Production method for aluminum alloy ingot, continuously cast aluminum alloy rod, and forged aluminum alloy product

By controlling element composition and employing a two-step melting process, the method addresses the issue of coarsely grown compounds in aluminum alloy scrap utilization, enhancing mechanical properties and energy efficiency in producing aluminum alloy ingots.

JP2024167695APending Publication Date: 2024-12-04RESONAC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023083946
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

The utilization of aluminum alloy scrap in producing aluminum alloys results in the formation of coarsely grown Al-Fe-Mn-Si compounds, which deteriorate the mechanical properties of the product, and increases energy consumption during the melting process.

Method used

A method for producing aluminum alloy ingots by controlling the composition of elements such as Cu, Mg, Si, Mn, Fe, Cr, Ti, B, and Zr within specific ranges, and employing a two-step melting process to refine the alloy, including a primary and secondary melting step to adjust the Si content, thereby suppressing the formation of coarse compounds and improving energy efficiency.

Benefits of technology

This method enables the production of high-quality 6000 series aluminum alloy ingots with improved mechanical properties and reduced energy consumption by refining the alloy composition and optimizing the melting process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167695000001_ABST
    Figure 2024167695000001_ABST
Patent Text Reader

Abstract

To provide a production method for a 6000-series aluminum alloy ingot which can suppress coarsening of a compound of Al-Fe-Mn-Si produced by elements mixed from aluminum alloy scrap while utilizing the scrap.SOLUTION: A production method for an aluminum alloy ingot includes: a primary melting step of obtaining a primary molten metal by melting raw materials including aluminum alloy scrap and an aluminum metal and having the same composition range of the additive elements as that of the aluminum alloy ingot except that an Si content ratio of 0.60 mass% or more and 0.90 mass% or less, so as to charge the aluminum alloy scrap and the aluminum metal in ascending order of melting points, and melting the materials and obtaining primary molten metal; and a secondary melting step of adding metal Si or Si-containing alloy to the obtained primary molten metal or molten metal in which an ingot obtained by solidifying the primary molten metal is molt, and adjusting the Si content ratio to be within a range of 0.90 mass% or more and 1.9% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an aluminum alloy ingot, a continuously cast aluminum alloy rod, and an aluminum alloy forged product. [Background technology]

[0002] In recent years, amid the global trend toward carbon neutrality, reducing CO2 emissions from manufacturing processes has become an issue. In order to reduce CO2 emissions during aluminum production, it is important to utilize scrap aluminum alloys, which have a lower melting point than pure aluminum (purity of 99.0% or more), in order to improve the energy consumption rate during melting.

[0003] Methods for manufacturing aluminum alloys and aluminum alloy products using aluminum alloy scrap as a raw material are known (e.g., Patent Documents 1 to 3). Aluminum alloy scrap is recovered from used aluminum products, and is produced as a recycled raw material by melting and adjusting the composition, and is used as the raw material for aluminum alloys. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2020-514556 [Patent Document 2] Special Publication No. 2020-527653 [Patent Document 3] JP 2022-137762 A Summary of the Invention [Problem to be solved by the invention]

[0005] When utilizing scrap aluminum alloys as raw materials for aluminum alloys derived from recycled materials, for example, when using scrap for 6000 series alloys, it is preferable to use scrap with a high purity, such as 6063 sash scraps generated from building materials. However, impurities such as Si, Fe, and Mn are mixed in from the scrap. If these compounds (e.g. Al-Fe-Mn-Si) grow coarsely and are present in the cast rod during the melting and casting process, the mechanical properties of the product will decrease.

[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for producing a 6000 series aluminum alloy ingot, which can utilize aluminum alloy scrap available on the market in the production of aluminum alloys, while suppressing coarsening of Al-Fe-Mn-Si compounds generated by elements mixed in from the aluminum alloy scrap, and can improve the fuel consumption rate in the melting process, while at the same time making use of aluminum alloy scrap available on the market. An object of the present invention is to provide a method for producing a 6000 series aluminum alloy ingot, a continuous cast aluminum alloy rod, and an aluminum alloy forged product. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides the following means.

[0008] A first aspect of the present invention is an aluminum alloy for producing an aluminum alloy ingot containing additive elements in the range of 0.30 mass% to 1.0 mass%, Cu in the range of 0.80 mass% to 1.8 mass%, Si in the range of 0.90 mass% to 1.9 mass%, Mn in the range of 0.30 mass% to 1.2 mass%, Fe in the range of 0.20 mass% to 0.65 mass%, Zn in the range of 0.25 mass% or less, Cr in the range of 0.050 mass% to 0.30 mass%, Ti in the range of 0.01 mass% to 0.1 mass%, B in the range of 0.0010 mass% to 0.030 mass%, and Zr in the range of 0.0010 mass% to 0.050 mass%, with the balance being Al and unavoidable impurities. The method for producing an aluminum alloy ingot includes a primary melting step in which raw materials including aluminum alloy scrap and aluminum ingot, the raw materials having the same compositional range as that of the aluminum alloy ingot except for a Si content of 0.60% by mass or more and 0.90% by mass or less, are charged, and the aluminum alloy scrap and the aluminum ingot are charged in order of decreasing melting point to obtain a primary molten metal by melting them, and a secondary melting step in which metallic Si or a Si-containing alloy is added to the primary molten metal obtained in the primary melting step or to a molten metal obtained by melting an ingot obtained by solidifying the primary molten metal, to adjust the Si content to within the range of 0.90% by mass or more and 1.9% by mass or less.

[0009] A second aspect of the present invention is the method for producing an aluminum alloy ingot according to the first aspect, wherein the aluminum alloy scrap is one or more of scrap containing a 3000 series alloy, scrap containing a 4000 series alloy, scrap containing a 5000 series alloy, and scrap containing a 6000 series alloy.

[0010] A third aspect of the present invention is a continuously cast aluminum alloy rod obtained by using an aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to the first or second aspect, and having a 0.2% yield strength of 350 MPa or more.

[0011] A fourth aspect of the present invention is an aluminum alloy forging obtained by using the continuously cast aluminum alloy rod according to the third aspect, and having a 0.2% yield strength of 370 MPa or more. Effect of the Invention

[0012] According to the manufacturing method of an aluminum alloy ingot of the present invention, it is possible to provide a manufacturing method of a 6000 series aluminum alloy ingot that can utilize aluminum alloy scrap available on the market while suppressing coarsening of Al-Fe-Mn-Si compounds generated by elements mixed in from the aluminum alloy scrap. [Brief description of the drawings]

[0013] [Figure 1] (a) is a conceptual diagram of the case where the primary molten metal obtained in the primary melting process is solidified into an ingot and then the ingot is fed into the secondary melting process, and (b) is a conceptual diagram of the case where the primary molten metal obtained in the primary melting process is fed directly into the secondary melting process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In addition, the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality. Furthermore, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not necessarily limited to them, and may be appropriately modified and implemented within the scope that does not change the effects of the present invention.

[0015] [Method of manufacturing aluminum alloy ingots] An aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to this embodiment will be described. The aluminum alloy ingot of this embodiment contains additive elements in the range of 0.30 mass% or more and 1.0 mass% or less, Cu in the range of 0.80 mass% or more and 1.8 mass% or less, Si in the range of 0.90 mass% or more and 1.9 mass% or less, Mn in the range of 0.30 mass% or more and 1.2 mass% or less, Fe in the range of 0.20 mass% or more and 0.65 mass% or less, Zn in the range of 0.25 mass% or less, Cr in the range of 0.050 mass% or more and 0.30 mass% or less, Ti in the range of 0.01 mass% or more and 0.1 mass% or less, B in the range of 0.0010 mass% or more and 0.030 mass% or less, Zr in the range of 0.0010 mass% or more and 0.050 mass% or less, with the balance being Al and unavoidable impurities.

[0016] The aluminum alloy ingot of this embodiment corresponds to a forged product of a 6000 series aluminum alloy in that it contains Mg and Si.

[0017] (Cu: 0.30 mass% or more, 1.0 mass% or less) Cu has the effect of finely dispersing Mg-Si compounds in the aluminum alloy and the effect of improving the tensile strength of the aluminum alloy by precipitating as Al-Cu-Mg-Si compounds including the Q phase. By keeping the Cu content within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.

[0018] (Mg: 0.80 mass% or more, 1.8 mass% or less) Mg has the effect of improving the tensile strength of aluminum alloys. Mg contributes to strengthening of aluminum alloys by dissolving in the aluminum parent phase or precipitating as Mg-Si compounds (Mg2Si) such as β” phase, or Al-Cu-Mg-Si compounds (AlCuMgSi) such as Q phase. Mg2Si also has the effect of suppressing the formation of CuAl2 phase in the aluminum alloy. Suppressing the formation of CuAl2 phase improves the corrosion resistance of aluminum alloy ingots. By keeping the Mg content within the above range, it is possible to improve the corrosion resistance as well as the mechanical properties at room temperature of the aluminum alloy ingot.

[0019] (Si: 0.90 mass% or more, 1.9 mass% or less) Like Mg, Si has the effect of improving the mechanical properties and corrosion resistance of an aluminum alloy ingot at room temperature. However, if an excessive amount of Si is added to an aluminum alloy, coarse primary crystal Si grains may crystallize, which may reduce the tensile strength of the aluminum alloy. By keeping the Si content within the above range, it is possible to improve the mechanical properties and corrosion resistance of an aluminum alloy ingot at room temperature while suppressing the crystallization of primary crystal Si.

[0020] (Mn: 0.30 mass% or more, 1.2 mass% or less) Mn has the effect of improving the tensile strength of the aluminum alloy by forming fine granular precipitates including intermetallic compounds such as Al-Mn-Fe-Si and Al-Mn-Cr-Fe-Si in the aluminum alloy. By keeping the Mn content within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.

[0021] (Fe: 0.20 mass% or more, 0.65 mass% or less) Fe has the effect of improving the tensile strength of the aluminum alloy by crystallizing in the aluminum alloy as fine crystals including intermetallic compounds such as Al-Mn-Fe-Si, Al-Mn-Cr-Fe-Si, Al-Fe-Si, Al-Cu-Fe, and Al-Mn-Fe. By keeping the Fe content within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved. The Fe / Mn relationship is less than 1.4. By having the Fe / Mn relationship be less than 1.4, crystallization of AlFeSi-based compounds having sizes of 2.0 μm or more can be suppressed, and mechanical properties can be improved.

[0022] (Cr: 0.050 mass% or more, 0.30 mass% or less) Cr has the effect of improving the tensile strength of the aluminum alloy by forming fine granular crystallized products containing intermetallic compounds such as Al-Mn-Cr-Fe-Si and Al-Fe-Cr in the aluminum alloy. By keeping the Cr content within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.

[0023] (Ti: 0.010 mass% or more, 0.10 mass% or less) Ti has the effect of refining the crystal grains of an aluminum alloy and improving the wrought workability. If the Ti content is less than 0.010% by mass, the effect of refining the crystal grains may not be sufficiently obtained. On the other hand, if the Ti content exceeds 0.10% by mass, coarse crystallized products may be formed, and the wrought workability may be deteriorated. In addition, if a large amount of coarse crystallized products containing Ti are mixed into an aluminum alloy ingot, the toughness may be deteriorated. Therefore, the Ti content is set to 0.010% by mass or more and 0.10% by mass or less. The Ti content is preferably 0.015% by mass or more and 0.050% by mass or less.

[0024] (B: 0.0010 mass% or more, 0.030 mass% or less) B has the effect of refining the crystal grains of the aluminum alloy and improving the wrought workability. By adding B to the aluminum alloy together with Ti, the effect of refining crystal grains is improved. If the content of B is less than 0.0010% by mass, the effect of refining crystal grains may not be sufficiently obtained. On the other hand, if the content of B exceeds 0.030% by mass, coarse crystallized matter may be formed and may be mixed into the aluminum alloy ingot as inclusions. In addition, if a large amount of coarse crystallized matter containing B is mixed into the final product of the aluminum alloy, the toughness may decrease. Therefore, the content of B is set to 0.0010% by mass or more and 0.030% by mass. The content of B is preferably 0.0050% by mass or more and 0.025% by mass.

[0025] (Zr: 0.0010 mass% or more, 0.050 mass% or less) When the Zr content is 0.050% by mass or less, it precipitates in the form of Al3Zr and Al-(Ti,Zr), which contributes to improving the strength of the aluminum alloy ingot through recrystallization suppression effect and precipitation strengthening. However, when the Zr content exceeds 0.050% by mass, it crystallizes as coarse Zr compounds, which may lead to a decrease in the corrosion resistance of the aluminum alloy ingot. For this reason, the Zr content is set to 0.050% by mass or less. In order to obtain the above-mentioned recrystallization suppression effect and the effect of improving the strength of the forged product through precipitation strengthening, the Zr content is preferably 0.0010% by mass or more.

[0026] (Zn: 0.250% by mass or less) The Zn content may be 0.250% by mass or less. If the Zn content exceeds 0.250% by mass, MgZn2 is generated and precipitates from the Al matrix to the grain boundaries, causing intergranular corrosion and leading to a decrease in the corrosion resistance of the aluminum alloy ingot. For this reason, it is preferable that the Zn content is 0.250% by mass or less, or that it is not contained at all.

[0027] (Inevitable impurities) Inevitable impurities are impurities that are inevitably mixed into the aluminum alloy from the raw materials or manufacturing process of the aluminum alloy ingot. Examples of inevitable impurities include Ni, Sn, Be, etc. The content of these inevitable impurities preferably does not exceed 0.1 mass%.

[0028] [Method of manufacturing aluminum alloy ingots] Next, a method for producing an aluminum alloy ingot according to this embodiment will be described. The aluminum alloy ingot of this embodiment can be produced, for example, by a method including a melting (molten metal formation) step and a casting step.

[0029] (melting process) In the melting (molten metal formation) process, a molten metal of an aluminum alloy is formed. In the method for producing an aluminum alloy ingot according to the present embodiment, the melting (molten metal formation) step is composed of two sub-steps (a primary melting step and a secondary melting step).

[0030] <1st dissolution process> In the primary melting step, raw materials including aluminum alloy scrap and aluminum ingot (aluminum ingot), which have the same composition ranges of contents of the above-mentioned added elements (Cu, Mg, Mn, Fe, Zn, Cr, Ti, B, Zr) as those of the aluminum alloy ingot to be produced except for the Si content being 0.60 mass% or more and 0.90 mass% or less, are charged, and the aluminum alloy scrap and aluminum ingot are charged in order of decreasing melting point, and melted to obtain a primary molten metal.

[0031] The primary molten metal obtained in the primary melting step may be solidified into an ingot, or may be transferred as is to a melting furnace in which the secondary melting step is carried out. FIG. 1 is a conceptual diagram showing such a configuration. FIG. 1(a) is a conceptual diagram showing a flow in which raw materials including blended aluminum alloy scrap are prepared, the raw materials are then charged into a primary melting furnace to carry out a primary melting process to obtain a primary molten metal, the primary molten metal is temporarily solidified into an ingot, and the ingot is used as a raw material to carry out a secondary melting process in a secondary melting furnace to obtain a secondary molten metal. On the other hand, FIG. 1(b) is a conceptual diagram showing a flow in which raw materials including blended aluminum alloy scrap are prepared, the raw materials are then charged into a primary melting furnace to carry out a primary melting process to obtain a primary molten metal, and the primary molten metal is transferred directly to a secondary melting furnace through a trough, where the secondary melting process is carried out to obtain a secondary molten metal.

[0032] In the first melting process, the aluminum alloy scrap and aluminum ingot are charged first, starting with the one with the lowest melting point. After the first scrap is completely melted, the next aluminum alloy scrap and aluminum ingot, whichever has the lowest melting point, are charged, and after the first scrap is completely melted, the next aluminum alloy scrap and aluminum ingot, whichever has the lowest melting point, are charged in this order. After the aluminum alloy scrap and aluminum ingot charged are completely melted, additive metals such as Cu scrap and mother alloy are charged. Examples of aluminum alloy scrap include scrap of Al-Mn-based (3000 series) alloys, such as aluminum cans and recycled aluminum can blocks, scrap of Al-Si-based (4000 series) alloys, such as ADC12 and A356, scrap of Al-Mg-based (5000 series) alloys, such as 5052 and 5083, and scrap of Al-Mg-Si-based (6000 series) alloys, such as 6063 and 6061. Aluminum bullion (pure aluminum) is classified into normal purity bullion, high purity bullion, and alloy bullion based on its purity and composition, and can be divided into ingots (cast metal for general raw material use), slabs (cast metal prepared for rolling), billets (cast metal prepared for extrusion), etc. based on its shape and use.

[0033] When the Si content is less than 0.60 mass%, for example, the Si content is adjusted to within the range of 0.60 mass% to 0.90 mass% by adding metal Si or a Si-containing alloy. Metal Si is preferred as the additive material because it is easy to adjust. When the Si content exceeds 0.90% by mass, aluminum ingot or aluminum alloy scrap with a low Si content is added to adjust the Si content to within a range of 0.60% to 0.90% by mass. Examples of aluminum alloy scrap with a low Si content include 3000 series alloy scrap, scrap containing 5000 series alloy, and scrap containing 6000 series alloy. The Si content (component analysis) can be carried out, for example, by emission spectrometry.

[0034] When Si, Fe, and Mn are mixed in scrap and melted, Al-Fe-Mn-Si compounds are generated at a certain temperature range during the melting process. The amount of this compound is particularly affected by the amount of Si. If the amount of compound increases, it is necessary to set the melting temperature to 850°C or higher in order to melt them. This is not desirable because it increases the energy used during melting. Furthermore, if the Si content falls below 0.6 mass%, the amount of Si added in the secondary melting step will be too large, and it will take time for all the added Si to melt, resulting in energy loss. Therefore, the Si content of the alloy composition obtained in the primary melting step must be 0.60 mass% or more and 0.90 mass% or less.

[0035] The higher the usage ratio (mixture ratio) of aluminum alloy scrap in the raw materials, the more preferable it is in terms of improving the energy consumption rate during melting. The blending ratio of the aluminum alloy scrap can be, for example, 50% or more. For example, it can be 60% or more, 70% or more, 80% or more, 90% or more, or 100%. On the other hand, the blending ratio of the aluminum alloy scrap can be less than 50%, for example, 40%, 30%, 20%, or 10%, although the effect of improving the energy consumption rate during melting is reduced.

[0036] The melting point of pure aluminum ingot is approximately 660°C. In contrast, ADC12, for example, has a melting point of 570°C, and even other aluminum alloys have melting points below 650°C, which is more than 10°C lower. This makes it easier to melt, and by utilizing this, the energy consumption during melting can be improved.

[0037] The aluminum alloy scrap can be used within the composition range of Al-Si (4000 series) alloys such as ADC12 and A356 containing 4 mass% to 12 mass% Si and 0.01 mass% to 3.0 mass% Cu, Al-Mn (3000 series) alloys containing 0.7 mass% to 1.4 mass% Mn and 0.5 mass% to 1.4 mass% Mg such as other aluminum cans and recycled aluminum can chunks, Al-Mg (5000 series) alloys such as 5052 and 5083 containing 2.0 mass% to 5.0 mass% Mg, and Al-Mg-Si (6000 series) alloys such as 6063 and 6061 containing 0.2 mass% to 0.8 mass% Si and 0.45 mass% to 1.2 mass% Mg. Aluminum can scraps are usually used after undergoing a heat treatment process at 400 to 500 degrees Celsius to remove the paint from the surface of the cans before being melted down. By adding an Al-Si alloy, the amount of Si added in the secondary melting process can be reduced, so it is preferable to use this in combination with scrap of other alloys.

[0038] <Secondary melting process> The secondary melting process is a process in which metal Si or a Si-containing alloy is added to the primary molten metal obtained in the primary melting process or to the molten metal obtained by melting an ingot obtained from the primary molten metal, to adjust the Si content to 0.90% by mass or more and 1.9% by mass. Metal Si is preferable as the additive material because it is easy to adjust.

[0039] The composition adjustment here is carried out at 700°C or higher and 800°C or lower. If the temperature is below 700°C, the Al-Fe-Mn-Si compounds will grow coarsely due to the temperature drop in the molten metal path when the molten metal is cast, impairing the mechanical properties of the product. Also, if the temperature exceeds 800°C, the amount of hydrogen dissolved in the air increases in the molten aluminum, increasing the amount of hydrogen gas in the molten metal, resulting in porosity in the cast product and impairing the mechanical properties. Therefore, the temperature should be between 700°C and 800°C.

[0040] (Casting process) The molten metal obtained in the secondary melting process is flux-treated, then undergoes GBF (gas bubbling filtration) treatment before being poured into a casting mold. The poured molten metal is continuously cast by either vertical continuous casting or horizontal continuous casting to obtain an aluminum alloy continuously cast rod.

[0041] In the method for producing an aluminum alloy ingot according to this embodiment, a melting facility may be used in which a melting furnace for performing a primary melting step and a melting furnace for adjusting the composition are arranged in series and connected by a trough, and the primary molten metal obtained in the primary melting step can be transferred to the melting furnace for adjusting the composition without casting.

[0042] [Aluminum alloy continuous casting rod] The continuously cast aluminum alloy rod of this embodiment is produced by carrying out continuous casting using an aluminum alloy ingot obtained by the method for producing an aluminum alloy ingot of this embodiment, by either vertical continuous casting or horizontal continuous casting, and has a 0.2% yield strength of 350 MPa or more.

[0043] [Aluminum alloy forgings] The aluminum alloy forged product according to this embodiment is manufactured using the aluminum alloy continuously cast rod according to this embodiment, and has a 0.2% yield strength of 370 MPa or more. For example, the aluminum alloy continuously cast rod according to the present embodiment can be subjected to a homogenization heat treatment step, a forging step, a solution treatment step, a quenching treatment step, and an aging treatment step to produce the aluminum alloy forged product according to the present embodiment. EXAMPLES

[0044] Next, specific examples of the present invention will be described, but the present invention is not limited to these examples.

[0045] (Example of aluminum alloy scrap) Table 1 shows the component analysis values ​​(mass%) of each scrap obtained by emission spectroscopy of aluminum alloy scrap obtained from secondary alloy manufacturers and scrap manufacturers. The component analysis was carried out in accordance with the emission spectroscopy analysis of aluminum and aluminum alloys specified in JIS H1305 2005. The melting point was measured by measuring the melting temperature of the sample using differential scanning calorimetry (DSC).

[0046] [Table 1]

[0047] (Examples, Comparative Examples 1 and 2) In the examples and comparative examples 1 and 2, the combinations (mixtures) of aluminum alloy scrap and aluminum ingot shown in Table 1 were made using raw materials with the mixing ratios shown in Table 2.

[0048] [Table 2]

[0049] In all of the examples and comparative examples 1 and 2, the contents of the additive elements other than Si were as follows: Cu in the range of 0.30 mass% or more and 1.0 mass% or less, Mg in the range of 0.80 mass% or more and 1.8 mass% or less, Mn in the range of 0.30 mass% or more and 1.2 mass% or less, Fe in the range of 0.20 mass% or more and 0.65 mass% or less, Zn in the range of 0.25 mass% or less, Cr in the range of 0.050 mass% or more and 0.30 mass% or less, Ti in the range of 0.01 mass% or more and 0.1 mass% or less, B in the range of 0.0010 mass% or more and 0.030 mass% or less, Zr in the range of 0.0010 mass% or more and 0.050 mass% or less, with the balance being Al and unavoidable impurities. Furthermore, in the examples, the Si content was blended so as to be within the range of 0.60 mass% or more and 0.90 mass% or less, whereas in the comparative examples, the Si content was blended so as to be outside the range of 0.60 mass% or more and 0.90 mass% or less.

[0050] In the examples, the raw materials were fed into a 15-ton melting furnace in the order of lowest melting point, and the entire amount was melted at a melting temperature of 780° C. On the other hand, in the comparative examples, the raw materials were fed into a 15-ton melting furnace in the order of highest melting point (Comparative Example 1), or in a random order, neither in order of lowest nor highest melting point (Comparative Example 2), and the entire amount was melted at a melting temperature of 780° C. The amount of LNG used to dissolve 1 ton in the examples and comparative examples (unit: [m 3 / Ton] was measured. LNG consumption is 100 [m 3 / Ton] less than 〇, 100 [m 3 / Ton] or more was judged as ×. The results are shown in Table 3.

[0051] [Table 3]

[0052] From Table 3, the amount of LNG used in the example is 85 [m 3 / Ton], whereas in Comparative Example 1 it was 120 [m 3 / Ton], and in Comparative Example 2, it was 115 [m 3 / Ton]. It was shown that feeding the raw materials, aluminum alloy scrap and aluminum ingot, into a melting furnace in the order of lowest melting point improves the energy consumption during melting compared to feeding the raw materials in the order of highest melting point, or feeding them randomly, neither in order of lowest nor highest melting point.

Claims

1. 1. A method for producing an aluminum alloy ingot containing additive elements in the range of 0.30% by mass to 1.0% by mass, Cu in the range of 0.80% by mass to 1.8% by mass, Si in the range of 0.90% by mass to 1.9% by mass, Mn in the range of 0.30% by mass to 1.2% by mass, Fe in the range of 0.20% by mass to 0.65% by mass, Zn in the range of 0.25% by mass or less, Cr in the range of 0.050% by mass to 0.30% by mass, Ti in the range of 0.01% by mass to 0.1% by mass, B in the range of 0.0010% by mass to 0.030% by mass, and Zr in the range of 0.0010% by mass to 0.050% by mass, with the balance being Al and inevitable impurities, a primary melting step of charging raw materials including aluminum alloy scrap and aluminum ingot, the raw materials having the same content ratios of the additive elements as those of the aluminum alloy ingot except that the content ratio of Si is 0.60% by mass or more and 0.90% by mass or less, wherein the aluminum alloy scrap and the aluminum ingot are charged in order of decreasing melting point and melted to obtain a primary molten metal; and a secondary melting step of adding metallic Si or a Si-containing alloy to the primary molten metal obtained in the primary melting step or to a molten metal obtained by melting an ingot formed by solidifying the primary molten metal, thereby adjusting the Si content to be within a range of 0.90% by mass or more and 1.9% by mass or less.

2. 2. The method for producing an aluminum alloy ingot according to claim 1, wherein the aluminum alloy scrap comprises at least one of scrap containing a 3000 series alloy, scrap containing a 4000 series alloy, scrap containing a 5000 series alloy, and scrap containing a 6000 series alloy.

3. 3. A continuously cast aluminum alloy rod obtained using an aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to claim 1 or 2, and having a 0.2% yield strength of 350 MPa or more.

4. An aluminum alloy forging obtained using the aluminum alloy continuously cast rod according to claim 3, having a 0.2% yield strength of 370 MPa or more.

Citation Information

Patent Citations

  • Casting recycled aluminum scrap

    JP2020514556A

  • High performance aluminum alloy with a large amount of recycled materials and method for making same

    JP2020527653A

  • Manufacturing method of aluminum alloy forging material

    JP2022137762A