsulation adhesive, comprising a first adhesive film layer, a POE adhesive film layer, and a second adhesive film layer stacked in sequence;
[0084] The POE film layer is filled with a number of transparent inorganic particles, and the thickness of the first film layer is greater than the thickness of the second film layer, so that the neutral layer of the photovoltaic encapsulation glue is close to the interface between the first film layer and the POE film layer;
[0085] Wherein, the transparent inorganic particles are TiO2, with a particle size of 10um, and the mass ratio of POE material to TiO2 in the POE film layer is 8:2;
[0086] The first adhesive film layer and the second adhesive film layer are made of the same material, including 100 parts of the EVA resin; 0.8-1.2 parts of a cross-linking agent; 0-3 parts of a UV absorber; and 0.1-0.2 parts of an antioxidant.
[0087] Specifically, the EVA resin is 100 parts; the cross-linking agent is 0.8 parts; the UV absorber is 1 part; the antioxidant is 0.1 parts;
[0088] The crosslinking agent includes dipentaerythritol hexaacrylate, diethylene glycol diacrylate phthalate, 1,6-hexanediol dimethacrylate, TAIC (triallyl isocyanurate), and PL-400, which are mixed in a weight ratio of 4:1:2:3:1;
[0089] Wherein, the UV absorber includes UV531;
[0090] The antioxidant is a mixture of phenols and phosphites, specifically a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 4:3.
[0091] Among them, the thickness of the photovoltaic encapsulation glue is 260um, the thickness of the first glue film layer is 120um, the thickness of the second glue film layer is 80um, and the thickness of the POE glue film layer is 60um.
[0092] Example 2
[0093] The present application embodiment provides a photovoltaic encapsulation adhesive, which is the same as embodiment 1, except that:
[0094] The first adhesive film layer contains TiO2 with a particle size of 10 um, and the mass ratio of the EVA resin to TiO2 is 10:1.
[0095] Example 3
[0096] The present application embodiment provides a photovoltaic encapsulation adhesive, which is the same as embodiment 1, except that:
[0097] The transparent inorganic particles in the POE film layer are TiO2, and the transparent inorganic particles include a mixture of first inorganic particles and second inorganic particles. The particle size of the first inorganic particles is 5um, the particle size of the second inorganic particles is 30um, and the mass ratio of the first inorganic particles to the second inorganic particles is 1:3.
[0098] Example 4
[0099] The present application embodiment provides a photovoltaic encapsulation adhesive, which is the same as embodiment 1, except that:
[0100] The transparent inorganic particles in the POE film layer are TiO2, and the transparent inorganic particles include a mixture of first inorganic particles and second inorganic particles. The particle size of the first inorganic particles is 5um, the particle size of the second inorganic particles is 20um, and the mass ratio of the first inorganic particles to the second inorganic particles is 1:3.
[0101] Example 5
[0102] The present application embodiment provides a photovoltaic encapsulation adhesive, which is the same as embodiment 1, except that:
[0103] The transparent inorganic particles in the POE adhesive film layer are modified TiO2, specifically polysiloxane-modified TiO2.
[0104] The polysiloxane-modified TiO2 can be seen in the above examples.
[0105] Example 6
[0106] The present application embodiment provides a photovoltaic encapsulation adhesive, which is the same as embodiment 1, except that:
[0107] The transparent inorganic particles in the POE film layer are irregular TiO2 particles.
[0108] Comparative Example 1
[0109] The embodiment of the present application provides a photovoltaic encapsulation adhesive, which is the same as embodiment 1, except that transparent inorganic particles are not doped in the POE layer.
[0110] Comparative Example 2
[0111] The embodiment of the present application provides a photovoltaic encapsulation adhesive, which is the same as embodiment 1, except that the thickness of the first adhesive film layer and the second adhesive film layer are the same, both of which are 120 um.
[0112] Comparative Example 3
[0113] The embodiment of the present application provides a photovoltaic encapsulation adhesive, which is the same as embodiment 1, except that the thickness of the first adhesive film layer and the second adhesive film layer are the same, both of which are 120 um, and the POE layer is not doped with transparent inorganic particles.
[0114] Detection Example
[0115] The three-layer composite photovoltaic encapsulation adhesive films prepared in the embodiments and comparative examples are respectively used to assemble a double-glass module, and the steps are as follows:
[0116] (1) Laying adhesive film, battery cell, adhesive film and glass on the glass in sequence; the second adhesive film layer is attached close to the battery cell;
[0117] (2) Place the laminate in a laminator for heating, vacuuming, laminating, and pressure-maintaining, then take it out and cool it to obtain a double-glass component.
[0118] The test method is as follows:
[0119] 1. Thermal conductivity: Refer to ASTM-E1461. The film is made into a square sheet with a side length of 10 mm and a thickness of 1 mm, and its thermal conductivity is tested using a laser thermal conductivity tester.
[0120] 2. Light transmittance: The test was conducted according to the method described in GB / T 29848-2013 “Ethylene-vinyl acetate copolymer (EVA) adhesive film for photovoltaic module encapsulation”. The results are shown in Table 1.
[0121] 3. According to IEC 61215-2021, each double-glass module was subjected to DH test, with humidity of 85%, temperature of 85°C and placement time of 1000h. The appearance test results before and after DH1000h are shown in Table 1;
[0122] 4. UV aging: The obtained film was subjected to UV irradiation aging test according to the requirements of the International Electrotechnical Commission standard IEC61345. Test conditions: the surface temperature of the test piece is 60±5℃, the UV wavelength range is 280-400nm, and the irradiation intensity is 15kW·h / m 2 The UV irradiation test time is 2000 hrs. The results are shown in Table 1.
[0123] 5. PID power attenuation: The PID of the photovoltaic module was tested according to the industry standard IEC 62804. The test conditions were: 1500V voltage, 85°C, 85% relative humidity, 192h. The results are shown in Table 1.
[0124] 6. Test the encapsulation films of various embodiments and comparative examples according to the method of GB / T 29848-2013; and test the power of each component according to the IEC61215 standard, and calculate its gain efficiency.
[0125] Table 1
[0126]
[0127] As can be seen from Table 1, by comparing Example 1, Example 2 and Comparative Example 1, it can be seen that by adding transparent inorganic particles, the thermal conductivity of the encapsulation film can be effectively improved, so that the heat generated by the photovoltaic element can be relieved in time, thereby improving the service life of the element;
[0128] By comparing Examples 1-6, it can be seen that after adding transparent inorganic particles, the transmittance of the device decreases slightly. It should be noted that the higher the transmittance of the film, the higher the light utilization rate of the battery cell after its encapsulation; the higher the haze of the film, the light trapping effect of the film is not necessarily the best. The present application achieves a better balance between transparency and haze by doping with an appropriate amount of transparent inorganic particles, while at the same time improving the light conversion efficiency of photovoltaic modules to a certain extent.
[0129] By comparing Examples 1-6 and Comparative Examples 1-3, it can be seen that after doping with transparent inorganic particles, although the visible light transparency is slightly reduced and the haze is increased, the overall gain efficiency is partially improved.
[0130] By comparing Example 1 with Comparative Example 1, it can be seen that after doping with transparent inorganic particles, the bubble content in the obtained three-layer composite film is significantly reduced.
[0131] By comparing Example 1 with Comparative Example 1, it can be seen that by adding transparent inorganic particles, especially titanium dioxide, it can effectively adsorb free acetic acid, so that the photovoltaic encapsulation film has better anti-PID performance;
[0132] By comparing Example 1 and Comparative Example 2, it can be seen that by specifically limiting the thickness of the first adhesive film layer and the second adhesive film layer, the anti-P ID performance of the photovoltaic encapsulation film can also be improved to a certain extent.
[0133] Peel force: Each double-glass component is hot-pressed and laminated at 145°C, and then tested according to the test method provided in GB / T29848-2018;
[0134] The components were tested under the following conditions: +85°C, relative humidity 85%, DH 2000h and then the above operation was repeated. The test results are shown in Table 2.
[0135] Table 2
[0136]
[0137] It can be seen from Table 2 that by adding transparent inorganic particles to the POE layer and controlling the thickness of the first adhesive film layer and the second adhesive film layer, the interlayer force of the encapsulation adhesive film layer is enhanced;
[0138] Adding transparent inorganic particles to the first adhesive film layer can increase the force of the film layer to a certain extent, but it also provides a path for water and oxygen to invade, so its packaging effect is relatively inferior;
[0139] Adding modified titanium dioxide to the POE layer can increase the force of the film layer. At the same time, since the surface of titanium dioxide is modified by organic groups, the dispersion of titanium dioxide is improved, the molecular force between the film layers is further enhanced, and the anti-PID performance of the photovoltaic encapsulation film can also be improved.
[0140] The photovoltaic encapsulation adhesive and its preparation method and photovoltaic module provided in the embodiments of the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A photovoltaic encapsulation adhesive, It is characterized in that include: A first adhesive film layer, a POE adhesive film layer, and a second adhesive film layer stacked in sequence; The POE film layer is filled with a number of transparent inorganic particles, the thickness of the first film layer is greater than the thickness of the second film layer, so that the neutral layer of the photovoltaic encapsulation glue is close to the interface between the first film layer and the POE film layer, and the thickness of the POE film layer is less than the thickness of the second film layer; The thermal conductivity of the transparent inorganic particles is greater than or equal to 3.9 W / (m·K), and the particle size of the transparent inorganic particles is in the range of 5-30 μm.
2. The photovoltaic encapsulation adhesive according to claim 1, It is characterized in that The transparent inorganic particles include TiO 2 , silicon nitride, and one or more combinations thereof, wherein the doping amount of the transparent inorganic particles in the POE film layer is 10-20wt%.
3. The photovoltaic encapsulation adhesive according to claim 1, It is characterized in that The transparent inorganic particles are modified TiO 2 , the modified TiO 2 TiO modified with organic groups 2 , the organic group includes a silane coupling group.
4. The photovoltaic encapsulation adhesive according to claim 1, It is characterized in that The transparent inorganic particles include a mixture of first inorganic particles and second inorganic particles, the particle size of the first inorganic particles is 5-10 um, the particle size of the second inorganic particles is 20-30 um, and the mass ratio of the first inorganic particles to the second inorganic particles is 1:(1-3).
5. The photovoltaic encapsulation adhesive according to claim 1, It is characterized in that The first adhesive film layer and the second inorganic adhesive film layer are made of the same material, and both include transparent EVA resin, a cross-linking agent, a UV absorber and an antioxidant.
6. The photovoltaic encapsulation adhesive according to claim 1, It is characterized in that The first adhesive film layer is filled with a plurality of transparent inorganic particles.
7. The photovoltaic encapsulation adhesive according to claim 6, It is characterized in that The photovoltaic encapsulation adhesive has a thickness of about 200-500 μm, the first adhesive film layer and the second adhesive film layer have thicknesses of 50-100 μm and 30-90 μm respectively, and the POE adhesive film layer has a thickness of 20-80 μm.
8. The photovoltaic encapsulation adhesive according to claim 1, It is characterized in that The POE adhesive film layer also includes a cross-linking agent, a UV absorber, and an antioxidant.
9. The method for preparing the photovoltaic encapsulation adhesive according to claim 1, It is characterized in that include: Step 1: Prepare POE film layer: POE material and transparent inorganic particles are blended and then extruded into granules to obtain POE masterbatch; Step 2: Three-layer lamination, the raw material of the first film, the POE masterbatch and the raw material of the second film are compounded by melt lamination; Step 3: shaping treatment, subjecting the three-layer film compounded in step 2 to UV curing and shaping treatment to obtain a photovoltaic module encapsulation film.
10. A photovoltaic module, comprising a front transparent encapsulation layer, a first photovoltaic encapsulation adhesive layer, a cell array, a second photovoltaic encapsulation adhesive layer and a back encapsulation layer, It is characterized in that The first photovoltaic encapsulation adhesive layer and the second photovoltaic encapsulation adhesive layer are the photovoltaic encapsulation adhesive layers described in any one of claims 1 to 8, and in the first photovoltaic encapsulation adhesive layer and / or the second photovoltaic encapsulation adhesive layer, the first adhesive film layer is arranged on the side of the POE adhesive film layer away from the battery cell array.
Citation Information
Cited By
Photovoltaic packaging adhesive film for BC battery and preparation method of photovoltaic packaging adhesive film